METHOD FOR SHAPING A COMPOSITE SHOVEL, COMPOSITE SHOVEL AND SHAPING TOOL FOR A COMPOSITE SHOVEL
The method addresses fiber wave motion and uneven foaming in composite blades by using space holding members and tension application, achieving consistent bending stiffness and natural frequency for improved performance.
Patent Information
- Application Number
- DE112018005440
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-25
- Filing Date
- 2018-09-20
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2038-09-20
AI Technical Summary
Existing composite blades face issues with fiber wave motion and uneven foaming agent distribution during thermal curing, leading to reduced bending rigidity, natural frequency variation, and compromised aerodynamic performance.
A method involving the use of space holding members and tension application to laminates, along with controlled expansion of a foaming agent, to maintain internal space and adjust thickness uniformly, ensuring consistent bending stiffness and natural frequency.
The method effectively suppresses fiber wave motion and ensures appropriate foaming agent distribution, resulting in a composite blade with desired performance characteristics and reduced weight.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical area
[0001] The present invention relates to a method for forming a composite shovel, a composite shovel and a forming tool for a composite shovel. State of the art
[0002] In the prior art, a gas turbine blade having an airfoil section extending from a blade end to a blade root is known as a composite blade (see, for example, JP H09-303104 A). The airfoil section includes a metal part in which a surface concavity is formed and a foam part provided in the surface concavity of the metal part. The metal part and the foam part are surrounded by a composite skin and bonded to the composite skin. Furthermore, the airfoil section is provided with an erosion protection layer covering the composite skin.
[0003] From DE 21 09 934 A, a method for manufacturing a shell component and a shell component manufactured by the method are known, on which the preamble of claims 1, 11, 13, 14 and 17 is based. In this method, shell parts are manufactured and joined to a core, wherein each shell component is inserted or molded into a shell mold half, wherein one or more support beams, support bolts, or insert bodies are then inserted into a shell component, wherein a bead of plastic or adhesive is subsequently applied in the area of the parting line between the shell components, in particular into both shell components, wherein the shell mold half is then joined under pressure, displacing the bead of plastic or adhesive, and wherein a foaming plastic mass in a reaction state is then filled, in particular pressed, into the shell component cavity through the support beam or the filling tube.
[0004] WO 2012 / 010 331 A1 describes a forming tool with two forming tools arranged one above the other to form a rotor blade of a wind turbine between them.
[0005] From DE 10 2008 022 548 A1, a rotor blade for a wind turbine is known, which has two shell halves extending along the longitudinal direction of the rotor blade from a blade root to the blade tip and connected to each other along their circumference, and at least one web device arranged between the shell halves and connected to them. Summary of the inventionTechnical problem
[0006] Furthermore, there is a composite blade that contains no metal parts, and another type of composite blade in which a foaming agent is incorporated inside a blade body formed by laminating reinforcing fiber preform materials. During thermal curing, the foaming agent is pressed from the inside of the composite blade towards a mold to form a blade with high dimensional accuracy while suppressing the formation of voids in the blade body.
[0007] However, with composite blades, there is a case where, during thermal curing, the reinforcing fiber preform material of the laminated blade body flows before the foaming agent expands, resulting in fiber wave motion. Furthermore, there is a case where, during foaming agent expansion, the foaming agent is not adequately filled into the interior of the blade body, and its thickness becomes insufficient. This reduces the flexural stiffness and natural frequency of the composite blade. If the natural frequency of the composite blade is reduced, the blade thickness must be increased to achieve the required flexural stiffness, thus reducing aerodynamic performance.Furthermore, in a case where the wave motion of the fibers and an individual difference in the thickness of the foaming agent occur, there is also a problem that a variation in the natural frequency of the composite blade increases, which makes it difficult to perform detuning to avoid a resonance point.
[0008] Therefore, the present invention has an object to provide a method for forming a composite blade, a composite blade and a mold for a composite blade, in which it is possible to form a high-quality composite blade that meets the required performance while reducing the weight. Solution to the problem
[0009] According to the present invention, there is provided a method for forming a composite blade having the features of claim 1 or 11, in which a composite blade made of a composite material is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade, a suction-side part, which is a part on a back side, and a pressure-side part, which becomes a ventral side, are superimposed and bonded to each other, the method including: a laying-up step of forming a suction-side laminate by laminating the reinforcing fiber preform material on a suction-side mold for forming the suction-side part, and forming a pressure-side laminate by laminating the reinforcing fiber preform material on a pressure-side mold for forming the pressure-side part;a space-holding part alignment step of arranging a space-holding part to hold an interior space formed by overlapping the suction-side laminate and the pressure-side laminate; a mold setting step of adjusting the suction-side mold tool and the pressure-side mold tool so that the suction-side laminate and the pressure-side laminate are overlapped and of arranging the foaming agent in the interior space held by the space-holding part; and a curing step of pressing the suction-side laminate and the pressure-side laminate towards the suction-side mold tool and the pressure-side mold tool from the inside by expanding the foaming agent through heating, and heating and curing the suction-side laminate and the pressure-side laminate.
[0010] In this configuration, the space-holding element is positioned, allowing the foaming agent to expand while the suction-side and pressure-side laminates undergo thermal curing in a state that holds the interior space. This space-holding element effectively confines the interior space, suppressing the flow of the reinforcing fiber preform material from both the suction-side and pressure-side laminates during thermal curing. This reduces fiber wave motion in the suction-side and pressure-side sections. Furthermore, the space-holding element allows for the appropriate filling of the interior space with the expanded foaming agent, thus enabling adjustment of the foaming agent thickness.For this reason, it is possible to adjust the thickness in one lay-up direction of each of the suction-side part and the pressure-side part, which are the suction-side laminate and the pressure-side laminate after curing, to the required thickness. In this way, it is possible to adjust the flexural rigidity of the composite blade to the required flexural rigidity, and therefore, it is also possible to adjust the natural frequency of the composite blade to the required natural frequency.
[0011] Furthermore, it is preferred that the space-holding part includes a suction-side space-holding part arranged on the suction-side laminate and a pressure-side space-holding part arranged on the pressure-side laminate.
[0012] According to this configuration, the space-holding part can be divided into the suction-side space-holding part and the pressure-side space-holding part, and therefore it is possible to easily arrange the foaming agent in the interior space held by the space-holding part.
[0013] Further, it is preferable that in the space-holding part aligning step, the suction-side space-holding part and the pressure-side space-holding part are arranged facing each other, an adhesive is arranged between the suction-side space-holding part and the pressure-side space-holding part at each of both end parts of the suction-side space-holding part and the pressure-side space-holding part in a blade width direction of the composite blade, and both end parts of the suction-side space-holding part and the pressure-side space-holding part are bonded to each other to form the space-holding part.
[0014] According to this configuration, the space-holding part can be formed integrally by bonding both end parts of the suction-side space-holding part and the pressure-side space-holding part with the adhesive.
[0015] Furthermore, it is preferred that in the suction-side space-holding part and the pressure-side space-holding part, the thickness on a middle section side in the blade width direction of the composite blade is made thinner than the thickness on an end section side.
[0016] According to this configuration, the suction-side space-holding part and the pressure-side space-holding part become thinner from the end part in the blade width direction towards the middle section, thereby keeping the stiffness constant in the blade width direction and thus making the expansion pressure from the foaming agent inside uniform.
[0017] According to the invention of claim 1, the space holding part is provided on the entire surface along an inner surface of the interior space.
[0018] According to this configuration, the entire inner surface of the interior space can be held by the space-holding member. Furthermore, the expanding foaming agent can press the entire inner surface of the interior space formed by the suction-side laminate and the pressure-side laminate through the space-holding member.
[0019] Further, it is preferable that a resin material or a cured composite material is used as the space-holding member.
[0020] According to this configuration, it is possible to use a cost-effective resin material as the space-holding element. Furthermore, a cured composite material, identical to that of the composite blade, can be used as the space-holding element, and therefore it is possible to perform the thermal curing heating of the composite blade without changing the heating conditions.
[0021] Furthermore, it is preferred that the space-holding part, in a case where a cured composite material is used, contains a reinforcing fiber preform material in which a fiber direction of reinforcing fibers contained in the composite material has an orientation of ±45° with a blade longitudinal direction of the composite blade as a reference.
