METHOD FOR PRODUCING A DEFECTIVE TEST COMPONENT BY LASER BEAM MELTING

DE502021005388D1Active Publication Date: 2024-10-31ARIANEGRP GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005388
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-07
Filing Date
2021-04-28
Publication Date
2024-10-31
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

Laser beam melting processes often result in defects such as pores, cracks, and bonding issues due to factors like laser beam attenuation, heat dissipation problems, and process by-products, which affect the mechanical properties of produced components.

Method used

A method to produce a defective test component by laser beam melting that replicates the process conditions of real manufacturing, identifying and targeting defect-prone areas using a process monitoring system to ensure the test component exhibits similar defects, allowing for effective investigation of their impact on mechanical properties.

Benefits of technology

Enables the production of a test component with defects comparable to production components, facilitating the transfer of defect investigation results to improve manufacturing quality and mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing a defective sample component by laser beam melting.

[0002] In laser beam melting, a generative layer-by-layer construction process for producing three-dimensional workpieces, a raw material powder is applied layer by layer to a build platform arranged in a process chamber and, depending on the desired geometry of the workpiece to be created, is exposed to laser radiation at specific locations by an irradiation device. The radiation penetrating the powder layer causes heating and, consequently, fusion and / or sintering of the raw material powder particles. The process chamber is usually sealed from the ambient atmosphere and is flowed through by a gas stream. This serves, on the one hand, to maintain a controlled protective gas atmosphere within the process chamber and, on the other hand, to transport process by-products such as weld spatter, welding fume particles, or soot particles from the irradiation zone and, if possible, to deposit them outside the workpiece to be created.

[0003] Various defects can occur in components manufactured by laser beam melting, such as pores, cracks, or bond layer defects, i.e., defects resulting from a lack of bonding between component layers. These defects can be caused by, for example, attenuation of the laser beam by process gases, a geometry-related lack of heat dissipation through the component, an unfavorable exposure strategy, or influences from the powder and process byproducts.

[0004] In order to investigate the influence of potential defects on the components to be manufactured and in particular their mechanical properties, it is known, for example from Gong H., "Generation and detection of defects in metallic parts fabricated by selective laser melting and electron beam melting and their effects on mechanical properties", 2013, that defective fatigue specimens can be produced by incorporating targeted defects in the 3D model.

[0005] US 2013 / 314504 A1 describes a method for quality assessment of a product produced by means of a generative laser sintering and / or laser melting process.

[0006] Component for an aircraft engine. First, a first data set is provided, which comprises spatially resolved color values ​​that each characterize the temperature of the component at an assigned component location during laser sintering and / or laser melting of the component. Furthermore, a second data set is provided, which comprises spatially resolved color values ​​corresponding to the first data set, each characterizing the temperature of a reference component at an assigned reference component location during laser sintering and / or laser melting of the reference component. Finally, a difference between the first data set and the second data set is determined, and the quality of the component is determined based on the difference between the first data set and the second data set.

[0007] US 2019 / 293550 A1 describes a method for imaging a three-dimensional component manufactured using a generative manufacturing process. In this method, at least two layer images of the component are acquired during its production using a detection device configured to capture a measured variable characterizing an energy input into the component with spatial resolution. By stacking the individual layer images, a three-dimensional image of the component is obtained that characterizes the energy input at each measured point of the component. Displaying this image ultimately enables monitoring and assessment of the component's manufacturing quality.

[0008] The invention is directed to the object of specifying a method for producing a defective sample component by laser beam melting under process conditions that are as close as possible to the process conditions in the actual manufacturing process of production components.

[0009] This object is achieved by a method having the features of claim 1. Preferred embodiments of the method are described in the dependent claims.

[0010] In a method for producing a defective sample component by laser beam melting, an analysis component is first produced by laser beam melting in a first construction process in which a plurality of raw material powder layers are successively applied to a construction platform and are irradiated with laser radiation in a location-selective manner depending on the desired geometry of the analysis component. The raw material powder can, for example, be a powder or a powder mixture made of metal, a metal alloy, ceramic or plastic. A metallic raw material powder preferably has particle sizes in the range of 15 to 45 µm. In contrast, larger particles are generally processed when laser beam melting plastic powders. To apply the raw material powder to the construction platform, a powder application device can be used, for example, which is parallel to a surface of the construction platform, i.e.is preferably movable back and forth horizontally over the surface of the build platform.

