SILVER INTERPASTE AND ITS USE FOR JOINING BUILDING COMPONENTS

DE502022001844D1Active Publication Date: 2024-10-31HERAEUS ELECTRONICS GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502022001844
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-17
Publication Date
2024-10-31
Estimated Expiration
2042-08-17

AI Technical Summary

Technical Problem

Existing silver sintering pastes exhibit undesirable squeeze-out behavior during the sintering process, particularly when the layer thickness is high or the contact surfaces of components are large, leading to an unstable connection.

Method used

A silver sintering paste composition comprising 5-40% silver flakes with specific particle size ranges and 50-85% silver particles, along with organic solvents and cellulose derivatives, is developed to minimize squeeze-out and enhance connection stability.

Benefits of technology

The optimized paste composition significantly reduces squeeze-out behavior and achieves a strong, electrically and thermally conductive connection between components, maintaining stability even under pressure sintering conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a silver sintering paste and a method for joining components in which this silver sintering paste can be used.

[0002] The term "component" as used herein refers specifically to components used in electronics, in short, electronic components. Examples include diodes, LEDs (light-emitting diodes), dies, IGBTs (insulated-gate bipolar transistors), MOSFETs (metal-oxide-semiconductor field-effect transistors), ICs (integrated circuits), sensors, heat sinks, resistors, capacitors, inductors, connecting elements (e.g., clips), base plates, antennas, leadframes, PCBs (printed circuit boards), flexible electronics, ceramic substrates, metal-ceramic substrates such as DCB substrates (direct copper bonded substrates), IMS (insulated metal substrates), and the like.

[0003] In the field of power and consumer electronics, sintering the joining of electronic components is a common process. Metal sintering paste, whose main components are dispersed sinterable metal particles, is frequently used as the joining material. Prominent examples of such sintering pastes include silver sintering pastes, which are well-known to those skilled in the art. Sintering joining technology is a very simple method for the stable joining of components, whereby the components to be joined are arranged in a sandwich configuration with their contact surfaces facing each other, and a sintering joining material, such as sintering paste, is applied between them. The sandwich configuration created using sintering paste is then subjected to a drying and sintering step, during which a mechanically strong, electrically and thermally conductive bond between the components is formed.The mechanically fixed connection of two components therefore involves attaching one component to or onto the second component via their respective contact surfaces.

[0004] Document WO 2022 / 128177 A1 discloses a sintering paste consisting of silver flakes and silver particles, with a binder made from a cellulose derivative. Documents US 2021 / 245242 A1 and US 11 278 955 B2 disclose further silver sintering pastes made from mixtures of silver flakes and silver particles.

[0005] The object of the invention was to provide a metal sintering paste with improved properties, particularly with regard to its squeeze-out behavior. Squeeze-out of a metal sintering paste is an undesirable phenomenon of the extrusion of metal sintering paste from the edge region of a sandwich assembly to be sintered during the sintering process. This squeeze-out phenomenon can occur particularly during pressure sintering and can be exacerbated when a relatively large amount of metal sintering paste is located between the components of a sandwich assembly to be joined, i.e., when the layer thickness of the metal sintering paste is high and / or when the contact areas of the components to be joined are large, for example, such that the overlap area formed by the contact surfaces to be joined is in the range of >100 mm², for example, >100 to 500 mm² or more.

[0006] Surprisingly, the task can be solved by providing a silver sintering paste consisting of: (A) 5 to 40 wt.%, preferably 10 to 30 wt.%, particularly preferably 15 to 25 wt.% silver flakes (silver platelets) with a particle size D90 in the range of 5 to 20 µm, preferably 7 to 18 µm, particularly preferably 8 to 15 µm, (B) 50 to 85 wt.%, preferably 55 to 80 wt.%, particularly preferably 60 to 75 wt.% silver particles with a particle size D90 in the range of 300 to 1000 nm, preferably 320 to 800 nm, particularly preferably 350 to 500 nm, (C) 10 to 25 wt.%, preferably 10 to 20 wt.%, particularly preferably 10 to 15 wt.% of at least one organic solvent, (D) 0 to 2 wt.%, preferably 0.1 to 1 wt.%, particularly preferably 0.1 to 0.5 wt.% of at least one cellulose derivative, and (E) 0 to 10 wt.% of at least one additive other than components (A) to (D).

