Stacked electrode arrangement in which bending behavior is reduced.

The electrode assembly with a four-layer structure and coated separators addresses bending issues by ensuring balanced electrode expansion, enhancing productivity and structural stability.

DE202019006095U1Active Publication Date: 2024-11-28LG ENERGY SOLUTION LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
DE202019006095
Authority / Receiving Office
DE · DE
Patent Type
Utility models
Current Assignee / Owner
Priority Date
2018-12-24
Filing Date
2019-12-19
Publication Date
2024-11-28
Estimated Expiration
2029-12-31

AI Technical Summary

Technical Problem

The lamination stack type electrode assembly experiences bending behavior during the activation process due to differential volume expansion of the positive and negative electrodes, leading to structural deformation and reduced productivity.

Method used

The electrode assembly is designed with a four-layer structure where electrodes and separators are stacked, and a coating material comprising inorganic particles and a binder polymer is applied to the separators to enhance adhesive forces between base unit bodies, ensuring balanced expansion and preventing bending.

Benefits of technology

The enhanced adhesive forces between base unit bodies prevent bending during charging and discharging, improving the assembly's productivity and structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000015_0000
    Figure 00000015_0000
  • Figure 00000015_0001
    Figure 00000015_0001
  • Figure 00000016_0000
    Figure 00000016_0000
Patent Text Reader

Abstract

Electrode arrangement comprising a unit body stack section produced by stacking at least two basic unit bodies (110a) forming a 4-layer structure, wherein a first electrode (111), a first separator (112), a second electrode (113) and a second separator (114) are stacked successively, wherein coating materials with adhesive strength are applied to the respective surfaces of the first and second separators, and wherein a basic unit body is bonded to its adjacent basic unit body in the unit body stack section.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] This application claims priority to Korean Patent Application No. 10-2018-0168229 filed on December 24, 2018, and the entire contents of the Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a lamination stack type electrode assembly, and more particularly to a lamination stack type electrode assembly capable of improving the bending behavior of an electrode assembly that may be caused by an activation process. State of the art

[0003] A secondary battery can be classified according to the structure of the electrode assembly. For example, the secondary battery can be divided into a stacked structure, a wound structure (jelly roll type), and a stackable / foldable structure. However, in the stacked structure, since the electrode units (positive electrodes, separators, and negative electrodes) that make up the electrode assembly are stacked separately from each other, it is very difficult to precisely align the electrode assembly, and many processes are required to manufacture the electrode assemblies. In addition, since the stackable / foldable structure generally requires two lamination devices and one folding device, the manufacturing process of the electrode assembly is very complicated.In particular, the stackable / foldable structure has the disadvantage that it is difficult to precisely align the complete cell or the bicell because the complete cell or the bicell is stacked by folding.

[0004] Accordingly, an electrode assembly with a lamination and stacking structure emerged. The lamination and stacking type structure can be fabricated by laminating base unit bodies formed by alternately stacking electrodes and separators to exert an adhesive force between the electrode and the separator in the base unit body, and simply stacking the base units repeatedly.

[0005] On the other hand, the secondary battery is manufactured through an assembly process in which the electrode assembly is housed in a battery case to inject the electrolyte and seal it, a pre-aging process in which the electrolyte thoroughly wets an electrode and a separator, and an activation process in which the battery structure is stabilized and made usable. During the activation process, a secondary battery is mounted on a predetermined jig to ensure smooth current flow, and charging and discharging are performed under the conditions required for activation. This is also called jig formation.Due to the characteristics of the secondary battery, this activation process should be performed first to activate the positive electrode active material during the first cycle and create a stable surface film (SEI, Solid Electrolyte Interface) on the negative electrode. Furthermore, pressurization can be performed during the jig formation process simultaneously with charging to prevent the formation of an uneven SEI film due to the gas generated during initial charging.

[0006] During the activation process described above, the volume of the positive and negative electrodes increases during charging and discharging of the secondary battery. During the activation process of the secondary battery, to which the electrode assembly consisting of the laminate and stack structure is applied, the secondary battery is bent over its entire length.

[0007] Fig. Figure 4 illustrates a mechanism in which bending behavior occurs during an activation process of a lamination and stacking type electrode assembly. In this regard, the electrode assembly of the conventional lamination and stacking type structure is formed by simply laminating the base unit, so no adhesive force is formed between the base unit and the adjacent base unit. On the other hand, an adhesive force is formed between the electrode and the separator in the base unit. This is because a lamination process is performed during the manufacturing of the base unit, and the binder is melted by the lamination process to form an adhesive force between the separator and the electrode.