[0011] The site-selective irradiation and subsequent solidification of the raw material powder layers can be carried out, for example, by a suitable irradiation device based on CAD data of the component to be produced. The irradiation device can comprise a radiation source, e.g., in the form of a diode-pumped ytterbium fiber laser, which emits laser light with a wavelength of approximately 1060 to 1080 nm, and in particular, e.g., 1064 nm. Furthermore, the irradiation device can comprise an optical unit for directing and processing the laser beam emitted by the radiation source, which can be embodied, for example, in the form of a scanner.

[0012] The build platform is preferably arranged in a process chamber that is sealable from the ambient atmosphere. The build platform is preferably vertically movable, so that as the build height of a component built layer by layer on the build platform increases, the build platform can be moved step by step vertically downward into a build chamber. After completion of the build process, the manufactured component is completely housed in the build chamber and embedded in raw material powder that was applied to the build platform during the build process but not irradiated.

[0013] During the production of the analysis component, a process monitoring system records at least one process parameter that is characteristic of the occurrence of component defects. Component defects can be, for example, pores, cracks, or bond layer defects. Based on the result of the process parameter recording, a defect-prone area of ​​the build platform is identified where an increased occurrence of component defects is to be expected. The defect-prone area of ​​the build platform can be a contiguous section or area of ​​the build platform. However, it is also conceivable that the defect-prone area of ​​the build platform is composed of several separately formed sections of the build platform.

[0014] In a second build process, at least one defective sample component is then produced by laser beam melting. A plurality of layers of raw material powder are successively applied to the build platform and are then selectively irradiated with laser radiation, at least in the defect-prone area of ​​the build platform, depending on the desired geometry of the at least one defective sample component. The at least one defective sample component is thus built in the defect-prone area of ​​the build platform under process conditions that correspond to the process conditions in the actual manufacturing process for production components, increasing the probability that the sample component actually has one or more component defects. This eliminates the need to "artificially" impart defects to the sample component.Furthermore, the process of defect formation in the test component is comparable to the process of defect formation in a production component.

[0015] The process described here can therefore produce a defective sample component that is optimally comparable to a defective production component. Investigations into the effects of defects in the sample component, for example, on the mechanical properties of the sample component, can thus be particularly well transferred to production components.

[0016] In a preferred embodiment of the method for producing a defective sample component, the process monitoring system detects the at least one process parameter as a function of a location in the analysis component. The process parameter is thus detected as a function of a location in the analysis component, which can be defined, for example, by corresponding location coordinates, in the planes of the individual layers of the analysis component parallel to a surface of the build platform.

[0017] To identify the defect-prone area of ​​the build platform, process parameter values ​​recorded at a location within the analysis component can be projected onto a plane corresponding to the surface of the build platform. This allows, for example, critical process parameter values ​​that indicate the development of defects and are measured in multiple superimposed layers of the analysis component to be accumulated in the plane corresponding to the surface of the build platform, enabling reliable identification of the defect-prone area of ​​the build platform.

[0018] A region of the build platform is preferably identified as a defect-prone region of the build platform if, upon irradiation of this region of the build platform with laser radiation, the process parameter recorded by the process monitoring system falls below or exceeds a target value. The target value preferably indicates a value of the process parameter at which good component quality, i.e., a substantially defect-free component structure, can be expected. In principle, it is conceivable to identify all sections of the build platform in which the process parameter falls below or exceeds the target value as a defect-prone region.However, it is also possible to define a certain tolerance range around the target value, so that a section of the build platform is only assigned to the defect-prone area of ​​the build platform if the process parameter in this section of the build platform falls below or exceeds the target value by a certain amount defined by the tolerance range.

[0019] In principle, it is conceivable to define the target value of the process parameter, which serves as the basis for identifying the defect-prone area of ​​the build platform, before the analysis component is created. However, the target value of the process parameter is preferably an average value of the process parameter, which is determined by averaging the process parameter values ​​recorded during the creation of the analysis component using the process monitoring system. With this approach, those sections of the build platform in which deviations of the process parameter from its average value occur are identified as defect-prone areas.

