UV PRE-CURABLE EPOXY COMPOSITION FOR TWO-STAGE ASSEMBLY PROCESS

DE502017016435D1Active Publication Date: 2024-10-10HENKEL KGAA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016435
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2017-06-28
Publication Date
2024-10-10
Estimated Expiration
2037-06-28

AI Technical Summary

Technical Problem

Epoxy resin-based adhesives used in the automotive industry and screen printing face issues with low viscosity after application, leading to poor bonding and defects due to running or squeezing out, while high-viscosity adhesives are difficult to handle and may still squeeze out during thermal curing.

Method used

An adhesive composition comprising at least 50% aromatic epoxy resin, a compound with one oxetane group, and a photoinitiator, which is pre-cured with radiation and then thermally cured, maintaining viscosity stability during thermal curing to prevent squeezing out.

Benefits of technology

The adhesive composition is easy to handle, meets high automotive sector requirements, and maintains viscosity stability during thermal curing, minimizing defects and ensuring strong bonding.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to adhesive compositions containing at least one aromatic epoxy resin, at least one compound having at least one oxetane group and at least one photoinitiator, a process for bonding at least two components and the use of corresponding adhesive compositions.

[0002] Epoxy resin-based adhesives are widely used in the automotive industry and other fields, for example, to bond components made of the same or similar materials. Epoxy adhesives are also used for screen printing, with screen printing being a particularly suitable method for bonding two components in the automotive sector. Using the screen printing process, the adhesive can be applied to the components very precisely, both in terms of the required thickness and the exact location. However, conventional adhesives often have the disadvantage of having too low a viscosity after application. These low-viscosity adhesives can then run after application or be pushed or squeezed out of the joining zone when the components are joined, which leads to inadequate bonding and defects.

[0003] Adhesives that have a high viscosity from the start, so they don't run or squeeze out after application, have the disadvantage of being more difficult to handle and may not be suitable for screen printing. Other adhesives can be pre-cured using UV radiation after application before thermal curing. While this prevents immediate runout after application, these adhesives are still squeezed out of the joining zone during joining, especially under pressure, because the viscosity of these adhesives drops significantly due to the temperature increase required for thermal curing.

[0004] UV-curing adhesive compositions based on epoxides are known from WO2007 / 036524 A1.

[0005] Therefore, there is still a need for epoxy resin-based adhesives that overcome these disadvantages. In particular, the objective was to provide an adhesive composition that is easy to handle, particularly suitable for screen printing, meets the high demands on adhesive properties in the automotive sector, and does not exhibit a viscosity that is too low during bonding to allow it to be squeezed out of the bonding zone.

[0006] The object is surprisingly achieved by the adhesive composition according to the claims. In a first aspect, the present invention therefore relates to an adhesive composition comprising (a) at least 50 wt.% of at least one aromatic epoxy resin; (b) at least one compound having at least one oxetane group; and (c) at least one photoinitiator, characterized in that the at least one compound having at least one oxetane group has exactly one oxetane group per molecule and / or the at least one compound having at least one oxetane group additionally has at least one hydroxyl group.

[0007] In particular, the object is surprisingly achieved by a method for bonding, wherein after the application of the said adhesive composition to a first substrate to be bonded, the adhesive composition is pre-cured with radiation, then the substrate is joined to a second substrate and thermally cured.

[0008] The adhesive compositions according to the invention are both easy to handle, particularly in screen printing, and meet the high demands regarding adhesive properties in the automotive sector. By using at least one compound with at least one oxetane group, it is possible to ensure that the viscosity of the adhesive composition does not drop upon heating for thermal curing, thereby minimizing or even completely preventing "squeezing out" of the adhesive composition. "At least one," as used herein, refers to 1 or more, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, or more. In the context of components of the adhesive compositions described herein, this information does not refer to the absolute amount of molecules but to the type of component. "At least one epoxy resin" therefore means, for example, one or more different epoxy resins, i.e.one or more different types of epoxy resins. When used in conjunction with quantities, the quantities refer to the total amount of the correspondingly designated type of ingredient, as defined above.

[0009] "Approximately", as used herein in connection with numerical values, refers to the referenced numerical value ±10%, preferably ±5%.

[0010] Where reference is made herein to the molecular weight of polymeric compounds, the data refer to the number-average molecular weight M n , unless otherwise stated. The molecular weight can be determined by GPC against a polystyrene standard.