[0008] When the electrode assembly of the lamination and stacking type structure is charged, the positive and negative electrodes expand. Because the volume expansion coefficients of the positive and negative electrodes are different, a bending behavior occurs, causing the base unit to bend completely due to stress accumulation within the base unit.

[0009] On the other hand, even in the case of an electrode assembly having a lamination and stacking type structure, if it is not pressed simultaneously with the initial charging, the adhesive force at the bonding interface is weakened by the activation gas at all bonding interfaces between the first electrode and the first separator, between the first separator and the second electrode, between the second electrode and the second separator, and between the base unit bodies. Therefore, even if the positive electrode and the negative electrode are expanded, the stress within the base unit body is distributed, and individual electrodes expand in the vertical direction, so that the above bending does not occur (see Fig. 5).

[0010] Furthermore, even in the electrode assembly with the lamination and stack type structure as shown in Fig.As shown in Figure 6, the electrode assembly of the stacked structure, in which the basic unit bodies of the first electrode / first separator / second electrode / second separator / first electrode / first separator are repeatedly stacked, has a bidirectionally symmetrical structure based on the second electrode. Thus, even if the volume of the electrode expands, the positive electrode and the negative electrode have the same expansion direction, so that bending behavior hardly occurs. However, the lamination and stacking type electrode assembly, in which the basic unit bodies of the first electrode / first separator / second electrode / second separator are repeatedly stacked, has an asymmetric expansion direction, and thus, as described above, structural deformation such as bending occurs during the charging and discharging of the activation process.

[0011] Therefore, in the case of applying a jig formation process of simultaneously performing charging and pressurizing the electrode assembly having the lamination and stack type structure, there is a need to develop an electrode assembly technology capable of preventing bending behavior. RevelationTechnical Problem

[0012] An object of the present invention is to improve the behavior that the electrode assembly is bent by an activation process in a lamination stack type electrode assembly.

[0013] Another object of the present invention is to improve the productivity of the battery by improving the bending behavior of the electrode assembly. Technical solution

[0014] An electrode assembly of the present invention includes a unit body stacking portion in which at least two base unit bodies are stacked, forming a four-layer structure by sequentially stacking a first electrode, a first separator, a second electrode, and a second separator, and wherein coating materials having an adhesive force are applied to the surfaces of the first and second separators and are applied to the electrode assembly, and the base unit body is adhered to an adjacent base unit body.

[0015] In the electrode assembly according to an embodiment of the present invention, an adhesive force between the base unit body and its adjacent base unit body may be equal to or greater than an adhesive force between the first electrode and the first separator in the base unit body.

[0016] In the electrode assembly according to an embodiment of the present invention, the second separator may be coated with the coating material on a side facing the second electrode and on an opposite side thereof, and the base unit bodies may be bonded to each other by the coating material of the second separator.

[0017] In the electrode assembly according to one embodiment of the present invention, the coating material may be formed from a mixture of inorganic particles and a binder polymer that bonds and fixes the inorganic particles together. At this time, the inorganic particles may form a densely packed structure to create interstitial volumes between the inorganic particles in the coating layer as a whole, and a pore structure may be formed in the coating layer by interstitial volumes defined by the inorganic particles.

[0018] In the electrode assembly according to an embodiment of the present invention, a difference between a thickness (d1) measured for 2 seconds under a pressure of 30 kgf and a thickness (d2) measured for 2 seconds under a pressure of 90 kgf may be 100 µm or less, which can prevent the bending behavior.

[0019] In the electrode assembly according to an embodiment of the present invention, the first electrode may be a positive electrode, and the second electrode may be a negative electrode.

[0020] In the electrode assembly according to an embodiment of the present invention, the base unit body can be formed by repeatedly stacking the 4-layer structure.

[0021] The present invention provides a secondary battery including the electrode assembly as described above, and such a secondary battery has an advantage of improving productivity by preventing bending behavior. Beneficial effects

[0022] According to an electrode assembly of the present invention, it is possible to prevent the bending behavior of the electrode assembly that may occur during the charging and discharging process because the separator of one base unit body and the first electrode of the other base unit body are bonded and fixed by the coating material applied to the separator by performing a lamination process for hot-pressing the electrode assembly before the first formation process. Short description of the drawings Fig. 1 is a side view showing the structure of a base unit according to an embodiment of the present invention. Fig. 2 is a side view showing the structure of a unit stacking portion according to an embodiment of the present invention. Fig.3 is a process diagram showing a process for manufacturing another base unit according to the present invention. Fig. Figure 4 is a schematic diagram of a principle in which bending behavior occurs in a conventional electrode assembly. Fig. Figure 5 is a schematic view showing the reason why bending behavior does not occur when a general activation process is performed on a lamination stack type electrode assembly instead of a jig formation. Fig. 6 is a schematic view showing a reason why bending behavior does not occur in an electrode assembly other than the lamination stack type structure of the present invention. Detailed description of the preferred embodiments

