Glass-containing preparation for use in an additive manufacturing process and molded parts produced therewith
The use of multi-component glass particles with adjusted Hansen parameters and broad particle size distribution in 3D printing preparations addresses the challenge of high solids content and viscosity, enabling high filling levels, low shrinkage, and varied optical properties in 3D printed components.
Patent Information
- Application Number
- DE102022110482
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-04-29
AI Technical Summary
Existing additive manufacturing processes face limitations in achieving high solids content without excessive viscosity, which affects processability and limits the range of achievable refractive indices and optical properties in 3D printed components.
A preparation for 3D printing using multi-component glass particles with a broad particle size distribution and adjusted Hansen parameters, combined with a monomer system, to achieve high filling levels and low viscosity, allowing for varied optical properties and minimal shrinkage.
The solution enables high filling levels with low viscosity, ensuring good processability and varied optical properties in 3D printed components, while minimizing shrinkage and enhancing mechanical stability.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Field of the invention
[0001] In general, the invention relates to a glass-containing preparation for additive manufacturing processes. In particular, the invention relates to a preparation with glass particles made from a multi-component glass with a high filler content.
[0002] Processes for the additive manufacturing of three-dimensional objects have the advantage over conventional manufacturing methods in that no mold of the object is required. Thus, additive manufacturing processes such as 3D printing can be used to produce even small quantities or even individual pieces cost-effectively.
[0003] 3D printing is primarily used for polymeric materials, but processes are also known that utilize preparations containing quartz glass. The preparation usually contains a polymerizable monomer with glass particles dispersed therein. A corresponding process is described in WO 2018 / 0650930A. The monomer is liquid at room temperature and thus serves as a dispersing medium. Upon polymerization of the monomer after application of the preparation, it becomes solid and acts as a binder between the glass particles. The resulting green body is subsequently debound by burning out the polymer matrix and then sintered, bonding the glass particles together.
[0004] To ensure high dimensional accuracy, the solids content in the preparation, i.e., the proportion of glass particles in the preparation, should be as high as possible. At the same time, however, the preparation must still be suitable for use in 3D printing. Therefore, special requirements are placed on the rheology of the preparation. The viscosity of the preparation must not be too high, otherwise the preparation is not suitable for use in 3D printing. At the same time, however, an increase in the solids content leads to an increase in the viscosity. Thus, the maximum solids content of a preparation for 3D printing is limited by its viscosity.
[0005] Furthermore, the prior art only discloses preparations whose glass particles are made of quartz glass. Thus, for example, the refractive indices achievable for the resulting body lie within a relatively narrow range. Furthermore, the particles are obtained via a bottom-up process, i.e., by formation from appropriate precursors in a sol-gel process or by pyrolytic deposition. As a result, the quartz particles have a predominantly spherical structure and a monodisperse or at least narrow particle size distribution. Object of the invention
[0006] The invention is therefore based on the object of providing a preparation for use in an additive manufacturing process, in particular in a 3D printing process, with which the smallest possible shrinkage can be achieved between the printed and sintered, compacted component. Furthermore, the optical properties of the component should be variable within a relatively wide range. A further object is to provide a corresponding additive manufacturing process for producing the component. Description of the invention
[0007] The problem is already solved by the subject matter of the independent claims. Advantageous embodiments and further developments are the subject matter of the dependent claims.
[0008] The invention describes a formulation of a preparation for additive manufacturing processes of three-dimensional bodies, in particular for 3D printing, which enables the smallest possible shrinkage between the printed and sintered compacted component and at the same time has good processability in the printing process.
[0009] The preparation comprises at least one monomer and glass particles dispersed therein. The glass particles comprise at least one multicomponent glass. A multicomponent glass, as defined by the invention, is a glass that, in addition to SiO2, contains at least one other glass component. A component, as defined by the invention, is understood to mean, in particular, a chemical element that is present in the glass at at least 1% of the total weight. By selecting the glass, optical properties such as the refractive index or the thermal expansion coefficient of the finished body can be adjusted.
[0010] The glass particles in the glass paste exhibit a cumulative particle size distribution that approximates the Andreassen model. Preferably, the glass particles have a maximum grain size d 99 of less than 500 µm, preferably less than 200 µm and particularly preferably less than 100 µm.
