MANUFACTURING METHOD OF CATALYST-COATED MEMBRANES
Patent Information
- Application Number
- DE502021005585
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-29
- Filing Date
- 2021-09-29
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-09-29
AI Technical Summary
Existing methods for producing catalyst-coated membranes for fuel cells and electrolyzers are time-consuming, costly, and unable to create nanostructured mesoporous catalyst layers, which are known to have higher mass activity but are not accessible due to the use of binders that block catalytically active centers and reduce electrical conductivity.
A method involving a glass-ceramic substrate for synthesizing a mesoporous catalyst layer, which is then transferred to a polymer membrane using thermal treatment, avoiding the use of binders and maintaining the mesoporous structure, allowing for improved catalytic activity and mechanical adhesion.
This method enables the rapid, reproducible, and economical production of catalyst-coated membranes with enhanced catalytic activity by transferring a binder-free, nanostructured mesoporous catalyst layer onto a polymer membrane, improving both proton and electrical conductivity.
Description
Technical area
[0001] The invention relates to a method for producing a catalyst-coated polymer membrane for an electrolyzer and / or a fuel cell, according to claim 1. In a first step, the method preferably comprises providing a glass-ceramic substrate. Subsequently, a mesoporous catalyst layer is preferably synthesized on the glass-ceramic substrate. In a subsequent step, a polymer membrane is preferably pressed onto the glass-ceramic substrate coated with the catalyst layer at a first temperature T 1 . This results in a sandwich structure. In a final process step, the sandwich structure is separated, whereby the catalyst layer is separated from the glass-ceramic substrate and adheres to the polymer membrane.
[0002] Furthermore, the invention relates to a polymer membrane according to claim 13, which was produced by the method of the type mentioned at the outset, as well as to an electrolyzer or a fuel cell according to claim 14, with such a polymer membrane. Background and state of the art
[0003] Fuel cells and electrolyzer cells consist of electrodes separated by an electrolyte (ion conductor). The electrolyte can consist of a semipermeable membrane that is permeable only to one type of ion, such as protons. In electrolyzer cells and fuel cells with proton-conducting membranes (PEMs), catalyst-coated gas diffusion layers (CCGs) and, above all, catalyst-coated membranes (CCMs), also known as membrane-electrode assemblies (MEAs), are used.
[0004] To produce a catalyst-coated membrane, electrocatalytically active catalyst layers are applied to proton-conducting membranes (Nafion, Aquivion). These are typically contacted with gas diffusion layers and assembled in a cell.
[0005] Furthermore, methods are known from the prior art (US 7972743 B2 and JP 2003211063 A) that enable the application of catalyst layers to a membrane via direct coating processes (blading, screen printing, or spraying). In these processes, catalysts are dispersed with an ionomer, which acts as an ion conductor and binder, to form an ink and then applied to the membrane.
[0006] The production of a catalyst-coated membrane using a coating known from the prior art, especially a homogeneous spray coating, is disadvantageously time-consuming and not reproducible with manual preparation. While production with a robot, preferably a spray robot, leads to more consistent results, it is costly.
[0007] In addition, indirect methods for applying a catalyst layer to a membrane are known.
[0008] For example, US20020136940 A1 discloses a so-called decal process. In this process, a catalyst is applied to a transfer medium (Teflon) and transferred from this transfer medium to the ion-conducting membrane via a hot-pressing step.
[0009] Documents US5879828 A and US6040077 A also disclose an indirect method, using a polymer (polyimide) substrate as the transfer medium. In these disclosures, the catalyst material is applied to the transfer medium and then pressed onto a Nafion membrane. The product obtained is a membrane comprising a catalyst layer.
[0010] US 2018 / 323459 A1 discloses a method for producing a catalyst-coated membrane assembly for a solid polymer electrolyte fuel cell. A cathode catalyst ink is applied to a support medium and then dried, thereby forming a cathode catalyst layer on the support medium. In a subsequent step, a membrane ionomer solution is applied to the surface of the cathode catalyst layer. While the ionomer solution coating is still wet, a layer of e-PTFE (expanded PTFE) is applied to the surface of the coated ionomer solution in a wet lamination step. This assembly is then dried and annealed in a drying and annealing step, completing the production of the e-PTFE-reinforced electrolyte membrane.Subsequently, the anode catalyst ink is applied to the surface of the section of e-PTFE layer via the web coating step. As before, this coating is dried in a drying step. Finally, the carrier medium is peeled off in a removal step.
[0011] The cathode catalyst ink used (commonly referred to as "ink") typically contains a binder. While a binder can achieve high proton conductivity, it also disadvantageously reduces the electrical conductivity of the catalyst layer and blocks catalytically active sites. In "ink"-based routes, the binder is typically added in excess to achieve sufficient mechanical strength or structural integrity, whereby achieving an optimum between electrical and proton conductivity is not possible.
[0012] The known methods (both direct and indirect methods) for producing a catalyst-coated membrane also have the disadvantage of not allowing nanostructured mesoporous catalyst layers on polymer membranes. However, such layers, in particular, offer significant advantages. It has been shown that, on a half-cell scale, mesoporously templated catalyst layers exhibit a significantly higher mass activity of the electrochemically active species than comparable conventional catalyst layers produced, for example, using an ink-based method.
[0013] The use of nanostructured mesoporous catalyst layers on polymer membranes in real environments is not known from the state of the art. Object of the invention
[0014] The object of the invention was therefore to eliminate the disadvantages of the prior art and to provide a polymer membrane with a nanostructured mesoporous catalyst layer and in particular a method for producing such a polymer membrane. Summary of the invention
[0015] The object of the invention is achieved by the features of the independent claims. Advantageous embodiments of the invention are described in the dependent claims.
[0016] In a preferred embodiment, the description relates to a method for producing a catalyst-coated polymer membrane for an electrolyzer and / or a fuel cell comprising the following steps: a) providing a glass-ceramic substrate; b) synthesizing a mesoporous catalyst layer on the glass-ceramic substrate; c) pressing a polymer membrane onto the glass-ceramic substrate coated with the catalyst layer at a first temperature T 1 , thereby producing a sandwich structure; d) separating the sandwich structure, wherein the catalyst layer is separated from the glass-ceramic substrate and adheres to the polymer membrane.
