Material for a light-emitting element, light-emitting element and metal-organic complex

A new organic compound with integrated charge carrier transport and light emission properties simplifies the manufacturing process of organic light-emitting elements, reducing costs and enhancing efficiency and lifespan.

DE112018000989B4Active Publication Date: 2024-10-24SEMICON ENERGY LAB CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE112018000989
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-02-22
Publication Date
2024-10-24
Estimated Expiration
2038-02-22

AI Technical Summary

Technical Problem

The manufacturing process of organic light-emitting elements is complicated and costly due to the need for co-evaporation of charge carrier transport and light-emitting materials, leading to increased device size and production time.

Method used

A new material for organic light-emitting elements is developed, comprising an organic compound with a molecular weight of 1300 or less, which integrates both charge carrier transport and light emission properties, allowing for separate application through a wet process, reducing the need for co-evaporation and simplifying the manufacturing process.

Benefits of technology

This approach results in a cost-effective, efficient, and reliable production of organic light-emitting elements with improved emission efficiency and extended lifespan, while minimizing manufacturing complexity and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Material for a light-emitting element, comprising: an organic compound wherein the organic compound in a molecule has a first scaffold with a charge carrier transport property and a second scaffold with a light emission property, and where the molecular weight of the organic compound is 1300 or less, wherein the organic compound is a metal-organic complex which furthermore contains a central metal, wherein the metal-organic complex has at least two different ligands, wherein one of the two different ligands comprises the second scaffold with a light-emitting property, and the other of the two different ligands has the first scaffold with an electron transport property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] One embodiment of the present disclosure relates to a light-emitting element, a display module, a lighting module, a display device, a light-emitting device, an electronic device, and a lighting device. Note that one embodiment of the present invention is not limited to the above technical field. The technical field of one embodiment of the invention disclosed in this specification and the like relates to an article, a method, or a manufacturing method. Another embodiment of the present invention relates to a process, a machine, a product, or a composition (composition of material).Therefore, as specific examples of the technical field of an embodiment of the present invention disclosed in this specification, there can be given a semiconductor device, a display device, a liquid crystal display device, a light-emitting device, a lighting device, a power storage device, a memory device, an imaging device, a method of driving any of them, and a manufacturing method of any of them. State of the art

[0002] The implementation of light-emitting elements (organic EL elements) comprising organic compounds and utilizing electroluminescence (EL) is continuously progressing. In a basic structure of such a light-emitting element, an organic compound layer (an EL layer) containing a light-emitting material is provided between a pair of electrodes. Charge carriers are injected by applying a voltage to the element, and light emission can be obtained from the light-emitting material by utilizing the recombination energy of the charge carriers.

[0003] Because such light-emitting elements are self-luminous, they offer advantages over liquid crystal displays when used as pixels in a display, for example: high visibility and no need for backlighting, and they are suitable for flat-panel display elements. Another major advantage is that a display incorporating such light-emitting elements can be manufactured thin and lightweight. Furthermore, a very fast response time is also a feature.

[0004] In such light-emitting elements, light-emitting layers can be successively formed in a two-dimensional form, thus achieving planar light emission. This feature is difficult to achieve with point light sources, such as incandescent lamps and LEDs, or linear light sources, such as fluorescent lamps. Consequently, EL elements also have great potential as planar light sources for use in lighting devices and the like.

[0005] As described above, displays or lighting devices including light-emitting elements are suitably used for a variety of electronic devices, and research and development of light-emitting elements has progressed with a view to higher efficiency or longer life.

[0006] Organic EL devices have become widely used thanks to the advancement of so-called function-separated structures, in which different layers or materials perform different functions. Although this has led to rapid improvements in the properties of the devices, it has increased the number of stacked layers, necessitated controlling the co-evaporation rate, and significantly complicated the device manufacturing process. Consequently, this has led to an increase in the size of the manufacturing apparatus, an increase in production cycle time, and a drastic increase in manufacturing costs.

[0007] Patent Document 1 discloses a dendrimer containing iridium as the central metal and having a charge-transporting framework. Patent Document 2 relates to metal complexes and their use in electronic devices, particularly in organic electroluminescent devices. In particular, various iridium metal complexes with three ligands are disclosed, comprising, for example, a carbazole and a 2-pyridylphenyl backbone. Patent Document 3 also discloses iridium metal complexes. However, unlike Patent Document 2, these have, for example, a carbazole and an acetylacetonate backbone. Patent Documents D4 and D5 each disclose various other iridium complexes with an organic ligand backbone. [Reference][Patent document] [Patent Document 1] Japanese Patent Laid-Open No. 2003-231692 [Patent document 2] WO 2016 / 000 803 A1 [Patent Document 3] US 2013 / 0088144 A1) [Patent Document 4] US 20140209873 A1 [Patent Document 5] WO 2011032626 A1 Summary of the inventionProblem to be solved by the invention

[0008] Therefore, an object of an embodiment of the present invention is to provide a novel material for a light-emitting element. Another object of an embodiment of the present invention is to provide a material for a light-emitting element that enables the production of a light-emitting element with a simplified process. Another object of an embodiment of the present invention is to provide a material for a light-emitting element that enables the production of a light-emitting element at a lower cost. Another object of an embodiment of the present invention is to provide a material for a light-emitting element that enables the realization of a light-emitting element with advantageous emission efficiency.Another object of an embodiment of the present invention is to provide a material for a light-emitting element that enables the provision of a light-emitting element with an advantageous lifetime.

[0009] Another object of an embodiment of the present invention is to provide a light-emitting element that can be manufactured in a simplified manner. Another object of an embodiment of the present invention is to provide a light-emitting element that can be manufactured cost-effectively. Another object of an embodiment of the present invention is to provide a light-emitting element with advantageous emission efficiency. Another object of an embodiment of the present invention is to provide a light-emitting element with a long lifetime.

[0010] An object of another embodiment of the present disclosure is to provide a light-emitting device, an electronic device, and a display device, each of which is cost-effective. Another object is to provide a light-emitting device, an electronic device, and a display device, each of which is highly reliable. An object of another embodiment of the present disclosure is to provide a light-emitting device, an electronic device, and a display device, each of which has low power consumption. An object of another embodiment of the present disclosure is to provide a light-emitting device, an electronic device, and a display device, each of which has favorable display quality.

[0011] The present invention is intended to achieve at least one of the above objects. Means to solve the problem

[0012] One embodiment of the present invention is a material for a light-emitting element comprising an organic compound whose molecular weight is 1300 or less and which has, in one molecule, a first skeleton having a charge carrier transport property and a second skeleton having a light-emitting property, and wherein the organic compound is an organometallic complex further containing a central metal, wherein the organometallic complex has at least two different ligands, wherein one of the two different ligands comprises the second skeleton having a light-emitting property, and wherein the other of the two different ligands has the first skeleton having an electron transport property.

[0013] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first framework is a framework including the LUMO.

[0014] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first framework is directly bonded to the second framework.

[0015] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first skeleton and the second skeleton are connected to each other via a meta-phenylene group or a biphenyl-3,3'-diyl group.

[0016] Another embodiment of the present invention is a material for a light-emitting element comprising an organic compound, wherein the organic compound has in one molecule a first framework having a hole transport property, a second framework having an electron transport property and a third framework having a light emission property, and wherein the molecular weight of the organic compound is 1300 or less.

[0017] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first framework is a framework having the HOMO.

[0018] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the second framework is a framework having the LUMO.

[0019] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first framework and / or the second framework is / is directly bonded to the third framework.

[0020] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first skeleton and / or the second skeleton are bonded to the third skeleton via a meta-phenylene group or a biphenyl-3,3'-diyl group

[0021] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the organic compound emits phosphorescence.

[0022] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the central metal is iridium.

[0023] Another embodiment of the present invention is a material for a light-emitting element having the above structure, wherein the first skeleton having a charge carrier transport property in the organometallic complex is a diphenyltriazine skeleton.

[0024] Another embodiment of the present invention is a light-emitting element in which the material for a light-emitting element having the above structure is deposited and used by an evaporation method.

[0025] Another embodiment of the present invention is a light-emitting element in which the material for a light-emitting element having any of the above structures is deposited and used by a wet process.

[0026] Another embodiment of the present invention is a light-emitting element comprising a light-emitting layer containing a first organic compound and the above material for a light-emitting element, wherein the organic compound contained in the material for a light-emitting element is an iridium complex, and wherein the same structure as the first skeleton having a carrier transport property of the iridium complex is contained in at least a part of a skeleton contained in the first organic compound.

[0027] Another embodiment of the present invention is a light-emitting element having the above structure, wherein the light-emitting layer further contains a second organic compound.

[0028] Another embodiment of the present invention is a light-emitting element having the above structure, wherein the first skeleton is an amine skeleton.

[0029] Another embodiment of the present invention is a light-emitting element having the above structure, wherein the first skeleton is a diphenylamine skeleton.

[0030] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0031] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0032] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0033] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0034] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0035] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0036] Another embodiment of the present invention is an organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

[0037] Another embodiment of the present disclosure is a light-emitting device including a light-emitting element having the above structure and a transistor or a substrate.

[0038] Another embodiment of the present disclosure is an electronic device comprising the above light-emitting device and a sensor, a control button, a speaker, or a microphone.

[0039] Another embodiment of the present disclosure is a lighting device comprising the light-emitting device having the above structure and a housing.

[0040] Note that the light-emitting device in this specification includes an image display device including a light-emitting element. The light-emitting device may further include a module in which a light-emitting element is provided with a connector such as an anisotropic conductive film or a TCP (Tape Carrier Package), a module in which a printed circuit board is provided at the end of a TCP, or a module in which an IC (Integrated Circuit) is directly mounted on a light-emitting element by a COG (Chip-on-Glass) method. A lighting device or the like may further include the light-emitting device. The light-emitting device may also be included in a lighting device or the like.

[0041] The invention is defined by the claims. Embodiments contained in the description that are not subject to the claims serve merely to illustrate individual aspects of the invention. Effect of the invention

[0042] In one embodiment of the present invention, a novel material for a light-emitting element can be provided. In another embodiment of the present invention, a material for a light-emitting element can be provided that enables the production of a light-emitting element through a simplified process. In another embodiment of the present invention, a material for a light-emitting element can be provided that enables the production of a light-emitting element at a lower cost. In another embodiment of the present invention, a material for a light-emitting element can be provided that enables the realization of a light-emitting element with advantageous emission efficiency.In another embodiment of the present invention, a material for a light-emitting element can be provided which enables the provision of a light-emitting element having an advantageous lifetime.

[0043] In another embodiment of the present invention, a light-emitting element can be provided that can be manufactured in a simplified manner. In another embodiment of the present invention, a light-emitting element can be provided that can be manufactured cost-effectively. In another embodiment of the present invention, a light-emitting element with advantageous emission efficiency can be provided. In another embodiment of the present invention, a light-emitting element with a long lifetime can be provided.

[0044] In another embodiment of the present disclosure, a light-emitting device, an electronic device, and a display device can be provided, each of which is inexpensive. Furthermore, a light-emitting device, an electronic device, and a display device can be provided, each of which is highly reliable. In another embodiment of the present disclosure, a light-emitting device, an electronic device, and a display device can be provided, each of which has low power consumption. In another embodiment of the present disclosure, a light-emitting device, an electronic device, and a display device can be provided, each of which has favorable display quality.

[0045] It should be noted that the description of these effects does not preclude the existence of further effects. In one embodiment of the present invention, it is not necessarily required to achieve all of the effects. Further effects will become apparent from and can be derived from the explanation of the description, the drawings, the claims, and the like. Short description of the drawings [ Fig. 1] Schematic representations of materials for a light-emitting element of the present invention. [ Fig. 2] Schematic representations of light-emitting elements. [ Fig. 3] Illustrations of an example of a method for manufacturing a light-emitting element. [ Fig. 4] A diagram showing an example of a method for manufacturing a light-emitting element. [ Fig. 5] Schematic representations of an active matrix light-emitting device. [ Fig. 6] Schematic representations of active matrix light-emitting devices. [ Fig. 7] A schematic diagram of an active matrix light-emitting device. [ Fig. 8] Schematic representations of a passive matrix light-emitting device. [ Fig. 9] Illustrations of a lighting device. [ Fig. 10] Illustrations of electronic devices. [ Fig. 11] A diagram of a light source device. [ Fig. 12] A representation of a lighting device. [ Fig. 13] A representation of a lighting device. [ Fig. 14] A representation of display and lighting devices installed in a vehicle. [ Fig. 15] Representations of an electronic device. [ Fig. 16] Representations of an electronic device. [ Fig. 17] 1 H NMR spectrum of [Ir(ppy)2(Czppy)]. [ Fig. 18] Absorption spectrum and emission spectrum of [Ir(ppy)2(Czppy)]. [ Fig. 19] 1 H NMR spectrum of [Ir(ppy)(Czppy)2]. [ Fig. 20] Absorption spectrum and emission spectrum of [Ir(ppy)(Czppy)2]. [ Fig. 21] A schematic diagram of an element structure of a light-emitting element. [ Fig. 22] Luminance-current density characteristics of a light-emitting element 1, a light-emitting element 2, and a comparison light-emitting element 1. [ Fig. 23] Luminance-voltage characteristics of a light-emitting element 1, a light-emitting element 2, and a comparison light-emitting element 1. [ Fig. 24] Power efficiency-luminance characteristics of a light-emitting element 1, a light-emitting element 2, and a comparison light-emitting element 1. [ Fig. 25] Current-voltage characteristics of a light-emitting element 1, a light-emitting element 2, and a comparison light-emitting element 1. [ Fig. 26] Emission spectra of a light-emitting element 1, a light-emitting element 2 and a comparison light-emitting element 1. [ Fig. 27] Luminance-current density characteristics of a light-emitting element 3. [ Fig. 28] Power efficiency-luminance characteristics of a light-emitting element 3. [ Fig. 29] Luminance-voltage characteristics of a light-emitting element 3. [ Fig. 30] Current-voltage characteristics of a light-emitting element 3. [ Fig. 31] External quantum efficiency-luminance characteristics of a light-emitting element 3. [ Fig. 32] Emission spectrum of a light-emitting element 3. [ Fig. 33] 1 H NMR spectrum of [Ir(czppm)2(ppy)]. [ Fig. 34] Absorption spectrum and emission spectrum of [Ir(czppm)2(ppy)]. [ Fig. 35] 1 H NMR spectrum of [Ir(ppy)2(5dptznppy)]. [ Fig. 36] Absorption spectrum and emission spectrum of [Ir(ppy)2(5dptznppy)]. [ Fig. 37] 1 H NMR spectrum of [Ir(5dptznppy)2(ppy)]. [ Fig. 38] Absorption spectrum and emission spectrum of [Ir(5dptznppy)2(ppy)]. [ Fig. 39] 1 H NMR spectrum of [Ir(ppy)2(dpappy)]. [ Fig. 40] Absorption spectrum and emission spectrum of [Ir(ppy)2(dpappy)]. [ Fig. 41] 1 H NMR spectrum of [Ir(dpappy)2(ppy)]. [ Fig. 42] Absorption spectrum and emission spectrum of [Ir(dpappy)2(ppy)]. [ Fig. 43] 1 H NMR spectrum of [Ir(mdppy)2(5dptznmdppy)]. [ Fig. 44] Absorption spectrum and emission spectrum of [Ir(mdppy)2(5dptznmdppy)]. [ Fig. 45] 1 H NMR spectrum of [Ir(5dptznmdppy)2(mdppy)]. [ Fig. 46] Absorption spectrum and emission spectrum of [Ir(5dptznmdppy)2(mdppy)]. [ Fig. 47] Luminance-current density characteristics of a light-emitting element 4 and a comparison light-emitting element 2. [ Fig. 48] Power efficiency-luminance characteristics of a light-emitting element 4 and a comparison light-emitting element 2. [ Fig. 49] Luminance-voltage characteristics of a light-emitting element 4 and a reference light-emitting element 2. [ Fig. 50] Current-voltage characteristics of a light-emitting element 4 and a comparison light-emitting element 2. [ Fig. 51] External quantum efficiency-luminance characteristics of a light-emitting element 4 and a reference light-emitting element 2. [ Fig. 52] Emission spectra of a light-emitting element 4 and a comparison light-emitting element 2. [ Fig. 53] Time dependence of the normalized luminance of a light-emitting element 4 and a comparison light-emitting element 2. [ Fig. 54] Luminance-current density characteristics of a light-emitting element 5. [ Fig. 55] Power efficiency-luminance characteristics of a light-emitting element 5. [ Fig. 56] Luminance-voltage characteristics of a light-emitting element 5. [ Fig. 57] Current-voltage characteristics of a light-emitting element 5. [ Fig. 58] External quantum efficiency-luminance characteristics of a light-emitting element 5. [ Fig. 59] An emission spectrum of a light-emitting element 5. [ Fig. 60] A representation of calculation results. Embodiments of the invention

[0046] Embodiments of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to the following description, and it will be readily apparent to those skilled in the art that the forms and details can be changed in various ways without departing from the spirit of the present invention. Therefore, the present invention should not be construed as being limited to the description of the following embodiments. (Embodiment 1)

[0047] A light-emitting layer of an organic EL element is mainly formed by the following process: A charge-transporting material (host material) and a light-emitting material (guest material) are deposited by co-evaporation, while being mixed together. To perform co-evaporation, it is necessary to provide multiple evaporation sources in an evaporation chamber. From the perspective of contamination prevention, a larger manufacturing facility is required, which is a major obstacle for new companies entering the business, as a huge initial investment is required. Furthermore, a complicated and time-consuming manufacturing process directly contributes to increased manufacturing costs.

[0048] In view of this, the inventors of the present invention have succeeded in drastically reducing the cost by simplifying a manufacturing apparatus because the manufacture of an element is simplified by using a material for a light-emitting element that simultaneously has both a function of a charge carrier transport material (host material) and a function of a light-emitting material (guest material) in one molecule, whereas in a conventional method, the deposition of these materials was carried out separately.

[0049] In particular, a light-emitting material is provided which, as in Fig. 1(A), simultaneously possesses both a first framework with charge-transport properties and a second framework with light-emitting properties in one molecule. The light-emitting material, which has a molecular weight of 1300 or less, is not a polymer, but if it has solubility, it can be formed by a wet process by dissolving it in a solvent.

[0050] Since the light-emitting material simultaneously comprises both a carrier-carrying framework and a light-emitting framework in a single molecule, a light-emitting layer can be formed using only the light-emitting material. In other words, a light-emitting layer with advantageous properties can be obtained without co-evaporation. Consequently, a light-emitting element with advantageous properties can be manufactured using a manufacturing device with a relatively simple structure, thereby providing a light-emitting element that is cost-effective and has high performance.

[0051] It should be noted that the first framework with a charge carrier transport property is a Fig. 1(B) shown framework with a hole transport property or a structure as in Fig. 1(C) can be used. Although not shown, a framework with a bipolar property can also be used. Furthermore, as shown in Fig. 1(D), a molecule can contain both a framework with an electron transport property and a framework with a hole transport property.

[0052] It should be noted that in the case where the first framework having a charge carrier transport property in the light-emitting element material is the framework having a hole transport property, the framework having a hole transport property is preferably the framework having the HOMO of the material. In the case where the first framework having a charge carrier transport property in the light-emitting element material is further the framework having an electron transport property, the framework having an electron transport property is preferably the framework having the LUMO of the material.In the case where the first framework having a charge carrier transport property is both a framework having a hole transport property and a framework having an electron transport property, in the material for a light-emitting element, the HOMO is preferably located in the framework having a hole transport property and the LUMO is located in the framework having an electron transport property.

[0053] The first framework and the second framework may also be directly bonded to each other, or they may be bonded to each other via a group interposed therebetween. The group interposed therebetween is preferably a meta-phenylene group or a biphenyl-3,3'-diyl group, since it is less likely to cause a reduction in the light emission energy level or the like.

[0054] In the case where the light-emitting element material has three frameworks, that is, a framework with a hole-transport property, a framework with an electron-transport property, and a framework with a light-emitting property, a light-emitting element with high emission efficiency can be manufactured without co-evaporation using the light-emitting element material in which an exciplex is used as an energy donor, making this a preferable structure. In this case, an excited state can be formed by the interaction of the framework with a hole-transport property and the framework with an electron-transport property in one molecule. Furthermore, it is also possible for an exciplex to be formed by a framework with a hole-transport property in one molecule and a framework with an electron-transport property in another molecule.By transferring excitation energy to a scaffold with a light-emitting property in the molecule in which an excited state or an exciplex is formed, or to a scaffold with a light-emitting property of another molecule in the ground state, efficient light emission can be obtained. Since the S1 level and the T1 level of the exciplex are close to each other, provided no scaffold having a lower triplet energy is included, intersystem crossing from the T1 level to the S1 level is facilitated and the generation probability of the S1 level can be increased, thereby expected to improve the light-emitting efficiency of the fluorescent light-emitting element. Delayed fluorescence can be observed from a light-emitting element in which light emission is obtained by such a mechanism.

[0055] Of course, the present invention can also be applied to a light-emitting phosphorescent element. Typically, an organometallic complex containing a central metal such as iridium, platinum, or the like is specified as the substance that emits phosphorescence. It is possible to introduce a carrier-transporting framework and a light-emitting framework as ligands. In the case of an organometallic complex containing a plurality of ligands, a structure can be used in which the frameworks have different properties depending on the ligand (e.g., an electron-transporting property, a hole-transporting property, or a light-emitting property). Furthermore, a ligand that simultaneously has both a light-emitting framework and a charge-transporting framework can also be used.Furthermore, these structures can be combined to obtain desired properties.

[0056] In the case where the organometallic complex has two or more ligands, the following structures can be exemplified: a structure having at least two different ligands, one ligand having a framework with a light-emitting property and another ligand having a framework with a hole-transport property; a structure having at least two different ligands, one ligand having a framework with a light-emitting property and another ligand having a framework with an electron-transport property; and a structure having at least two different ligands, one ligand having a framework with a hole-transport property, another ligand having a framework with an electron-transport property, and at least one of the two ligands that are different from each other further has a framework with a light-emitting property.

[0057] Because a framework with charge-transporting properties and a framework with light-emitting properties are contained within a single molecule, it is possible to control their positional relationship. In a wet process using evaporation or a variety of materials, although the concentration of the light-emitting material (guest) and the concentration of the charge-transporting material (host) can be adjusted, it is not possible to control their positional relationship or arrangement. It is known that the energy transfer efficiency depends greatly on the shape, distance, and position of the host molecule (energy donor) and the guest molecule (energy acceptor).Since a framework with charge carrier transport properties and a framework with light emission properties are contained in one molecule, it is possible to maintain a state where the spacing, position, and positional relationship of the frameworks, which are related to energy transfer, are better. In this case, a light-emitting element with very high emission efficiency can be obtained.

[0058] Note that the molecular weight of the light-emitting element material of one embodiment of the present invention is preferably 1300 or less. When the molecular weight is 1300 or less, the light-emitting element material can be prevented from decomposing upon evaporation, and a light-emitting element with a long lifetime and high reliability can be obtained.

[0059] Furthermore, even materials that cannot be evaporated can be deposited by a wet process, typified by a spin coating method and an inkjet method, by dissolving them in a suitable solvent.

