Method for coating a spectacle lens
A coating process using ion-assisted electron beam evaporation and organosilan compounds on glasses forms a durable anti-fogging layer, addressing the lack of permanence in existing coatings and maintaining optical performance.
Patent Information
- Application Number
- DE102013207903
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2013-04-30
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2033-04-30
AI Technical Summary
Existing glasses coatings, particularly anti-reflective coatings, do not provide a permanent anti-fogging solution, requiring regular application of hydrophilic sprays or cloths, and surface activation treatments under vacuum conditions are time-consuming and disruptive.
A method involving ion-assisted electron beam evaporation of SiO2 or SiO2/Al2O3 layers with high silanol group density, followed by application of organosilan compounds, creates a permanent anti-fogging effect without compromising optical properties.
The method results in a durable, abrasion-resistant anti-fogging coating that maintains optical clarity under typical fogging conditions, ensuring clear vision without the need for regular treatments.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a method for coating a spectacle lens according to the preamble of patent claim 1.
[0002] Today's spectacle lenses (prescription glasses, sunglasses, ski / sports goggles, safety goggles) fog up under unfavorable conditions. These conditions include, on the one hand, the transition from a cold to a warm environment (e.g., when you come from outside into a heated home in winter when temperatures are low, or when you leave an air-conditioned building in a country with tropical climates), and on the other hand, when the lens comes into contact with a source of warm or hot air with high relative humidity (e.g., when you lift the lid of a pot of boiling water, when you open a hot oven, when you open a dishwasher while it is still warm, or when steam-saturated warm air rises from a cup of hot beverage).
[0003] Fig.Figure 3 shows a fogged-up lens. It appears "milky" and is no longer transparent. Typically, the wearer has to remove their glasses after fogging and wait until the fog disappears, or they have to wipe it off with a cloth.
[0004] If you examine the coating with a light microscope, as is the case with Fig. 4 shows that the fog consists of small water droplets. These typically have a diameter of 20 µm. The surface coverage of these droplets is approximately 50%, which is also predicted by kinetic theoretical models (see, for example, BJ Briscoe and KP Galvin, Solar Energy, 46(4), 1991, pages 191-197).
[0005] The reason a fogged lens appears milky is because the light propagation is disrupted by the droplets. Fig.5 shows such a droplet 501 schematically and defines the contact angle θ as the angle that the droplet 501 forms on the surface 502 of the spectacle lens 500 to this surface 502.
[0006] Fig. Figure 6 shows the light transmission T through a water-fogged surface as a function of the contact angle θ of the water droplets. The reduction in transmission T is accompanied by an increase in the amount of scattered light, which makes the glass appear milky. Fig. 6, that a lower contact angle θ of the water droplets than 45° is advantageous, so the transmission T is high and the scattered light component is low.
[0007] Since the condensation of water cannot be prevented under the conditions in which spectacle lenses fog up, according to the Fig.6 shows an approach to treating the surface in such a way that the water droplets form a small contact angle θ with the surface.
[0008] There are approaches to implementing this for spectacle lenses. Typically, these are sprays or liquid-soaked wipes. The liquids used belong to the group of hydrophilic surfactants. There are numerous such products on the market, for example, a product from Nanofilm sold under the brand name Clarity Defog It™, and a product from Essilor called Optifog. What these products have in common is that the anti-fog effect is not permanent; the solution must be applied to the surface regularly.
[0009] There are also approaches that use physical effects to prevent the formation of water droplets. These include, for example, ventilation systems in ski goggles.
[0010] Furthermore, there are solutions for ophthalmic lenses that are provided with a hard coating and ensure a permanent anti-fog effect. Examples include products from SDC Technologies and Gelwell. For example, WO 2012 / 024 387 A1 from SDC Technologies, Inc., describes stable organosiloxane coating compositions that, after curing, form transparent, abrasion-resistant, chemical-resistant, and water-washable anti-fog coatings. The coating compositions contain an epoxy-functional alkoxysilane, a tetrafunctional alkoxysilane, an alkoxysilyl-functional polymer with polyethylene oxide segments, an alkoxysilyl-functional cationic surfactant, and a carboxylic acid-functional compound.Articles coated with the coating compositions, methods for coating substrates with the anti-fog coating compositions, and methods for preparing the coating compositions are also described in this document.