[0023] The terms and words used in the present specification and claims should not be construed as being limited to common terms or dictionary terms, and the inventor can properly define the concept of the terms to best describe his invention. The terms and words should be construed as meanings and concepts consistent with the technical idea of ​​the present invention. Accordingly, the embodiments described in the specification and the configurations described in the drawings are only the most preferred embodiments of the present invention and do not represent all the technical ideas of the present invention. It is understood that there may be various equivalents and variations in their place at the time of filing the present application.

[0024] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0025] An electrode assembly according to an embodiment of the present invention includes a unit body stacking portion in which one or more base unit bodies are stacked, forming a four-layer structure by sequentially stacking a first electrode, a first separator, a second electrode, and a second separator, and wherein coating materials having adhesive force are applied to the surfaces of the first and second separators and are applied to the electrode assembly, and the base unit body is adhered to an adjacent base unit body.

[0026] The electrode assembly according to an embodiment of the present invention is not simply composed of a plurality of repeatedly stacked base unit bodies. By performing a lamination process of heating and pressing the electrode assembly formed by stacking a plurality of base unit bodies under a temperature condition that maximizes the adhesive force of the coating material applied to the separator, the separator of one base unit body and the first electrode of the adjacent base unit body are bonded to each other, so that the respective bonding interfaces of the base unit body and the adjacent base unit are bonded to each other.

[0027] In the electrode assembly according to the present invention, the base unit is formed by alternately stacking electrodes and separators. At this time, the same number of electrodes and separators are stacked. For example, as shown in Fig. As illustrated in Figure 1, the base unit 110a can be formed by stacking two electrodes 111 and 113 and two separators 112 and 114. At this time, the positive electrode and the negative electrode can, of course, face each other through a separator. When the base unit is formed in this way, an electrode is located at one end of the base unit (see the electrode with reference numeral 111 in Figures Fig. 1 and Fig. 2), and a separator (see the separator with the reference number 114 in the Fig. 1 and Fig. 2) is located at the other end of the base unit.

[0028] The present invention has a fundamental function of making it possible to form a unit stacking section by repeatedly stacking one type of basic unit or by stacking two or more types of basic units in a predetermined order. To implement this function, the basic unit may have the following structure.

[0029] First, the base unit body can be formed by sequentially stacking a first electrode, a first separator, a second electrode, and a second separator. Specifically, base unit bodies 110a and 110b are formed by sequentially stacking a first electrode 111, a first separator 112, a second electrode 113, and a second separator 114 from top to bottom or from bottom to top, as shown in Fig.1. At this time, the first electrode 111 and the second electrode 113 are opposite electrodes. For example, if the first electrode 111 is a positive electrode, the second electrode 113 is a negative electrode.

[0030] As described above, when the first electrode, the first separator, the second electrode, and the second separator are sequentially stacked, the base unit 110a can be repeatedly stacked to form a unit stacking portion 100a, as shown in Fig. 2 is illustrated by a manufacturing step (second step) for a unit stack section, which will be described later.

[0031] With reference to Fig.3 describes the process for manufacturing the base unit of the present invention. First, a first electrode material 121, a first separator material 122, a second electrode material 123, and a second separator material 124 are prepared. Here, the first separator material 122 and the second separator material 124 may be the same material. Then, the first electrode material 121 is cut to a predetermined size by the cutting device C1, and the second electrode material 123 is also cut to a predetermined size by the cutting device C2. Then, the first electrode material 121 is stacked on the first separator material 122, and the second electrode material 123 is stacked on the second separator material 124.

[0032] Then, it is preferable to bond the electrode material and the separator material together in the laminating devices L1 and L2. The base unit body in which the electrode and the separator are integrally combined can be manufactured by such adhesion. The bonding methods may vary. The laminating devices L1 and L2 apply pressure or heat to the material for adhesion. Such adhesion facilitates stacking of the base unit bodies when manufacturing the unit body stacking unit. Furthermore, such adhesion is advantageous for the alignment of the base unit bodies. When the first separator material 122 and the second separator material 124 are cut to a predetermined size by the cutting device C3 after such bonding, the base unit body 110a can be manufactured. During this process, the end of the separator is not bonded to the end of the adjacent separator.