[0017] In order to transfer high-performance catalyst layers (nanostructured mesoporous catalyst layers) into a PEM electrolyzer, a process had to be developed that enabled the application of a mesoporous layer to the polymer membrane. The inventors faced various challenges in developing the preferred process and had to solve them with a high degree of inventiveness.
[0018] For example, the polymer membrane cannot be directly coated with the mesoporous catalyst, as the synthesis of a mesoporous templated catalyst layer requires thermal treatment, which would destroy the polymer membrane. Therefore, a method had to be found to synthesize an intact catalyst layer and then transfer it to the polymer membrane without damaging it. Furthermore, because the catalyst layer is highly porous, it is very fragile; therefore, it must be created on a rigid substrate and thermally treated.
[0019] The thermal treatment for synthesizing a catalyst layer is considered a significant departure from the state of the art. As described above, the prior art does not yet use catalyst layers that can be produced by thermal treatment to produce a catalyst-coated polymer membrane. On the contrary, the carbon-based substrates made of ETFE, FEP, PFA, and ECTFE disclosed in the prior art undergo morphological and textural changes at temperatures ranging from -200 to 330 °C (melting point: PTFE (327 °C); ETFE (265-275 °C); FEP (260 °C); PFA (310 °C); and ECTFE (220 to 227 °C). Glass-ceramic substrates or silicon, in contrast, are "stable" at significantly higher temperatures (temperature resistance of glass fiber carbon in inert gas or vacuum: up to 3000 °C).In this respect, glass-ceramic substrates can be used advantageously compared to other rigid materials, since a higher temperature range can be used during thermal treatment for synthesis.
[0020] The combination of the present process steps leads to a surprising synergistic effect, which results in the advantageous properties and the associated overall success of the invention, with the individual features interacting with each other. Another important advantage of the process according to the invention is the extremely rapid, reproducible, and economical synthesis procedure.
[0021] In other words, the description preferably relates to the compression of a catalyst layer synthesized on a suitable substrate by thermal treatment onto a polymer membrane. Or, more preferably, in other words, the compression of a mesoporous-templated, binder-free catalyst layer synthesized on a suitable substrate by thermal treatment onto a polymer membrane.
[0022] Furthermore, the substrate used had to ensure that the resulting catalyst layer could be transferred to a membrane without damage. Surprisingly, a glass-ceramic substrate was particularly well-suited for this purpose. By using a glass-ceramic substrate to synthesize an easily removable, yet stable, mesoporous layer, the layer can be advantageously pressed onto a polymer membrane without the use of a binder. Avoiding the binder advantageously leads to increased activity in a layer serving as a catalyst due to better accessibility to the active sites.
[0023] For the purposes of the invention, a glass-ceramic substrate is preferably a material that has glass-like and / or ceramic properties. The following properties are preferably understood as glass-like: Can be combined with many other materials without interactions Can be formed at very high temperatures, but remains dimensionally stable when cold Tolerates relatively high temperatures Gas-tight
[0024] Characteristic ceramic properties are preferred relatively low tensile strength brittle behavior high temperature resistance low thermal shock resistance poor thermal conductivity insolubility in water, poor solubility in acids, bases and salt solutions.
[0025] The glass-ceramic substrate therefore advantageously possesses sufficient structural integrity. Furthermore, it can withstand thermal treatment in an oxygen-containing atmosphere. Furthermore, mechanical adhesion of the synthesized catalyst layer is advantageously ensured while still allowing the layer to be removed again.
[0026] It is preferred that the substrate to be used also has exclusively glass or ceramic properties.
[0027] Other substrates (titanium, silicon, quartz glass) are unsuitable because they have a thin oxide layer naturally present (titanium) or is produced in a controlled manner (silicon) on their surface. If these substrates are coated, the oxygen functions present on the substrate surface can form covalent and / or ionic bonds with the catalyst layer during thermal treatment, resulting in strong mechanical adhesion. This strong adhesion prevents transfer of the catalyst layer after the pressing process. Teflon is also unsuitable as a substrate. Among other things, Teflon decomposes at the temperatures required for the synthesis of the nanostructured mesoporous catalyst layer (T3 - thermal treatment), producing harmful vapors.The synthesis of a mesoporous catalyst layer on the glass-ceramic substrate, which preferably occurs before the application of the mesoporous catalyst layer to the polymer membrane, advantageously leads to the indirect (transfer) method mentioned above, thus enabling the thermal treatment necessary for the synthesis. As already explained, the polymer membrane would be destroyed under the influence of high temperatures, thus ruling out direct synthesis. The indirect method has emerged as a particularly preferred alternative.
[0028] After the discussed synthesis of the catalyst layer onto the glass-ceramic substrate, a polymer membrane is pressed onto the glass-ceramic substrate coated with the catalyst layer at a first temperature T 1 . The mesoporous catalyst layer is preferably transferred to a polymer membrane by pressing (at elevated temperature). In the region of the membrane's glass transition point, the polymer chains contained therein become mobile and can be displaced relative to one another. The catalyst layer penetrates a certain distance into the membrane, depending on temperature, contact pressure, and time. Upon cooling of the membrane, the polymer chains solidify and form a covalent bond with the catalyst layer. The adhesion forces between the catalyst and the membrane are greater than between the catalyst layer and the glass-ceramic substrate. In a subsequent separation step, the membrane is peeled off, separating the catalyst layer from the glass-ceramic substrate.
[0029] A sandwich structure, within the meaning of the invention, is preferably a material-to-material composite, preferably consisting of the polymembrane, catalyst layer, and glass-ceramic substrate. The polymembrane, catalyst layer, and glass-ceramic substrate are stacked on top of each other by pressing under increased pressure. However, they can be separated from each other without great force, allowing a user to separate the sandwich structures, for example, using tweezers or small pliers (see [Fig.]). Fig. 2 ). It has been shown that the pressing process step does not destroy the mesoporous structure of the catalyst layer, so that this structure can be advantageously transferred to the polymer membrane.
[0030] Nanostructuring is primarily understood as the structuring of a solid at the atomic level (nanoscale). Targeted modification (implantation) alters atomic, chemical, etc., properties of the solid, usually near the surface.
