Method for producing electrode mixtures, and apparatus for this purpose
The solvent-free mechanical mixing method for electrode mixtures forms a fibrillated binder network, addressing efficiency and cost issues in lithium-ion battery production by enhancing production efficiency and quality.
Patent Information
- Application Number
- DE102023112620
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-14
AI Technical Summary
Existing methods for producing electrode mixtures for lithium-ion batteries are time and energy-consuming due to the need for solvent removal in a complex drying process, which affects production efficiency and cost-effectiveness.
A method involving mechanical mixing of active material, additives, and binder without solvents, using shear forces to form a homogeneous particle composite structure, followed by controlled mechanical power input to create a fibrillated binder network, ensuring uniformity and electrical connectivity.
This approach reduces solvent usage, enhances production efficiency, and results in a high-quality electrode mixture that is easy to process, improving the manufacturing process of lithium-ion batteries.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to a method for producing electrode mixtures, a device for carrying out the method, the use of a device for carrying out the method, and an electrode mixture produced according to the method.
[0002] In recent years, battery technology, and in particular lithium-ion technology, has moved into the spotlight, as it is essential for the functionality of, for example, fully electric vehicles, but also for stationary energy storage systems. A long-lasting, high-capacity battery that is cost-effective to manufacture is a prerequisite for the acceptance of fully electric vehicles.
[0003] Currently, mainly lithium-ion batteries are used.
[0004] A typical lithium-ion cell electrode consists of a copper foil acting as the anode and an aluminum foil acting as the cathode. The foils are usually coated on both sides with active material and, at least for the cathode, with additives.
[0005] During charging of the lithium-ion cell, lithium ions migrate from the cathode through an electrolyte to the anode, where they are held in place by particles of the active material. This process is reversible, so that when the battery discharges, the lithium-ion current flows from the anode to the cathode.
[0006] The electrodes must meet high standards in order to produce a reliable, high-capacity lithium-ion battery.
[0007] The electrode layer must have pores into which the electrolyte can penetrate, enabling the transport of lithium ions to each particle of the active material. Ideally, the active material should be wetted by the electrolyte over as large an area as possible. Furthermore, the particles of the active material must be electrically connected to the metal foil—in the described example, to the copper or aluminum foil—to ensure the transport of electrons to and from each particle of the active material.
[0008] Furthermore, the particles of the active material must be bound both to each other and to the metal foil, for which a binder material is used. Finally, the layer thickness should be as uniform as possible.
[0009] To produce the layers, the starting materials—that is, the active material, the binder, and any additives—must be mixed together and dispersed into a so-called "slurry" (paste). Typically, a liquid solvent (e.g., water or N-methyl-2-pyrrolidone (NMP)) is added, which then has to be removed again in complex drying processes after the electrode mixture has been applied to the film.
[0010] This is time-consuming and energy-intensive. Furthermore, the automated production of electrode mixtures requires bulky drying equipment.
[0011] Based on the described state of the art, it is therefore an object of the present invention to provide a method for producing electrode mixtures which reduces the amount of solvent required or, in the best case, even manages completely without solvent and yet provides a readily processable electrode mixture of high quality.
[0012] Furthermore, it is an object of the present invention to provide a device for carrying out the method.
[0013] With regard to the method, this problem is solved by a process for producing electrode mixtures from different substances, namely from active material with a mass fraction w1, optionally additives with a mass fraction w2 and binder with a mass fraction w3, where w1 and w3 are each > 0%, w2 ≥ 0% and w1, w2 and w3 are each < 100%, with the steps 1) Filling in the active material and an initial percentage p a1 the additives and / or a first percentage share p b1 the binder into a container, where 0% ≤ p α1 ≤ 100% and 0% ≤ p b1 ≤ 100%, but either 0% < p α1 or 0% < p b1 is, A) Introducing a first mechanical power P1 into the substances contained in the container, by means of shear forces or impact forces, wherein shear forces are preferred, 2) Adding a second percentage p a2 the additives and / or a further percentage p b2 the binder into the container, where 0% ≤ p a2 ≤ 100% - p α1 and 0% ≤ P b2 ≤ 100% - p b1 B) Introducing a second mechanical force P2 into the substances contained in the container, by means of shear forces or impact forces, shear forces being preferred, during a time interval T2, wherein P2 > P1, and W) Repeating steps A) and B) while binder and optionally additives are not yet completely introduced, wherein before step A) and / or between step A) and B) the step K) Adding a further percentage p ak the additives and / or a further percentage p bk the binder is added to the container, with k=3 on the first repetition and k being increased by 1 after each repetition, as well as 0%≤pak≤100%−∑i=1k−1pai and 0%≤pbk≤100%−∑i=1k−1pbi
[0014] When an electrode mixture is produced for a cathode, the active material can be, for example, lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate or other lithium or sodium metal oxides.