[0033] In this way, the electrode can be bonded to an adjacent separator in the base unit body. Alternatively, the separator can be bonded to the electrode. At this time, the electrode is preferably bonded to the separator as a whole, from the side facing the separator. This is because the electrode can be securely fixed to the separator. Typically, the electrode is smaller than the separator.

[0034] For this purpose, an adhesive can be applied to the separator. However, to use the adhesive as described above, it is necessary to apply the adhesive to the bonding surface in the form of meshes or dots. The reason for this is that reactive ions such as lithium ions cannot pass through the separator if the adhesive is unconditionally applied to the entire bonding surface. Therefore, when using an adhesive, it is difficult to completely bond the electrode, even if it is possible to bond the electrode as a whole (i.e., across the entire bonding surface) to the separator.

[0035] Alternatively, the electrode can be fully bonded to the separator by a separator having a coating layer with adhesive strength. The separator can comprise a porous separator substrate, such as a polyolefin-based separator substrate, and a porous coating layer applied to one or both sides of the separator substrate. At this time, the coating layer can be formed from a mixture of inorganic particles and a binder polymer that bonds and fixes the inorganic particles together.

[0036] Here, the inorganic particles can improve the thermal stability of the separator. That is, the inorganic particles can prevent the separator from shrinking at high temperatures. Furthermore, the binder polymer can improve the mechanical stability of the separator by fixing the inorganic particles. Furthermore, the binder polymer can bond the electrode to the separator. Unlike the adhesive described above, since the binder polymer is distributed throughout the coating layer, adhesion can occur over the entire bonding surface. Therefore, using such a separator can more securely attach the electrode to the separator. The laminating device described above can be used to improve adhesion.

[0037] However, the inorganic particles can form a densely packed structure to create interstitial volumes between the inorganic particles as a whole in the coating layer. At this time, the pore structure in the coating layer can be formed by the interstitial volume defined by the inorganic particles. Due to this pore structure, lithium ions can easily pass through the separator even when a coating layer is formed on the separator. For comparison, the interstitial volume defined by the inorganic particles may be blocked by the binder polymer depending on its location.

[0038] The filling structure here can be described as a structure containing gravel in a glass bottle. Therefore, when the inorganic particles form a filling structure, the interstitial volume between the inorganic particles is not formed locally in the coating layer, but rather the interstitial volume between the inorganic particles is formed entirely within the coating layer. Accordingly, as the size of the inorganic particles increases, the size of the pores also increases by the interstitial volume. Due to this charge structure, lithium ions can easily pass through the separator across the entire surface of the separator.

[0039] The unit body stacking portion of the present invention is formed by repeatedly stacking the base unit bodies, and the joining interface between a base unit body and an adjacent base unit body is bonded.

[0040] As described above, in the conventional lamination and stacking type electrode assembly, an adhesive force is formed between the electrode and the separator in the base unit body. However, since the unit body stacking portion is formed by simply laminating the base unit bodies, no adhesive force is formed between the base unit bodies. When a formation process including pressurization and charging is performed on the electrode assembly with the same structure, the first electrode and the second electrode are expanded. At this time, since the volume expansion coefficients of the first electrode and the second electrode are different, a bending behavior occurs in which the base unit as a whole is bent when stress accumulates inside the base unit body.

[0041] According to the present invention, by heating and pressing the electrode assembly before the formation process, the adhesive strength of the coating material applied to the separator surface is maximized, and one base unit is attached to another base unit. Even if the positive electrode and the negative electrode expand during the subsequent formation process, the stress caused by the volume expansion of the electrode is relieved and the directionality of the expansion is balanced, so that the bending behavior of the electrode assembly does not occur because the positive electrode and the negative electrode are continuous.

[0042] As described above, the coating material is formed from a mixture of inorganic particles and a binder polymer that bonds and fixes the inorganic particles together, and the coating material can be applied to the first separator and the second separator, respectively. In one embodiment of the present invention, in the first separator, the coating material is applied to both sides facing the first electrode and the second electrode, and in the second separator, the coating material is applied to a surface facing the second electrode and its opposite surface.

[0043] The binder polymer contained in the coating material exhibits adhesive strength upon heating. Since the temperature at which the adhesive strength is maximized varies for each type of binder polymer, the optimal temperature during the heating and pressing process of the electrode assembly of the present invention is preferably the temperature at which the adhesive strength of the binder polymer is maximized.