[0011] Today's high-quality lenses are usually coated with an anti-reflective coating. This reduces unwanted reflections that can irritate the wearer. It is advantageous if the surface of anti-reflective coated lenses can be modified to achieve a permanent anti-fog effect, eliminating the need for the wearer to regularly reapply the lens, e.g., with a spray. Particular attention must be paid to ensuring that the optical effect of the anti-reflective coating is maintained.
[0012] US 2012 / 0019767A1, from which the invention is based, describes an optical article, in particular a spectacle lens, which is provided with a coating having silanol groups on its surface. The coating is typically an antireflective coating. Due to the chemical properties of the silanol groups, water droplets on the surface of the coating form a high contact angle θ of generally between 50° and 90°, sometimes exceeding 90°. The surface of this coating, in particular the silanol groups, is modified according to the teaching of US 2012 / 0019767A1 by coupling a hydrophilic reagent, namely a specific organosilane compound. This organosilane compound can consist of a linear or branched polyethylene glycol or polypropylene glycol, which has one or more silane-functional groups.The chain lengths of these linear or branched polyethylene glycols or polypropylene glycols in question consist of a plurality of repeating units. According to this document, the organosilane compound can be, for example, a compound from the compound class 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane or 2-[methoxy(polyethyleneoxy)propyl]-trichlorosilane. The document further states that this hydrophilic functional reagent is applied to the anti-reflection-coated glass in a wet-chemical or vacuum deposition step, so that the silane functional groups can chemically bond to the silanol groups of the outermost layer. On the surface treated in this way, condensing water does not form droplets (complete spreading of the water) or only forms droplets with a small contact angle below 30°. This eliminates any disturbing scattered light, and the wearer of the glasses does not experience any impairment of their clear vision.This effect occurs under both typical conditions under which lenses fog up, namely when moving from a cold to a warm environment or when the lens is exposed to a water vapor-saturated air stream.
[0013] For the spectacle wearer, the surface modification just described is only advantageous if the effect is permanent, i.e., if it survives conditions that prevail when a spectacle wearer cleans their lenses. In particular, the abrasion of the lens is worth mentioning here. The decisive factor here is the number and / or reactivity of the silanol groups on the outermost surface of the lens. If the number and / or reactivity of these groups is high, many molecules of the hydrophilic agent can be firmly bound per unit surface area. It is known that the number of silanol groups on the surface depends on a natural occurrence in the layer itself and / or on a surface activation treatment to which the coating is subjected after its production.
[0014] The document states that the various layers of an anti-reflective coating are preferably deposited under vacuum conditions by vapor deposition using one of the following methods: i) by evaporation, optionally ion beam assisted; ii) by ion beam sputtering; iii) by cathode sputtering; iv) by plasma-assisted chemical vapor deposition. The document is silent on the relationships between the number of silanol groups on the outermost surface of the spectacle lens—that is, the surface of the outermost layer of the anti-reflective coating—the natural occurrence of these silanol groups in this layer, and the deposition conditions of this outermost layer.
[0015] According to US 2012 / 0 019 767 A1, a surface activation treatment for generating silanol groups or at least increasing their proportion on the surface of a coating is generally carried out under vacuum. It can be a bombardment with energetic and / or reactive species—for example, with an ion beam (“ion pre-cleaning” or “IPC”) or with an electron beam—a corona discharge treatment, an ion spallation treatment, a UV treatment, or a plasma-assisted treatment under vacuum—usually using an oxygen or argon plasma. However, it can also be a wet-chemical treatment, namely an acidic or basic treatment and / or a solvent-based treatment, e.g., with water, hydrogen peroxide, or an organic solvent. Several treatments can also be combined.
[0016] A surface activation treatment to generate silanol groups and / or to increase their proportion on the surface of a coating, as proposed in US 2012 / 0 019 767 A1, represents an additional process step that requires additional time and additional equipment. Furthermore, it may be incompatible with upstream or downstream process steps, or only with great effort. A wet-chemical surface activation treatment, for example, requires breaking the vacuum if the anti-reflective coating is deposited using a vacuum deposition process. If the hydrophilic reagent that creates a small contact angle of water on the ophthalmic lens surface is also subsequently applied under vacuum conditions, a wet-chemical surface activation treatment is disruptive due to the pumping times required to evacuate the vacuum chamber.