[0007] In a preferred embodiment, the silver sintering paste consists of: (A) 5 to 40 wt.%, preferably 10 to 30 wt.%, particularly preferably 15 to 25 wt.% silver flakes with a particle size D10 in the range of 0.5 to 2 µm, preferably 0.7 to 1.5 µm, D50 in the range of 2.4 to 4 µm, preferably 3 to 3.8 µm and D90 in the range of 5 to 20 µm, preferably 7 to 18 µm, particularly preferably 8 to 15 µm, (B) 50 to 85 wt.%, preferably 55 to 80 wt.%, particularly preferably 60 to 75 wt.% silver particles with a particle size D10 in the range of 90 to 150 nm, preferably 100 to 120 nm, D50 in the range of 150 to 250 nm, preferably 200 to 220 nm, and D90 in the range of 300 to 1000 nm, preferably 320 to 800 nm, particularly preferably 350 to 500 nm, (C) 10 to 25 wt.%, preferably 10 to 20 wt.%, particularly preferably 10 to 15 wt.% of at least one organic solvent, (D) 0 to 2 wt.%, preferably 0.1 to 1 wt.%, particularly preferably 0.1 to 0.5 wt.% of at least one cellulose derivative, and (E) 0 to 10 wt.%.-% at least one additive different from components (A) to (D).

[0008] The terms "particle size D10" and "particle size D90" used herein in connection with the silver flakes (A) refer to the primary particle diameter, which can be determined by means of static automated analysis of microscopic images and which is less than 10% or 90% of the particles, respectively, in terms of volume fraction. The term "particle size D50" used herein in connection with the silver flakes (A) refers to the volume-mean primary particle diameter, which can be determined by means of static automated analysis of microscopic images. The so-called Equivalent Circular Area Diameter (ECAD) can be used as a measure for the primary particle diameter (see RENLIANG XU ET AL: "Comparison of sizing small particles using different technologies", POWDER TECHNOLOGY, ELSEVIER, BASEL (CH), Vol. 132, No. 2-3, June 24, 2003 (2003-06-24), pages 145-153).Static automated analysis of microscopic images can be performed, for example, using the Morphologi 4 measuring system from Malvern Instruments, according to the dry determination method.

[0009] The terms "particle size D10" and "particle size D90" used herein in connection with the silver particles (B) refer to the primary particle diameter, which can be determined by laser diffraction and is less than 10% or 90% of the particles, respectively, by volume. The term "particle size D50" used herein in connection with the silver particles (B) refers to the volume-average primary particle diameter, which can be determined by laser diffraction. The so-called Equivalent Circular Area Diameter (ECAD) can be conveniently used as a measure of the primary particle diameter (see Renliang Xu et al.: "Comparison of sizing small particles using different technologies", Powder Technology, Elsevier, Basel (CH), Vol. 132, No. 2-3, June 24, 2003 (2003-06-24), pages 145-153).Laser diffraction measurements can be performed using a suitable particle size analyzer, such as a Malvern Instruments Mastersizer 3000 or Mastersizer 2000, according to the wet method. In the wet method, sample preparation involves, for example, dispersing 1 g of silver particles of type (B) in 200 ml of ethanol using ultrasound.

[0010] Component (A) consists of silver flakes with a particle size D90 in the range of 5 to 20 µm, preferably 7 to 18 µm, and particularly preferably 8 to 15 µm. Preferably, the silver flakes have a particle size D10 in the range of 0.5 to 2 µm, preferably 0.7 to 1.5 µm, D50 in the range of 2.4 to 4 µm, preferably 3 to 3.8 µm, and D90 in the range of 5 to 20 µm, preferably 7 to 18 µm, and particularly preferably 8 to 15 µm.

[0011] The aspect ratio of silver flakes can be greater than 5:1, ranging from >5:1 to several hundred:1. The aspect ratio of particles describes the quotient of their largest and smallest dimensions, and thus their shape. To avoid misunderstandings, in the case of particles in the form of flakes or platelets, the quotient of largest and smallest dimensions is the quotient of the largest dimension and the platelet thickness. It can be determined by scanning electron microscopy and evaluation of the electron micrographs by determining the dimensions of a statistically significant number of individual particles.