[0022] This configuration allows the space-holding part to be provided with elastic force. This allows the space-holding part to be bent by the expansion pressure of the foaming agent due to its elastic force, and thus, the space-holding part can be appropriately pressed against the suction-side laminate and the pressure-side laminate. As reinforcing fibers, not only carbon fibers but also highly elastic resin fibers such as Kevlar (registered trademark) or Vectran (registered trademark) can be used as resin fibers with higher elasticity than carbon fibers.
[0023] Furthermore, it is preferred that the space-holding element has a heat resistance capable of maintaining the interior space between a temperature at the beginning of the heating in the curing step and a temperature at which the foaming agent expands.
[0024] According to this configuration, the interior space can be adequately held by the space-holding element until the foaming agent expands.
[0025] Furthermore, it is preferable that in the space-holding part alignment step, in the blade width direction of the compound blade, both end parts of the space-holding part are arranged so that they are closer to the side of the interior than both end parts of the compound blade.
[0026] According to this configuration, the suction-side laminate and the pressure-side laminate can also be appropriately connected to each other at both end parts in the blade width direction in a case where the space-holding part is provided.
[0027] Furthermore, it is preferred that in the mold setting step the suction-side molding tool is arranged on the lower side in a vertical direction and the pressure-side molding tool is arranged on the upper side in a vertical direction.
[0028] In this configuration, the suction-side laminate and the pressure-side laminate are arranged in a curved state, which is convex downwards. For this reason, circumferential stress can be exerted on the suction-side laminate and the pressure-side laminate due to their own weight.
[0029] Furthermore, it is preferred that the suction-side laminate and the pressure-side laminate each have a reinforcing fiber preform material provided on the interior side for the innermost layer, and that in a plane that intersects a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material for the innermost layer is the largest area among the reinforcing fiber preform materials contained in the suction-side laminate and in the pressure-side laminate.
[0030] In this case, it is preferable that, in the laying step, a tension is applied to the reinforcing fiber preform material for the innermost layer in an in-plane direction intersecting the laying direction of the reinforcing fiber preform material for the innermost layer.
[0031] According to this configuration, by applying tension to the reinforcing fiber preform material for the innermost layer, it is possible to suppress the flow of the reinforcing fiber preform materials included in the suction-side laminate and the pressure-side laminate.
[0032] According to the present invention, a method with the features of claim 13 for forming a composite blade is further provided, in which a composite blade made of a composite material is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade a suction-side part, which is a part on a back side, and a pressure-side part, which becomes a belly side, are placed one on top of the other and joined together,wherein the method comprises: a lay-up step of forming a suction-side laminate by laminating the reinforcing fiber preform material onto a suction-side mold for forming the suction-side part and of forming a pressure-side laminate by laminating the reinforcing fiber preform material onto a pressure-side mold for forming the pressure-side part; a mold setting step of adjusting the suction-side mold and the pressure-side mold so that the suction-side laminate and the pressure-side laminate are superimposed, and of arranging a foaming agent in an interior space formed by superimposing the suction-side laminate and the pressure-side laminate; and a curing step of pressing the suction-side laminate and the pressure-side laminate towards the suction-side mold and the pressure-side mold from the inside by expanding the foaming agent through heating,and heating and curing of the suction-side laminate and the pressure-side laminate, wherein the suction-side laminate and the pressure-side laminate each have a reinforcing fiber preform material for the innermost layer provided on the side of the interior, and in a plane that intersects a laying direction of the reinforcing fiber preform material, an area of the innermost reinforcing fiber preform material is the largest area among the reinforcing fiber preform materials contained in the suction-side laminate and the pressure-side laminate, and in the laying step a stress is applied to the reinforcing fiber preform material for the innermost layer in a direction in the plane that intersects the laying direction of the reinforcing fiber preform material of the innermost layer.
[0033] According to this configuration, by applying tension to the reinforcing fiber preform material for the innermost layer, it is possible to suppress the flow of the reinforcing fiber preform materials contained in the suction-side laminate and the pressure-side laminate. Therefore, it is possible to reduce the wave motion of the fibers generated in the suction-side part and the pressure-side part. In this way, it is possible to adjust the bending rigidity of the composite blade to the required bending rigidity, and therefore, it is also possible to adjust the natural frequency of the composite blade to the required natural frequency.
[0034] According to the present invention, there is further provided a composite blade made of a composite material having the features of claim 14, which is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, the composite blade including: a suction-side part, which is a part on a back side; a pressure-side part, which becomes a ventral side and is superimposed on and bonded to the suction-side part; a space holding part for holding an internal space, which is formed by superimposing the suction-side part and the pressure-side part;and a foaming agent provided in an interior of the space holding part in which, in a blade width direction, both end parts of the space holding part are located closer to the side of the interior space than both end parts of the suction side part and the pressure side part, the space holding part being provided on the entire surface along an inner surface of the interior space;
[0035] According to this configuration, the spacer element is arranged in such a way as to reduce the wave motion of the fibers generated in the suction-side and pressure-side sections, and to allow the thickness of the foaming agent to be adjusted appropriately. Therefore, it is possible to provide a composite blade that meets the required performance (flexural stiffness and natural frequency). Furthermore, even when the spacer element is present, both end sections of the spacer element are located on the interior side, allowing the suction-side laminate (suction-side section) and the pressure-side laminate (pressure-side section) to be appropriately bonded to each other at both end sections in the blade width direction.
[0036] Furthermore, it is preferred that the space-holding part includes a suction-side space-holding part arranged on the suction-side part, a pressure-side space-holding part facing the suction-side space-holding part and arranged on the pressure-side part, and an adhesive provided on each of the two end parts of the suction-side space-holding part and the pressure-side space-holding part in a blade width direction and provided between the suction-side space-holding part and the pressure-side space-holding part.
[0037] According to this configuration, the space holding part can be divided into the suction-side space holding part and the pressure-side space holding part, and therefore, at the time of molding, it is possible to easily arrange the foaming agent in the internal space held by the space holding part.
[0038] Furthermore, it is preferred that the suction-side part and the pressure-side part each have a reinforcing fiber preform material for the innermost layer provided on the side of the interior, and that in a plane that intersects a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material for the innermost layer is the largest area among the reinforcing fiber preform materials contained in the suction-side part and the pressure-side part.
[0039] According to this configuration, by applying tension to the reinforcing fiber preform material for the innermost layer at the time of molding, it is possible to suppress the flow of the reinforcing fiber preform materials contained in the suction-side laminate before curing of the suction-side part and the pressure-side laminate before curing of the pressure-side part. Therefore, it is possible to reduce the wave motion of the fibers generated in the suction-side part and the pressure-side part.
[0040] According to the present invention, a composite blade made of a composite material with the features of claim 17 is further provided, which is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, wherein the composite blade comprises: a suction-side part, which is a part on a back side; a pressure-side part, which becomes a belly side and is placed on the suction-side part and connected to it;and a foaming agent provided in an internal space formed by superposing the suction-side part and the pressure-side part, wherein the suction-side part and the pressure-side part each have a reinforcing fiber preform material for the innermost layer provided on the internal space side, and in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material for the innermost layer is the largest area among the reinforcing fiber preform materials contained in the suction-side part and the pressure-side part;
[0041] According to this configuration, by applying tension to the reinforcing fiber preform material for the innermost layer at the time of molding, it is possible to suppress the flow of the reinforcing fiber preform materials contained in the suction-side laminate before curing of the suction-side part and the pressure-side laminate before curing of the pressure-side part. Therefore, it is possible to reduce the wave motion of the fibers generated in the suction-side part and the pressure-side part.
[0042] According to the present invention, a molding tool with the features of claim 18 is provided for a composite blade, wherein a composite blade made of a composite material is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade a suction-side part, which is a part on a back side, and a pressure-side part, which becomes a belly side, are superimposed and joined together, wherein the molding tool comprises: a suction-side molding tool for laminating the reinforcing fiber preform material onto it and for forming a suction-side laminate, which is a suction-side part before forming; and a pressure-side molding tool for laminating the reinforcing fiber preform material onto it and for forming a pressure-side laminate, which is a pressure-side part before forming.wherein the suction-side laminate and the pressure-side laminate each have a reinforcing fiber preform material for the innermost layer, which is provided on one side of an interior formed by overlapping the suction-side laminate and the pressure-side laminate, and in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material for the innermost layer is the largest area among the reinforcing fiber preform materials contained in the suction-side part and the pressure-side part, and the suction-side mold and the pressure-side mold each contain a mold main body,on which the reinforcing fiber preform material is laminated and a stress application mechanism for applying a stress to the reinforcing fiber preform material for the innermost layer in a laying direction of the reinforcing fiber preform material of the innermost layer-cutting direction in the plane.