[0011] The Andreassen model describes the possibility of filling a space as densely as possible with spherical particles, so that the remaining void is as small as possible while still allowing the mixture to flow. By using particles with a broad particle size distribution, a volume can be filled with a significantly higher filling ratio, i.e., with more particles per volume, than when using particles with a narrow particle distribution or even monodisperse particles. Thus, with particles with a broad particle distribution, the smaller particles can settle into the voids formed between the larger particles, thus making better use of the space. The Andreassen model provides an idealized particle size distribution with which the maximum filling ratio of a space with spherical particles can be achieved while simultaneously allowing the mixture to flow: Q3(d)=(dD)q d particle size D maximum particle size q partition coefficient
[0012] The particle size "d" is determined as follows: the individual particles of a powder, regardless of their actual shape, are divided into different fractions based on the diameter of a sphere with their equivalent volume (volume-equivalent sphere diameter). To determine the particle distribution Q, the respective number of the corresponding fractions within the powder is determined. The Andreassen equation uses the particle distribution Q3(d), which is calculated from the volume of the respective fractions.
[0013] The q-value represents the slope of the Andreassen equation in a log-log plot. Varying the q-value takes into account deviations of the real particles from the ideal model particles. These deviations can arise, for example, from a particle shape that deviates from an ideal sphere or from interactions between the particles or with the dispersion medium.
[0014] Particles that tend to agglomerate due to interaction with the disperse phase exhibit poorer rheological properties at low q values, i.e., with broad particle size distributions that would indicate a high filler content. Therefore, a higher q value can be advantageous here. However, with an increasing q value, the mixture becomes coarser and more difficult to process. Mixtures with a high fineness content, in contrast, exhibit a low q value.
[0015] The inventors have surprisingly discovered that higher fill levels in the paste can be achieved by choosing the q-value. The q-value is selected so that it is small enough to allow the finest possible particle composition, yet large enough that correspondingly coarse particles ensure sufficient flowability of the paste. Therefore, the Andreassen equation of the glass pastes according to the invention has a q-value in the range of 0.2 to 0.5. Particularly high maximum volume fill levels are achieved in glass pastes whose Andreassen equation has a q-value in the range of 0.25 to 0.4.
[0016] Real particle distributions can only partially represent the idealized Andreassen model. Due to the material properties and the manufacturing process, the particle distributions correspond more or less to the ideal distribution. In practice, this is achieved by mixing different particle size distributions so that the mixture distribution corresponds as closely as possible to the Andreassen distribution. These mixtures can be calculated using calculation tools (e.g. EMMA). The individual fractions are then compared to each other in a volume-weighted ratio. The resulting mixed fraction of glass particles ideally exhibits a cumulative particle size distribution, whereby the cumulative particle size distribution of the Q3real fraction shows only a slight deviation from the ideal cumulative Andreassen distribution function Q3-Andreassen. Thus, the particle size distribution of the Q fraction 3,real, which corresponds to a random sample with n particle fractions, a squared distance δ 2 from the ideal cumulative Andreassen distribution function Q 3-Andreassen δ2=1n∑v=1n[Q3,real(d)−Q3,Andreassen(d)]2 of less than 0.03. Here, the value n ≥ 100, preferably in the range from 100 to 1000. According to an advantageous embodiment, the distance δ 2 from the ideal cumulative Andreassen distribution less than 0.02, preferably less than 0.015.
[0017] Due to the small deviation of the particle distribution from the ideal Andreassen distribution, relatively high filler contents can be achieved in the glass pastes according to the invention, while at the same time the viscosity is low enough for processing the corresponding paste in an additive manufacturing process, particularly in 3D printing. According to one embodiment, the viscosity of the paste at room temperature and a shear rate of 200 1 / s is in the range of 150 to 10,000 mPas. Preferably, the viscosity at room temperature and a shear rate of 200 1 / s is less than 6,000 mPas or even less than 3,000 mPas.
[0018] Alternatively or additionally, according to a further embodiment, the paste has a viscosity of less than 10,000 mPas at room temperature and a shear rate of 30 l / s. The viscosity at this shear rate is preferably in the range of 150 to 10,000 mPas; preferably, the viscosity at this shear rate is less than 6,000 mPas, particularly preferably less than 3,000 mPas.