[0060] It should be noted that a light-emitting layer can also be formed by mixing such a material for a light-emitting element of one embodiment of the present invention with a generally used host material or guest material. Since the light-emitting substance of the material for a light-emitting element of one embodiment of the present invention inherently has a high carrier transport property, a high recombination efficiency can be maintained while lowering the driving voltage of the element, thereby achieving both high efficiency and a low driving voltage. It should be noted that in this case, the organic compounds such asthe host material and the guest material contained in the light-emitting layer and different from each other are preferably organic compounds having the same framework with a charge carrier transport property as the material for a light-emitting element.

[0061] In Fig. 2 shows examples of light-emitting elements using the light-emitting element material of one embodiment of the present invention. A light-emitting element using the light-emitting element material of one embodiment of the present invention is one embodiment of the present invention. The light-emitting element includes an anode 101, a cathode 102, and an EL layer 103, and the light-emitting element material described above is used in the EL layer.

[0062] The EL layer 103 includes at least one light-emitting layer 113, and the light-emitting layer 113 is formed using the light-emitting element material described above. By using the light-emitting element material, which includes both a carrier-transporting framework and a light-emitting framework in one molecule as described above, a light-emitting layer having advantageous properties can be formed without co-evaporation. This simplifies the apparatus for forming the light-emitting element, reduces initial investment, and allows the light-emitting element to be manufactured inexpensively.

[0063] It should be noted that the EL layer 103 as in Fig. 2, in addition to the light-emitting layer 113, includes a hole injection layer 111, a hole transport layer 112, an electron transport layer 114, and an electron injection layer 115; however, the structure of the light-emitting element is not limited to this, and various layers such as a hole injection layer, a hole transport layer, an electron transport layer, an electron injection layer, a charge blocking layer, an exciton blocking layer, and a charge generation layer may be used.

[0064] Next, examples of specific structures and materials of the light-emitting element described above will be described.

[0065] Two types of multilayer structure of the EL layer 103 are described in this embodiment: the structure shown in Fig. 2(A) and comprises the hole injection layer 111, the hole transport layer 112, the electron transport layer 114 and the electron injection layer 115 in addition to the light emitting layer 113; and the structure shown in Fig. 2(B) and includes the electron-transport layer 114 and a charge-generation layer 116 in addition to the hole-injection layer 111, the hole-transport layer 112, and the light-emitting layer 113. Materials for forming the electrodes and the EL layer will be described specifically below.

[0066] The anode 101 is preferably formed using a metal, an alloy, or a conductive compound having a high work function (particularly 4.0 eV or more), a combination of these, or the like. Specific examples include indium oxide-tin oxide (ITO), indium oxide-tin oxide containing silicon or silicon oxide, indium oxide-zinc oxide, and indium oxide containing tungsten oxide and zinc oxide (IWZO). Such conductive metal oxide films are generally formed by a sputtering method, but may also be formed by using a sol-gel method or the like. In one example of the formation method, an indium oxide-zinc oxide film is formed by a sputtering method using a target obtained by adding 1 wt% to 20 wt% of zinc oxide to indium oxide.Furthermore, an indium oxide film containing tungsten oxide and zinc oxide (IWZO) can be formed by a sputtering method using a target obtained by adding 0.5 wt% to 5 wt% of tungsten oxide and 0.1 wt% to 1 wt% of zinc oxide to indium oxide. Alternatively, gold (Au), platinum (Pt), nickel (Ni), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), cobalt (Co), copper (Cu), palladium (Pd), a nitride of a metal material (e.g., titanium nitride), and the like can be used. Graphene can also be used. Note that when a composite material described below is used for a layer in contact with the anode 101 in the EL layer 103, an electrode material can be selected without considering its work function.

[0067] The hole-injection layer 111 is a layer containing a substance with an acceptor property. A compound containing an electron-withdrawing group (a halogen group or a cyano group) can be used as the substance with an acceptor property. Organic acceptors, such as ethylene oxide, can be used. B. 7,7,8,8-tetracyano-2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCNQ), 1,3,4,5,7,8-hexafluorotetracyano-naphthoquinodimethane (abbreviation: F6-TCNNQ), 3,6-difluoro-2,5,7,7,8,8-hexacyanoquinodimethane, chloranil, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (abbreviation: HAT-CN) and the like, and inorganic oxides such as molybdenum oxide, vanadium oxide, ruthenium oxide, tungsten oxide, manganese oxide and the like can be used. Alternatively, phthalocyanine-based metal complexes such as phthalocyanine-based metal complexes can be used. B. Phthalocyanine (abbreviation: H2Pc), copper phthalocyanine (abbreviation: CuPc) and the like, aromatic amine compounds, such as4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), N,N'-bis{4-[bis(3-methylphenyl)amino]phenyl}-N,N'-diphenyl-(1,1'-biphenyl)-4,4'-diamine (abbreviation: DNTPD) and the like, high molecular weight compounds such as poly(3,4-ethylenedioxythiophene) / poly(styrenesulfonic acid) (PEDOT / PSS), and the like.

[0068] As an organic acceptor, a compound in which an electron-withdrawing group is bonded to a condensed aromatic ring containing a plurality of heteroatoms, such as HAT-CN, is particularly preferred due to its thermal stability. The organic compound with an acceptor property can extract electrons from an adjacent hole-transport layer (or hole-transport material) by applying an electric field.

[0069] Alternatively, a composite material in which a substance with a hole-transporting property contains an acceptor substance can be used for the hole-injection layer 111. By using a composite material in which a substance with a hole-transporting property contains an acceptor substance, a material for forming an electrode can be selected without considering its work function. In other words, in addition to a material with a high work function, a material with a low work function can also be used for the anode 101. As the acceptor substance, the above organic acceptor, a transition metal oxide, or an oxide of a metal belonging to any of Groups 4 to 8 of the Periodic Table can be used.As the oxide of a metal from Groups 4 to 8 of the Periodic Table, vanadium oxide, niobium oxide, tantalum oxide, chromium oxide, molybdenum oxide, tungsten oxide, manganese oxide, rhenium oxide, and the like are preferred due to their high electron-accepting property. Among them, molybdenum oxide is particularly preferred because of its stability in air, low hygroscopicity, and ease of handling. As the organic acceptor, 7,7,8,8-tetracyano-2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCNQ), chloranil, and the like are preferred.

[0070] The substance having a hole transport property used for the composite material preferably has a hole mobility of 10 -6 cm 2 / Vs or higher. Substances with hole-transport properties include aromatic amines such as N,N'-di(p-tolyl)-N,N'-diphenyl-p-phenylenediamine (abbreviation: DTDPPA), 4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), N,N'-bis{4-[bis(3-methylphenyl)amino]phenyl}-N,N'-diphenyl-(1,1'-biphenyl)-4,4'-diamine (abbreviation: DNTPD) and 1,3,5-tris[N-(4-diphenylaminophenyl)-N-phenylamino]benzene (abbreviation: DPA3B), carbazole derivatives such as3-[N-(9-phenylcarbazol-3-yl)-N-phenylamino]-9-phenylcarbazole (abbreviation: PCzPCA1), 3,6-bis[N-(9-phenylcarbazol-3-yl)-N-phenylamino]-9-phenylcarbazole (abbreviation: PCzPCA2), 3-[N-(1-naphthyl)-N-(9-phenylcarbazol-3-yl)amino]-9-phenylcarbazole (abbreviation: PCzPCN1), 4,4'-di(N-carbazolyl)biphenyl (abbreviation: CBP), 1,3,5-tris[4-(N-carbazolyl)phenyl]benzene (abbreviation: TCPB), 9-[4-(10-phenyl-9-anthryl)phenyl]-9H-carbazole (abbreviation: CzPA) and 1,4-bis[4-(N-carbazolyl)phenyl]-2,3,5,6-tetraphenylbenzene, as well as aromatic hydrocarbons, such as2-tert-butyl-9,10-di(2-naphthyl)anthracene (abbreviation: t-BuDNA), 2-tert-butyl-9,10-di(1-naphthyl)anthracene, 9,10-bis(3,5-diphenylphenyl)anthracene (abbreviation: DPPA), 2-tert-butyl-9,10-bis(4-phenylphenyl)anthracene (abbreviation: t-BuDBA), 9,10-di(2-naphthyl)anthracene (abbreviation: DNA), 9,10-diphenylanthracene (abbreviation: DPAnth), 2-tert-butylanthracene (abbreviation: t-BuAnth), 9,10-bis(4-methyl-1-naphthyl)anthracene (abbreviation: DMNA), 2-tert-Butyl-9,10-bis[2-(1-naphthyl)phenyl]anthracene, 9,10-bis[2-(1-naphthyl)phenyl]anthracene, 2,3,6,7-tetramethyl-9,10-di(1-naphthyl)anthracene, 2,3,6,7-Tetramethyl-9,10-di(2-naphthyl)anthracene, 9,9'-bianthryl, 10,10'-diphenyl-9,9'-bianthryl, 10,10'-bis(2-phenylphenyl)-9,9'-bianthryl, 10,10'-Bis[(2,3,4,5,6-pentaphenyl)phenyl]-9,9'-bianthryl, anthracene, tetracene, pentacene, coronene, rubrene, perylene and 2,5,8,11-Tetra(tert-butyl)perylene. The aromatic hydrocarbon may comprise a vinyl backbone.Examples of aromatic hydrocarbons with a vinyl group include 4,4'-bis(2,2-diphenylvinyl)biphenyl (abbreviation: DPVBi) and 9,10-bis[4-(2,2-diphenylvinyl)phenyl]anthracene (abbreviation: DPVPA). Alternatively, a compound with an aromatic amine skeleton, such as4,4'-Bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB), N,N'-Bis(3-methylphenyl)-N,N'-diphenyl-[1,1'-biphenyl]-4,4'-diamine (abbreviation: TPD), 4,4'-Bis[N-(spiro-9,9'-bifluoren-2-yl)-N-phenylamino]biphenyl (abbreviation: BSPB), 4-Phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-Phenyl-3'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), 4-Phenyl-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-Diphenyl-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), 4,4'-Di(1-naphthyl)-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBNBB), 9,9-Dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]fluoren-2-amine (abbreviation: PCBAF) or N-Phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]spiro-9,9'-bifluoren-2-amine (abbreviation: PCBASF), a compound with a carbazole skeleton, such as1,3-bis(N-carbazolyl)benzene (abbreviation: mCP), 4,4'-di(N-carbazolyl)biphenyl (abbreviation: CBP), 3,6-bis(3,5-diphenylphenyl)-9-phenylcarbazole (abbreviation: CzTP) or 3,3'-bis(9-phenyl-9H-carbazole) (abbreviation: PCCP), a compound with a thiophene skeleton, such as. B. 4,4',4"-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II), 2,8-diphenyl-4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]dibenzothiophene (abbreviation: DBTFLP-III) or 4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-6-phenyldibenzothiophene (abbreviation: DBTFLP-IV), or a compound with a furan skeleton, such as B. 4,4',4"-(benzene-1,3,5-triyl)tri(dibenzofuran) (abbreviation: DBF3P-II) or 4-{3-[3-(9-phenyl-9H-fluoren-9-yl)phenyl]phenyl}dibenzofuran (abbreviation: mmDBFFLBi-II).Among the above, the compound having an aromatic amine framework and the compound having a carbazole framework are preferred because of their reliability, high hole transport properties, and contribution to reducing the driving voltage.

[0071] Furthermore, the hole-injection layer 111 can also be formed by a wet process. In this case, a conductive high-molecular compound or the like to which an acid, such as an aqueous solution of poly(ethylenedioxythiophene) / poly(styrenesulfonic acid) (PEDOT / PSS), an aqueous solution of polyaniline / camphorsulfonic acid (PANI / CSA), PTPDES, Et-PTPDEK, PPBA, or polyaniline / poly(styrenesulfonic acid) (PANI / PSS), can be used.

[0072] By providing the hole-injection layer 111, a high hole-injection property can be achieved, resulting in the ability to drive a light-emitting element at a low voltage. Furthermore, the organic acceptor is easy to use because it is easily deposited by evaporation.

[0073] For the hole transport layer 112, a material may be appropriately selected from the above materials having a hole transport property or from any other materials having a hole transport property.

[0074] The light-emitting layer 113 is formed by the above-described material for a light-emitting element of one embodiment of the present invention. In a light-emitting element of one embodiment of the present invention, a light-emitting layer with advantageous properties can be formed by only the material for a light-emitting element, since a framework with a charge-carrier transport property and a host function and a framework with a light-emitting property and a light-emitting function are contained in one molecule.

[0075] As the scaffold having a charge carrier transport property and having a host function, a condensed aromatic ring scaffold, a heterocyclic scaffold, and the like, which have a higher excitation energy than the scaffold having a light-emitting property and having a light-emitting function, can be used.

[0076] Specifically, a host function can be roughly divided into a hole-transport function, an electron-transport function, and a bipolar function, each realized by different frameworks. A framework with a hole-transport function can be specified as a framework having a π-electron-rich heteroaromatic ring or an arylamine framework. More specifically, frameworks with a diphenylamine structure or frameworks with a pyrrole ring, a furan ring, a thiophene ring, and the like can be used; furthermore, these rings can also be bonded to another heteroaromatic ring. Specifically, a carbazole ring, a dibenzofuran ring, a dibenzothiophene ring, or heteroaromatic rings with such a ring structure can be specified. A framework with an electron-transport property can be specified as a framework with a π-electron-deficient heteroaromatic ring.More specifically, a pyridine ring, a diazine ring, a triazine ring, and the like can be used; further, these rings can also be bonded to another heteroaromatic ring. Specifically, a pyridine ring, a phthalazine ring, a pyrimidine ring, a pyrazine ring, a triazine ring, a quinoline ring, a quinazoline ring, or a quinoxaline ring can be used, or a heteroaromatic ring having such a ring structure can be used. For a skeleton having a bipolar property, a condensed aromatic hydrocarbon ring such as anthracene or pyrene can be appropriately used.

[0077] As a framework having a light-emitting property that has a function of emitting light, luminophores such as an anthracene framework, a pyrene framework, a perylene framework, and the like, or frameworks in which an aromatic ligand is orthometalated to iridium or platinum can be given.

[0078] In the light-emitting element material of one embodiment of the present invention, co-evaporation is unnecessary. Thus, in the case where vacuum evaporation is used, a light-emitting element can be formed without a complicated manufacturing process, thereby achieving a large-scale cost reduction effect.

[0079] It should be noted that in the case where a light-emitting layer is formed from the material for a light-emitting element using a wet process, the material for a light-emitting element is dissolved or dispersed in an appropriate liquid medium, a wet process (e.g., a spin coating method, a casting method, a die coating method, a blade coating method, a roll coating method, an inkjet method, a printing method, a spray coating method, a curtain coating method, or a Langmuir-Blodgett method) is performed to form a layer, and then the solvent is removed or baking is performed.

[0080] As the liquid medium used for the wet process, organic solvents can be used, for example, ketones such as methyl ethyl ketone and cyclohexanone, fatty acid esters such as ethyl acetate, halogenated hydrocarbons such as dichlorobenzene, aromatic hydrocarbons such as toluene, xylene, mesitylene and cyclohexylbenzene, aliphatic hydrocarbons such as cyclohexane, decalin and dodecane, dimethylformamide (DMF) and dimethyl sulfoxide (DMSO).

[0081] It should be noted that the material for a light-emitting element of one embodiment of the present invention may be mixed with a charge-transport material having a hole-transport property and / or an electron-transport property and used to adjust the charge balance in the light-emitting layer. Furthermore, the material for a light-emitting element of one embodiment of the present invention may be mixed with another light-emitting material and used. It should be noted that the charge-transport material may also be a material in which a plurality of types of substances are mixed. In the case where a mixed host material is used, a material having an electron-transport property and a material having a hole-transport property are preferably mixed.By mixing a material with an electron-transport property and a material with a hole-transport property, the transport property of the light-emitting layer 113 can be easily controlled, and control of a recombination region can be easily performed. The ratio of the content of the material with a hole-transport property to that of the material with an electron-transport property can be as follows: Material with a hole-transport property: Material with an electron-transport property = 1:9 to 9:1.

[0082] Furthermore, these mixed host materials can form an exciplex. Regarding the exciplex, a combination is selected to form an exciplex that emits light with a wavelength that overlaps those of the absorption bands on the lowest energy side of a fluorescent substance or a phosphorescent substance, thereby allowing energy to be transferred quickly and easily and efficiently achieving light emission. Such a structure is also preferred because it reduces the driving voltage.

[0083] As a material having a hole transport property in the charge carrier transport material, compounds with aromatic amine skeletons, such as B. 2-[N-(9-phenylcarbazol-3-yl)-N-phenylamino]spiro-9,9'-bifluorene (abbreviation: PCASF), 4,4',4''-tris[N-(1-naphthyl)-N-phenylamino]triphenylamine (abbreviation: 1'-TNATA), 2,7-bis[N-(4-diphenylaminophenyl)-N-phenylamino]-spiro-9,9'-bifluorene (abbreviation: DPA2SF), N,N'-bis(9-phenylcarbazol-3-yl)-N,N'-diphenylbenzene-1,3-diamine (abbreviation: PCA2B), N-(9,9-dimethyl-2-diphenylamino-9H-fluoren-7-yl)diphenylamine (abbreviation: DPNF), N,N',N''-Triphenyl-N,N',N'-tris(9-phenylcarbazol-3-yl)benzene-1,3,5-triamine (abbreviation: PCA3B), 2-[N-(4-diphenylaminophenyl)-N-phenylamino]spiro-9,9'-bifluorene (abbreviation: DPASF), N,N'-bis[4-(carbazol-9-yl)phenyl]-N,N'-diphenyl-9,9-dimethylfluorene-2,7-diamine (abbreviation: YGA2F), NPB, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-[1,1'-biphenyl]-4,4'-diamine (abbreviation: TPD), 4,4'-Bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), BSPB, 4-Phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-Phenyl-3'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), N-(9,9-Dimethyl-9H-fluoren-2-yl)-N-{9,9-dimethyl-2-[N'-phenyl-N'-(9,9-dimethyl-9H-fluoren-2-yl)amino]-9H-fluoren-7-yl}phenylamine (abbreviation: DFLADFL), PCzPCA1, 3-[N-(4-Diphenylaminophenyl)-N-phenylamino]-9-phenylcarbazole (abbreviation: PCzDPA1), 3,6-Bis[N-(4-diphenylaminophenyl)-N-phenylamino]-9-phenylcarbazole (abbreviation: PCzDPA2), DNTPD, 3,6-Bis[N-(4-diphenylaminophenyl)-N-(1-naphthyl)amino]-9-phenylcarbazole (abbreviation: PCzTPN2), PCzPCA2, 4-Phenyl-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-Diphenyl-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-Naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), 4,4'-Di(1-naphthyl)-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBNBB),3-[N-(1-Naphthyl)-N-(9-phenylcarbazol-3-yl)amino]-9-phenylcarbazole (abbreviation: PCzPCN1), 9,9-Dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]fluoren-2-amine (abbreviation: PCBAF), N-Phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]spiro-9,9'-bifluoren-2-amine (abbreviation: PCBASF), N-(4-Biphenyl)-N-(9,9-dimethyl-9H-fluoren-2-yl)-9-phenyl-9H-carbazol-3-amine (abbreviation: PCBiF) and N-(1,1'-Biphenyl-4-yl)- N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluoren-2-amine (abbreviation: PCBBiF), compounds with carbazole skeletons, such as 1,3-bis(N-carbazolyl)benzene (abbreviation: mCP), CBP, 3,6-bis(3,5-diphenylphenyl)-9-phenylcarbazole (abbreviation: CzTP) and 9-phenyl-9H-3-(9-phenyl-9H-carbazol-3-yl)carbazole (abbreviation: PCCP), compounds with thiophene skeletons, such as 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II), 2,8-Diphenyl-4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]dibenzothiophene (abbreviation: DBTFLP-III) and 4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-6-phenyldibenzothiophene (abbreviation: DBTFLP-IV) and compounds with furan skeletons, such as 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzofuran) (abbreviation: DBF3P-II) and 4-{3-[3-(9-phenyl-9H-fluoren-9-yl)phenyl]phenyl}dibenzofuran (abbreviation: mmDBFFLBi-II).

[0084] As a material having a hole transport property in the charge transport material, a metal complex such as bis(10-hydroxybenzo[h]quinolinato)beryllium(II) (abbreviation: BeBq2), bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(III) (abbreviation: BAlq), bis(8-quinolinolato)zinc(II) (abbreviation: Znq), bis[2-(2-benzoxazolyl)phenolato]zinc(II) (abbreviation: ZnPBO), bis[2-(2-benzothiazolyl)phenolato]zinc(II) (abbreviation: ZnBTZ) and the like, a heterocyclic compound having a polyazole skeleton such as2-(4-Biphenylyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (abbreviation: PBD), 3-(4-Biphenylyl)-4-phenyl-5-(4-tert-butylphenyl)-1,2,4-triazole (abbreviation: TAZ), 1,3-Bis[5-(p-tert-butylphenyl)-1,3,4-oxadiazol-2-yl]benzene (abbreviation: OXD-7), 9-[4-(5-Phenyl-1,3,4-oxadiazol-2-yl)phenyl]-9H-carbazole (abbreviation: CO11), 2,2',2''-(1,3,5-Benzenetriyl)tris(1-phenyl-1H-benzimidazole) (abbreviation: TPBI), 2-[3-(Dibenzothiophen-4-yl)phenyl]-1-phenyl-1H-benzimidazole (abbreviation: mDBTBIm-II) and the like, a heterocyclic compound having a diazine skeleton, such as2-[3-(Dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTPDBq-II), 2-[3'-(Dibenzothiophen-4-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTBPDBq-II), 2-[3'-(9H-Carbazol-9-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mCzBPDBq), 2-[4-(3,6-Diphenyl-9H-carbazol-9-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2CzPDBq-III), 7-[3-(Dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 7mDBTPDBq-II), 6-[3-(Dibenzothiophen-4-yl)phenyl]dibenzo[f, h]quinoxaline (abbreviation: 6mDBTPDBq-II), 4,6-bis[3-(phenanthren-9-yl)phenyl]pyrimidine (abbreviation: 4,6mPnP2Pm), 4,6-bis[3-(4-dibenzothienyl)phenyl]pyrimidine (abbreviation: 4,6mDBTP2Pm-II), 4,6-bis[3-(9H-carbazol-9-yl)phenyl]pyrimidine (abbreviation: 4,6mCzP2Pm) and the like, a heterocyclic compound having a triazine skeleton, such as2-{4-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn) and the like, and a heterocyclic compound having a pyridine skeleton such as 3,5-bis[3-(9H-carbazol-9-yl)phenyl]pyridine (abbreviation: 35DCzPPy), 1,3,5-tri[3-(3-pyridyl)phenyl]benzene (abbreviation: TmPyPB) and the like.

