PREFORM MADE OF POLYESTER

DE502019012521D1Active Publication Date: 2024-12-05ALPLA WERKE ALWIN LEHNER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012521
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-02
Filing Date
2019-07-29
Publication Date
2024-12-05
Estimated Expiration
2039-07-29

AI Technical Summary

Technical Problem

Polyester containers are prone to stress cracking due to material inhomogeneity and environmental influences, leading to failure and potential explosion, especially in reusable containers subjected to aggressive washing and high internal pressures.

Method used

A preform made of polyester based on furandicarboxylic acid and diols, with a spiro compound added to enhance molecular mobility and protect ester bonds from nucleophilic attacks, reducing crack formation and improving Environmental Stress Cracking Resistance (ESCR).

Benefits of technology

The addition of spiro compounds significantly increases the durability of polyester containers, allowing them to withstand higher chemical and environmental stresses, internal pressures, and extreme temperatures, preventing cracking and failure, as demonstrated by the ISBT stress cracking test.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Field of the invention

[0001] The invention relates to a preform made of polyester for producing a plastic container in a blow molding process and a process for producing a preform. State of the art

[0002] In the packaging sector, the market share of polyesters is increasing. In addition to conventional materials such as polyethylene terephthalate (PET) and its copolyesters, bio-based polyesters such as polyethylene furanoate (PEF) will also establish themselves on the market in the future.

[0003] These polyesters have many advantages over other plastic groups: They can be made partly or, in the case of PEF, entirely from renewable raw materials, have very good recyclability (provided no additives / dyes that are harmful to recycling are added), and their inherent transparency creates design advantages that are not available to other plastics.

[0004] In addition, polyester containers are available not only as disposable packaging, but also as reusable packaging. Compared to glass, for example, this results in significant weight savings and advantageous mechanical properties (e.g., no shattering). Furthermore, the energy required to produce polyester containers is significantly lower than for glass production.

[0005] The production of plastic containers often takes place in two stages: First, a preform is produced using the injection molding process. This preform is then heated beyond its glass transition point and blown into the bottle. The first step in preform production is a primary forming process. During this process, the melt must be rapidly cooled to inhibit crystallization and freeze the material amorphously.

[0006] During this cooling process, or later after the preform has been blown into a bottle and the bottle has cooled down, so-called residual stresses can be frozen in the material, especially in the vicinity of the injection point, which often lead to stress cracking in the further process.

[0007] This is due to the inhomogeneity of the material. The material contains regions of low molecular density and regions of high molecular density, with crack formation being initiated primarily in the region of low molecular density. The inflation process from the preform to the finished container creates additional stresses in the material, which increase the susceptibility to stress cracking. Additional stresses due to internal pressure in the container (e.g. in carbonated drinks, aerosols, etc.), especially in containers with a volume greater than 1.5 l, and external influences such as contact with chemicals (particularly alkalis) intensify or accelerate crack formation. This crack formation is accelerated particularly by detergents, fragrance-active substances such as aldehydes, ketones and short carboxylic acids and solvents such as acetone and ammonia.As a result, it is often not possible to fill many detergents, cosmetic products, window cleaning agents, varnishes and paints into polyester containers.

[0008] The cracking process is often referred to as environmental stress cracking (ESC), and a material's resistance to this process is therefore referred to as environmental stress cracking resistance (ESCR). If a material exhibits poor ESCR, the container may rupture. Depending on the internal pressure, the crack's expansion may even lead to an explosion.

[0009] A further explanation for the behavior described above can be identified in the ester bond: Environmental influences or contact with chemicals (e.g., alkalis such as NaOH) can lead to saponification of the ester, which manifests itself in the form of hydrolysis or chain scission in the material and is reflected in deteriorated material properties. Container failure is accelerated by the saponification reaction.

[0010] While the above-mentioned problems apply to any container made of polyester (e.g., disposable bottles), reusable packaging is particularly exposed to an additional risk: After use and before being put back on the market, reusable packaging is subjected to an intensive washing process at high temperatures (sometimes up to 75°C) and using aggressive chemicals (washing solutions). This increasing stress often manifests itself in the clouding of the bottle, a visual appearance caused by a multitude of tiny microcracks. These microcracks cause the material to become brittle and subsequently lead to the formation of macrocracks and thus to container failure.

