Electrode arrangement, manufacturing an electrode arrangement and secondary battery with an electrode arrangement
By setting the angle between the inner end and maximum curvature point of the electrode assembly to 40°-98°, the core deformation and internal short circuit issues in cylindrical batteries are mitigated, improving battery stability and lifespan.
Patent Information
- Application Number
- DE202024103667
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Priority Date
- 2023-11-02
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2034-07-31
AI Technical Summary
Cylindrical batteries face issues with core deformation due to electrode contraction and expansion, leading to core collapse and internal short circuits, especially with low-resistance, high-capacity designs and the use of silicon-based active materials, which deteriorate battery life and pose safety risks.
An electrode assembly design where the angle between the inner end of the first electrode and the maximum curvature point is set between 40° and 98°, maintaining a cylindrical shape and preventing core collapse by adjusting the angle and curvature of the electrode assembly during manufacturing.
Prevents core deformation, reduces the risk of internal short circuits, and enhances the stability and lifespan of the battery by maintaining the core cavity's circular shape during charging and discharging processes.
Smart Images

Figure 00000000_0002_ABST 
Figure 00000000_0001_ABST 
Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL AREA
[0001] The present invention relates to an electrode arrangement, the manufacture of an electrode arrangement and a secondary battery with the electrode arrangement, and in particular to an electrode arrangement in which core deformation is improved by changing a design of the electrode arrangement, the manufacture of an electrode arrangement and a cylindrical secondary battery with the electrode arrangement. State of the art
[0002] For a cylindrical battery, a coiled roll electrode assembly is manufactured by coiling a long electrode of a predetermined width into a coil shape. The cylindrical battery, created by inserting such an electrode assembly into a battery casing, experiences repeated contraction and expansion of one electrode during charging and discharging. In particular, if a tab (in the tab) is located in a core of the electrode assembly, or if the degree of contraction / expansion of the electrode assembly increases due to a silicon-based active material added to a negative electrode, the pressure acting on a core section of the electrode assembly increases significantly.
[0003] The core section of the cylindrical battery is a space containing a winding core (mandrel) used for winding the electrode assembly, and there is an empty space, that is, a core cavity, used in a cylindrical battery assembly process, such as inserting the electrode assembly into the battery casing and a welding process.
[0004] Recently, with the increasing prevalence of low-resistance, high-capacitance designs, there has been a rise in cases where the electrode array incorporates multiple tabs or incorporates a silicon-based active material. This also increases the risk of core deformation of the electrode array due to contraction / expansion.In particular, there are problems such as a decrease in battery life due to a phenomenon (core collapse) where the core cavity fails to maintain a circular shape and collapses, and a negative electrode and a positive electrode coming into direct contact, causing an internal short circuit, which leads to heat generation and ignition, due to a phenomenon (core impact) where an end section of the positive electrode located on the core section and the negative electrode adjacent to it are deformed beyond a certain degree, resulting in damage to a separator between the positive and negative electrodes.
[0005] To solve the problems of reduced battery life, separator damage, and internal short circuits due to electrode assembly deformation, it is necessary to develop a technology capable of addressing the phenomenon of the core cavity failing to maintain a circular shape and collapsing in the relevant area, and suppressing the occurrence of internal short circuits due to separator damage. SUMMARY OF THE INVENTION
[0006] The present invention arose in the endeavor to design an electrode arrangement in such a way as to counteract core deformation, and to manufacture an electrode arrangement and to provide a secondary battery with the electrode arrangement.
[0007] However, the problem to be solved by the present invention is not limited to the problem described above, and other, undescribed problems will be obvious to the person skilled in the art from the following description. TECHNICAL SOLUTION
[0008] The present invention is defined by the subject matter of the independent claims. Specific examples of the present invention are given by the additional features of the dependent claims.
[0009] An electrode assembly comprises a first electrode, a separator, and a second electrode. The first electrode, the separator, and the second electrode are stacked on top of each other and wound around a winding axis. The angle formed between a line extending from the winding axis through an inner end of the first electrode and a line extending from the winding axis through a point of maximum curvature of the first electrode is between 40° and 98°. This angle can be determined in a plane perpendicular to the winding axis.
[0010] The terms first electrode and second electrode are used herein in accordance with the relevant technical field of battery design and manufacture, particularly with regard to a secondary battery. The first electrode and / or the second electrode may be configured to accept and store charge carriers such as electrons and / or ions (especially lithium ions). The first electrode and the second electrode may have opposite polarities so that they can accept or release charge carriers during a charging process of the electrode assembly, and vice versa during a discharging process of the electrode assembly. The materials and functionality of the first electrode and the second electrode may be selected or designed as known to those skilled in the art, unless otherwise specified herein.
[0011] For example, the first electrode can be a positive electrode and the second electrode can be a negative electrode. In other examples, the first electrode can be a negative electrode and the second electrode can be a positive electrode. Generally, a positive electrode can include a current collector, which may be provided as a plate, sheet, or film onto which a positive active material is applied. For example, the positive active material may contain a lithium metal oxide such as lithium cobalt oxide or lithium iron phosphate, or any other suitable material. The positive electrode current collector can be made of an electrically conductive material, such as aluminum. Generally, a negative electrode can also include a current collector, which may be provided as a plate, sheet, or film onto which a negative active material is applied.For example, the negative active material can contain a carbon-based material, such as graphite. The current collector of the negative electrode can be made of an electrically conductive material, such as copper.
[0012] The term separator is used herein in accordance with the relevant technical field of battery design and manufacturing, particularly with regard to a secondary battery. Specifically, the separator may be a porous membrane configured to allow charge carriers (e.g., ions, lithium ions, and / or electrons) to pass through while being essentially impermeable to solid materials. The separator may be placed between the first and second electrodes to prevent a short circuit between them.
[0013] The transfer of charge carriers between the first and second electrodes can be facilitated by an electrolyte, which may be present, at least partially, between the first and second electrodes. The electrolyte can be added to the electrode assembly after it is placed in a battery casing. In specific examples, it can be assumed that the electrode assembly contains an electrolyte such that it is present between the first and second electrodes.
[0014] The first electrode, the separator, and the second electrode can be provided as layers. The first electrode, the separator, and the second electrode can be stacked in a specific sequence. In specific examples, the second electrode, the separator, the first electrode, and another separator are stacked in this sequence to form a so-called monocell. In other examples, one or more monocells can be stacked (repeatedly) on top of the monocell in the aforementioned sequence to form a multicell.
[0015] The electrode assembly can comprise a single cell (or a multi-cell) wound into a roll. Such a roll can also be referred to as a jellyroll. In particular, within the single cell, the first electrode, the separator, and the second electrode, and optionally another separator, can be wound together around the winding axis. Thus, the electrode assembly can have a cylindrical shape, especially a cylindrical shape with a helical cross-section. Furthermore, the first electrode, the separator, and the second electrode of the electrode assembly can be wound together (i.e., in a state where they are stacked on top of each other in the aforementioned order) around the winding axis, so that the electrode assembly exhibits (general) cylindrical symmetry with respect to the winding axis.In cylindrical symmetry, an axial direction can be parallel to the winding axis; a radial direction can be perpendicular to the winding axis and (approximately) perpendicular to an outer circumferential surface of the electrode array; and a circumferential direction can be perpendicular to both the axial and radial directions and circular around the winding axis. Additionally, a winding direction can specify a direction along one or each of the first electrode, the separator, and the second electrode in a top view. The winding direction can thus follow a helical path around the winding axis. Depending on the context, the winding direction can be approximated as circular around the winding axis, like the circumferential direction, in the sense of a winding direction.
[0016] Unless otherwise specified, an azimuth angle, as used herein, can indicate an angle between two lines in a plane perpendicular to the winding axis. The two lines forming the azimuth angle may intersect at the winding axis.
[0017] Unless otherwise specified, geometric features relating to a line, angle, curvature, etc., as used herein, generally refer to a top view of the electrode assembly parallel to the winding axis. Thus, unless otherwise specified, such geometric features may refer to the (approximately) cylindrical geometry of the electrode assembly in a wound state around the winding axis. Furthermore, unless otherwise specified, any straight line or line as used herein may denote a straight line.
[0018] The cylindrical symmetry referred to herein can be an approximation such that a spiral shape in plan view and / or a spiral cross-section of the electrode arrangement is considered to be an approximate circular shape in plan view and / or a circular cross-section. The plan view can refer to a view parallel to the winding axis. The electrode arrangement can have a spiral end face around the winding axis if the first electrode, the separator, and the second electrode are wound around the winding axis. The cross-section of the electrode arrangement can refer to a cross-section perpendicular to the winding axis. The cross-section of the electrode arrangement can be spiral around the winding axis if the first electrode, the separator, and the second electrode are wound around the winding axis.
[0019] One, some, or all of the first electrode, the separator, and the second electrode may have a rectangular shape in a plan view before winding. The winding axis may be parallel to (at least) one of the edges of the first electrode, the separator, and the second electrode. In specific examples, the first electrode, the separator, and the second electrode may each have a rectangular shape in a plan view and be arranged such that their respective edges are parallel to each other.
[0020] In general, the term curvature can be used here as it is commonly used in mathematics. In particular, curvature can specify the degree by which a curve deviates from a straight line. Alternatively or additionally, curvature can specify the degree by which a surface deviates from a plane. Curvature, as used here, can specify for any part of a curve how much the direction of the curve changes over a small (infinitesimal) distance traveled (e.g., in angles per unit distance). Curvature can be a measure of a change in direction at a point along the curve. In particular, curvature can be a measure of the (instantaneous) rate of change of a unit tangent vector to the curve at point P as point P moves along the curve at a unit velocity.In a specific example, the position of the point P(s) can be a function of the parameter s, which can be, for example, time or an arc length from a given origin; and T(s) can be a unit tangent vector of the curve at P(s), which is also the derivative of P(s) with respect to s.
[0021] The curve referred to herein may be a profile (and / or contour, outline, or the like) of the first electrode in plan view (i.e., in a view parallel to the winding direction). In particular, the first electrode may be provided as a sheet or layer, so that in plan view the first electrode is perceived as a thick (ideally helical) curve. Alternatively or additionally, the same may be true for the second electrode and / or the separator. The curve may be continuously differentiable near P, so that a tangent along the curve may vary continuously. The curve may be twice differentiable at each P, so that a curvature exists along the curve, for example, as a derivative of T(s) with respect to s, as defined above.
[0022] Alternatively or additionally, the curvature, as used herein, can be determined with respect to an osculating circle (circle of curvature) on the curve. An osculating circle at point P of a curve can be a circle that has the same tangent and the same curvature as the curve. A tangent line can be an approximation of a curve at a point P on the curve. The osculating circle can be an approximation of the curve at point P. If the curvature at a point is not zero, then the reciprocal of the curvature is considered to be a radius of curvature, i.e., the radius of an osculating circle. The center of the osculating circle is considered to be the center of curvature and can be constructed by plotting the radius of curvature perpendicular to the tangent of the curve in the direction in which the curve bends.
[0023] Furthermore, the curvature as used herein can be determined as a derivative (or differential quotient) of a central angle at the center of the osculating circle with respect to a circular arc at the osculating circle.
[0024] In each of the above options for determining the curvature of the first electrode, the curvature can be determined from a top-view or cross-sectional image of the electrode assembly taken at a viewing angle parallel to the winding axis. Specifically, the curve can be determined as the profile of the first electrode when visually identified in an image taken at a viewing angle of the electrode assembly parallel to the winding axis. The curvature can then be determined from this curve.
[0025] The point of maximum curvature, as used herein, can specify a point on (or of or in) the first electrode (or the second electrode) where the curvature of the first electrode (or the second electrode) is greatest (i.e., maximal) in a top view of the electrode assembly. Thus, the point of maximum curvature can be a point on the first electrode where the first electrode exhibits the greatest curvature in a top view of the electrode assembly. Alternatively or additionally, the point of maximum curvature can be a point on the first electrode where the oscillating circle at the first electrode is smallest. Additionally or alternatively, the same can apply to the second electrode and / or the separator.
[0026] In specific examples, the overall curvature of the first electrode may (tend to) decrease as the first electrode extends from the winding axis to an outer circumference of the electrode assembly. In other words, the curvature of the first electrode may generally decrease in a radial outward direction or in an outward direction (winding direction) along the first electrode's spiral. The general decrease in the curvature of the first electrode in a radial outward direction (or winding direction) may be due to the winding of the first electrode, separator, and second electrode together around the winding axis. Additionally or alternatively, the curvature of the second electrode and / or separator may generally decrease in a radial outward direction.
[0027] Simultaneously, the point of maximum curvature can occur in a section closer to the winding axis than to the outer circumference of the electrode assembly. A portion of the electrode assembly that is closer to the winding axis than to the outer circumference in a top view of the electrode assembly can be designated as a core section. The core section can further be specified in detail as below. The point of maximum curvature can occur or be located in the core section of the electrode assembly (in a top view). This can apply to the first electrode. Additionally or alternatively, this can also apply to the second electrode and / or the separator.