[0015] When an electrode mixture is produced for an anode, graphite, carbon such as activated carbon or graphene, or silicon-carbon composites can be used as the active material. The mass fraction w1 can be up to 99.9%, preferably being between 90% and 99.9%.
[0016] The additives used are mostly conductive additives, such as conductive carbon blacks, which are particularly necessary in the production of an electrode mixture for a cathode, as the active material is often poorly electrically conductive. In addition to conductive additives, electrode mixtures for anodes and cathodes may contain, for example, silicon or silicon compounds, solid electrolytes, nanoparticulate aerosils, oxalic acids, graphene, carbon nanotubes (CNTs), styrene-butadiene rubber (SBR), or conductive graphites, where preferably the mass fraction w2 ≥ 0 and < 10%. Particularly with silicon or silicon compounds or solid electrolytes, the mass fractions can also be significantly higher than 10%.
[0017] The mass fraction w3 of the binder is also between 0.1 and 10% in a preferred embodiment. Polymeric binders, such as fluorinated polymer binders like PVDF and PTFE, are particularly suitable. Alternatively, carboxymethylcellulose (CMC) could also be used as a binder. Many polymer binders, and especially PTFE, exhibit fibrillation at a specific temperature and upon the application of energy, particularly shear energy, which improves the processability of the electrode mixture.
[0018] Step A) can be performed simultaneously with step 1) or after step 1).
[0019] In step A), the components added to the container in step 1) are mixed dry, meaning no solvent, such as water, is added. This produces a largely homogeneous mixture. A particle composite structure forms, meaning the particles of the active material are surrounded by the binder and / or the (conductive) additives.
[0020] After step A), step 2) is carried out, in which further proportions of the additives and / or further proportions of the binders are added. It is not necessary for any further proportions to be added in step 2). For example, if all the proportions intended for step B) have already been added in step 1), no further proportion needs to be added in step 2). The proportions p a2 and p b2 Therefore, both can also be 0%. In other words, step 2) can be omitted.
[0021] In step B), which can be carried out either after step 2) or during step 2), a second mechanical power P2 is introduced into the mixture by means of shear forces, although impact forces could also be used instead, which is higher than the first mechanical power.
[0022] The mechanical power input in both step A) and step B) can be achieved, for example, using appropriately designed mixing tools in a mixing vessel. In step B), the rotational speed is increased compared to the speed in step A). The mechanical power inputs P1 and P2 do not need to be constant but can change during the execution of the respective step. For example, the rotational speed of the mixing tool can be kept constant during the execution of the individual steps. However, since the density and flowability of the mixture change during the execution of the individual steps, the input power also changes. It is essential, however, that the input mechanical power is greater in step B) than in step A).
[0023] Alternatively, the mechanical power could also be applied in a continuous extruder. Different mechanical power outputs during successive time intervals can then be achieved through zones of varying lengths along the extruder's mixing axis and through different geometries of mixing elements in the respective zones.
[0024] A PTFE binder, for example, initially exists as an agglomerate consisting of individual, ball-of-wool particles made of bead-like polymer fibers. In step B), due to the adhesion of the polymeric binder components to the surfaces of the active material, a thread-like / fiber-like structure forms, which develops into a network, usually a spiderweb-like network, in which the previously formed particle composite structures are embedded. In other words, the active material is coated with the binder and, if applicable, the additives.
[0025] Depending on the application, the time interval T2 of step B) can be between 1 and 90 minutes, with the duration preferably being chosen between 10 and 30 minutes.
[0026] If all desired components of the electrode mixture to be produced have already been added before step B), the process according to the invention can end here. However, if not all binders and any additives have been completely added, steps A) and B) are repeated, with further proportions of the additives and / or binders being added before step A) and / or between steps A) and B) of the repetition. Thus, subsequently added proportions of binder and / or additives also undergo steps A) and B).
[0027] In a preferred embodiment, particularly in the production of electrode mixtures for cathodes, it is provided that w2 > 0%, p a1 >0% and p b1= 0%. In other words, in step 1), only a portion of the additives or the entire amount of additives is added, and no binder at all. Binder is only added in step 2), or in step K), if steps A) and B) are repeated.
[0028] In a further preferred embodiment, at least in the last execution of step B) and preferably in all executions of step B), the power P2 is dimensioned such that in step B) the temperature of the substances taken up in the container increases and step B) is terminated as soon as the temperature of the substances taken up in the container reaches the predetermined temperature T. H reached.
[0029] The following applies to T H preferably T H > 50°C, especially preferably 50°C < T H < 80°C and ideally 50°C < T H < 70°C. The temperature T H should not be significantly exceeded.