[0031] A nanostructured mesoporous catalyst layer is preferably understood as an ordered nanostructure of the mesoporous catalyst layer. This means that a catalyst layer comprises approximately identical structural elements (e.g., mesopores with a diameter of 2 to 50 nm) in a repetitive (periodic) manner (e.g., arranged in a row).
[0032] The catalyst layer preferably comprises a variety of compounds that exhibit different catalytic activities, particularly for different applications. The process is preferably as generic as possible to ensure the use of an optimal catalyst.
[0033] In a preferred embodiment, the description relates to a method for
[0034] Production of a catalyst-coated polymer membrane for an electrolyzer and / or a fuel cell comprising the following steps: a) Providing a glass-ceramic substrate; b) Synthesizing a catalyst layer, which can be produced via a thermal treatment, onto the glass-ceramic substrate, wherein a catalyst precursor is provided; c) Pressing a polymer membrane onto the glass-ceramic substrate coated with the catalyst layer at a first temperature T 1 , thereby producing a sandwich structure; d) Separating the sandwich structure, wherein the catalyst layer is separated from the glass-ceramic substrate and adheres to the polymer membrane.
[0035] It has been shown that the preferred process can also be used to produce catalyst layers that do not have a mesoporous structure. In particular, it was previously unknown in the context of producing a catalyst-coated polymer membrane that a catalyst layer can be produced via thermal treatment. This particularly enables catalyst layers that advantageously do not require a binder.
[0036] In a further preferred embodiment, the method is characterized in that the glass-ceramic substrate is a glassy carbon.
[0037] Glassy carbon is a synthetic material made of pure carbon that combines glassy ceramic properties with those of graphite and is therefore particularly suitable for use as a glass-ceramic substrate. However, it was not foreseeable that the use of such a substrate would lead to the successful production of a mesoporous templated catalyst layer on a polymer membrane. For those skilled in the art, the use of glassy carbon as a substrate in the production of oxide layers (catalyst layers) is unusual, as it requires thermal treatment at temperatures higher than 300 °C and an oxygen-containing atmosphere. Furthermore, the use of glassy carbon as a transfer medium in the hot-press process (pressing at elevated temperatures) is unusual, as it fractures easily under pressure.
[0038] In another preferred embodiment, substrates with graphitic carbon coatings can be used as glass-ceramic substrates. The carbon in the coating exhibits similar behavior to glassy carbon. Furthermore, other carbon modifications are also preferably suitable for such coatings.
[0039] In a further preferred embodiment, the glass-ceramic substrate comprises materials and / or coatings that decompose during thermal treatment. The decomposition (or change in the coating) is preferably slight, so that the bond between the templated mesoporous catalyst layer and the substrate is weakened but not lost. In the event that detachment by thermal decomposition of the upper layer of the substrate fails, chemical treatment is also conceivable. For example, etching or detachment of the uppermost substrate layer could preferably be implemented.
[0040] In a further preferred embodiment, the method is characterized in that the following method step is located between method step c) and method step d): c1) Cooling the sandwich structure to a second temperature T 2
[0041] Cooling is particularly important when the sandwich structure has been heated to a temperature above the glass transition point of the polymer membrane, because particularly below the glass transition temperature, strong adhesion forces develop between the catalyst layer and the membrane. This leads to the most complete (and damage-free) transfer of the catalyst layer from the glass-ceramic substrate to the polymer membrane.
[0042] In a further preferred embodiment, the method is characterized in that method step b) comprises the following steps: (i) preparing a suspension comprising a template, a metal precursor and a solvent; (ii) applying the suspension to the glass-ceramic substrate so that a suspension film is formed on the glass-ceramic substrate; (iii) drying the suspension film on the glass-ceramic substrate at a temperature T 4 so that the solvent within the suspension film evaporates and a layer of a catalyst precursor with integrated template structures is obtained; (iv) thermally treating the glass-ceramic substrate comprising catalyst precursors at a third temperature T 3 and a calcination time t 3 so that a mesoporous catalyst layer is formed.
[0043] In this context, a metal salt as a catalyst precursor is preferably dispersed together with a template in a suitable solvent, and this mixture is transferred to the glass-ceramic substrate. Subsequent evaporation of the solvent leads to a favorable periodic arrangement of the template surrounded by a catalyst precursor. Subsequent thermal treatment at preferred temperatures between 300 °C and 600 °C combusts the template and converts the precursor into the actual catalyst, preferably a metal oxide. Removing the template creates interconnected pores that advantageously provide a high surface area for catalytic processes.
[0044] The synthesis of a catalyst layer can only take place at temperatures T 3 above 350 °C, since in this temperature range the polymer templates are completely removed and the noble metal salt is converted into an oxidic species. For this reason, the conventional substrates known for this purpose from the prior art cannot be used. The glass-ceramic substrate, on the other hand, enables precisely such a use due to its temperature stability, and it can be thermally treated. The advantage of the present invention therefore lies in the particular fact that after the coating process (steps (i) - (iii)) on a glass-ceramic substrate and a subsequent thermal treatment at > 350 °C in air, a binder-free, mesoporous structured catalyst layer is obtained, which can be transferred to a membrane.Binders, which typically consist of Nafion ionomer solutions, have the advantage of achieving high proton conductivities, but at the same time, the electrical conductivity of the catalyst layer is reduced and catalytically active sites are blocked. In "ink"-based routes, the binder is usually added in excess to achieve sufficient mechanical strength or structural integrity, whereby the optimum between electrical and proton conductivity is not accessible. The route proposed in the invention allows the binder-free synthesis of a catalyst layer and opens up the possibility of controlled addition of additional ionomers to increase proton conductivity without significantly reducing electrical conductivity. Furthermore, nanostructured catalysts become accessible that have a significantly higher surface-to-volume ratio than ink-based systems.
[0045] The oxidative decomposition of the top layer of the glass-ceramic substrate leads to the beginning of detachment of the adhering catalyst layer. However, the layer remains attached to the substrate. This effect is surprising, as the expert expects complete detachment or disintegration of the oxide layer on the glass-ceramic substrate.