[0028] When the first electrode is wound around the winding axis, it extends, in a top view, between an inner end and an outer end in the winding direction. The inner end can be located radially inward, for example, near or at the winding axis. The outer end can be located radially outward, for example, at or near the outer circumference of the electrode assembly. The same can apply, alternatively or additionally, to the second electrode.
[0029] According to the present disclosure, a straight line (a first line) can be formed that connects the winding axis with an inner end of the first electrode in a plane perpendicular to the winding axis. For example, such a line extends from the winding axis through the inner end of the first electrode in a plane perpendicular to the winding axis. The line can be imaginary and can be constructed specifically to determine an angle between it (i.e., the first line) and another line (i.e., the second line, as detailed below) that passes through the winding axis and the point of maximum curvature.
[0030] According to the present disclosure, a straight line (a second line) can be formed that connects the winding axis with the point of maximum curvature of the first electrode in a plane perpendicular to the winding axis. For example, such a line extends from the winding axis through the point of maximum curvature of the first electrode in a plane perpendicular to the winding axis. The line can be imaginary and can be constructed specifically to determine the angle between it (i.e., the second line) and the line extending through the winding axis and the inner end of the first electrode (i.e., the first line).
[0031] In the present disclosure, the angle between the line extending from the winding axis through an inner end of the first electrode and the line extending from the winding axis through the point of maximum curvature (i.e., between the first line and the second line) can be 40° or greater and 98° or less in a view parallel to the winding axis. Alternatively, the angle can be within any range of values disclosed herein. As mentioned above, the view parallel to the winding axis can also mean a viewing angle in the axial direction of a cylindrical symmetry of the electrode arrangement.
[0032] Alternatively or additionally, an electrode assembly may be provided in which a first electrode, a separator, and a second electrode are stacked and wound together. At a core section of the electrode assembly, an angle formed between a longitudinal end section of the first electrode and a point where the curvature of the first electrode is greatest may be greater than 40° and 98° or less about a winding axis.
[0033] The core section can be specified as above and / or as below. The longitudinal end section of the first electrode can correspond to the inner end of the first electrode. The point at which the curvature of the first electrode is greatest can correspond to the point of maximum curvature. The angle can be determined in a top view of the electrode assembly or in a cross-section of the electrode assembly perpendicular to the winding axis and can correspond to an azimuth angle, with the vertex lying on or coinciding with the winding axis.
[0034] Such an electrode arrangement with the characteristics described above may be capable of achieving any of the technical effects mentioned herein. In particular, one, some, or all of the electrodes of the electrode arrangement may be subject to contraction and / or expansion in response to charging and discharging processes, which may lead to deformation of the electrode arrangement. This deformation may cause a winding core of the electrode arrangement to lose its cylindrical shape and therefore collapse.
[0035] The electrode arrangement, as disclosed herein, may have an angle between the inner end of the first electrode and the point of maximum curvature of the first electrode in order to suppress such a problematic phenomenon as the winding core of the electrode arrangement being unable to maintain a cylindrical shape due to deformation of the electrode arrangement and therefore collapsing.
[0036] Consequently, the electrode arrangement as disclosed herein can help prevent damage to the first electrode, the second electrode, and the separator. The electrode arrangement as disclosed herein can also help prevent an internal short circuit between the first electrode and the second electrode. Therefore, the claimed subject matter can contribute to increasing the stability and overall service life of a battery.
[0037] A manufacturing process for an electrode array can implement an angle between the inner end of the first electrode and the point of maximum curvature of the first electrode in the manner described, thereby enabling a continuous manufacturing process, for example, using conventional roll-to-roll processing equipment, and thereby increasing productivity and cost-effectiveness. The process can further achieve any of the technical effects mentioned above and / or detailed below.
[0038] In one embodiment, the point of maximum curvature can be a point at which the curvature of the first electrode is at its maximum in a region in a cross-section of the electrode arrangement perpendicular to the winding axis, wherein the region extends from the inner end of the first electrode over an azimuth angle of 0° and 180° in a direction opposite to a winding direction in which the electrode arrangement is wound around the winding axis.
[0039] As stated above, the winding direction used herein can follow the winding of the first electrode (and / or the second electrode and separator), which may be a helical path around the winding axis. Thus, the winding direction of the first electrode can begin at the inner end of the first electrode and follow the winding of the first electrode to its outer circumferential end in plan view (and / or in a cross-section perpendicular to the winding axis). However, in the context of determining the azimuth angle, the winding direction can be a circular direction around the winding axis in the direction of the winding of the first electrode (i.e., a direction in the sense of a winding direction).
[0040] The azimuth angle can be determined in the cross-section of the electrode assembly perpendicular to the winding axis (or in the top view of the electrode assembly), with the vertex of the azimuth angle coinciding with the winding axis. Within the context of the aforementioned region in the cross-section of the electrode assembly, one leg of the azimuth angle can be defined by a straight line extending from the winding axis to the inner end of the first electrode (i.e., the first line). The other leg of the azimuth angle can be defined by a straight line extending from the winding axis to the boundary of the aforementioned region in the cross-section of the electrode assembly.
[0041] This region extends over (or spans or encompasses) an azimuth angle from 0° to 180°. In other words, this region encompasses the entire area between a boundary corresponding to an azimuth angle of 0° and another boundary corresponding to an azimuth angle of 180°. The boundaries meet at / in the winding axis, and another boundary is defined by the outer circumference of the electrode array. A straight line extending from the winding axis through the inner end of the first electrode—that is, the first line as described above—can correspond to an azimuth angle of 0°. The region extends opposite to the winding direction; that is, it encompasses an area opposite to an initial segment of the first electrode extending from its inner end in the winding direction.If this area extends over an azimuth angle range of 0° to 180°, it may comprise half the cross-section of the electrode array perpendicular to the winding axis (and / or half the top view of the electrode array), bounded by a straight line passing through the winding axis and the inner end of the first electrode. Accordingly, the aforementioned area may be semicircular or semi-circular in shape.
[0042] Alternatively or additionally, the point where the curvature is greatest can be a point where the curvature is greatest in a range above 0° and 180° or less in a direction opposite to the direction in which the electrode arrangement is wound, based on the longitudinal end section of the first electrode.
[0043] In one embodiment, the point of maximum curvature of the first electrode can be formed in or on a part of the electrode arrangement within 3 turns of the first electrode from its inner end.
[0044] The portion of the electrode assembly surrounded by a third turn of the first electrode from its inner end can be called the core section. The core section can correspond to the core section described above. The core section can be implemented with any, some, or all of the features described below.
[0045] Alternatively or additionally, the core section can be an electrode array that is a region within 3 turns of an end section of the first electrode in a longitudinal direction. The longitudinal direction can refer to a state of the electrode array before winding and can correspond to the winding direction after winding, as used herein. One end can refer to the inner end of the first electrode.
[0046] In one embodiment, the first electrode comprises a first electrode current collector and a first electrode active material layer provided on at least one surface of the first electrode current collector, such that the first electrode active material layer extends to an inner end of the first electrode current collector and the inner end of the first current collector corresponds to the inner end of the first electrode.
[0047] In other words, the first electrode can encompass the first current collector and the first active material layer applied to it. In the direction opposite to the winding direction, the first electrode ends (at its inner end) where the first current collector ends. That is, the first electrode may not extend further than the first current collector in the winding direction.
[0048] The active material layer can refer to a layer that contains or is formed from an electrode active material as specified above. For example, the first electrode can be a positive electrode, and the active material layer can be a layer of a positive active material.
[0049] Alternatively or additionally, the first electrode comprises a first electrode current collector and a first electrode active material layer provided on at least one surface of the first electrode current collector, wherein the first electrode current collector and the first electrode active material layer have longitudinal end sections at the same position.
[0050] In one embodiment, the first electrode can comprise a first uncoated electrode section in which the first electrode active material layer is not provided. The electrode arrangement further comprises a first electrode tab that is physically connected to or formed on the first uncoated electrode section.
[0051] The first uncoated electrode section can refer to a section of the first electrode, in particular of the first current collector, that is free of the first active material layer (i.e., free of the first active material or the active material of the first electrode).
[0052] At least one electrode tab can be formed from, on, or attached to the first uncoated electrode section. The first uncoated electrode section can be cut or notched (e.g., by forming one or more slots, notches, or cuts, or the like, from an edge of the first uncoated electrode section into the first uncoated electrode section) to form one or more first electrode tabs. Alternatively or additionally, at least one electrode tab can be provided separately and attached to the first current collector or the first uncoated electrode section.
[0053] In one embodiment, an angle formed between the line extending from the winding axis through the inner end of the first electrode (i.e., the first line, see above) and a line extending from the winding axis through a point where the curvature of the first electrode is 1 or less may be greater than 0°. A mathematical value of the curvature may be determined as described above and / or as detailed below. In particular, the point where the curvature of the first electrode is 1 or less may be located within three turns from the inner end of the first electrode, i.e., in the core section of the electrode assembly. The angle mentioned herein may refer to an azimuth angle, as described above, with the vertex of the angle lying on (i.e., coinciding with) the winding axis.
[0054] In one embodiment, the angle formed between the line extending from the winding axis through the inner end of the first electrode (i.e., the first line) and the line extending from the winding axis through the point of maximum curvature of the first electrode (i.e., the second line) can be determined after activation of the electrode arrangement.
[0055] Activation, as used herein, can refer to a process in which specific temperature(s) and charge and discharge conditions are applied to the electrode assembly (or a battery cell containing it) to prepare the electrode assembly for use in a secondary battery. Activation can also be referred to as formation. Activation may include an aging process, a charge process, and a discharge process, which may be performed in a specific sequence and, optionally, repeated in a specific sequence. The aging process may be configured to allow an electrolyte to penetrate the first and second electrodes. For example, the aging process may be performed by storing the electrode assembly at a specific temperature (e.g., 30°C) for a specific duration (e.g., 30 minutes, 1 hour, 2 hours, or 3 hours).The charging process can be configured to form a solid electrolyte interphase (SEI) layer from electrolyte decomposition on the surface of the negative electrode. The charging process can include charging the electrode array to a specific charge level. Optionally, after charging, a further aging process can be performed at an elevated temperature (e.g., 40 °C, 50 °C, 60 °C, or 70 °C). The electrode array can then be discharged at a specific C-rate (e.g., 0.1 C, 0.2 C, 0.5 C, or 1.0 C). Optionally, a degassing process can be performed to remove any gas formed during the activation processes described above.
[0056] The first electrode and / or the second electrode can contract and / or expand during activation. Therefore, the technical effect achieved by the present invention can be particularly advantageous for an electrode arrangement after it has undergone (at least part of) the activation process.
[0057] Alternatively or additionally, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can be measured after activation.
[0058] In one embodiment, the angle formed between the straight line extending from the winding axis through the inner end of the first electrode and the straight line extending from the winding axis through the point of maximum curvature is determined after 50 charging and discharging cycles under conditions of 25 °C, 1 C charge and 1 C discharge.
[0059] Thus, the angle between the first line and the second line, as described herein, can be determined after at least 50 charge and discharge cycles (repetitions) of the electrode arrangement. This allows the condition or quality of the electrode arrangement to be determined with increased accuracy.
[0060] Alternatively or additionally, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can be measured after 50 charging and discharging cycles under conditions of 25 °C, 1 C charging and 1 C discharging.
[0061] In one embodiment, the circularity of the first electrode in or on a portion of the electrode assembly within three turns of the first electrode from its inner end can be 89% or more. As mentioned above, the portion of the electrode assembly within three turns of the first electrode from its inner end can be referred to as the core section of the electrode assembly.
[0062] Alternatively or additionally, the circularity of the first electrode in the core section of the electrode arrangement can be 89% or more.
[0063] Circularity (roundness), as used herein, may refer to roundness according to the principles of mathematical geometry. In particular, circularity may be determined according to ISO 1101. Circularity, as used herein, may be determined as a two-dimensional parameter in a top view of the electrode array. Additionally or alternatively, circularity may be determined in detail as below.
[0064] In one embodiment, the first electrode can have a first surface facing the winding axis and a second surface on a side opposite the first surface. A first extension line can be formed by extending a straight line connecting two points where the direction of curvature changes within a distance of 5 mm from the inner end of the first electrode on the first surface of the first electrode. A second extension line can be formed by extending a straight line connecting two points within a distance of 5 mm from the inner end of the first electrode on a surface of the second electrode facing the first surface of the first electrode. The first and second extension lines can form an angle of 25° or less.In particular, the first extension line and the second extension line can form an angle of 25° or less within the core section, i.e., within three turns of the first electrode from the inner end.