[0011] US 2017 / 012453 A1 describes a polyester polymerized from a monomeric dicarboxylic acid, an esterified monomeric dicarboxylic acid, or a combination of the dicarboxylic acids and a polyol monomer. The dicarboxylic acids include furandicarboxylic acid. The polyol monomers contain C2-C14 polyols and spirodiol. The polyester is easy to mold. It is particularly suitable for extrusion blow molding because it can prevent or at least mitigate sagging or sagging of the extruded tube.

[0012] JP 2016 218393 A discloses a printer cartridge made of a polyester made from a furandicarboxylic acid with spiro compounds. As a result, the polyester exhibits low temperature fixability, allowing the printer cartridge to withstand increased thermal stress.

[0013] US 2016 / 0167279 A1 describes a preform that enables the production of PEF containers (bottles) with the expected properties, particularly mechanical ones, through an industrial injection-stretch blow molding process. The preform consists of a thermoplastic PEF polymer composed of a 2,5-furandicarboxylic acid (2,5-DCA) monomer and a monoethylene glycol (MEG) monomer.

[0014] JP 2004 035040 A describes a container molded from a copolymer polyester resin consisting of terephthalic acid as the main dicarboxylic acid composition, 80-60 mol% ethylene glycol, and 20-40 mol% spiroglycol composition. The container exhibits high heat resistance, transparency, and impact resistance, is easy to mold, and is suitable for use as a beverage container suitable for high-temperature filling.

[0015] WO 2016 / 174577 A1 discloses a container with an outer layer comprising a bisphenol A polycarbonate and an inner layer comprising a terephthalic acid copolyester or a polyethylene furanoate, or a combination thereof. The inner layer forms a barrier between the outer layer and the interior of the container. The transparency of the container decreases by less than or equal to 5% after sterilization in an autoclave for 30 minutes at 120°C. After 50 cycles of hot filling with water for 30 minutes at 90°C, the transparency decreases by less than or equal to 5%.

[0016] WO 2017 / 093685 A1 relates to a thermoplastic polyester comprising: at least one 1,4:3,6-dianhydrohexitol unit (A); at least one cyclic diol unit (B) other than cyclohexanedimethanol units; 1,4:3,6-dianhydrohexitol units (A) and at least one aromatic carboxylic acid diacid unit (C), wherein the polyester is free of ethylene glycol units. Object of the invention

[0017] The disadvantages of the described prior art give rise to the problem which initiated the present invention of reducing the tendency of crack formation in containers made of polyesters. Description

[0018] Polyester preforms are used to produce a plastic container in a blow molding process. The preform, also known as a preform, is usually formed into a tubular preform body using an injection molding process. It is closed at one longitudinal end and has a neck section with a pouring opening at the other longitudinal end.

[0019] The stated object is achieved with a polyester preform according to claim 1 for producing a plastic container in that the polyester is essentially based on a furandicarboxylic acid and diols, with the diols originating firstly from the group of spiro compounds and secondly from the group of conventional diols. The polyester of the preform therefore essentially consists of a furandicarboxylic acid and a component selected from the group of spiro compounds and conventional diols, and a combination thereof.

[0020] This composition of the polyester surprisingly allows the polyester to be partially bio-based while simultaneously significantly reducing the tendency of the plastic container produced from the preform to crack. This reduction in cracking can be achieved by adding the spiro compound. For the purposes of this application, a spiro compound is understood to be a polycyclic organic compound whose rings are connected at a single atom. The atom at which the neighboring rings are connected is called the spiro atom. The spiro atom acts as a kind of joint between the neighboring rings, allowing the rings to remain flexible and movable relative to one another. By connecting the polyester molecules with the spiro compounds, the polyester molecules possess increased mobility or flexibility. This allows tensions in the molecular structure to be reduced or dampened.