[0017] The document US 2012 / 0 019 767 A1 also does not provide any information as to how a layer can be realized using the proposed alternative to the surface activation treatment, namely when the natural occurrence of silanol groups in the layer itself is sufficiently high.
[0018] US 2004 / 0 290 126 A1 discloses a method for producing a coating on a substrate for the production of displays. The document describes the growth of a layer by ion-assisted electron beam evaporation of SiO2 or Al2O3 under an inflow of oxygen and argon ions with an energy between 50 and 250 eV and an ion current between 20 and 500 mA.
[0019] US Pat. No. 6,358,572 B1 describes a method for producing a coating on a glass substrate. A layer is grown by ion-assisted electron beam evaporation of SiO2 and GeO2 under the influence of argon ions with an energy between 100 and 1 MeV.
[0020] EP 1 953 187A1 shows a method for coating a spectacle lens in which an anti-reflection layer is applied to a hard-coat coating.
[0021] Martin PJ, "Ion-based methods for optical thin film deposition," Journal of Materials Science, January 1986, Vol. 21, Issue 1, pp. 1-25, discloses the coating of modern precision optics such as power lasers and laser gyroscopes with SiO2. During the coating process, the substrate surface is modified by oxygen and argon ion bombardment. The publication states that the ion beam energy of the ion source can be adjusted within a range between 30 and 1200 eV.
[0022] Samson F., Ophthalmic lens coatings, Surface and Coatings Technology, 81 (1996), pp. 79-86, describes the AR coating of ophthalmic lenses using ion-assisted electron beam evaporation. In particular, the fabrication of a SiO2 coating using an argon ion beam with an energy of 100 eV is described.
[0023] It is the object of the invention to provide a simple and thus cost-effective method for producing a coating on a spectacle lens in which at least one layer has a high density of silanol groups.
[0024] This object is achieved by a method having the features of patent claim 1.
[0025] Advantageous embodiments and further developments of the invention are the subject of the subclaims.
[0026] The method according to the invention for producing a coating on a spectacle lens comprises the following steps: - Provision of the spectacle lens, which may optionally already have a first coating - Growth of a layer with a high density of particularly surface silanol groups on the spectacle lens by ion-assisted electron beam evaporation of SiO2 or a mixture of SiO2 with up to 10 mass percent Al2O3 under inflow of gaseous O2 and under application of Ar + -Ions with a kinetic energy between 50 and 200 eV at an ion current density between 10 and 100 µA / cm 2at the site of growth of the layer. The invention further provides that a coating is deposited directly onto the grown SiO2 or SiO2 / Al2O3 layer, said coating comprising at least one organosilane compound with a polyoxyalkylene group comprising fewer than 80 carbon atoms and at least one silicon atom producing at least one hydrolyzable group.
[0027] A spectacle lens (hereinafter also referred to as a spectacle lens substrate if it is to be clarified that no coating is present) according to the present invention can be a mineral glass or an organic glass. The organic glass can consist, for example, of a thermoplastic or thermosetting plastic material. Particularly preferred classes of plastic materials include polycarbonate, polythiourethanes, polyepisulfides and resins resulting from the polymerization or copolymerization of alkylene glycol bis allyl carbonates. A representative of the latter group of species is sold, for example, under the trade name CR-39® by PPG Industries. Well-known representatives of the polythiourethane group are the materials manufactured by Mitsui Chemicals under the trade names MR7, MR8, MR174, MR10.
[0028] In the present invention, a coating / layer that is "on" a spectacle lens or a coating, or that is applied / grows "on" a spectacle lens / coating, is understood to be a coating / layer that (i) is positioned above the spectacle lens / coating, (ii) is not necessarily in contact with the spectacle lens / coating, i.e., one or more (intermediate) coatings / layers may be arranged between the spectacle lens / coating in question, and (iii) does not necessarily completely cover the spectacle lens / coating. When a "layer 1 is arranged under a layer 2," this is intended to mean that layer 2 is arranged further away from the spectacle lens / coating than layer 1.When a “layer 1 is arranged above or on top of a layer 2”, this means that layer 1 is arranged further away from the lens / coating than layer 2.