[0011] The adhesive composition contains at least one aromatic epoxy resin. Typically, these resins contain epoxy groups, or epoxy resins (on average) have at least two epoxy groups per molecule, preferably two to ten epoxy groups per molecule. "Epoxide groups," as used herein, refer to 1,2-epoxide groups (oxiranes).

[0012] Examples of suitable resins include, but are not limited to, (poly)glycidyl ethers, which are usually obtained by reacting epichlorohydrin or epibromohydrin with aromatic polyphenols in the presence of alkali, or (poly)glycidyl ethers of phenol-formaldehyde novolak resins, alkyl-substituted phenol-formaldehyde resins (epoxy novolak resins), phenol-hydroxybenzaldehyde resins, cresol-hydroxybenzaldehyde resins, dicyclopentadiene-phenol resins, and dicyclopentadiene-substituted phenol resins. Polyphenols suitable for this purpose include resorcinol, pyrocatechol, hydroquinone, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), bisphenol F (bis(4-hydroxyphenyl)methane), 1,1-bis(4-hydroxyphenyl)isobutane, 4,4-dihydroxybenzophenone, 1,1-bis(4-hydroxyphenyl)ethane and 1,5-hydroxynaphthalene.Also suitable are diglycidyl ether of ethoxylated resorcinol (DGER), diglycidyl ether of resorcinol, pyrocatechol, hydroquinone, bisphenol, bisphenol A, bisphenol AP (1,1-bis(4-hydroxyphenyl)-1-phenylethane), bisphenol F, bisphenol K, bisphenol S, and tetramethylbiphenol.

[0013] Preferably, the at least one aromatic epoxy resin has an epoxy equivalent of between 130 and 1000 g / mol equivalent, in particular between 140 and 500 g / mol equivalent, preferably between 150 and 250 g / mol equivalent. The epoxy equivalent can be determined according to DIN 16945.

[0014] The composition particularly preferably contains at least one aromatic epoxy resin that is liquid at 25°C. Preferably, it contains at least one aromatic epoxy resin that is liquid at 25°C and has a viscosity at 25°C of less than 10 Pas, in particular from 0.01 to 10 Pas, preferably from 0.1 to 7 Pas, particularly preferably from 1 to 5 Pas. The viscosity can be determined according to DIN 53105. Particularly preferred are liquid epoxy resins obtained by reacting bisphenol A or bisphenol F or mixtures thereof, in particular mixtures of bisphenol A and bisphenol F, and epichlorohydrin.

[0015] In particular, in addition to the liquid aromatic epoxy resin, the composition may contain at least one aromatic epoxy resin having a viscosity at 50°C of greater than 10 Pas, in particular of 10 to 200 Pas, preferably of 20 to 100 Pas. The viscosity can be determined according to DIN 53105. These epoxy resins are particularly preferably polyglycidyl ethers of novolak resins. Novolak resins are condensates of phenols or phenol derivatives with formaldehyde. These epoxy resins are particularly preferably polyglycidyl ethers of phenol novolak and / or cresol novolak, in particular phenol-formaldehyde resins (phenol novolak).

[0016] The adhesive composition preferably contains at least one epoxy resin selected from epoxy resins based on bisphenol or epoxy resins based on novolak resins, in particular phenol-formaldehyde resins, or mixtures thereof. In a preferred embodiment, the adhesive composition contains at least one epoxy resin obtained by reacting bisphenol A or bisphenol F or mixtures thereof, in particular mixtures of bisphenol A and bisphenol F, and epichlorohydrin. In another preferred embodiment, the adhesive composition contains at least one epoxy resin that is a polyglycidyl ether of novolak resins, in particular phenol novolak and / or cresol novolak, preferably phenol-formaldehyde resins.In a particularly preferred embodiment, the adhesive composition contains at least two different epoxy resins, preferably a mixture of at least one epoxy resin based on bisphenol, in particular bisphenol A or bisphenol F or mixtures thereof, and an epoxy resin based on novolak resins, in particular phenol-formaldehyde resins.

[0017] The proportion of the at least one aromatic epoxy resin or of all aromatic epoxy resins contained therein in the total adhesive composition is at least 50% by weight, preferably 50 to 98% by weight, in particular 60 to 97% by weight, particularly preferably 70 to 95% by weight.