[0085] Examples of the light-emitting material include phosphorescent compounds such as: B. Tris{2-[5-(2-methylphenyl)-4-(2,6-dimethylphenyl)-4H-1,2,4-triazol-3-yl-κN2]phenyl-κC}iridium(III) (abbreviation: Ir(mpptz-dmp)3), Tris(5-methyl-3,4-diphenyl-4H-1,2,4-triazolato]iridium(III) (abbreviation: Ir(Mptz)3), Tris[4-(3-biphenyl)-5-isopropyl-3-phenyl-4H-1,2,4-triazolato]iridium(III) (Abbreviation: Ir(iPrptz-3b)3),Tris[3-(5-biphenyl)-5-isopropyl-4-phenyl-4H-1,2,4-triazolato]iridium(III) (Abbreviation: Ir(iPr5btz)3), Tris[3-methyl-1-(2-methylphenyl)-5-phenyl-1H-1,2,4-triazolato]iridium(III) (abbreviation: Ir(Mptz1-mp)3), Tris[1-methyl-5-phenyl-3-propyl-1H-1,2,4-triazolato]iridium(III) (abbreviation: Ir(Prptz1-Me)3), fac-Tris[1-(2,6-diisopropylphenyl)-2-phenyl-1H-imidazole]iridium(III) (abbreviation: Ir(iPrpmi)3), Tris[3-(2,6-dimethylphenyl)-7-methylimidazo[1,2-f]phenanthridinato]iridium(III) (abbreviation: Ir(dmpimpt-Me)3), Bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2'] iridium(III)tetrakis(1-pyrazolyl)borate (abbreviation: FIr6), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2' ]iridium(III)picolinate (abbreviation: Flrpic), bis[2-(3',5'-bistrifluoromethylphenyl)pyridinato-N,C 2' ]iridium(III)picolinate (abbreviation: Ir(CF3ppy)2(pic)), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2']iridium(III)acetylacetonate (abbreviation: FIr(acac)), tris(4-methyl-6-phenylpirimidinato)iridium(III) (abbreviation: Ir(mppm)3), tris(4-t-butyl-6-phenylpyrimidinato)iridium(III) (abbreviation: Ir(tBuppm)3), (acetylacetonato)bis(6-methyl-4-phenylpyrimidinato)iridium(III) (abbreviation: Ir(mppm)2(acac)), (acetylacetonato)bis(6-tert-butyl-4-phenylpyrimidinato)iridium(III) (abbreviation: Ir(tBuppm)2(acac)), (acetylacetonato)bis[6-(2-norbornyl)-4-phenylpyrimidinato]iridium(III) (abbreviation: Ir(nbppm)2(acac)), (acetylacetonato)bis[5-methyl-6-(2-methylphenyl)-4-phenylpyrimidinato]iridium(III) (abbreviation: Ir(mpmppm)2(acac)), (acetylacetonato)bis{4,6-dimethyl-2-[6-(2,6-dimethylphenyl)-4-pyrimidinyl-κN3]phenyl-κC}iridium(III) (abbreviation: Ir(dmppm-dmp)2(acac)), (acetylacetonato)bis(4,6-diphenylpyrimidinato)iridium(III) (abbreviation: Ir(dppm)2(acac)), (acetylacetonato)bis(3,5-dimethyl-2-phenylpyrazinato)iridium(III) (abbreviation: Ir(mppr-Me)2(acac)),(acetylacetonato)bis(5-isopropyl-3-methyl-2-phenylpyrazinato)iridium(III) (abbreviation: Ir(mppr-iPr)2(acac)), tris(2-phenylpyridinato-N,C, 2' )iridium(III) (abbreviation: Ir(ppy)3), bis(2-phenylpyridinato-N,C 2' )iridium(III)acetylacetonate (abbreviation: Ir(ppy)2(acac)), bis(benzo[h]quinolinato)iridium(III)acetylacetonate (abbreviation: Ir(bzq)2(acac)), tris(benzo[h]quinolinato)iridium(III) (abbreviation: Ir(bzq)3), tris(2-phenylquinolinato-N,C 2' )iridium(III) (abbreviation: Ir(pq)3), bis(2-phenylquinolinato-N,C 2' )iridium(III)acetylacetonate (abbreviation: Ir(pq)2(acac)), bis(2,4-diphenyl-1,3-oxazolato-N, C 2' )iridium(III)acetylacetonate (abbreviation: Ir(dpo)2(acac)), bis[2-(4'-perfluorophenylphenyl)pyridinato]iridium(III)acetylacetonate (abbreviation: Ir(p-PF-ph)2(acac)), bis(2-phenylbenzothiazolato-N, C 2')iridium(III)acetylacetonate (abbreviation: Ir(bt)2(acac)), (diisobutyrylmethanato)bis[4,6-bis(3-methylphenyl)pyrimidinato]iridium(III) (abbreviation: [Ir(5mdppm)2(dibm)]), bis[4,6-bis(3-methylphenyl)pyrimidinato](dipivaloylmethanato)iridium(III) (abbreviation: [Ir(5mdppm)2(dpm)]), bis[4,6-di(naphthalen-1-yl)pyrimidinato](dipivaloylmethanato)iridium(III) (abbreviation: [Ir(d1npm)2(dpm)]), (acetylacetonato)bis(2,3,5-triphenylpyradinato)iridium(III) (abbreviation: [ Ir(tppr)2(acac)), bis(2,3,5-triphenylpyradinato)(dipivaloylmethanato)iridium(III) (abbreviation: Ir(tppr)2(dpm)), (acetylacetonato)bis[2,3-bis(4-fluorophenyl)quinoxalinato]iridium(III) (Ir(Fdpq)2(acac)), tris(1-phenylisoquinolinato-N,C 2' )iridium(III) (abbreviation: Ir(piq)3), bis(1-phenylisoquinolinato-N,C 2')iridium(III) acetylacetonate (abbreviation: Ir(piq)2(acac)), 2,3,7,8,12,13,17,18-octaethyl-21H,23H-porphyrinplatinum(II) (abbreviation: PtOEP) and the like, thermally activated delayed fluorescence (TADF) materials such as. B. 2-(Biphenyl-4-yl)-4,6-bis(12-phenylindolo[2,3-a]carbazol-11-yl)-1,3,5-triazine (abbreviation: PIC-TRZ), 2-{4-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), 2-[4-(10H-phenoxazin-10-yl)phenyl]-4,6-diphenyl-1,3,5-triazine (abbreviation: PXZ-TRZ), 3-[4-(5-phenyl-5,10-dihydrophenazin-10-yl)phenyl]-4,5-diphenyl-1,2,4-triazole (abbreviation: PPZ-3TPT), 3-(9,9-Dimethyl-9H-acridin-10-yl)-9H-xanthen-9-one (abbreviation: ACRXTN), bis[4-(9,9-dimethyl-9,10-dihydroacridine)phenyl]sulfone (abbreviation: DMAC-DPS), 10-phenyl-10H,10'H-spiro[acridin-9,9'-anthracene]-10'-one (abbreviation: ACRSA) and the like, and fluorescent compounds such as N,N'-diphenyl-N,N'-bis[4-(9-phenyl-9H-fluoren-9-yl)phenyl]pyrene-1,6-diamine (abbreviation: 1,6FLPAPrn), N,N'-bis(3-methylphenyl)-N,N'-bis[3-(9-phenyl-9H-fluoren-9-yl)phenyl]pyrene-1,6-diamine (abbreviation: 1,6mMemFLPAPrn), N,N'-bis[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-N,N'-bis(4-tert-butylphenyl)pyrene-1,6-diamine (abbreviation: 1,6tBu-FLPAPrn), N,N'-diphenyl-N,N'-bis[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-3,8-dicyclohexylpyrene-1,6-diamine (abbreviation: ch-1,6FLPAPrn), N,N'-Bis[4-(9H-carbazol-9-yl)phenyl]-N,N'-diphenylstilbene-4,4'-diamine (abbreviation: YGA2S), 4-(9H-Carbazol-9-yl)-4'-(10-phenyl-9-anthryl)triphenylamine (abbreviation: YGAPA), 4-(9H-Carbazol-9-yl)-4'-(9,10-diphenyl-2-anthryl)triphenylamine (abbreviation: 2YGAPPA), N,9-Diphenyl-N-[4-(10-phenyl-9-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation: PCAPA), Perylene, 2,5,8,11-Tetra(tert-butyl)perylene (abbreviation: TBP), 4-(10-Phenyl-9-anthryl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBAPA), N,N''-(2-tert-butylanthracene-9,10-diyldi-4,1-phenylene)bis[N,N',N'-triphenyl-1,4-phenylenediamine] (abbreviation: DPABPA), N,9-diphenyl-N-[4-(9,10-diphenyl-2-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation: 2PCAPPA), N-[4-(9,10-diphenyl-2-anthryl)phenyl]-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPAPPA), N,N,N',N',N'',N'',N''',N'''-Octaphenyldibenzo[g,p]chrysen-2,7,10,15-tetraamine (abbreviation: DBC1), Coumarin 30, N-(9,10-diphenyl-2-anthryl)-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2PCAPA), N-[9,10-bis(1,1'-biphenyl-2-yl)-2-anthryl]-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2PCABPhA), N-(9,10-diphenyl-2-anthryl)-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPAPA), N-[9,10-bis(1,1'-biphenyl-2-yl)-2-anthryl]-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPABPhA), 9,10-bis(1,1'-biphenyl-2-yl)-N-[4-(9H-carbazol-9-yl)phenyl]-N-phenylanthracen-2-amine (abbreviation: 2YGABPhA), N,N,9-Triphenylanthracene-9-amine (abbreviation: DPhAPhA), Coumarin 6, Coumarin 545T, N,N'-Diphenylquinacridone (abbreviation: DPQd), Rubrene, 2,8-Di-tert-butyl-5,11-bis(4-tert-butylphenyl)-6,12-diphenyltetracene (abbreviation: TBRb), Nile Red, 5,12-bis(1,1'-biphenyl-4-yl)-6,11-diphenyltetracene (abbreviation: BPT), 2-(2-{2-[4-(Dimethylamino)phenyl]ethenyl}-6-methyl-4H-pyran-4-ylidene)propanedinitrile (abbreviation: DCM1), 2-{2-methyl-6-[2-(2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCM2), N,N,N',N'-Tetrakis(4-methylphenyl)tetracene-5,11-diamine (abbreviation: p-mPhTD), 7,14-diphenyl-N,N,N',N'-tetrakis(4-methylphenyl)acenaphtho[1,2-a]fluoranthene-3,10-diamine (abbreviation: p-mPhAFD), 2-{2-Isopropyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTI), 2-{2-tert-Butyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTB), 2-(2,6-Bis{2-[4-(dimethylamino)phenyl]ethenyl}-4H-pyran-4-ylidene)propanedinitrile (abbreviation: BisDCM), 2-{2,6-Bis[2-(8-methoxy-1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: BisDCJTM), 5,10,15,20-tetraphenylbisbenzo[5,6]indeno[1,2,3-cd:1',2',3'-Im]perylene and the like.

[0086] The light-emitting layer 113 having the above-described structure can be formed by co-evaporation by a vacuum evaporation method or by a gravure printing method, an offset printing method, an inkjet method, a spin coating method, a dip coating method, or the like using a mixed solution.

[0087] An electron-transport layer 114 is a layer containing a substance having an electron-transport property. Examples of the substance having an electron-transport property are a heterocyclic compound having a polyazole backbone, such as bis(10-hydroxybenzo[h]quinolinato)beryllium(II) (abbreviation: BeBq2), bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(III) (abbreviation: BAlq), bis(8-quinolinolato)zinc(II) (abbreviation: Znq), bis[2-(2-benzoxazolyl)phenolato]zinc(II) (abbreviation: ZnPBO), or bis[2-(2-benzothiazolyl)phenolato]zinc(II) (abbreviation: ZnBTZ); a heterocyclic compound having a polyazole backbone, such as2-(4-Biphenylyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (abbreviation: PBD), 3-(4-Biphenylyl)-4-phenyl-5-(4-tert-butylphenyl)-1,2,4-triazole (abbreviation: TAZ), 1,3-Bis[5-(p-tert-butylphenyl)-1,3,4-oxadiazol-2-yl]benzene (abbreviation: OXD-7), 9-[4-(5-Phenyl-1,3,4-oxadiazol-2-yl)phenyl]-9H-carbazole (abbreviation: CO11), 2,2',2''-(1,3,5-Benzenetriyl)tris(1-phenyl-1H-benzimidazole) (abbreviation: TPBI) or 2-[3-(Dibenzothiophen-4-yl)phenyl]-1-phenyl-1H-benzimidazole (abbreviation: mDBTBIm-II); a heterocyclic compound with a diazine skeleton, such as2-[3-(Dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTPDBq-II), 2-[3'-(Dibenzothiophen-4-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTBPDBq-II), 2-[3'-(9H-carbazol-9-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mCzBPDBq), 4,6-bis[3-(phenanthren-9-yl)phenyl]pyrimidine (abbreviation: 4,6mPnP2Pm) or 4,6-bis[3-(4-dibenzothienyl)phenyl]pyrimidine (abbreviation: 4,6mDBTP2Pm-II); and a heterocyclic compound having a pyridine skeleton, such as 2-[3'-(dibenzothiophen-4-yl)biphenyl-3-yl]dibenzo[f,h]quinoline (abbreviation: 2mDBTBPDBQu-II), 3,5-bis[3-(9H-carbazol-9-yl)phenyl]pyridine (abbreviation: 35DCzPPy), or 1,3,5-tri[3-(3-pyridyl)phenyl]benzene (abbreviation: TmPyPB). Among the above, the heterocyclic compound having a diazine skeleton and the heterocyclic compound having a pyridine skeleton are preferred because of their reliability.In particular, the heterocyclic compound with a diazine (pyrimidine or pyrazine) skeleton exhibits a high electron transport property and also contributes to a reduction in the driving voltage.

[0088] Between the electron-transport layer and the light-emitting layer, a layer that controls the transport of electron carriers can be further provided. This layer is a layer in which a small amount of a substance with high electron-capturing properties is added to the above material with high electron-transport properties. This layer can regulate the carrier balance by suppressing the transport of electron carriers. Such a structure is very effective in preventing problems (such as a shortened element lifetime) that occur when electrons pass through the light-emitting layer.

[0089] Further, an electron injection layer 115 may be provided between the electron transport layer 114 and the cathode 102 in contact with the cathode 102. An alkali metal, an alkaline earth metal, or a compound thereof, such as lithium fluoride (LiF), cesium fluoride (CsF), or calcium fluoride (CaF2), may be used for the electron injection layer 115. For example, a layer composed of a substance having an electron transport property and containing an alkali metal, an alkaline earth metal, or a compound thereof may be used. Furthermore, an electride may be used for the electron injection layer 115. Examples of the electride include a substance in which electrons are added at a high concentration to calcium oxide-alumina.It should be noted that a layer made of a substance having an electron-transport property and containing an alkali metal or an alkaline earth metal is preferably used as the electron-injection layer 115 because electron injection from the cathode 102 can be performed efficiently.

[0090] Instead of the electron injection layer 115, a charge generation layer 116 may further be provided ( Fig. 2(B)). The charge generation layer 116 denotes a layer that can inject holes into a layer in contact with the cathode side of this layer and electrons into a layer in contact with the anode side when a potential is applied thereto. The charge generation layer 116 includes at least one p-type layer 117. The p-type layer 117 is preferably formed using the composite material mentioned above as a material usable for the hole injection layer 111. Furthermore, the p-type layer 117 may have a structure in which a film containing the above-mentioned acceptor substance as a material contained in the composite material and a film containing a hole transport material are stacked.When a potential is applied to the p-type layer 117, electrons are injected into the electron-transport layer 114 and holes are injected into the cathode 102, thereby causing the light-emitting element to operate. At this time, if a layer containing the light-emitting element material of one embodiment of the present invention exists at the position in the electron-transport layer 114 where it is in contact with the charge generation layer 116, a decrease in luminance over the operating time of the light-emitting element can be suppressed, thus enabling a light-emitting element with a long lifetime to be obtained.

[0091] It should be noted that the charge generation layer 116 is preferably provided with an electron relay layer 118 and / or an electron injection buffer layer 119 in addition to the p-type layer 117.

[0092] The electron-transmitting layer 118 contains at least one substance with an electron-transport property and has a function of preventing interaction between the electron-injection buffer layer 119 and the p-type layer 117 to transfer electrons quickly and easily. The LUMO level of the substance with an electron-transport property contained in the electron-transmitting layer 118 is preferably between the LUMO level of an acceptor substance in the p-type layer 117 and the LUMO level of a substance contained in a layer located in the electron-transport layer 114 and in contact with the charge-generation layer 116. The energy level or LUMO level of the substance having an electron transport property used for the electron relay layer 118 is particularly preferably higher than or equal to -5.0 eV, more preferably higher than or equal to -5.0 eV and lower than or equal to -3.0 eV.It should be noted that as a substance having an electron-transport property used for the electron-transmitting layer 118, a phthalocyanine-based material or a metal complex comprising a metal-oxygen bond and an aromatic ligand is preferably used.

[0093] For the electron injection buffer layer 119, a substance having a high electron injection property, such as an alkali metal, an alkaline earth metal, a rare earth metal, or a compound thereof (an alkali metal compound (including an oxide such as lithium oxide, a halide, and a carbonate such as lithium carbonate or cesium carbonate), an alkaline earth metal compound (including an oxide, a halide, and a carbonate), or a rare earth metal compound (including an oxide, a halide, and a carbonate)) can be used.

[0094] Furthermore, in the case where the electron injection buffer layer 119 is formed to contain the substance having an electron transport property and a donor substance, an organic compound such as tetrathianaphthacene (abbreviation: TTN), nickelocene, or decamethylnickelocene can also be used as the donor substance, as well as an alkali metal, an alkaline earth metal, a rare earth metal, and a compound thereof (an alkali metal compound (including an oxide such as lithium oxide, a halide, and a carbonate such as lithium carbonate or cesium carbonate), an alkaline earth metal compound (including an oxide, a halide, and a carbonate), or a rare earth metal compound (including an oxide, a halide, and a carbonate)).Note that, as a substance having an electron-transport property, a material similar to the above-described material used for the electron-transport layer 114 may be used.

[0095] As the substance for forming the cathode 102, a metal, an alloy, or a conductive compound having a low work function (particularly, 3.8 eV or lower), a combination thereof, or the like can be used. As specific examples of such a cathode material, elements belonging to groups 1 and 2 of the periodic table, such as alkali metals such as lithium (Li) and cesium (Cs), magnesium (Mg), calcium (Ca), and strontium (Sr), alloys containing them (MgAg and AlLi), rare earth metals such as europium (Eu) and ytterbium (Yb), and alloys containing them can be given. However, when the electron injection layer is provided between the cathode 102 and the electron transport layer, various conductive materials such as silicon dioxide (SiO) and lithium hydroxide (LiO) can be used for the cathode 102. B. Al, Ag, ITO or indium oxide-tin oxide containing silicon or silicon oxide can be used regardless of the work function.These conductive materials can be deposited by a dry process, such as a vacuum evaporation method or a sputtering method, an inkjet method, a spin-coating method, or the like. They can also be formed by a wet process using a sol-gel method, or they can be formed by a wet process using a paste of a metal material.

[0096] Various methods can be used for forming the EL layer 103, regardless of whether it is a dry process or a wet process. For example, a vacuum evaporation method or a wet process (such as a spin coating method, a casting method, a die coating method, a blade coating method, a roll coating method, an inkjet method, a printing method (e.g., a gravure printing method, an offset printing method, or a screen printing method), a spray coating method, a curtain coating method, or a Langmuir-Blodgett method) can be used.

[0097] Furthermore, different deposition methods can be used to form the electrodes or layers described above.

[0098] Here, a method of forming an EL layer 786 by a droplet ejection method is described based on Fig. 3 described. Fig. 3(A) to Fig. 3(D) are cross-sectional views illustrating the process of forming the EL layer 786.

[0099] First, a conductive film 772 is formed over an insulating planarization film 770, and an insulating film 730 is formed to cover a part of the conductive film 772 (see Fig. 3(A)).

[0100] Next, a droplet 784 is ejected from a droplet ejection device 783 onto an exposed portion of the conductive film 772, that is, an opening of the insulating film 730, so that a layer 785 containing a composition is formed. The droplet 784 is a composition containing a solvent and adheres to the conductive film 772 (see Fig. 3(B)).

[0101] It should be noted that the step of ejecting the droplet 784 may be performed under reduced pressure.

[0102] Next, the solvent is removed from the composition-containing layer 785, and the resulting layer is solidified to form the EL layer 786 (see Fig. 3(C)).

[0103] It should be noted that a drying step or a heating step may be performed as a method for removing the solvent.

[0104] Next, a conductive film 788 is formed over the EL layer 786; thus, a light-emitting element 782 is formed (see Fig. 3(D)).

[0105] When the EL layer 786 is formed by a droplet ejection method as described above, the composition can be selectively ejected; thus, the waste of a material can be reduced. Furthermore, no lithography process or the like is required for molding, and therefore, the process can be simplified and cost reduction can be achieved.

[0106] It should be noted that the "droplet ejection method" described above is a general term for a method using a droplet ejection means, such as a nozzle including an outlet of a composition or a head including one or more nozzles.

[0107] Next, a droplet ejection device used in the droplet ejection method is described by Fig. 4 described. Fig. 4 is a conceptual illustration of a droplet ejection device 1400.

[0108] The droplet ejection device 1400 includes a droplet ejection means 1403. The droplet ejection means 1403 further includes a head 1405, a head 1412, and a head 1416.

[0109] The heads 1405 and 1412 are connected to a control means 1407 controlled by a computer 1410; accordingly, a preprogrammed pattern can be drawn.

[0110] Furthermore, the drawing can be performed, for example, at a time based on a mark 1411 formed over a substrate 1402. Alternatively, the reference point can be determined based on an outer edge of the substrate 1402. Here, the mark 1411 is captured by an imaging means 1404 and converted into a digital signal by an image processing means 1409. The computer 1410 detects this signal, generates a control signal, and transmits it to the control means 1407.

[0111] An image sensor or the like using a charge-coupled device (CCD) or a complementary metal oxide semiconductor (CMOS) can be used as the imaging means 1404. Note that information about a pattern to be formed over the substrate 1402 is stored in a storage medium 1408, and a control signal based on this information is transmitted to the control means 1407, so that the head 1405, the head 1412, and the head 1416 of the droplet ejection means 1403 can be separately controlled. Materials to be ejected are supplied to the head 1405, the head 1412, and the head 1416 from a material supply source 1413, a material supply source 1414, and a material supply source 1415, respectively, via pipes.

[0112] Head 1405, head 1412, and head 1416 each have an internal structure including a space, indicated by a dashed line 1406, filled with a liquid material, and a nozzle serving as an outlet. Although not shown, the internal structure of head 1412 is similar to that of head 1405. By providing the nozzles of head 1405 and head 1412 with different sizes, drawing with different materials in different widths can be performed simultaneously. Each head can eject multiple types of light-emitting materials or the like for drawing. In the case of drawing over a wide area, the same material for drawing can be ejected from a plurality of nozzles simultaneously to improve throughput.In case of using a large substrate, the head 1405, the head 1412 and the head 1416 can move the substrate in the directions of the arrows X, Y and Z shown in FIG. Fig. 4, and the area to be drawn can be freely determined. Therefore, the same pattern can be drawn multiple times on a substrate.

[0113] Furthermore, the composition ejection step may be performed under reduced pressure. During ejection, the substrate may be heated. The composition ejection is followed by a drying and / or baking step. These two steps, namely the drying and baking steps, are heat treatment steps; however, they differ in purpose, temperature, and time. The drying and baking steps are performed by laser light irradiation, rapid thermal annealing, a heating furnace, or the like under normal pressure or reduced pressure. Note that there is no particular limitation on the timing of this heat treatment and the number of heat treatments. The appropriate temperature for the drying and baking steps depends on the material of the substrate and the properties of the composition.

[0114] In the manner described above, the EL layer 786 can be formed with the droplet ejection device.