[0043] According to this configuration, the tension application mechanism can apply tension to the reinforcing fiber preform material for the innermost layer, and therefore, it is possible to suppress the flow of the reinforcing fiber preform materials contained in the suction-side laminate and the pressure-side laminate. Therefore, it is possible to reduce the wave motion of the fibers generated in the suction-side part and the pressure-side part. Character list Fig. 1 is a plan view schematically showing a composite blade formed by a method for forming a composite blade according to Embodiment 1. Fig. 2 is a cross-sectional view schematically showing a thick part of the composite blade according to Embodiment 1. Fig. 3 is a schematic diagram of an example showing a part of an inner surface cladding plate of the composite blade according to Embodiment 1. Fig. 4 is a schematic diagram of an example showing a part of the inner surface cladding plate of the composite blade according to Embodiment 1. Fig. 5 is a schematic diagram of an example showing a part of the inner surface cladding plate of the composite blade according to Embodiment 1. Fig. Figure 6 is an explanatory diagram of a foaming agent used by a method for forming a composite blade according to embodiment 1. Fig. Figure 7 is an explanatory diagram regarding the method for forming a composite blade according to embodiment 1. Fig. Figure 8 is a schematic diagram showing an inner surface cladding plate of a composite blade according to embodiment 2. Fig. Figure 9 is a schematic diagram showing an inner surface cladding plate of a composite blade according to embodiment 3. Fig. Figure 10 is an explanatory diagram showing a laminated structure of a composite blade according to embodiment 4. Fig. Figure 11 is a schematic diagram showing a forming tool for forming the compound blade according to embodiment 4. Description of the embodiments
[0044] Embodiments related to the present invention will be described in detail below based on the drawings. The present invention is not limited to the embodiments. Furthermore, components that can be easily replaced by those skilled in the art or are substantially the same are included in the following embodiments. Furthermore, the components described below can be combined as appropriate, and in a case where there are multiple embodiments, it is also possible to combine the respective embodiments. [Version 1]
[0045] A method for forming a composite blade 10 according to this embodiment is a method for forming a blade using a composite material of reinforcing fibers and resin. The composite blade 10 can be, for example, a turbine rotor blade or a turbine guide vane used in a gas turbine, a gas turbine engine, or the like. In this embodiment, it is described that the composite blade 10 is applied to a turbine rotor blade. However, the method for forming the composite blade 10 is also applicable to a turbine guide vane.
[0046] Fig. Figure 1 is a top view schematically showing a compound blade formed by the method for forming a compound blade according to embodiment 1. Fig. Figure 2 is a cross-sectional view schematically showing a thick part of the composite blade according to this embodiment and is a cross-sectional view along line AA of Fig. 1. Fig. 3 to Fig. Figure 5 shows a schematic diagram of an example showing part of an inner surface cladding plate of the composite blade according to embodiment 1. Fig. Figure 6 is an explanatory diagram of a foaming agent used in the method for forming a composite blade according to embodiment 1. Fig. Figure 7 is an explanatory diagram regarding the method for forming a composite blade according to embodiment 1.
[0047] First, before describing the method for forming the compound blade 10, the compound blade 10 will be described. As in Fig. As shown in Figure 1, the compound blade 10 is a turbine blade and extends from the blade root, which is a fixed end, to the blade top, which is a free end. Here, the direction connecting the blade root and the blade top is a blade longitudinal direction and an L-direction, as shown in Figure 1. Fig. Figure 1 shows. Furthermore, in the compound blade 10, one side is angled in the direction perpendicular to the blade longitudinal direction. Fig. 1. One side is a leading edge and the other a trailing edge. The direction connecting the leading edge and the trailing edge is a blade width direction and a W direction, as shown in Fig. 1 shown.
[0048] Furthermore, as in Fig. Figure 2 shows the composite blade 10 formed such that it is curved in the blade width direction, and the side that is convex from the inside of the composite blade 10 to the outside is the back side, and the side that is concave from the inside of the composite blade 10 to the outside is the belly side. Here, the direction connecting the back side and the belly side is a direction of the blade thickness and a direction T, as shown in Fig. 2 shown.
[0049] In the composite blade 10, the thickness increases towards the blade thickness on the blade root side and is designed to be thinner towards the blade top. For this reason, the blade top of the composite blade 10 has a thin section where the thickness is thin in the direction of the blade thickness, and the blade root side has a thick section 10b (see Fig. 2), in which the thickness is thick in the direction of the shovel thickness.
[0050] Several composite blades 10 are provided, which are arranged at predetermined intervals in the circumferential direction on the outer circumference of a rotor that rotates around a shaft center. A fluid then flows from the leading edge to the trailing edge between the composite blades 10.
[0051] As in Fig. As shown in Figure 2, the composite blade 10 comprises a suction-side blade element (suction-side part) 12, which is a part on the rear side, and a pressure-side blade element (pressure-side part) 14, which is a part on the belly side, an inner surface cladding plate (space-holding part) 18, which holds an interior space 20 formed by the suction-side blade element 12 and the pressure-side blade element 14, and a foaming agent 16, which is provided inside the inner surface cladding plate 18.
[0052] The suction-side blade element 12 is formed by laminating several prepregs as reinforcing fiber preform materials in which reinforcing fibers are impregnated with resin, and thermally curing the prepregs. The suction-side blade element 12 is formed by a suction-side mold 32, which will be described later. The suction-side blade element 12 is formed in a curved shape in which the outer surface of the composite blade 10 becomes convex. Furthermore, the suction-side blade element 12 is formed in a curved shape in which the inner surface of the composite blade 10 becomes concave and serves as part of the inner surface that configures the interior 20.
[0053] The pressure-side blade element 14 is formed by laminating several prepregs as reinforcing fiber preform materials, in which reinforcing fibers are impregnated with resin, and by thermally curing the prepregs similarly to the suction-side blade element 12. The pressure-side blade element 14 is formed by a pressure-side mold 34, which will be described later. The pressure-side blade element 14 is formed in a curved shape in which the outer surface of the composite blade 10 becomes concave. Furthermore, the pressure-side blade element 14 is formed in a curved shape in which the inner surface of the composite blade 10 becomes convex and serves as part of the inner surface that configures the interior 20.
[0054] Then, both end sections in the blade width direction of the suction-side blade element 12 and both end sections in the blade width direction of the pressure-side blade element 14 are connected to each other in a neutral plane P, which is a plane with its center in the direction of the blade thickness of the composite blade 10. Furthermore, an inner surface between both end sections in the blade width direction of the suction-side blade element 12 and an inner surface between both end sections in the blade width direction of the pressure-side blade element 14 are formed, separate from the neutral plane P towards the outer surface side, and the interior space 20 is formed by these inner surfaces. The interior space 20 is large on the blade root side of the composite blade 10 and becomes smaller towards the blade top side of the composite blade 10.
[0055] In this embodiment, the prepreg is used as the reinforcing fiber preform material. However, as long as it contains reinforcing fibers and resin, any material can be used. For example, in addition to carbon fibers, glass fibers and aramid fibers can be used as reinforcing fibers. However, there is no limitation, and plastic fibers or metal fibers can be used. Furthermore, the resin is preferably a thermosetting resin. However, it may be a thermoplastic resin. As the thermosetting resin, epoxy resin, polyester resin, and vinyl ester resin are exemplified. As the thermoplastic resin, polyamide resin, polypropylene resin, ABS (acrylonitrile butadiene styrene) resin, polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyphenylene sulfide (PPS), and the like are exemplified. However, the resin impregnated in the reinforcing fibers is not limited to these, and other resins can also be used.
[0056] The inner surface cladding plate 18 is provided along the inner surface of the interior 20. The inner surface cladding plate 18 is configured, for example, with the same prepreg as the suction-side blade element 12 and the pressure-side blade element 14. The inner surface cladding plate 18 is manufactured from a cured composite material at the time of molding the composite blade 10. That is, the cured inner surface cladding plate 18 is attached during the assembly of the composite blade 10. In embodiment 1, the inner surface cladding plate 18 is configured with a prepreg. However, any material can be used. For example, it can be configured with resin only, and highly elastic resin fibers such as Kevlar (registered trademark) or Vectran (registered trademark) can be used as reinforcing fibers.