[0029] A coating can consist of one or more individual layers. A coating can also fulfill multiple functions simultaneously.
[0030] The first coating may, for example, be or include a hard coating.
[0031] A hard coating is a coating that is harder than the plastic material from which the lens substrate is made. A hard coating typically consists of an organic / inorganic hybrid polymer or a purely organic polymer. The thickness of this hard coating is usually between 1 µm and 10 µm. Mineral lenses do not have a hard coating.
[0032] The first coating may, for example, also be an anti-reflection or anti-reflective coating, comprise such a coating and / or comprise components, in particular a layer or a layer stack, which together with the subsequently grown layer and optionally one or more further layers forms an anti-reflection or anti-reflective coating.
[0033] For the purposes of the present invention, an anti-reflective coating is a coating deposited on the surface of a spectacle lens that improves the reflection-reducing properties of the finished spectacle lens. This leads to a reduction in light reflection at the interface between the spectacle lens and air across a relatively large portion of the visible spectrum.
[0034] Anti-reflective coatings are traditionally known to be composed of a single layer or a multilayer stack of dielectric materials. These are preferably multilayer coatings comprising high-refractive-index (HI) layers and low-refractive-index (LI) layers. The materials of the individual layers of the layer stack are typically ceramic materials that are transparent at least in the visible spectral range. Examples of these materials are TiO2, Ta2O5, Nb2O5, ZrO2, Al2O3, SiO2, etc., or suitable mixed oxides. Typically, the outermost layer of an anti-reflective layer stack is a layer of a low-refractive-index material, such as SiO2 or a mixture of SiO2 and Al2O3. The thickness of these layers is generally between 10 and 100 nm. The total thickness of the anti-reflective layer stack is typically between 100 and 1000 nm.
[0035] The layer of SiO2 or a mixture of SiO2 and Al2O3 grown according to the invention with the high density of surface silanol groups can, but need not necessarily, be the outermost layer of an anti-reflection layer stack. When this layer forms the outermost layer of an anti-reflection layer stack, it combines two functionalities: achieving the reflection-reducing property and providing a sufficient number of surface silanol groups for docking the functional hydrophilic reagent described above to create an abrasion-resistant anti-fog coating of the type described above.
[0036] The layer can grow very slowly or very quickly. Thicker layers are generally produced at a higher deposition rate than thinner ones. For this application, it has proven advantageous to grow the layer at a rate between 0.5 and 10 nm / s. In particular, if the layer grown from SiO2 or a mixture of SiO2 and Al2O3 forms the outermost layer of an anti-reflection layer stack, it is advantageous to use a deposition rate between 0.5 and 5 nm / s. The highest structural quality layers, which are not absolutely necessary for this application, can be achieved at growth rates between 0.5 and 2 nm / s.
[0037] SiO2 and Al2O3 grow substoichiometrically, i.e., with an oxygen deficit, during evaporation of the respective compounds. This is explained by at least partial decomposition of the respective compounds during evaporation using an electron beam evaporator. Substoichiometric layers become less transparent with increasing oxygen deficiency due to the corresponding proportion of (semi-)metallic species Si and Al. For this reason, it is advisable to add oxygen during layer growth. The invention therefore provides for the optional addition of gaseous oxygen. If the inflowing amount of gaseous O2 is between 10 and 40 sccm, highly transparent layers and thus highly transparent anti-reflective coatings can be produced.
[0038] The deposition of the layer takes place in a vacuum due to the process. Layers that meet the requirements for transparency, adhesion, etc. are usually deposited at a pressure in the range between 10-3 and 10 -7 hPa. Since the purity requirements for the separated materials are comparatively low, a lower pressure is not necessary.
[0039] The layer can be deposited with any desired thickness using the process according to the invention. Especially when the SiO2 or SiO2 / Al2O3 layer is part of the layer system of an anti-reflective coating, it is usually deposited with a final layer thickness in the range between 25 and 120 nm. The total thickness of this layer is often between 50 and 100 nm, preferably between 60 and 80 nm.