[0019] One embodiment provides that the fill level, i.e., the volume fraction of the glass particles in the total volume of the paste, is at least 12 vol.%, preferably at least 15 vol.%, and particularly preferably at least 20 vol.%. The fill level is preferably in the range from 12 to 50 vol.%, in particular in the range from 20 to 40 vol.%.
[0020] The Andreassen equation, which the paste according to the invention satisfies, has a q-value in the range of 0.2 to 0.5. To achieve a correspondingly low q-value and thus a high filler content in the glass paste system, the dispersed particles should be adapted as closely as possible to the disperse phase, especially to the monomer. If the glass particles and the disperse phase exhibit good surface compatibility, smaller q-values can be achieved in the powder mixtures, thereby optimizing the particle packing. The interactions between the individual phases can be described by the Hansen parameters δ i The Hansen parameter δ i takes into account both the disperse fraction δ D , the polar part δ P and the proportion of surface interactions through hydrogen bonds δ H : δi=δD2+δP2+δH2
[0021] The closer the Hansen parameters of glass particles and dispersant are to each other, the stronger the attractive interactions between dispersed particles (disperse phase) and the dispersant, and the more stable the dispersion. A further development of the invention therefore provides that the glass particles used and the monomers in the paste are matched to each other with regard to their Hansen parameters. Therefore, glass particles and monomers preferably have a small Hansen parameter distance (HSP distance) Ra with Ra=4(δD,i−δD,j)2+(δP,i−δP,j)2+(δH,i−δH,j)2
[0022] The smaller the distance Ra between glass particles and monomer, the better they can be mixed together and the smaller the exponent q in the Andreassen equation can be chosen without adversely affecting the flowability of the paste or dispersion. It has proven particularly advantageous if the squared distance R a 2 the Hansen parameters of the glass particles and the monomers Ra2=4(δD,i−δD,j)2+(δP,i−δP,j)2+(δH,i−δH,j)2 less than 200 MPa, preferably less than 150 MPa and particularly preferably less than 100 MPa.
[0023] The Hansen parameters of glass particles and monomers can be adjusted by the glass composition and / or by the choice of monomers. The polymerization reaction can be initiated thermally or by exposure to electromagnetic radiation, preferably in the UV-VIS range. The monomer acts as a binder, which, after polymerization, forms a polymer matrix for the glass particles and thus initially stabilizes the printed body. This polymer matrix is subsequently removed from the body by burning out, and the glass particles are bonded together through a sintering process, so that the resulting molded body exhibits high mechanical stability.
[0024] One embodiment of the invention provides that the monomer has an acrylic group as at least one polymerizable group. The monomer can thus also be referred to as an acrylate. The acrylate can be monofunctional or have multiple acrylic groups. According to one embodiment, the preparation contains an acrylate- or vinyl-functionalized molecule as monomer, for example, correspondingly functionalized silsesquioxanes or (methyl)siloxanes. Furthermore, the following monomers and mixtures thereof are particularly suitable as acrylates: hydroxyethyl methacrylate (HEMA), hexanediol diacrylate (HDDA), acryloylmorpholine (ACMO), pentaerythritol tetraacrylate (PPTTA), and trimethylolpropane triacrylate (TMPTA).
[0025] According to another embodiment, the monomer has an epoxy function or an episulfide function as the polymerizable group.
[0026] According to one embodiment, a monomer, in particular an acrylate, is used whose Hansen parameter δ D in the range of 15.5 to 17.5 MPa, δ P in the range of 10.5 to 11.5 MPa and δ H in the range of 9.5 to 10.5 MPa.
[0027] In addition to the monomer, the dispersing phase may contain additional solvents. According to one embodiment, the preparation contains a solvent, wherein the solvent is selected such that the squared distance R a 2 the Hansen parameters of the glass particles and the solvent molecules Ra2=4(δD,i−δD,j)2+(δP,i−δP,j)2+(δH,i−δH,j)2 less than 200 MPa, preferably less than 150 MPa and particularly preferably less than 100 MPa.