[0057] Furthermore, the inner surface cladding plate 18 is designed to cover the entire inner surface of the interior 20. Both end parts of the inner surface cladding plate 18, in the blade width direction of the composite blade 10, are positioned closer to the side of the interior 20 than both end parts of the composite blade 10. Therefore, both end parts of the suction-side blade element 12 and both end parts of the pressure-side blade element 14 are connected to each other at the end parts of the composite blade 10.
[0058] The inner surface cladding panel 18 exhibits heat resistance capable of maintaining the interior space 20 during the molding of the composite blade 10. Specifically, the inner surface cladding panel 18 possesses heat resistance that acts as stiffness, maintaining the interior space 20 between a heating temperature at the beginning of the thermal curing process and a foaming temperature at which a (later described) foaming agent 16 expands (foams) during the molding of the composite blade 10. For example, in the inner surface cladding panel 18, the glass transition temperature of the resin contained therein is 80°C or higher and is equal to or higher than the curing temperature of the suction-side blade element 12 and the pressure-side blade element 14.
[0059] The above-described inner surface liner plate 18 includes a suction-side liner plate 18a disposed on the suction-side blade member 12 and a pressure-side liner plate 18b disposed on the pressure-side blade member 14. Furthermore, the suction-side liner plate 18a and the pressure-side liner plate 18b are bonded to each other by an adhesive 19 at both end portions in the blade width direction. The adhesive 19 is an adhesive sheet 19 sandwiched between the suction-side liner plate 18a and the pressure-side liner plate 18b at the time of molding. The adhesive sheet 19 may be the same as the resin contained in the inner surface liner plate 18, or may be an adhesive sheet bonded at normal temperature, which is not particularly limited.
[0060] The suction-side cladding plate 18a and the pressure-side cladding plate 18b are formed by laminating and curing prepregs. The suction-side cladding plate 18a is formed in a curved shape, with the outer surface in contact with the suction-side blade element 12 being convex. Furthermore, the suction-side cladding plate 18a is formed in a curved shape, with the inner surface in contact with the foaming agent 16 being concave. The thickness of the suction-side cladding plate 18a in the direction of the blade thickness is dimensioned such that it is constant in both the blade longitudinal and blade width directions. Furthermore, the suction-side fairing plate 18a contains a prepreg in which, when the blade longitudinal direction of the composite blade 10 is set as the reference direction, the fiber direction of the reinforcing fibers contained in the prepreg has an orientation of ±45° with respect to the reference direction.The suction-side cladding panel 18a contains such a prepreg, wherein the suction-side cladding panel 18a may have a structure with an applied elastic force. The elastic force of the suction-side cladding panel 18a is dimensioned such that the suction-side cladding panel 18a is bent when internal pressure (expansion pressure) is exerted on it by the expansion of the foaming agent 16 at the time of forming the composite blade 10, and is able to retain the interior 20 before the foaming agent 16 expands.
[0061] The pressure-side cladding plate 18b is formed in a curved shape, such that the outer surface in contact with the pressure-side blade element 14 is concave. Furthermore, the pressure-side cladding plate 18b is formed in a curved shape, such that the inner surface in contact with the foaming agent 16 is convex. The thickness of the pressure-side cladding plate 18b, in the direction of the blade thickness, is dimensioned such that it is constant in both the blade longitudinal and blade width directions, similar to the suction-side cladding plate 18a. The pressure-side cladding plate 18b also contains a prepreg in which, when the blade longitudinal direction of the composite blade 10 is set as the reference direction, the fiber direction of the reinforcing fibers contained in the prepreg has an orientation of ±45° with respect to the reference direction, similar to the suction-side cladding plate 18a.The pressure-side cladding panel 18b contains such a prepreg, wherein the pressure-side cladding panel 18b can also have a structure with the same elasticity as that of the suction-side cladding panel 18a applied to it.
[0062] Next, the structure of an end part in the blade width direction of the inner surface cladding plate 18 is described with reference to the Fig. 3 to Fig. 5. The blade width-direction end portion of the inner surface liner plate 18 is formed by bonding the blade width-direction end portions of the suction-side liner plate 18a and the pressure-side liner plate 18b with the adhesive 19. That is, a joining edge 21 is formed at each of the blade width-direction end portions of the suction-side liner plate 18a and the pressure-side liner plate 18b, and the joining edges 21 are joined to each other with the adhesive 19.
[0063] As an example of the in Fig. In the end section of the inner surface cladding plate 18 shown in Figure 3, the end section of the suction-side cladding plate 18a is bent towards the outer surface in the blade width direction to form a connecting edge 21a on the inner surface, and the end section of the pressure-side cladding plate 18b is slightly bent towards the inner surface in the blade width direction to form a connecting edge 21b on the inner surface. In this way, the connecting edges 21a and 21b of the suction-side cladding plate 18a and the pressure-side cladding plate 18b project outwards from the outer surface of the inner surface cladding plate 18.
[0064] As an example of the in Fig. 4, the blade width-direction end portion of the suction-side liner plate 18a is folded back toward the inner surface side to form a connecting edge 21a on the outer surface side, and the blade width-direction end portion of the pressure-side liner plate 18b is folded back toward the inner surface side to form a connecting edge 21b on the outer surface side. In this way, the connecting edges 21a and 21b of the suction-side liner plate 18a and the pressure-side liner plate 18b protrude toward the inner side of the inner surface liner plate 18.
[0065] As an example of the end part of the interior surface cladding panel 18, as in Fig. As shown in Figure 5, the end part of the suction-side cladding plate 18a is folded back towards the inner surface in the blade width direction to form a connecting edge 21a on the outer surface, and the inner surface of the end part of the suction-side cladding plate 18b is used as the connecting edge 21b as it is. In this way, the connecting edges 21a of the suction-side cladding plate 18a project towards the inside of the inner surface cladding plate 18 and are provided along the inner surface of the pressure-side cladding plate 18b.
[0066] The foaming agent 16 is filled inside the interior surface cladding panel 18. The foaming agent 16 is placed inside the interior surface cladding panel 18 before foaming and is then heated and foamed to be filled inside the interior surface cladding panel 18. The foaming agent 16 filled inside the interior surface cladding panel 18 is formed into a stratified foam layer. As shown in Fig. As shown in Figure 6, the foaming agent 16 is configured to include a resin component 25, a foam component 26, and a fiber component 27. The resin component 25 is cured by heating and can be the same resin contained in the reinforcing fiber preform material. The foam component 26 is foamed by heating, for example, by generating carbon dioxide gas or the like and forming bubbles 28 in the resin component 25. The fiber component 27 is added such that the foaming by the foam component 26 occurs in a stable, uneven foam shape.
[0067] In the foaming agent 16, the one on the left side of Fig. The state shown in Figure 6 is the state before foaming, and the foaming agent 16 in the pre-foaming state is heated to generate bubbles 28, thereby expanding the volume of the foaming agent 16, and after the volume has expanded, the resin component 25 is cured.
[0068] Next, the above-described method for forming the composite blade 10 will be described with reference to Fig. 7 described. In both methods for forming the composite blade 10 of this embodiment, a placement step S1, an inner surface cladding plate alignment step (space-holding part alignment step) S2, a mold setting step S3, a curing step S4 and a demolding step S5 are carried out successively.
[0069] In the placement step S1, a suction-side placement step S1a is performed to form a suction-side laminate 12a, which is part of the suction-side blade element 12 before forming, and a pressure-side placement step S1b is performed to form a pressure-side laminate 14a, since it is part of the pressure-side blade element 14 before forming.
[0070] In the suction-side placement step Sla, a prepreg is laminated onto the suction-side mold 32 to form the suction-side blade element 12 and thus create the suction-side laminate 12a. The suction-side mold 32 has a suction-side forming surface 32a for forming the outer surface of the suction-side blade element 12 and a flat suction-side forming adjustment surface 32b that surrounds the suction-side forming surface 32a. The suction-side forming surface 32a is recessed in a concave shape to form the outer surface of the suction-side blade element 12 into a curved, convex shape. In the suction-side placement step Sla, the suction-side mold 32 is positioned so that the suction-side forming surface 32a faces upwards in the vertical direction. Then, a prepreg is laminated onto the suction-side molding surface 32a of the suction-side molding die 32 to form the suction-side laminate 12a.In the suction-side laying step Sla, suction is performed each time some layers of the prepregs are laminated, thereby forming the suction-side laminate 12a.