[0046] The synthesis on the glass-ceramic substrate is successful because even a short calcination time (preferably 10 minutes) at high temperatures (preferably 300 °C - 600 °C) is sufficient to generate an active catalyst layer. Longer calcination times can lead to degradation of the catalyst layer due to the more extensive decomposition of the supporting glass-ceramic substrate.
[0047] The preferred synthesis approach is based on templates that serve as placeholders for a desired pore structure. During synthesis, the template is enclosed by the surrounding material (catalyst precursor) and, upon removal, leaves behind a defined porous material. Depending on the template size, pore structures with pore sizes ranging from a few micrometers to a few nanometers are formed. Materials with an ordered pore structure and a monomodal pore size distribution can therefore be preferentially synthesized using so-called templating processes. In this synthesis approach, templates serve as placeholders for the desired pore shape.
[0048] In further preferred embodiments, the template preferably comprises surfactants, block copolymers, and / or dendritic core-shell polymers. The template leads to advantageous mesoporous structures within the catalyst layer, whereby the template can form micelles or also have other structures. In further alternatives, the template can also comprise a non-micelle-forming core-shell macromolecule, effectively a unimolecular micelle. Furthermore, block copolymers can also adopt lamellar structures.
[0049] In a preferred embodiment, templates are designed as soft templates. Soft templates are deformable structure-directing units. These can be micelles or lamellar structures made of amphiphilic polymers (often block copolymers). The micelles or lamellae typically form above a critical concentration of a polymer dispersed in a solvent. Soft templates also include dendritic or hyperbranched core-shell polymers, where the core and shell of the polymers exhibit different hydrophilicities and are thus also amphiphilic.
[0050] In another preferred embodiment, templates are designed as hard templates. Hard templates are rigid, structure-directing units. Nanostructured hard templates include metals, oxides, often silicon oxides (e.g., MCM group, SBA group, FDU group, KIT group, MSU group, TUD group, HMM group, FSM group), and carbons (e.g., CMK group). These hard templates can be individual nanoparticles or larger nanostructured structures.
[0051] In a further preferred embodiment, the method is characterized in that method step b) comprises the following steps: (i) preparing a suspension comprising a metal precursor and a solvent; (ii) applying the suspension to the glass-ceramic substrate so that a suspension film is formed on the glass-ceramic substrate; (iii) drying the suspension film on the glass-ceramic substrate at a temperature T 4 so that the solvent within the suspension film evaporates and a layer of a catalyst precursor with integrated template structures is obtained; (iv) thermally treating the glass-ceramic substrate comprising catalyst precursors at a third temperature T 3 and a calcination time t 3 so that a catalyst layer is formed.
[0052] As already described, the process can also be used to produce catalyst layers that do not have a mesoporous structure. In this context, the use of a template can preferably be omitted.
[0053] In a further preferred embodiment, the process is characterized in that the temperature T 1 is in a range between 80°C and 800°C, preferably in a range between 100°C and 300°C and in particular at 120°C.
[0054] Pressing at elevated temperatures, preferably in the ranges of 80°C and 800°C, advantageously enables low-force pressing, allowing the transfer of the mesoporous catalyst layer (from the glass-ceramic substrate to the polymer membrane) despite the low forces. Elevated temperatures lead to an improved reaction of the various materials in the sandwich structure and enable complete transfer of the catalyst layer from the glass-ceramic substrate to the polymer membrane. In the range of 100°C and 300°C, the energy costs are kept relatively low, and the pressing time can be reduced to a minimum. Pressing at approximately 120°C leads to particularly good, reproducible results, allowing the process to be automated.In addition, a sandwich structure that is particularly easy to separate is obtained. In particular, the temperature of about 120 °C is particularly advantageous for using a Nafion membrane as a polymer membrane, since this has a glass transition temperature of 110 °C.
[0055] A manual hydraulic heat press is preferably used to apply the pressing force, with the sandwich structure being heated by two heating plates arranged above and below the structure. However, other variants are also possible to achieve the pressing force and the preferred temperature T 1 . For example, the transfer can be performed with one hand by a user, for example, by sufficiently heating the sandwich structure with a hot air stream, a heating plate, or an oven, and then pressing it firmly with the hand.
[0056] Advantageously, the process according to the invention enables the coating or synthesis of a mesoporous catalyst layer onto a complexly structured glass-ceramic substrate. This substrate, in turn, can serve as a stamp for the formation of patterns (or similar patterns) on the polymer membrane during the transfer of the catalyst layer to the polymer membrane (in a sandwich structure) in the course of the present invention. Furthermore, the glass-ceramic substrate can also be designed to be very small, so that, in interaction with other glass-ceramic substrates, a pattern can be created on the membrane.
[0057] All parameter ranges disclosed in this document, such as temperatures, forces, pressures, distances, etc., naturally include all values within the specified ranges, as well as their maximum and minimum limits. It is obvious to a person skilled in the art that the values are also subject to certain fluctuations. In the present case, the temperature range is approximately 80°C to 800°C, and preferably approximately 100°C to 300°C, and in particular approximately 120°C. This can be applied analogously to all other parameter ranges in the document.
[0058] Terms such as "substantially," "approximately," "about," "approximately," etc., preferably describe a tolerance range of less than ± 40%, preferably less than ± 20%, more preferably less than ± 10%, even more preferably less than ± 5%, and especially less than ± 1%, and always include the exact value. "Similar" preferably describes quantities that are "approximately equal." "Partially" preferably describes at least 5%, more preferably at least 10%, and especially at least 20%, in some cases at least 40%.
[0059] In a further preferred embodiment, the method is characterized in that the polymer membrane is pressed onto the glass-ceramic substrate coated with the catalyst layer with a contact pressure p 1 in a range from 1000 N / cm 2< to 3000 N / cm 2< and a time t 1 in a range from 5 min to 60 min.
[0060] In the described pressure ranges of 1000 N / cm² to 3000 N / cm², a short processing time can be achieved. Furthermore, the pressure prevents the glass-ceramic substrate from being destroyed, while advantageously enabling the interaction of the composite partners, allowing the mesoporous catalyst layer to form a covalent bond with the polymer chains of the polymer membrane.
[0061] In a further preferred embodiment, the process is characterized in that the polymer membrane is pressed onto the glass-ceramic substrate coated with the catalyst layer with a contact pressure p 1 in a range from 300 N / cm 2 to 10,000 N / cm 2 and a time t 1 in a range from 5 s to 300 min. The specified pressure range in combination with the time range advantageously results in a particularly uniformly developed mesoporous catalyst layer.