[0030] The polymeric binder, especially a PTFE binder, typically only exhibits fibrillation at significantly higher temperatures. Surprisingly, however, this is achieved at lower temperatures through the application of mechanical energy.
[0031] If, in a specific application, it turns out that the time interval in which step B) is carried out is too short because the temperature T H Since the cooling time is reached very quickly, it can be extended by cooling the container.
[0032] In another preferred embodiment, after the last execution of step B), the following is provided: Step C) Introducing a third mechanical power P3 into the substances contained in the container by means of shear forces or impact forces, wherein shear forces are preferred, during a time interval T3, wherein P3 < P2.
[0033] If shear forces are introduced into the mixture via a mixing tool, the speed of the mixing tool can be reduced in step C).
[0034] To achieve an optimally structured dry mix, the mechanical power input in step C) can be reduced, which surprisingly improves the mix quality. It has been found that a high mechanical power input (P2) is only required at the beginning to form the network-like structure. Once fibrillation of the binder begins, the complete formation of the structure can be achieved with a lower power input.
[0035] It is generally advantageous if the time interval T3 is shorter than the time interval T2.
[0036] In a preferred embodiment, the temperature increase in step B) is used to raise the temperature to the predetermined temperature T. HThe required energy is supplied entirely or at least 80% by mechanical energy, i.e., by shear forces.
[0037] Additional external heating is not absolutely necessary.
[0038] As soon as the temperature T H Once the temperature limit is reached or exceeded, the mechanical power introduced into the mixture is reduced, so that no further significant temperature increase occurs.
[0039] Essentially, the temperature of the mixture is kept constant and the mixture is simply agitated. This completes the fibrillation process and yields a so-called structured dry mixture, which is well-suited for electrode production.
[0040] In a preferred embodiment, in step C) the power is dimensioned such that the temperature of the substances contained in the container is within an interval between 0.8 x T H and 1.1 x T Hand preferably in an interval between 0.9 x T H and 1.05 x T H is held.
[0041] In a further preferred embodiment, after the last execution of step B) and, if applicable, after step C), the following step follows: D) Cooling of the substances contained in the container to a temperature T L < T H , while a fourth mechanical power P4 is introduced into the substances contained in the container by means of shear forces, wherein P4 < P2 and preferably P4 < P3.
[0042] Thus, at the end of step C), the mixture is cooled while simultaneously being agitated to ensure thorough mixing. In principle, it would also be possible to cool a stationary, immobile mixture so that P4 = 0. Intermittent agitation and resting of the mixture during cooling is also possible. The temperature T Lis preferably < 45°, particularly preferably < 40°C and best < 35°C.
[0043] Moving the mixture during cooling significantly alters its structure, i.e., its ability to be transported and dosed.
[0044] Cooling is advantageously supported by cooling, for example, the walls of a mixing container in which the mixture is held. Alternatively and / or additionally, cooling can also be achieved using a cold gas stream and / or with the aid of liquefied gases such as nitrogen or CO2, e.g., also in the form of dry ice.
[0045] In another preferred embodiment, it is provided that after step D) the following step follows: E) Comminution of the substances contained in the container into a plurality of agglomerates by introducing a fifth mechanical power P5 with P5 >P4, wherein the agglomerates preferably have an average particle size between 0.05 and 5 mm.
[0046] This measure ensures that the so-called structured mixture is fine-grained, free-flowing, and can therefore be easily removed from a mixing container and fed into further processing for the purpose of creating the electrode.
[0047] The process according to the invention requires no solvents whatsoever.
[0048] The quality of the mixture can be further improved by carrying out the process in a protective gas atmosphere. This is particularly advantageous for step B). However, it is best if all steps of the process are carried out in a protective gas atmosphere. For example, specially conditioned dry air or an inert gas can be used as the protective gas atmosphere.
[0049] In a preferred embodiment, an electrode is produced by either rolling out an electrode mixture produced according to the described method and laminating it onto a conductive foil or pressing it onto a conductive foil.
[0050] The device for carrying out the described method comprises a mixing container with a mixing container wall and a mixing container bottom, a mixing tool arranged in the mixing container and a wall scraper, wherein the mixing tool is rotatable about a tool axis w and the mixing container is rotatable about a container axis b, wherein the tool axis w and the container axis b are spaced apart from each other.
[0051] The device can thus be used for all process steps. This allows both the mixing provided in step A) and the subsequent introduction of mechanical energy by means of shear forces in steps B) and C) within the mixing vessel to take place. In a preferred embodiment, the device includes a heating and / or cooling device for temperature control of the mixture arranged in the mixing vessel. For example, the mixing vessel can be designed with two walls, such that a temperature control fluid, i.e., a cooling or heating fluid, can be circulated between the two walls. In particular, the cooling device can significantly reduce the duration of step C) or limit the temperature of the mixture and / or the temperature rise in step A) and / or step B), which is highly advantageous.