[0071] In the pressure-side placement step S1b, a prepreg is laminated onto the pressure-side mold 34 to form the pressure-side blade element 14 and create the pressure-side laminate 14a. The pressure-side mold 34 has a pressure-side molding surface 34a for forming the outer surface of the pressure-side blade element 14 and a flat pressure-side mold setting surface 34b surrounding the pressure-side molding surface 34a. The pressure-side molding surface 34a is shaped to protrude in a convex form to shape the outer surface of the pressure-side blade element 14 into a curved, concave shape. In the pressure-side placement step S1b, the pressure-side mold 34 is positioned so that the pressure-side molding surface 34a faces upwards in the vertical direction. Then a prepreg is laminated onto the pressure-side mold surface 34a of the pressure-side mold tool 34 to form the pressure-side laminate 14a.By means of the pressure-side application step S1b, similar to the suction-side application step Sla, suction is carried out each time some layers of prepregs are laminated, thereby forming the pressure-side laminate 14a.
[0072] In the interior surface cladding panel alignment step S2, an alignment step S2a of the suction-side cladding panel for the arrangement of the suction-side cladding panel 18a on the suction-side laminate 12a and a pressure-side cladding panel alignment step S2b for the arrangement of the pressure-side cladding panel 18b on the pressure-side laminate 14a are carried out.
[0073] In the alignment step S2a of the suction-side cladding panel, the inner surface of the suction-side cladding panel 18a is positioned upwards in a vertical direction so that the outer surface of the suction-side cladding panel 18a is in contact with the suction-side laminate 12a.
[0074] In the alignment step S2b of the suction-side cladding plate, the inner surface of the pressure-side cladding plate 18b is positioned vertically upwards so that the outer surface of the pressure-side cladding plate 18b is in contact with the pressure-side laminate 14a.
[0075] In Embodiment 1, the suction-side cladding plate 18a and the pressure-side cladding plate 18b are arranged in a state where they are separate bodies. However, a configuration may be adopted in which the suction-side cladding plate 18a and the pressure-side cladding plate 18b are bonded together in advance with an adhesive, and the integrated inner surface cladding plate 18 is arranged on the suction-side laminate 12a or the pressure-side laminate 14a.
[0076] In the mold setting step S3, the suction-side mold tool 32 and the pressure-side mold tool 34 are adjusted, and the foaming agent 16 is placed. Specifically, in mold setting step S3, the suction-side mold tool 32 is positioned vertically on its lower side, and the pressure-side mold tool 34 is positioned vertically on its upper side. Then, in mold setting step S3, the suction-side mold setting surface 32b of the suction-side mold tool 32 and the pressure-side mold setting surface 34b of the pressure-side mold tool 34 are aligned, with the suction-side laminate 12a on the suction-side mold tool 32 and the pressure-side laminate 14a on the pressure-side mold tool 34 being aligned on the neutral plane P.Furthermore, when the suction-side laminate 12a and the pressure-side laminate 14a are superimposed, the joining edge 21a of the suction-side liner plate 18a and the joining edge 21b of the pressure-side liner plate 18b are arranged facing each other, and the adhesive sheet is sandwiched between the joining edge 21a and the joining edge 21b, thereby forming the inner surface liner plate 18. In Embodiment 1, the end portions in the blade width direction of the suction-side liner plate 18a and the pressure-side liner plate 18b are bonded to each other. However, if it is necessary to bond the end portions in the blade longitudinal direction of the suction-side liner plate 18a and the pressure-side liner plate 18b, joining edges may be formed at the end portions in the blade longitudinal direction and bonded to each other.
[0077] Then, in the mold setting step S3, the internal cavity 20 is formed by the suction-side laminate 12a and the pressure-side laminate 14a, which are placed on top of each other, and the inner surface cladding panel 18 is placed on the inner surface of the interior 20.
[0078] Furthermore, in the mold setting step S3, the foaming agent 16 is installed inside the inner surface cladding panel 18 before foaming, prior to the placement of the suction-side laminate 12a and the pressure-side laminate 14a on top of each other. The foaming agent 16 is formed in sheet form before foaming. In the mold setting step S3 of embodiment 1, the suction-side molding tool 32 is located on the lower side of the pressure-side molding tool 34, and thus the foaming agent 16 is installed on the inner surface of the suction-side cladding panel 18a before foaming.
[0079] In curing step S4, the suction-side laminate 12a, the pressure-side laminate 14a, and the foaming agent 16 are heated while the suction-side mold 32 and the pressure-side mold 34 are pressed in a converging direction. During curing step S4, the heating causes the foaming component 26 of the foaming agent 16 to foam before the resin component 25 of the foaming agent 16 and the resin of the prepreg (the suction-side laminate 12a and the pressure-side laminate 14a) cure, while the interior 20 is held in place by the inner surface cladding panel 18. As the foaming component 26 foams, bubbles 28 form due to the foaming component 26, with the resin component 25 expanding before curing.For this reason, due to the expansion of the foaming agent 16 from the interior of the inner space 20 outwards, pressure (expansion pressure) is exerted by the inner surface cladding panel 18, so that the suction-side laminate 12a and the pressure-side laminate 14 are pressed towards the suction-side molding tool 32 and the pressure-side molding tool 34 by the foaming agent 16 before curing. At this point, the inner space 20 is held by the inner surface cladding panel 18, and therefore the foaming agent 16 is appropriately filled into the inner space 20 (the interior of the inner surface cladding panel 18).Subsequently, after the foaming of the foam component 26 of the foaming agent 16, the resin of the prepreg is cured first, or the resin of the resin component 25 of the foaming agent 16 and the resin of the prepreg are cured simultaneously, whereby the suction-side laminate 12a and the pressure-side laminate 14a are thermally cured in a state pressed by the foaming agent 16. Then, the resin component 25 of the foaming agent 16 is thermally cured after the curing of the resin of the prepreg or simultaneously with the curing of the resin of the prepreg, whereby the foaming agent 16 is integrated with the suction-side laminate 12a and the pressure-side laminate 14a. Then, the suction-side laminate 12a, the pressure-side laminate 14a, and the foaming agent 16 are cured, thereby forming the composite blade 10.
[0080] In demolding step S5, the suction-side molding tool 32 and the pressure-side molding tool 34 are moved away from each other, whereby the formed composite blade 10 is released from the suction-side molding tool 32 and the pressure-side molding tool 34.
[0081] As described above, according to embodiment 1, the inner surface cladding plate 18 is arranged, making it possible to expand the foaming agent 16 while the suction-side laminate 12a and the pressure-side laminate 14a are thermally cured in a state in which the interior 20 is held. For this reason, the interior 20 is held by the inner surface cladding plate 18, so that it is possible to suppress the flow of the prepregs of the suction-side laminate 12a and the pressure-side laminate 14a during the thermal curing of the suction-side laminate 12a and the pressure-side laminate 14a. Therefore, it is possible to reduce any wave motion of the fibers that is generated in the suction-side blade element 12 and the pressure-side blade element 14. Furthermore, the interior space 20 is held by the interior surface cladding panel 18, and therefore the interior space 20 can be filled with the expanded foam agent 16 in a suitable manner.Therefore, it is possible to adjust the thickness of the foaming agent 16 appropriately. For this reason, it is possible to bring the thickness of both the suction-side blade element 12 and the pressure-side blade element 14 to the required thickness in the application direction after curing. In this way, it is possible to achieve the required flexural stiffness without reducing the flexural stiffness of the composite blade 10, and thus it is also possible to adjust the natural frequency of the composite blade 10 to the required natural frequency.
[0082] Further, according to Embodiment 1, the inner surface lining plate 18 can be divided into the suction-side lining plate 18a and the pressure-side lining plate 18b, and therefore, it is possible to easily arrange the foaming agent 16 inside the inner surface lining plate 18.
[0083] Furthermore, according to Embodiment 1, the entire inner surface of the interior space 20 can be held by the inner surface lining plate 18. Furthermore, the expanding foaming agent 16 can press the entire inner surface of the interior space 20 formed by the suction-side laminate 12a and the pressure-side laminate 14a through the inner surface lining plate 18.
[0084] Furthermore, according to Embodiment 1, a prepreg that is a composite material of the composite blade 10 can be used as the material of the inner surface cladding plate 18. For this reason, it is possible to perform thermal curing heating of the composite blade 10 without changing the heating conditions.
