BUILDING MATERIAL WITHOUT HYDRAULIC BINDER

DE602019060812T2Active Publication Date: 2024-10-23ETH ZURICH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602019060812
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-12
Filing Date
2019-09-11
Publication Date
2024-10-23
Estimated Expiration
2039-09-11

AI Technical Summary

Technical Problem

The use of hydraulic binders like cement in construction materials poses significant energy and environmental concerns, and there is a need for a material that can be produced with minimal auxiliary products using locally available resources, while maintaining workability and setting behavior similar to concrete or cement grout.

Method used

A process involving the extraction of a mineral fraction with clay particles from soil, adjustment of particle size, preparation of an aqueous slurry, addition of dispersing and coagulating agents, and evaporation to create a solid construction material with a compressive strength of at least 1.4 MPa, without the need for hydraulic binders, using phosphates and polyacrylate salts as dispersing agents and inorganic salts with divalent metal cations as coagulating agents.

Benefits of technology

This process allows for the production of a solid construction material with compressive strength suitable for load-bearing elements, reducing the need for hydraulic binders and enabling on-site construction with minimal auxiliary products, achieving workability and setting characteristics similar to conventional cement grouts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to construction materials that can be obtained from the soil insofar as the soil contains clay particles without the addition of hydraulic binder. STATE OF THE ART

[0002] In the construction sector, the most widely used inorganic building material is concrete, which consists of aggregates combined with a hydraulic binder. However, the use of hydraulic binders, such as cement, presents infrastructure challenges because cement production requires significant amounts of energy and the presence of a concrete plant, resulting in considerable monetary and environmental costs. Therefore, it is preferable to minimize the use of such hydraulic binders to reduce construction costs. Ideally, a building material that can be produced using naturally occurring resources near the construction site with minimal use of auxiliary products is preferred.However, it is also important that such a construction material has similar workability to concrete or cement grout and similar setting behavior to concrete grout so as not to have to adapt the construction procedures and / or tools which are basically designed for hydraulic binder grouts such as cement.

[0003] WO2015 / 155110 A1 discloses a process for the manufacture of ceramic tiles comprising clays and monovalent cation salts such as chlorides, bromides and dispersants such as (meth)acrylic acid polymers, phosphates or polyphosphates, sodium di- or metasilicates or liquid sodium silicate. SUMMARY OF THE INVENTION

[0004] The present invention offers a method for manufacturing a solid building material, preferably substantially free of hydraulic binders such as cement, which enables and facilitates the use of soil in the manufacture of the building material with a minimum of auxiliary products and without the need to add hydraulic binders.

[0005] The process also makes it possible to obtain a construction material which, in its fluid state, can be used in a manner analogous to cement grouts, in terms of rheology and setting time, which allows, for example, the manufacture of solid construction materials, such as load-bearing building elements on site, or on site, of the construction site.

[0006] The present invention therefore provides a method for manufacturing a solid building material preferably substantially free of hydraulic binder, comprising the steps of: a. extract a mineral fraction including clay particles from a soil; b. optionally adjust the particle size distribution of the extracted mineral fraction, in particular with respect to its clay, sand, gravel or silt content if necessary; c. prepare a first aqueous grout from at least a portion of the extracted mineral fraction, optionally adjusted for particle size distribution; d. add a dispersing agent capable of dispersing the clay particles to the first grout to obtain a second aqueous grout; e. add a coagulating agent capable of causing the clay particles to agglomerate to the second grout to obtain an aqueous construction material grout; f. introduce the construction material grout into formwork; and g.to allow the evaporation of water contained in the grout material to obtain a solid building material, characterized in that the solid building material is a load-bearing element having a compressive strength of at least 1.4 MPa, wherein the dispersing agent is selected from phosphates and polyacrylate salts such as monovalent salts thereof, and wherein the coagulant is selected from inorganic salts having a divalent metallic cation of carbonate, chloride, nitrate, sulfate, oxide, or hydroxide, more preferably from alkaline earth metal salts of carbonate, chloride, nitrate, sulfate, oxide, or hydroxide.

[0007] The present invention further provides a solid building material obtained by the process according to any of the variants of the aforementioned process, having a compressive strength of at least 1.4 MPa.