[0018] The adhesive composition preferably contains at least 30% by weight, preferably 40 to 80% by weight, in particular 50 to 70% by weight, in each case based on the total adhesive composition, of at least one epoxy resin based on bisphenol, in particular bisphenol A or bisphenol F or mixtures thereof.

[0019] The adhesive composition preferably contains at least 10 wt.%, preferably 10 to 50 wt.%, in particular 20 to 40 wt.%, in each case based on the total adhesive composition, of at least one epoxy resin based on novolak resins, in particular phenol-formaldehyde resins.

[0020] The adhesive composition particularly preferably contains at least 30 wt.%, preferably 40 to 80 wt.%, in particular 50 to 70 wt.%, in each case based on the total adhesive composition, of at least one epoxy resin based on bisphenol, in particular bisphenol A or bisphenol F or mixtures thereof, and at least 10 wt.%, preferably 10 to 50 wt.%, in particular 20 to 40 wt.%, in each case based on the total adhesive composition, of at least one epoxy resin based on novolak resins, in particular phenol-formaldehyde resins.

[0021] In addition to the aromatic epoxy resin, the adhesive composition contains at least one compound with at least one oxetane group, preferably 1 to 4, in particular 1 to 2, particularly preferably exactly one oxetane group per molecule. "Oxetane group," as used herein, refers to a four-membered ring containing one oxygen atom. In addition to the oxetane group, these compounds may also contain at least one hydroxyl group, preferably 1 to 4, in particular 1 to 2, particularly preferably exactly one hydroxyl group per molecule.

[0022] Preferably, the compound with at least one oxetane group, in particular exactly one oxetane group, is a monomeric compound.

[0023] Preferably, the at least one compound having at least one oxetane group, in particular also having a hydroxyl group, has a molecular weight of less than 1000 g / mol, preferably less than 500 g / mol, more preferably less than 300 g / mol. In particular, the at least one compound having at least one oxetane group, in particular also having a hydroxyl group, has a molecular weight of 70 to 1000 g / mol, preferably 100 to 500 g / mol, more preferably 120 to 200 g / mol.

[0024] Particularly preferably, the adhesive composition contains at least one compound having an oxetane group according to formula (I): wherein R 1< represents alkyl, alkoxy, alkoxyalkyl, aryloxyalkyl, hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, aryl, aryloxy, hydroxyaryl or hydroxyaryloxy, and R 2< and R 3< independently represent hydrogen, alkyl, alkoxy, alkoxyalkyl, aryloxyalkyl, hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, aryl, aryloxy, hydroxyaryl or hydroxyaryloxy.

[0025] Most preferably, the adhesive composition contains as at least one compound having an oxetane group and at least one hydroxyl group a hydroxyoxetane according to the above-mentioned formula (I), wherein R 1< represents alkyl, alkoxy, alkoxyalkyl, aryloxyalkyl, hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, aryl, aryloxy, hydroxyaryl or hydroxyaryloxy, R 2< represents hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, hydroxyaryl or hydroxyaryloxy, and R 3< independently represents hydrogen, alkyl, alkoxy, alkoxyalkyl, aryloxyalkyl, hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, aryl, aryloxy, hydroxyaryl or hydroxyaryloxy.

[0026] Preferably, the at least one hydroxyoxetane of formula (I) a 3-alkyl-3-(hydroxyalkyl)oxetane [ie R 1< = alkyl, R 2< = hydroxyalkyl, all R 3< = H], a 3,3-di(hydroxyalkyl)oxetane [ie R 1< , R 2< = hydroxyalkyl, all R 3< = H], a 3-alkyl-3-(hydroxyalkoxy)oxetane [ie R 1< = alkyl, R 2< = hydroxyalkoxy, all R 3< = H], a 3-alkyl-3-(hydroxyalkoxyalkyl)oxetane [ie R 1< = alkyl, R 2< = hydroxyalkoxyalkyl, all R 3< = H], or a mixture of these hydroxyoxetanes, particularly preferably a 3-alkyl-3-(hydroxyalkyl)oxetane [ie R 1< = alkyl, R 2< = hydroxyalkyl, all R 3< = H] and / or a 3-Alkyl-3-(hydroxyalkoxy)oxetane [ie R 1 < = alkyl, R 2 < = hydroxyalkoxy, all R 3 < = H].