[0062] For the duration of the pressing (until the separation of the polymer membrane), the composite of glass-ceramic substrate exists as a sandwich structure.
[0063] In a further preferred embodiment, the process is characterized in that the polymer membrane is pressed onto the glass-ceramic substrate coated with the catalyst layer at a contact pressure p 1 in a range of approximately 2000 N / cm 2 and a time t 1 in a range of approximately 15 min. Preferably, the pressing was carried out at a temperature of approximately 120°C. It has been shown that, by implementing these parameters, particularly good mesoporous catalyst layers can be applied to polymembranes. This advantageously results in synergistic effects of contact pressure, contact time, and contact temperature, which lead to a particularly long service life of the polymer membrane.
[0064] In a further preferred embodiment, the polymer membrane is pressed onto the glass-ceramic substrate coated with the catalyst layer with a contact pressure p 1 of, in particular, approximately 200 kg / m 2 .
[0065] In a further preferred embodiment, the polymer membrane is applied to the glass-ceramic substrate coated with the catalyst layer with a time of about t 1 = 15 min.
[0066] In a further preferred embodiment, the process is characterized in that the temperature T 2 corresponds to a temperature below the glass transition point of the polymer membrane and the temperature T 4 lies in a range between 18°C -80°C.
[0067] Once the temperature T2 has cooled to a temperature below the glass transition temperature of the polymer membrane, the sandwich structures can be separated. Cooling the membrane below the glass transition temperature causes the polymer chains to solidify and form strong bonds (due to covalent bonding and / or van der Waals forces) with the catalyst layer. Since the temperature below the glass transition temperature is already sufficient and no further cooling is required, relatively short processing times can be achieved. Furthermore, no cooling units are required to enable rapid cooling.
[0068] In a preferred embodiment, the sandwich structure is removed from the heating plates after hot pressing, allowing the sandwich structure to cool rapidly. The temperature T 2 is preferably approximately 50°C.
[0069] In the case of a Nafion membrane, the temperature T 2 is preferably below 110°C. More preferably, the temperature T 2 is between 18°C and 108°C. However, variants in which the temperature T 2 is at very low temperatures, below 0°C, are also conceivable.
[0070] Drying of the layer on the glassy carbon substrate can take place in a temperature range from room temperature to 80°C. This advantageously requires very little energy. Furthermore, at such temperatures, the waste heat from the heating systems is sufficient as drying energy to achieve rapid drying of the suspension film. This also leads to significant economic savings in the process.
[0071] In a preferred embodiment, the thermal treatment takes place in heating systems. For removing the template, a tube furnace in an air stream or a muffle furnace can be used, for example. Such furnaces exhibit a uniform temperature distribution, thus advantageously ensuring the repeatability of the process. Furthermore, the waste heat from the furnaces can be advantageously used for further process steps (e.g., drying), thereby saving energy.
[0072] In a further preferred embodiment, the thermal treatment can also be carried out using further methods instead of heating in a furnace. The glass-ceramic substrate comprising catalyst precursors is preferably thermally treated using rapid thermal annealing (RTA) with the waste heat from a halogen lamp. Furthermore, the glass-ceramic substrate comprising catalyst precursors is preferably heated using flash lamp annealing. This advantageously leads to rapid heating and exclusive heating of the surface. Furthermore, the laser annealing method is also preferred. This method leads to even faster heating of the glass-ceramic substrate comprising catalyst precursors, achieving a very shallow penetration depth and heating only the surface. Heating a suitable substrate with an induction furnace would be possible. This also leads to very rapid heating.
[0073] In a further preferred embodiment, the process is characterized in that the temperature T 3 is in a range between 350°C and 700°C, preferably between 350°C and 600°C, and the calcination time t 3 is in a range between 1 minute and 1440 minutes, in particular 10 minutes.
[0074] To thermally decompose the template and convert the inorganic species into a crystalline metal oxide, the catalyst precursor is preferentially calcined.
[0075] Calcination leads to a drastic loss of volume in the layer, caused by the combustion of the template and the transformation of the amorphous pore wall into a crystalline material. Since the adhesion of the layer to the substrate is comparatively strong, partly due to covalent bonds between the substrate surface and the metal oxide species, the layer contracts exclusively perpendicular to the substrate without cracking.
[0076] In a further preferred embodiment, the process is characterized in that the template comprises one or more amphiphilic block copolymers.
[0077] Preferred templates for the synthesis of ordered mesoporous solids are amphiphilic molecules. These advantageously form micelles through self-assembly and self-assemble into liquid-crystalline phases. These liquid crystals, with a nanostructure typically ranging from 2 nm to 50 nm, serve preferentially as endotems in the synthesis of mesoporous oxides.
[0078] In a further preferred embodiment, the glass-ceramic substrate comprising catalyst precursors is thermally treated in an inert atmosphere. Block copolymer substrates decompose even in inert atmospheres at temperatures above 350°C. If the catalyst synthesis is carried out in an inert atmosphere, a further thermal treatment is preferably carried out in an air atmosphere to weaken the bond between the catalyst layer and the glass-ceramic substrate.