[0115] In the case where the EL layer 786 is formed by a wet process using a composition in which various organic materials or organic-inorganic halide perovskites are dissolved or dispersed in a solvent with the droplet ejection device, various organic solvents can be used to obtain a coating composition. As organic solvents that can be used for the above composition, various organic solvents such as benzene, toluene, xylene, mesitylene, tetrahydrofuran, dioxane, ethanol, methanol, n-propanol, isopropanol, n-butanol, t-butanol, acetonitrile, dimethyl sulfoxide, dimethylformamide, chloroform, methylene chloride, carbon tetrachloride, ethyl acetate, hexane, and cyclohexane can be used. In particular, a low-polar benzene derivative such as benzene derivatives such as benzene, toluene, xylene, mesitylene, tetrahydrofuran, dioxane, ethanol, methanol, n-propanol, isopropanol, n-butanol, t-butanol, acetonitrile, dimethyl sulfoxide, dimethylformamide, chloroform, methylene chloride, carbon tetrachloride, ethyl acetate, hexane, and cyclohexane can be used.Benzene, toluene, xylene, or mesitylene is preferably used because a solution with an appropriate concentration can be prepared and a material contained in an ink can be prevented from deteriorating due to oxidation or the like. Furthermore, toluene, xylene, or mesitylene is particularly preferred because a boiling point of 100°C or higher is preferable when considering film uniformity, film thickness uniformity, and the like after formation.

[0116] It should be noted that the above structure may be combined with other structures of other embodiments and this embodiment, if necessary.

[0117] In the following, an embodiment of a light-emitting element in which several light-emitting units are arranged one above the other (also referred to as a multi-layer element) is described with reference to Fig. 2(C). This light-emitting element is a light-emitting element that includes a plurality of light-emitting units between an anode and a cathode. A light-emitting unit has a structure similar to that shown in Fig. 2(A). In other words, the EL layer 103 shown in Fig. 2(A) or Fig. 2(B) is a light-emitting element comprising a single light-emitting unit, whereas the light-emitting element shown in Fig. 2(C) is a light-emitting element including a plurality of light-emitting units.

[0118] In Fig. 2(C), a first light-emitting unit 511 and a second light-emitting unit 512 are stacked between an anode 501 and a cathode 502, and a charge generation layer 513 is provided between the first light-emitting unit 511 and the second light-emitting unit 512. The anode 501 and the cathode 502 correspond to the anode 101 and the cathode 102, respectively, in Fig. 2(A), and the materials used in the description of Fig. 2(A) may be used. Furthermore, the first light-emitting unit 511 and the second light-emitting unit 512 may have the same structure or different structures.

[0119] The charge generation layer 513 has a function of injecting electrons into one of the light-emitting units and injecting holes into the other of the light-emitting units when a voltage is applied between the anode 501 and the cathode 502. That is, in Fig. 2(C) the charge generation layer 513 injects electrons into the first light-emitting unit 511 and holes into the second light-emitting unit 512 when a voltage is applied.

[0120] Preferably, the charge generation layer 513 is formed with a structure similar to that of the Fig. 2(B). A composite material of an organic compound and a metal oxide is characterized by a charge-generation property and a charge-transport property; therefore, low-voltage operation and low-current operation can be achieved. Note that in the case where a surface of a light-emitting unit on the anode side is in contact with the charge-generation layer 513, the charge-generation layer 513 can also serve as a hole-injection layer of the light-emitting unit; therefore, a hole-injection layer does not necessarily need to be provided in the light-emitting unit.

[0121] In the case where the charge generation layer 513 is further provided with the electron injection buffer layer 119, this layer serves as an electron injection layer in the light-emitting unit on the anode side; therefore, another electron injection layer does not necessarily need to be formed in the light-emitting unit.

[0122] The light-emitting element, which includes two light-emitting units, is Fig. 2(C); however, an embodiment of the present invention can be equally applied to a light-emitting element in which three or more light-emitting units are stacked one above the other. As in the above manner, when a plurality of light-emitting units separated by the charge generation layer 513 are arranged between a pair of electrodes, an element capable of emitting light with high luminance at a low current density and having a longer lifetime can be obtained. Furthermore, a light-emitting device capable of operating at a low voltage and having low power consumption can be obtained.

[0123] Furthermore, when the emission colors of the light-emitting units differ from each other, light emission of a desired color can be obtained from the light-emitting element as a whole. Furthermore, white light emission with high color rendering properties can be obtained when two light-emitting units are formed, blue fluorescence is obtained from the first light-emitting unit, and green phosphorescence and red phosphorescence are obtained from the second light-emitting unit. For example, white light emission with very high efficiency can be obtained when three light-emitting units are formed, blue fluorescence is obtained from the first light-emitting unit, yellow phosphorescence is obtained from the second light-emitting unit, and blue fluorescence is obtained from the third light-emitting unit. (Embodiment 2)

[0124] In this embodiment, a light-emitting device using the light-emitting element described in Embodiment 1 is described.

[0125] A light-emitting device of an embodiment of the present invention is described with reference to Fig. 5. It should be noted that Fig. 5(A) is a plan view illustrating the light-emitting device, and Fig. 5(B) a cross-sectional view along AB and CD in Fig. 5(A). This light-emitting device includes a driving circuit section (source line driving circuit) 601, a pixel section 602, and a driving circuit section (gate line driving circuit) 603, which control light emission of a light-emitting element and are represented by dotted lines. In addition, 604 represents a sealing substrate, 605 represents a sealing agent, and a space 607 is located in an interior part surrounded by the sealing agent 605.

[0126] Note that a lead line 608 is a line for transmitting signals input to the source line driving circuit 601 and the gate line driving circuit 603, and receives a video signal, a clock signal, a start signal, a reset signal, and the like from an FPC (flexible printed circuit) 609 serving as an external input terminal. Note that, although only the FPC is illustrated here, a printed wiring board (PWB) may be attached to this FPC. The light-emitting device in this specification includes not only the light-emitting device itself but also the one provided with the FPC or the PWB.

[0127] In the following, a cross-sectional structure is presented based on Fig. 5(B). The driver circuit portion and the pixel portion are formed over an element substrate 610. Here, the source line driver circuit 601, which is the driver circuit portion, and a pixel in the pixel portion 602 are shown.

[0128] Note that the source line driver circuit 601 is formed of a CMOS circuit combining an n-channel FET 623 and a p-channel FET 624. Furthermore, the driver circuit may be formed of various CMOS circuits, PMOS circuits, or NMOS circuits. Furthermore, in this embodiment, a driver-integrated type is described, in which the driver circuit is formed over the substrate; however, the driver circuit does not necessarily have to be formed over the substrate and may be formed externally.

[0129] Furthermore, the pixel section 602 is formed of a plurality of pixels, each including a switching FET 611, a current control FET 612, and an anode 613 electrically connected to its drain. Without being limited thereto, a pixel section may be used in which three or more FETs are combined with a capacitor.

[0130] There is no particular limitation on the type and crystallinity of a semiconductor used for the FETs; an amorphous semiconductor may be used, or a crystalline semiconductor may be used. Examples of the semiconductor used for the FETs include Group 13 semiconductors, Group 14 semiconductors, compound semiconductors, oxide semiconductors, and organic semiconductor materials. In particular, oxide semiconductors are preferably used. As examples of the oxide semiconductors, an In-Ga oxide, an In-M-Zn oxide (M is Al, Ga, Y, Zr, La, Ce, or Nd), and the like can be cited. Note that an oxide semiconductor material having an energy gap of 2 eV or more, preferably 2.5 eV or more, more preferably 3 eV or more, is preferably used, in which case the off-state current of the transistors can be reduced.

[0131] Note that an insulator 614 is formed to cover an end portion of the anode 613. Here, it can be formed using a positive photosensitive acrylic resin film.

[0132] Furthermore, to improve coverage, the insulator 614 is formed to have a curved surface with a curvature at its upper end portion or lower end portion. For example, in the case where positive photosensitive acrylic is used as the material of the insulator 614, only the upper end portion of the insulator 614 preferably has a curved surface with a radius of curvature (0.2 μm to 3 μm). Furthermore, either a negative photosensitive resin or a positive photosensitive resin can be used as the insulator 614.

[0133] An EL layer 616 and a cathode 617 are formed over the anode 613. The anode 613, the EL layer 616 and the cathode 617 correspond to the anode 101, the EL layer 103 and the cathode 102, respectively, in Fig. 2(A), or correspond to the anode 501, the EL layer (the first light-emitting unit 511, the charge generation layer 513 and the second light-emitting unit 512) and the cathode 502 in Fig. 2(C).

[0134] Furthermore, the sealing substrate 604 is fixed to the element substrate 610 with the sealant 605, so that a structure is obtained in which a light-emitting element 618 is provided in the space 607 enclosed by the element substrate 610, the sealing substrate 604, and the sealant 605. Note that the space 607 is filled with a filler; in some cases, it is filled with an inert gas (e.g., nitrogen or argon), and in other cases, it is filled with the sealant 605. Preferably, a recess is formed in the sealing substrate to provide a desiccant therein; thus, deterioration due to the influence of moisture can be suppressed.

[0135] An epoxy-based resin or a glass frit is preferably used as the sealant 605. Furthermore, these materials are preferably materials that allow as little moisture or oxygen permeation as possible. A glass substrate, a quartz substrate, or a plastic substrate formed from fiber-reinforced plastics (FRP), polyvinyl fluoride (PVF), polyester, acrylic, or the like can be used as the element substrate 610 and the seal substrate 604.

[0136] In this specification and the like, for example, a transistor and a light-emitting element can be formed using various substrates. The substrate type is not limited to any particular type. Examples of the substrate include a semiconductor substrate (e.g., a single-crystal substrate or a silicon substrate), an SOI substrate, a glass substrate, a quartz substrate, a plastic substrate, a metal substrate, a stainless steel substrate, a substrate including a stainless steel foil, a tungsten substrate, a substrate including a tungsten foil, a flexible substrate, an attachment film, paper containing a fiber material, a base material film, and the like. Examples of the glass substrate include barium borosilicate glass, aluminum borosilicate glass, soda-lime glass, and the like.For the flexible substrate, the fixing film, the base material film, and the like, the following can be exemplified: plastics, typically polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polyethersulfone (PES); a synthetic resin such as acrylic or the like; polytetrafluoroethylene (PTFE), polypropylene, polyester, polyvinyl fluoride, and polyvinyl chloride; polyamide, polyimide, aramid, epoxy; an evaporation-formed inorganic film; and paper. In particular, when transistors are manufactured using a semiconductor substrate, a single-crystal substrate, an SOI substrate, or the like, small transistors can be manufactured that have small variations in characteristics, size, shape, or the like and that have high current capability.When a circuit includes such transistors, the circuit may have lower power consumption, or the circuit may have increased integration.

[0137] Furthermore, a flexible substrate can be used as the substrate, and the transistor or light-emitting element can be formed directly over the flexible substrate. Alternatively, a separation layer can be provided between the substrate and the transistor, or between the substrate and the light-emitting element. The separation layer can be used to separate a semiconductor device partially or completely formed thereover from the substrate and transfer it to another substrate. The transistor can also be transferred to a substrate with low heat resistance or to a flexible substrate.It should be noted that for the above-described separation layer, for example, a structure in which inorganic films, namely a tungsten film and a silicon oxide film, are stacked, or a structure in which an organic resin film made of polyimide or the like is formed over a substrate can be used.

[0138] In other words, the transistor or light-emitting element may be formed using one substrate, and then the transistor or light-emitting element may be transferred to another substrate to dispose the transistor or light-emitting element over the substrate. Examples of the substrate onto which the transistor or light-emitting element is transferred include, in addition to the above-described substrates over which the transistor can be formed, a paper substrate, a cellophane substrate, an aramid film substrate, a polyimide film substrate, a stone substrate, a wood substrate, a cloth substrate (including a natural fiber (silk, cotton, or hemp), a synthetic fiber (nylon, polyurethane, or polyester), a regenerated fiber (acetate, cupro, viscose, or regenerated polyester), or the like), a leather substrate, and a rubber substrate.When such a substrate is used, formation of a transistor with excellent characteristics, formation of a transistor with low power consumption, manufacture of a durable device, imparting heat resistance, weight reduction, or reduction in thickness can be achieved.

[0139] Fig. 6 illustrates examples of a light-emitting device in which a light-emitting element that emits white light is formed and color layers (color filters) and the like are provided to enable full-color display. Fig. 6(A) illustrates a substrate 1001, a base insulating film 1002, a gate insulating film 1003, gate electrodes 1006, 1007, and 1008, a first interlayer insulating film 1020, a second interlayer insulating film 1021, a peripheral portion 1042, a pixel portion 1040, a driving circuit portion 1041, anodes 1024W, 1024R, 1024G, and 1024B of light-emitting elements, a partition wall 1025, an EL layer 1028, a cathode 1029 of the light-emitting elements, a sealing substrate 1031, a sealant 1032, and the like.

[0140] In Fig. 6(A), color layers (a red color layer 1034R, a green color layer 1034G, and a blue color layer 1034B) are further provided on a transparent base material 1033. In addition, a black layer (black matrix) 1035 may be provided. The transparent base material 1033 provided with the color layers and the black layer is positioned and fixed to the substrate 1001. Note that the color layers and the black layer are covered with a cover layer. Furthermore, Fig. 6(A) illustrates a light-emitting layer whose light is not transmitted to the outside through a color layer and a light-emitting layer whose light is transmitted to the outside through a corresponding color layer. Since light transmitted through no color layer is white, and light transmitted through a color layer is red, blue, or green, an image can be displayed using pixels of the four colors.

[0141] Fig. 6(B) illustrates an example in which the color layers (the red color layer 1034R, the green color layer 1034G, and the blue color layer 1034B) are formed between the gate insulating film 1003 and the first interlayer insulating film 1020. In this way, the color layers can be provided between the substrate 1001 and the sealing substrate 1031.

[0142] Furthermore, the light-emitting device described above is a light-emitting device having a structure in which light is taken out to the side of the substrate 1001 over which the FETs are formed (bottom emission type); however, a light-emitting device having a structure in which light is taken out to the side of the sealing substrate 1031 (top emission type) may also be used. Fig. 7 shows a cross-section of a light-emitting device with a top-emission structure. In this case, a substrate that does not transmit light can be used as the substrate 1001. The process up to the step of forming a connection electrode that connects the FET and the anode of the light-emitting element is performed in a similar manner to the light-emitting device with a bottom-emission structure. Then, a third interlayer insulating film 1037 is formed to cover an electrode 1022. This interlayer insulating film may have a planarization function. The third interlayer insulating film 1037 may be formed using a material similar to that of the second interlayer insulating film or using other different materials.

[0143] The anodes 1024W, 1024R, 1024G and 1024B of the light-emitting elements each serve as anode, but they can also serve as cathode. In the case of a Fig. In the light-emitting device with a top-emission structure shown in Figure 7, the anodes are preferably further reflective electrodes. The EL layer 1028 has a structure similar to the structure of the EL layer 103 in Fig. 2(A) or the EL layer (the first light-emitting unit 511, the second light-emitting unit 512 and the charge generation layer 513) in Fig. 2(C), where white light emission can be obtained.

[0144] With a top issue structure like in Fig. 7, sealing can be performed with the sealing substrate 1031 on which the color layers (the red color layer 1034R, the green color layer 1034G, and the blue color layer 1034B) are provided. The sealing substrate 1031 can be provided with the black layer (black matrix) 1035 positioned between pixels. The color layers (the red color layer 1034R, the green color layer 1034G, and the blue color layer 1034B) and the black layer can be covered with a cover layer. Note that a light-transmitting substrate is used as the sealing substrate 1031.

[0145] Although an example is shown here in which full-color display is performed using four colors, namely red, green, blue, and white, there is no particular limitation, and full-color display may be performed using three colors, namely red, green, and blue, or using four colors, namely red, green, blue, and yellow.

[0146] Fig. Figure 8 illustrates a passive matrix light-emitting device that is an embodiment of the present disclosure. It should be noted that Fig. 8(A) is a perspective view illustrating the light-emitting device, and Fig. 8(B) is a cross-sectional view obtained by cutting Fig. 8(A) along XY. In Fig. 8, an EL layer 955 is provided above a substrate 951 between an electrode 952 and an electrode 956. One end portion of the electrode 952 is covered with an insulating layer 953. Further, a partition layer 954 is provided over the insulating layer 953. The sidewalls of the partition layer 954 are inclined such that the distance between one sidewall and the other sidewall decreases toward the surface of the substrate. That is, a cross-section taken toward the short side of the partition layer 954 is trapezoidal, and the lower side (the side facing the direction equal to the surface direction of the insulating layer 953 and in contact with the insulating layer 953) is shorter than the upper side (the side facing the direction equal to the surface direction of the insulating layer 953 and not in contact with the insulating layer 953).The partition layer 954 provided in this way can prevent defects of the light-emitting element due to static electricity or the like.

[0147] In the light-emitting device described above, many very small light-emitting elements arranged in a matrix can be separately controlled by the FETs formed in the pixel portion, thus the light-emitting device can be advantageously used as a display device that displays an image. < <beleuchtungsvorrichtung>>

[0148] A lighting device which is an embodiment of the present disclosure is described with reference to Fig. 9 described. Fig. 9(B) is a plan view of the lighting device, and Fig. 9(A) is a cross-sectional view along ef in Fig. 9(B).

[0149] In the lighting device, an anode 401 is formed over a substrate 400, which serves as a support and has light transmission. The anode 401 corresponds to the anode 101 in Fig. 2(A) and Fig. 2(B). When light is extracted via the anode 401 side, the anode 401 is formed using a material having a light transmittance property.

[0150] A contact pad 412 for applying a voltage to a cathode 404 is provided above the substrate 400.

[0151] An EL layer 403 is formed over the anode 401. The EL layer 403 corresponds, for example, to the EL layer 103 in Fig. 2(A) and Fig. 2(B). It should be noted that for their structures, reference should be made to the corresponding description.

[0152] The cathode 404 is formed such that it covers the EL layer 403. The cathode 404 corresponds to the cathode 102 in Fig. 2(A). The cathode 404 is formed using a material with a high reflectance when light is extracted via the anode 401 side. The cathode 404 is connected to the pad 412, thereby applying a voltage.

[0153] The anode 401, the EL layer 403, and the cathode 404 form a light-emitting element. The light-emitting element and a sealing substrate 407 are bonded together with sealants 405 and 406 for sealing, thereby completing the lighting device. Only one of the sealants 405 and 406 may be used. The inner sealant 406 (not shown) Fig. A desiccant can also be added (as shown in Figure 9(B)). Consequently, moisture can be adsorbed, resulting in improved reliability.

[0154] If parts of the contact pad 412 and the anode 401 extend outside the sealing means 405 and 406, the protruding parts can serve as external input terminals. Furthermore, an IC chip 420 or the like mounted with a converter or the like can be provided thereon. <<Elektronische Geräte> >

[0155] Examples of an electronic device embodying the present disclosure will be described. Examples of the electronic device include a television (also referred to as a television or television receiver), a monitor of a computer or the like, a digital camera, a digital video camera, a digital photo frame, a mobile phone (also referred to as a cellular phone or mobile phone device), a portable game console, a portable information terminal, an audio playback device, and a large-scale gaming machine such as a pinball machine. Specific examples of these electronic devices are shown below.

[0156] Fig. 10(A) shows an example of a television set. In the television set, a display section 7103 is installed in a housing 7101. Furthermore, the housing 7101 is supported by a stand 7105. Images can be displayed on the display section 7103, and light-emitting elements are arranged in a matrix in the display section 7103.

[0157] The television can be operated using a control switch on the housing 7101 or a separate remote control 7110. Control buttons 7109 on the remote control 7110 can control the TV channels and volume, and images displayed on the display section 7103. Furthermore, the remote control 7110 can be provided with a display section 7107 for displaying information output from the remote control 7110.

[0158] It should be noted that the television is equipped with a receiver, a modem, and the like. The receiver can receive general television broadcasts. Furthermore, when connected to a communications network via the modem, either wirelessly or non-wirelessly, unidirectional (from a transmitter to a receiver) or bidirectional (e.g., between a transmitter and a receiver or between receivers) data communication can be performed.

[0159] Fig. 10(B1) illustrates a computer including a main body 7201, a housing 7202, a display section 7203, a keyboard 7204, an external connection terminal 7205, a pointing device 7206, and the like. Note that this computer is manufactured by arranging light-emitting elements in a matrix and using them for the display section 7203. The computer in Fig. 10(B1) can also be a Fig. 10(B2) shown structure. The computer in Fig. 10(B2) is provided with a second display section 7210 instead of the keyboard 7204 and the pointing device 7206. The second display section 7210 is a touchscreen, and an input operation can be performed by controlling the input display displayed on the second display section 7210 with a finger or an associated stylus. Furthermore, the second display section 7210 can also display images other than the input display. The display section 7203 may also be a touchscreen. By connecting the two displays with a hinge, problems can be prevented, for example, the displays can be prevented from cracking or being damaged during storage or carrying of the computer.

[0160] Fig. 10(C) and Fig. 10(D) illustrate examples of a portable information terminal. The portable information terminal is provided with a display section 7402 installed in a case 7401, as well as an operation button 7403, an external connection terminal 7404, a speaker 7405, a microphone 7406, and the like. Note that the portable information terminal includes the display section 7402, which is formed by arranging light-emitting elements in a matrix.

[0161] The Fig. 10(C) and Fig. The portable information terminals shown in Figure 10(D) may also have a structure in which information can be input by touching the display portion 7402 with a finger or the like. In this case, operations such as making a call and writing an email can be performed by touching the display portion 7402 with a finger or the like.

[0162] The screen of the display section 7402 mainly has three modes. The first mode is a display mode, which mainly displays images. The second mode is an input mode, which mainly inputs information such as text. The third mode is a display and input mode, which combines two modes: the display mode and the input mode.

[0163] For example, in the case of making a call or writing an e-mail, the display section 7402 is set to a text input mode in which mainly characters are input so that the characters displayed on the screen can be input. In this case, a keyboard or number keys are preferably displayed on almost the entire screen of the display section 7402.

[0164] Further, when a detecting device including a sensor for detecting inclination, such as a gyroscope sensor or an acceleration sensor, is provided within the portable information terminal, the display on the screen of the display section 7402 can be automatically switched by determining the orientation of the portable information terminal (vertical or horizontal).

[0165] Furthermore, the screen modes are switched by touching the display section 7402 or by operating the operation knob 7403 of the housing 7401. Alternatively, switching can be performed depending on the type of images displayed on the display section 7402. For example, if a signal of an image displayed on the display section is moving image data, switching to the display mode is performed. If it is text data, switching to the input mode is performed.

[0166] Furthermore, in the case where there is no input by touching the display section 7402 for a certain time in the input mode while detecting a signal detected by an optical sensor in the display section 7402, the screen mode can be controlled to switch from the input mode to the display mode.

[0167] The display section 7402 can also serve as an image sensor. For example, when the display section 7402 is touched with a palm or finger, an image of the palm print, fingerprint, or the like is captured, thereby enabling personal authentication. Furthermore, an image of a finger vein, a palm vein, or the like can be captured by using a backlight emitting near-infrared light or a scanning light source emitting near-infrared light for the display section.

[0168] It should be noted that in the above electronic devices, a combination of the structures described in this specification may be used as needed.

[0169] Furthermore, the light-emitting element of one embodiment of the present invention is preferably used for the display section. The light-emitting element can be a light-emitting element with favorable emission efficiency. In addition, a light-emitting element with a low drive voltage can be obtained. Therefore, the electronic device incorporating the light-emitting element of one embodiment of the present invention can be a low-power electronic device.