[0028] The use of at least one solvent selected from the group consisting of acetone, acetonitrile, anisole, n-butyl acetate, diethylene glycol monoethyl ether, dimethyl sulfoxide, methyl ethyl ketone, 2-phenoxyethanol, propylene glycol monoethyl acetate, γ-valerolactone, and 2-propanol has proven advantageous. Alternatively, corresponding mixtures can also be used.
[0029] The respective glass composition of the particles in the paste can be used to adjust both the optical, thermal, or mechanical properties of the body printed with the paste, as well as the Hansen parameters of the glass particles. According to one embodiment, the paste comprises a borosilicate glass, an alkali borosilicate glass, a barium glass, or a soda-lime glass. Table 1 shows examples of the glass compositions based on working examples 1 to 6. Table 1: Glass compositions of some examples Glass 1 Glass 2 Glass 3 Glass 4 Glass 5 Glass 6 Oxide % by weight % by weight % by weight % by weight % by weight % by weight SiO2 84.8 56 67 81 64 70 B2O3 10 10 20.8 13 8.3 7 Al2O3 4.7 10 5 2.3 4.2 13 Bi2O3 Li2O 0.7 Na2O 2.4 3.2 6.5 5 K2O 1.5 0.5 7 CaO 0.6 BaO 0.5 24 1.3 ZnO 6 1 TiO2 4 1.5 ZrO2 0.5 F 0.7 MgO 2
[0030] The inventors have discovered that the q-value can be influenced by the shape of the glass particles or their aspect ratio, thus increasing the maximum filler content of a flowable paste. It has proven advantageous for the glass particles to be predominantly non-spherical in the form of flakes or scales. In particular, the glass particles have surfaces created by glass breakage as a result of a grinding process, particularly as a result of dry and / or wet grinding processes. According to one embodiment, the glass particles are shard-shaped.
[0031] The shape of particles can be described by their roundness or circularity. These can be determined using optical image analysis of a sample image. For this purpose, a sufficiently large sample containing more than 10,000 particles is measured by analyzing a corresponding image, for example, a microscope, SEM, or camera image, using dynamic image analysis. Roundness and circularity are determined based on two-dimensional projections of the particles. For technical reasons, the resolution is limited to particle sizes of at least 30 µm. Selecting a sufficiently large sample ensures that all conceivable particle orientations are captured.
[0032] The glass particles have an average, cumulative, and volume-related particle shape whose roundness is in the range of 0.3 to 0.9, preferably in the range of 0.4 to 0.8, and particularly preferably in the range of 0.55 to 0.75. The roundness of a particle is calculated from the ratio of the largest diameter or cross-section to the smallest diameter or cross-section of the measured particle.
[0033] Alternatively or additionally, the glass particles have a circularity in the range of 0.6 to 0.95, preferably 0.66 to 0.87, and particularly preferably 0.7 to 0.85. Circularity refers to the ratio of the cross-sectional area of a particle to its circumference.
[0034] Particles with a roundness of < 0.3 or a circularity of < 0.6 are fibrous, while particles with a roundness of > 0.9 or a circularity of > 0.95 are almost perfect spheres. The particles of the two embodiments described above are shard-shaped particles.
[0035] The shard-shaped particles can be obtained by comminuting a suitable glass in a top-down milling process. The shard shape of the particles is retained even in finer-ground particles. This makes it possible to transfer the specific particle shape limits to finer powders in the µm and sub-µm range.
[0036] The invention further relates to a molded body produced or producible by a 3D printing process using the preparation according to the invention. One embodiment of the production process provides that, in a first step, the preparation is converted into a three-dimensional structure using a 3D printer. To stabilize the structure, the monomer is polymerized. This can be radically or cationically, for example, and can be initiated thermally or by exposure to electromagnetic radiation, particularly in the UV-VIS range. The polymer material is burned out of the resulting body, and the body, freed from the binder, is subsequently sintered. Character description
[0037] The invention is explained below using exemplary embodiments and the Fig. 1 to 12 are explained in more detail. They show: Fig. 1 a schematic representation of the preparation according to one embodiment, Fig. 2 the representation of the particle size distribution of a powder mixture and a particle size distribution according to the Andreassen equation, Fig. 3 shows the particle size distribution of a powder mixture according to another embodiment, Fig. 4 to 6 show the particle size distribution of the individual glass powders of the embodiment according to Fig. 3, Fig. 7 and Fig. 8 shows the particle size distribution of further embodiments, Fig. 9 the relationship between viscosity and particle size distribution, Fig. 10 schematic drawings for determining the roundness value and the circularity value as well as Fig. 11 and Fig. 12 SEM images of particle mixtures of different embodiments.