[0012] The silver flakes can have a specific surface area, for example, in the range of 1 to 5 m² / g. The specific surface area in m² / g can be determined using BET measurement according to DIN ISO 9277:2014-01 (static volumetric measurement method, gas used: nitrogen).

[0013] The silver flakes can have a tapped density, for example, in the range of 1 to 5 g / cm³. Tapped density is the density of a solid that is further compacted by tamping or vibrating compared to its bulk density. The tapped density in g / cm³ can be determined according to DIN EN ISO 787-11:1995-10.

[0014] The silver flakes are usually coated. The weight specifications given here include the weight of the coating on the silver flakes.

[0015] The silver flakes can comprise flakes of pure silver (purity of at least 99.9 wt%) and / or flakes of silver alloys with up to 10 wt% of at least one other alloying metal. Examples of suitable alloying metals are copper, gold, nickel, palladium, platinum, and aluminum. Silver flakes made of pure silver are preferred.

[0016] The aforementioned coating can be a firmly adhering layer on the surface of the silver flakes. It is typically an organic coating. The proportion of the organic coating can, for example, range from 0.5 to 1.5 wt%, based on silver or silver alloy. Generally, such an organic coating can comprise 90 to 100 wt% of one or more fatty acids and / or fatty acid derivatives. Examples of fatty acid derivatives include, in particular, fatty acid salts and fatty acid esters. Examples of fatty acids include caprylic acid (octanoic acid), capric acid (decanoic acid), lauric acid (dodecanoic acid), myristic acid (tetradecanoic acid), palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), oleic acid (9-octadecenoic acid), arachidic acid (eicosanoic acid / icosanoic acid), behenic acid (docosanoic acid), and lignoceric acid (tetracosanoic acid).

[0017] In a DSC analysis (differential scanning calorimetry, dynamic differential calorimetry) of the coated silver flakes, performed in a temperature range of, for example, 25°C to 400°C with a heating rate of 10K / min under air access, the coating of the silver flakes may be characterized, for example, by one or two exothermic peaks in the temperature range of, for example, 200 to 270°C.

[0018] In a TGA analysis (thermogravimetric analysis) of the coated silver flakes carried out in a temperature range of, for example, 25°C to 400°C with a heating rate of 10K / min under air access, the coating of the silver flakes may be characterized, for example, by a weight loss starting at, for example, 130 to 150°C and ending at, for example, 220 to 240°C, in the range of, for example, 0.7 to 1.5 wt.%.

[0019] Type (A) silver flakes are available, for example, from the companies Metalor or Ames Goldsmith.

[0020] Component (B) consists of silver particles with a particle size D90 in the range of 300 to 1000 nm, preferably 320 to 800 nm, and particularly preferably 350 to 500 nm. Preferably, the silver particles have a particle size D10 in the range of 90 to 150 nm, preferably 100 to 120 nm; D50 in the range of 150 to 250 nm, preferably 200 to 220 nm; and D90 in the range of 300 to 1000 nm, preferably 320 to 800 nm, and particularly preferably 350 to 500 nm. The silver particles of component (B) are so-called submicron silver particles, not to be confused with even smaller nano-silver particles, which have D90 particle sizes of <250 nm.

[0021] The silver particles are not silver flakes; their aspect ratio is significantly lower than that of silver flakes, ranging, for example, from 1:1 to 5:1. Ideally spherical particles have an aspect ratio of 1:1. The aspect ratio of the silver particles, ranging from 1:1 to 5:1, means that the silver particles have, for example, a spherical, essentially spherical, elliptical, egg-shaped, or irregular form, but in no case the form of flakes.

[0022] The silver particles can comprise particles of pure silver (purity of at least 99.9 wt%) and / or those of silver alloys with up to 10 wt% of at least one other alloying metal. Examples of suitable alloying metals are copper, gold, nickel, palladium, platinum, and aluminum. Silver particles made of pure silver are preferred.

[0023] The silver particles can have a specific surface area, for example, in the range of 1 to 8 m² / g. The specific surface area in m² / g can be determined using BET measurement according to DIN ISO 9277:2014-01 (static volumetric measurement method, gas used: nitrogen).

[0024] The silver particles can have a tapped density, for example, in the range of 3 to 6 g / cm³. Tapped density is the density of a solid that is further compacted by tamping or vibration compared to its bulk density. The tapped density in g / cm³ can be determined according to DIN EN ISO 787-11:1995-10.