[0044] The electrode assembly of the present invention is characterized in that the coating material imparts an adhesive force to the bonding interface between the base unit bodies, and the adhesive force in the unit body stacking portion between a base unit body and an adjacent base unit body is equal to or greater than the adhesive force between the first electrode and the first separator in the base unit body.

[0045] This is because the electrolyte is not well impregnated at the bonding interface (referred to as a "lamination surface") between the first separator and the first electrode in the base unit body because it is adhered by the coating material already applied to the separator when the base unit body is manufactured, while the electrolyte between a base unit and a base unit is well impregnated because the adhesion between a base unit body and a base unit body has not been achieved before the heating and pressing process (lamination method) of the present invention, and therefore the adhesive force is well developed by the subsequent heating and pressing process.Thus, in the electrode assembly of the present invention, the adhesion in the unit body stacking portion between the base unit bodies and between the adjacent base unit bodies becomes equal to or greater than the adhesion between the first electrode and the first separator in the base unit body.

[0046] A method for manufacturing a secondary battery including the electrode assembly of the present invention will be described below.

[0047] The method for manufacturing a secondary battery of the present invention includes the following steps: preparing a base unit body forming a 4-layer structure in which a first electrode, a first separator, a second electrode, and a second separator are sequentially stacked (S100); manufacturing a base unit body stacked portion by repeatedly stacking the base unit body (S200); accommodating the electrode assembly including the unit body stacked portion in a battery case, then injecting an electrolyte and sealing the battery case (S300); and adhering a second separator of one base unit body to a first electrode of its adjacent base unit body in the unit body stacked portion by applying heat and pressure (S400).

[0048] Since the step of manufacturing the base unit body (S100) and the step of manufacturing the unit body stacking portion (S200) have been described above, the process after the stacking portion manufacturing step will be described in detail.

[0049] The assembly step (S300) includes inserting the electrolyte assembly prepared above into the battery case and then injecting the electrode. In some cases, there is a step of storing the assembled secondary battery at room temperature and atmospheric pressure for a predetermined period of time (burn-in) to allow the electrode to be well impregnated into the first electrode, first separator, second electrode, and second separator.

[0050] The lamination step (S400) is a step of applying an adhesive force between the base unit body constituting the unit body stacking portion and the adjacent base unit, in which the adhesive force of the binder contained in the coating material applied to the first separator is formed by heating and pressing, so as to enable the base unit bodies to be bonded to each other.

[0051] Therefore, it is preferable to adjust the temperature of the lamination step by appropriately selecting and adjusting the temperature at which the bonding strength of the binder is maximized, taking into account the physical properties of the binder. Specifically, the temperature of the lamination step may be, but is not limited to, 45°C to 85°C. In one embodiment of the present invention, the temperature of the lamination step was preferably 45°C to 70°C.

[0052] If the lamination temperature is too low, it is difficult to achieve the object of the present invention because the adhesion between a base unit body and an adjacent base unit body is not sufficient, and if it is too high, the adhesion of the binder rapidly decreases and the coating material layer containing the binder may be peeled off from the separator.

[0053] The pressure of the lamination step (S400) can be selected within a suitable numerical range, taking into account the thickness of the electrode assembly, the electrode, and the physical properties of the binder applied to the separator. Specifically, it can be 1 to 10 kgf / cm 2 , preferably 2 to 6 kgf / cm 2 and more preferably 3 to 5 kgf / cm 2 If the pressure is less than 1 kgf / cm 2, it may be difficult to achieve the object of the present invention due to insufficient pressure and insufficient adhesion between a base unit body and a base unit body, and when the pressure is 10 kgf / cm 2 exceeds, the pressure is too strong to damage the electrode assembly, which is undesirable.

[0054] The pressing time of the lamination step (S400) can be 2 to 20 minutes, and more preferably 5 to 15 minutes. The pressing time can be appropriately selected within the above range, taking into account the thickness of the electrode assembly and the properties of the binder applied to the separator.

[0055] The lamination step (S400) according to one embodiment of the present invention is performed before the initial formation process. In the present invention, the formation process should be understood as a concept that involves an initial charge that is fully or partially charged to a certain state of charge (SOC) capacity to stabilize the structure of the electrode.