[0020] In a preferred embodiment of the method for producing a defective sample component, at least 50%, in particular at least 60%, preferably at least 70%, particularly preferably at least 80%, and particularly preferably at least 90% of the surface of the build platform is irradiated with laser radiation in a location-selective manner during the production of the analysis component in at least some of the raw material powder layers. Thus, an analysis component is preferably constructed whose cross-sectional area, in at least some of its layers, occupies at least 50%, in particular at least 60%, preferably at least 70%, particularly preferably at least 80%, and particularly preferably at least 90% of the surface of the build platform.If desired, an analysis component can also be constructed whose shape is at least partially adapted to the shape of the build platform and has a cross-sectional area in at least some of its layers, preferably in all layers, that corresponds to the surface of the build platform.

[0021] This ensures that, during the creation of the analysis component, the process parameters characteristic of the occurrence of component defects can be recorded over the largest possible area of ​​the build platform. The defect-prone area of ​​the build platform can then be identified with particular reliability.

[0022] As the process parameter characteristic for the occurrence of component defects, a process parameter is preferably recorded that is characteristic of a temperature of an area of ​​a raw material powder layer irradiated with laser radiation. In particular, a value of the process parameter that is above a target value, which indicates that a temperature of an area of ​​a raw material powder layer irradiated with laser radiation is above a target temperature, can be interpreted as an indication that the area of ​​the build platform in which the increased process parameter value or the increased temperature is recorded is to be classified as a defect-prone area of ​​the build platform.An increased temperature can occur in an area of ​​the build platform, for example, if there is a disruption of the gas flow in this area of ​​the build platform, which serves, on the one hand, to maintain a controlled protective gas atmosphere within the process chamber and, on the other hand, to transport process by-products such as welding spatter, welding fume particles or soot particles out of the irradiation zone and, if possible, to deposit them outside the workpiece to be created.

[0023] An area of ​​the build platform in which an elevated process parameter value or an elevated temperature occurs and which is therefore classified as a defect-prone area of ​​the build platform is often also an area of ​​the build platform in which a reduced flow velocity of the gas stream flowing through the process chamber is present. A reduction in the flow velocity of the gas stream flowing through the process chamber is often observed, for example, in the area of ​​a gas outlet of the process chamber. In this case, an area of ​​the build platform adjacent to the gas outlet of the process chamber is identified as a defect-prone area of ​​the build platform.

[0024] The process parameter characteristic of a temperature in a region of a raw material powder layer irradiated with laser radiation is preferably detected by detecting an emission of infrared radiation in the region of the raw material powder layer irradiated with laser radiation. In particular, an emission of radiation, and in particular a radiation intensity in the near infrared range, can be detected and used as the process parameter characteristic of a temperature in the region of the raw material powder layer irradiated with laser radiation. The infrared radiation can be detected, for example, using a high-resolution camera.

[0025] An optical tomography system, for example, can be used as a process monitoring system to detect the process parameters characteristic of the occurrence of component defects. Using a high-resolution camera, the optical tomography system can detect the radiation emission, particularly the radiation intensity in the near-infrared range, in an area of ​​a raw material powder layer irradiated with laser radiation. This can then be used to draw conclusions about the temperature in the area of ​​the raw material powder layer irradiated with laser radiation. The recorded radiation intensity and / or temperature values ​​can then be projected onto a plane corresponding to a surface of the build platform.Furthermore, a graphical representation can be generated in which increased radiation intensity and / or temperature values ​​are color-coded, so that in the graphical representation an area of ​​the build platform in which increased radiation intensities and / or temperatures were measured is color-coded and can therefore be easily identified as a defect-prone area of ​​the build platform.

[0026] In one variant of the method for producing a defective test component, during the production of the test component in the defect-prone area of ​​the build platform, at least 50%, in particular at least 60%, preferably at least 70%, particularly preferably at least 80%, and particularly preferably at least 90% of the area of ​​a region of the build platform lying outside the defect-prone area of ​​the build platform is location-selectively irradiated with laser radiation in at least some of the raw material powder layers. During the construction of the at least one defective test component, therefore, preferably not only the defect-prone area of ​​the build platform is location-selectively irradiated with laser radiation, but also a significant portion of the area of ​​the area of ​​the build platform lying outside the defect-prone area of ​​the build platform.If desired, during the construction of the at least one defective test component, a total area corresponding at least approximately to the surface of the construction platform can be irradiated in at least part of the raw material powder layers, preferably in all layers.