[0052] It is particularly preferred that at least one section of the mixing vessel base is designed with a double wall in such a way that a cooling or heating fluid can be passed between the two walls of the double wall.
[0053] It has been shown that the quality of the mixture improves when, during operation of the device, the mixing tool and mixing container are rotated in the same direction around the tool axis w and the container axis b, respectively. Looking inside the mixing container at the bottom, both the mixing container and the mixing tool are thus rotated clockwise or counterclockwise. Mixing methods are known for other applications in which the mixing tool and mixing container are rotated in opposite directions around the tool axis w and the container axis b, respectively; that is, one of the elements, the mixing tool and mixing container, is rotated clockwise around its axis, while the other element is rotated counterclockwise. However, in the production of electrode mixtures, the synchronous movement of the mixing tool and mixing container has proven effective.
[0054] In a preferred embodiment, the wall scraper is also designed as a bottom scraper, so that the scraper also prevents the permanent adhesion of the mixture to the bottom of the mixing container, at least in sections.
[0055] In a further preferred embodiment, the wall scraper is in contact with the mixing vessel wall and preferably also with the mixing vessel bottom, and / or the mixing tool is in contact with the mixing vessel bottom. This prevents a thin film of the electrode mixture from forming on the wall or bottom. Since direct contact can lead to increased wear of the vessel wall, the vessel bottom, or the wall scraper and mixing tool, a preferred embodiment provides that the wall scraper and / or the mixing tool is made of a plastic, particularly preferably PTFE or polyamide, at least on a section in contact with the mixing vessel wall or bottom. The mixing tool and / or wall scraper can be made entirely of plastic, or only the section in contact with the mixing vessel wall or bottom can be made of plastic.The area in contact with the bottom of the mixing container must be made of plastic.
[0056] The mixing tool used in the device can also be optimized for producing the electrode mixture. In a preferred embodiment, the mixing tool therefore comprises a tool shaft and at least one mixing element projecting radially beyond the tool shaft. Preferably, the mixing element consists of several mixing elements spaced apart axially, or the mixing element comprises a shearing element arranged within an imaginary ring and a rolling element projecting axially beyond the shearing element. Particularly preferably, the mixing element has more than one, e.g., two, rolling elements projecting axially beyond the shearing element.
[0057] The mixing element can have radially outwardly directed knife-like elements. It is also possible to design the mixing element as a plate with external teeth.
[0058] Due to the high tool speeds and the sometimes abrasive raw material components, wear can occur on the mixing element. Therefore, in a preferred embodiment, the surfaces in contact with the mixture are specially protected against wear. This can be achieved on the mixer shafts or the stationary wall / bottom scraper, for example, by spray coatings with hard metal or ceramic, or alternatively with polyurethanes and other plastics, since copper- and zinc-free processing is particularly required for battery electrodes. The surface of the mixing elements can also be protected from wear by coating, by manufacturing them from a ceramic or a powder-metallurgical material, or by welding on wear-resistant elements. The rolling elements projecting axially from the shearing element can, for example, be made of a ceramic material or a powder-metallurgical material.consisting of a hard metal or having elements made from it that are glued or soldered onto a steel holding element.
[0059] In a further preferred embodiment, a pneumatic conveying device is provided with which the mixture can be conveyed from the mixing container. For example, the pneumatic conveying device can be designed as a suction lance that is or can be arranged inside the mixing container. It can also be integrated into the wall scraper, for example. Preferably, the suction lance terminates at the bottom of the mixing container at the radially innermost lower corner of the wall scraper or at the corner formed by the mixing container and wall scraper on the wall in the direction of flow of the mixture.
[0060] In this case, the container bottom does not need to have a drain opening. In particular, the measure in step E) makes the structured dry mix free-flowing, so that it can be easily extracted using the conveying device.
[0061] Alternatively, the bottom of the mixing container can have a closable discharge opening, and a pneumatic conveying line can be arranged beneath this opening so that any material exiting the mixing container through the discharge opening falls into the pneumatic conveying line. Alternatively, a mechanical discharge device such as a belt or vibrating trough, or simply a collection container, can be arranged beneath the discharge opening.
[0062] The pneumatic conveying system can be operated with a protective gas, preferably conveyed in a closed circuit. The protective gas provides, for example, dry air to prevent moisture from being introduced during the process. The air can be specially conditioned to achieve a very low dew point.
[0063] Further advantages, features, and applications will become clear from the following description of a preferred embodiment and the accompanying figures. These show: Fig. 1 a first embodiment of a mixer according to the invention, Fig. 2 a second embodiment of a mixer according to the invention and Fig. 3 a flowchart of the method according to the invention.