[0170] Fig. Figure 11 shows an example of a liquid crystal display device in which a light-emitting element is used for a backlight. Fig. The liquid crystal display device shown in Figure 11 includes a housing 901, a liquid crystal layer 902, a backlight unit 903, and a case 904. The liquid crystal layer 902 is connected to a driver IC 905. The light-emitting element is used for the backlight unit 903, to which a current is supplied via a terminal 906.

[0171] The light-emitting element of one embodiment of the present invention is preferably used as the light-emitting element. By using the light-emitting element for the backlight of the liquid crystal display device, a backlight with reduced power consumption can be achieved.

[0172] Fig. 12 illustrates an example of a table lamp that is an embodiment of the present disclosure. Fig. The table lamp shown in Fig. 12 includes a housing 2001 and a light source 2002, and a lighting device using a light-emitting element is used as the light source 2002.

[0173] Fig. 13 illustrates an example of an indoor lighting device 3001. The light-emitting element of one embodiment of the present invention is preferably used for the lighting device 3001.

[0174] Fig. 14 illustrates a car that is an embodiment of the present disclosure. In the car, light-emitting elements are mounted on a windshield and a dashboard. Display regions 5000 to 5005 are display regions provided using light-emitting elements. Preferably, the light-emitting element of one embodiment of the present invention is used in a car because it can reduce the power consumption of the display regions 5000 to 5005.

[0175] The display portion 5000 and the display portion 5001 are display devices provided in the car windshield and employing light-emitting elements. When light-transmitting electrodes are formed as the first and second electrodes of these light-emitting elements, so-called see-through display devices through which the opposite side can be seen can be obtained. A see-through display can be provided without obstructing the view even when mounted on the car windshield. Note that when a driving transistor or the like is provided, it is preferable to use a light-transmitting transistor such as an organic transistor containing an organic semiconductor material or a transistor employing an oxide semiconductor.

[0176] The display portion 5002 is a display device provided in a pillar portion and employing a light-emitting element. The display portion 5002 can compensate for the view obstructed by the pillar by displaying an image captured by an imaging means provided in the vehicle body. Similarly, the display portion 5003 in the instrument panel can supplement the view obstructed by the vehicle body by displaying an image captured by an imaging unit outside the vehicle body, eliminating blind spots and improving safety. By displaying images that compensate for non-visible areas, safety can be determined easily and conveniently.

[0177] Display areas 5004 and 5005 can provide various information, such as navigation information, a speedometer, a tachometer, a mileage reading, a fuel gauge, a gearshift indicator, and an air conditioning setting. The content or layout of the display can be changed according to a user's preference. Note that such information can also be displayed on display areas 5000 to 5003. Display areas 5000 to 5005 can also be used as lighting devices.

[0178] Fig. 15(A) and Fig. 15(B) shows an example of a bi-folding tablet computer. Fig. 15A illustrates the tablet computer unfolded. The tablet computer includes a case 9630, a display section 9631a, a display section 9631b, a display mode switch 9034, a power switch 9035, a power-saving mode switch 9036, a clasp 9033, and an operation switch 9038. In the tablet computer, a light-emitting device including the light-emitting element of one embodiment of the present invention is used for the display section 9631a and / or the display section 9631b.

[0179] A portion of the display section 9631a may serve as a touchscreen area 9632a, and data can be input when a displayed operation button 9637 is touched. Note that the structure of the display section 9631a is not limited to the exemplary structure in which half of the area has only a display function and the other half has a touchscreen function. A structure in which the entire area of ​​the display section 9631a has a touchscreen function may also be adopted. For example, the entire area of ​​the display section 9631a may display keyboard buttons to serve as a touchscreen, and the display section 9631b may be used as a display screen.

[0180] As with the display section 9631a, a part of the display section 9631b may be a touchscreen area 9632b. When a keyboard display / hide toggle button 9639 on the touchscreen is touched with a finger, a stylus, or the like, keyboard buttons may be displayed on the display section 9631b.

[0181] In addition, touch input can be performed on the touchscreen area 9632a and the touchscreen area 9632b simultaneously.

[0182] The display mode switch 9034 can further select the orientation of a display between portrait, landscape, and the like, the orientation of a display between monochrome and color, or the like. The power-saving mode switch 9036 can optimize the luminance of the display according to the amount of external light during use, which is detected by an optical sensor integrated in the tablet computer. In addition to the optical sensor, another detection device, such as a sensor for detecting inclination, e.g., a gyroscope sensor or an acceleration sensor, can be integrated in the tablet computer.

[0183] Although Fig. While FIG. 15(A) illustrates an example in which the display portion 9631a and the display portion 9631b have the same display area, an embodiment of the present disclosure is not limited to this example. The display portion 9631a and the display portion 9631b may have different areas or different display qualities. For example, one of them may be a display screen capable of performing a higher-resolution display compared to the other.

[0184] Fig. 15(B) illustrates a folded state. In this embodiment, an example is shown in which the tablet computer includes the case 9630, a solar cell 9633, a charge / discharge control circuit 9634, a battery 9635, and a DC-DC converter 9636. It should be noted that Fig. 15(B) exemplifies a structure in which the charge / discharge control circuit 9634 includes the battery 9635 and the DC-DC converter 9636.

[0185] Note that since the tablet computer can be folded in two, the casing 9630 can be placed in the folded state when the tablet computer is not in use. Therefore, the display portion 9631a and the display portion 9631b can be protected; consequently, a tablet computer with excellent durability and reliability for long-term use can be provided.

[0186] In addition, the Fig. 15(A) and Fig. 15(B) may have a function of displaying various information (e.g., a still image, a moving image, and a text image), a function of displaying a calendar, a date, a time, or the like on the display portion, a touch input function of operating or editing information displayed on the display portion by touch input, a function of controlling processing by various types of software (programs), and the like.

[0187] The solar cell 9633, which is attached to a surface of the tablet computer, can supply power to the touchscreen, the display section, an image signal processing section, or the like. Note that the solar cell 9633 is preferably provided on one or two surfaces of the case 9630, in which case the battery 9635 can be charged efficiently.

[0188] Furthermore, the structure and working methods of the Fig. 15(B) shown charge / discharge control circuit 9634 by means of a block diagram in Fig. 15(C). Fig. 15(C) illustrates the solar cell 9633, the battery 9635, the DC-DC converter 9636, a converter 9638, switches SW1 to SW3 and the display section 9631. The battery 9635, the DC-DC converter 9636, the converter 9638 and the switches SW1 to SW3 correspond to the Fig. 11(B) shown charge / discharge control circuit 9634.

[0189] First, an example of the operation in the case where power is generated by the solar cell 9633 using external light will be described. The voltage of the power generated by the solar cell is increased or decreased by the DC-DC converter 9636 to become a voltage for charging the battery 9635. Then, when the power charged by the solar cell 9633 is used to drive the display section 9631, the switch SW1 is turned on, and the voltage is increased or decreased by the converter 9638 to a voltage required for the display section 9631. In addition, when no display is performed on the display section 9631, the battery 9635 can be charged by turning off SW1 and turning on SW2.

[0190] Note that although the solar cell 9633 is described as an example of a power generation means, there is no particular limitation on the power generation means, and the battery 9635 can also be charged by another power generation means, such as a piezoelectric element (piezo element) or a thermoelectric conversion element (Peltier element). Charging can also be performed by a non-contact power transmission module that wirelessly (contactlessly) transmits and receives power, or by a combination with another charging means; the power generation means need not necessarily be provided.

[0191] An embodiment of the present disclosure is not limited to the tablet computer with the Fig. 15 as long as the display section 9631 is provided.

[0192] Fig. 16(A) to Fig. 16(C) illustrate a foldable portable information terminal 9310. Fig. 16(A) illustrates the portable information terminal 9310 in an unfolded state. Fig. 16(B) illustrates the portable information terminal 9310 in a state where it is changed from the unfolded state to a folded state or vice versa. Fig. 16(C) illustrates the portable information terminal 9310 in the folded state. The portable information terminal 9310 is highly portable in the folded state and highly searchable in the unfolded state due to a seamless large display area.

[0193] A display screen 9311 is supported by three housings 9315 connected to each other by hinges 9313. Note that the display screen 9311 may be a touchscreen (an input / output device) on which a touch sensor (an input device) is mounted. Furthermore, the shape of the portable information terminal 9310 can be reversibly changed from the unfolded state to the folded state by folding the display screen 9311 between two housings 9315 at the hinges 9313. The light-emitting device of one embodiment of the present disclosure can be used for the display screen 9311. A display area 9312 of the display screen 9311 is a display area positioned on a side surface of the portable information terminal 9310 in the folded state.On the display area 9312, information icons, shortcuts of frequently used applications or programs, and the like can be displayed, and confirmation of information and launching of applications and the like can be easily performed. [Example 1]<<Synthesebeispiel 1> >

[0194] In this example, a synthesis method of a material for a light-emitting element of one embodiment of the present invention will be described in detail. Specifically, this example describes a synthesis example of [2-{(9H-carbazol-9-yl)-2-pyridinyl-κN}phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-rC]iridium(III) (abbreviation: [Ir(ppy)2(Czppy)]), which is an organometallic complex containing iridium as the central metal and having a ligand having a first framework with a hole-transport property and a second framework with a light-emitting property. A structure of [Ir(ppy)2(Czppy)] is shown below.

[0195] It should be noted that in [Ir(ppy)2(Czppy)], the carbazole framework corresponds to the first framework with a hole transport property and the 2-pyridylphenyl framework corresponds to the second framework with a light emission property. <Schritt 1: Synthese von 4-Chlor-2-phenylpryridin>

[0196] First, 12 g of 2,4-dichloropyridine, 9.9 g of a phenylboronic acid, 34 g of potassium carbonate, 400 mL of DME, and 240 mL of water were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Furthermore, 0.94 g of tetrakis(triphenylphosphine)palladium(0) was added, followed by microwave irradiation (2.45 GHz, 400 W) for 2 hours. After the reaction, extraction with ethyl acetate was performed. Purification was then performed by silica gel column chromatography using dichloromethane as the eluent to obtain 12 g of the target substance (a yellow oily substance in 80% yield). A synthesis scheme of Step 1 is shown below at (a-1). <Schritt 2: Synthese von 9-(2-Phenylpyridin-4-yl)-9H-carbazol (Abkürzung: HCzppy)>

[0197] Subsequently, 12 g of 4-chloro-2-phenylpyridine obtained in step 1, 13 g of 9H-carbazole, and 11 g of sodium tert-butoxide (abbreviation: tert-BuONa) were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Furthermore, 280 ml of toluene, 1.3 g of tri-tert-butylphosphine, and 3.0 g of tris(dibenzylideneacetone)dipalladium(0) (abbreviation: Pd2(dba)3) were added, and the mixture was heated and stirred at 120 °C for 5 hours. The resulting reactant was filtered, and the solvent of the filtrate was distilled off, followed by purification by silica gel column chromatography using dichloromethane and hexane in a 1:1 ratio as the eluent to obtain 11 g of the target substance (a yellow oily substance in a yield of 53%). A synthesis scheme of step 2 is shown below in (a-2). <Schritt 3: Synthese von [Ir(ppy)2(Czppy)]>

[0198] Next, 2.8 g of di-μ-chloro-tetrakis{2-[2-pyridinyl-κN]phenyl-κC}diiridium(III) (abbreviation: [Ir(ppy)2Cl)]2) and 200 ml of dichloromethane were added to a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 2.0 g of silver triflate and 40 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid.

[0199] Subsequently, 2.2 g of HCzppy obtained in step 2, 50 ml of 2-ethoxyethanol (abbreviation: 2-EE), and 50 ml of N,N-dimethylformamide (abbreviation: DMF) were added to the solid, and the mixture was refluxed for 17 hours under a nitrogen atmosphere. The resulting mixture was concentrated and purified by silica gel column chromatography using dichloromethane and hexane in a ratio of 1:1 as the eluent, gradually reducing the hexane content during the purification and finally using only dichloromethane as the eluent. This was followed by further purification by silica gel column chromatography using chloroform and hexane in a ratio of 3:2 as the eluent.The obtained solution was concentrated, followed by recrystallization with a mixed solvent of dichloromethane and methanol to obtain the organometallic complex of one embodiment of the present invention, [Ir(ppy)2(Czppy)], as an orange solid (in a yield of 19%).

[0200] Using a train sublimation method, 0.52 g of the resulting orange solid was purified by sublimation. During sublimation purification, the solid was heated at 300 °C under a pressure of 2.6 Pa with an argon flow rate of 5 ml / min. After sublimation purification, an orange target solid was obtained in 74% yield. A synthesis scheme of step 3 is shown below in (a-3).

[0201] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the orange solid obtained in step 3 are shown below. In Fig. 17 will be the 1 H-NMR chart is shown. These results reveal that [Ir(ppy)2(Czppy)], which is the organometallic complex of one embodiment of the present invention and represented by the above structural formula (100), was obtained in this synthesis example.

[0202] 1 H NMR. δ (CDCl3): 6.85-6.98 (m, 11H), 7.20 (dd, 1H), 7.32-7.35 (t, 2H), 7.42-7.45 (t, 2H), 7.59-7.65 (m, 6H), 7.67 (d, 1H), 7.70-7.72 (t, 3H), 7.92 (dd, 2H), 8.13-8.16 (t, 3H).

[0203] Subsequently, a UV-visible absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a deoxidized dichloromethane solution of [Ir(ppy)2(Czppy)] and an emission spectrum thereof were measured. The absorption spectrum measurement was performed at room temperature using a UV-visible spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The emission spectrum measurement was performed at room temperature in such a manner that an absolute PL quantum yield measurement system (C11347-01, manufactured by Hamamatsu Photonics KK) was used and the deoxidized dichloromethane solution (0.010 mmol / L) was sealed in a quartz cell under a nitrogen atmosphere in a glove box (LABstar M13 (1250 / 780), manufactured by Bright Co., Ltd.).

[0204] The measurement results of the obtained absorption and emission spectrum are shown in Fig. 18. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 18, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 18 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0205] As in Fig. As shown in Figure 18, the organometallic complex of one embodiment of the present invention, [Ir(ppy)2(Czppy)], has an emission peak at 537 nm, and a yellow-green light emission was observed from the dichloromethane solution. [Example 2]<<Synthesebeispiel 2> >

[0206] In this example, a synthesis method of a material for a light-emitting element of one embodiment of the present invention will be described in detail. Specifically, this example describes a synthesis example of bis[2-{4-(9H-carbazol-9-yl)-2-pyridinyl-κN}phenyl-κC][2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)(Czppy)]2), which is an organometallic complex containing iridium as the central metal and having a ligand having a first framework with a hole-transport property and a second framework with a light-emitting property. A structure of [Ir(ppy)(Czppy)]2 is shown below.

[0207] It should be noted that in [Ir(ppy)(Czppy)]2, the carbazole framework corresponds to the first framework with a hole transport property and the 2-pyridylphenyl framework corresponds to the second framework with a light emission property. <Schritt 1: Synthese von Di-µ-chlor-tetrakis[4-(9H-carbazol-9-yl)-2-pyridinyl-κN)phenyl-κC]diiridium(III) (Abkürzung: [Ir(Czppy)2Cl]2)>

[0208] First, 6.1 g of HCzppy, 2.9 g of iridium(III) chloride hydrate, 90 mL of 2-ethoxyethanol, and 30 mL of water were placed in a round-bottomed flask equipped with a reflux tube and irradiated with microwaves (2.45 GHz, 200 W) for 2 hours while being purged with argon. The resulting mixture was filtered, followed by washing with methanol to obtain 6.3 g of the target substance (a yellow solid in a yield of 76%). A synthesis scheme of Step 1 is further shown below at (b-1). <Schritt 2: Synthese von [Ir(ppy)(Czppy)2]>

[0209] Subsequently, 4.3 g of [Ir(Czppy)2Cl]2 obtained in step 1 and 250 ml of dichloromethane (abbreviation: DCM) were added to a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.9 g of silver triflate and 40 ml of isopropanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 1.6 g of 2-phenylpyridine (abbreviation: Hppy), 50 ml of 2-ethoxyethanol, and 50 ml of N,N-dimethylformamide (abbreviation: DMF) were added to the solid, and the mixture was refluxed for 17 hours under a nitrogen atmosphere.

[0210] The resulting mixture was concentrated and purified by silica gel column chromatography using dichloromethane and hexane in a ratio of 1:1 as eluent. Further purification was performed by silica gel column chromatography using chloroform and hexane in a ratio of 3:2 as eluent. The resulting solution was concentrated, followed by recrystallization with dichloromethane and methanol to obtain [Ir(ppy)(Czppy)2] as an orange solid (in a yield of 7%). A synthesis scheme of step 2 is further shown below in (b-2).

[0211] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the orange solid obtained in step 2 are shown below. In Fig. 19 will be the 1 H-NMR chart is shown. These results reveal that [Ir(ppy)(Czppy)2], which is the organometallic complex of one embodiment of the present invention and represented by the above structural formula (101), was obtained in Synthesis Example 2.

[0212] 1 H NMR. δ (CD2Cl2): 6.82-6.96 (m, 9H), 7.04-7.07 (t, 1H), 7.29-7.37 (m, 6H), 7.42-7.46 (m, 4H), 7.67-7.74 (m, 8H), 7.80 (d, 1H), 7.83 (d, 1H), 7.93 (d, 1H), 7.98 (d, 1H), 8.12-8.15 (ms, 4H), 8.23-8.25 (ms, 2H).

[0213] Subsequently, a UV-visible absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a deoxidized dichloromethane solution of [Ir(ppy)(Czppy)2] and an emission spectrum thereof were measured. The absorption spectrum measurement was performed at room temperature using a UV-visible spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The emission spectrum measurement was performed at room temperature in such a manner that an absolute PL quantum yield measurement system (C11347-01, manufactured by Hamamatsu Photonics KK) was used and the deoxidized dichloromethane solution (0.010 mmol / L) was sealed in a quartz cell under a nitrogen atmosphere in a glove box (LABstar M13 (1250 / 780), manufactured by Bright Co., Ltd.).

[0214] The measurement results of the obtained absorption and emission spectrum are shown in Fig. 20. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 20, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 20 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0215] As in Fig. As shown in Figure 20, the organometallic complex of one embodiment of the present invention, [Ir(ppy)(Czppy)2], has an emission peak at 530 nm, and a yellow-green light emission was observed from the dichloromethane solution. [Example 3]

[0216] In this example, element structures, manufacturing methods, and properties of the following light-emitting elements are described: as a light-emitting element of an embodiment of the present invention, a light-emitting element 1 in which [2-{(9H-carbazol-9-yl)-2-pyridinyl-κN}phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)2(Czppy)]) (structural formula (100)) is used as the guest material of the light-emitting layer, which was described in Example 1, and a light-emitting element 2 in which [Ir(ppy)(Czppy)]2) (structural formula (101)) is used as the guest material of the light-emitting layer, which was described in Example 2, as well as a comparative light-emitting element 1 in which Tris(2-phenylpyridinato-N, C 2' )iridium(III) (abbreviation: Ir(ppy)3). It should be noted that Fig. Figure 21 illustrates an element structure of the light-emitting elements used in this example, and Table 1 shows the specific structures. The chemical formulas of the materials used in this example are shown below. [Table 1] erste Elektrode Lochinjektionsschicht Lochtransportschicht Licht emittierende Schicht Elektronentransportschicht Elektroneninjektionsschicht zweite Elektrode Licht emittierendes Element 1 ITO (70 nm) DBT3P- II :MoOx (4:2 60 nm) PCCP (20 nm) * mPCCzPTzn-02 (15 nm) Bphen (10 nm) LiF (1 nm) Al (200 nm) Licht emittierendes Element 2 ITO (70 nm) DBT3P-II:MoOx (4:2 60 nm) PCCP (20 nm) ** mPCCzPTzn-02 (15 nm) Bphen (10 nm) LiF (1 nm) Al (200 nm) Light-emitting reference element 1 ITO (70 nm) DBT3P-II:MoOx (4:2 60 nm) PCCP (20 nm) *** mPCCzPTzn-02 (15 nm) Bphen (10 nm) LiF (1 nm) Al (200 nm) * mPCCzPTzn-02:PCCP:[Ir(ppy)2(Czppy)] (0.5:0.5:0.10 (20 nm)\0.8:0.2:0.10 (20 nm) ** mPCCzPTzn-02:PCCP:[Ir(ppy)(Czppy)2] (0.5:0.5:0.10 (20 nm)\0.8:0.2:0.10 (20 nm) *** mPCCzPTzn-02:PCCP:[Ir(ppy)3] (0.5:0.5:0.10 (20 nm)\0.8:0.2:0.10 (20 nm) <Herstellung der Licht emittierenden Elemente>

[0217] For each of the light-emitting elements described in this example, as shown in Fig. 21, a hole injection layer 1911, a hole transport layer 1912, a light emitting layer 1913, an electron transport layer 1914, and an electron injection layer 1915 are disposed in this order over an anode 901 formed over a substrate 1900, and a cathode 1903 is disposed over the electron injection layer 1915.

[0218] First, the anode 1901 was formed over the substrate 1900. The electrode area was set to 4 mm 2 (2 mm × 2 mm). A glass substrate was used as the substrate 1900. The anode 1901 was formed by a sputtering method using indium tin oxide (ITO) containing silicon oxide to a thickness of 70 nm.

[0219] As a pretreatment, a surface of the substrate was washed with water, baked at 200 °C for one hour, and then UV ozone treatment was performed for 370 seconds. Afterward, the substrate was transferred to a vacuum evaporation device, where the pressure was increased to approximately 10 -4 Pa, vacuum baking was performed at 170 °C for 60 minutes in a heating chamber of the vacuum evaporation apparatus, and then the substrate was cooled for approximately 30 minutes.

[0220] Next, the hole injection layer 1911 was formed over the anode 1901. After the pressure in the vacuum evaporation device was reduced to 10 -4 Pa, the hole injection layer was formed in 1911 by co-evaporation of 1,3,5-tri(dibenzothiophen-4-yl)benzene (abbreviation: DBT3P-II) and molybdenum oxide to a thickness of 60 nm, with the weight ratio of DBT3P-II to molybdenum oxide being 4:2.

[0221] Subsequently, the hole transport layer 1912 was formed over the hole injection layer 1911. The hole transport layer 1912 was formed by evaporating 9-phenyl-9H-3-(9-phenyl-9H-carbazol-3-yl)carbazole (abbreviation: PCCP) to a thickness of 20 nm.

[0222] Next, the light-emitting layer 1913 was formed over the hole transport layer 1912.

[0223] The light-emitting layer 1913 in the light-emitting element 1 was formed by co-evaporation using 9-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9'-phenyl-2,3'-bi-9H-carbazole (abbreviation: mPCCzPTzn-02) as the host material, PCCP as the auxiliary material, and [Ir(ppy)2(Czppy)] as the guest material (phosphorescent material), with the weight ratio of mPCCzPTzn-02 to PCCP and [Ir(ppy)2(Czppy)] being 0.5:0.5:0.10. The thickness was set to 20 nm. Furthermore, mPCCzPTzn-02, PCCP, and [Ir(ppy)2(Czppy)] were co-evaporated, with the weight ratio of mPCCzPTzn-02 to PCCP and [Ir(ppy)2(Czppy)] being 0.8:0.2:0.10. The thickness was set to 20 nm. Consequently, the light-emitting layer 1913 has a multilayer structure with a thickness of 40 nm.