[0027] The term "alkyl" here preferably stands for linear or branched alkyl radicals having 1 to 24 carbon atoms, for example, having 1 to 12 or 1 to 8 carbon atoms. The term "alkyl" particularly preferably stands for methyl or ethyl.

[0028] The term "alkoxy" here preferably stands for methoxy, ethoxy, propoxy, butoxy, phenylethoxy, particularly preferably ethoxy and / or propoxy, and comprises up to 20 alkoxy units or a combination of two or more alkoxy units, which may be arranged randomly, blockwise or gradient-like.

[0029] Particularly preferably, at least one hydroxyoxetane selected from the group consisting of 3-methyl-3-(hydroxymethyl)oxetane, 3-ethyl-3-(hydroxymethyl)oxetane, and 3,3-di(hydroxymethyl)oxetane (trimethylolpropane oxetane; TMPO) is used as the hydroxyoxetane. Mixtures of these compounds can also be used. Most preferably, the adhesive composition contains trimethylolpropane oxetane as the at least one compound having at least one oxetane group.

[0030] The adhesive composition preferably contains 1 to 20 wt.%, preferably 2 to 15 wt.%, in particular 5 to 10 wt.%, in each case based on the total adhesive composition, of the at least one compound having at least one oxetane group, in particular also having a hydroxyl group.

[0031] The adhesive compositions described herein can be precured by a light-initiated polymerization reaction. The compositions are cationically polymerized using a cationic photoinitiator that forms cations upon absorption of a specific wavelength of light.

[0032] The cationic photoinitiator can be one of those commonly used for cationic polymerization. Examples include onium salts with low nucleophilicity anions, such as halonium salts, iodonium salts, sulfonium salts, sulfoxonium salts, or diazonium salts. Suitable anions include, for example, hexafluoroantimonate, hexafluorophosphate, or tetrakis(pentafluorophenyl)borate. Sulfonium and iodonium salts are preferred, with the counterion being selected from hexafluoroantimonate, hexafluorophosphate, and (tetrakis(pentafluoroaryl))borates, especially triarylsulfonium and bis(alkylphenyl)iodonium salts with hexafluoroantimonate as the counterion, particularly preferably triarylsulfonium hexafluoroantimonate salts.

[0033] The adhesive composition preferably contains 0.1 to 5 wt.%, preferably 0.5 to 3 wt.%, in particular 1 to 2 wt.%, in each case based on the total adhesive composition, of the at least one photoinitiator.

[0034] Optionally, the adhesive compositions according to the invention can also contain reactive diluents as a further component to adjust the flow behavior. For the purposes of this invention, reactive diluents are low-viscosity substances containing hydroxyl or epoxy groups and having an aliphatic or aromatic structure, in particular compounds containing epoxy groups. Typical examples of reactive diluents are monoglycidyl ethers of C6 to C14 monoalcohols or alkylphenols as well as the monoglycidyl ethers of cashew nut shell oil, mono- or diglycidyl ethers of ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, neopentylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, cyclohexanedimethanol, triglycidyl ethers of trimethylolpropane as well as the glycidyl esters of C6 to C24 carboxylic acids or mixtures thereof.Reactive diluents with an epoxy group are particularly preferred, with monoglycidyl ethers of C6 to C14 monoalcohols or alkylphenols being preferred. Reactive diluents with an epoxy group differ from aromatic epoxy resins and are not considered to be such.

[0035] In a preferred embodiment, the adhesive composition contains up to 20 wt.%, preferably 1 to 15 wt.%, in particular 2 to 10 wt.%, in each case based on the total adhesive composition, of the at least one reactive diluent, preferably a monoglycidyl ether of C6 to C14 monoalcohols or alkylphenols.

[0036] The adhesive compositions of the invention can, in principle, also contain all additional components known and customary in the art. Such additional components include, but are not limited to, adhesion promoters, fillers, plasticizers, diluents, flow agents, coupling agents, wetting agents, flame retardants, viscosity control agents, preservatives, stabilizers, defoamers, and dyes. The additional components should preferably not be UV-absorbing. The additives are preferably present in an amount of less than 10 wt. %, in particular less than 3 wt. %, preferably less than 1 wt. %, based in each case on the total adhesive composition.