[0065] Alternatively or additionally, the first electrode can have a first surface in one direction of the winding axis of the electrode array and a second surface opposite the first surface. A first extension line can be formed by extending a straight line connecting two points where the direction of curvature changes at a (spaced) distance of 5 mm from the longitudinal end section of the first electrode on the first surface of the first electrode. A second extension line can be formed by extending a straight line connecting two points at a (spaced) distance of 5 mm from the longitudinal end section of the first electrode on a surface of the second electrode facing the first surface of the first electrode, forming an angle of 25° or less.
[0066] In one embodiment, the first electrode has no crack or fold. In particular, the first electrode has no crack or fold in or on any part of the electrode assembly within 3 turns of the first electrode from its inner end, i.e., within the core section.
[0067] In one embodiment, the flatness fraction of the first electrode in or on a part of the electrode arrangement within 3 turns of the first electrode from its inner end, i.e. within the core section, may be greater than 3% and 13.5% or less.
[0068] The flatness used herein may be determined in accordance with the definition in the field of manufacturing and mechanical engineering. The flatness may be determined in accordance with ISO 12781-1. The flatness fraction used herein may be determined in detail as below.
[0069] The present disclosure may further provide a method for manufacturing an electrode assembly. The method may comprise: arranging a first electrode, a separator, and a second electrode one on top of the other in that order to form a stack; and winding the stack around a winding axis using a core. The core may comprise a first core section and a second core section. During winding, the separator may be held between the first core section and the second core section. The arrangement may be carried out such that an angle formed between a line extending from the winding axis through an inner end of the first electrode and a line extending from the winding axis through a point of maximum curvature of the first electrode is greater than 40° and 98° or less.
[0070] Such a method may be suitable for providing the electrode arrangement as disclosed herein. Thus, the method as disclosed herein may also be suitable for achieving the technical effects mentioned above and detailed below.
[0071] Alternatively or additionally, a method for manufacturing an electrode assembly may be provided, wherein a first electrode, a separator, and a second electrode are stacked on top of each other and wound in the electrode assembly. The method may comprise: (a) feeding the first electrode, separator, and second electrode in a roll-to-roll manner; (b) arranging the fed first electrode, separator, and second electrode in sequence to form a stack; and (c) winding the stack.
[0072] The winding can be carried out using a winding core that has a spacer part into which the separator is inserted; a first winding core part provided on one side of the spacer part in relation to the spacer part; and a second winding core part provided on the other side of the spacer part and having a cross-sectional area that is different from that of the first winding core part.
[0073] The arrangement can be carried out such that an angle formed between a longitudinal end section of the first electrode and a point where a curvature of the first electrode is greatest is greater than 40° and 98° or less about a winding axis.
[0074] The roll-to-roll method or roll-to-roll process may be used herein in accordance with the understanding in the field of manufacturing and industrial processing. In particular, the roll-to-roll method may involve carrying out one or more processes that begin with a roll of flexible material and rewinding after the process(s) to produce an output roll.
[0075] In particular, the first electrode, the separator and the second electrode can each be provided in a continuous manner, especially in a roll-to-roll manner, to be stacked on top of each other in the aforementioned order.
[0076] Here, the spacer can refer to a cavity formed in the center of the electrode arrangement after winding, particularly after removing a winding core used to hold and wind the first electrode, the second electrode and the separator together.
[0077] The cross-sectional areas of the first winding core part and the second winding core part can be determined in a top view (i.e., in a view parallel to the winding axis) and / or in a cross-section perpendicular to the winding axis.
[0078] In one embodiment, the first winding core section and the second winding core section may not be symmetrical to each other in a cross-section perpendicular to the winding axis. In particular, the first winding core section and the second winding core section may have different shapes and / or different sizes in a cross-section perpendicular to the winding axis.
[0079] In one embodiment, in a cross-section perpendicular to the winding axis, an area of the first winding core section is smaller than an area of the second winding core section. The arrangement of the first electrode, the separator, and the second electrode can be carried out such that the inner end of the first electrode is located on an outer circumferential surface of the first winding core section.
[0080] Alternatively or additionally, the cross-sectional area of the first winding core section can be smaller than the cross-sectional area of the second winding core section. The arrangement of the first electrode, the separator, and the second electrode can be carried out such that the longitudinal end section of the first electrode is located on an outer circumferential surface of the first winding core section.
[0081] Alternatively or additionally, the winding is carried out while maintaining a (tensile) tension of 3.92 N (or 400 gf) or higher.
[0082] Furthermore, the present disclosure provides an electrode arrangement that is produced by the method disclosed herein.
[0083] A secondary battery may have the electrode arrangement as disclosed herein.
[0084] In one embodiment, the secondary battery can have a battery housing, in particular a cylindrical battery housing, in which the electrode arrangement is received.
[0085] As a further example, an electrode arrangement is provided in which a first electrode, a separator and a second electrode are stacked and wound on top of each other, wherein at a core section of the electrode arrangement an angle formed between a longitudinal end section of the first electrode and a point where a curvature of the first electrode is greatest is 40° or greater and 98° or less about a winding axis.
[0086] A method for manufacturing an electrode assembly in which a first electrode, a separator, and a second electrode are stacked and wound on top of each other may comprise: (a) a feeding process of feeding the first electrode, the separator, and the second electrode in a roll-to-roll manner; (b) an arranging process of arranging the fed first electrode, the separator, and the second electrode in sequence to form a stack;and (c) a winding process of winding the stack, wherein the winding is carried out using a winding core comprising a spacer section in which the separator is inserted, a first winding core section provided on one side of the spacer section with respect to the spacer section, and a second winding core section provided on the other side of the spacer section having a cross-sectional area different from that of the first winding core section, and wherein the arrangement process is carried out such that an angle formed between a longitudinal end section of the first electrode and a point at which a curvature of the first electrode is greatest is greater than 40° and 98° or less about a winding axis, and an electrode arrangement produced by the method.
[0087] Another embodiment of the present invention provides a secondary battery with the electrode arrangement described above and a battery housing for receiving the electrode arrangement.
[0088] The electrode arrangement according to an embodiment of the present invention sets the angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest, thereby making it possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first electrode and the second electrode, thereby improving the stability and lifetime characteristics of the battery.
[0089] The method for manufacturing an electrode assembly makes it possible to produce an electrode assembly whose angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest has been set in a simpler way and is suitable for a continuous process using state-of-the-art roll-to-roll process equipment, thereby ensuring productivity and economy.
[0090] Furthermore, the secondary battery according to the present invention can address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, preventing damage to the second electrode and the separator and preventing an internal short circuit between the first electrode and the second electrode, thereby improving the stability and lifetime characteristics of the battery.
[0091] The effects of the present invention are not limited to the effects mentioned above, and effects not described here will be obvious to the person skilled in the art from the present description and the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS Fig.1 Images showing a CT image of an electrode arrangement according to Example 1 and a curvature of a first electrode extracted from the CT image; Fig. 2 images showing a CT image of an electrode arrangement according to Example 2 and a curvature of the first electrode extracted from the CT image; Fig. 3 images showing a CT image of an electrode arrangement according to comparison example 1 and a curvature of the first electrode extracted from the CT image; Fig. 4 images showing a CT image of an electrode arrangement according to comparison example 2 and a curvature of the first electrode extracted from the CT image; Fig. 5 images showing a CT image of an electrode arrangement according to comparison example 3 and a curvature of the first electrode extracted from the CT image; Fig.6 a CT image of an electrode arrangement according to comparison example 4 and an image showing the occurrence of a core crack of a first electrode; Fig. 7 a CT image of an electrode arrangement according to comparison example 5 and an image showing the occurrence of a core crack of a first electrode; Fig. 8 a graph showing a correlation between a flatness fraction of a first electrode and an angle formed between a longitudinal end section of the first electrode and a point where a curvature of the first electrode is greatest; Fig. 9 shows a correlation between an angle formed between a longitudinal end section of a first electrode and a point where the curvature of the first electrode is greatest, a flatness fraction of the first electrode and a core deformation during the manufacture of an electrode arrangement according to an embodiment of the present invention; Fig. 10 an image showing a CT image of the electrode arrangement according to Example 1 and an arrangement relationship between the curvature of the first electrode extracted from the CT image and a winding core; Fig. 11 an image showing a CT image of the electrode arrangement according to comparison example 2 and an arrangement relationship between the curvature of the first electrode extracted from the CT image and a winding core; Fig. 12 schematically assessing whether a core impact has occurred; Fig. 13 CT images showing sliding areas of longitudinal end sections of first electrodes of secondary batteries according to reference test example 1 and reference test example 2; DETAILED DESCRIPTION
[0092] If a part in the entire present description “has”, “has”, or “constitutes” a constitutive element, unless specifically described otherwise, this does not mean that another constitutive element is excluded, but rather means that another constitutive element may further be included.
[0093] Whenever an element is described as being “on” another element in the entire present description, the element may be in direct contact with another element, or there may be an element in between.
[0094] An exemplary embodiment of the present invention provides an electrode arrangement in which a first electrode, a separator and a second electrode are stacked and wound on top of each other, wherein at a core section of the electrode arrangement an angle formed between a longitudinal end section of the first electrode and a point where a curvature of the first electrode is greatest is 52° or greater and 68° or less about a winding axis.
[0095] Here, the first electrode can include a first surface in one direction of a winding axis of the electrode arrangement and a second surface opposite the first surface.
[0096] Additionally, the curvature can be calculated from a multitude of measurement points located on the first surface of the first electrode extracted from a computed tomography (CT) image, as described below.
[0097] The electrode arrangement according to an exemplary embodiment of the present invention sets the angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest, thereby making it possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first electrode and the second electrode, thereby improving the stability and lifetime characteristics of the battery.
[0098] In particular, the electrodes contained in the electrode assembly undergo repeated contraction / expansion during the charging and discharging of a battery. However, outward expansion is limited by the rigidity of the battery casing, which surrounds an outer surface of the electrode assembly. This can concentrate the stress in one direction, leading to a cavity—an empty space located at the core section. Consequently, the risk of core deformation of the electrode assembly can also increase.
[0099] Core deformation can be classified into a phenomenon where the core cavity of the electrode arrangement no longer maintains a circular shape and collapses when the internal stress reaches a certain level or more, i.e., core collapse, and a phenomenon where an end section of a first electrode located at the core section and a second electrode adjacent to it are deformed beyond a certain level, leading to damage of a separator between the first and second electrodes and bringing the first and second electrodes into direct contact with each other, i.e., core impact.
[0100] In particular, core collapse can be concentrated in an area susceptible to the internal stress of the electrode assembly. Specifically, core collapse can be concentrated in an area where the curvature of the first electrode is a certain value or less, i.e., a flat area. That is, deformation due to internal stress can begin in the core section of the electrode assembly from an area where the curvature of the first electrode is a certain value or less, and after a certain point, the core cavity no longer maintains a circular shape and can collapse completely. In an electrode assembly where core collapse has occurred, lithium ions can no longer be transferred uniformly between the first and second electrodes, so the battery lifespan can deteriorate.
[0101] Here, the curvature of the first electrode can be influenced by a step due to the thickness of an electrode, a tab, or the like, the shape of the winding core, the voltage applied to the electrode assembly during winding, and so forth. For example, the winding core may comprise a pair of core sections separated around the spacer section, into which a separator is inserted. When a certain voltage level is applied, the winding core is deformed, inevitably creating a region where the curvature of the first electrode is a certain value or less—that is, a flat region. Core collapse can occur in this region where the curvature of the first electrode is a certain value or less.
[0102] In this case, adjusting the angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can improve the phenomenon of the core cavity not maintaining a circular shape and collapsing, i.e., core collapse. This can prevent damage to the second electrode and the separator, and prevent an internal short circuit between the first and second electrodes, thereby improving the stability and lifespan characteristics of the battery.
[0103] According to an embodiment of the present invention, an angle formed at a core section of the electrode arrangement between a longitudinal end section of the first electrode and a point where the curvature of the first electrode is greatest may be greater than 40° and 98° or less about a winding axis.In particular, at the core section of the electrode arrangement, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest may be greater than 40° and 98° or less, 45° or more and 95° or less, 45° or more and 90° or less, 45° or more and 80° or less, 45° or more and 70° or less, 45° or more and 65° or less, 50° or more and 95° or less, 50° or more and 90° or less, 50° or more and 80° or less, 50° or more and 70° or less, 50° or more and 65° or less, 60° or more and 95° or less, 60° or more and 90° or less, 60° or more and 80° or less, 60° or more and 70° or less or 60° or more and 65° or less around the winding axis.
[0104] If the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest fulfills the range described above, it is possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of the electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first and second electrodes, thereby improving the stability and lifespan characteristics of the battery.
[0105] In the following, a curvature measurement target, a curvature measurement method and a curvature measurement time are described in more detail with regard to the angle formed between the longitudinal end section of the first electrode of the present invention and the point at which the curvature of the first electrode is greatest.