[0056] During the initial charging step, lithium ions move from the lithium transition metal oxide used as the positive electrode to the carbon electrode used as the negative electrode. Since lithium ions are highly reactive at this time, they react with the negative carbon electrodes to form compounds such as Li2CO3, LiO, and LiOH. These compounds form SEI films on the surface of the negative electrodes. The SEI film is a non-conductor formed as the amount of ion migration in the battery increases. The formation of the SEI film prevents lithium ions and other substances from reacting at the negative electrode during subsequent battery charging. Furthermore, the SEI film acts as an ion tunnel, allowing only lithium ions to pass through.After the SEI film is formed, lithium ions do not react with the negative electrode or other substances, thus reversibly maintaining the amount of lithium ions and reversibly maintaining the charging and discharging of the lithium secondary battery, thus improving battery life. Furthermore, even when the SEI film is exposed to high temperatures or repeated charging and discharging, the battery thickness is less likely to change.

[0057] When performing the initial charge, a large amount of side reaction gases is generated, which may cause the SEI film to form unevenly due to the flow of the side reaction gas. To solve this problem, a process of pressing the secondary battery can be performed simultaneously with the initial charge. Pressing can be performed using a jig or the like, but is not limited to this, as a means by which the secondary battery can be pressed. The pressurization of the battery cell can be 100 kgf / cm 2 up to 500 kgf / cm 2 take place.

[0058] The volume of the first electrode and the second electrode is expanded by the formation process. Therefore, to achieve the objective of the present invention, it is preferable that the lamination step (S400) be performed before the first formation process or during the first formation process.

[0059] At this time, the temperature during the formation process may be 45°C or less. When the temperature during the first formation process exceeds 45°C, the binder contained in the coating material applied to the separator exerts an adhesive force that can bond a base unit body to a base unit body in abutting relationship. Therefore, since it is not necessary to perform the heating and pressing process before the first formation process, the manufacturing method of the present invention can be particularly useful when the temperature in the first formation process needs to be set to 45°C or less.

[0060] After the lamination and formation process as described above has been performed, one or more of an aging process, a degassing process, and a formation process may be further included.

[0061] The present invention will be described in detail below with reference to examples. However, the embodiments according to the present invention can be modified in various other forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. The embodiments of the present invention are provided to describe the present invention in more detail to those skilled in the art. Manufacturing Example 1Preparation of a positive electrode

[0062] A positive electrode mixture slurry was prepared by adding 96.25 wt% LiCoO2 as the positive electrode active material, 1.5 wt% carbon black as the conductive material, and 2.25 wt% PVDF as a binder to N-methyl-2-pyrrolidone (NMP) as the solvent. The positive electrode mixture slurry was coated onto a positive electrode plate, a thin aluminum film (Al film) with a thickness of 12 µm, and dried to prepare a positive electrode, followed by roller pressing. Production of a negative electrode

[0063] A negative electrode mixture slurry was prepared by adding 96 wt% carbon powder as the negative electrode active material, 3 wt% carbon black as the conductive material, and 1 wt% polyvinylidene fluoride (PVdF) as a binder to N-methyl-2-pyrrolidone (NMP) as a solvent. The negative electrode mixture slurry was coated onto a negative electrode plate, a thin copper film (Cu film) with a thickness of 10 µm, and dried to prepare a negative electrode, followed by roller pressing. Manufacturing a base unit body

[0064] On both sides of the polyolefin separator, a separator coated with a coating material containing a binder A was prepared, and a base unit body was bonded with a positive electrode / separator / negative electrode / separator using a Fig. 3 shown laminating device.

[0065] Binder A is a mixture of PVdF-HFP copolymer with a molecular weight of 410-450 kg / mol (a polymer material with an HFP content of 15 mol% or more and a Tm of 140 degrees or less compared to PVdF) and PVDF-CTFE copolymer with a molecular weight of 250 to 300 kg / mol and a Tm of 160 °C or higher. Assembly step

[0066] The three base unit bodies were stacked to form a unit body stacking section, and the unit body stacking section was housed in an outer bag material made of a CPP / aluminum / nylon laminate plate. Ethyl methyl carbonate electrolyte containing LiPF6 was injected, and the outer bag material was heat-sealed to complete the secondary battery assembly. Production example 2

[0067] In Production Example 1, the assembly of the secondary battery was completed in the same manner as in Production Example 1, except that the type of binder contained in the coating material applied to the separator was changed to Binder B.