[0224] The light-emitting layer 1913 in the light-emitting element 2 was formed by co-evaporation using mPCCzPTzn-O2 as the host material, PCCP as the auxiliary material, and [Ir(ppy)(Czppy)2] as the guest material (phosphorescent material), with the weight ratio of mPCCzPTzn-O2 to PCCP and [Ir(ppy)(Czppy)2] being 0.5:0.5:0.10. The thickness was set to 20 nm. Furthermore, mPCCzPTzn-O2, PCCP, and [Ir(ppy)(Czppy)2] were deposited by co-evaporation, with the weight ratio of mPCCzPTzn-O2 to PCCP and [Ir(ppy)(Czppy)2] being 0.8:0.2:0.1. The thickness was set to 20 nm. Consequently, the light-emitting layer 1913 has a multilayer structure with a thickness of 40 nm.

[0225] The light-emitting layer 1913 in Comparative Light-Emitting Element 1 was formed by co-evaporation using mPCCzPTzn-O2 as the host material, PCCP as the auxiliary material, and [Ir(ppy)3] as the guest material (phosphorescent material), with the weight ratio of mPCCzPTzn-O2 to PCCP and [Ir(ppy)3] being 0.5:0.5:0.10. The thickness was set to 20 nm. Furthermore, mPCCzPTzn-O2, PCCP, and [Ir(ppy)3] were deposited by co-evaporation, with the weight ratio of mPCCzPTzn-O2 to PCCP and [Ir(ppy)3] being 0.8:0.2:0.1. The thickness was set to 20 nm. Consequently, the light-emitting layer 1913 has a multilayer structure with a thickness of 40 nm.

[0226] Next, the electron-transport layer 1914 was formed over the light-emitting layer 1913. The electron-transport layer 1914 was formed as follows: mPCCzPTzn-02 and bathophenanthroline (abbreviation: Bphen) were sequentially deposited by evaporation to a thickness of 15 nm and 10 nm, respectively.

[0227] Subsequently, the electron injection layer 1915 was formed over the electron transport layer 1914. The electron injection layer 1915 was formed by evaporating lithium fluoride (LiF) to a thickness of 1 nm.

[0228] Thereafter, the cathode 1903 was formed over the electron injection layer 1915. The cathode 1903 was formed using aluminum by an evaporation method to a thickness of 200 nm.

[0229] Through the above steps, the light-emitting elements, each including an EL layer between a pair of electrodes, were formed over the substrate 1900. The hole-injection layer 1911, the hole-transport layer 1912, the light-emitting layer 1913, the electron-transport layer 1914, and the electron-injection layer 1915 described above are functional layers constituting the EL layer of one embodiment of the present invention. Furthermore, in all evaporation steps of the above manufacturing method, evaporation was performed by a resistance heating method.

[0230] Each of the light-emitting elements prepared as described above was sealed using another substrate (not shown). Sealing using the substrate was performed in the following manner: The another substrate was attached to the substrate 1900 with a sealant in a glove box containing a nitrogen atmosphere, a sealing material was applied to enclose the light-emitting element formed over the substrate 1900, and then irradiated with 365 nm UV light at 6 J / cm 2 and heat treatment was carried out at 80 °C for 1 hour. <<Betriebseigenschaften der Licht emittierenden Elemente> >

[0231] The operating characteristics of the fabricated light-emitting elements (light-emitting elements 1 and 2, and comparative light-emitting element 1) were measured. Note that the measurements were performed at room temperature. The results are presented in Fig. 23 to Fig. 25 shown.

[0232] The results reveal that the light-emitting elements of the embodiments of the present invention (Light-emitting Element 1, Light-emitting Element 2, and Comparative Light-emitting Element 1) exhibit excellent current efficiency and high external quantum efficiency. Table 2 shows the initial values ​​of the main characteristics of the light-emitting elements at about 1000 cd / m 2 . [Table 2] Voltage (V) Current (mA) Current density (mA / cm 2 ) Chromaticity (x,y) Luminance (cd / m 2 ) Power efficiency (cd / A) Power efficiency (Im / W) external quantum efficiency (%) Light-emitting element 1 3,2 0,056 1,4 (0,38,0,59) 840 60 59 17 Light-emitting element 2 3,1 0,054 1,3 (0,37,0,60) 820 61 62 17 Light-emitting reference element 1 3,3 0,080 2,0 (0,35,0,61) 1000 52 49 15

[0233] Fig. Figure 26 shows the emission spectra of the light-emitting element 1, the light-emitting element 2 and the comparative light-emitting element 1 through which a current with a current density of 2.5 mA / cm 2 flows. As in Fig. As shown in Figure 26, the emission spectrum of the light-emitting element 1 has a peak at about 531 nm, which is presumably due to the light emission from [Ir(ppy)2(Czppy)], the organometallic complex, contained in the light-emitting layer 1913. The emission spectrum of the light-emitting element 2 has a peak at about 531 nm, which is presumably due to the light emission from [Ir(ppy)(Czppy)2], the organometallic complex, contained in the light-emitting layer 1913. The emission spectrum of the comparative light-emitting element 1 has a peak at about 517 nm, which is presumably due to the light emission from [Ir(ppy)3], the organometallic complex, contained in the light-emitting layer 1913.Note that the organometallic complex of one embodiment of the present invention used in light-emitting element 1 and light-emitting element 2 has a carbazole skeleton at the 4-position of a 2-phenylpyridine skeleton, allowing carriers (electrons or holes) to be easily injected and transported, improving the emission efficiency of the elements, and reducing the driving voltage. This indicates that light-emitting elements 1 and 2 have higher current efficiency and lower driving voltage than comparative light-emitting element 1. [Example 4]

[0234] In this example, an element structure, a manufacturing method, and the properties of a light-emitting element 3 in which the light-emitting layer is formed solely by bis{2-[6-(9H-carbazol-9-yl)-4-pyrimidinyl-κN3]phenyl-κC}-{2-[2-pyridinyl-κN]phenyl-κC}iridium(III) (abbreviation: [Ir(czppm]2(ppy)]), structural formula (102)), which is the material for a light-emitting element of the present invention, are described. It should be noted that Fig. Figure 21 shows an element structure of the light-emitting element used in this example, and Table 3 shows the specific structures. The chemical formulas of the materials used in this example are shown below. [Table 3] Hole injection layer Hole transport layer Light-emitting layer Electron transport layer Electron injection layer 50 nm 20 nm 30 nm 30 nm 15 nm 1 nm DBT3P-II: MoOx (2:1) PCBBiF Ir(Czppm)2(ppy) 2mDBTBPDBq-II BPhen LiF <Herstellung des Licht emittierenden Elements>

[0235] In the light-emitting element described in this example, as shown in Fig. 21, a hole injection layer 1911, a hole transport layer 1912, a light emitting layer 1913, an electron transport layer 1914, and an electron injection layer 1915 are disposed in this order over an anode 1901 formed over a substrate 1900, and a cathode 1903 is disposed over the electron injection layer 1915.

[0236] First, the anode 1901 was formed over the substrate 1900. The electrode area was set to 4 mm 2 (2 mm × 2 mm). A glass substrate was used as the substrate 1900. The anode 1901 was formed by a sputtering method using indium tin oxide (ITO) containing silicon oxide to a thickness of 70 nm.

[0237] As a pretreatment, one surface of the substrate was washed with water for 190°C, baked for one hour at 200°C, and then UV ozone treatment was performed for 370 seconds. Afterward, the substrate was transferred to a vacuum evaporation device, where the pressure was reduced to approximately 10 -4 Pa, vacuum baking was performed at 170 °C for 60 minutes in a heating chamber of the vacuum evaporation apparatus, and then the substrate was cooled for approximately 30 minutes.

[0238] Next, the hole injection layer 1911 was formed over the anode 1901. After the pressure in the vacuum evaporation device was reduced to 10 -4 Pa, the hole injection layer was formed in 1911 by co-evaporation of 1,3,5-tri(dibenzothiophen-4-yl)benzene (abbreviation: DBT3P-II) and molybdenum oxide to a thickness of 50 nm, with the weight ratio of DBT3P-II to molybdenum oxide being 2:1.

[0239] Subsequently, the hole transport layer 1912 was formed over the hole injection layer 1911. The hole transport layer 1912 was formed by evaporating N-(1,1'-biphenyl-4-yl)-9,9-dimethyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9H-fluoren-2-amine (abbreviation: PCBBiF) to a thickness of 20 nm.

[0240] Next, the light-emitting layer 1913 was formed over the hole-transporting layer 1912. The light-emitting layer 1913 was formed by evaporating bis{2-[6-(9H-carbazol-9-yl)-4-pyrimidinyl-κN3]phenyl-κC}-{2-[2-pyridinyl-κN]phenyl-κC}iridium(III) (abbreviation: [Ir(czppm]2(ppy)]), represented by the above structural formula (102), to a thickness of 30 nm.

[0241] Next, the electron-transport layer 1914 was formed over the light-emitting layer 1913. The electron-transport layer 1914 was formed by evaporating 2-[3'-(dibenzothiophen-4-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTBPDBq-II), represented by the above structural formula (iv), to a thickness of 30 nm and then evaporating bathophenanthroline (abbreviation: Bphen), represented by the structural formula (vi), to a thickness of 15 nm.

[0242] Subsequently, the electron injection layer 1915 was formed over the electron transport layer 1914. The electron injection layer 1915 was formed by evaporating lithium fluoride (LiF) to a thickness of 1 nm.

[0243] Thereafter, the cathode 1903 was formed over the electron injection layer 1915. The cathode 1903 was formed using aluminum by an evaporation method to a thickness of 200 nm.

[0244] Through the above steps, the light-emitting element including an EL layer between a pair of electrodes was formed over the substrate 1900. The hole-injection layer 1911, the hole-transport layer 1912, the light-emitting layer 1913, the electron-transport layer 1914, and the electron-injection layer 1915 described above are functional layers constituting the EL layer of one embodiment of the present invention. Furthermore, in all evaporation steps of the above manufacturing method, evaporation was performed by a resistance heating method.

[0245] The light-emitting element manufactured as described above was sealed using another substrate (not shown). Sealing using the substrate was performed in the following manner: The substrate was attached to the substrate 1900 with a sealant in a glove box containing a nitrogen atmosphere, a sealing material was applied to enclose the light-emitting element formed over the substrate 1900, and then irradiated with 365 nm UV light at 6 J / cm 2 and heat treatment was carried out at 80 °C for 1 hour. <<Betriebseigenschaften des Licht emittierenden Elements> >

[0246] The operating characteristics of the fabricated light-emitting element 3 were measured. Note that the measurement was conducted at room temperature (in an atmosphere maintained at 25 °C). The results are shown in Fig. 27 to Fig. 31 shown.

[0247] The results reveal that the light-emitting element 3 of one embodiment of the present invention exhibits excellent current efficiency and high external quantum efficiency even when the light-emitting layer is formed using only one material. Table 4 shows the initial values ​​of the main characteristics of the light-emitting element at about 1000 cd / m² 2 . [Table 4] Voltage (V) Current (mA) Current density (mA / cm 2 ) Chromaticity x Chromaticity y Power efficiency (cd / A) external quantum efficiency (%) 3,3 0,09 2,2 0,52 0,48 43 15

[0248] Fig. 32 shows the emission spectrum of the light-emitting element 3, through which a current with a current density of 2.5 mA / cm 2 flows. As in Fig. 32, the emission spectrum of the light-emitting element 3 has a peak at about 568 nm, which is presumably due to the light emission of [Ir(czppm)2(ppy)], the organometallic complex, contained in the light-emitting layer 1913. Note that the organometallic complex of one embodiment of the present invention used in the light-emitting element 3 has a carbazole skeleton at the 6-position of a 4-phenylpyridine skeleton, so that carriers (electrons or holes) can be easily injected and transported, the emission efficiency of the element can be improved, and the driving voltage can be reduced.Since the carbazole framework (a framework with a charge carrier transport property) is positioned at the periphery of the light-emitting framework, the light-emitting framework in this molecule interacts with a light-emitting framework in another molecule, thereby suppressing concentration quenching. Thus, the light-emitting layer enables high external quantum efficiency despite being composed of a single material. The above results demonstrate that by using the light-emitting element material of one embodiment of the present invention, even a light-emitting element having a light-emitting layer composed of a single material and not employing co-evaporation can exhibit advantageous properties such as high current efficiency and low operating voltage. [Example 5]<<Synthesebeispiel 3> >

[0249] This synthesis example describes a synthesis method of bis{2-[6-(9H-carbazol-9-yl)-4-pyrimidinyl-κN3]phenyl-rC}-{2-[2-pyridinyl-κN]phenyl-κC}iridium(III) (abbreviation: [Ir(czppm]2(ppy)]), which is an organometallic complex containing iridium as the central metal and having a ligand that has a first framework with a hole-transport property and a second framework with a light-emitting property. A structure of [Ir(czppm]2(ppy)] is shown below.

[0250] It should be noted that in [Ir(czppm)]2(ppy)], the carbazole framework corresponds to the first framework with a hole transport property and the 4-phenylpyrimidine framework corresponds to the second framework with a light emission property. <Schritt1: Synthese von 4-Carbazol-9-yl-6-phenylpyrimidin (Abkürzung: Hczppm)>

[0251] First, 0.053 g of sodium hydride (60% in petroleum) and 30 mL of dry N,N-dimethylformamide (abbreviation: dry DMF) were placed in a three-necked flask, and the air in the flask was replaced with nitrogen. 1.76 g of carbazole and 30 mL of dry DMF were added to this flask, and the mixture was stirred at room temperature for 1 hour. Then, 1.76 g of 4-chloro-6-phenylpyrimidine and 30 mL of dry DMF were added, and stirring was carried out at room temperature for 4 hours to induce a reaction. After the reaction, water was added to the resulting solution, and suction filtration was performed to obtain a solid. The resulting solid was purified by flash column chromatography using dichloromethane as the eluent to obtain the target pyrimidine derivative Hczppm (white powder, yield 62%). A synthesis scheme of step 1 is shown below. <Schritt 2: Synthese von Di-µ-chlor-tetrakis{2-[2-pyridinyl-κN)phenyl-κC}diiridium(III) (Abkürzung: [Ir(ppy)2Cl]2)>

[0252] 30 mL of 2-ethoxyethanol, 10 mL of water, 3.88 g of 2-phenylpyridine (abbreviation: Hppy), and 3.49 g of iridium chloride hydrate (IrCl3·H2O) (manufactured by Furuya Metal Co., Ltd.) were placed in a recovery flask equipped with a reflux tube, and the air in the flask was replaced with argon. Subsequently, microwave irradiation (2.45 GHz, 100 W) was carried out for 2 hours to induce a reaction. After the reaction, the resulting mixture was subjected to suction filtration and washing using methanol to obtain the dinuclear complex [Ir(ppy)2Cl]2 (yellow solid, yield 59%). A synthesis scheme of step 2 is shown below. <Schritt 3: Synthese von Bis{2-[6-(9H-carbazol-9-yl)-4-pyrimidinyl-κN3]phenyl-κC}-{2-[2-pyridinyl-κN]phenyl-κChiridium(III) (Abkürzung: [Ir(czppm)2(ppy)])>

[0253] 3.69 g of the dinuclear complex [Ir(ppy)2Cl]2] obtained in step 2 and 390 ml of dichloromethane were placed in an opaque three-necked flask, and the air in the flask was replaced with nitrogen. Subsequently, a solution in which 2.27 g of silver trifluoromethanesulfonate was dissolved in 180 ml of methanol was added dropwise to the mixture, and the mixture was stirred at room temperature for 24 hours. The resulting mixture was filtered through a filter aid, and the filtrate was concentrated to obtain a solid. Subsequently, the obtained solid, 3.90 g of Hczppm, and 40 ml of ethanol were placed in a three-necked flask equipped with a reflux tube, and the air in the flask was replaced with nitrogen. After heat treatment at 90 °C for 48 hours, the resulting mixture was subjected to suction filtration.After the obtained residue was purified by silica gel column chromatography using hexane and ethyl acetate as eluents in a ratio of 6:1, recrystallization was performed with a mixed solvent of dichloromethane and methanol. Thus, [Ir(czppm)2(ppy)], which is the material for a light-emitting element of one embodiment of the present invention, was obtained as a yellow-orange powder in a yield of 6%. A synthesis scheme of Step 3 is shown below.

[0254] The nuclear magnetic resonance ( 1 The analysis results of the yellow-orange powder obtained in step 3, obtained by H-NMR spectroscopy, are shown below. In Fig. 33(A) and in Fig. 33(B) is a 1 H-NMR diagram shown. Fig. 33(B) is a graph showing the range from 6.50 ppm to 8.75 ppm in Fig. 33(A) is an enlarged view. These results reveal that [Ir(czppm)2(ppy)], which is the material for a light-emitting element of one embodiment of the present invention and represented by the above structural formula, was obtained in Synthesis Example 3.

[0255] 1 H NMR. δ (CD2Cl2): 6.82 (d, 1H), 6.87-7.03 (m, 8H), 7.10 (t, 1H), 7.37-7.40 (m, 4H), 7.47-7.51 (m, 4H), 7.75-7.78 (m, 2H), 7.88 (t, 2H), 7.97 (d, 1H), 8.03 (d, 1H), 8.12 (d, 4H), 8.18 (dd, 4H), 8.23 ​​(s, 2H), 8.36 (s, 1H), 8.61 (s, 1H).

[0256] Subsequently, a UV-visible absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(czppm)2(ppy)] and an emission spectrum thereof were measured. The absorption spectrum measurement was performed at room temperature using a UV-visible spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (9.9 µmol / L) placed in a quartz cell. The emission spectrum measurement was performed at room temperature in such a manner that an absolute PL quantum yield measurement system (C11347-01, manufactured by Hamamatsu Photonics KK) was used and the deoxidized dichloromethane solution (9.9 µmol / L) was sealed in a quartz cell under a nitrogen atmosphere in a glove box (LABstar M13 (1250 / 780), manufactured by Bright Co., Ltd.). The measurement results of the obtained absorption and emission spectrum are shown in Fig. 34. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 34, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 34 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (9.9 µmol / L) in a quartz cell.

[0257] As in Fig. As shown in Figure 34, the material for a light-emitting element of the present invention, [Ir(czppm)2(ppy)], has an emission peak at 574 nm, and yellow light emission was observed. [Example 6]<<Synthesebeispiel 4> >

[0258] This synthesis example describes a synthesis method of [4-(4,6-diphenyl-1,3,5-triazin-2-yl)-2-(2-pyridinyl-κN)phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)2(5dptznppy)]), which is an organometallic complex containing iridium as the central metal and a ligand having a first framework with an electron-transport property and a second framework with a light-emitting property. A structural formula of [Ir(ppy)2(5dptznppy)] is shown below. <Schritt 1: Synthese von 3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenylboronsäurepinacolester>

[0259] First, 2.0 g of 2-(3-bromophenyl)-4,6-diphenyl-1,3,5-triazine, 1.6 g of bis(pinacolato)diboron (abbreviation: (Bpin)2), 1.5 g of potassium acetate, and 25 ml of N,N-dimethylformamide were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. In addition, 0.042 g of a [1,1'-bis(diphenylphosphino)ferrocene]palladium(II) dichloride-dichloromethane adduct (abbreviation: Pd(dppf)2Cl) was added. 20 CH2Cl2) was added, and the mixture was heated and stirred at 150 °C for 3 hours. The solvent of the resulting reaction solution was distilled off, and the residue was purified by silica gel column chromatography using toluene as the eluent to obtain 2.0 g of the target substance (a white solid in 80% yield). A synthesis scheme of Step 1 is shown below. <Schritt 2: Synthese von 2-[3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenyl]pyridin (Abkürzung: H5dptznppy)>

[0260] Subsequently, 2.8 g of 3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenylboronic acid pinacol ester obtained in Step 1, 0.9 g of 2-bromopyridine, 1.6 g of potassium carbonate, 50 ml of tetrahydrofuran (abbreviation: THF), and 25 ml of water were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Furthermore, 0.33 g of tetrakis(triphenylphosphine)palladium(0) was added, and the mixture was heated and stirred at 70 °C for 24 hours. After the reaction, extraction with ethyl acetate was performed. Purification was then carried out by silica gel column chromatography using dichloromethane as the eluent to obtain 2.2 g of a target substance (a white solid in a yield of 98%). A synthesis scheme of Step 2 is shown below. <Schritt 3: Synthese von [4-(4,6-Diphenyl-1,3,5-triazin-2-yl)-2-(2-pyridinyl-κN)phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (Abkürzung: [Ir(ppy)2(5dptznppy)])>

[0261] Subsequently, 1.9 g of [Ir(ppy)2Cl]2 and 190 ml of dichloromethane were added to a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.1 g of silver triflate and 90 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 2.0 g of H5dptznppy obtained in step 2 and 70 ml of ethanol were added to the solid, and the mixture was refluxed for 24 hours under a nitrogen atmosphere. The resulting reactant was filtered, and a residue was purified by silica gel column chromatography using dichloromethane as the eluent. Subsequently, purification was carried out by high-performance liquid chromatography using chloroform as the mobile phase.The resulting solution was concentrated, followed by recrystallization with a mixed solvent of dichloromethane and hexane to obtain a yellow solid (yield 28%). A synthesis scheme of step 3 is shown below.

[0262] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the yellow solid obtained in step 3 are shown below. In Fig. 35 will be the 1 H-NMR diagram is shown. These results reveal that [Ir(ppy)2(5dptznppy)], which is the organometallic complex of one embodiment of the present invention, was obtained in this synthesis example.

[0263] 1 H NMR. δ (CDCl3): 6.84–6.99 (m, 9H), 7.13 (d, 1H), 7.53–7.64 (m, 11H), 7.68 (d, 2H), 7.74 (t, 1H), 7.91 (t, 2H), 8.21 (d, 2H), 8.76 (d, 4H), 9.03 (s, 1H). Note that the peak at approximately 5.30 is due to dichloromethane.

[0264] Subsequently, a UV-VIS absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(ppy)2(5dptznppy)] and an emission spectrum thereof were measured. The measurement of the absorption spectrum was performed at room temperature using a UV-VIS spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. In addition, the measurement of the emission spectrum was performed at room temperature using a fluorescence spectrophotometer (FS920, manufactured by Hamamatsu Photonics KK) with the degassed dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The measurement results of the obtained absorption and emission spectra are shown in Fig. 36. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 36, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 36 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0265] As in Fig. As shown in Figure 36, the organometallic complex of one embodiment of the present invention, [Ir(ppy)2(5dptznppy)], has an emission peak at 510 nm, and yellow-green light emission was observed from the dichloromethane solution. [Example 7]<<Synthesebeispiel 5> >

[0266] This synthesis example describes a synthesis method of bis[4-(4,6-diphenyl-1,3,5-triazin-2-yl)-2-(2-pyridinyl-κN)phenyl-κC][2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(5dptznppy)2(ppy)]), which is an organometallic complex containing iridium as the central metal and a ligand having a first framework with an electron-transport property and a second framework with a light-emitting property. A structural formula of [Ir(5dptznppy)2(ppy)] is shown below. <Schritt 1: Synthese von 2-[3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenyl]pyridin (Abkürzung: H5dptznppy)>

[0267] The synthesis was carried out in a similar manner to step 2 of Synthesis Example 4 in Example 6. <Schritt 2: Synthese von [Ir(5dptznppy)2(ppy)]>

[0268] 1.9 g of [Ir(ppy)2Cl]2 and 190 ml of dichloromethane were placed in a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.1 g of silver triflate and 90 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 2.0 g of H5dptznppy and 70 ml of ethanol were added to the solid, and the mixture was refluxed for 24 hours under a nitrogen atmosphere. The resulting reactant was filtered, and a residue was purified by silica gel column chromatography using dichloromethane as the eluent. Subsequently, purification was carried out by high-performance liquid chromatography using chloroform as the mobile phase.The resulting solution was concentrated, followed by recrystallization with a mixed solvent of dichloromethane and hexane to obtain a yellow solid (yield 3.5%). A synthesis scheme of step 2 is shown below.