[0064] In Fig.Figure 1 shows a first embodiment of a device according to the invention for carrying out the method. The device has a container with a container wall 1 and a container bottom 2. The mixing container is rotatable about the container axis b.
[0065] A mixing tool is arranged in the mixing vessel, which can be rotated around the mixing tool axis w by means of a motor 4 and a drive belt 5. The vessel wall is double-walled and provided with a partition plate that divides the cavity formed in the double wall into an inner section 6 and an outer section 7. A temperature control fluid, e.g., a cooling fluid in the illustrated embodiment, can be introduced into the inner section 6 via the fluid supply 8, so that the cooling fluid flows in the direction of the arrow along the bottom and the wall, reaching the outer section 7, where it is then drawn off. The fluid supply 8 is designed here as a rotary feedthrough, which facilitates both the supply and discharge of the fluid and transfers the fluid from the stationary part to the rotating part of the vessel.
[0066] Alternatively, the separating plate can be omitted. In that case, a return channel should be arranged on the outer wall of the double jacket to allow the temperature control fluid to be drawn off.
[0067] The temperature control fluid allows the container, and thus the mixture contained within it, to be heated or cooled. The mixing tool 3 has several mixing elements 9, 10. The mixing elements 10, located in the upper part of the mixing tool 3, consist of a plurality of parallel circular rings, which may have recesses on their circumferential surface (not shown) to increase the shear forces applied.
[0068] The discs marked with the reference number 10 can, as in the embodiment shown in Fig. The elements shown in Figure 1 are arranged only in the upper part of the mixing tool 3. However, they can also be distributed over the entire length of the mixing tool 3. In that case, the lower mixing part 9 can be omitted.
[0069] In the embodiment shown in Fig. The lower mixing element 9 is also annular, with a series of recesses (not shown) in its circumferential surface. Upper rolling elements 11 and lower rolling elements 12 extend perpendicular to the lower mixing element 9. The lower rolling elements 12 are in contact with the bottom of the container 2 or are positioned very close to it. The distance to the bottom of the container should be less than 1 mm. The lower rolling elements 12 prevent any part of the mixture from settling at the bottom. The upper rolling elements 11 ensure that the entire mixture moves within the mixer. The upper mixing elements 10 could also be omitted. In this case, it would be advantageous for the upper rolling elements 11 to extend further upwards to reduce the area where no mixing or rolling motion takes place.
[0070] Furthermore, a wall scraper 13 is provided which is in contact with the container wall 1 and with an annular area of the container bottom 2 in order to prevent adhesion of the electrode mixture to the container wall and the bottom areas not covered by the lower rolling elements 12.
[0071] To remove the finished mixture, a suction lance 14 can be inserted into the mixing container or moved back and forth from a raised position, in which the suction lance does not immerse itself in the mixture, and from a lower position, in which the suction lance does immerse itself in the mixture.
[0072] In Fig. 1 represents the lower position, while the upper position is only indicated by dashed lines.
[0073] The finished mixture can be extracted via the suction lance 14. In this embodiment, the suction lance 14 is also double-walled, with conveying gas being supplied through the cavity of the double wall via a feeder 15. The mixture is extracted via the suction lance 14 and separated from the conveying gas in the separator or filter 16. The conveying gas can be completely reintroduced into the container via the feeder 15 and can be designed as a protective gas, e.g., as dry air, to prevent unwanted moistening of the mixture. The mixture separated from the conveying gas in the filter 16 can be discharged at the lower end of the filter via a flap or airlock system (not shown).
[0074] In Fig. Figure 2 shows a second embodiment of the device according to the invention. Where possible, the same reference numerals were used for similar elements as in the embodiment of Fig. 1 shown, used.
[0075] Therefore, only the differences to the embodiment of will be discussed below. Fig. 1 shown.
[0076] The mixing tool 3 here has significantly more of the annular mixing elements 10. The lower mixing element 9 has only downward-facing rolling elements 12. The upward-facing rolling element 11 is missing. The mixing container has an opening in its base 2, which can be opened for emptying the container by means of a spherical segment-shaped closure 17. The mixture falling from the discharge opening falls into the collection tray 18 of a conveying device, which in the illustrated embodiment is pneumatically operated. The mixture is transported by the conveying fluid along line 19 into the separator 16. The conveying fluid is then returned to the mixing container via line 20 and to the tray 18 via line 21. The system can be essentially airtight, so that a protective gas atmosphere can be maintained.
[0077] Since the bottom of the container 2 now has a drain opening, the cooling / heating system is configured somewhat differently. Temperature control fluid is supplied via the inlet and outlet 8 of the cooling system through a line 22 extending into the double wall of the bottom of the container 2, and extracted again via a line 23 extending only to just below the fluid level. The temperature control fluid is circulated by a pump, and the heat dissipated from the double wall is transferred to an external, second cooling circuit via a heat exchanger. The circulating temperature control fluid automatically maintains a constant fluid level in the double wall.