[0038] Fig.Figure 1 shows a schematic representation of an embodiment of a preparation in the form of a printing paste 1. The printing paste 1 has a continuous phase 3 and glass particles 200, 201, 202 dispersed therein. The dispersant 3 contains monomers which can undergo a photoinduced or thermally induced polymerization reaction to form a polymer. In the Fig. In the embodiment shown in Figure 1, the dispersant 3 contains a monomer with at least one acrylate function and additionally a solvent. The monomer and solvent are selected so that they are readily miscible and have similar Hansen parameters. The dispersed glass particles comprise a multi-component glass and have a shard-like shape. The glass particles 200, 201, 202 were obtained by a top-down milling process of glass frits and have a particle size distribution, wherein the cumulative particle size distribution of the fraction Q 3realideal cumulative Andreassen distribution function Q 3-Andreassen Q3(d)=(dD)q a squared distance δ 2 δ2=1n∑v=1n[Q3,real(d)−Q3,Andreasen(d)]2 of less than 0.03. The distribution coefficient q of the Andreassen equation lies in the range between 0.2 and 0.5.
[0039] To obtain the particle size distribution described above, a glass particle mixture with different particle size fractions is used. The mixing ratio is adjusted to achieve the deviation from the ideal Andreassen equation selected above. Fig. In the embodiment shown in Figure 1, three different glass powders 200, 201, 202, each with different particle size distributions, were mixed. Fig. In the embodiment shown in Figure 1, the glass powder has a maximum grain size d 99of less than 500 µm, preferably less than 200 µm or even less than 100 µm. This enables high resolution when using the glass paste in 3D printing.
[0040] In Fig. 2 shows the particle size distribution 5 of a glass powder as a comparison example and the particle size distribution according to the Andreassen equation 4. Fig. 2 shows that there are sometimes significant deviations between the real particle size distribution 5 of the comparison example and the Andreassen particle size distribution 4. This is particularly the case for very small and large particle sizes. The comparison example has a quadratic distance δ 2 of more than 0.03.
[0041] Fig.Figure 3 shows the particle size distribution 50 of an embodiment and the corresponding Andreassen distribution 4. The Andreassen equation has a gradient value q of 0.26. The glass powder of the Fig. The exemplary embodiment shown in Figure 3 was made from three different glass powders with different particle size distributions. These were mixed so that the mixture distribution corresponds as closely as possible to the Andreassen distribution. The optimal mixing ratio for this is determined using calculation tools, such as EMMA. Due to this mixture, the glass powder has a particle size distribution of 50, which only deviates slightly from the Andreassen distribution of 4. Fig. 4 to 6 are the particle size distributions 51, 52, 53 of the individual glass powder mixtures from which the Fig.3. The mixture comprises 27 vol.% glass particles with particle size distribution 53, 10 vol.% of the mixture with particle size distribution 52, and 63 vol.% of the mixture with particle size distribution 51.
[0042] The Fig. Figure 7 shows another exemplary embodiment of a glass powder mixture. Here, the particle size distribution 54 of the glass powder mixture also shows only minor deviations from a particle size distribution 4 according to the Andreassen distribution. In this example, the Andreassen distribution 4 has a q-value of 0.3.
[0043] Here, the Fig. The powder mixture shown in Figure 7 was adapted to the calculated particle size distribution shown in Table 2 by mixing three different powder mixtures: Table 2: calculated particle size distribution d 10 [µm] d 50 [µm] d 90 [µm] d 99 [µm] 0,11 0,82 2,75 6,5
[0044] The maximum particle size is 8.1 µm.