[0025] The silver particles are usually coated. The weight specifications given here therefore include the weight of the coating on the silver particles.

[0026] The aforementioned coating can be a firmly adhering layer on the surface of the silver particles. It is typically an organic coating. The proportion of the organic coating can, for example, range from 0.5 to 1.5 wt%, based on the silver or silver alloy. Generally, such an organic coating can comprise 90 to 100 wt% of one or more fatty acids and / or fatty acid derivatives. Examples of fatty acid derivatives include, in particular, fatty acid salts and fatty acid esters. Examples of fatty acids include caprylic acid (octanoic acid), capric acid (decanoic acid), lauric acid (dodecanoic acid), myristic acid (tetradecanoic acid), palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), oleic acid (9-octadecenoic acid), arachidic acid (eicosanoic acid / icosanoic acid), behenic acid (docosanoic acid), and lignoceric acid (tetracosanoic acid).

[0027] In a DSC analysis of the coated silver particles carried out in the temperature range of, for example, 25°C to 400°C with a heating rate of 10K / min under air access, the coating of the silver particles may be characterized, for example, by one or two exothermic peaks in the temperature range of, for example, 200 to 270°C.

[0028] In a TGA analysis of the coated silver particles carried out in a temperature range of, for example, 25°C to 400°C with a heating rate of 10K / min under air access, the coating of the silver particles may be characterized, for example, by a weight loss starting at, for example, 140 to 160°C and ending at, for example, 230 to 250°C, in the range of, for example, 0.9 to 1.4 wt.%.

[0029] Type (B) silver particles are available, for example, from the company Ames Goldsmith.

[0030] Component (C) is at least one organic solvent. Examples of suitable organic solvents include terpineols, N-methyl-2-pyrrolidone, ethylene glycol, dimethylacetamide, 1-tridecanol, 2-tridecanol, 3-tridecanol, 4-tridecanol, 5-tridecanol, 6-tridecanol, isotridecanol, 2-ethyl-1,3-hexanediol, 2-(2-ethylhexyloxy)ethanol, benzyl alcohol, diethylene glycol monobutyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, dibasic esters (preferably dimethyl esters of glutaric, adic, or succinic acid, or mixtures thereof), glycerol, diethylene glycol, triethylene glycol, and aliphatic, especially saturated aliphatic hydrocarbons with 5 to 32 carbon atoms, more preferably 10 to 25 carbon atoms, and even more More preferably 16 to 20 carbon atoms.

[0031] The optional, but preferably, component (D) comprising the silver sintering paste according to the invention is at least one cellulose derivative. Examples include methylcellulose, ethylcellulose, ethylmethylcellulose, carboxycellulose, hydroxypropylcellulose, hydroxyethylcellulose, and hydroxymethylcellulose.

[0032] The optional component (E) is at least one additive different from components (A) to (D). Examples include surfactants, defoamers, wetting agents, and anti-corrosion additives.

[0033] Component (E) preferably does not include glass particles (glass frit); in other words, the silver sintering paste according to the invention preferably does not include glass particles.

[0034] Component (E) preferably does not include any thermally decomposable metal precursors (metal precursor compounds), i.e., no metal precursors that decompose into the corresponding metal during the sintering process. Accordingly, silver precursors commonly found in prior art silver sintering pastes, such as silver oxide, silver carbonate, silver lactate, and the like, are therefore preferably not included in component (E). In other words, the silver sintering paste according to the invention preferably does not include any thermally decomposable metal precursors. Furthermore, it has been shown that the absence of such metal or silver precursors has a positive effect on the storage stability of a silver sintering paste according to the invention.

[0035] An essential feature of the silver sintering paste according to the invention appears to be that it comprises a combination of a relatively small proportion of silver flakes of type (A) with a relatively large proportion of submicron silver particles of type (B), and preferably without any proportion of said metal or silver precursors.

[0036] The sum of the wt.% of components (A) to (E) is 100 wt.%, based on the silver sintering paste according to the invention. Accordingly, a silver sintering paste according to the invention can be produced by mixing components (A) to (C), (A) to (D), and (A) to (E), respectively. Conventional devices known to those skilled in the art can be used for this purpose, for example, agitators, three-roll mills, jet mixers, and / or disperser mixers.