[0078] Alternatively, only the side wall of the mixing tank can be provided with a double jacket, so that the feed line 22 ends near the bottom of the tank.
[0079] In a particularly preferred embodiment of the method according to the invention, the Fig. The outlined procedure was used.
[0080] In step 1), an additive, e.g., a conductive additive intended for the production of the electrode mixture, is divided into several parts, e.g., two parts. The first part is then mixed with the active material in step A). The aim of this step is to encapsulate or coat the active material with the additive.
[0081] Only then, in step 2), is another portion (in this example, the remaining portion) of the additives added, and the active materials and the additives are mixed together in step B). This step results in better encapsulation / coating of the active materials with the additives.
[0082] If, instead, the entire quantity of additives is added simultaneously, significantly more care must be taken during the mixing step, as the additives themselves can tend to form agglomerates and separate from the active materials. If a rotating mixing tool is used, the peripheral speed of the mixing tool in step B) should be 10 to 80 m / s, preferably between 20 and 50 m / s, and ideally between 25 and 35 m / s. A lower peripheral speed can be selected in step A).
[0083] Step W checks whether all desired components have been added in full. If so, the process continues with step C. If not, and in the described example no binder has yet been added, steps K), A), K), B) are repeated until all desired components have been added in full.
[0084] In the preferred embodiment, all binder components are added in steps K), A), K), B).
[0085] In the second step A) (after step K)), the reactants of the electrode mixture are mixed together. After a further step K), a further step B) follows, in which a second mechanical power P2 is introduced into the substances held in the container by means of shear forces.
[0086] In particular, step B), but also all other steps, can be carried out, for example, using sharp-edged, rapidly rotating mixing tools or in appropriately designed mixers with such mixing tools. During this step, the applied mechanical power P2 causes heating, which can be increased by external heat energy or reduced by heat dissipation. According to the invention, the temperature reached in the mixture remains below 70 °C, as this is surprisingly sufficient to cause the polymers of the plastic binder to adhere to the particle surface and be drawn into thread-like structures, thus forming a network structure in which the previously formed particle composite structure is embedded. At 70 °C, the temperature is surprisingly significantly below the temperatures of 80–120 °C considered optimal for the fibrillation of PTFE.However, the temperature proved to be entirely sufficient for optimal adhesion of the polymers to the particle surfaces. Due to the intensive and targeted fibrillation and the associated formation of a network structure, partially lumpy to plastic, dough-like masses are created in the mixer, which resist simple emptying, subsequent material transport, and ultimately precise and uniform dosing onto the metallic foil.
[0087] To prevent the formation of fibrils or polymer fibers from being damaged and thus shortened, and to promote adhesion to particle surfaces and the linking and stretching of fibers into increasingly finer and thinner strands, the mechanical power P3 is reduced compared to the mechanical power P2 in step C). This prevents further temperature increases and comminution of the formed fibers. Cooling should also be avoided as much as possible to allow the mass to mature at a nearly constant temperature. The fibrillated mass becomes increasingly plasticized and, depending on the binder content, forms a dough-like, easily moldable mass.
[0088] If a sufficiently malleable plastic mass has already been formed in step B) that cannot be improved further, or can hardly be improved, by the maturation in step C), then step C) can be reduced to a few seconds or even skipped entirely.
[0089] Therefore, in order to transform these lumpy to plastic masses into a form that allows them to be easily removed from the mixer and transported between the mixer and the downstream processing process without problems, ideally over distances of several meters, and above all, to be easily dosed, step D) follows, in which the mixture is heated to a temperature T L The material is cooled to, for example, 45 °C, while a fourth mechanical power input, P4, is introduced, which is also lower than the second mechanical power input, P2. The fourth mechanical power input, P4, can also be chosen to be lower than the third mechanical power input, P3. If a mixing tool is used, the peripheral speed can be reduced to, for example, 5 m / s or less.
[0090] During cooling, the plastic mass solidifies and, due to the movement through the mixing tool and the rotating mixing container, is broken down into a lumpy to crumbly structure with a very broad particle size distribution. The lower the temperature of the mixture, the more crumbly it becomes. At this point, the mixture is easily transportable but, due to the broad particle size distribution, still difficult to meter, especially if uniform metering over a wider dispensing cross-section is required.
[0091] To further improve dosing capability, the mixture – after cooling – is comminuted in a further step E), which can be achieved, for example, by the mixing tool used, which is operated at a significantly increased second mixing speed, thereby introducing a fifth mechanical power P5. If a mixing tool is used, the peripheral speed of the mixing tool can be increased, for example, to 5 to 20 m / s.