[0085] Furthermore, according to embodiment 1, it is possible to exert an elastic force on the inner surface cladding panel 18. For this reason, the inner surface cladding panel 18 is bent by the expansion pressure of the foaming agent 16 due to its elastic force, and therefore it is possible to press the inner surface cladding panel 18 against the suction-side laminate 12a and the pressure-side laminate 14a in a suitable manner.
[0086] Furthermore, according to embodiment 1, since the inner surface cladding panel 18 has a heat resistance that is able to maintain the interior space 20 between the heating temperature at the beginning of the heating and the foaming temperature until the foaming agent 16 expands, the interior space 20 can be maintained accordingly until the foaming agent 16 expands.
[0087] Furthermore, according to embodiment 1, the inner surface cladding plate 18 is located on the inside of the composite blade 10 in the blade width direction, and thus it is also possible in a case where the inner surface cladding plate 18 is provided to connect the suction-side laminate 12a and the pressure-side laminate 14a at both end parts in the blade width direction in a suitable manner.
[0088] Furthermore, according to embodiment 1, since the suction-side forming tool 32 is arranged vertically on the lower side and the pressure-side forming tool 34 is arranged vertically on the upper side, the suction-side laminate 12a and the pressure-side laminate 14a are arranged in a curved, downward-facing convex state. For this reason, it is possible to exert a circumferential stress on the suction-side laminate 12a and the pressure-side laminate 14a by their own weight.
[0089] In embodiment 1, the thickness of both the suction-side lining plate 18a and the pressure-side lining plate 18b is dimensioned such that it is constant in the longitudinal and lateral directions of the blade. However, there is no limitation to this configuration. The thickness on the middle section side in the lateral direction of both the suction-side lining plate 18a and the pressure-side lining plate 18b can be thinner than the thickness on the end section side. According to this configuration, the suction-side lining plate 18a and the pressure-side lining plate 18b become thinner towards the middle section from the end section in the lateral direction of the blade, thereby maintaining a constant stiffness in the lateral direction and thus ensuring a uniform expansion pressure due to the foaming agent 16 in the interior 20. [Embodiment 2]
[0090] Next, a compound blade 10 according to embodiment 2 is described with reference to Fig. 8 described. In embodiment 2, different parts are described than in embodiment 1 in order to avoid an overlap of descriptions, and described parts with the same configurations as those in embodiment 1 are marked with the same reference numerals. Fig. Figure 8 is a schematic diagram showing an inner surface cladding plate of a composite blade according to embodiment 2.
[0091] In the composite blade 10 of embodiment 2, an inner surface cladding plate 41 is arranged in a wing profile section of the composite blade 10. The inner surface cladding plate 41 is located on the blade root side (the lower side in Fig. 8) continuously and on the top of the shovel (the upper side in Fig. 8) connected. That is, the inner surface cladding plate 41 is a continuous plate having one end part on the top of the blade and extending from the top of the blade to the tail side, folded back to the top of the blade on the tail side to extend from the tail side to the top of the blade, thus providing the other end part on the top of the blade. Subsequently, both end parts are bonded together on the top of the blade by the adhesive 19, making it possible to handle the inner surface cladding plate 41 without having to divide it. Likewise, in embodiment 2, similar to embodiment 1, if it is necessary to bond the end parts in the blade width direction of the inner surface cladding plate 41, connecting edges can be formed on the end parts in the blade width direction and bonded together.In the inner surface cladding plate 41, the internal cavity at the end part on the blade foot side is wide, and the internal cavity becomes narrower towards the end part on the blade top.
[0092] As described above, according to Embodiment 2, the blade root side of the inner surface liner plate 41 is a closed end portion, and therefore, the foaming agent 16 disposed inside the inner surface liner plate 41 tends to flow toward the blade top at the time of expansion. Thus, the interior of the inner surface liner plate 41 can be properly filled with the foaming agent 16. Furthermore, the blade root side of the inner surface liner plate 41 is a closed end portion, so that even when excessive compression in the blade thickness direction occurs, it is possible to suppress the inflow of the foaming agent 16 into the blade root portion. [Embodiment 3]
[0093] Next, a compound blade 10 according to embodiment 3 is described with reference to Fig. 9 described. Likewise, in embodiment 3, different parts are described than in embodiments 1 and 2 in order to avoid an overlap of descriptions, and described parts with the same configurations as those in embodiments 1 and 2 are identified with the same reference numerals. Fig. Figure 9 is a schematic diagram showing an inner surface cladding plate of a composite blade according to embodiment 3.
[0094] In the composite blade 10 of embodiment 3, an inner surface cladding plate 51 is arranged over a region from an airfoil section to a blade root section of the composite blade 10. The inner surface cladding plate 51 is located on the blade root side (the lower side in Fig. 9) continuously and on the top of the shovel (the upper side in Fig. 9). That is, the inner surface liner plate 51 is a continuous plate that has one end portion on the blade top side, extends from the blade top side to the blade root side, is folded back to the blade top side on the blade root side to extend from the blade root side to the blade top side, thereby providing the other end portion on the blade top side. Then, both end portions are bonded to each other by the adhesive 19 on the blade top side, thereby making it possible to handle the inner surface liner plate 51 without dividing it. Also, in Embodiment 3, similarly to Embodiment 1, when it is necessary to connect the end portions in the blade width direction of the inner surface liner plate 51, connecting edges may be formed at the end portions in the blade width direction and bonded to each other.In the inner surface cladding plate 51, the end part is located on the blade foot side inside the blade foot section, and therefore a core material 52 is arranged inside the end part on the blade foot side of the inner surface cladding plate 51.
[0095] The core material 52 is configured using a light metal, a cured composite material, or the like, and is pre-filled in the interior of the end section on the blade root side of the inner surface fairing plate 51. Prepregs 53 of the suction-side laminate 12a and the pressure-side laminate 14a, which are continuous to the airfoil section, are laminated such that they are wound onto the outer surface side of the inner surface fairing plate 51, in which the interior is filled with the core material 52. That is, the prepreg 53 wound around the end section on the blade root side of the inner surface fairing plate 51 is continuous from the suction-side laminate 12a to the pressure-side laminate 14a.
[0096] The prepreg 53, in which, when the blade longitudinal direction is set as a reference direction, the reinforcing fibers contained in the prepreg 53 have an orientation of ±45° with respect to the reference direction, and the prepreg 53 with an orientation of 0° are contained in several laminated prepregs 53 that configure the inner surface covering plate 51. The prepreg 53 with an orientation of 0° is included, whereby a centrifugal load acting in the blade longitudinal direction can be carried by the inner surface covering plate 51.
[0097] As described above, according to Embodiment 3, the end part on the blade root side of the inner surface liner plate 51 can be located inside the blade root portion of the composite blade 10. For this reason, it is possible to make the end part on the blade root side of the inner surface liner plate 51 act as a holding portion with respect to the centrifugal load applied in the blade longitudinal direction, and thus the inner surface liner plate 51 can bear the centrifugal load. [Embodiment 4]
[0098] Next, a compound blade 10 according to embodiment 4 is described with reference to the Fig. 10 and Fig. 11 described. Likewise, in embodiment 4, different parts are described than in embodiments 1 to 3 in order to avoid an overlap of descriptions, and described parts with the same configurations as those in embodiments 1 to 3 are marked with the same reference numerals. Fig. Figure 10 is an explanatory diagram showing a laminated structure of a composite blade according to embodiment 4. Fig. Figure 11 is a schematic diagram showing a forming tool for forming the composite blade according to embodiment 4.
[0099] In the composite blade 10 of embodiment 4, the suction-side blade element 12 and the pressure-side blade element 14, which are formed by laminating several prepregs 62, each have a prepreg 61 of the innermost layer, which is provided on the side of the interior 20. That is, the prepreg 61 of the innermost layer is arranged between the suction-side blade element 12 (the suction-side laminate 12a) and the suction-side cladding plate 18a and between the pressure-side blade element 14 (the pressure-side laminate 14a) and the pressure-side cladding plate 18b in the direction of the blade thickness (the bearing direction). In the prepreg 61 of the innermost layer, the area of it in a plane that intersects the laying direction of the prepreg 62 is the largest area among the prepregs 62 contained in the suction-side blade element 12 and the pressure-side blade element 14.At this point, the innermost layer of prepreg 61 is arranged such that the end part on the blade's upper surface protrudes from the other prepregs 62. Then, a stress is applied to the end part on the blade's upper surface that protrudes from the other prepregs 62 in the innermost layer of prepreg 61.