[0037] The silver sintering paste according to the invention can be used in a sintering process, for example, in a sintering process as described above. Sintering is understood to mean the joining of two or more components by heating while preventing the silver flakes and silver particles from reaching the liquid phase. The resulting solid mechanical bond is both electrically and thermally conductive; it consists practically or almost entirely of silver. The invention also relates to a method for joining components in which (1) a sandwich arrangement is provided, comprising at least two components and a silver sintering paste according to the invention located between the components, (2) optionally, but preferably, the silver sintering paste is dried, and (3) the sandwich arrangement is sintered. Drying is understood to mean the removal of organic solvent from the applied sintering paste according to the invention.When working with a silver sintering paste according to the invention, steps (1), (2), and (3) form a step sequence of the type (1)-(2)-(3), with step (2) being optional. In one embodiment of the process carried out with the silver sintering paste according to the invention, step (1) may already include drying, and step (2) may therefore be omitted; in another embodiment, step (1) does not include drying or only partially includes drying, and the optional step (2) may be omitted or preferably performed; if step (2) is omitted here, it may take place during or overlap with step (3).

[0038] The components can – insofar as they are not already made of metal – comprise at least one metal contact surface, for example in the form of a metallization layer, over which the aforementioned sandwich arrangement is carried out within the framework of the inventive method.

[0039] In step (1), the two or more components are first brought into contact with each other. This contact is achieved using the silver sintering paste according to the invention, which is optionally already dried. For this purpose, a sandwich arrangement is provided in which the silver sintering paste according to the invention is located between each pair of at least two components. A sandwich arrangement is understood to be an arrangement in which two components are located one above the other and are arranged substantially parallel to each other.

[0040] The sandwich arrangement can be manufactured using a method known from the prior art. In this process, the relevant metal contact surface of one of the components is provided with the silver sintering paste according to the invention. Subsequently, the other component is placed with its metal contact surface onto the silver sintering paste that has been applied to the metal contact surface of the first component.

[0041] The application of the silver sintering paste according to the invention to the relevant metal contact surface of one component can be carried out using conventional methods, for example by printing processes such as screen printing or stencil printing. Alternatively, the application of the silver sintering paste according to the invention can also be carried out by dispensing technology, jetting, pin transfer or dipping.

[0042] The wet film thickness of the silver sintering paste according to the invention is preferably in the range of 20 to 400 µm. The preferred wet film thickness depends, for example, on the application method chosen. If the silver sintering paste according to the invention is applied, for example, by screen printing, then a wet film thickness of, for example, 20 to 60 µm may be preferred. If the application is carried out, for example, by stencil printing, then the preferred wet film thickness may be, for example, in the range of 20 to 400 µm. For example, in dispensing technology, the preferred wet film thickness may be, for example, in the range of 20 to 400 µm, depending on the application tool used, for example, when using a hollow needle in the range of 20 to 100 µm or, for example, when using a wide-slot nozzle that also functions as a doctor blade in the range of 50 to 400 µm.

[0043] Following the application of the silver sintering paste according to the invention to the metal contact surface of one component, the metal contact surface of this component, which may already be partially or completely dried with the silver sintering paste, is brought into contact with the corresponding metal contact surface of the component to be joined via the silver sintering paste. Thus, a layer of undried, partially, or completely dried silver sintering paste according to the invention is located between the components to be joined, forming the sandwich arrangement.

[0044] According to a preferred embodiment, the proportion of organic solvent in the silver sintering paste after drying is, for example, 0 to 5 wt.%, based on the original proportion of organic solvent in the silver sintering paste according to the invention. In other words, during drying according to this preferred embodiment, for example, 95 to 100 wt.% of the organic solvent(s) originally contained in the silver sintering paste according to the invention are removed.

[0045] The drying temperature in step (2) is preferably in the range of 100 to 150 °C. Typical drying times are, for example, in the range of 5 to 45 minutes. To shorten the drying time, a vacuum can be used, for example, a pressure in the range of 100 to 300 mbar.