[0021] By incorporating a spiro compound, the ester bond can be protected from nucleophilic attack, in addition to increasing the mobility of the molecular chains, as the spiro compound sterically protects the ester bond. Attack by alkalis, especially their hydroxide ions, which are used in the washing of reusable containers, can therefore be prevented by adding spiro compounds to the polyester.

[0022] The group of conventional diols includes monoethylene glycol, diethylene glycol, propylene glycol, or butylene glycol. The preform can therefore be made from a wide variety of polyesters or copolymers, since a wide range of diols is suitable for reacting with furandicarboxylic acid to form polyester, and the polyester is suitable for incorporating spiro compounds into the polymer structure. According to the invention, the proportion of the spiro compound is at least 1, preferably at least 2 percent by weight, with the weight percentages being based on the total weight of the preform. Even the addition of a small amount of spiro compounds or a spiro-based monomer to the polyester results in a significant improvement in the ESCR.The following test method (Standard ISBT Stress Cracking Test), for example, can be used to determine the ESCR of a polyester container: The container is filled with water so that it contains its nominal volume of water. The container is then pressurized to 77 + / - 0.5 psi (equivalent to 531 ± 4 kPa) and closed. The water level is marked on the container. The container is then placed in a bath of 0.2 wt% caustic soda solution. The caustic soda solution must cover the entire bottom of the container. The time until the container fails is a measure of its stress cracking resistance. Failure can occur due to an explosion of the container or a leak. The leak can be identified by a decrease in the water level in the container or a drop in the internal pressure. The Standard ISBT Stress Cracking Test is particularly suitable for determining the ESCR of plastic polyester bottles.

[0023] A test according to the standard ISBT Stress Cracking Test showed that it takes almost twice as long for a polyester bottle made from polyester mixed with 4% by weight of spiro compounds to fail compared to a polyester bottle containing no spiro compounds. The polyester bottle containing 4% by weight of spiro compounds failed after 70 minutes. A comparison polyester bottle, identical in material and shape except for the spiro compounds, failed after just 40 minutes. This test demonstrates that the addition of spiro compounds makes the polyester bottle more durable and can withstand greater stress in terms of chemical contact, environmental influences, and / or internal pressure.

[0024] In a further preferred embodiment of the invention, the proportion of spiro compounds is between 1 and 35 percent by weight, preferably between 2 and 10 percent by weight, and particularly preferably between 3 and 5 percent by weight, wherein the weight percentages are based on the total weight of the preform. Depending on the expected load on the polyester container produced from the preform, the proportion of spiro compounds can be increased to prevent cracking and the consequent failure of the container. Stress cracking, which, as described above, inevitably occurs during the forming of the preform into the polyester container, can be significantly reduced by providing the spiro compounds.

[0025] In a particularly preferred embodiment, the spiro compound is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (spiroglycol). Other spiro compounds are also excellently suited to sterically protecting the ester bond through their methyl and ethyl groups.

[0026] The special spiro-based polyester is preferably a copolyester based on PEF, PPF, or PBF. The preform or container can therefore also be bio-based and simultaneously exhibit the advantages resulting from the addition of the spiro compounds. It is irrelevant whether the polyester or container is colored, coated, or textured. PPF is the abbreviation for polypropylene furanoate, and PBF is the abbreviation for polybutylene furanoate. The polyester is preferably a copolymer with polyethylene furanoate, polypropylene furanoate, or polybutylene furanoate as the first monomer unit and spirodiol as the second monomer unit.

[0027] It is advantageous if the preform body has a wall thickness between 1 mm and 16 mm. The inclusion of the spiro compound in the polyester allows for the production of even very thick preforms that, despite their thickness, exhibit hardly any crystallization phenomena and do not become cloudy during slow cooling. These preforms are intended for polyester containers that can replace glass containers. This makes it possible to produce polyester containers whose properties match the positive characteristics of glass containers, such as stability and reusability.