[0027] This ensures that sufficient weld spatter, welding fume particles, and soot particles are generated during the construction of at least one defective sample component to cause the desired defects in the sample component. Furthermore, the probability is increased that contaminants carried away by the gas flow flowing through the process chamber from the immediate irradiation zone will be deposited on one area of ​​the component rather than outside it. This allows the process conditions prevailing during the construction of large components to be simulated particularly realistically.

[0028] A final sample component can be produced from the at least one defective sample component produced by laser beam melting through machining. For example, the defective sample component produced by laser beam melting can be brought into its final desired shape by milling or grinding.

[0029] Alternatively, however, it is also conceivable for the at least one defective sample component to be produced in the form of a final contour sample component. An additional forming process to produce the final contour of the defective sample component can then be dispensed with. Preferably, surface finishing of the defective sample component can then also be dispensed with.

[0030] In the defect-prone area of ​​the build platform, a plurality of defective test components can also be created. The defective test components are then preferably separated from each other by a gap, so that the defective test components can subsequently be easily separated from each other.

[0031] The gap between adjacent defective test components can have a width of approximately 0.15 mm to approximately 0.35 mm, in particular a width of approximately 0.2 mm to approximately 0.3 mm and preferably a width of approximately 0.25 mm.

[0032] In the following, the invention is described in more detail with reference to the attached schematic figures, in which: Figure 1 shows a schematic representation of a build platform for producing a component by laser beam melting; Figure 2 shows a graphic representation obtained by projecting process parameter values ​​acquired by a process monitoring system during the production of an analysis component into a plane corresponding to a surface of the build platform; and Figure 3 shows a plurality of sample components produced by the method according to the invention.

[0033] Figure 1shows a top view of a construction platform 10, as is typically used in a machine for manufacturing components by laser beam melting. The construction platform 10 is arranged in a process chamber 12, which can be sealed against the ambient atmosphere. An inert gas, for example argon or the like, is supplied to the process chamber 12 via a gas inlet 14. The inert gas fed into the process chamber 12 via the gas inlet 14 flows over the construction platform 10 in a direction that is Figure 1 indicated by the arrows. The inert gas is discharged from the process chamber 12 via a gas outlet 16.

[0034] The construction platform 10 is mounted by means of a Figure 1A powder application device (not shown) which is movable back and forth in a horizontal direction parallel to a surface of the construction platform 10 over the surface of the construction platform 10 is used to apply a raw material powder layer by layer. The raw material powder can be, for example, a powder or a powder mixture of metal, a metal alloy, ceramic or plastic, wherein the raw material powder usually has particle sizes in the range of <100 µm. The raw material powder layers are applied by means of a Figure 1 also not shown, which comprises a radiation source in the form of a laser radiation source and a scanner for directing and processing the laser beam emitted by the radiation source, is subjected to laser radiation in a location-selective manner.

[0035] The radiation penetrating the raw material powder layer causes heating and consequently a fusion and / or sintering of the raw material powder particles. The location-selective irradiation and subsequent solidification of the raw material powder layers can be carried out, for example, using CAD data of a component B to be produced. The build platform 10 is movable in the vertical direction, so that with increasing construction height of the component B built up layer by layer on the build platform 10, the build platform can be moved step by step in the vertical direction downwards into a build chamber (also not shown). After completion of the construction process, the component B is completely received in the build chamber 10 and embedded in raw material powder that was applied to the build platform 10 during the construction process but was not irradiated.

[0036] The irradiation of the raw material powder layers is usually carried out according to a predetermined irradiation pattern. For example, the movement of the laser beam over the raw material powder layers follows scan vectors S, where the scan vectors S, as shown in Figure 1 shown, can define a stripe pattern with a plurality of mutually adjacent stripes M. In a stripe M of the stripe pattern, mutually adjacent scan vectors S are, for example, aligned opposite to each other. A hatch angle h, which is determined by a scan vector S and an x-axis of a coordinate system defined in a plane of the surface of the construction platform 10, is in the illustration according to Figure 1 approx. 45°. Figure 1 However, it only illustrates one example of a conceivable irradiation pattern.