[0046] After completion of step (1) and step (2), respectively, the sandwich arrangement is finally subjected to a sintering process. This sintering step (3) of the inventive method can be carried out under pressure or without pressure. Pressureless execution means that a sufficiently strong bond between the components can be achieved without the application of mechanical pressure. As already mentioned at the outset, the silver sintering paste according to the invention is characterized by a low or preferably even non-existent squeeze-out behavior; in other words, the silver sintering paste according to the invention is particularly suitable for the inventive method designed as pressure sintering.

[0047] The actual sintering takes place at a temperature of, for example, 200 to 280 °C, and as mentioned, either as a pressureless process or by making appropriate use of the slight or non-existent squeeze-out behavior as pressure sintering.

[0048] In pressure sintering, the process pressure is preferably below 30 MPa and more preferably below 15 MPa. For example, the process pressure is in the range of 1 to 30 MPa and more preferably in the range of 5 to 15 MPa.

[0049] For example, sintering time ranges from 2 to 90 minutes, pressure sintering from 2 to 5 minutes, and pressureless sintering from 30 to 75 minutes.

[0050] The sintering process can take place in an atmosphere that is not subject to any particular restrictions. Thus, sintering can be carried out in an atmosphere containing oxygen. Alternatively, it is also possible to carry out sintering in an oxygen-free atmosphere or in a vacuum. For the purposes of this invention, an oxygen-free atmosphere is understood to be an atmosphere whose oxygen content is no more than 300 ppm by weight, preferably no more than 100 ppm by weight, and even more preferably no more than 50 ppm by weight.

[0051] The sintering process is carried out in a conventional device suitable for sintering, in which the process parameters described above can be set. Examples 1. Production of silver sintering pastes:

[0052] The silver sintering pastes 1 to 5 according to the invention, as well as the comparison pastes V1-V3, were prepared according to Table 1 (all values ​​in wt.%). For this purpose, the organic solvents and, if applicable, the ethylcellulose were first homogenized at 80°C to form a solvent system. Subsequently, the silver flakes and the silver particles were added portion by portion to the solvent system and completely dispersed. 2. Evaluation of the silver sintering pastes: a) Production of test setups serving as models:

[0053] The silver sintering pastes 1 to 5 according to the invention, as well as the comparison pastes V1 to V3, were applied by stencil printing to a silver-metallized copper-ceramic substrate with a wet film thickness of 300 µm. Immediately afterwards, the respective areas of the printed silver sintering paste were fully covered with another silver-metallized copper-ceramic substrate (20 mm x 20 mm). The resulting sandwich arrangements were dried in normal air at 120°C for 10 minutes. The subsequent pressure sintering was carried out under a nitrogen atmosphere (<100 ppm oxygen) in a hot press at 230°C and 12 MPa for 5 minutes. b) Assessment of squeeze-out behavior:

[0054] The sintered test setups were visually assessed to determine whether any unwanted extrusion of silver sintering paste had occurred at the edges.

[0055] If no sintered paste was visible at the edge of the contact surface of the substrate during the sintering process, the extrusion behavior was rated as "+" (no unwanted squeeze out).

[0056] If sintered silver sintering paste was visible on at least one edge of the test setup next to the silver-metallized copper ceramic substrate on only <20% of the circumferential edge, the extrusion behavior was classified as "low".

[0057] If sintered silver sintering paste was visible on at least one edge of the test setup next to the silver-metallized copper ceramic substrate on >50% of the circumferential edge, the extrusion behavior was classified as "strong". c) Determination of shear strength:

[0058] To determine the shear strength, the components were sheared with a shear chisel at a speed of 2 mm / min at 20°C. The force was measured using a 10 kN load cell (Zwick Roell Z010, Germany). Table 1: Composition and evaluation of the silver sintering pastes 1 to 5 according to the invention and of the comparison pastes V1 to V3 1 2 3 4 5 V1 V2 V3 Silverflakes* 7 10 12 17 30 52 84 - Silver particles** 80 77 75 70 57 35 - 87 Ethylcellulose 0,1 - 0,1 0,1 0,1 0,1 0,3 0,1 Terpineol 6,45 6,50 6,45 6,45 6,45 6,45 7,85 6,45 Diethylene glycol butyl ether 6,45 6,50 6,45 6,45 6,45 6,45 - 6,45 Dimethyl succinate - - - - - - 7,85 - Evaluation: Squeeze-out behavior small amount + + + + + + strong Shear strength (N / mm²< ) 40 40 41 45 40 30 30 55 * Fatty acid-coated silver flakes: D90: 9 µm, D50: 3 µm, D10: 1 µm ** Fatty acid-coated silver particles: D90: 400 nm, D50: 200 nm, D10: 105 nm