[0045] In Fig. Figure 8 shows the particle size distribution 55 of a powder mixture of another exemplary embodiment. The particle size distribution 55 was obtained by mixing three different glass powders with different particle size distributions. The individual powders were mixed such that the particle size distribution 55 of the mixture was as close as possible to the Andreassen distribution 4. For this purpose, the glass powders were mixed such that the mixture had the calculated particle size distribution shown in Table 3. Table 3: Calculated particle size distribution d 10 [µm] d 50 [µm] d 90 [µm] d 99 [µm] 0,13 0,58 3,27 6,54
[0046] In this example, the Andreassen distribution 4 has a q-value of 0.3 and the maximum particle size is 8.2 µm.
[0047] Fig. Figure 9 illustrates the influence of the particle size distribution of the glass powder on the rheological properties of the corresponding printing paste. Fig. Figure 9 shows the relationship between viscosity and shear rate of a comparative example 6 and an exemplary embodiment 7. Both pastes have a filler content of 40 vol%. Both exemplary embodiments contain an epoxy as the monomer. Comparative example 6 has a conventional glass powder with an average particle size d 50 of 6 µm, whereby the particle size distribution does not correspond to the Andreassen distribution. In contrast, embodiment 7 contains a glass powder mixture which was mixed from three different glass powders with different particle size distributions. The glass powder mixture comprises 55 vol.% of a glass powder with a particle size distribution with d 50 = 6 µm., 10 vol% of a glass powder with a particle size distribution with d 50 = 1.2 µm and 35 vol.% of a glass powder with a particle size distribution of d 50= 0.14 µm. This composition was determined using an EMMA calculation tool and fitted to an Andreassen distribution with a q-value of 0.25. The squared distance is a squared distance δ 2 to the Andreassen equation is less than 0.03.
[0048] Out of Fig. Figure 9 clearly shows that by using a glass particle mixture whose particle size distribution essentially corresponds to or approximates the Andreassen distribution, printing pastes with comparatively low viscosities and advantageous rheological properties for the printing process can be obtained, even at high filler levels. A blend of different grain fractions based on Andreassen's law leads to a noticeable reduction in viscosity at a comparable filler content.
[0049] Surprisingly, despite a relatively high proportion of very small particles, i.e., a high fineness, a corresponding paste exhibits little or no strong interactions between the individual particles. In fact, a relatively high proportion of particles with a particle size in the sub-µm range is necessary for the desired rheological properties. Fig. In the embodiment shown in Figure 9, this proportion is 30 to 40 vol.%.
[0050] Fig.Figure 10 shows the determination of roundness (a)) and circularity (b)). The particle shape of particles can be described by their roundness or circularity. These can be determined using optical image analysis, for example using a camera analysis, for example on microscope or SEM images. For this purpose, the sample of measured particles must be as large as possible. Preferably, a sample of more than 10,000 particles is carried out. In practice, these analyses are carried out using dynamic image analysis, as this method can be used to analyze a complete particle collective with several hundred thousand particles. The resolution of this method is limited to particles with a size of at least 30 µm.
[0051] Fig.Figure 11 shows an SEM image of a section of a glass powder mixture of one exemplary embodiment. The individual glass particles have a shard-like shape. This shape results from the particle production process using a top-down milling process. In this process, a glass frit is crushed by milling. At the Fig. For the sample shown in Figure 11, the particle shape was determined using roundness and circularity. Table 4 shows the results. Table 4: Determined particle shape Particle shape 10 vol.% 50 vol.% 90 vol.% 99% by volume Average value Roundness 0,89 0,7 0,49 0,34 0,65 Circularity 0,66 0,83 0,89 0,90 0,8
[0052] Glass powders with particle shapes whose roundness is 0.3 to 0.9, preferably 0.4 to 0.8 and particularly preferably 0.55 to 0.75 and / or whose circularity is 0.6 to 0.95, preferably 0.66 to 0.87 and particularly preferably 0.7 to 0.85, have proven to be advantageous.
[0053] In Fig.Figure 12 shows SEM images of a glass powder of another embodiment. The enlargement of section 8 clearly shows that the shard shape is retained even with finer grinding of the particles. Thus, even finer powders with particle sizes in the µm and sub-µm range can exhibit the particle shape limits described above.