[0037] In a preferred embodiment, the adhesive composition contains (a) at least 50% by weight, preferably 50 to 98% by weight, in particular 60 to 97% by weight, particularly preferably 70 to 95% by weight of an aromatic epoxy resin; (b) 1 to 20% by weight, preferably 2 to 15% by weight, in particular 5 to 10% by weight, of at least one compound having at least one oxetane group, in particular also having a hydroxyl group, in particular a hydroxyoxetane; (c) 0.1 to 5% by weight, preferably 0.5 to 3% by weight, in particular 1 to 2% by weight of at least one photoinitiator; and (d) optionally up to 20% by weight, preferably 1 to 15% by weight, in particular 2 to 10% by weight of at least one reactive diluent, in particular having exactly one epoxy group per molecule.

[0038] Unless otherwise stated, the weight percentages refer to the total adhesive composition.

[0039] In a further preferred embodiment, the adhesive composition contains (a) at least 50% by weight of an aromatic epoxy resin; wherein (a1) at least 30% by weight, preferably 40 to 80% by weight, in particular 50 to 70% by weight, of at least one epoxy resin based on bisphenol, in particular bisphenol A or bisphenol F or mixtures thereof, and (a2) at least 10% by weight, preferably 10 to 50% by weight, in particular 20 to 40% by weight of at least one epoxy resin based on novolak resins, in particular phenol-formaldehyde resins; (b) 1 to 20% by weight, preferably 2 to 15% by weight, in particular 5 to 10% by weight, of at least one compound having at least one oxetane group, in particular also having a hydroxyl group, in particular a hydroxyoxetane; (c) 0.1 to 5% by weight, preferably 0.5 to 3% by weight, in particular 1 to 2% by weight of at least one photoinitiator; and (d) optionally up to 20 wt.%, preferably 1 to 15 wt.%, in particular 2 to 10 wt.-% of at least one reactive diluent, in particular with exactly one epoxy group per molecule.

[0040] The invention further relates to a bonding method, wherein, after applying the adhesive composition to a first substrate to be bonded, the adhesive composition is precured with radiation. Subsequently, the substrate is joined to a second substrate and thermally cured. In particular, the method involves a screen printing method, since the screen printing method allows for high precision in terms of the application location and application thickness, ensuring that the adhesive is applied in the correct amount at the right location. This saves adhesive while simultaneously resulting in optimal bonding with the fewest possible errors.

[0041] In the first step, the adhesive composition described above is applied to a substrate to be bonded, preferably by screen printing.

[0042] The epoxy resin adhesives of the present invention can be used for a variety of materials. Suitable materials include, but are not limited to, metals such as aluminum and steel; thermoplastic polymers such as polyethylene, polypropylene, polyurethane, polyacrylate, and polycarbonate, as well as their copolymers; thermoset polymers such as vulcanized rubbers; urea-formaldehyde foams; melamine resins; wood; glass; graphitic substrates; carbon fiber composites (CFCs), glass fiber composites (GFCs), and other composites. The epoxy resin adhesives can be used to bond identical, similar, or different materials, such as steel and steel, steel and aluminum, CFCs and steel, CFCs and aluminum, polycarbonate and vulcanized rubber, or aluminum and wood.

[0043] The adhesive composition, i.e. the uncured adhesive composition before application, preferably has a viscosity at 25°C of less than 100 Pas, in particular from 0.01 to 100 Pas, preferably from 0.1 to 50 Pas, more preferably from 1 to 20 Pas. A corresponding viscosity is particularly advantageous for handling and optimal application of the adhesive composition, in particular for the screen printing process. The viscosity can be determined by means of photorheology, preferably using a plate-plate configuration with d = 15 mm, a distance of 0.1 mm and a mercury lamp as the UV source. For example, the measurement can be carried out using an Anton Paar MCR 302 with an Omnicure S2000 lamp.

[0044] After application, the applied adhesive composition is pre-cured using radiation, in particular light, preferably UV radiation. This pre-curing fixes the initially typically low-viscosity adhesive composition before it is thermally cured after joining to the second substrate to be bonded. The pre-curing of the composition typically occurs through cationic polymerization initiated by radiation, such as light. The light used to initiate the polymerization reaction is preferably short-wave light, for example UV light. Pre-curing does not lead to complete curing. Complete curing of the adhesive composition is only achieved through thermal curing.

[0045] Pre-curing typically occurs at temperatures below 50 °C, preferably at temperatures between 10 and 30 °C. The duration of irradiation for pre-curing, especially with UV radiation, is preferably 0.1 to 300 seconds, more preferably 1 to 100 seconds.