Claims

1. A silver sinter paste consisting of: (A) 5 to 40 wt.% of silver flakes having a particle size D90 in the range of 5 to 20 µm, (B) 50 to 85 wt.% of silver particles having a particle size D90 in the range of 300 to 1000 nm, (C) 10 to 25 wt.% of at least one organic solvent, (D) 0 to 2 wt.% of at least one cellulose derivative, and (E) 0 to 10 wt.% of at least one additive other than the previously mentioned constituents (A) to (D), wherein the term "particle size D90" used in connection with the silver flakes (A) means the primary particle diameter, determined by means of automated static analysis of microscopic images, with which a volume proportion of 90% of the particles is below said primary particle diameter, and wherein the term "particle size D90" used in connection with the silver particles (B) means the primary particle diameter, determined by means of laser diffraction, with which a volume proportion of 90% of the particles is below said primary particle diameter.

2. The silver sinter paste according to claim 1, in which the silver flakes have a particle size D10 in the range of 0.5 to 2 µm and a particle size D50 in the range of 2.4 to 4 µm, and in which the silver particles have a particle size D10 in the range of 90 to 150 nm and a particle size D50 in the range of 150 to 250 nm, wherein the term "particle size D10" used in connection with the silver flakes (A) means the primary particle diameter, determined by means of automated static analysis of microscopic images, with which a volume proportion of 10% of the particles is below said primary particle diameter, wherein the term "particle size D50" used in connection with the silver flakes (A) means the volume-average primary particle diameter, determined by means of automated static analysis of microscopic images, wherein the term "particle size D10" used in connection with the silver particles (B) means the primary particle diameter, determined by means of laser diffraction, with which a volume proportion of 10% of the particles is below said primary particle diameter, and wherein the term "particle size D50" used in connection with the silver particles (B) means the volume-average primary particle diameter, determined by means of laser diffraction.

3. The silver sinter paste according to claim 1 or 2, in which the silver flakes have an aspect ratio of > 5:1, determined by scanning electron microscopy and evaluation of the electron microscopic images by determining the dimensions of a statistically significant number of individual particles.

4. The silver sinter paste according to any of the preceding claims, in which the silver flakes have a specific surface area in the range of 1 to 5 m2 / g, determined by means of a BET measurement according to DIN ISO 9277:2014-01, static-volumetric measuring method, gas used: nitrogen.

5. The silver sinter paste according to any of the preceding claims, in which the silver flakes have a tapped density in the range of 1 to 5 g / cm3, determined according to DIN EN ISO 787-11:1995-10.

6. The silver sinter paste according to any of the preceding claims, in which the silver particles have an aspect ratio of 1:1 to 5:1, determined by scanning electron microscopy and evaluation of the electron microscopic images by determining the dimensions of a statistically significant number of individual particles.

7. The silver sinter paste according to any of the preceding claims, in which the silver particles have a specific surface area in the range of 1 to 8 m2 / g, determined by means of a BET measurement according to DIN ISO 9277:2014-01, static-volumetric measuring method, gas used: nitrogen.

8. The silver sinter paste according to any of the preceding claims, in which the silver particles have a tapped density in the range of 3 to 6 g / cm3, determined according to DIN EN ISO 787-11:1995-10.

9. The silver sinter paste according to any of the preceding claims, wherein the at least one cellulose derivative is selected from the group consisting of methyl cellulose, ethyl cellulose, ethyl methyl cellulose, carboxy cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose and hydroxymethyl cellulose.

10. The silver sinter paste according to any of the preceding claims, not comprising any glass particles.

11. The silver sinter paste according to any of the preceding claims, not comprising any thermally decomposable metal precursors.

12. A method for joining components, in which a sandwich arrangement is provided (1), which comprises at least two components and a silver sinter paste according to any of the preceding claims located between the components, the silver sinter paste is optionally dried (2) and the sandwich arrangement is sintered (3).

13. The method according to claim 12, wherein sintering is carried out under pressure or without pressure.

14. The method according to claim 12 or 13, wherein the components are components used in electronics.