[0092] This process produces agglomerates with an average particle size between 0.05 and 5 mm, making them highly suitable for gravimetric dosing across wide dosing cross-sections. This completes the electrode mixture. In step F), this mixture can be rolled out and laminated onto a conductive film to create an electrode.
[0093] The following are preferred examples of implementation: Nr. 1 2 3 4 5 6 7 Active material Lithium-nickel-manganese-cobalt oxides (NCM) NCM NCM graphite graphite NCM graphite Additive soot soot soot - silicon soot soot binder PTFE PVDF PVDF PTFE PTFE PTFE PTFE p b1 = 0%? No No Yes Yes Yes Yes Yes Step C)? possible No No possible possible possible possible Step D)? Yes No No Yes Yes Yes Yes Step E)? possible No No possible possible possible possible
[0094] In embodiment 4, no additive is used. In embodiments 1 and 2, binder is added in step A). In all other embodiments, it is added in step B), or in the last step performed, or in the first step K). Steps C) to E) are omitted in embodiments 2 and 3. While step D) is performed in embodiment 1 and embodiments 4-7, it is optional for steps C and E.
[0095] It has been shown that at least the last step (B) should be carried out for a duration of 3-30 minutes, and ideally for 3-10 minutes. The temperature at the end of step B) should be less than 70°C, and ideally between 50°C and 70°C.
[0096] Step C) is preferably performed for a duration of between 1 and 10 minutes, during which the temperature of the absorbed substances is kept nearly constant. If necessary, step C) can be performed for a longer period to noticeably improve the network structure.
[0097] During step D), cooling and simultaneous coarse grinding take place. This step should be carried out for a period of time between 3 and 90 minutes, and particularly preferably between 3 and 30 minutes, whereby the temperature drops below 45 °C, preferably below 40 °C and best of all below 35 °C.
[0098] Step E) should only be performed for a short period of time, between 5 and 60 seconds, and preferably between 5 and 30 seconds. During this time, the temperature should not rise again or should at least only change slightly. List of reference symbols 1 Container wall 1 2 Container bottom 2 3 Mixing tool 4 engine 5 drive belts 6 inner section in the double wall 7 outer section in the double wall 8 Fluid supply and discharge 9, 10 Mixing part 11, 12 rolling element 13 wall scrapers 14 suction lances 15 Feed 16 Separator 17 spherical segment-like closure 18 drip tray 19, 20, 21, 22, 23 Management
Claims
[1] Process for the production of electrode mixtures from different substances, namely from active material with a mass fraction w1, optionally additives with a mass fraction w2 and binder with a mass fraction w3, where w1 and w3 are each > 0%, w2≥ 0% and w1, w2 and w3 are each < 100%, comprising the steps 1) Filling the active material and a first percentage p a1 of the additives and / or a first percentage p b1 the binder into a container, where 0% ≤ p α1 ≤ 100% and 0% ≤ p b1 ≤ 100%, but either 0% < p α1 or 0% < p b1 is, A) introducing a first mechanical power P1 into the substances contained in the container, by means of shear forces or impact forces, with shear forces being preferred, 2) Filling a second percentage portion p a2 the additives and / or a further percentage p b2the binder in the container, where 0% ≤ p a2 ≤ 100% - p a1 and 0% ≤ p b2 ≤ 100% - p b1 B) introducing a second mechanical power P2 into the substances contained in the container, by means of shear forces or impact forces, shear forces being preferred, during a second time interval T2, in order to produce a second mixture, where P2> P1, and W) Repeat steps A) and B) as long as the binder and, if applicable, additives have not yet been completely introduced, whereby between steps A) and B) the step K) Adding a further percentage share p ak the additives and / or a further percentage p bk the binder is added to the container, with k=3 for the first repetition and k being increased by 1 after each repetition, and 0%≤pak≤100%−∑i=1k−1pai and 0%≤pbk≤100%−∑i=1k−1pbi is. [2] Method according to claim 1, characterized by that w2> 0%, p a1 >0% and p b1 = 0%. [3] Method according to one of the preceding claims, characterized by that at least during the last execution of step B) and preferably during all executions of step B) it is ensured that the temperature of the substances contained in the container reaches a predetermined temperature T H does not exceed, preferably T H > 40°C , particularly preferably 40°C < T H < 80°C and preferably 50°C < T H < 70° C. [4] Method according to one of the preceding claims, characterized bythat at least during the last execution of step B) and preferably during all executions of step B), the power P2 is dimensioned such that in step B) the temperature of the substances contained in the container increases and step B) is terminated as soon as the temperature of the substances contained in the container reaches the predetermined temperature T H reached. [5] Method according to one of the preceding claims, characterized by that after the last execution of step B) follows: Step C) Introducing a third mechanical power P3 into the substances contained in the container by means of shear forces or impact forces, with shear forces being preferred, during a third time interval T3, where P3 < P2. [6] Method according to claim 5, characterized by that T3 < T2. [7] Method according to claim 5 or 6, characterized bythat in step C) the power is dimensioned such that the