[0106] According to one embodiment of the present invention, the curvature for the first electrode can be measured at the core section of the electrode arrangement.
[0107] Here, the "core section" can be an area that includes a cavity located on a winding axis of the electrode arrangement and part of a stacked structure of the wound separator / second electrode / separator / first electrode.
[0108] In other words, the core section can have a cavity located on the winding axis of the electrode assembly and a region extending to an end section of the first electrode in a longitudinal direction, located on the innermost side where the winding of the electrode assembly begins—that is, a region that does not contain the first electrode. Additionally, the core section can further have a region of a predetermined length extending from an end section of the first electrode in the longitudinal direction in which the first electrode is wound.
[0109] According to one embodiment of the present invention, the core section can be a region within 3 turns of an end section of the first electrode in the longitudinal direction. In particular, the core section can be a region within 1 to 2.5 turns or within 1.5 to 2 turns of an end section of the first electrode in the longitudinal direction.
[0110] Here, 1 turn can refer to the length required to wind an electrode or separator, contained within an electrode assembly, 360° from a reference point. This length can be determined based on the outer diameter of a winding core used to wind the electrode assembly, the thicknesses of the separator and electrode, and the number of turns of the separator and electrode positioned on the inside of the reference point. For example, 1 turn of the first electrode can refer to the length required to wind the first electrode 360° from its longitudinal end section in the direction in which the electrode assembly is wound.
[0111] In other words, the core section can refer to an area extending to a point less than 3 turns from an end section of the first electrode in the longitudinal direction, an area extending to a point within 1 to 2.5 turns from an end section of the first electrode in the longitudinal direction, or an area extending to a point within 1.5 to 2.5 turns from an end section of the first electrode in the longitudinal direction.
[0112] Since the point at which the curvature of the first electrode is greatest can be determined depending on the area of the core section, if the area of the core section described above is satisfied, the point at which the curvature of the first electrode is greatest can be determined more efficiently, and the reliability of the determined point at which the curvature of the first electrode is greatest can be higher.
[0113] According to one embodiment of the present invention, the curvature can be measured at the core section of the electrode arrangement, it can be measured for the first electrode at the core section of the electrode arrangement, and it can be measured by extracting the first electrode from a CT image of the core section of the electrode arrangement.
[0114] If the curvature measurement target is the first electrode located at the core section of the electrode array, the reliability of the curvature measurement can be higher. By adjusting the position of the first electrode's longitudinal end section, the angle between this end section and the point where the first electrode's curvature is greatest can be more easily adjusted. This reduces the deformation of the end section of the first electrode located at the core section and of the adjacent second electrode, thus addressing the phenomenon of core impact damage to the separator located between the first and second electrodes.
[0115] According to an embodiment of the present invention, the curvature can be calculated from a plurality of measurement points located on the first surface of the first electrode, which was extracted from a computed tomography (CT) image. In particular, the curvature with respect to the first surface of an extracted first electrode, which is in a direction of the winding axis of the electrode assembly, can be measured after extracting the first electrode from a CT image of the electrode assembly. Specifically, the curvature can be calculated from a plurality of measurement points located at regular intervals on the first surface of the first electrode. For example, the plurality of measurement points can be located at 2° intervals on the first surface of the extracted first electrode around the winding axis.
[0116] According to one embodiment of the present invention, the number of measuring points can be 180 or more. In particular, the number of measuring points can be 180 or more and 720 or fewer. In particular, the number of measuring points can be 240 or more and 660 or fewer, 300 or more and 600 or fewer, or 360 or more and 540 or fewer.
[0117] If the above-described range of the number of measuring points is met, the point at which the curvature of the first electrode is greatest can be determined more efficiently, and the reliability of the determined point at which the curvature of the first electrode is greatest can be higher.
[0118] According to an embodiment of the present invention, the curvature can be measured at separate measuring points within the above-described range of the number of measuring points, which are located at regular intervals or are arbitrarily selected, on the core section, and the point at which the curvature is greatest can be determined.
[0119] According to one embodiment of the present invention, the curvature can be a curvature according to Formula 1 below. In particular, the curvature calculated at the measurement point can be calculated according to Formula 1 below using coordinate values, i.e., x-coordinate and y-coordinate, obtained from a plurality of measurement points located on the first surface of the first electrode extracted from the CT image. k=(x'y''−y'x'') / (x'2+y'2)3 / 2
[0120] In formula 1 above, k is a curvature of the first electrode, x is an x-coordinate of the measurement point, y is a y-coordinate of the measurement point, x' is a first derivative of x and y' is a first derivative of y, x'' is a second derivative of x and y'' is a second derivative of y.
[0121] In other words, calculating the curvature can mean measuring x- and y-coordinate values at a multitude of points at regular intervals on the surface of the first electrode, and calculating curvature values using the measured x- and y-coordinates and Formula 1. Specifically, the curvature can be calculated as a parametric expression of a plane curve, and the curvature, that is, the degree of bending, increases as the k-value increases according to Formula 1. In particular, the curvature can be calculated using the formula above by a Python program, and the x- and y-coordinate values can range from -3 to +3. It should be noted that x' and y' can represent the slope of a tangent at each coordinate, and x'' and y'' can represent the rate of change of the slope.
[0122] If necessary, a value can be used for the curvature value that is normalized using a radius of curvature of the electrode arrangement for each measuring point.
[0123] According to an embodiment of the present invention, the angle formed between the longitudinal end section of the first electrode and a point where the curvature of the first electrode is 1 or less can be greater than 0° around the winding axis at the core section of the electrode arrangement.
[0124] In particular, at the core section of the electrode arrangement, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is 1 or less can be greater than 0° and less than 50° around the winding axis.
[0125] In particular, at the core section of the electrode arrangement, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is 1 or less, can be 5° or more and less than 50°, 10° or more and 45° or less, or 15° or more and 40° or less around the winding axis.
[0126] In other words, a region where the curvature of the first electrode is 1 or less, i.e., a flat region, can be located between the point where the curvature of the first electrode is greatest and the longitudinal end section of the first electrode, and cannot overlap the longitudinal end section of the first electrode.
[0127] According to one embodiment of the present invention, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can be measured in a range above 0° and 180° or less in a direction opposite to the direction in which the electrode arrangement is wound, based on the longitudinal end section of the first electrode. That is, the point where the curvature is greatest can be a point where the curvature is greatest in a range above 0° and 180° or less in the opposite direction to the direction in which the electrode arrangement is wound, based on the longitudinal end section of the first electrode.
[0128] In other words, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can be measured in the range above 0° and 180° or less in the opposite direction to the direction W in which the electrode arrangement is wound, i.e. in a direction of rotation R of the winding core used to wind the electrode arrangement, based on the longitudinal end section of the first electrode.
[0129] In particular, the stress generated as the cycle progresses is concentrated in one direction of the core cavity due to the stiffness of the battery casing. This can lead to core deformation in a shallow area that is relatively susceptible to stress. In this case, in the area above 0° and 180° or less, opposite to the direction W in which the electrode assembly is wound (i.e., in the direction of rotation R of the winding core, based on the longitudinal end section of the first electrode), the number of turns of the first electrode to the outermost layer is relatively smaller, and the distance from the longitudinal end section of the first electrode that can slide is relatively longer compared to an area above 180° and 360° or less. This does not relieve the concentrated stress. Therefore, the risk of deformation in the direction of the core cavity can be higher at the corresponding location.
[0130] Additionally, as described below, the voltage applied to the electrode array during winding causes deformation of the winding core. Therefore, if the winding core has a spacer section, the point where the curvature of the first electrode is greatest and the flat area can occur symmetrically along this spacer section. However, the flat area located in the region above 0° and 180° or less in the direction of rotation R of the winding core is more susceptible to core deformation based on the longitudinal end section of the first electrode, and the risk of core deformation may be higher in this flat area even after acceleration cycles.
[0131] If the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest is measured in the range above 0° and 180° or less in the opposite direction to the direction in which the electrode arrangement is wound, based on the longitudinal end section of the first electrode, the point where the curvature of the first electrode is greatest can therefore be determined more efficiently, and the effect of reducing core deformation by adjusting the angle can be better.
[0132] According to one embodiment of the present invention, the angle formed between the longitudinal end section of the first electrode and the point at which the curvature of the first electrode is greatest can be measured after activation. In particular, the angle formed between the longitudinal end section of the first electrode and the point at which the curvature of the first electrode is greatest can be measured after activation in a standby state for normal use and in a normally used state, that is, before the occurrence of core deformation. For example, the angle formed between the longitudinal end section of the first electrode and the point at which the curvature of the first electrode is greatest can be measured after 50 charge and discharge cycles under conditions of 25 °C, 1 C charge, and 1 C discharge.
[0133] Here, the term "post-activation" can mean after a predetermined number of cycles for manufacturing a secondary battery and completing a product. Specifically, "post-activation" can include a storage state prior to the start of active use, encompassing multiple cycles for power supply purposes (i.e., before and after sale), and a state in which self-discharge has occurred during storage.
[0134] Activation can refer to a step in testing the stability of a battery by repeating aging and charging / discharging cycles after the assembly of an electrode array and battery casing. A "post-activation core deformation state" can be easily achieved by performing a predetermined number of cycles, for example, 50 cycles under 1°C / 1°C conditions at 25°C for a battery obtained at any point after assembly. However, the activation conditions are not limited to the above, as long as they are within the range used in the art to achieve the same purpose.
[0135] The point at which the curvature of the first electrode is greatest can be determined depending on the curvature measurement time. Therefore, if the curvature measurement time described above is met, the point at which the curvature of the first electrode is greatest can be determined more efficiently, and the reliability of the determined point at which the curvature of the first electrode is greatest can be higher.
[0136] Fig. Figure 8 is a graph showing a correlation between a flatness fraction of a first electrode and an angle formed between a longitudinal end segment of the first electrode and a point where the curvature of the first electrode is greatest. In particular, Fig. 8(a) a scatterplot matrix in which all factors extracted from CT images before and after 27 acceleration cycles (1C / 1C 50 cycles) of the same cell are quantified, and Fig.8(b) is a graph showing a correlation between a flatness fraction of the first electrode and the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest.
[0137] In particular, with reference to Fig.8. The location where core deformation occurs is determined by the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest, or by the value of the flatness fraction of the first electrode. This location of core deformation in the electrode assembly may coincide with an area where the curvature of the first electrode is 1 or less, i.e., a flat area. That is, the lower the flatness fraction, the lower the risk of core deformation occurring in the flat area where the core deformation takes place.
[0138] It should be noted that, as an additional influencing factor regarding the occurrence of core deformation, if a first electrode tab is positioned at 12 o'clock, a second electrode tab located at the outermost part is preferably arranged between 5 and 8 o'clock or between 6 and 7 o'clock, the longitudinal end section of the first electrode located on the core section is preferably arranged between 5 and 9 o'clock or between 6.5 and 8 o'clock, and the longitudinal end section of the first electrode located at the outermost part is preferably arranged between 4 and 6 o'clock or between 4.5 and 5.5 o'clock. It should be noted that an area of the core cavity is preferably 10 mm². 2 or more and 40 mm 2 or less or 27 mm 2 or more and 33 mm 2or less. If the additional influencing factors described above each meet the ranges described above, the effect of reducing core deformation may be greater. It should be noted that the unit "clock" indicates the relative position of each factor in a clockwise direction when the first electrode tab is positioned at 12 o'clock on the CT image, and can be measured in the opposite direction W to the direction in which the electrode array is wound, i.e., in the direction of rotation R of the winding core used to wind the electrode array. For example, 6 o'clock means forming an angle of 180° with the first electrode tab positioned at 12 o'clock.
[0139] According to one embodiment of the present invention, the first electrode may not have a crack or a fold on the core section of the electrode assembly. Here, the crack may refer to a crack that is visually detectable with the naked eye on the surface of the first electrode, and the fold may refer to a case in which a crease or wrinkle, visually detectable with the naked eye, has occurred on the surface of the first electrode.
[0140] When an electrode assembly containing a cracked first electrode is inserted into a battery casing, the risk of low voltage and short circuits due to foreign matter increases significantly. However, since the electrode assembly according to one embodiment of the present invention does not have a first electrode with cracks or folds in the core section, battery stability can be improved.
[0141] According to one embodiment of the present invention, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can exhibit a positive correlation with the flatness fraction of the first electrode at the core section of the electrode arrangement. In particular, with reference to Fig. 8(b) the correlation coefficient between the flatness fraction of the first electrode and the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest is approximately 0.756.
[0142] Here, the flatness percentage (%) can refer to a portion of the flat area of the first electrode that is a measurement target, and the flat area can refer to an area with a curvature equal to or less than a reference value.