Claims
[1] Preparation, in particular printing paste for 3D printing, comprising a preparation with at least one polymerizable monomer and glass particles dispersed therein, wherein the glass particles comprise a multi-component glass and the glass particles have a cumulative particle size distribution, wherein the cumulative particle size distribution of the fraction Q 3real , which represents a random sample with n particle fractions, where n is chosen to be greater than 100, from the ideal cumulative Andreassen distribution function Q 3-Andreassen a squared distance δ 2 δ2=1n∑v=1n[Q3,real(d)−Q3,Andreassen(d)]2 of less than 0.03, where the ideal cumulative Andreassen distribution function Q 3, Andreassen , (d) the equation Q3(d)=(dD)q where d is the particle size, D is the maximum particle size and q is a distribution coefficient and where the distribution coefficient q is in the range between 0.2 and 0.5 and the glass particles have an average, cumulative and particle volume-related particle shape whose roundness is 0.3 to 0.9 and / or whose circularity is 0.6 to 0.
95. [2] Preparation according to the preceding claim, wherein the preparation has a square distance δ 2 from the ideal cumulative Andreassen distribution function Q 3,Andreassen of less than 0.02, preferably less than 0.
015. [3] Preparation according to one of the preceding claims, wherein the distribution coefficient q is in the range from 0.25 to 0.
4. [4] Preparation according to one of the preceding claims, wherein the viscosity of the preparation at room temperature and a shear rate of 200 1 / s is in the range from 150 to 10,000 mPas, preferably less than 6,000 mPas, particularly preferably less than 3,000 mPas and / or the viscosity of the preparation at room temperature and a shear rate of 30 1 / s is in the range from 150 to 10,000 mPas, preferably less than 6,000 mPas, particularly preferably less than 3,000 mPas. [5] Preparation according to one of the preceding claims, wherein the preparation has a filling level of at least 12 vol.%, preferably at least 15 vol.% and particularly preferably at least 20 vol.%. [6] Preparation according to one of the preceding claims, wherein glass particles and monomer Hansen parameter δ i with δi=δD2+δP2+δH2 Have, where δ D the dispersed fraction, δ P the polar part and δ His the proportion of hydrogen bonds and the squared distance of the Hansen parameters of glass particles and monomer Ra2=4(δD,i−δD,j)2+(δP,i−δP,j)2+(δH,i−δH,j)2 less than 200 MPa, preferably less than 150 MPa and particularly preferably less than 100 MPa. [7] Preparation according to one of the preceding claims, wherein the preparation contains as monomer an acrylate, an epoxide or episulfide, preferably an acrylate selected from hydroxyethyl methacrylate (HEMA), hexanediol diacrylate (HDDA), acrylolymorpholine (ACMO), pentaerythriol tetraacrylate (PPTTA), trimethylolpropane triacrylate (TMPTA), mixtures thereof and / or acryl-functionalized silsesquioxane or (methyl)siloxanes. [8] Preparation according to one of the preceding claims, wherein the preparation contains at least one solvent in addition to the monomer, wherein the solvent is preferably selected from the group consisting of acetone, acetonitrile, anisole, n-butyl acetate, diethylene glycol monoethyl ether, dimethyl sulfoxide, methyl ethyl ketone, 2-phenoxyethanol, propylene glycol monoethyl acetate, γ-valerolactone, 2-propanol, or mixtures thereof. [9] Preparation according to one of the preceding claims, wherein the multi-component glass comprises a borosilicate glass, alkali borosilicate glass, a barium glass or a soda-lime glass. [10] Preparation according to one of the preceding claims, wherein the glass particles have an average, cumulative and particle volume-related particle shape whose roundness is 0.4 to 0.8 and preferably 0.55 to 0.75 and / or whose circularity is 0.66 to 0.87 and preferably 0.7 to 0.
85. [11] Preparation according to one of the preceding claims, wherein the glass particles are obtained by comminuting a corresponding glass, preferably by dry and / or wet grinding processes and / or are non-spherical in the form of flakes. [12] Preparation according to one of the preceding claims, wherein the glass particles have a maximum grain size d 99 of less than 500 µm, preferably less than 200 µm and particularly preferably less than 100 µm. [13] Use of a preparation, in particular printing paste, according to one of the preceding claims in an additive manufacturing process, preferably in a 3D printing process. [14] Shaped body produced or producible by a 3D printing process with a preparation according to one of the preceding claims 1 to 12.
Citation Information
Patent Citations
WO2018650930A1