[0068] Binder B is a mixture of PVdF-HFP copolymer with a molecular weight of 380-400 kg / mol (a polymer material with an HFP content of 8 mol% or less and a Tm of 150 °C or higher compared to PVdF) and PVDF-CTFE copolymer with a molecular weight of 250 to 300 kg / mol and a Tm of 160 °C or higher. Production example 3

[0069] The assembly of the secondary battery was completed in the same manner as in Preparation Example 1, except that the solvent of the electrolyte in the assembly step of Preparation Example 1 was replaced with dimethyl carbonate. Comparison example 1

[0070] After the assembled secondary battery of Preparation Example 1 was aged at room temperature for about 72 hours, the bag with the electrode assembly was placed on a pressurization jig and subjected to a pressure of 5 kgf / cm 2 and a temperature of 25 °C for 11 minutes. The secondary battery was then charged while pressurized at room temperature with a pressure of 5 kgf / cm 2 was loaded with, and then completely discharged. Examples 1 to 5

[0071] After the assembled secondary battery of Preparation Example 1 was aged at room temperature for about 72 hours, the bag with the electrode assembly was placed on a pressurization jig and subjected to a pressure of 5 kgf / cm 2and respective temperatures of 45, 50 °C, 55 °C, 60 °C and 65 °C for 11 minutes. The secondary battery was then charged while maintained at room temperature with a pressure of 5 kgf / cm 2 was pressurized and then completely discharged. Comparison example 2

[0072] After the assembled secondary battery of Preparation Example 1 was aged at room temperature for about 72 hours, the bag with the electrode assembly was placed on a pressurization jig and subjected to a pressure of 5 kgf / cm 2 and a temperature of 70 °C for 11 minutes. The secondary battery was then charged while it was pressurized at room temperature with a pressure of 5 kgf / cm 2 was pressurized and then completely discharged. Comparative examples 3 to 4

[0073] After the assembled secondary battery of Production Example 2 was aged at room temperature for about 72 hours, the bag with the electrode assembly was placed on a pressurization jig and subjected to a pressure of 5 kgf / cm 2 and respective temperatures of 55 °C and 60 °C for 11 minutes. The secondary battery was then charged while maintained at room temperature with a pressure of 5 kgf / cm 2 was pressurized and then completely discharged. Comparative examples 6 to 8

[0074] After the assembled secondary battery of Production Example 2 was aged at room temperature for about 72 hours, the bag with the electrode assembly was placed on a pressurization jig and subjected to a pressure of 5 kgf / cm 2and respective temperatures of 65 °C, 70 °C and 75 °C for 11 minutes. The secondary battery was then charged while kept at room temperature with a pressure of 5 kgf / cm 2 was pressurized and then completely discharged. Example 9

[0075] After the assembled secondary battery of Preparation Example 3 was aged at room temperature for about 72 hours, the bag with the electrode assembly was placed on a pressurization jig and subjected to a pressure of 5 kgf / cm 2 and a temperature of 55 °C for 11 minutes. The secondary battery was then charged while it was pressurized at room temperature with a pressure of 5 kgf / cm 2 was pressurized and then completely discharged. Comparison example 5

[0076] After the assembled secondary battery of Preparation Example 1 was aged at room temperature for about 72 hours, the secondary battery was charged while being maintained at room temperature with a pressure of 1 kgf / cm 2 was pressurized and then completely discharged. Comparison example 6

[0077] After the assembled secondary battery of Preparation Example 1 was aged at room temperature for about 72 hours, the secondary battery was charged while being maintained at room temperature with a pressure of 10 kgf / cm 2 was pressurized and then completely discharged. Experimental Example 1 - Measuring the adhesive force after loading

[0078] For each secondary battery of Examples 1 to 8 and Comparative Examples 1 to 4, the pouch was opened to remove the electrode assembly. A sample was then taken from the electrode assembly for adhesive strength measurement and immediately adhered to a microscope slide. The peeling was performed at a 90-degree angle and at a speed of 10 mm / min to measure the adhesive strength. The results are shown in Table 1. Table 1 outline binder Temperature during lamination (°C) Adhesive strength (gf / 20mm) Comparison example 1 A 25 0 Example 1 45 25 Example 2 B 50 35 Example 3 55 41 Example 4 60 20,5 Example 5 65 9 Comparison example 2 70 1 Comparison example 3 55 2 Comparison example 4 60 2 Example 6 65 4 Example 7 70 25 Example 8 75 3,8

[0079] As shown in Table 1, the temperature at which the adhesive strength is maximized varies according to the type of binder contained in the coating material applied to the separator. The binder of Preparation Example 1 exhibited the maximum adhesive strength during lamination at 55°C, and the binder of Preparation Example 2 exhibited the maximum adhesive strength at 70°C. Therefore, in the lamination process of the present invention, the temperature conditions are preferably selected according to the temperature of the binder, taking into account the adhesive performance.