[0143] This means that the flatness fraction can refer to a proportion of an area with a curvature value equal to or less than a reference curvature value in the first electrode, which is a measurement target. For example, the flatness fraction can be a percentage of the number of measurement points with a curvature of 1 or less, based on 100% of the total number of measurement points.
[0144] Since the flatness fraction of the first electrode can be determined depending on the reference curvature value, if the range of the reference curvature value described above is met, the flatness fraction of the first electrode can be determined more efficiently, and the reliability of the determined flatness fraction of the first electrode can be higher.
[0145] According to one embodiment of the present invention, the flatness fraction of the first electrode on the core section of the electrode arrangement can be greater than 3% and 13.5% or less. In particular, the flatness fraction of the first electrode on the core section of the electrode arrangement can be greater than 3% and 13.5% or less, 5% or greater and 13% or less, 5% or greater and 10% or less, 7% or greater and 10% or less, or 7.5% or greater and 10% or less.
[0146] If the above-described area of the flatness fraction of the first electrode is fulfilled, it is possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of the electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first and second electrodes, thereby improving the stability and lifespan characteristics of the battery.
[0147] According to one embodiment of the present invention, the roundness (circularity) of the first electrode at the core section of the electrode arrangement can be 89% or more. In particular, the circularity of the first electrode at the core section of the electrode arrangement can be 89% or more, or 90% or more, and can be 89% or more and 99% or less, or 90% or more and 98% or less.
[0148] Here, the circularity (%) can be a ratio of the minimum distance between the winding axis and the first electrode based on 100% of the maximum distance between the winding axis and the first electrode. Specifically, the circularity can refer to a ratio (%) of the minimum distance (Rmin) between the winding axis and the first electrode to the maximum distance (Rmax) between the winding axis and the first electrode.
[0149] If the circularity range described above is met, the shape of the electrode arrangement can be closer to a circle, and the resistance to voltage acting on the core section can be improved. Accordingly, it is possible to address the phenomenon where the core cavity does not maintain a circular shape due to deformation of the electrode arrangement caused by the contraction / expansion of an electrode during battery charging and discharging, and collapses. This prevents damage to the second electrode and the separator, and also prevents an internal short circuit between the first and second electrodes, thereby improving the battery's stability and lifespan characteristics.
[0150] However, circularity can differ from the flatness fraction, which refers to the portion of the area with a curvature equal to or less than the reference value at the first electrode, which is a measurement target. For example, there are cases where circularity meets the range described above, but the flatness fraction does not, depending on the shape of the electrode array. In this case, adjusting the flatness fraction to the range described above, in addition to circularity, can eliminate the possibility of the electrode array deviating from a circular shape at a specific location. Consequently, compared to simply adjusting circularity, controlling the shape of the electrode array may be easier, and the effect of reducing core deformation may be more pronounced.This means that the flatness percentage can be a more accurate reference for the degree to which the shape of the electrode arrangement is "close to a circular shape".
[0151] According to one embodiment of the present invention, the first electrode can comprise a first electrode current collector and a first electrode active material layer provided on at least one surface of the first electrode current collector, and the first electrode current collector and the first electrode active material layer can have longitudinal end sections at the same position. In other words, an end section of the first electrode can have a free-edged shape in the longitudinal direction.
[0152] This allows the area of an unnecessary uncoated section on the first electrode current collector to be reduced in order to ensure cost-effectiveness, and a slotting process can be carried out after the formation of an active material layer on an electrode, so that the slotting process and a roll-to-roll process, which includes a winding process, can be carried out more efficiently.
[0153] Here, the description “same position” means that the end sections are the same in the longitudinal direction and may include a housing in which the end sections are formed in substantially the same positions due to a process error that may occur in the slotting process or the like.
[0154] According to one embodiment of the present invention, the first electrode may comprise a first uncoated electrode section which is not provided with a first electrode active material layer, and may further comprise a first electrode tab which is provided on the first uncoated electrode section.
[0155] In other words, the first electrode current collector can comprise a first electrode-coated section in which the first electrode active material is coated, and a first uncoated electrode section in which the first electrode active material is not coated, and can include a tab on the first uncoated electrode section. Specifically, the first electrode current collector can comprise a first uncoated electrode section and a first electrode tab provided on the first uncoated electrode section.
[0156] That is, an end section of the first electrode in the longitudinal direction can have a free-edge shape, the first uncoated electrode section can be located between both longitudinal end sections of the first electrode, and the first electrode tab provided on the first uncoated electrode section can be a middle tab.
[0157] According to one embodiment of the present invention, the first electrode current collector is not particularly limited as long as it exhibits conductivity without inducing a chemical change in the battery. In particular, stainless steel, aluminum, nickel, titanium, burnt carbon, aluminum, or stainless steel, each surface-treated with carbon, nickel, titanium, silver, or the like, or the like, can be used for the first electrode current collector. That is to say, the first electrode current collector can be provided in the form of surface-treated stainless steel, aluminum foil, or the like.
[0158] Additionally, the first electrode current collector typically has a thickness of 3 to 50 µm, and its surface can be formed with microscopic irregularities to improve the adhesion of the first electrode active material. For example, the first electrode current collector can be used in various forms, such as a film, a sheet, a foil, a mesh, a porous body, a foamed body, and a nonwoven body.
[0159] According to one embodiment of the present invention, the first electrode active material can be a first electrode active material that is typically used. In particular, the first electrode active material can be a layered compound such as a lithium cobalt oxide (LiCoO2) and a lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; a lithium manganese oxide such as the chemical formula Li1+xMn2-xO4 (0≤x≤0.33), LiMnO3, LiMn2O3 and LiMnO2; a lithium copper oxide (Li2CuO2); a vanadium oxide such as LiV3O8, V2O5 and Cu2V2O7; a lithium nickel oxide of the Ni-site type, represented by the chemical formula LiNi1-yMyO2 (where M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B and Ga, and satisfies 0.01≤y≤0.3);A lithium manganese compound oxide represented by the chemical formula LiMn₂-zMzO₂ (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01 ≤ z ≤ 0.1) or Li₂Mn₃MO₈ (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); LiMn₂O₄, in which a portion of the Li of the chemical formula is substituted with an alkaline earth metal ion, or the like, but is not limited thereto. The first electrode may be Li metal.
[0160] According to one embodiment of the present invention, the first electrode active material layer can further comprise a first electrode conductivity material and a first electrode binder. The first electrode conductivity material is used to impart conductivity to the electrode and can be used without particular restriction as long as it does not cause any chemical change and exhibits electronic conductivity in a battery to be configured.Specific examples of the first electrode conductivity material may include graphite, such as natural or synthetic graphite; a carbon-based material, such as carbon black, acetylene carbon black, ketjen carbon black, sewer carbon black, furnace carbon black, lamp carbon black, thermal carbon black, and carbon fiber; metal powders or metal fibers, such as copper, nickel, aluminum, and silver; a conductive whisker, such as zinc oxide and potassium titanate; a conductive metal oxide, such as titanium oxide; or a conductive polymer, such as a polyphenylene derivative, and the like, and any one of these or a mixture of two or more of them may be used.
[0161] Additionally, the first electrode binder serves to improve the adhesion between particles of the first electrode active material and the adhesion between the first electrode active material and the first electrode current collector. Specific examples may include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and any one of these or a mixture of two or more thereof may be used.
[0162] According to one embodiment of the present invention, the second electrode can comprise a second electrode current collector and a second electrode active material layer provided on the second electrode current collector. In particular, the second electrode can comprise a second electrode current collector and a second electrode active material layer formed on one or both surfaces of the second electrode current collector and comprising a second electrode active material. In other words, the second electrode active material layer can be formed on a second electrode-coated section of the second electrode current collector, and a surface not provided with the second electrode active material layer can be expressed as a second uncoated electrode section.
[0163] According to one embodiment of the present invention, the second electrode current collector can comprise a second electrode-coated section in which the second electrode active material layer is formed, and a second uncoated electrode section in which the second electrode active material layer is not formed, and can include a tab on the second uncoated electrode section. In particular, the second electrode current collector can comprise a second uncoated electrode section and a second electrode tab formed on the second uncoated electrode section. Accordingly, the manufactured electrode arrangement can include one or more second electrode tabs.
[0164] According to one embodiment of the present invention, the second electrode active material layer can comprise a second electrode active material, comprising one or more selected from the group consisting of silicon-based materials and carbon-based materials. Additionally, the second electrode active material layer can further comprise a second electrode conductivity material and a second electrode binder, and materials known to those skilled in the art can be used without limitation for the second electrode active material, the second electrode conductivity material, and the second electrode binder.
[0165] According to one embodiment of the present invention, the second electrode current collector is not particularly limited as long as it exhibits conductivity without inducing a chemical change in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, burnt carbon, aluminum, or stainless steel, each surface-treated with carbon, nickel, titanium, silver, or the like, or similar materials, can be used for the second electrode current collector. In particular, transition metals that readily adsorb carbon, such as copper and nickel, can be used for the second electrode current collector. The thickness of the second electrode current collector can be 5 µm or more and 30 µm or less. However, the thickness of the second electrode current collector is not limited to these values.
[0166] According to one embodiment of the present invention, the second electrode binder may comprise at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid and the materials described above in which a hydrogen is substituted by Li, Na, Ca, etc., and may also comprise various copolymers thereof.
[0167] According to one embodiment of the present invention, the second electrode conductivity material is not particularly limited as long as it exhibits conductivity without inducing a chemical change in the battery, and, for example, graphite, such as natural graphite or synthetic graphite; carbon black, such as acetylene carbon black, ketjen carbon black, sewer carbon black, furnace carbon black, lamp carbon black, and thermal carbon black; a conductive fiber, such as a carbon fiber and a metal fiber; a conductive tube, such as a carbon nanotube; metal powders, such as fluorocarbon, aluminum, and nickel powders; a conductive whisker, such as zinc oxide and potassium titanate; a conductive metal oxide, such as titanium oxide; a conductive material, such as a polyphenylene derivative, and the like may be used.
[0168] According to one embodiment of the present invention, the electrode arrangement can comprise a plurality of separators. For example, the electrode arrangement can have a structure in which a separator / a second electrode / a separator / a first electrode are stacked sequentially. The separator serves to separate the first electrode and the second electrode and to provide a migration path for lithium ions. Any separator can be used without particular restriction, as long as it is commonly used as a separator in a secondary battery. In particular, a separator with a high moisture retention capacity for an electrolyte and low resistance to electrolyte migration is preferably used.In particular, a porous polymer film, for example, a porous polymer film made from a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a stacked structure with two or more layers thereof, can be used. Additionally, an ordinary porous nonwoven fabric, for example, a nonwoven fabric made from high-melting-point glass fibers, polyethylene terephthalate fibers, or the like, can be used. Furthermore, a separator can be used in which the separator material described above is used as a base layer, and a slurry containing a ceramic component or a polymer material to ensure heat resistance or mechanical strength is applied to the base layer.The separator, with a single-layer or multi-layer structure, can be used selectively. The separator thickness can range from 5 µm or more to 20 µm or less. However, the thickness of the separator is not limited to these values.
[0169] According to one embodiment of the present invention, the angle formed between the first electrode and the second electrode can be 25° or less.In particular, the first electrode may include a first surface in one direction of the winding axis of the electrode arrangement and a second surface opposite the first surface, and a first extension line formed by extending a straight line connecting two points where a direction of curvature changes at a spaced distance of 5 mm from the longitudinal end section of the first electrode on the first surface of the first electrode, and a second extension line formed by extending a straight line connecting two points at a spaced distance of 5 mm from the longitudinal end section of the first electrode on a surface of the second electrode facing the first surface of the first electrode, forming an angle of 25° or less.In this case, the angle formed by the first electrode and the second electrode can be measured, for example after an additional 200 charging and discharging cycles at 40 °C or higher after activation.
[0170] If the angular range described above is maintained, the end section of the first electrode, located at the core section, and the adjacent second electrode will not be deformed beyond a certain degree. This prevents damage to the separator between the first and second electrodes and avoids direct contact between them (core impact). Consequently, damage to the second electrode and the separator, as well as an internal short circuit between the first and second electrodes, can be prevented, thus improving the battery's stability and lifespan.
[0171] According to one embodiment of the present invention, the first electrode and the second electrode can be a positive electrode and a negative electrode, respectively. In particular, the first electrode can be a positive electrode and the second electrode can be a negative electrode.
[0172] A method for producing an electrode assembly in which a first electrode, a separator, and a second electrode are stacked and wound one on top of the other may comprise: (a) a feeding process for feeding the first electrode, the separator, and the second electrode in a roll-to-roll manner; (b) an arranging process for arranging the fed first electrode, the separator, and the second electrode in sequence to form a stack; and (c) a winding process for winding the stack.