[0040] The Ar exposure used in the growing layer according to the invention + Ions can be generated using an end-Hall ion source, for example. Such a system provides a high ion current density even at low ion energies and a comparatively wide ion beam.
[0041] Spectacle lenses in which the outermost layer was grown under one of the conditions specified above can be provided with an abrasion-resistant hydrophilic coating using the agents mentioned in the above-mentioned document US 2012 / 0 019 767 A1. Accordingly, the invention provides that a coating comprising at least one organosilane compound with a polyoxyalkylene group comprising fewer than 80 carbon atoms and at least one silicon atom producing at least one hydrolyzable group is deposited directly onto the grown SiO2 or SiO2 / Al2O3 layer.
[0042] It has proven effective if the at least one organosilane compound consists of a linear or branched polyethylene glycol or polypropylene glycol containing one or more silane-functional groups. Such compounds are also suitable for the mass production of ophthalmic lenses from an economic, ecological, and manufacturing perspective.
[0043] Sufficient reactivity of the organosilane compounds for coupling to silanol groups of the outermost layer is achieved when the chain length of the linear or branched polyethylene glycol or polypropylene glycol consists of 2 to 30 repeating units.
[0044] Organosilane compounds whose silane-functional groups comprise at least one of the following molecular groups are particularly suitable: trimethoxysilane, triethoxysilane, tripropoxysilane, trichlorosilane, dichloromethoxysilane, chlorodimethoxysilane. Examples of this class of compounds are: 2-[methoxy(polyethyleneoxy[6-9])propyl]-trimethoxysilane, 2-[methoxy(polyethyleneoxy[6-9])propyl]-trichlorosilane, 2-[methoxy(polyethyleneoxy[9-11])propyl]-trimethoxysilane, 2-[methoxy(polyethyleneoxy[9-11])propyl]-trichlorosilane, 2-[methoxy(polyethyleneoxy[11-13])propyl]-trimethoxysilane, 2-[methoxy(polyethyleneoxy[11-13])propyl]-trichlorosilane, 2-[methoxy(polyethyleneoxy[13-15])propyl]-trimethoxysilane, 2-[Methoxy(polyethyleneoxy[13-15])propyl]-trichlorosilane, bis-propyl-trimethoxysilane polyethylene oxide[6-9]), bis-propyltrichlorosilane Polyethylene oxide[6-9], etc.
[0045] The at least one organosilane compound can be a chlorosilane-functional molecule that is applied wet-chemically. The best results are achieved when the hydrophilic agent, i.e., this organosilane compound(s), is (are) dissolved in an anhydrous solvent for application. Suitable anhydrous solvents include, in particular, one or more compounds from the following group: toluene, aliphatic alkanes, cycloaliphatic alkanes, aliphatic ethers, cycloaliphatic ethers, aromatic systems, aliphatic ketones, cycloaliphatic ketones, and halogenated solvents, such as dichloromethane or chloroform.
[0046] The at least one organosilane compound is preferably used in an amount of 1 to 10 percent by weight in the anhydrous solvent. According to current knowledge, a solution of the hydrophilic agents in anhydrous toluene is particularly preferred.
[0047] If hydrophilic agents from the methoxysilane group are used, catalytic amounts of water are advantageous for coupling. In the context of the present invention, catalytic amounts of water are understood to mean concentrations in the ppm to 1% range.
[0048] The coupling reaction can be carried out by immersing the ophthalmic lenses coated according to the invention in one of the solutions described above. The best results are achieved when strict attention is paid to the exclusion of moisture. The immersion time is preferably between 1 minute and 100 minutes. This process step is preferably carried out between 0.5 minutes and 24 hours after the growth of the SiO2 or SiO2 / Al2O3 layer. With this type of process, the reagents form a hydrophilic layer on the surface of the ophthalmic lenses coated as described, with a layer thickness of 1 to 15 nm. With the method described in US 2012 / 0019767 A1, layers with a layer thickness of up to 5 nm are achieved. Such a layer is not optically effective orcan be incorporated into the optical design of any anti-reflective coating, allowing the reflective color of the anti-reflective lens to be precisely and homogeneously adjusted. The resulting hydrophilic layer is also abrasion-resistant. No further treatment of the lens is required.