[0046] After pre-curing, the adhesive composition preferably has a viscosity at 25°C of greater than 1000 Pas, in particular from 1000 to 50,000 Pas, preferably from 2000 to 20,000 Pas, and more preferably from 3000 to 10,000 Pas. Such a viscosity is particularly advantageous for the subsequent process, as it prevents the adhesive from running or being squeezed out under pressure during joining. Furthermore, storage at this stage of the process would be possible.

[0047] After pre-curing, the first substrate is joined to the second substrate and thermally cured. Thermal curing typically occurs at temperatures above 50°C, preferably between 50 and 200°C, in particular between 70 and 150°C, preferably between 80 and 120°C. Joining and subsequent thermal curing preferably occur under pressure, with the first substrate being joined to the second substrate under pressure, and the pressure subsequently being maintained during thermal curing.

[0048] By using at least one compound with at least one oxetane group, especially a hydroxyoxetane, it is possible to ensure that the viscosity of the adhesive composition does not decrease after pre-curing upon heating for thermal curing, thereby minimizing or even completely preventing the "squeezing out" of the adhesive composition. Thus, it is particularly advantageous if the viscosity of the adhesive composition does not decrease after pre-curing upon heating.

[0049] Finally, the invention also relates to the product bonded using the adhesive compositions described herein or produced according to the described method for bonding two substrates. Furthermore, the invention also relates to the use of the compositions described herein for bonding at least two substrates or components, in particular according to the described method.

[0050] All embodiments disclosed in connection with the adhesive compositions are equally applicable to the cured formulations and the described processes and vice versa.

[0051] In the following, the invention is illustrated by examples, but is not limited to them. Examples Implementation:

[0052] The compositions were mixed according to Table 1 and then the viscosity behavior during UV curing and subsequent thermal curing was measured.

[0053] Viscosity was measured using photorheology, using a plate-to-plate configuration with d = 15 mm, a gap of 0.1 mm, and a mercury lamp as the UV source. The measurements were performed using an Anton Paar MCR 302 with an Omnicure S2000 mercury lamp. Table 1: Compositions (quantities in wt.%) V1 E1 E2 E3 Aromatic epoxy resin 1< 62,42 59,92 57,42 54,92 Epoxy Novolac 2< 29,94 29,94 29,94 29,94 Reactive Thinner 3< 6,41 6,41 6,41 6,41 TMPO 4< - 2,5 5 7,5 UV hardener 5< 1,23 1,23 1,23 1,23 E: According to the invention; V: Comparative example 1: Aromatic epoxy resin based on a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin; epoxy equivalent weight of 165 g / mol, viscosity at 25°C of 2.5 Pas 2: Epoxy novolac based on a reaction product of ephichlorohydrin with a phenol-formaldehyde novolac with an epoxy equivalent weight of 178 g / mol, a viscosity at 52°C of 35 Pas 3: Monoglycidyl ether of para-tert-butylphenol; epoxy equivalent weight of 220 g / mol 4: Trimethylolpropane oxetane 5: Mixture of triarylsulfonium hexafluoroantimonate salts

[0054] Figure 1 shows the viscosity development (solid curve) of the reference composition V1 with respect to time and temperature (dashed curve). During the initial UV curing, the viscosity increases sharply. During the subsequent heating for thermal curing, the viscosity initially drops sharply before the onset of thermal curing leads to a renewed increase in viscosity. The drop in viscosity at the beginning of heating causes the corresponding compositions to sag, especially when additional pressure is applied during thermal curing in a screen printing process.

[0055] Figure 2 shows the viscosity development of composition E2 (solid curve) compared to the viscosity development of the reference composition V1 (dashed curve). It is clearly evident that in the case of composition E2, the viscosity does not decrease upon heating, but rather increases steadily. The other compositions E1 and E3 also show a similar development. Because the viscosity does not decrease, these compositions remain dimensionally stable and do not flow unintentionally during thermal curing.

Claims

1. An adhesive composition comprising: (a) at least 50 wt.% of at least one aromatic epoxy resin; (b) at least one compound having at least one oxetane group; and (c) at least one photoinitiator, characterized in that the at least one compound having at least one oxetane group has exactly one oxetane group per molecule and / or the at least one compound having at least one oxetane group additionally has at least one hydroxyl group.