[0037] The gas flow conducted through the process chamber 12 serves, on the one hand, to maintain a controlled protective gas atmosphere within the process chamber 12. On the other hand, the gas flow carries process byproducts, such as weld spatter, welding fume particles, or soot particles, out of the irradiation zone and deposits them, if possible, outside the component B to be produced. The removal of contaminants from the irradiation zone is facilitated if the irradiation direction, i.e., the orientation of the scan vectors S, and the gas flow direction, are different. Furthermore, a specific flow velocity of the gas flow conducted through the process chamber 12 is required for reliable removal of contaminants from the irradiation zone.A disturbed gas flow and in particular a reduced flow velocity of the gas flow conducted through the process chamber 12 can result in impurities such as welding spatter, welding fume particles or soot particles that arise during the irradiation of the raw material powder and cannot be transported out of the irradiation zone as desired. This can lead to an undesired attenuation of the laser beam. Furthermore, an excessively low gas flow velocity can result in impurity particles being deposited on component B rather than outside the component being built. Particles that are not transported away as desired are covered with raw material powder when the next raw material powder layer is applied and melted together with the raw material powder. These effects can lead to the formation of defects such as pores, cracks or bond layer defects in the component produced by laser beam melting.

[0038] In order to investigate the influence of defects on the properties, especially the mechanical properties, of components manufactured by laser beam melting, defective sample components must be created. The process described below allows the creation of a defective sample component under process conditions that are as close as possible to the process conditions in the actual manufacturing process for production components.

[0039] In the method described here for producing a defective sample component by laser beam melting, an analysis component is first produced by laser beam melting in a first construction process in which a plurality of raw material powder layers are successively applied to the construction platform 10 and are irradiated with laser radiation in a location-selective manner depending on the desired geometry of the analysis component.

[0040] In particular, during the production of the analysis component, at least 50%, in particular at least 60%, preferably at least 70%, particularly preferably at least 80%, and particularly preferably at least 90% of the surface of the build platform 10 is irradiated with laser radiation in a location-selective manner in at least some of the raw material powder layers. Consequently, a cross-sectional area of ​​the analysis component occupies at least 50%, in particular at least 60%, preferably at least 70%, particularly preferably at least 80%, and particularly preferably at least 90% of the surface of the build platform 10 in at least some of its layers. Preferably, an analysis component is constructed whose shape is adapted to the shape of the build platform 10 and has a cross-sectional area in all layers that corresponds to the surface of the build platform 10.

[0041] During the production of the analysis component, at least one process parameter characteristic of the occurrence of component defects is recorded by means of a process monitoring system 18, which here is embodied in the form of an optical tomography system. In particular, the process monitoring system 18 records the at least one process parameter as a function of a location in the analysis component, which is defined by corresponding location coordinates in the planes of the individual layers of the analysis component parallel to the surface of the build platform 10.

[0042] Based on the result of the process parameter recording, a defect-prone area 20 of the build platform 10 is identified, in which an increased occurrence of component defects is to be expected. Figure 1In the illustrated build platform 10, the defect-prone region 20 of the build platform 10 is located adjacent to the gas outlet 16 and in side regions of the build platform 10 in a half of the build platform 10 facing the gas inlet 14. In the embodiment shown here, the defect-prone region 20 of the build platform 10 comprises several separately formed sections. However, the defect-prone region 20 of the build platform 10 can also be formed by a single, contiguous section of the build platform 10.

[0043] To identify the defect-prone area 20 of the construction platform 10, the process parameter values ​​recorded as a function of a location in the analysis component are projected into a plane corresponding to a surface of the construction platform 10. A corresponding graphical representation showing such a projection of process parameter values ​​recorded by a process monitoring system 18 during the production of the analysis component into a plane corresponding to a surface of the construction platform 10 is shown in Figure 2 In this representation, critical process parameter values ​​that indicate the formation of defects and are measured in several superimposed layers of the analysis component can be accumulated in the plane corresponding to the surface of the build platform 10.