[0049] In addition to immersion, alternative processes are possible, namely the application of the hydrophilic agent solution to the lens by means of spin coating, the application of the hydrophilic agent solution to the lens by means of spray coating, the application of the hydrophilic agent solution to the lens by means of flow coating or the evaporation of the hydrophilic agent solution in a vacuum and deposition onto the lens in a vacuum.
[0050] The invention will now be described in more detail with reference to the drawings. They show: Fig.1 vacuum coating system for coating a spectacle lens with a layer having a high density of surface silanol groups Fig. 2 Flowchart with the essential steps of a method according to the invention Fig. 3 Photograph of a fogged-up lens (state of the art) Fig. 4 Microscopic image of the fogged lens after Fig. 3 (state of the art) Fig. 5 Schematic representation of a water droplet on a fogged lens Fig. 6 Transmission of light through a fogged glass surface as a function of the contact angle of a water droplet Fig. 7 Model of a binding mechanism of trimethoxysilane-functional agents to silanol groups on surfaces a) Hydrolysis b) Condensation c) Hydrogen coupling d) Bond formation Fig. 8 Structural models of hydrophilic reagents on a glass surface a) Example of a loop-like structure b) Example of a brush-like structure c) Example of a brush-like structure
[0051] The Fig. Figure 1 shows a vacuum coating system 100 with a vacuum chamber 110 for coating a plurality of ophthalmic lenses 101 with a layer having a high density of surface silanol groups. The vacuum chamber 110 is evacuated to a high vacuum. Located within the vacuum chamber 110 of the vacuum coating system 100 is a cap 102 that supports the ophthalmic lenses 101 to be coated.
[0052] An electron beam evaporator 103 is arranged beneath the dome 102. The electron beam evaporator 103 comprises an electron source 104 from which an electron beam 105 emerges, which is deflected by a magnetic field B onto a crucible 106. The crucible 106 contains the evaporation material (not shown), namely, according to the invention, SiO2 (or a mixture of SiO2 and Al2O3) in tablet or powder form.
[0053] The vacuum chamber 110 also contains an ion source 107 of the “End-Hall” type. This emits Ar + -ions.
[0054] Finally, a gas inlet 108 is provided which can be controlled by means of a control valve 109 in order to introduce O2 gas into the vacuum chamber 110.
[0055] The Fig.Figure 2 shows a flowchart 200 with the essential steps of a method according to the invention. In a first step 201, a substrate material in the form of an uncoated ophthalmic lens blank (ophthalmic lens substrate) is provided. Due to prior abrasive processing or casting, the ophthalmic lens blank already possesses the desired prescribed light-refracting properties.
[0056] On this ophthalmic lens blank, in the present embodiment consisting of polycarbonate, a hard coating in the form of a 5 µm thick layer of a polysiloxane lacquer is first applied in an immersion bath process (step 202).
[0057] The spectacle lens is then placed on the cap 102 into the vacuum chamber 110 of the vacuum coating system 100 described above. In this vacuum chamber 110, in addition to the above-mentioned electron beam evaporation source 103, there are further thermal evaporation sources not shown in the drawing, namely one for Al2O3 and one for TiO2.
[0058] First, a layer of Al2O3 with a thickness of 57 nm is applied to the hard coating (step 203). A layer of quartz (SiO2) with a thickness of 25 nm is then applied to this layer using the electron beam evaporation source 103 described above (step 204). A second layer of aluminum oxide with a thickness of 44 nm is then deposited on top of this layer (step 205). This layer deposition is followed by the deposition of a second layer of quartz with a thickness of 61 nm (step 206). This is followed by a third layer of aluminum oxide with a thickness of 60 nm (step 207). A first high-index layer of titanium oxide with a thickness of 8.5 nm is then applied to this layer (step 208). This is followed by the deposition of a layer of aluminum oxide with a thickness of 45 nm (step 209), on which a second high-index layer of titanium oxide with a thickness of 22 nm is then applied (step 210).The coating is applied to both sides of the lens. Finally, a third layer of quartz with a thickness of 106 nm is applied to this layer (step 211). This layer stack forms an anti-reflective coating. The process steps for the anti-reflective coating deposition are summarized in the drawing with reference numeral 212.