[0100] Furthermore, the plurality of prepregs 62 are arranged such that the area intersecting the laying direction becomes smaller toward the innermost layer prepreg 61 from the outer surface side in the blade thickness direction. That is, the plurality of prepregs 62 are arranged side by side in the blade thickness direction such that the positions of the end portions on the blade top surface are located on the blade root side from the outer surface side toward the innermost layer prepreg 61.
[0101] A case of forming the suction-side laminate 12a or the pressure-side laminate 14a, each comprising the innermost layer prepreg 61, is described as being applied, for example, to the suction-side mold 32. The suction-side mold 32 comprises a mold body 65, a stress application mechanism 66, a blade root-side fastening pin 67 for fastening the end part to the blade root side of the suction-side laminate 12a, and a blade tip fastening pin 68 for fastening the end part to the blade top of the innermost layer prepreg 61 contained in the suction-side laminate 12a.
[0102] In Fig. 11 corresponds to its right-left direction of the blade longitudinal direction of the suction-side forming tool 32. As in Fig.As shown in Figure 11, the main body of the mold 65 has a suction-side molding surface for forming the outer surface of the suction-side blade element 12. The blade root side of the suction-side molding surface has an inclined surface that slopes vertically towards the bottom and a side surface that is a vertical surface connected to the inclined surface. The suction-side laminate 12a is formed by laminating the multiple prepregs 62 and the innermost layer prepreg 61 onto the suction-side molding surface. Since the suction-side molding surface is the outer surface of the suction-side laminate 12a, the multiple prepregs 62 are laminated such that the area intersecting the lay-up direction decreases vertically towards the top. Furthermore, the end part is laminated onto the blade root side of the suction-side laminate 12a along the inclined surface and the side surface.The innermost layer of prepreg 61 is then placed on the upper surfaces of the multiple prepregs 62 to cover the entire surface of the multiple prepregs 62. The suction-side cladding plate 18a is placed on the upper surface of the innermost layer of prepreg 61.
[0103] The stress application mechanism 66 is provided on the blade surface of the suction-side laminate 12a, which is laminated onto the mold body 65 and moves outwards in a horizontal direction relative to the mold body 65. The end part on the blade surface of the prepreg 61 of the innermost layer of the suction-side laminate 12a is attached to the stress application mechanism 66.
[0104] The blade foot side fastening pin 67 is a pin for fastening the end part on the blade foot side of the suction-side laminate 12a, which is laminated onto the mold tool main body 65, on the side surface of the mold tool main body 65 and penetrates into the suction-side laminate 12a, which is to be attached to the mold tool main body 65.
[0105] The blade tip fastening pin 68 is a pin for fastening the end part on the blade top of the prepreg 61 of the innermost layer to the stress application mechanism 66 and penetrates the suction-side laminate 12a, which is to be attached to the stress application mechanism 66.
[0106] In the suction-side mold 32, the end part on the blade root side of the suction-side laminate 12a is attached by the blade root side fastening pin 67, the end part on the blade top side of the innermost layer prepreg 61 is attached by the blade tip fastening pin 68, and the end part on the blade top side of the innermost layer prepreg 61 is pulled outwards in a horizontal direction by the tension application mechanism 66. In this way, the innermost layer prepreg 61 is tensioned to hold the multiple prepregs 62 downwards, thereby suppressing the flow of the multiple prepregs 62.
[0107] The suction-side mold 32 was described above. However, the pressure-side mold 34 also has the same configuration, and therefore, its description is omitted.
[0108] As described above, according to embodiment 4, it is possible to suppress the flow of the prepreg 62 contained in the suction-side laminate 12a and the pressure-side laminate 14a, respectively, by applying stress to the prepreg 61 of the innermost layer. For this reason, it is possible to reduce the wave motion of the fibers generated in the suction-side blade element 12 and in the pressure-side blade element 14. In this way, it is possible to adjust the bending stiffness of the composite blade 10 to the required bending stiffness and thus also to adjust the natural frequency of the composite blade 10 to the required natural frequency.
[0109] In embodiment 4, the inner surface cladding plate 18 (the suction-side cladding plate 18a and the pressure-side cladding plate 18b) is arranged. However, the inner surface cladding plate 18 does not have to be arranged, and the presence or absence of the inner surface cladding plate 18 is not particularly restricted. List of reference symbols 10 compound bucket 10b thick part 12 suction-side blade element 12a suction-side laminate 14 pressure-side blade element 14a pressure-side laminate 16 foaming agents 18 Interior surface cladding panel 18a suction-side cladding plate 18b pressure-side cladding plate 19 Adhesive 20 Interior 21 Connecting edge 21a Connecting edge of the suction-side cladding panel 21b Connecting edge of the pressure-side cladding plate 25 resin component 26 Foam component 27 Fiber component 28 bladder 32 suction-side forming tool 34 pressure-side forming tool 41 Interior surface cladding panel 51 Interior surface cladding panel 52 core material 53 Prepreg 61 Prepreg of the innermost layer 62 Prepreg 65 Mold tool main body 66 Stress application mechanism 67 Shovel foot side fastening pin 68 Shovel tip fastening pin
Claims
[1] A method of forming a composite blade (10), in which a composite blade (10) made of a composite material is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade (10), a suction-side part (12) which is a part on a back side and a pressure-side part (14) which becomes a belly side are superimposed and bonded to each other, the method comprising: a laying step (S1) of forming a suction-side laminate (12a) by laminating the reinforcing fiber preform material on a suction-side mold (32) for molding the suction-side part (12) and forming a pressure-side laminate (14a) by laminating the reinforcing fiber preform material on a pressure-side mold (34) for molding the pressure-side part (14); a space holding member aligning step (S2) of arranging a space holding member (18; 41; 51) for holding an internal space (20) formed by superimposing the suction-side laminate (12a) and the pressure-side laminate (14a); a shape adjustment step (S3) of adjusting the suction-side molding tool (32) and the pressure-side molding tool (34) so that the suction-side laminate (12a) and the pressure-side laminate (14a) are superimposed, and of arranging a foaming agent (16) in the interior space (20) held by the space holding member (18); and a curing step (S4) of pressing the suction-side laminate (12a) and the pressure-side laminate (14a) toward the suction-side molding tool (32) and the pressure-side molding tool (34) from the inside by expanding the foaming agent (16) by heating, and heating and curing the suction-side laminate (12a) and the pressure-side laminate (14a), characterized by, that the space-holding part (18;41;51) is provided on the entire surface along an inner surface of the interior space (20). [2] A method for forming a composite blade (10) according to claim 1, wherein the space holding member (18) includes a suction-side space holding member (18a) disposed on the suction-side laminate (12a) and a pressure-side space holding member (18b) disposed on the pressure-side laminate (14a). [3] A method of forming a composite blade (10) according to claim 2, wherein in the space-holding part aligning step (S2), the suction-side space-holding part (18a) and the pressure-side space-holding part (18b) are arranged to face each other, an adhesive (19) is arranged between the suction-side space-holding part (18a) and the pressure-side space-holding part (18b) at each of both end parts of the suction-side space-holding part (18a) and the pressure-side space-holding part (18b) in a blade width direction (W) of the composite blade (10), and both end parts of the suction-side space-holding part (18a) and the pressure-side space-holding part (18b) are bonded to each other to form the space-holding part (18). [4] A method of forming a composite blade (10) according to claim 2 or 3, wherein in each of the suction-side space-holding part (18a) and the pressure-side space-holding part (18b), a thickness on a middle portion side in the blade width direction (W) is made thinner than a thickness on an end portion side. [5] A method of forming a composite blade (10) according to any one of claims 1 to 4, wherein a resin material or a cured composite material is used as the space-holding part (18). [6] A method of forming a composite blade (10) according to claim 5, wherein the space-holding member (18) when using a cured composite material includes: a reinforcing fiber preform material in which a fiber direction of reinforcing fibers included in the composite material has an orientation of ±45° with a blade longitudinal direction (L) of the composite blade (10) as a reference. [7] A method of forming a composite blade (10) according to any one of claims 1 to 6, wherein the space holding member (18) has a heat resistance capable of maintaining the internal space (20) between a temperature at the start of heating in the curing step (S4) and a temperature at which the foaming agent (16) expands. [8] A method of forming a composite blade (10) according to any one of claims 1 to 7, wherein in the space holding part aligning step (S2), in the blade width direction (W) of the composite blade (10), both end parts of the space holding part (18) are arranged to be closer to the inner space (20) side than both end parts of the composite blade (10). [9] A method of forming a composite blade (10) according to any one of claims 1 to 8, wherein in the shape