[0173] wherein the winding is carried out using a winding core having a spacer section into which the separator is inserted, a first winding core section provided on one side of the spacer section with respect to the spacer section, and a second winding core section provided on the other side of the spacer section having a cross-sectional area different from that of the first winding core section, and wherein the arrangement process is carried out such that an angle formed between a longitudinal end section of the first electrode and a point where a curvature of the first electrode is greatest is greater than 40° and 98° or less about a winding axis; and an electrode arrangement produced by the method.
[0174] The method for manufacturing an electrode assembly makes it possible to produce an electrode assembly whose angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest has been set in a simpler way and is suitable for a continuous process using state-of-the-art roll-to-roll process equipment, thereby ensuring productivity and economy.
[0175] Furthermore, according to an embodiment of the present invention, the secondary battery can address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, preventing damage to the second electrode and the separator and preventing an internal short circuit between the first electrode and the second electrode, thereby improving the stability and lifetime characteristics of the battery.
[0176] Here, the core section, the longitudinal end section of the first electrode and the curvature, in particular a curvature measurement target, a curvature measurement method and a curvature measurement time, can be the same as those described above for the electrode arrangement.
[0177] According to one embodiment of the present invention, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can be greater than 40° and 98° or less, 45° or more and 95° or less, 45° or more and 90° or less, 45° or more and 80° or less, 45° or more and 70° or less, 45° or more and 65° or less, 50° or more and 95° or less, 50° or more and 90° or less, 50° or more and 80° or less, 50° or more and 70° or less, 50° or more and 65° or less, 60° or more and 95° or less, 60° or more and 90° or less, 60° or more and 80° or less, 60° or more and 70° or less or 60° or more and 65° or less around the winding axis.
[0178] If the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest fulfills the range described above, it is possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of the electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first and second electrodes, thereby improving the stability and lifespan characteristics of the battery.
[0179] The method for manufacturing an electrode assembly can be carried out in a roll-to-roll manner. In particular, steps (a) to (c) can be carried out in a roll-to-roll manner, processing a plurality of flexible metal foils and the like as they move between rolls. Here, the roll-to-roll manner can refer to feeding an electrode current collector by unwinding a roll on which a flexible, thin, sheet-like electrode current collector is wound, forming an electrode mixture layer by applying an electrode slurry comprising an electrode active material to at least one surface of the electrode current collector, drying the electrode slurry, and then rewinding and collecting an electrode current collector processed from another roll.
[0180] The method for manufacturing an electrode assembly enables the production of an electrode assembly whose angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest has been set, in a continuous process using roll-to-roll process equipment used in the industry.
[0181] This means that the method for manufacturing an electrode assembly enables an electrode assembly, whose angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest has been set, to be manufactured in a continuous process using state-of-the-art roll-to-roll process equipment, thereby ensuring productivity and economy.
[0182] Fig.Figure 9 shows a correlation between an angle formed between a longitudinal end section of a first electrode and a point where the curvature of the first electrode is greatest, a flatness fraction of the first electrode and a core deformation during the manufacture of an electrode arrangement according to an embodiment of the present invention.
[0183] In particular, it shows Fig. 9(a) schematically a method for producing an electrode arrangement, and the Fig. 9(b) to Fig. Figure 9(d) shows a winding core according to an embodiment of the present invention, a CT image of the electrode arrangement, and a curvature of the first electrode extracted from the CT image. In particular, it shows Fig. 9(b) a flat area of the electrode arrangement, Fig. Figure 9(c) shows a point where the curvature of the electrode arrangement is greatest, and Fig.Figure 9(d) shows a CT image of the electrode arrangement in relation to the winding core according to an embodiment of the present invention. It should be noted that Fig. 9(e) is an image of core deformation occurring in the flat region of the electrode arrangement according to the Fig. 9(b) to Fig. 9(d) after cycles.
[0184] According to an embodiment of the present invention, the winding can be carried out using a winding core which has a spacer part into which the separator is inserted, a first winding core part which is provided on one side of the spacer part in relation to the spacer part, and a second winding core part which is provided on the other side of the spacer part and has a cross-sectional area which is different from that of the first winding core part.
[0185] In particular, the winding core can have a spacer section S into which the separator is inserted, a first winding core section A provided on one side with respect to the spacer section S, and a second winding core section B provided on the other side having a cross-sectional area different from that of the first winding core section A. Because the winding core has the spacer section, a stack, such as a separator inserted into the spacer section, can be wound by rotating the winding core in a direction opposite to a direction of rotation R of the winding core.
[0186] If the winding core has a first winding core section and a second winding core section with the same cross-sectional area as the first, deformation of the winding core due to tension during winding can occur, and the circularity of a core section of the manufactured electrode assembly can decrease. That is, the core section is deformed into an oval shape due to tension during winding, which can be detrimental in terms of processability, outer diameter, and circularity.
[0187] On the other hand, if the winding core has a first winding core section and a second winding core section with a different cross-sectional area than that of the first winding core section, the deformation and asymmetry of the winding core due to stress during winding are minimized, and the average circularity of the core section is increased, thereby minimizing the occurrence of core collapse.
[0188] Since the winding core has, in particular, a first winding core section and a second winding core section with a different cross-sectional area than that of the first winding core section, deformation can occur in a relatively small winding core section when a high voltage is applied to the winding core. Accordingly, with the spacer section as its center point, the point where the curvature of the first electrode is greatest may be located adjacent to a relatively large winding core section, and the flat area of the first electrode may be located adjacent to a relatively small winding core section.
[0189] Additionally, in the region above 0° and 180° or less, in the opposite direction to the direction W in which the electrode arrangement is wound (i.e., in the direction of rotation R of the winding core, based on the longitudinal end section of the first electrode), the number of turns of the first electrode to the outermost layer is relatively smaller, and the distance from the longitudinal end section of the first electrode that can slide is relatively longer compared to a region above 180° and 360° or less. This does not relieve the concentrated stress. Therefore, the risk of deformation towards the core cavity may be higher at the corresponding location.
[0190] This means that the winding core can comprise a pair of winding core parts separated around the spacer part into which a separator is inserted, and when a certain voltage level is applied, the winding core is deformed, inevitably creating an area where the curvature of the first electrode is a certain value or less, i.e., a flat area, and core collapse can occur in the area where the curvature of the first electrode is a certain value or less.
[0191] In this case, in the range above 0° and 180° or less, in the opposite direction to the direction W in which the electrode arrangement is wound, i.e., in the direction of rotation R of the winding core, based on the longitudinal end section of the first electrode, the phenomenon of core collapse can be addressed by adjusting the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest.
[0192] According to an exemplary embodiment of the present invention, the cross-sectional area of the first winding core part can be smaller than the cross-sectional area of the second winding core part, and the arrangement process can be carried out such that the longitudinal end section of the first electrode is arranged on an outer circumferential surface of the first winding core part.
[0193] In particular, with reference to Fig. 9(a) to Fig.9(d) The arrangement process is carried out such that the position of the longitudinal end section of the first electrode is set according to an input length of the separator, an input timing control of the first electrode, and the like, and the longitudinal end section of the first electrode is arranged on an outer circumferential surface of the first winding core section. Even if the diameter of the winding core is different, the position of the longitudinal end section of the first electrode can be set by adjusting an input length of the separator, an input timing control of the first electrode, and the like.
[0194] According to an exemplary embodiment of the present invention, the arrangement process can be carried out such that the longitudinal end section of the first electrode is positioned at a location that is 40% or more and 60% or less away from the spacer section, based on 100% of the length of the outer circumferential surface of the first core section. In particular, the arrangement process can be carried out such that the longitudinal end section of the first electrode is positioned at a location that is 40% to 50% or 50% to 60%, for example 50%, away from the spacer section, based on 100% of the length of the outer circumferential surface of the first core section. In other words, the longitudinal end section of the first electrode can be positioned at a 1 / 2-point on the outer circumferential surface of the first core section, which is the point furthest from the spacer section of the core on the outer circumferential surface of the first core section.
[0195] If the arrangement process is carried out such that the longitudinal end section of the first electrode is positioned on the outer circumferential surface of the first winding core section, the angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest can be adjusted within a specific range. Furthermore, the manufactured electrode arrangement can address the phenomenon of the core cavity not maintaining a circular shape due to deformation of the electrode arrangement caused by contraction / expansion during battery charging and discharging, thus preventing damage to the second electrode and the separator, and preventing an internal short circuit between the first and second electrodes, thereby improving the stability and lifespan characteristics of the battery.
[0196] According to one embodiment of the present invention, the winding process can be carried out while maintaining a tensile stress of 400 gf or higher. In particular, the tensile stress can be 400 gf or higher and 500 gf or less. Specifically, the tensile stress can be 410 gf or higher, 420 gf or higher, 430 gf or higher, 440 gf or higher, or 450 gf or higher, and can be 590 gf or less, 580 gf or less, 570 gf or less, 560 gf or less, or 550 gf or less.
[0197] If the (tensile) stress fulfills the range described above, due to the high (tensile) stress in the winding process with the spacer section as the center point, the point where the curvature of the first electrode is greatest may be located at a position adjacent to a relatively large winding core, the flat area of the first electrode may be located at a position adjacent to a relatively small winding core, and the positions of the point where the curvature of the first electrode is greatest and the flat area of the first electrode may be constant.
[0198] An exemplary embodiment of the present invention provides an electrode arrangement which is produced by the above-described method for producing an electrode arrangement.
[0199] The electrode arrangement according to an exemplary embodiment of the present invention sets the angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest, thereby making it possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first electrode and the second electrode, thereby improving the stability and lifetime characteristics of the battery.
[0200] An exemplary embodiment of the present invention provides a secondary battery with the electrode arrangement described above and a battery housing for receiving the electrode arrangement. In particular, the secondary battery can have the electrode arrangement according to an exemplary embodiment described above and a battery housing for receiving the electrode arrangement.
[0201] The secondary battery according to the present invention can address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery and collapses, preventing damage to the second electrode and the separator and preventing an internal short circuit between the first electrode and the second electrode, thereby improving the stability and lifetime characteristics of the battery.
[0202] According to an exemplary embodiment of the present invention, the battery housing can have a cylindrical shape. In particular, the battery housing can have a cylindrical shape, a square shape, a pouch shape, or the like, depending on the intended use, but is not limited to such shapes.
[0203] According to an exemplary embodiment of the present invention, the battery casing can contain an electrolyte. In particular, the electrolyte can be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten-type inorganic electrolyte, which can be used in the manufacture of the lithium secondary battery, but is not limited to these. In particular, the electrolyte can contain a non-aqueous organic solvent and a metal salt.
[0204] According to an exemplary embodiment of the present invention, the non-aqueous organic solvent can be, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyllactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivative, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivative, tetrahydrofuran derivative, ether, methyl propionate or ethyl propionate.
[0205] According to an exemplary embodiment of the present invention, a lithium salt can be used as the metal salt, and the lithium salt is a material that is readily soluble in the non-aqueous electrolyte solution, in which, for example, one or more species selected from the group consisting of F-, Cl-, I-, NO3-, N(CN)2-, BF4-, ClO4-, PF6-, (CF3)2PF4-, (CF3)3PF3-, (CF3)4PF2-, (CF3)5PF-, (CF3)6P-, CF3SO3-, CF3CF2SO3-, (CF3SO2)2N-, (FSO2)2N-, CF3CF2(CF3)2CO-, (CF3SO2)2CH-, (SF5)3C-, (CF3SO2)3C-, CF3(CF2)7SO3-, CF3CO2-, CH3CO2-, SCN- and (CF3CF2SO2)2N- consists of an anion of the lithium salt that can be used.
[0206] According to an exemplary embodiment of the present invention, one or more additives, for example a compound based on halogenated alkylene carbonates, such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, triamide hexaphosphoric acid, a nitrobenzene derivative, sulfur, a quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, an ammonium salt, pyrrole, 2-methoxyethanol or aluminum trichloride, may further be included in the electrolyte for the purpose of improving the battery's lifetime characteristics, suppressing a decrease in battery capacity, improving the battery's discharge capacity and the like, in addition to the electrolyte components described above.
[0207] An exemplary embodiment of the present invention provides a battery module with the secondary battery as a single cell and a battery pack comprising the battery module. Since the battery module and the battery pack include the secondary battery with high capacity, high battery stability and long service life characteristics, the battery module and the battery pack can be used as a power source for a medium-sized and large-sized device selected from the group consisting of an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle and an energy storage system.
[0208] Examples are described in detail below to specifically describe the present invention. However, the examples according to the present invention can be modified in other ways, and the scope of the present invention is not intended to be limited to the following examples. The examples in this description are provided to explain the present invention more fully to those skilled in the art. EXAMPLES Example 1 Creating an electrode arrangement
[0209] A first electrode active material slurry was prepared by adding Li(Ni0.89Co0.07Mn0.04)O2 as a first electrode active material, CNT as a first electrode conductivity material, and polyvinylidene fluoride (PVdF) as a first electrode binder to N-methyl-2-pyrrolidone (NMP) in a weight ratio of 97.92:0.5:1.58. The first electrode active material slurry was applied in a width direction to an aluminum current collector with a thickness of 15 µm and a length of 63.9 mm, followed by drying and rolling to form a first electrode active material layer, thus producing a first electrode with a thickness of 135 µm.