temperature of the substances contained in the container is in an interval between 0.8 x T H and 1.1 x T H and preferably in an interval between 0.9 x T H and 1.05 x T H is held. [8] Method according to one of the preceding claims, characterized by that after the last execution of step B) and, if applicable, after step C) follows: D) Cooling of the substances in the container to a temperature T L < T H , while a fourth mechanical power P4 is introduced into the substances contained in the container by means of shear forces or impact forces, with shear forces being preferred, where P4 < P2 . [9] Method according to claim 8, characterized by that after step D) follows: E) Comminution of the substances contained in the container into a plurality of agglomerates by introducing a fifth mechanical power P5 with P5>P4, wherein the agglomerates preferably have an average grain size between 0.05 and 5 mm. [10] Method according to one of the preceding claims, characterized by that at least during the last execution of step B), this step B) and preferably all steps of the process are carried out in a protective gas atmosphere. [11] Method according to one of the preceding claims, characterized by that a polymer binder, preferably PTFE or PVDF, is used as the binder, with PTFE being particularly preferred. [12] A method for producing an electrode, wherein an electrode mixture is produced by a method according to any one of the preceding claims and the electrode mixture is either rolled out and laminated onto a conductive foil or pressed onto the conductive foil. [13] Device for carrying out a method according to one of claims 1 to 11, wherein the device comprises a mixing container with a mixing container wall and a mixing container bottom, a mixing tool arranged in the mixing container and a wall scraper, wherein the mixing tool is rotatable about a tool axis w and the mixing container about a container axis b, wherein the tool axis w and the container axis b are spaced apart from one another. [14] Device according to claim 13, characterized bythat a heating and / or cooling device is provided for cooling a mixture arranged in the mixing container, wherein the mixing container is preferably designed with a double wall such that a cooling or heating fluid can be passed between the two walls of the double wall, wherein particularly preferably at least one section of the mixing container base is also designed with a double wall such that a cooling or heating fluid can be passed between the two walls of the double wall. [15] Device according to claim 13 or 14, characterized by that during operation of the device the mixing tool and mixing container are rotated in the same direction around the tool axis w and the container axis b, respectively. [16] Device according to one of claims 13 to 15, characterized bythat the wall scraper is in contact with the mixing container wall and / or that the mixing tool is in contact with the mixing container bottom, wherein the wall scraper and / or the mixing tool is preferably made of a plastic, particularly preferably of PTFE or polyamide, at least on a section in contact with the mixing container wall or mixing container bottom. [17] Device according to one of claims 13 to 16, characterized by that the mixing tool has a tool shaft and at least one mixing part projecting in the radial direction beyond the tool shaft, wherein the mixing tool preferably has a plurality of mixing parts which are arranged spaced apart from one another in the axial direction and / or the mixing part consists of a shearing element arranged within an imaginary circular ring and a rolling element projecting in the radial direction beyond the shearing element. [18] Device according to one of claims 13 to 16, characterized bythat a pneumatic conveying device is provided with which the mixed material can be conveyed from the mixing container. [19] Device according to claim 18, characterized by that the pneumatic conveying device is designed as a suction lance which is or can be arranged in the interior of the mixing container, wherein the suction lance is preferably integrated into the wall scraper. [20] Device according to claim 18, characterized by that the mixing container bottom has a closable emptying opening and a pneumatic conveying line is arranged below the emptying opening in such a way that mixed material emerging from the mixing container via the emptying opening falls into the pneumatic conveying line. [21] Device according to one of claims 19 to 20, characterized by that the pneumatic conveying device is operated with protective gas, whereby the protective gas is preferably conveyed in a closed circuit. [22] Use of a device according to one of claims 13 to 21 for carrying out a method according to one of claims 1 to 11. [23] Electrode mixture produced by a process according to any one of claims 1 to 11.
Citation Information
Patent Citations
Positive electrode material for lithium ion battery, preparation method of positive electrode material and lithium ion battery
CN113764629A
Method for the continuous production of a battery electrode
DE102022105662A1
Method for producing electrode active material particle aggregates and method for producing electrode
WO2019235531A1
CN000113764629A
Mixing and or kneading machine
GB1317950A
Cited By
Mixer for producing an electrode mixture with pressure-based conveying device
DE102024132785A1
Methods for the production and conditioning of electrode mixtures and of dry electrodes from the electrode mixtures
DE102024132804A1