2. The adhesive composition according to claim 1, characterized in that the at least one aromatic epoxy resin has at least two epoxy groups per molecule and / or is selected from epoxy resins based on bisphenol or epoxy resins based on novolak resins, in particular phenol-formaldehyde resins, or from mixtures thereof.

3. The adhesive composition according to claim 1 or claim 2, characterized in that the at least one aromatic epoxy resin has an epoxy equivalent between 130 and 1000 g / mol equivalent, in particular between 140 and 500 g / mol equivalent, preferably between 150 and 250 g / mol equivalent.

4. The adhesive composition according to one of claims 1 to 3, characterized in that the adhesive composition contains at least two different aromatic epoxy resins, preferably a mixture of at least one epoxy resin based on bisphenol, in particular bisphenol A or bisphenol F or mixtures thereof, and of an epoxy resin based on novolak resins, in particular phenol-formaldehyde resins.

5. The adhesive composition according to one of claims 1 to 4, characterized in that the adhesive composition contains at least one compound having an oxetane group according to formula (I): where R1 represents alkyl, alkoxy, alkoxyalkyl, aryloxyalkyl, hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, aryl, aryloxy, hydroxyaryl or hydroxyaryloxy, and R2 and R3 each independently represent hydrogen, alkyl, alkoxy, alkoxyalkyl, aryloxyalkyl, hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, aryl, aryloxy, hydroxyaryl or hydroxyaryloxy, in particular R2 represents hydroxyalkyl, hydroxyalkoxy, hydroxyalkoxyalkyl, hydroxyaryl or hydroxyaryloxy.

6. The adhesive composition according to one of claims 1 to 5, characterized in that the adhesive composition contains, as at least one compound having an oxetane group, hydroxyoxetane selected from the group consisting of 3-methyl-3-(hydroxymethyl)oxetane, 3-ethyl-3-(hydroxymethyl)oxetane, 3,3-di(hydroxymethyl)oxetane (trimethylolpropane oxetane; TMPO) and mixtures thereof.

7. The adhesive composition according to one of claims 1 to 6, characterized in that the adhesive composition further contains a reactive diluent.

8. The adhesive composition according to one of claims 1 to 7, characterized in that the composition contains: (a) 50 to 98 wt.%, in particular 60 to 97 wt.%, particularly preferably 70 to 95 wt.% of an aromatic epoxy resin; (b) 1 to 20 wt.%, preferably 2 to 15 wt.%, in particular 5 to 10 wt.% of at least one compound having at least one oxetane group, wherein the at least one compound having at least one oxetane group has exactly one oxetane group per molecule, and / or the at least one compound having at least one oxetane group additionally has at least one hydroxyl group; (c) 0.1 to 5 wt.%, preferably 0.5 to 3 wt.%, in particular 1 to 2 wt.% of at least one photoinhibitor; and (d) optionally up to 20 wt.%, preferably 1 to 15 wt.%, in particular 2 to 10 wt.% of at least one reactive diluent, in particular having exactly one epoxy group per molecule.

9. A method for bonding at least two substrates, wherein after applying an adhesive composition according to one of claims 1 to 8 to a first substrate to be bonded, the adhesive composition is pre-cured by radiation and then the substrate is joined to a second substrate and thermally cured.

10. The method for bonding according to claim 9, characterized in that the method is carried out by a screen printing process.

11. The method for bonding according to claim 9 or claim 10, characterized in that before application, the adhesive composition has a viscosity at 25°C of less than 100 Pas, in particular from 0.01 to 100 Pas, preferably from 0.1 to 50 Pas, preferably from 1 to 20 Pas, and / or after pre-curing, the adhesive composition has a viscosity at 25°C of greater than 1000 Pas, in particular from 1000 to 50000 Pas, preferably from 2000 to 20000 Pas, preferably from 3000 to 10000 Pas, wherein the viscosity is determined as stated in the description.

12. The method for bonding according to one of claims 9 to 11, characterized in that after pre-curing, the viscosity of the adhesive composition does not drop when heated for thermal curing.

13. A product which has been bonded by means of an adhesive composition according to one of claims 1 to 8 or which has been produced by means of a method for bonding at least two substrates according to claims 9 to 12.

14. Use of an adhesive composition according to one of claims 1 to 8 for bonding at least two substrates, in particular in the method for bonding at least two substrates according to claims 10 to 12.