[0028] In a further embodiment of the invention, the preform is designed to form a reusable container. The reusable container is resistant to aggressive chemicals that typically have to be used to clean the reusable container for hygienic reasons before it is put back on the market. The spiro compounds protect the ester bonds and prevent them from being weakened by saponification reactions. Such saponification reactions occur, for example, between polyesters and alkalis used in the cleaning of reusable containers.

[0029] Another aspect of the invention relates to a polyester container made from a preform according to the above description, wherein the container comprises a spiro compound and withstands more than 30 minutes of the standard ISBT stress cracking test with a 0.2% alkali solution. These resistance values ​​demonstrate that a polyester container containing spiro compounds can withstand high levels of chemical attack and / or internal pressure. Thus, the polyester container according to the invention not only withstands cleaning with chemicals without cracking—it is also suitable for filling detergents, fragrances, and solvents that attack and destroy conventional polyester containers.

[0030] In a further preferred embodiment of the invention, the container is designed to be refillable or reusable. The chemicals required for cleaning, particularly alkalis, to refill the container do not attack the polyester or attack it only to a limited extent, since the ester bonds of the polyester are protected from chemical attack by the spiro compounds.

[0031] In another particularly preferred embodiment of the invention, the container is designed such that it can withstand an internal pressure after filling of up to 3 bar, preferably up to 5 bar, and particularly preferably up to 12 bar, and is thus suitable for filling carbonated beverages or aerosols. The spiro connections reduce cracking, making the polyester container so stable that it can withstand internal pressures of up to 12 bar. It can therefore not only hold pressurized liquids but can also be designed as an aerosol can. Furthermore, it is suitable for having a filling volume of more than 1.5 liters and for holding a carbonated liquid of more than 1.5 liters.

[0032] The invention is preferably characterized in that the container is designed to withstand temperatures between -19°C and 96°C, making it suitable for filling container contents at temperatures between -19°C and 96°C. The provision of the spiro compound in the polyester also increases the glass transition temperature of the polyester. This makes the container suitable for hot-filling products and for pasteurizing the container contents directly in the container.

[0033] In a method for producing a preform, a mixture of polyester plastic granules is prepared, wherein the polyester is made essentially from a furandicarboxylic acid and diols, and a preform is produced from the mixture by injection molding. According to a further aspect of the invention, a spiro compound is added to the polyester plastic granules during polymerization, or the spiro compound is added to the polyester plastic granules during melting prior to injection molding, and after the addition of the spiro compound, the mixture contains a proportion of the spiro compound of at least 1, preferably at least 2, percent by weight, wherein the percent by weight is based on the total weight of the mixture.

[0034] The required amount of spiro compounds can be copolymerized simply and quickly through transesterification, as no additional process step is required. Rather, the spiro compound can be introduced into a polyester without spirodiols, with a second polyester with a high concentration of spirodiols, through transesterification, and added during existing process steps, namely the polymerization of the polyester or the melting of the plastic granules. It has been shown that the spiro compound forms a homogeneous bond with the polyester during polymerization or melting of the polyester, and the modified polyester can very well meet the functional requirements described above.

[0035] It is advantageous if the spiro compound contains between 1 and 35 percent by weight, preferably between 2 and 10 percent by weight, and particularly preferably between 3 and 5 percent by weight, with the percentages being based on the total weight of the mixture. By selecting the amount of spiro compounds, the required functional properties of the polyester container can be adjusted such that the requirements profile regarding chemical resistance, temperature resistance, and pressure resistance can be met.

[0036] The publication also relates to a copolymer for producing a preform from a polyester, wherein the polyester is produced essentially from a furandicarboxylic acid and diols, and a spiro compound, wherein the proportion of the spiro compound is at least 1, preferably 2, percent by weight, and the weight percentages are based on the total weight of the copolymer. The copolymer therefore preferably comprises polyethylene furanoate, polypropylene furanoate, or polybutylene furanoate as the first monomer units and a spiro compound as a second monomer unit. The functional properties of the preform or polyester container produced from the copolymer can therefore be achieved with a relatively small amount of spiro compounds. To produce the preform mixture, the spiro compound can be added to the polyester during its polymerization or during melting for injection molding of the preform.