[0079] For the templating of ordered mesoporous catalyst layers, amphiphilic block copolymers containing a hydrophilic polyethylene oxide block (PEO) are preferably used
[0080] In a further preferred embodiment, the process is characterized in that the amphiphilic block copolymer is selected from the group comprising AB block copolymers (polyethylene oxide-block-polystyrene (PEO-PS), polyethylene oxide-block-polymethyl methacrylate (PEO-PMMA), poly-2-vinylpyridine-block-polyallyl methacrylate (P2VP-PAMA), polybutadiene-block-polyethylene oxide (PB-PEO), polyisoprene-block-polydimethylaminoethyl methacrylate (PI-PDMAEMA), polybutadiene-block-polydimethylaminoethyl methacrylate (PB-PDMAEMA), polyethylene-block-polyethylene oxide (PE-PEO), polyisobutylene-block-polyethylene oxide (PIB-PEO) and poly(ethylene-co-butylene)-block-poly(ethylene oxide) (PEB-PEO), polystyrene-block-poly(4-vinylpyridine) (PS-P4VP), polyisoprene block polyethylene oxide (PI-PEO), polydimethoxyaniline block polystyrene (PDMA-PS), polyethylene oxide block poly-n-utyl acrylate (PEO-PBA), polybutadiene bock-poly (2-vinylpyridine (PB-P2VP)), polyethylene oxide block polylactide (PEO-PLA),Polyethylenoxid-block-polyglycolid (PEO-PLGA), Polyethylenoxid-block-polycaprolacton (PEO-PCL), Polyethylen-block-polyethylenglycol (PE-PEO), Polystyrol-block-polymethylmethacrlyt (PS-PMMA), Polystyrol-block-polyacrylsäure (PS-PAA), polypyrrol-block-polycaprolacton (PPy-PCL), Polysilicon-block-polyetylenoxid (PDMS-PEO), ABA-Block Copolymeren (Polyethylenoxid-block-polybutadien-block-polyethylenoxid (PEO-PB-PEO), Polyethylenoxid-block-polypropylenoxid-block-polyethylenoxid (PEO-PPO-PEO), Polypropylenoxid-block-polyethylenoxid-block-polypropylenoxid (PPO-PEO-PPO), Polyethylenoxid-block-polyisobutylen-block-polyethylenoxid (PEO-PIB-PEO), Polyethylenoxid-block-polybutadien-block-polyethylenoxid (PEO-PB-PEO), ), Polylactid-block-polyethylenoxid-block-polylactidd (PLA-PEO-PLA), Polyglycolid-block-polyethylenoxid-block-polyglycolid (PGLA-PEO-PGLA), Polylactid-cocaprolacton-block-polyethylenoxid-block-polylactid-co-caprolacton (PLCL-PEO-PLCL),Polycaprolactone-block-polytetrahydrofuran-block-polycaprolactone (PCL-PTHF-PCL), Polypropylene oxide-block-polyethylene oxide-block-polypropylene oxide (PPG-PEO-PPG), Polystyrene-block-polybutadiene-block-polystyrene (PS-PB-PS), Polystyrene-block-polyethylene-ran-butylene-block-polystyrene (PS-PEB-PS), polystyrene block-polyisoprene-block-polystyrene (PS-PI-PS), ABC block copolymers (polyisoprene-block-polystyrene-block-polyethylene oxide (PI-PS-PEO), polystyrene-block-polyvinylpyrrolidone-block-polyethylene oxide (PS-PVP-PEO), Polystyrene-block-poly-2-venylpyridine-block-polyethylene oxide (PS-P2VP-PEO), Polystyrene-block-poly-2-vinylpyridine-block-polyethylene oxide (PS-P2VP-PEO), polystyrene-block-polyacrylic acid-polyethylene oxide (PS-PAA-PEO)), polyethylene oxide-block-polylactide-block-decane (PEO-PLA-decane), as well as other amphiphilic polymers (polyethylene oxide alkyl ethers (PEO-Cxx), e.g. Brij35, Brij56, Brij58) or mixtures thereof, preferably PEO-PB, PEO-PPO, PEO-PB-PEO, PEO-PPO-PEO,
[0081] In a further preferred embodiment, the process is characterized in that a metal salt or several metal salts of different metals, or their hydrates, are used as the metal precursor.
[0082] In further preferred embodiments, metal nanoparticles can also be used as metal precursors, which can be deposited as a layer using mesoporous templates using polymer templates. Metal nanoparticles can advantageously be obtained as industrial waste products and thus reused in a recycling process.
[0083] In a further preferred embodiment, the process is characterized in that the metal salts are selected from the group comprising metal nitrate, metal halide, metal sulfate, metal acetate, metal citrate, metal alkoxide or mixtures thereof.
[0084] In alternative embodiments, other salts can also be used provided they are soluble in the suitable solvent, if necessary with the addition of further complexing substances.
[0085] In a further preferred embodiment, the process is characterized in that the metals contained in the metal precursor are selected from the group comprising alkali metals, preferably lithium, sodium, potassium, rubidium, cesium, alkaline earth metals, preferably magnesium, calcium, strontium, barium, metals of the third main group of the periodic table, preferably boron, aluminum, indium, gallium, thallium, metals of the fourth main group of the periodic table, preferably tin, silicon, germanium, lead, metals of the fifth main group of the periodic table, preferably bismuth, and transition metals, preferably iridium, ruthenium, cobalt, zinc, copper, manganese, cadmium, vanadium, yttrium, zirconium, scandium, titanium.
[0086] In a preferred embodiment, the process is characterized by the use of ruthenium and / or iridium as metal precursors. These two metals, in particular, lead to a catalyst layer with high stability.
[0087] In a further preferred embodiment, the process is characterized in that water or a C1-C4 alcohol, C2-C4 ester, C2-C4 ether, formamide, acetonitrile, acetone, tetrahydrofuran, benzyl, toluene, dimethyl sulfoxide, dichloromethane, chloroform or mixtures thereof are used as solvent, preferably methanol, ethanol, formamide and / or tetrahydrofuran.
[0088] The advantages and preferred embodiments of the process according to the invention can be transferred analogously to the polymer membrane according to the invention, as well as to the fuel cell or electrolyzer and vice versa.
[0089] In a further preferred embodiment, the invention relates to a polymer membrane for an electrolyzer and / or a fuel cell, preferably produced by a method of the type mentioned above, comprising a nanostructured mesoporous catalyst layer.
[0090] A polymer membrane comprising a nanostructured mesoporous catalyst layer offers significant advantages. For example, the higher mass activity of the species in a mesoporous catalyst layer has been demonstrated (see also Fig. 6 ).
[0091] In a further preferred embodiment, the invention relates to a fuel cell or electrolyzer comprising a polymer membrane of the type mentioned above. The use of a polymer membrane according to the invention leads to improved energy generation (generated current per milligram of Pt).
[0092] The application in PEM electrolysers and fuel cells for the production or reconversion of hydrogen is particularly preferred.
[0093] The preferred nanostructured mesoporous polymer membrane according to the invention can also be used in other areas. In medical technology, mesoporous materials are preferably used as drug carriers. Macromolecules are stored in the porous system and can be released as an active ingredient at a suitable location over a longer period of time. The ability to adjust the porosity and the material is an important factor here.