[0059] According to the state of the art, it is now common practice to apply a superhydrophobic layer, a so-called top coat, to the outermost layer - in this example the third quartz layer - which ensures that the lens is easy to clean. Top coat materials are generally from the class of perfluorinated alkanes and can be coupled to OH groups in the outermost layer of the anti-reflective layer package via a silane-functional group. These OH groups on the surface are also referred to in the art as silanol groups. Top coats based on perfluorinated molecules are abrasion-resistant due to the described chemical coupling, i.e. their functionality is still intact even when the lens is in use (approximately after 2 years of daily cleaning by the wearer).Due to the chemical properties of the top coat, water droplets form a high contact angle (>90°) with the described surface, i.e. macroscopic water droplets roll off the surface.
[0060] In the case of fogging of a lens coated with the coatings just described, the microscopic droplets of condensed water also form a high contact angle with the surface. Fig. 6 can be seen, this is an unfavourable area, ie a lot of scattered light is formed, the transmission of the lens decreases, it appears milky, the wearer can no longer see anything through the lens.
[0061] Therefore, the first need is to modify the surface of the outermost layer of the coating of the spectacle lens in such a way that condensing water does not form droplets with a high contact angle with the surface, but rather forms a contact angle Θ< 30° with the surface or even spreads completely.
[0062] When selecting such a surface treatment, care must be taken to ensure that the optical properties of the anti-reflection coating package are not adversely affected, so that the coating retains its optical functionality, namely its reflection-reducing property.
[0063] To achieve this, the state of the art involves coupling a functional hydrophilic reagent to the surface of the outermost layer, both on the front and back of the lens.
[0064] This hydrophilic functional reagent is then applied to the anti-reflective coated lens in a wet chemical or vacuum deposition step, allowing the silane functional groups to chemically bond to the silanol groups of the outermost layer. For example, in the case of a trimethoxysilane (RSi(OMe)3), the bonding to the silanol groups (SiOH groups) on the surface 701 of the outermost layer 700 occurs with the elimination of methanol (MeOH) and water (H2O), as is the case with Fig. 7 shows, namely in the steps a) hydrolysis, b) condensation, c) hydrogen coupling and d) bond formation.
[0065] Both brush-like and loop-like structures can form on the surface 801, as shown in the three examples a), b) and c) of the Fig. 8 for polyethylene glycols (PEG).
[0066] Condensing water does not form droplets on the surface 701 treated in this way. The water either spreads completely, or only droplets with a small contact angle Θ below 30° form.
[0067] This eliminates distracting scattered light, and the wearer's clear vision isn't impaired. This effect occurs under both typical conditions in which lenses fog up: during the cold-to-warm transition and when the lens is exposed to a water vapor-saturated air stream.
[0068] For the wearer, the surface modification just described is only beneficial if the effect is permanent. The decisive factor is the number and / or reactivity of the silanol groups on the outermost surface of the lens. If the number / reactivity of these groups is high, many molecules of the hydrophilic agent can be tightly bound per unit surface area.
[0069] In experiments, the inventors found that the conditions under which the last layer of the anti-reflection layer stack is deposited are crucial for the number and strength of the coupling of the molecules of the hydrophilic agent.
[0070] The following deposition conditions of the above-mentioned third layer of quartz with a thickness of 106 nm are used as an example: a) Evaporation process: Electron beam evaporation b) Vacuum conditions: High vacuum c) Evaporation rate: 1 nm / s d) Addition of O2 gas: 20 sccm e) Ar + -Ion energy 150 eV f) Ar + -Ion current density 80 µA / cm 2 at the location of the substrate to be coated. In order to graphically illustrate the relevance of the deposition conditions of this layer, process step 211 is shown as a double-bordered field.