[0210] Next, a second electrode active material composition was prepared by mixing natural graphite (C, average particle diameter: 17 µm) as the second electrode active material, carbon black as the second electrode conductivity material, and styrene-butadiene rubber (SBR) as the second electrode binder in a weight ratio of 97.7:1.3:1.0. Then, 7.8 g of distilled water were added to 5 g of the second electrode active material composition, followed by stirring, to produce a second electrode active material slurry. The second electrode active material slurry was applied to a copper (Cu) metal thin film as a second electrode current collector with a thickness of 8 µm and a length of 65.2 mm in one width direction, followed by drying (drying temperature 120 °C, 1 minute) to form a second electrode with a thickness of 166 µm.In this case, the temperature of the circulating air was 60 °C.
[0211] Two separators were then arranged sequentially and wound using a 3.2 mm diameter core. The second electrode was then inserted between the two separators, which were subsequently wound. In this case, the core used had a spacer into which a separator was inserted, a first core section, and a second core section with a cross-sectional area different from that of the first. The cross-sectional areas of the first and second core sections were 15 mm². 2 or 10 mm 2 .
[0212] After the separators and the second electrode were wound around three turns, the first electrode was inserted and wound, and a PET sealing strip was applied and finished to wrap the upper and lower outer circumferential surfaces of the electrode assembly at the end section where the winding was completed.
[0213] In this case, based on the first core section being located in a 6 o'clock direction and the second core section being located in a 12 o'clock direction of the electrode array, the positions of the longitudinal end sections located on the core section and the outermost section of the first electrode, and the position of the tab, were set as shown in Table 1 below. Here, FE (free edge) means that the electrode current collector and the electrode active material layer have longitudinal end sections in the same position, and the unit "o'clock" means that if the first electrode tab is at 12 o'clock on the CT image, the relative position of each factor is shown clockwise.
[0214] The area and circularity of the core cavity, measured from computed tomography (CT) images, are as shown in Table 1 below, and after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted on the core section of the electrode assembly to form 60.8° around the winding axis.In this case, with respect to the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest, the curvatures measured at each measurement point on the CT image were compared. The measurement point where the curvature has the greatest value in the range above 0° and 180° or less in the opposite direction to the direction in which the electrode assembly is wound, based on the longitudinal end section of the first electrode, was determined to be the point (Curvature Max.) where the curvature of the first electrode is greatest. The angle formed between the point where the curvature of the first electrode is greatest and the longitudinal end section of the first electrode was measured around the winding axis and is shown in Table 2 below. In the following examples, comparison examples, and experimental examples, the point (Curvature Max.)), where the curvature of the first electrode is greatest, measured using the same method. [Table 1] Influencing factor Adjustment range FE position at the core section of the first electrode (clock) 6,5-8 FE position at the outermost section of the first electrode (clock) 4,5-5,5 Tab position at the outermost second electrode (clock) 6-7 Area of the core cavity (mm²) 2 ) 27-33 Circularity (%) 89-92 Manufacturing a secondary battery
[0215] A secondary battery was manufactured by inserting the electrode assembly into a cylindrical battery casing, injecting an electrolyte solution in which ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a volume ratio of 20:5:75 and LiPF6 was dissolved in it in an amount of 1.4 M, and closing the cylindrical battery casing with a cap assembly. Example 2
[0216] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted to be 65° around the winding axis at the core section of the electrode assembly. Comparative example 1
[0217] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted to be 98.9° about the winding axis at the core section of the electrode assembly. Comparative example 2
[0218] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted to be 112.4° about the winding axis at the core section of the electrode assembly. Comparative example 3
[0219] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted to be 129.3° about the winding axis at the core section of the electrode assembly. Comparative example 4
[0220] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25°C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted to be 40° around the winding axis at the core section of the electrode assembly. Comparative example 5
[0221] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was adjusted to be 20° around the winding axis at the core section of the electrode assembly. Experimental Examples: Experimental Example 1: Evaluation of the Flatness Percentage
[0222] The flatness percentages of the secondary batteries from Example 1 and comparison examples 1 to 3 were evaluated using the following procedure, and the results are shown in Table 2 below. Fig. 1 to Fig. 4 shown.
[0223] 1) The first electrode is extracted from the CT image of the electrode arrangement.
[0224] 2) On the first surface of the first electrode, measuring points are set at 2° intervals from an end section of the first electrode in the longitudinal direction, and the x-coordinates and y-coordinates of the measuring points are measured.
[0225] 3) The curvature (k) for each measurement point is calculated according to the following formula 1 using the x-coordinate and y-coordinate of the measurement point. k=(x'y''−y'x'') / (x'2+y'2)3 / 2
[0226] In formula 1 above, k is a curvature of the first electrode, x is an x-coordinate of the measurement point, y is a y-coordinate of the measurement point, x' is a first derivative of x and y' is a first derivative of y, x'' is a second derivative of x and y'' is a second derivative of y.
[0227] 4) If the curvature value calculated at each measurement point is 1 or less, the corresponding measurement point is assessed as a flat area, and a ratio of the number of measurement points assessed as a flat area, based on 100% of the total number of measurement points, was assessed as the flatness percentage (%). Experimental Example 2: Assessment of Core Collapse
[0228] The occurrence or absence of core collapse in the secondary batteries of Examples 1 and 2 and Comparison Examples 1 to 5 was evaluated using the following procedure, and the occurrence or absence of core impact was re-evaluated every 200 cycles. The results are shown in Table 2 below. Fig. 1 to Fig. 7 each.
[0229] 1) The first electrode is extracted from the CT image of the electrode arrangement.
[0230] 2-1) An area of the core cavity surrounded by the first electrode is measured from an end section of the first electrode in the longitudinal direction to a point corresponding to one turn in the longitudinal direction of the first electrode.
[0231] 2-2) If the area of the core cavity is less than 100%, based on 100% of the sum of the cross-sectional areas of the spacer, first winding core section and second winding core section of the winding core used to wind the electrode assembly, core collapse is assessed as having occurred.
[0232] 3-1) On the first surface of the first electrode, an extension line of the straight line corresponding to the minimum value (Dmin) and the maximum value (Dmax) of the diameter of the core cavity of the extracted first electrode is drawn, and a concentric circle is drawn using the intersection point of each straight line as the central axis, i.e. the winding axis.
[0233] 3-2) The maximum spaced distance (Rmax) between the winding axis and the first electrode and the minimum spaced distance (Rmin) between the winding axis and the first electrode from an end section of the first electrode in the longitudinal direction to a point corresponding to one turn in the longitudinal direction of the first electrode are each measured.
[0234] 3-3) A ratio (%) of the minimum spaced distance (Rmin) between the winding axis and the first electrode to the maximum spaced distance (Rmax) between the winding axis and the first electrode, i.e., the core cavity circularity, is calculated. If the calculated core cavity circularity was less than 89%, core collapse was considered to have occurred.
[0235] On the other hand, in the case where an unknown secondary battery (unknown cell) is acquired, the above method for evaluating whether core collapse has occurred can be applied by evaluating whether core collapse occurred at the time of initial detection, re-evaluating whether core collapse has occurred every 200 cycles, and comparing and analyzing the result with the core collapse conditions of the secondary battery of the exemplary embodiment according to the present invention. Experimental Example 3: Evaluation of the core impact
[0236] The occurrence or absence of core impact in the secondary batteries of Examples 1 and 2 and Comparison Examples 1 to 5 was assessed by the following procedure, and the occurrence or absence of core impact was reassessed every 200 cycles, and the results are shown in Table 2 below. Fig. 1 to Fig. 7 shown.
[0237] Fig. Figure 12 schematically shows a procedure for assessing whether core impact has occurred. In particular, it shows Fig. 12(a) schematically a method for assessing whether core impact has occurred when deformation has occurred in the second electrode, and Fig. Figure 12(b) schematically shows a method for evaluating whether core impact has occurred if no deformation has occurred in the second electrode.
[0238] 1) On a first surface of a first electrode 300, a first extension line E1 is formed by extending a straight line connecting a longitudinal end section 310 of the first electrode and a point that is 5 mm away from the end section. 2-1) If the second electrode is deformed,
[0239] At the core section of the electrode arrangement, a second extension line E2 is formed on a surface of a second electrode 100 facing the first surface of the first electrode by extending a straight line connecting two points where a direction of curvature changes within a distance of 5 mm from the longitudinal end section 310 of the first electrode. 2-2) If no deformation occurs in the second electrode,
[0240] At the core section of the electrode arrangement, a second extension line E2 is formed on the surface of the second electrode 100, which faces the first surface of the first electrode, by extending a straight line connecting two points that are 5 mm apart from the longitudinal end section 310 of the first electrode.
[0241] 3) If an angle from the first extension line E1 to the second extension line E2 in a counterclockwise direction with respect to the intersection of the first extension line E1 and the second extension line E2 exceeded 25°, it was assessed that the core impact had occurred.
[0242] On the other hand, in the case where an unknown secondary battery (unknown cell) is acquired, the above method for evaluating whether core impact has occurred can be applied by evaluating whether core impact occurred at the time of initial detection, re-evaluating whether core impact has occurred every 200 cycles, and comparing and analyzing the result with the core collapse conditions of the secondary battery of the exemplary embodiment according to the present invention. Experimental Example 4: Evaluation of the occurrence of a core crack
[0243] The occurrence or non-occurrence of a core crack was evaluated for the electrode arrangements from Example 1, Example 2 and Comparative Examples 1 to 5 using the following procedure, and the results are shown in Table 2 and Figure 5 below. Fig. 6 and Fig. 7 shown.
[0244] In particular, the electrode assemblies from Examples 1 and 2 and Comparative Examples 1 to 5 were fabricated, and the fabricated electrode assemblies were disassembled to visually inspect the core section for cracks or wrinkles. If cracks or wrinkles were found in the core section, the core crack was considered to have occurred. [Table 2] First electrode FE curvature Max. angle (°) Flatness percentage (%) Results of the core collapse assessment Results of the core impact assessment Results of the assessment of the occurrence of a core crack Example 1 60,8 7,72 0 / 2 0 / 2 0 / 2 Example 2 65 9,6 0 / 2 0 / 2 0 / 2 Comparative example 1 98,9 13,9 2 / 2 0 / 2 0 / 2 Comparative example 2 112.4 17.0 2 / 2 1 / 2 0 / 2 Comparative example 3 129.3 16.49 2 / 2 1 / 2 0 / 2 Comparative example 4 40 3,0 1 / 2 1 / 2 1 / 2 Comparative example 5 20 1,0 1 / 2 1 / 2 1 / 2
[0245] Fig. 6. A CT image of an electrode arrangement according to comparative example 4 and an image showing the occurrence of a core crack in a first electrode; and Fig. 7 a CT image of an electrode arrangement according to comparison example 5 and an image showing the occurrence of a core crack of a first electrode;
[0246] In particular, the Fig. 6(a) and Fig. 7(a) CT images of the electrode arrangements according to Comparative Example 4 and Comparative Example 5, and the Fig. 6(b) and Fig. Figure 7(b) shows exploded views of cracks that occurred in the first electrodes at the core sections of the electrode arrangement according to Comparative Example 4 and the electrode arrangement according to Comparative Example 5. Here, the red circles represent the area of core impact corresponding to the longitudinal end section of the first electrode and the area of crack formation of the first electrode at the core section, respectively.
[0247] Referring to Table 2 and the Fig. 6(b) and Fig.7(b) In the case of the electrode arrangements according to comparative examples 4 and 5, it can be seen that on the core section of the electrode arrangement the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was 40° or less around the winding axis, thereby concentrating the stress produced by the deformation of the winding core on the longitudinal end section of the first electrode, causing wrinkles or cracks in the core section.
[0248] If cracks and resulting foreign matter occur in the first electrode at the core section of the electrode assembly during the winding process, the defect rate can increase and the processability can deteriorate. Accordingly, by eliminating the input of the first electrode, where cracks are expected to occur during the manufacturing process, it is possible to prevent a decrease in the productivity of the electrode assembly and the secondary battery.
[0249] In particular, when a cracked electrode assembly is inserted into the battery casing, the risk of low voltage and short circuits due to foreign matter in the first electrode within the battery casing increases significantly. Accordingly, the risk of cracking in the first electrode can be reduced by adjusting the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest during the winding process. That is to say, it is evident that the electrode assembly and its manufacture according to an embodiment of the present invention are suitable for a continuous process using prior art roll-to-roll processing equipment, thereby ensuring the productivity and cost-effectiveness of the electrode assembly, including the first electrode and the secondary battery. Reference test example: Evaluation of the electrode sliding range Reference test example 1
[0250] The secondary battery of Example 1 was prepared and charged and discharged 50 times under conditions of 25 °C, 1 C charge and 1 C discharge.