[0094] Furthermore, applications of nanostructured mesoporous polymer membranes in relation to material separation - such as in the context of filtration or osmosis - are conceivable. FIGURES
[0095] In the following, the invention will be explained in more detail with reference to figures, without being limited to these. Short description of the figures
[0096] Fig. 1 Schematic flow diagram of the preferred process for producing a catalyst-coated polymer membrane Fig. 2 Graphical representation together with schematic sketches before (A) and after (B) the transfer of a mesoporous catalyst layer onto a circular membrane Fig. 3 SEM image comparing a schematic sketch of mesoporous RuO x layers, before and after transfer from a glass-ceramic substrate to the polymer membrane Fig. 4 SEM image of mesoporous IrO x layers calcined at different temperatures before and after transfer from a glass-ceramic substrate to the polymer membrane Fig. 5Comparison of a transferred mesoporous IrO x layer with a conventional IrO x layer prepared on Nafion membranes with similar geometric Ir loadings Fig. 6 Diagram showing the electrocatalytic activity of a catalyst-coated membrane with templated mesoporous iridium oxide catalyst produced by the preferred method according to the invention compared to a catalyst-coated membrane with commercial Ir catalyst produced by a spray method Detailed description of the illustrations
[0097] Fig. 1illustrates, in a schematic process diagram, a preferred process for producing a catalyst-coated polymer membrane for an electrolyzer and / or a fuel cell. The process is preferably divided into two processes. On the one hand (process A), a mesoporous catalyst layer is synthesized on a glass-ceramic substrate, particularly preferably a glassy carbon. On the other hand (process B), the mesoporous catalyst layer is transferred to the polymer membrane.
[0098] In a first step of process A, a homogeneous suspension is prepared, wherein the suspension preferably comprises a metal precursor (e.g. Ir(OAc) 3 ), a solvent (e.g. EtOH) and a micelle-forming template (e.g. 10k-Pb; PEO-PB-PEO). In a next step, the suspension is applied to a glass-ceramic substrate, particularly preferably a glassy carbon, and calcined in air to form a mesoporous catalyst layer.
[0099] In process B, a polymer membrane is pressed onto the glass-ceramic substrate containing the mesoporous catalyst layer at elevated temperature (hot-pressing process). Finally, the polymer membrane is separated from the glass-ceramic substrate, leaving the catalyst layer adhering to the polymer membrane.
[0100] The Fig. 2The sequence of illustrations shown shows a preferred process for producing a catalyst-coated polymer membrane. In particular, a graphic representation is illustrated together with schematic sketches before (A) and after (B) the transfer of a mesoporous catalyst layer to a circular membrane. A glassy carbon is provided with a mesoporous RuO x catalyst layer. Subsequently, a Nafion membrane is pressed onto the glassy carbon comprising the catalyst layer, whereby after separation of the pressed composite, the catalyst layer adheres to the membrane.
[0101] Fig. 3 shows a SEM image (scanning electron microscope) in comparison with a schematic sketch of mesoporous RuO x layers, before and after transfer from a glass-ceramic substrate to the polymer membrane. Fig. 3shows the retention of the mesopore morphology during the preferred process sequence, especially after the transfer of the catalyst layer to the polymer membrane.
[0102] Fig. 4 shows an SEM image of mesoporous IrOx layers calcined at different temperatures, before and after transfer from a glass-ceramic substrate to the polymer membrane. The mesopore morphology of the catalyst layer is retained even at different temperatures.
[0103] Fig. 5 shows photographs and SEM images of catalyst layers on membranes. A catalyst-coated membrane produced by a preferred method according to the invention is compared with a catalyst-coated membrane from the prior art. The catalyst-coated membrane produced by the preferred method according to the invention
[0104] Membrane (i) with a mesoporous oxide layer exhibits ordered mesopores and a nanocrystalline structure. In contrast, the catalyst-coated membrane (ii), fabricated from an ink using a spray method, does not exhibit a defined nanostructure.
[0105] The Fig. 6The diagram shows the electrocatalytic activity of a catalyst-coated membrane prepared using the transfer method with a templated mesoporous iridium oxide catalyst compared to a catalyst-coated membrane prepared using a spray method with a commercial Ir catalyst. The membrane coated with a mesoporous catalyst layer using the transfer method achieves an Ir mass activity approximately 35% higher than the reference system, with a comparable geometric Ir loading. The same Pt / C catalyst, applied using a spray method, serves as the cathode coating in both catalyst-coated membranes. The systems differ in their anode coatings.
Claims
1. Process for the production of a catalyst-coated polymer membrane for an electrolyser and / or a fuel cell comprising the following steps: a) providing a glass-ceramic substrate; b) synthesising a mesoporous catalyst layer on the glass-ceramic substrate; wherein the process step b) comprises the following steps: (i) preparing a suspension comprising a template, a metal precursor and a solvent; (ii) applying the suspension to the glass-ceramic substrate such that a suspension film is formed on the glass-ceramic substrate; (iii) drying the suspension film on the glass-ceramic substrate at a temperature T4 so that the solvent within the suspension film evaporates and a layer of a catalyst precursor with integrated template structures is obtained; (iv) thermally treating the glass-ceramic substrate comprising the catalyst precursors at a third temperature T3 and a calcination time calcination time t3, so that a mesoporous catalyst layer is formed, c) pressing a polymer membrane onto the glass-ceramic substrate coated with the catalyst layer at a first temperature T1 whereby a sandwich structure is produced; d) separating the sandwich structure, whereby the catalyst layer is separated from the glass-ceramic substrate and adhering to the polymer membrane.
2. Process according to claim 1 characterised in that the glass-ceramic substrate is a glassy carbon.
3. Process according to one or both of the preceding claims characterised in that the process step c) and the process step d) the following process step is interposed: cl) cooling the sandwich structure to a second temperature T2.
4. Process according to one or more of the preceding claims characterised in that the temperature T1 is in a range between 80°C and 800°C, preferably in a range between 200°C and 600°C and in particular at 400°C.