[0044] In the representation output by the process monitoring system 18 according to Figure 2The critical process parameter values ​​are illustrated by the points P, which occur in clusters adjacent to the gas outlet 16 as well as in side areas of the construction platform 10 in a half of the construction platform 10 facing the gas inlet 14 and thereby identify these sections of the construction platform as a defect-prone area 20 of the construction platform 10. It is understood that the graphic representation according to Figure 2 can also be output in color, so that critical process parameter values ​​can be displayed in an easily recognizable signal color, such as red. This enables particularly simple and reliable identification of the defect-prone area 20 of the build platform 10.

[0045] In the representation according to Figure 2The measured process parameter values ​​are then displayed as critical process parameter values, for example, in a corresponding color, if the process parameter detected by the process monitoring system 18 falls below or exceeds a setpoint. The setpoint of the process parameter is an average value of the process parameter, which is obtained by averaging the values ​​of the process parameter detected during the production of the analysis component using the process monitoring system 18. The values ​​displayed in accordance with Figure 2The points P illustrated thus indicate in which areas of the build platform 10 deviations of the process parameter from its mean value occur particularly frequently. Consequently, an area of ​​the build platform 10 is identified as a defect-prone area 20 of the build platform 10 if, upon irradiation of this area of ​​the build platform 10 with laser radiation, the process parameter detected by the process monitoring system 18 falls below or exceeds a target value, wherein the target value in the exemplary embodiment described here is the mean value of the process parameter values ​​measured during the production of the analysis component.

[0046] The process monitoring system 18, which in the exemplary embodiment described here is designed in the form of an optical tomography system, detects, as the process parameter characteristic of the occurrence of component defects, a process parameter that is characteristic of a temperature of a region of a raw material powder layer irradiated with laser radiation. For this purpose, the optical tomography system is equipped with a high-resolution camera that is capable of detecting the emission of radiation and, in particular, a radiation intensity in the near infrared range in the region of the raw material powder layer irradiated with laser radiation. The temperature in the irradiation zone, i.e., in the region of the raw material powder layer irradiated with laser radiation, can be determined from the measured radiation emissions.

[0047] It has been shown that the above-described disturbances in the gas flow conducted through the process chamber 12 lead to an elevated temperature occurring in the area of ​​the raw material powder layer irradiated with laser radiation. Temperature deviations from the target temperature, and in particular temperatures above the target temperature, can therefore be interpreted as an indication that the area of ​​the build platform 10 in which the elevated temperature is measured should be classified as a defect-prone area 20 of the build platform 10.

[0048] After identifying the defect-prone area 20 of the build platform 10, at least one defective sample component 22 is produced by laser beam melting in a second build process. A plurality of raw material powder layers are successively applied to the build platform 10 and are irradiated with laser radiation in a location-selective manner, at least in the defect-prone area 20 of the build platform 10, depending on the desired geometry of the at least one defective sample component. Due to its construction in the defect-prone area 20 of the build platform 10, there is an increased probability that a defect will occur in the sample component 22, so that the sample component 22 can subsequently be used to investigate the influence of this defect on its properties, and in particular its mechanical properties.

[0049] During the production of the defective sample component 22, at least 50%, in particular at least 60%, preferably at least 70%, particularly preferably at least 80%, and particularly preferably at least 90% of the area of ​​a region of the build platform 10 located outside the defect-prone region 20 of the build platform is selectively irradiated with laser radiation in at least some of the raw material powder layers and preferably in all raw material powder layers. This ensures that sufficient welding spatter, welding fume particles, and soot particles are generated during the construction of the at least one defective sample component 22 to cause the desired defects in the sample component 22.

[0050] A final test component can be produced from the defective test component 22 by machining, such as milling or grinding. Alternatively, however, it is also conceivable for the defective test component 22 to be produced in the form of a final contour test component, which can dispense with subsequent machining and / or surface finishing.

[0051] Furthermore, as shown in Figure 3, a plurality of defective sample components 22 can also be produced, each separated from one another by a gap 24 so that the defective sample components 22 can be easily separated from one another. The gap between adjacent defective sample components can have a width of approximately 0.15 mm to approximately 0.35 mm, in particular a width of approximately 0.2 mm to approximately 0.3 mm, and preferably a width of approximately 0.25 mm.