[0080] Experimental Example 2 - Measurement of Wet Adhesive Strength According to an Electrolyte. Twenty secondary batteries manufactured as in Example 3 and Example 9 were prepared, and the pouch was opened to remove the electrode assembly from the pouch. A sample was then taken out for adhesive strength measurement and immediately adhered to a glass slide. The peeling was performed at a speed of 10 mm / min at an angle of 90 degrees to the bonding interface between the positive electrode and the separator in the base unit body to measure the adhesive strength (this is called the bonding surface bonding strength). The bonding strength was measured in the same way for the bonding interface between the base unit body and the base unit body (this is called the bonding surface bonding strength).During peeling, a peel test was conducted by holding the electrode and the separator together to prevent damage to the adhesive force of the sample, and the adhesive force measurement results are shown in Table 2 below. Table 2 solvent Adhesive strength (gf / 20 mm) Laminating surface Stacking area Example 3 Ethyl methyl carbonate 30~41 38~50 Example 9 Dimethyl carbonate 46~56 50~60

[0081] In the electrode assembly of the present invention, after charging, an adhesive force is formed between a base unit body and an adjacent base unit body (stacked surface), and the magnitude of the adhesive force is similar to or greater than the adhesive force between the electrode in the base unit body and the separator (laminate surface). As described above, in the electrode assembly of the present invention, an adhesive force is formed between a base unit body and an adjacent base unit body through a heating and pressing process before the formation process, and the positive electrode and the negative electrode constituting the electrode assembly thereby become continuous.Thus, even if electrode expansion occurs due to charging, the stress caused by electrode expansion is alleviated and the directionality of the expansion disappears, so that the bending behavior of the electrode assembly can be prevented. Experimental Example 3 - Checking for an existing bend

[0082] For each secondary battery of Examples 2 to 4 and Comparative Examples 5 and 6, the pouch was opened to remove the electrode assembly. After a force of 30 kgf was applied to the electrode assembly for 2 seconds, the thickness of the electrode assembly was measured (d1). Then, after a force of 90 kgf was applied for 2 seconds, the thickness of the electrode assembly was measured (d2). The difference between d1 and d2 was measured, and the results are shown in Table 3. The larger the difference in thickness, the greater the bending behavior. When the thickness difference is 0, it means that no bending occurred. Table 3 outline Laminating conditions Thickness difference Temperature (°C) Pressure (kgf / cm 2 ) (µm) Example 2 50 5 100 Example 3 55 5 0 Example 4 60 5 0 Comparison example 5 25 1 200 Comparison example 6 25 10 320

[0083] Referring to Table 3, each electrode assembly according to Examples 2 to 4 of the present invention had a thickness difference of 100 μm or less, and no bending behavior occurred, or even if the bending behavior occurred, it was difficult to visually confirm the bending with the naked eye. On the other hand, each electrode assembly of Comparative Examples 5 and 6, in which only pressurization was performed without heating, had a thickness difference of 200 μm or more before the formation process, and it was found that the bending behavior was enhanced compared to the above examples.

[0084] Therefore, in order to prevent the bending behavior of the electrode assembly, it is desirable to form an adhesive force at a bonding interface (stacking surface) between a base unit body and a base unit body by performing a lamination process of heating and pressing on the electrode assembly at an appropriate temperature before the formation process. QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] Korean Patent Application No. 10-2018-0168229

[0001]

Claims

[1] An electrode assembly comprising a unit body stacking portion formed by stacking at least two base unit bodies (110a) forming a 4-layer structure in which a first electrode (111), a first separator (112), a second electrode (113), and a second separator (114) are sequentially stacked, wherein coating materials are applied with adhesive force to the respective surfaces of the first and second separators, and wherein a base unit body is adhered to its adjacent base unit body in the unit body stacking portion. [2] The electrode assembly according to claim 1, wherein the adhesive force between the base unit body and its adjacent base unit body is equal to or greater than the adhesive force between the first electrode and the first separator in the base unit body. [3] The electrode assembly according to claim 1, wherein the second separator is coated with the coating material on a side facing the second electrode and on an opposite side thereof, and the base unit bodies are bonded to each other by the coating material of the second separator. [4] The electrode assembly according to claim 1, wherein a difference between a thickness (d1) measured for 2 seconds under a pressure of 30 kgf and a thickness (d2) measured for 2 seconds under a pressure of 90 kgf is 100 µm or less. [5] The electrode assembly of claim 1, wherein the first electrode is a positive electrode and the second electrode is a negative electrode. [6] The electrode assembly according to claim 1, wherein the base unit body is formed by repeatedly stacking the 4-layer structure. [7] A secondary battery comprising an electrode assembly according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Stack-type electrode assembly with no deflection of the electrode and manufacturing methods thereof

    KR1020200078908A