setting step (S3), the suction-side mold (32) is arranged on the lower side in a vertical direction and the pressure-side mold (34) is arranged on the upper side in the vertical direction. [10] A method of forming a composite blade (10) according to any one of claims 1 to 9, wherein the suction-side laminate (12a) and the pressure-side laminate (14a) each have a reinforcing fiber preform material (61) for the innermost layer provided on the inner space (20) side, and in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material (61) for the innermost layer is the largest area among the reinforcing fiber preform materials included in the suction-side laminate (12a) and the pressure-side laminate (12a). [11] A method of forming a composite blade (10), in which a composite blade (10) made of a composite material is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade (10), a suction-side part (12) which is a part on a back side and a pressure-side part (14) which becomes a belly side are superimposed and bonded to each other, the method comprising: a laying step (S1) of forming a suction-side laminate (12a) by laminating the reinforcing fiber preform material on a suction-side mold (32) for molding the suction-side part (12) and forming a pressure-side laminate (14a) by laminating the reinforcing fiber preform material on a pressure-side mold (34) for molding the pressure-side part (14); a space holding member aligning step (S2) of arranging a space holding member (18; 41; 51) for holding an internal space (20) formed by superimposing the suction-side laminate (12a) and the pressure-side laminate (14a); a shape adjustment step (S3) of adjusting the suction-side molding tool (32) and the pressure-side molding tool (34) so that the suction-side laminate (12a) and the pressure-side laminate (14a) are superimposed, and of arranging a foaming agent (16) in the interior space (20) held by the space holding member (18); and a curing step (S4) of pressing the suction-side laminate (12a) and the pressure-side laminate (14a) toward the suction-side molding tool (32) and the pressure-side molding tool (34) from the inside by expanding the foaming agent (16) by heating, and heating and curing the suction-side laminate (12a) and the pressure-side laminate (14a), characterized by, that the suction-side laminate (12a) and the pressure-side laminate (14a) each have a reinforcing fiber preform material (61) for the innermost layer provided on the side of the inner space (20), and in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material (61) for the innermost layer is the largest area among the reinforcing fiber preform materials included in the suction-side laminate (12a) and the pressure-side laminate (12a). [12] A method of forming a composite blade (10) according to claim 10 or 11, wherein in the laying step (S1), a tension is applied to the reinforcing fiber preform material (61) for the innermost layer in an in-plane direction intersecting the laying direction of the reinforcing fiber preform material (61) of the innermost layer. [13] A method of forming a composite blade (10), in which a composite blade (10) made of a composite material is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade (10), a suction-side part (12) which is a part on a back side and a pressure-side part (14) which becomes a belly side are superimposed and bonded to each other, the method comprising: a laying step (S1) of forming a suction-side laminate (12a) by laminating the reinforcing fiber preform material on a suction-side mold (32) for molding the suction-side part (12) and forming a pressure-side laminate (14a) by laminating the reinforcing fiber preform material on a pressure-side mold (34) for molding the pressure-side part (14); a shape adjustment step (S3) of adjusting the suction-side molding tool (32) and the pressure-side molding tool (34) so that the suction-side laminate (12a) and the pressure-side laminate (14a) are superimposed, and of arranging a foaming agent (16) in an interior space (20) formed by superimposing the suction-side laminate (12a) and the pressure-side laminate (14a); and a curing step (S4) of pressing the suction-side laminate (12a) and the pressure-side laminate (14a) toward the suction-side molding tool (32) and the pressure-side molding tool (34) from the inside by expanding the foaming agent (16) by heating, and heating and curing the suction-side laminate (12a) and the pressure-side laminate (14a), characterized by , that the suction-side laminate (12a) and the pressure-side laminate (14a) each have a reinforcing fiber preform material (61) for the innermost layer provided on the side of the interior space (20), in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material (61) for the innermost layer is the largest area among the reinforcing fiber preform materials included in the suction-side laminate (12a) and the pressure-side laminate (14a), and in the laying step (S1), a tension is applied to the reinforcing fiber preform material (61) for the innermost layer in an in-plane direction intersecting the laying direction of the reinforcing fiber preform material (61) of the innermost layer. [14] A composite blade (10) made of a composite material, which is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, the composite blade (10) comprising: a suction side part (12) which is a part on a back side; a pressure-side part (14) which becomes a belly side and is placed over and connected to the suction-side part (12); a space-holding part (18; 41; 51) for holding an interior space (20) formed by superimposing the suction-side part (12) and the pressure-side part (14); and a foaming agent (16) provided in the interior (20) of the space-holding part (18; 41; 51), wherein in a blade width direction (W) both end parts of the space holding part (18; 41; 51) are located closer to the side of the inner space (20) than both end parts of the suction-side part (12) and the pressure-side part (14), characterized by , that the space-holding part (18;41;51) is provided on the entire surface along an inner surface of the interior space (20). [15] Composite blade (10) according to claim 14, wherein the space-holding part (18) includes: a suction-side space-holding part (18a) arranged on the suction-side part (12), a pressure-side space-holding part (18b) facing the suction-side space-holding part (12) and arranged on the pressure-side part (14), and an adhesive (19) provided at each of the two end parts of the suction-side space-holding part (18a) and the pressure-side space-holding part (18b) in a blade width direction (W) and provided between the suction-side space-holding part (18a) and the pressure-side space-holding part (18b). [16] The composite blade (10) according to claim 14 or 15, wherein the suction-side part (12) and the pressure-side part (14) each have a reinforcing fiber preform material (61) for the innermost layer provided on the side of the inner space (20), and in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material (61) for the innermost layer is the largest area among the reinforcing fiber preform materials included in the suction-side part (12) and the pressure-side part (14). [17] A composite blade (10) made of a composite material, which is formed by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, the composite blade (10) comprising: a suction-side part (12) which is a part on a back side; a pressure-side part (14) which becomes a belly side and is laid over and connected to the suction-side part (12); and a foaming agent (16) provided in an interior space (20) formed by superimposing the suction-side part (12) and the pressure-side part (14), characterized by , that the suction-side part (12) and the pressure-side part (14) each have a reinforcing fiber preform material (61) for the innermost layer provided on the side of the interior space (20), and in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material (61) for the innermost layer is the largest area among the reinforcing fiber preform materials contained in the suction-side part (12) and the pressure-side part (14). [18] A molding tool for molding a composite blade (10) made of a composite material by curing a reinforcing fiber preform material in which reinforcing fibers are impregnated with resin, and in the composite blade (10), a suction-side part (12) which is a part on a back side and a pressure-side part (14) which becomes a belly side are superimposed and joined to each other, the molding tool comprising: a suction-side forming tool (32) for laminating the reinforcing fiber preform material thereon and for forming a suction-side laminate (12a) which is a suction-side part (12) before forming; and a pressure-side forming tool (34) for laminating the reinforcing fiber preform material thereon and for forming a pressure-side laminate (14a) which is a pressure-side part (14) before forming, wherein the suction-side laminate (12a) and the pressure-side laminate (14a) each have a reinforcing fiber preform material (61) for the innermost layer provided on one side of an inner space (20) formed by superposing the suction-side laminate (12a) and the pressure-side laminate (14a), in a plane intersecting a laying direction of the reinforcing fiber preform material, an area of the reinforcing fiber preform material (61) for the innermost layer is the largest area among the reinforcing fiber preform materials included in the suction-side part (12) and the pressure-side part (14), and the suction-side molding die (32) and the pressure-side molding die (34) each include: a mold main body (65) onto which the reinforcing fiber preform material is laminated, and a stress application mechanism (66) for applying a stress to the reinforcing fiber preform material (61) for the innermost layer in an in-plane direction intersecting a laying direction of the reinforcing fiber preform material (61) of the innermost layer.
Citation Information
Patent Citations
Rotor blade for a wind turbine
DE102008022548A1
Shell structure with core - made by assembling half shells then inserting foam corethrough tube
DE2109934A1
Multiple constitution part blade for gas turbine
JP1997303104A
Mould assembly and method of closing a mould assembly
WO2012010331A1
JP000H09303104A