[0251] During 200 cycles from SOC of 0% to SOC of 100% under conditions of 4.25 V–2.5 V 1°C / 1°C at 25°C, the position of the longitudinal end segment of the first electrode at SOC of 0% and SOC of 100% was extracted from the CT image and recorded, and a sliding range of the longitudinal end segment of the first electrode was measured. Subsequently, the sliding range of the longitudinal end segment of the first electrode from CT images before activation and at SOC of 100% was evaluated and is presented in Fig. 13 shown. Reference test example 2
[0252] The sliding range of the longitudinal end section of the first electrode was measured in the same way as in reference experiment example 1, except that the secondary battery from example 2 was used. Subsequently, the sliding range of the longitudinal end section of the first electrode was evaluated from CT images taken before activation and at a state of charge (SOC) of 100% and is shown in Fig. 13 shown.
[0253] Fig. 13 CT images showing the sliding regions of longitudinal end sections of first electrodes of secondary batteries according to reference test example 1 and reference test example 2. In particular, Fig. 13 CT images before activation and at SOC of 100% of the secondary batteries according to reference test example 1 and reference test example 2, and images showing the sliding area of the longitudinal end section of the first electrode.
[0254] With reference to Fig.It was confirmed that in reference test example 1, a slip of 1.69° (= 18.41° (SOC 100) - 16.72° (before activation)) occurred, and in reference test example 2, a slip of 1.78° (= 55.08° (SOC 100) - 53.30° (before activation)) occurred. That is, as a result of measurements in both reference test example 1 and reference test example 2, it was confirmed that the longitudinal end section of the first electrode slips within the range of 1° to 3° relative to the initial position.
[0255] This shows that in the secondary batteries according to examples 1 and 2, slippage of the first electrode can occur due to contraction / expansion of the electrode before activation and at SOC of 100%, but the slippage occurs within a specific range (1° to 3°).
[0256] This means that the winding process is carried out while a (tensile) tension of a specific value or higher is maintained, so that the position of the point where the curvature of the first electrode is greatest is kept constant. Therefore, it is evident that even as the cycle progresses, the range of the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest is maintained within the sliding range (1° to 3°) of the longitudinal end section of the first electrode.
[0257] Fig. 1 and Fig. 2 images showing CT images of the electrode arrangements according to examples 1 and 2 and the curvatures of the first electrodes extracted from the CT images;
[0258] Fig. 3 to Fig.5 images showing CT images of electrode arrangements according to comparison examples 1 to 3 and the curvatures of the first electrodes extracted from the CT images;
[0259] In particular, press Fig. 1 to Fig. 5 in color coordinates a ratio assumed by measurement points that have a curvature equal to or less than an arbitrarily set reference value with respect to the curvature measured at each measurement point. Here, the set reference value is a specific value within a range of 0.5 to 1.0, and the range of the color index expressed on the right-hand side of the color coordinates is 0 to 0.8 in (a) of the Fig. 1 to Fig. 5 and is 1 to 1.5 in (b) the Fig. 1 to Fig. 5.
[0260] In particular, in (a) the Fig. 1 to Fig.5, if the color distribution range of the curvature measured at each measurement point is set to 0 to 0.8, a section in which areas with low k-values are distributed is implemented as color coordinates to visually express a flat area and a flatness component, and in (b) the Fig. 1 to Fig. 5. When the color distribution range of the curvature measured at each measurement point is set to 1 to 1.5, a section containing areas with high k-values is implemented as color coordinates to visually represent a point where the curvature is greatest. In this case, each measurement point was extracted from the CT image of the first electrode as described above, and the longitudinal end section of the first electrode, located at the core section, was aligned to be in the 6 o'clock direction.
[0261] Referring to Table 2, Fig. 1 to Fig. 5, Fig. 6(a) and Fig. 7(a), in the case of the electrode arrangements according to Example 1 and Example 2, after 50 cycles under conditions of 4.25 V-2.5 V 1 C / 1 C at 25 °C, the angles between the longitudinal end section of the first electrode, extracted from the CT image of the core section, and the point where the curvature of the first electrode is greatest, were 60.8° and 65° respectively, and it was confirmed that core collapse and core impact did not occur even after 500 cycles under conditions of 4.2 V (0.25 C) - 2.85 V (0.33 C) at 40 °C.
[0262] On the other hand, as in comparative examples 1 to 3, if the angle between the longitudinal end section of the first electrode extracted from the CT image of the core section and the point where the curvature of the first electrode is greatest was greater than 98°, or as in comparative examples 4 and 5, if the angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was 40° or less, i.e., if the angle range described above was not met, it was confirmed that the angle formed between the first extension line and the second extension line was 25° or greater and core impact occurred, or even if core impact did not occur, core collapse occurred because the area of the core cavity was less than 100%, based on 100% of the sum of the cross-sectional areas of the winding core used for winding, or the circularity of the core cavity was less than 89%. was.
[0263] It can thus be seen that, according to an embodiment of the present invention, the electrode arrangement and the secondary battery, including the same, adjust the angle between the longitudinal end section of the first electrode, extracted from the CT image of the core section, and the point where the curvature of the first electrode is greatest, to a specific range. This makes it possible to address the phenomenon that the core cavity does not maintain a circular shape due to the deformation of an electrode arrangement caused by the contraction / expansion of an electrode during charging and discharging of the battery, and collapses, in order to prevent damage to the second electrode and the separator and to prevent an internal short circuit between the first and second electrodes, thereby improving the stability and lifetime characteristics of the battery.
[0264] Fig.Figure 10 is an image showing a CT image of the electrode arrangement according to Example 1 and an arrangement relationship between the curvature of the first electrode extracted from the CT image and a winding core; and Fig. Figure 11 is an image showing a CT scan of the electrode arrangement according to comparison example 2 and an arrangement relationship between the curvature of the first electrode extracted from the CT scan and a winding core. Here, we show Fig. 10(a) and Fig. 11(a) schematically an arrangement relationship between winding cores A and B, each used for winding, and a section corresponding to a section where the curvature of the Fig. 10(b) and Fig. 11(b) measured first electrode is largest on the outer circumferential surfaces of the in Fig. 10(a) and Fig. 11(a) shown winding core B shown.
[0265] Referring to Table 2 and Fig. 10 and Fig.11. In the case of the electrode arrangement according to Example 1, the arrangement process was carried out such that the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was greater than 40° and 98° or less about the winding axis. As a result, it was confirmed that core collapse and core impact did not occur even after 50 cycles under conditions of 4.2 V–2.5 V 1°C / 1°C at 25°C or 500 cycles under conditions of 4.2 V (0.25°C)–2.85 V (0.33°C) at 40°C.
[0266] On the other hand, as in comparative example 2, if the angle formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was greater than 98° around the winding axis, that is, if the angular range formed between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest was not satisfied, it was confirmed that the angle formed between the first extension line and the second extension line was 25° or greater and core impact occurred, or even if core impact did not occur, core collapse occurred because the area of the core cavity was less than 100%, based on 100% of the sum of the cross-sectional areas of the winding core used for winding, or the calculated circularity of the core cavity was less than 89%.
[0267] It is evident that the method for manufacturing an electrode assembly makes it possible to manufacture an electrode assembly whose angle between the longitudinal end section of the first electrode and the point where the curvature of the first electrode is greatest has been set in a simpler way and is suitable for a continuous process using state-of-the-art roll-to-roll process equipment, thereby ensuring productivity and economy.
[0268] The foregoing detailed description is intended to illustrate and explain the present invention. Furthermore, the foregoing description is intended to show and describe only the preferred embodiment of the present invention, and as described above, the present invention can be used in various other combinations, modifications, and environments, and can be altered and modified within the scope of the concept of the invention disclosed in the present description, within the scope corresponding to the foregoing disclosure, and / or within the scope of the general knowledge in the field. Accordingly, the foregoing detailed description of the invention is not intended to limit the invention to the disclosed embodiments. Furthermore, the attached claims should be interpreted to include other embodiments. EXPLANATION OF REFERENCE NUMBERS AND SYMBOLS 100 second electrode 300 first electrode 310 Longitudinal end section of the first electrode E1 first extension straight E2 second extension straight R Direction of rotation of the winding core W Winding direction of the electrode arrangement A first winding core part B second winding core part S spacer
Claims
[1] An electrode assembly comprising a first electrode, a separator, and a second electrode stacked and wound around a winding axis, wherein an angle formed between a straight line extending from the winding axis through an inner end of the first electrode and a straight line extending from the winding axis through a maximum curvature point of the first electrode is between 40° and 98°. [2] The electrode assembly according to claim 1, wherein the curvature maximum point is a point at which the curvature of the first electrode is maximum in a region in a cross section of the electrode assembly perpendicular to the winding axis, the region extending from the inner end of the first electrode over an azimuth angle of 0° and 180° in a direction opposite to a winding direction in which the electrode assembly is wound around the winding axis. [3] An electrode assembly according to claim 1 or 2, wherein the maximum curvature point of the first electrode is formed in or on a part of the electrode assembly within 3 turns of the first electrode from the inner end thereof. [4] The electrode assembly according to any one of the preceding claims, wherein the first electrode comprises a first electrode current collector and a first electrode active material layer provided on at least one surface of the first electrode current collector such that the first electrode active material layer extends to an inner end of the first electrode current collector and the inner end of the first current collector corresponds to the inner end of the first electrode. [5] The electrode assembly of claim 4, wherein the first electrode comprises a first uncoated electrode portion in which the first electrode active material layer is not provided, and wherein the electrode assembly further comprises a first electrode tab physically connected to or formed on the first uncoated electrode portion. [6] An electrode assembly according to any one of the preceding claims, wherein an angle formed between the straight line extending from the winding axis through the inner end of the first electrode and a straight line extending from the winding axis through a point where the curvature of the first electrode is 1 or less is greater than 0°. [7] Electrode arrangement according to one of the preceding claims, wherein the angle formed between the straight line extending from the winding axis through the inner end of the first electrode and the straight line extending from the winding axis through the maximum curvature point of the first electrode is determined after activation of the electrode arrangement. [8] An electrode assembly according to any one of the preceding claims, wherein the angle formed between the straight line extending from the winding axis through the inner end of the first electrode and the straight line extending from the winding axis through the curvature maximum point is determined after 50 times of charging and discharging under conditions of 25°C, 1 C charge and 1 C discharge. [9] An electrode assembly according to any preceding claim, wherein a circularity of the first electrode in or at a part of the electrode assembly within 3 turns of the first electrode from the inner end thereof is 89% or more. [10] Electrode arrangement according to one of the preceding claims, wherein the first electrode has a first surface facing the winding axis and a second surface opposite the first surface, and wherein a first extension line is formed by extending a straight line connecting two points at which a curvature direction changes within a distance of 5 mm from the inner end of the first electrode on the first surface of the first electrode, wherein a second extension line is formed by extending a straight line connecting two points within a distance of 5 mm from the inner end of the first electrode on a surface of the second electrode facing the first surface of the first electrode, wherein the first extension line and the second extension line form an angle of 25° or less. [11] An electrode assembly according to any preceding claim, wherein the first electrode has no crack or fold in or on any part of the electrode assembly within 3 turns of the first electrode from the inner end thereof. [12] An electrode assembly according to any preceding claim, wherein a flatness percentage of the first electrode in or at a part of the electrode assembly within 3 turns of the first electrode from the inner end thereof is greater than 3% and 13.5% or less. [13] An electrode assembly manufactured by a method, the method comprising: Arranging a first electrode, a separator and a second electrode on top of each other in this order to form a stack; and Winding the stack around a winding axis using a winding core, wherein the winding core has a first winding core part and a second winding core part, wherein during winding the separator is held between the first winding core part and the second winding core part, and wherein the arranging is performed such that an angle formed between a straight line extending from the winding axis through an inner end of the first electrode and a straight line extending from the winding axis through a curvature maximum point of the first electrode is greater than 40° and 98° or less. [14] Electrode assembly according to claim 13, wherein the first winding core part and the second winding core part are not symmetrical to each other in a cross section perpendicular to the winding axis. [15] Electrode arrangement according to claim 13 or 14, wherein in a cross section perpendicular to the winding axis, an area of the first winding core part is smaller than an area of the second winding core part, and wherein the arranging is performed such that the inner end of the first electrode is arranged on an outer peripheral surface of the first winding core part. [16] An electrode assembly according to any one of claims 13 to 15, wherein the winding is performed while maintaining a tension of 3.92 N or higher. [17] Secondary battery comprising: the electrode arrangement according to one of claims 1 to 12 and 16.