[0037] A final aspect of the publication relates to plastic granules for producing a polyester preform, the polyester being made essentially from a furandicarboxylic acid, diols, and a spiro compound, the proportion of the spiro compound being at least 1, preferably 2, percent by weight, and the percent by weight being based on the total weight of the plastic granules. If the plastic granules contain the spiro compounds, they are incorporated into the structure of the polyester during polymerization. The intrinsic viscosity (IV) of the plastic granules is greater than or equal to 0.5 and less than or equal to 1.5 dl / g, measured in analogy to the ASTM D4603 test standard. Measured in analogy to the ASTM D4603 test standard means that the ASTM D4603 test standard, which only applies to PET, is to be applied to a test specimen made essentially from a furandicarboxylic acid, diols, and a spiro compound.Furthermore, the plastic granules are crystalline. The crystallinity of the plastic granules is greater than 20%. Furthermore, the plastic granules do not stick together at a drying temperature greater than or equal to 130°C.

Claims

1. A preform made of a polyester for producing a plastic container in a blow molding process which comprises a tube-like preform body which is closed at its one longitudinal end and at its other longitudinal end has a neck section provided with an opening for pouring, wherein the preform is produced by injection molding, wherein the polyester is based on furandicarboxylic acid and diols, wherein the diols are derived partly from the group of spiro compounds and partly from the group of conventional diols, wherein the group of conventional diols comprises monoethylene glycol, diethylene glycol, propylene glycol or butylene glycol, wherein the proportion of said spiro compound is at least 1, preferably at least 2 percent by weight, the percentages by weight being based on the total weight of the preform.

2. The preform according to claim 1, characterized in that the proportion of said spiro compound is between 1 and 35 percent by weight, preferably between 2 and 10 percent by weight and particularly preferably between 3 and 5 percent by weight, the percentages by weight being based on the total weight of the preform.

3. The preform according to any one of the preceding claims, characterized in that said spiro compound is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (spiroglycol).

4. The preform according to any one of the preceding claims, characterized in that said polyester is a copolyester based on PEF, PPF or PBF.

5. The preform according to any one of the preceding claims, characterized in that the preform body has a wall thickness which is between 1 mm and 16 mm.

6. The preform according to any one of the preceding claims, characterized in that said preform is formed to form a reusable container.

7. The polyester container made of a preform according to any one of the preceding claims, wherein said container has a spiro compound and withstands more than 30 min in the standard ISBT stress cracking test with a 0.2% alkali.

8. The container according to claim 7, characterized in that said container is formed in such a way that it is suitable for refilling or as a reusable bottle.

9. The container according to any one of claims 7 or 8, characterized in that the container is formed in such a way that it withstands an internal pressure after filling of up to 3 bar, preferably up to 5 bar and particularly preferably up to 12 bar and thereby is suitable for the filling of carbonated beverages or aerosols.

10. The container according to any one of claims 7 to 9, characterized in that the container is formed in such a way that it withstands temperatures between -19 °C and 96 °C and thereby is suitable for a filling process of container contents with a temperature between -19 °C and 96 °C.

11. A process for producing a preform, wherein - a mixture of polyester plastic granules is prepared, wherein said polyester is made of a furandicarboxylic acid and diols, wherein the diols are derived partly from the group of spiro compounds and partly from the group of conventional diols, wherein the group of conventional diols comprises monoethylene glycol, diethylene glycol, propylene glycol or butylene glycol, and - a preform is produced by injection molding from said mixture, wherein during the polymerization of the polyester a spiro compound is added to it, or the spiro compound is added to the polyester plastic granules during melting prior to injection molding and the mixture, after the addition of said spiro compound, contains a proportion of the spiro compound of at least 1, preferably at least 2 percent by weight, the percentages by weight being based on the total weight the mixture.

12. The process according to claim 11, characterized in that the proportion of said spiro compound contains between 1 and 35 percent by weight, preferably between 2 and 10 percent by weight and particularly preferably between 3 and 5 percent by weight, the percentages by weight being based on the total weight of the mixture.