[0269] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the yellow solid obtained above are shown below. In Fig. 37 will be the 1 H-NMR diagram is shown. These results reveal that [Ir(5dptznppy)2(ppy)], which is the organometallic complex of one embodiment of the present invention, was obtained in this synthesis example.

[0270] 1 H-NMR. δ (CDCl3): 6,89-7,05 (m, 6H), 7,16 (d, 1H), 7,19 (d, 1H), 7,52-7,65 (m, 16H), 7,71 (d, 1H), 7,75-7,80 (m, 2H), 7,94 (d, 1H), 8,20-8,27 (m, 4H), 8,74 (d, 4H), 8,78 (d, 4H), 9,07 (d, 2H).

[0271] Subsequently, a UV-VIS absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(5dptznppy)2(ppy)] and an emission spectrum thereof were measured. The absorption spectrum measurement was performed at room temperature using a UV-VIS spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. In addition, the emission spectrum measurement was performed at room temperature using a fluorescence spectrophotometer (FS920, manufactured by Hamamatsu Photonics KK) with the degassed dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The measurement results of the obtained absorption and emission spectra are shown in Fig. 38. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 38, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 38 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0272] As in Fig. As shown in Figure 38, the organometallic complex of one embodiment of the present invention, [Ir(5dptznppy)2(ppy)], has an emission peak at 501 nm, and a yellow-green light emission was observed from the dichloromethane solution. [Example 8]<<Synthesebeispiel 6> >

[0273] This synthesis example describes a synthesis method for [2-(4-diphenylamino-2-pyridinyl-κN)phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)2(dpappy)]), an organometallic complex containing iridium as the central metal and a ligand having a first framework with a hole-transport property and a second framework with a light-emitting property. A structural formula of [Ir(ppy)2(dpappy)] is shown below. <Schritt 1: Synthese von 4-Chlor-2-phenylpryridin>

[0274] The synthesis of 4-chloro-2-phenylpyridine was carried out in a similar manner to step 1 of Synthesis 1 in Example 1. <Schritt 2: Synthese von 4-Diphenylamino-2-phenylpyridin (Abkürzung: Hdpappy)>

[0275] Subsequently, 4.5 g of 4-chloro-2-phenylpyridine obtained in step 1, 4.9 g of diphenylamine, and 4.1 g of sodium tert-butoxide were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Further, 105 ml of toluene, 0.57 ml of tri-tert-butylphosphine, and 1.1 g of tris(dibenzylideneacetone)dipalladium(0) (abbreviation: Pd2(dba)3) were added, and the mixture was heated and stirred at 120 °C for 5 hours. The resulting reactant was filtered, and the solvent of the filtrate was distilled off, followed by purification by silica gel column chromatography using ethyl acetate and hexane in a 2:1 ratio as the eluent to obtain 2.4 g of the target compound (a yellow solid in a yield of 31%). A synthesis scheme of step 2 is shown below. <Schritt 3: Synthese von [2-(4-Diphenylamino-2-pyridinyl-κN)phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (Abkürzung: [Ir(ppy)2(dpappy)])>

[0276] Next, 1.8 g of [Ir(ppy)2Cl]2 and 180 ml of dichloromethane were added to a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.1 g of silver triflate and 86 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 1.5 g of HDPPPy obtained in step 2, 35 ml of 2-ethoxyethanol, and 35 ml of N,N-dimethylformamide (abbreviation: DMF) were added to the solid, and the mixture was refluxed for 17 hours under a nitrogen atmosphere. The resulting mixture was concentrated and purified by silica gel column chromatography using dichloromethane and hexane in a ratio of 1:1 as the eluent. Purification was then carried out by high-performance liquid chromatography using chloroform as the mobile phase.The obtained solution was concentrated and then recrystallized with a mixed solvent of dichloromethane and hexane to obtain an orange solid (yield 20%).

[0277] Using a train sublimation process, 0.41 g of the resulting orange solid was purified by sublimation. During sublimation purification, the solid was heated at 310 °C under a pressure of 1.5 Pa with an argon flow rate of 5 ml / min. After sublimation purification, an orange target solid was obtained in 68% yield. A synthesis scheme of step 3 is shown below.

[0278] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the orange solid obtained in step 3 are shown below. In Fig. 39 will be the 1 H NMR diagram is shown. These results reveal that [Ir(ppy)2(dpappy)] was obtained in this synthesis example.

[0279] 1 H NMR. δ (CD2Cl2): 6.34 (dd, 1H), 6.68-6.92 (m, 10H), 7.01 (t, 1H), 7.11 (d, 1H), 7.22-7.26 (m, 7H), 7.29 (d, 1H), 7.37-7.40 (m, 4H), 7.53 (d, 1H), 7.59 (t, 1H), 7.66 (t, 3H), 7.74 (d, 1H), 7.87 (d, 1H), 7.91 (d, 1H).

[0280] Subsequently, a UV-VIS absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(ppy)2(dpappy)] and an emission spectrum thereof were measured. The measurement of the absorption spectrum was performed at room temperature using a UV-VIS spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. In addition, the measurement of the emission spectrum was performed at room temperature using a fluorescence spectrophotometer (FS920, manufactured by Hamamatsu Photonics KK) with the degassed dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The measurement results of the obtained absorption and emission spectra are shown in Fig. 40. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 40, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 40 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0281] As in Fig. As shown in Figure 40, the organometallic complex of one embodiment of the present invention, [Ir(ppy)2(dpappy)], has an emission peak at 531 nm, and a yellow-green light emission was observed from the dichloromethane solution. [Example 9]<<Synthesebeispiel 7> >

[0282] This synthesis example describes a synthesis method of bis[2-(4-diphenylamino-2-pyridinyl-κN)phenyl-κC][2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(dpappy)2(ppy)]), which is an organometallic complex containing iridium as the central metal and a ligand having a first framework with a hole-transport property and a second framework with a light-emitting property. A structural formula of [Ir(dpappy)2(ppy)]) is shown below. <Schritt 1: Synthese von 4-Chlor-2-phenylpryridin>

[0283] The synthesis of 4-chloro-2-phenylpyridine was carried out in a similar manner to step 1 of Synthesis Example 1 in Example 1. <Schritt 2: Synthese von 4-Diphenylamino-2-phenylpyridin (Abkürzung: Hdpappy)>

[0284] The synthesis of Hdpappy was carried out in a similar manner to step 2 of Synthesis Example 6 in Example 8. <Schritt 3: Synthese von Bis[2-(4-diphenylamino-2-pyridinyl-κN)phenyl-κC][2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (Abkürzung: [Ir(dpappy)2(ppy)])>

[0285] First, 1.8 g of di-μ-chloro-tetrakis{2-[2-pyridinyl-κ / N]phenyl-κC}diiridium(III) (abbreviation: [Ir(ppy)2Cl]2) and 180 ml of dichloromethane were added to a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.1 g of silver triflate and 86 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 1.5 g of HDPPP, 35 ml of 2-ethoxyethanol (abbreviation: 2-EE), and 35 ml of N,N-dimethylformamide (abbreviation: DMF) were added to the solid, and the mixture was refluxed for 17 hours under a nitrogen atmosphere. The resulting mixture was concentrated and purified by silica gel column chromatography using dichloromethane and hexane in a ratio of 1:1 as eluent.Subsequently, purification was performed by high-performance liquid chromatography using chloroform as the mobile phase. The resulting solution was concentrated, followed by recrystallization with a mixed solvent of dichloromethane and hexane to obtain an orange solid (yield 7.7%).

[0286] Using a train sublimation process, 0.22 g of the resulting orange solid was purified by sublimation. During sublimation purification, the solid was heated at 300 °C under a pressure of 1.5 Pa with an argon flow rate of 5 ml / min. After sublimation purification, an orange target solid was obtained in 64% yield. A synthesis scheme of step 3 is shown below.

[0287] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the orange solid obtained in step 3 are shown below. In Fig. 41 will be the 1 H-NMR diagram is shown. These results reveal that [Ir(dpappy)2(ppy)], which is the organometallic complex of one embodiment of the present invention, was obtained in this synthesis example.

[0288] 1 H NMR. δ (CD2Cl2): 6.29 (dd, 1H), 6.43 (dd, 1H), 6.72-6.69 (m, 3H), 6.75-7.73 (m, 2H), 6.80-6.79 (m, 2H), 6.89-6.86 (m, 1H), 6.95 (t, 1H), 7.10 (d, 1H), 7.42-7.19 (m, 26H), 7.60 (t, 1H), 7.65 (d, 1H), 7.71 (d, 1H), 7.87 (d, 1H).

[0289] Subsequently, a UV-VIS absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(dpappy)2(ppy)] and an emission spectrum thereof were measured. The measurement of the absorption spectrum was performed at room temperature using a UV-VIS spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. In addition, the measurement of the emission spectrum was performed at room temperature using a fluorescence spectrophotometer (FS920, manufactured by Hamamatsu Photonics KK) with the degassed dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The measurement results of the obtained absorption and emission spectra are shown in Fig. 42. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 42, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 42 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0290] As in Fig. As shown in Figure 42, the organometallic complex of one embodiment of the present invention, [Ir(dpappy)2(ppy)], has an emission peak at 534 nm, and yellow-green light emission was observed from the dichloromethane solution. [Example 10]<<Synthesebeispiel 8> >

[0291] This synthesis example describes a synthesis method of [4-(4,6-diphenyl-1,3,5-triazin-2-yl)-2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]bis[2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(mdppy)2(5dptznmdppy)]), which is an organometallic complex containing iridium as the central metal and having a ligand with a first framework having an electron-transport property and a second framework having a light-emitting property. A structural formula of [Ir(mdppy)2(5dptznmdppy)] is shown below. <Schritt 1: Synthese von 3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenylboronsäurepinacolester>

[0292] First, 10 g of 2-(3-bromophenyl)-4,6-diphenyl-1,3,5-triazine, 7.9 g of bis(pinacolato)diboron (abbreviation: (Bpin)2), 7.6 g of potassium acetate, and 125 ml of DMF were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Furthermore, 0.21 g of a [1,1'-bis(diphenylphosphino)ferrocene]palladium(II) dichloride-dichloromethane adduct (abbreviation: Pd(dppf)2Cl2·CH2Cl2) was added, and the mixture was heated and stirred at 150 °C for 3 hours. The solvent of the resulting reaction solution was distilled off and purified by silica gel column chromatography using toluene as the eluent to obtain 7.1 g of the target compound (a white solid in 63% yield). A synthesis scheme of Step 1 is shown below. <Schritt 2: Synthese von 5-Brom-2-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-4-methylpyridin>

[0293] Subsequently, a solution in which 6.0 g of 3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenylboronic acid pinacol ester obtained in step 1, 4.4 g of 2,5-dibromo-4-methylpyridine, and 3.9 g of potassium carbonate were dissolved in 21 ml of water, 84 ml of toluene, and 21 ml of ethanol were added to a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Furthermore, 0.64 g of tetrakis(triphenylphosphine)palladium(0) was added, and the mixture was heated and stirred at 100 °C for 13 hours. After the reaction, extraction with toluene was performed. The solvent was distilled off; Subsequently, recrystallization was performed using a mixed solvent of ethyl acetate and hexane to obtain 6.4 g of the target substance (a white solid, yield 97%). A synthesis scheme of step 2 is shown below. <Schritt 3: Synthese von 2-[3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenyl]-4-methyl-5-phenylpyridin (Abkürzung: H5dptznmdppy)>

[0294] Subsequently, 6.4 g of 5-bromo-2-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-4-methylpyridine obtained in step 2, 1.8 g of 2-phenylboronic acid, 3.4 g of tripotassium phosphate, 65 ml of toluene, and 6.5 ml of water were placed in a three-necked flask equipped with a reflux tube, and the atmosphere in the flask was replaced with nitrogen. Subsequently, 0.22 g of 2-dicyclohexylphosphino-2',6'-dimethoxybiphenyl (abbreviation: SPhos) and 0.12 g of tris(dibenzylideneacetone)dipalladium(0) (abbreviation: Pd2(dba)3) were added, and the mixture was heated for 8 hours. After the reaction, extraction with toluene was performed. Subsequently, purification was performed by silica gel column chromatography using toluene as the eluent to obtain 5.4 g of the target compound (a pale yellow solid in 86% yield). A synthesis scheme of step 3 is shown below. <Schritt 4: Synthese von Di-µ-chlor-tetrakis[2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]diiridium(III) (Abkürzung: [Ir(mdppy)2Cl]2)>

[0295] Subsequently, 3.2 g of 4-methyl-2,5-diphenylpyridine (abbreviation: Hmdppy), 1.9 g of iridium(III) chloride hydrate, 21 ml of 2-ethoxyethanol (abbreviation: 2-EE), and 7 ml of water were added to a round-bottomed flask equipped with a reflux tube, and the mixture was irradiated with microwaves (2.45 GHz, 100 W) for 1 hour while being bubbled with argon. The resulting mixture was filtered, followed by washing with methanol to obtain 3.2 g of a target substance (a yellow solid in a yield of 72%). A synthesis scheme of step 4 is further shown below. <Schritt 5: [4-(4,6-Diphenyl-1,3,5-triazin-2-yl)-2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]bis[2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]iridium(III) (Abkürzung: [Ir(mdppy)2(5dptznmdppy)])>

[0296] Subsequently, 3.2 g of [Ir(mdppy)2Cl]2 obtained in step 4 and 230 ml of dichloromethane were added to a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.5 g of silver triflate and 110 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The obtained mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 5.4 g of H5dptznmdppy obtained in step 3 and 75 ml of ethanol were added to the solid, and the mixture was refluxed for 17 hours under a nitrogen atmosphere. The obtained reactant was filtered, and a residue was purified by silica gel column chromatography using chloroform as the eluent. Subsequently, purification was carried out by high-performance liquid chromatography using chloroform as the mobile phase.The resulting solution was concentrated, followed by recrystallization with a mixed solvent of chloroform and hexane to obtain a yellow solid (yield 41%). A synthesis scheme of step 5 is shown below.

[0297] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the yellow solid obtained in step 5 are shown below. In Fig. 43 will be the 1 H NMR diagram is shown. These results reveal that [Ir(mdppy)2(5dptznmdppy)] was obtained in this synthesis example.

[0298] 1 H NMR. δ (CD2Cl2): 2.31 (s, 3H), 2.34 (s, 3H), 2.43 (s, 3H), 6.83-6.98 (m, 6H), 7.03-7.09 (m, 6H), 7.15 (d, 1H), 7.30-7.39 (m, 9H), 7.49 (d, 2H), 7.54 (s, 1H), 7.57-7.63 (m, 6H), 7.70 (t, 2H), 7.80 (s, 2H), 8.08 (s, 1H), 8.21 (d, 1H), 8.78 (d, 4H), 9.03 (s, 1H).

[0299] Subsequently, a UV-VIS absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(mdppy)2(5dptznmdppy)] and an emission spectrum thereof were measured. The measurement of the absorption spectrum was performed at room temperature using a UV-VIS spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. In addition, the measurement of the emission spectrum was performed at room temperature using a fluorescence spectrophotometer (FS920, manufactured by Hamamatsu Photonics KK) with the degassed dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The measurement results of the obtained absorption and emission spectra are shown in Fig. 44. The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 44, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 44 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0300] As in Fig. As shown in Figure 44, the organometallic complex of one embodiment of the present invention, [Ir(mdppy)2(5dptznmdppy)], has an emission peak at 519 nm, and yellow-green light emission was observed from the dichloromethane solution. [Example 11]<<Synthesebeispiel 9> >

[0301] This synthesis example describes a synthesis method of bis[4-(4,6-diphenyl-1,3,5-triazin-2-yl)-2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC][2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(5dptznmdppy)2(mdppy)]), which is an organometallic complex containing iridium as the central metal and having a ligand with a first framework having an electron-transport property and a second framework having a light-emitting property. A structural formula of [Ir(5dptznmdppy)2(mdppy)] is shown below. <Schritt 1: Synthese von 3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenylboronsäurepinacolester>

[0302] The synthesis of 3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenylboronic acid pinacol ester was carried out in a similar manner to Step 1 of Synthesis Example 8 in Example 10. <Schritt 2: Synthese von 5-Brom-2-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-4-methylpyridin>

[0303] The synthesis of 5-bromo-2-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-4-methylpyridine was carried out in a similar manner to Step 2 of Synthesis Example 8 in Example 10. <Schritt 3: Synthese von 2-[3-(4,6-Diphenyl-1,3,5-triazin-2-yl)phenyl]-4-methyl-5-phenylpyridin (Abkürzung: H5dptznmdppy)>

[0304] The synthesis of H5dptznmdppy was carried out in a similar manner to step 3 of Synthesis Example 8 in Example 10. <Schritt 4: Synthese von Di-µ-chlor-tetrakis[2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]diiridium(III) (Abkürzung: [Ir(mdppy)2Cl]2)>

[0305] The synthesis of [Ir(mdppy)2Cl]2 was carried out in a similar manner to step 4 of Synthesis Example 8 in Example 10. <Schritt 5: Synthese von [Ir(5dptznmdppy)2(mdppy)]>

[0306] 3.2 g of [Ir(mdppy)2Cl]2 obtained in step 4 and 230 ml of dichloromethane were placed in a three-necked flask, and the atmosphere in the flask was replaced with nitrogen. A mixed solution of 1.5 g of silver triflate and 110 ml of methanol was added dropwise to the flask, followed by stirring for 20 hours at room temperature. The resulting mixture was filtered through Celite, and the filtrate was concentrated to a solid. Subsequently, 5.4 g of H5dptznmdppy obtained in step 3 and 75 ml of ethanol were added to the solid, and the mixture was refluxed for 17 hours under a nitrogen atmosphere. The obtained reactant was filtered, and a residue was purified by silica gel column chromatography using chloroform as the eluent. Purification was then carried out by high-performance liquid chromatography using chloroform as the mobile phase.The resulting solution was concentrated, followed by recrystallization with a mixed solvent of chloroform and hexane to obtain a yellow solid (yield 7.1%). A synthesis scheme of step 5 is shown below.

[0307] It should be noted that the nuclear magnetic resonance ( 1 H-NMR spectroscopy analysis results of the yellow solid obtained in step 5 are shown below. In Fig. 45 will be the 1 H-NMR diagram is shown. These results reveal that [Ir(5dptznmdppy)2(mdppy)], which is the organometallic complex of one embodiment of the present invention, was obtained in this synthesis example.

[0308] 1 H-NMR. δ (CD2Cl2): 2,34 (s, 3H), 2,43 (s, 3H), 2,45 (s, 3H), 6,89-7,00 (m, 3H), 7,05-7,12 (m, 6H), 7,20 (dd, 2H), 7,31-7,40 (m, 9H), 7,51 (s, 1H), 7,55-7,65 (m, 14H), 7,74 (d, 1H), 7,83 (s, 1H), 8,12 (s, 2H), 8,22 (d, 1H), 8,27 (d, 1H), 8,76 (d, 4H), 8,80 (d, 4H), 9,08 (d, 2H).

[0309] Subsequently, a UV-VIS absorption spectrum (hereinafter referred to simply as "absorption spectrum") of a dichloromethane solution of [Ir(5dptznmdppy)2(mdppy)] and an emission spectrum thereof were measured. The measurement of the absorption spectrum was performed at room temperature using a UV-VIS spectrophotometer (V550, manufactured by JASCO Corporation) with the dichloromethane solution (0.010 mmol / L) placed in a quartz cell. In addition, the measurement of the emission spectrum was performed at room temperature using a fluorescence spectrophotometer (FS920, manufactured by Hamamatsu Photonics KK) with the degassed dichloromethane solution (0.010 mmol / L) placed in a quartz cell. The measurement results of the obtained absorption and emission spectra are shown in Fig. 46. ​​The horizontal axis represents the wavelength, and the vertical axes represent the absorption intensity and the emission intensity. In Fig. 46, two solid lines are shown: A thin solid line represents the absorption spectrum and a thick solid line represents the emission spectrum. The Fig. The absorption spectrum shown in Figure 46 is a result obtained by subtracting a measured absorption spectrum of only dichloromethane placed in a quartz cell from the measured absorption spectrum of the dichloromethane solution (0.010 mmol / L) in a quartz cell.

[0310] As in Fig. As shown in Figure 46, the organometallic complex of one embodiment of the present invention, [Ir(5dptznmdppy)2(mdppy)], has an emission peak at 510 nm, and yellow-green light emission was observed from the dichloromethane solution. [Example 12]

[0311] In this example, element structures, manufacturing methods, and properties of the following light-emitting elements are described: as a light-emitting element of an embodiment of the present invention, a light-emitting element 4 using [Ir(mdppy)2(5dptznmdppy)] (structural formula (103)) as the guest material of the light-emitting layer, which was described in Example 10, and a comparative light-emitting element 2 using [Ir(ppy)3] as the guest material of the light-emitting layer. It should be noted that Fig. Figure 21 illustrates an element structure of the light-emitting elements used in this example, and Table 5 shows the specific structures. The chemical formulas of the materials used in this example are shown below. [Table 5] Hole injection layer Hole transport layer Light-emitting layer Electron transport layer Electron injection layer 40 nm 20 nm 40 nm 20 nm 10 nm 1 nm Light-emitting element 4 DBT3P-II : MoOx (2:1) PCCP mPCCzPTzn-02 : PCCP : Ir(mdppy)2(5dptznmdppy) mPCCzPTzn-02 NBPhen LiF Light-emitting reference element 2 mPCCzPTzn-02 : PCCP : Ir(ppy)3 <Herstellung der Licht emittierenden Elemente>

[0312] For each of the light-emitting elements described in this example, as shown in Fig. 21, a hole injection layer 1911, a hole transport layer 1912, a light emitting layer 1913, an electron transport layer 1914, and an electron injection layer 1915 are disposed in this order over an anode 901 formed over a substrate 1900, and a cathode 1903 is disposed over the electron injection layer 1915.

[0313] First, the anode 1901 was formed over the substrate 1900. The electrode area was set to 4 mm 2 (2 mm × 2 mm). A glass substrate was used as the substrate 1900. The anode 1901 was formed by a sputtering method using indium tin oxide (ITO) containing silicon oxide to a thickness of 70 nm.

[0314] As a pretreatment, a surface of the substrate was washed with water, baked at 200 °C for one hour, and then UV ozone treatment was performed for 370 seconds. Afterward, the substrate was transferred to a vacuum evaporation device, where the pressure was increased to approximately 10 -4 Pa, vacuum baking was performed at 170 °C for 60 minutes in a heating chamber of the vacuum evaporation apparatus, and then the substrate was cooled for approximately 30 minutes.

[0315] Next, the hole injection layer 1911 was formed over the anode 1901. After the pressure in the vacuum evaporation device was reduced to 10 -4 Pa, the hole injection layer was formed in 1911 by co-evaporation of 1,3,5-tri(dibenzothiophen-4-yl)benzene (abbreviation: DBT3P-II) and molybdenum oxide to a thickness of 40 nm, with the weight ratio of DBT3P-II to molybdenum oxide being 2:1.