[0052] In addition to the defective sample components 22 that were constructed in the defect-prone area 20 of the build platform 10, Figure 3 also shows further sample components 26 that were constructed in an area of ​​the build platform 10 that is not attributable to the defect-prone area 20. It can therefore be assumed that the further sample components 26 are less likely to have component defects than the defective sample components 22. The further sample components 26 can then be used, for example, as comparison samples.

Claims

1. A method for producing a defective test component (22) by laser beam melting, wherein i) in a first building process, an analysis component is produced by laser beam melting by successively applying a plurality of raw material powder layers to a building platform (10) and irradiating them site-selectively with laser radiation in dependence on the desired geometry of the analysis component; ii) during the production of the analysis component, at least one process parameter which is characteristic of the occurrence of component defects is detected by means of a process monitoring system (18); iii) a defect-prone region (20) of the building platform (10) in which an increased occurrence of component defects is to be expected is identified on the basis of the result of the detection of the process parameter; and iv) in a second building process, at least one defective test component (22) is produced by laser beam melting by successively applying a plurality of raw material powder layers to the building platform (10) and irradiating them site-selectively with laser radiation at least in the defect-prone region (20) of the building platform (10) in dependence on the desired geometry of the at least one defective test component (22).

2. The method according to claim 1, wherein the process monitoring system (18) detects the at least one process parameter in dependence on a location in the analysis component.

3. The method according to claim 2, wherein, for identifying the defect-prone region (20) of the building platform (10), values of the process parameter detected in dependence on a location in the analysis component, are projected into a plane corresponding to a surface of the building platform (10).

4. The method according to any one of claims 1 to 3, wherein a region of the building platform (10) is identified as a defect-prone region (20) of the building platform (10) if, upon irradiation said region of the building platform (10) with laser radiation, the process parameter detected by the process monitoring system (18) falls below or exceeds a set value.

5. The method according to claim 4, wherein an average value of the process parameter, which is obtained by averaging the values of the process parameter detected during the production of the analysis component with the aid of the process monitoring system (18), is used as the set value of the process parameter.

6. The method according to any one of claims 1 to 5, wherein upon the production of the analysis component, in at least some of the raw material powder layers, at least 50%, in particular at least 60%, preferably at least 70%, more preferably at least 80% and particularly preferably at least 90% of the area of the building platform (10) is irradiated site-selectively with laser radiation.

7. The method according to any one of claims 1 to 6, wherein the process parameter which is characteristic for the occurrence of component defects is a process parameter which is characteristic for a temperature of an region of a raw material powder layer which is irradiated with laser radiation.

8. The method according to claim 7, wherein the detection of the process parameter characteristic of a temperature of a region of a raw material powder layer which irradiated with laser radiation is carried out on the basis of the detection of an emission of infrared radiation in the region of the raw material powder layer which is irradiated with laser radiation.

9. The method according to any one of claims 1 to 8, wherein an optical tomography system is used as the process monitoring system (18) for detecting the process parameter which is characteristic for the occurrence of component defects.

10. The method according to any one of claims 1 to 9, wherein upon the production of the defective test component (22) in the defect-prone region (20) of the building platform (10), in at least some of the raw material powder layers, at least 50%, in particular at least 60%, preferably at least 70%, more preferably at least 80% and particularly preferably at least 90% of the area of a region of the building platform (10) lying outside the defect-prone region (20) of the building platform (10) is irradiated site-selectively with laser radiation.

11. The method according to any one of claims 1 to 10, wherein a final test component is produced from the at least one defective test component (22) by machining.

12. The method according to any one of claims 1 to 10, wherein the at least one defective test component (22) is produced in the form of a final contour test component that does not require surface finishing.

13. The method according to any one of claims 1 to 12, wherein in the defect-prone region (20) of the building platform (10), a plurality of defective test components (22) are produced, which are separated from each other by a gap (24).

14. The method according to claim 13, wherein the gap between mutually adjacent defective test components (22) has a width of approximately 0.15 mm to approximately 0.35 mm, in particular a width of approximately 0.2 mm to approximately 0.3 mm and preferably a width of approximately 0.25 mm.