[0071] In the described embodiment, the ophthalmic lens coated in this way is immersed in a hydrophilic agent consisting of 2-[methoxy(polyethyleneoxy[6-9])propyl]trichlorosilane, dissolved in anhydrous toluene at a concentration of 5 wt.% in a subsequent step 213, 30 s after removal from the vacuum chamber 110. Strict exclusion of moisture is essential. The immersion time is 1 min. With this type of process, the reagents form a hydrophilic layer on the surface of the ophthalmic lenses coated as described, with a layer thickness of 1.5 nm. Such a layer is not optically effective. Likewise, the hydrophilic layer produced in this way is permanently abrasion-resistant. Post-treatment of the ophthalmic lens is unnecessary. The optical function of the anti-reflection coating is fully retained.
[0072] The application is not limited to spectacle lenses alone, but can include any optical components (lenses, prisms) or assemblies thereof.
Claims
[1] Method for producing a coating on a spectacle lens (101) comprising the steps: - Providing (201) the spectacle lens (101), which may optionally have a first coating - growing (211) a layer on the spectacle lens (101) by ion-assisted electron beam evaporation of SiO2 or a mixture of SiO2 with up to 10 mass percent Al2O3, wherein the growth (211) of the layer is carried out under the action of Ar + -Ions with a kinetic energy between 50 and 200 eV at the site of growth of the layer characterized by , that - the growth (211) of the layer takes place under the inflow of gaseous O2 and that the application of Ar + -ions at an ion current density between 10 and 100 µA / cm 2 at the place where the layer grows, and that - a coating is deposited (213) directly onto the grown layer, said coating comprising at least one organosilane compound having a polyoxyalkylene group comprising less than 80 carbon atoms and at least one silicon atom producing at least one hydrolyzable group. [2] Method according to claim 1, characterized by that the layer forms a component, preferably the outermost layer, of an anti-reflective coating. [3] Method according to one of the preceding claims, characterized by that the layer is grown at a speed between 0.5 and 10 nm / s, preferably between 0.5 and 5 nm / s, more preferably between 0.5 and 2 nm / s. [4] Method according to one of the preceding claims, characterized by that the inflowing amount of gaseous O2 is between 10 and 40 sccm. [5] Method according to one of the preceding claims, characterized bythat the growth of the layer at a pressure in the range between 10 -3 and 10 -7 hPa. [6] Method according to one of the preceding claims, characterized by that the layer is grown with a final layer thickness in the range between 25 and 120 nm, preferably between 50 and 100 nm, most preferably between 60 and 80 nm. [7] Method according to one of the preceding claims, characterized by that the at least one organosilane compound consists of a linear or branched polyethylene glycol or polypropylene glycol which has one or more silane-functional groups. [8] Method according to claim 7, characterized by that the chain length of the linear or branched polyethylene glycol or polypropylene glycol consists of 2 to 30 repeating units. [9] Method according to claim 8, characterized bythat the silane functional groups comprise at least one of the following molecular groups: trimethoxysilane, triethoxysilane, tripropoxysilane, trichlorosilane, dichloromethoxysilane, chlorodimethoxysilane. [10] Method according to one of the preceding claims, characterized by that the at least one organosilane compound is a chlorosilane-functional molecule, that the at least one organosilane compound is applied wet-chemically and that the at least one organosilane compound is dissolved in an anhydrous solvent for application. [11] Method according to claim 10, characterized by that the anhydrous solvent comprises at least one compound from the following group: toluene, aliphatic alkanes, cycloaliphatic alkanes, aliphatic ethers, cycloaliphatic ethers, aromatic systems, aliphatic ketones, cycloaliphatic ketones, halogenated solvents. [12] Method according to one of claims 10 or 11, characterized bythat the at least one organosilane compound is used in an amount of 1 to 10 percent by weight in the anhydrous solvent. [13] Method according to one of the preceding claims, characterized by that the coating comprising at least one organosilane compound is deposited in the absence of moisture. [14] Method according to one of the preceding claims, characterized by that the coating comprising at least one organosilane compound is deposited by spray coating or flooding.
Citation Information
Patent Citations
Transparent laminate, plastic lens for eyeglass and primer composition
EP1953187A1
Optical Article Comprising a Temporary Anti-Fogging Coating with Improved Durability
US20120019767A1
Method for manufacturing a nonlinear optical thin film
US6358572B1
Anti-fog organosiloxane coating compositions and coatings
WO2012024387A1
Optical article comprising a temporary Anti-fogging coating with improved durability
EP2519474B1