[0316] Subsequently, the hole transport layer 1912 was formed over the hole injection layer 1911. The hole transport layer 1912 was formed by evaporating 9-phenyl-9H-3-(9-phenyl-9H-carbazol-3-yl)carbazole (abbreviation: PCCP) to a thickness of 20 nm.

[0317] Next, the light-emitting layer 1913 was formed over the hole transport layer 1912.

[0318] The light-emitting layer 1913 in the light-emitting element 4 was formed by co-evaporation using 9-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9'-phenyl-2,3'-bi-9H-carbazole (abbreviation: mPCCzPTzn-02) as the host material, using PCCP as the auxiliary material, and using [4-(4,6-diphenyl-1,3,5-triazin-2-yl)-2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]bis[2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(mdppy)2(5dptznmdppy)]) as the guest material (phosphorescent material). where the weight ratio of mPCCzPTzn-02 to PCCP and [Ir(mdppy)2(5dptznmdppy)] was 0.6:0.4:0.10. The thickness was set to 40 nm.

[0319] The light-emitting layer 1913 in Comparative Light-Emitting Element 2 was formed by co-evaporation using mPCCzPTzn-O2 as the host material, PCCP as the auxiliary material, and [Ir(ppy)3] as the guest material (phosphorescent material), with the weight ratio of mPCCzPTzn-O2 to PCCP and [Ir(ppy)3] being 0.5:0.5:0.10. The thickness was set to 20 nm. Furthermore, mPCCzPTzn-O2, PCCP, and [Ir(ppy)3] were deposited by co-evaporation, with the weight ratio of mPCCzPTzn-O2 to PCCP and [Ir(ppy)3] being 0.8:0.2:0.1. The thickness was set to 20 nm. Consequently, the light-emitting layer 1913 has a multilayer structure with a thickness of 40 nm.

[0320] Next, the electron-transport layer 1914 was formed over the light-emitting layer 1913. The electron-transport layer 1914 was formed as follows: mPCCzPTzn-02 and bathophenanthroline (abbreviation: Bphen) were sequentially deposited by evaporation to a thickness of 15 nm and 10 nm, respectively.

[0321] Subsequently, the electron injection layer 1915 was formed over the electron transport layer 1914. The electron injection layer 1915 was formed by evaporating lithium fluoride (LiF) to a thickness of 1 nm.

[0322] Thereafter, the cathode 1903 was formed over the electron injection layer 1915. The cathode 1903 was formed using aluminum by an evaporation method to a thickness of 200 nm.

[0323] Through the above steps, the light-emitting elements, each including an EL layer between a pair of electrodes, were formed over the substrate 1900. The hole-injection layer 1911, the hole-transport layer 1912, the light-emitting layer 1913, the electron-transport layer 1914, and the electron-injection layer 1915 described above are functional layers constituting the EL layer of one embodiment of the present invention. Furthermore, in all evaporation steps of the above manufacturing method, evaporation was performed by a resistance heating method.

[0324] Each of the light-emitting elements prepared as described above was sealed using another substrate (not shown). Sealing using the substrate was performed in the following manner: The another substrate was attached to the substrate 1900 with a sealant in a glove box containing a nitrogen atmosphere, a sealing material was applied to enclose the light-emitting element formed over the substrate 1900, and then irradiated with 365 nm UV light at 6 J / cm 2 and heat treatment was carried out at 80 °C for 1 hour. <<Betriebseigenschaften der Licht emittierenden Elemente> >

[0325] The operating characteristics of the fabricated light-emitting elements (Light-emitting Element 4 and Comparative Light-emitting Element 2) were measured. Note that the measurement was conducted at room temperature (in an atmosphere maintained at 25 °C). The results are presented in Fig. 47 to Fig. 51 shown.

[0326] The results reveal that the light-emitting elements of the embodiments of the present invention (Light-emitting Element 4 and Comparative Light-emitting Element 2) exhibit excellent current efficiency and high external quantum efficiency. Table 6 shows the initial values ​​of the main characteristics of the light-emitting elements at about 1000 cd / m 2 . [Table 6] Voltage (V) Current (mA) Current density (mA / cm 2 ) Chromaticity (x,y) Power efficiency (cd / A) Power efficiency (Im / W) external quantum efficiency (%) Light-emitting element 4 2,8 0,053 1,3 (0,33,0,64) 94 106 26 Light-emitting reference element 2 3,2 0,051 1,3 (0,31,0,64) 85 83 23

[0327] Fig. Figure 52 shows the emission spectra of the light-emitting element 4 and the comparative light-emitting element 2, through which a current with a current density of 2.5 mA / cm 2 flows. As in Fig. 52, the emission spectrum of the light-emitting element 4 has a peak at about 520 nm, which is presumably due to the light emission from [Ir(mdppy)2(5dptznmdppy)], the organometallic complex, contained in the light-emitting layer 1913. The emission spectrum of the comparative light-emitting element 2 has a peak at about 516 nm, which is presumably due to the light emission from [Ir(ppy)3], the organometallic complex, contained in the light-emitting layer 1913.

[0328] Note that the organometallic complex of one embodiment of the present invention used in the light-emitting element 4 has a ligand in which a diphenyltriazine skeleton is bonded to a diphenylpyridine skeleton, allowing carriers (electrons or holes) to be easily injected and transported. As a result, the emission efficiency of the element can be improved and the driving voltage can be reduced, and the light-emitting element 4 has higher current efficiency and lower driving voltage compared to the comparative light-emitting element 2.

[0329] Next, Fig. 53 is a graph showing a change in luminance versus operating time under the following conditions: the current value was 2 mA and the current density was constant. These results reveal that the light-emitting element 4, which is the light-emitting element of one embodiment of the present invention, is a light-emitting element having favorable reliability, just like the comparative light-emitting element 2. [Example 13]

[0330] In this example, element structures, manufacturing methods, and properties of the following light-emitting elements are described: as a light-emitting element of an embodiment of the present invention, a light-emitting element 5 using [Ir(ppy)2(dpappy)] (structural formula (104)) as the guest material of the light-emitting layer, which was described in Example 8, and a comparative light-emitting element 3 using [Ir(ppy)3] as the guest material of the light-emitting layer. It should be noted that Fig. Figure 21 illustrates an element structure of the light-emitting elements described in this example, and Table 7 shows the specific structures. The chemical formulas of the materials used in this example are shown below. [Table 7] Hole injection layer Hole transport layer Light-emitting layer Electron transport layer Electron injection layer 40 nm 20 nm 40 nm 20 nm 10 nm 1 nm Light-emitting element 5 DBT3P-II : MoOx (2:1) PCCP mPCCzPTzn-02 : PCBBiF : Ir(ppy)2(dpappy) (0.6:0.4:0.1) mPCCzPTzn-02 NBPhen LiF Light-emitting reference element 3 mPCCzPTzn-02 : PCBBiF : Ir(PPY)3 (0.6:0.4:0.1) <Herstellung der Licht emittierenden Elemente>

[0331] For each of the light-emitting elements described in this example, as shown in Fig. 21, a hole injection layer 1911, a hole transport layer 1912, a light emitting layer 1913, an electron transport layer 1914, and an electron injection layer 1915 are disposed in this order over an anode 901 formed over a substrate 1900, and a cathode 1903 is disposed over the electron injection layer 1915.

[0332] First, the anode 1901 was formed over the substrate 1900. The electrode area was set to 4 mm 2 (2 mm × 2 mm). A glass substrate was used as the substrate 1900. The anode 1901 was formed by a sputtering method using indium tin oxide (ITO) containing silicon oxide to a thickness of 70 nm.

[0333] As a pretreatment, a surface of the substrate was washed with water, baked at 200 °C for one hour, and then UV ozone treatment was performed for 370 seconds. Afterward, the substrate was transferred to a vacuum evaporation device, where the pressure was increased to approximately 10 -4 Pa, vacuum baking was performed at 170 °C for 60 minutes in a heating chamber of the vacuum evaporation apparatus, and then the substrate was cooled for approximately 30 minutes.

[0334] Next, the hole injection layer 1911 was formed over the anode 1901. After the pressure in the vacuum evaporation device was reduced to 10 -4 Pa, the hole injection layer was formed in 1911 by co-evaporation of 1,3,5-tri(dibenzothiophen-4-yl)benzene (abbreviation: DBT3P-II) and molybdenum oxide to a thickness of 40 nm, with the weight ratio of DBT3P-II to molybdenum oxide being 2:1.

[0335] Subsequently, the hole transport layer 1912 was formed over the hole injection layer 1911. The hole transport layer 1912 was formed by evaporating 9-phenyl-9H-3-(9-phenyl-9H-carbazol-3-yl)carbazole (abbreviation: PCCP) to a thickness of 20 nm.

[0336] Next, the light-emitting layer 1913 was formed over the hole transport layer 1912.

[0337] The light-emitting layer 1913 in the light-emitting element 5 was formed by co-evaporation using 9-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9'-phenyl-2,3'-bi-9H-carbazole (abbreviation: mPCCzPTzn-02) as a host material, using N-(1,1'-biphenyl-4-yl)-9,9-dimethyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9H-fluoren-2-amine (abbreviation: PCBBiF) as an auxiliary material, and using [2-(4-diphenylamino-2-pyridinyl-κN)phenyl-rC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)2(dpappy)]) was formed as the guest material (phosphorescent material), with the weight ratio of mPCCzPTzn-02 to PCBBiF and [Ir(ppy)2(Czppy)] being 0.6:0.4:0.1. The thickness was set to 40 nm.

[0338] The light-emitting layer 1913 in Comparative Light-Emitting Element 3 was formed by co-evaporation using mPCCzPTzn-02 as the host material, PCBBiF as the auxiliary material, and [Ir(ppy)3] as the guest material (phosphorescent material), with the weight ratio of mPCCzPTzn-02 to PCBBiF and [Ir(ppy)3] being 0.6:0.4:0.1. The thickness was set to 40 nm.

[0339] Next, the electron-transport layer 1914 was formed over the light-emitting layer 1913. The electron-transport layer 1914 was formed as follows: mPCCzPTzn-02 and 2,9-bis(naphthalen-2-yl)-4,7-diphenyl-1,10-phenanthroline (abbreviation: NBphen) were sequentially deposited by evaporation to a thickness of 20 nm and 10 nm, respectively.

[0340] Subsequently, the electron injection layer 1915 was formed over the electron transport layer 1914. The electron injection layer 1915 was formed by evaporating lithium fluoride (LiF) to a thickness of 1 nm.

[0341] Thereafter, the cathode 1903 was formed over the electron injection layer 1915. The cathode 1903 was formed using aluminum by an evaporation method to a thickness of 200 nm.

[0342] Through the above steps, the light-emitting elements, each including an EL layer between a pair of electrodes, were formed over the substrate 1900. The hole-injection layer 1911, the hole-transport layer 1912, the light-emitting layer 1913, the electron-transport layer 1914, and the electron-injection layer 1915 described above are functional layers constituting the EL layer of one embodiment of the present invention. Furthermore, in all evaporation steps of the above manufacturing method, evaporation was performed by a resistance heating method.

[0343] Each of the light-emitting elements prepared as described above was sealed using another substrate (not shown). Sealing using the substrate was performed in the following manner: The another substrate was attached to the substrate 1900 with a sealant in a glove box containing a nitrogen atmosphere, a sealing material was applied to enclose the light-emitting element formed over the substrate 1900, and then irradiated with 365 nm UV light at 6 J / cm 2 and heat treatment was carried out at 80 °C for 1 hour. <<Betriebseigenschaften der Licht emittierenden Elemente> >

[0344] The operating characteristics of the fabricated light-emitting elements (Light-emitting Element 5 and Comparative Light-emitting Element 3) were measured. Note that the measurement was conducted at room temperature (in an atmosphere maintained at 25 °C). The results are presented in Fig. 54 to Fig. 58 shown.

[0345] These results reveal that the light-emitting elements of the embodiments of the present invention (Light-emitting Element 5 and Comparative Light-emitting Element 3) exhibit excellent current efficiency and high external quantum efficiency. Table 8 shows the initial values ​​of the main characteristics of the light-emitting elements at about 1000 cd / m 2 . [Table 8] Voltage (V) Current (mA) Current density (mA / cm 2 ) Chromaticity (x,y) Power efficiency (cd / A) Power efficiency (Im / W) external quantum efficiency (%) Light-emitting element 5 2,7 0,068 1,7 (0,33,0,63) 62 72 17 Light-emitting reference element 3 2,5 0,035 0,9 (0,31,0,64) 47 59 13

[0346] Fig. Figure 59 shows the emission spectra of the light-emitting element 5 and the comparative light-emitting element 3, through which a current with a current density of 2.5 mA / cm 2 flows. As in Fig. 59, the emission spectrum of the light-emitting element 5 has a peak at about 523 nm, which is presumably due to the light emission from [Ir(ppy)2(dpappy)], the organometallic complex, contained in the light-emitting layer 1913. The emission spectrum of the comparative light-emitting element 3 has a peak at about 517 nm, which is presumably due to the light emission from [Ir(ppy)3], the organometallic complex, contained in the light-emitting layer 1913.

[0347] It should be noted that the organometallic complex of one embodiment of the present invention used in the light-emitting element 5 has a ligand in which a diphenylamine skeleton is bonded to a diphenylpyridine skeleton, so that charge carriers (electrons or holes) can be easily injected and transported. Thus, the light-emitting element 5 can be a light-emitting element with favorable emission efficiency.

[0348] PCBBiF was used as the auxiliary material in the light-emitting layer of light-emitting element 5 and comparative light-emitting element 3. As shown in the above structural formula, PCBBiF is an organic substance containing a diphenylamine skeleton. It was found that it is advantageous if the skeleton contained in the auxiliary material PCBBiF and the charge-transport skeleton contained in the light-emitting material are the same. [Example 14]

[0349] This example presents calculation results regarding the HOMO and LUMO distributions of the organometallic complexes represented by structural formulas (C1) to (C3), which are structures of one embodiment of the present invention. The structural formulas of the organometallic complexes represented by (C1) to (C3) are shown below.

[0350] Gaussian 09 was used for molecular orbital calculations. 6-311 G was used as the basis function, and a structural optimization of the singlet ground state (S0) of each molecule was performed using B3PW91 \6-311 G.

[0351] Fig. Figure 60 shows the electron density distribution of the HOMO and LUMO of each structure obtained by calculation.

[0352] How Fig. As shown in Figure 60, the HOMO of the organometallic complex represented by structural formula (C1) is mainly distributed in a phenylpyridine ligand and an iridium ion, and the LUMO thereof is mainly distributed in diphenyltriazine. The HOMO of the organometallic complex represented by structural formula (C2) is also mainly distributed in a phenylpyridine derivative ligand and an iridium ion, and the LUMO thereof is mainly distributed in diphenyltriazine. The HOMO of the organometallic complex represented by structural formula (C3) is mainly distributed in a phenylpyridine ligand and an iridium ion, and the LUMO thereof is mainly distributed in a phenylpyrimidine derivative ligand.

[0353] Consequently, the LUMO of the organometallic complex represented by structural formula (C1) and the organometallic complex represented by structural formula (C2) is distributed in the diphenyltriazine, which is the framework with charge-carrier transport properties, and it is suggested that it affects charge-carrier transport and electron injection. On the other hand, in the organometallic complex represented by structural formula (C3), the LUMO is not distributed in the triazine, which is the framework with charge-carrier transport properties, and it can be assumed that it has less effect on charge-carrier transport and electron injection.

[0354] One embodiment of the present invention is a material for a light-emitting element comprising an organic compound whose molecular weight is 1300 or less and which has, in one molecule, a first skeleton having a charge-carrier transport property and a second skeleton having a light-emitting property. Considering the above calculation results, the LUMO of the organometallic complexes represented by (C1) and (C2) is distributed in the diphenyltriazine skeleton, thus they can be organic compounds in which the diphenyltriazine skeleton corresponds to the first skeleton having a charge-carrier transport property, which carries out charge-carrier transport and electron injection, and the phenylpyridine skeleton corresponds to the second skeleton having a light-emitting property.On the other hand, in the organometallic complex represented by (C3), the LUMO is not distributed in the dimethyltriazine framework, and the LUMO is distributed in the phenylpyridine framework, which suggests that, with respect to the transport of charge carriers and the injection of electrons, the framework with a light-emitting property simultaneously undertakes both the transport of charge carriers and the emission of light. Reference symbol 101 Anode 102 Cathode 103 EL layer 111 Hole injection layer 112 Hole transport layer 113 Light-emitting layer 114 Electron transport layer 115 Electron injection layer 116 Charge generation layer 117 p-type layer 118 Electron conduction layer 119 Electron injection buffer layer 400 substrate 401 Anode 403 EL layer 404 Cathode 405 Sealants 406 Sealants 407 Sealing substrate 412 Contact Point 420 IC chip 501 Anode 502 Cathode 511 first light-emitting unit 512 second light-emitting unit 513 Charge generation layer 601 Driver circuit section (source line driver circuit) 602 pixel section 603 Driver circuit section (gate line driver circuit) 604 Sealing substrate 605 Sealant 607 Room 608 Line 609 flexible printed circuit 610 element substrate 611 Switching FET 612 Current control FET 613 Anode 614 Insulator 616 EL layer 617 Cathode 618 Light-emitting element 730 insulating film 770 insulating planarization film 772 leading film 782 Light-emitting element 783 Droplet ejection device 784 droplets 785 shift 786 EL layer 788 leading film 901 housing 902 Liquid crystal layer 903 backlight unit 904 housing 905 driver IC 906 connection 951 Substrat 952 Electrode 953 insulating layer 954 Partition layer 955 EL layer 956 Electrode 1001 Substrat 1002 Basic Insulating Film 1003 Gate insulating film 1006 Gate electrode 1007 Gate electrode 1008 Gate electrode 1020 first interlayer insulating film 1021 second interlayer insulating film 1022 Electrode 1024W anode 1024R anode 1024G anode 1024B anode 1025 partition wall 1028 EL layer 1029 cathode 1031 Sealing substrate 1032 Sealants 1033 transparent base material 1034R red paint layer 1034G green color layer 1034B blue paint layer 1035 Black Matrix 1037 third interlayer insulating film 1040 pixel section 1041 Driver circuit section 1042 Peripheral section 1400 droplet ejector 1402 Substrat 1403 Droplet ejection agents 1404 imaging media 1405 head 1406 dashed line 1407 tax revenues 1408 storage medium 1409 Image processing equipment 1410 computers 1411 Marking 1412 head 1413 Material supply source 1414 Material supply source 1415 Material supply source 1416 head 1900 substrate 1901 Anode 1903 Cathode 1911 hole injection layer 1912 hole transport layer 1913 Light-emitting layer 1914 Electron transport layer 1915 Electron injection layer 2001 Housing 2002 Light Source 3001 Lighting device 5000 display area 5001 display area 5002 display area 5003 Display area 5004 Display area 5005 display area 7101 housing 7103 Display section 7105 feet 7107 Display section 7109 control button 7110 remote control 7201 Main part 7202 housing 7203 Display section 7204 keyboard 7205 external connection port 7206 Pointing device 7210 second display section 7401 housing 7402 Display section 7403 control knob 7404 external connection port 7405 speakers 7406 Microphone 9033 clasp 9034 switches 9035 power switch 9036 Switch 9038 control switch 9310 portable information terminal 9311 display screen 9312 display area 9313 Joint 9315 housing 9630 case 9631 Display section 9631a Display section 9631b Display section 9632a Touchscreen area 9632b Touchscreen area 9633 solar cell 9634 charge / discharge control circuit 9635 battery 9636 DC-DC converter 9637 control button 9638 converters 9639 Button< / beleuchtungsvorrichtung>

Claims

[1] Material for a light-emitting element comprising: an organic compound, wherein the organic compound has in one molecule a first framework with a charge carrier transport property and a second framework with a light emission property, and wherein the molecular weight of the organic compound is 1300 or less, wherein the organic compound is an organometallic complex further containing a central metal, wherein the organometallic complex has at least two different ligands, wherein one of the two different ligands comprises the second framework with a light-emitting property, and where the other of the two different ligands has the first framework with an electron transport property. [2] The material for a light-emitting element according to claim 1, wherein the first framework is a framework having the LUMO. [3] The material for a light-emitting element according to claim 1, wherein the first framework is directly bonded to the second framework. [4] The material for a light-emitting element according to claim 1, wherein the first skeleton and the second skeleton are bonded to each other via a meta-phenylene group or a biphenyl-3,3'-diyl group. [5] Material for a light-emitting element comprising: an organic compound, wherein the organic compound has in one molecule a first framework with a hole transport property, a second framework with an electron transport property and a third framework with a light emission property, and wherein the molecular weight of the organic compound is 1300 or less. [6] The material for a light-emitting element according to claim 5, wherein the first framework is a framework having the HOMO. [7] The material for a light-emitting element according to claim 5, wherein the second framework is a framework having the LUMO. [8] The material for a light-emitting element according to claim 5, wherein the first framework and / or the second framework is / are directly bonded to the third framework. [9] The material for a light-emitting element according to claim 5, wherein the first skeleton and / or the second skeleton are bonded to the third skeleton via a meta-phenylene group or a biphenyl-3,3'-diyl group. [10] The material for a light-emitting element according to claim 1, wherein the organic compound emits a phosphorescent light. [11] A material for a light-emitting element according to claim 1, wherein the central metal is iridium. [12] The material for a light-emitting element according to claim 11, wherein the first skeleton having a charge carrier transport property in the organometallic complex is a diphenyltriazine skeleton. [13] The material for a light-emitting element according to claim 1, wherein one of the ligands of the organometallic complex has a framework having a hole transport property. [14] Light-emitting element (782) comprising: the material for a light-emitting element according to claim 1, wherein the material for a light-emitting element according to claim 1 is deposited and used by an evaporation method. [15] Light-emitting element (782) comprising: the material for a light-emitting element according to claim 1, wherein the material for a light-emitting element according to claim 1 is deposited and used by a wet process. [16] Light-emitting element (782) comprising: a light-emitting layer (113) comprising a first organic compound and the material for a light-emitting element according to claim 1, wherein the organic compound contained in the material for a light-emitting element is an iridium complex, and wherein a structure similar to that of the first framework having a charge carrier transport property of the iridium complex is contained in at least a part of a framework contained in the first organic compound. [17] The light-emitting element (782) according to claim 16, wherein the light-emitting layer (113) further contains a second organic compound. [18] The light-emitting element (782) of claim 16, wherein the first framework is an amine framework. [19] The light-emitting element (782) of claim 16, wherein the first framework is a diphenylamine framework. [20] An organometallic complex represented by the following structural formula:wherein the organometallic complex is used in a light-emitting element. [21] Organometallic complex represented by the following structural formula:wherein the organometallic complex is used in a light-emitting element. [22] An organometallic complex represented by the following structural formula:wherein the organometallic complex is used in a light-emitting element. [23] Organometallic complex represented by the following structural formula, wherein the organometallic complex is used in a light-emitting element. [24] Organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element. [25] An organometallic complex represented by the following structural formula:wherein the organometallic complex is used in a light-emitting element. [26] Organometallic complex represented by the following structural formula: wherein the organometallic complex is used in a light-emitting element.

Citation Information

Patent Citations

  • Organic compound, organic el element and display

    JP2003231692A

  • Phosphorescent Iridium Metal Complex, Light-Emitting Element, Light-Emitting Device, Electronic Appliance, and Lighting Device

    US20130088144A1

  • Organometallic complex and organic light-emitting diode including the same

    US20140209873A1

  • Metal complexes

    WO2011032626A1

  • Metal complexes

    WO2016000803A1