5. Process according to one or more of the preceding claims characterised in that the polymer membrane is applied to the glass-ceramic substrate coated with the catalyst layer with a contact pressure p1 in a range from 100 N / cm2 to 10000 N / cm2, preferably 1000 N / cm2 to 3000 N / cm2 and a time t1 in a range from 5 s to 300 min, preferably 5 min to 60 min.
6. Process according to claim 1 characterised in that the temperature T2 corresponds to a temperature below the glass point of the polymer membrane and the temperature T4 is in a range between 18°C - 80°C and / or the temperature T3 is in a range between 350°C and 700°C, preferably between 350°C and 600°C, and the calcination time t3 is in a range between 1 minute and 1440 minutes, in particular 10 minutes.
7. Process according to claim 1 characterised in that the suspension comprises one or more amphiphilic block copolymers.
8. Process according to claim 7 characterised in that the amphiphilic block copolymer is selected from the group comprising AB block copolymers (polyethylene oxide-block-polystyrene (PEO-PS), polyethylene oxide-block-polymethyl methacrylate (PEO-PMMA), poly-2-venlypyridine-block-polyallyl methacrylate (P2VP-PAMA), polybutadiene-block-polyethylene oxide (PB-PEO), polyisoprene-block-polydimethylam inoethylmetacrylate (PI-PDMAEMA), polybutadiene-bock-polydimethylam inoethylmetacrlyte (PB-PDMAEMA), polyethylene block polyethylene oxide (PE-PEO), polyisobutylene block polyethylene oxide (PIB-PEO) and poly(ethylene-co-butylene)-block-poly(ethylene oxide) (PEB-PEO), polystyrene-block-poly(4-vinylpyridine) (PS-P4VP), polyisoprene-block-polyethylene oxide (PI-PEO), polydimethoxyaniline-block-polystyrene (PDMA-PS), polyethylene oxide-block-poly-n-utyl acrylate (PEO-PBA), polybutadiene-bock-poly(2-vinylpyridine(PB-P2VP)), polyethylene oxide-block-polylactide (PEO-PLA), polyethylene oxide-block-polyglycolide (PEO-PLGA), polyethylene oxide block-polycaprolactone (PEO-PCL), polyethylene-block-polyethylene glycol (PE-PEO), polystyrene-block-polymethyl methacrylate (PS-PMMA), polystyrene-block-polyacrylic acid (PS-PAA), polypyrrole-block-polycaprolactone (PPy-PCL), polysilicone-block-polyetylene oxide (PDMS-PEO), ABA block copolymers (polyethylene oxide-block-polybutadiene-block-polyethylene oxide (PEO-PB-PEO), polyethylene oxide-block-polypropylene oxide-block polyethylene oxide (PEO-PPO-PEO), polypropylene oxide-blockpolyethylene oxide-block-polypropylene oxide (PPO-PEO-PPO), polyethylene oxide-block-polyisobutylene-block-polyethylene oxide (PEO-PIB-PEO), polyethylene oxide-block-polybutadiene-block-polyethylene oxide (PEO-PB-PEO)), polylactide-block-polyethylene oxide-block-polylactide (PLA-PEO-PLA),polyglycolide-block-polyethylene oxide-block-polyglycolide (PGLA-PEO-PGLA), polylactide-co-caprolactone-block-polyethylene oxide-block-polylactide-co-caprolactone (PLCL-PEO-PLCL), polycaprolactone-block-polytetrahydrofuran-blockpolycaprolactone (PCL-PTHF-PCL), polypropylene oxide block-polyethylene oxide-block-polypropylene oxide (PPG-PEO-PPG), polystyrene-block-polybutadiene-block-polystyrene (PS-PB-PS), polystyrene-block-polyethylene-ran-butylene-block-polystyrene (PS-PEB-PS), polystyrene-block-polyisoprene-block-polystyrene (PS-PI-PS), ABC block copolymers (polyisoprene-block-polystyrene-block-polyethylene oxide (PI-PS-PEO), polystyrene-block-polyvinylpyrrolidone-block-polyethylene oxide (PS-PVP-PEO), polystyrene-block-poly-2-venylpyridine-block-polyethylene oxide (PS-P2VP-PEO), polystyrene-block-poly-2-venylpyridine-block-polyethylene oxide (PSP2VP-PEO), polystyrene-block-polyacrylic acid-polyethylene oxide (PS-PAA-PEO)), polyethylene oxide-block-polylactide-block-decane (PEO-PLA-decane), and other amphiphilic polymers (polyethylene oxide alkyl ether (PEO-C), e.g. Brij35, Brij56, Brij58) or mixtures of these, preferably PEO-PB, PEO-PPO, PEO-PB-PEO, PEO-PPO-PE9. Process according to claim 1 characterised in that the metal precursor used is one or more metal salts of respectively of different metals, or their hydrates, are used as the metal precursor.
10. Process according to claim 9 characterised in that the metal salts are selected from the group comprising metal nitrate, metal halide, metal sulphate, metal acetate, metal citrate, metal alkoxide or mixtures thereof.
11. Process according to one or both of the preceding claims 9 and / or 10 characterised in that the metals contained in the metal precursor are selected from the group comprising alkali metals, preferably lithium, sodium, potassium, rubidium, caesium, alkaline earth metals, preferably magnesium, calcium, strontium, barium, metals of the third main group of the periodic table, preferably boron, aluminium, indium, gallium, thallium, metals of the fourth main group of the periodic table, preferably tin, silicon, germanium, lead, metals of the fifth main group of the periodic table, preferably bismuth, and transition metals, preferably iridium, ruthenium, cobalt, zinc, copper, manganese, cadmium, vanadium, yttrium, zirconium, scandium, titanium.
12. Process according to claim 1 characterised in that the solvent is water or a C1-C4 alcohol, C2-C4 ester, C2-C4 ether, formamide, acetonitrile, acetone, tetrahydrofuran, benzyl, toluene, dimethyl sulphoxide, dichloromethane, chloroform or mixtures thereof preferably methanol, ethanol, formamide and / or tetrahydrofuran.
13. Polymer membrane for an electrolyser and / or a fuel cell, preferably produced by a process according to one or of the preceding claims, comprising a nanostructured mesoporous catalyst layer.
14. Fuel cell or electrolyser comprising a polymer membrane according to claim 13.