[0008] Preferred embodiments of the present invention are described in the dependent claims. DESCRIPTION OF THE DRAWINGS

[0009] Fig. 1 shows the evolution of the yield stress as a function of the dispersing agent content in the grout. Fig. 2 shows the evolution of the Vicat needle penetration depth as a function of time. Fig. 3 shows the effect of the magnesium-based coagulant on the grout after 24 hours, comparing a grout without magnesium (left) and with magnesium (right). Fig. 4 shows the evolution of compressive strength as a function of time, i.e., as a function of the degree of drying. DESCRIPTION OF FAVORITE ACHIEVEMENTS

[0010] The present invention therefore provides a method for manufacturing a solid building material preferably substantially free of hydraulic binders such as cement, lime or pozzolana, comprising the steps of: a. Extract a mineral fraction containing clay particles from a soil; b. Optionally adjust the particle size distribution of the extracted mineral fraction, particularly with respect to its clay, sand, gravel, or silt content if necessary; c. Prepare a first aqueous grout from at least a portion of the extracted mineral fraction, optionally adjusted for particle size distribution; d. Add a dispersing agent capable of dispersing the clay particles to the first grout to obtain a second aqueous grout; e. Add a coagulating agent capable of causing the clay particles to agglomerate to the second grout to obtain an aqueous construction material grout; f. Introduce the construction material grout into formwork; and g. Allow the water contained in the material grout to evaporate to obtain a solid construction material. characterized in that the solid construction material is a load-bearing element having a compressive strength of at least 1.4 MPa, wherein the dispersing agent is selected from phosphates and polyacrylate salts such as monovalent salts thereof, and wherein the coagulant is selected from inorganic salts having a divalent metallic cation of carbonate, chloride, nitrate, sulfate, oxide, or hydroxide, more preferably from alkaline earth metal salts of carbonate, chloride, nitrate, sulfate, oxide, or hydroxide.

[0011] The extraction of the mineral fraction containing clay particles from the soil can be carried out on-site, for example, by excavating the soil, thus avoiding the need to transport additional mineral materials such as clay, silt, rubble, and sand to the construction or production site. The clay particles are preferably smaller than 4 µm, and more preferably smaller than 2 µm, according to standard NF P18-560. The clay particles are preferably hydrated aluminosilicates, and more preferably from the phyllosilicate family, such as kaolinite. The technologies required to obtain this mineral fraction are within the capabilities of those skilled in the art of building materials.

[0012] The particle size distribution of the extracted mineral fraction can be adjusted on-site by sieving or sedimentation analysis. Alternatively, when the local conditions of the extracted mineral fraction require it, the composition can be supplemented by adding other mineral fractions, such as silt, sand, gravel, or pebbles, to achieve the desired particle size. The specific content of silt, sand, gravel, or pebbles in the mineral fraction will depend on the requirements of the construction material and its intended use.

[0013] A useful composition of the mineral fraction presents about 5 to 30% by weight of clay particles, preferably 10 to 25% by weight of clay particles, 5 to 10% by weight of silt, 25 to 55% by weight of sand and 20 to 47% by weight of gravel, relative to the total weight of dry mineral material contained in the mineral fraction.

[0014] The preparation of the first aqueous grout from at least a portion of the extracted mineral fraction, which may have been adjusted for particle size, can be carried out by mixing at least a portion of the extracted mineral fraction with an aqueous solution or water, for example, in a concrete mixer. The amount of water can be varied depending on the intended use and is generally chosen to ensure a fluid grout. For example, a water-to-mineral fraction ratio between 0.1 and 0.6. Or a water-to-mineral fraction ratio such that a flowability in terms of spreading after vibration of between 30 and 50 cm is achieved.

[0015] The addition of a dispersing agent capable of dispersing clay particles to the first grout to obtain a second aqueous grout is preferably carried out after the first aqueous grout has been mixed, while the mixing action continues. The dispersing agent can be added either in solid form or as a dispersion or aqueous solution. The dispersing agent capable of dispersing clay particles is preferably chosen from among aluminates, phosphates, silicate solutions, and polyacrylate salts, such as monovalent salts thereof. A useful dispersing agent chosen from among phosphates is sodium hexametaphosphate. A useful dispersing agent chosen from among silicates is sodium silicate solution. A useful dispersing agent chosen from among polyacrylate salts is sodium polyacrylate.It is important to choose the dispersing agent from among monovalent salts, preferably alkali metal salts such as sodium or potassium, and not alkaline earth metal salts, which are divalent. Adding the dispersing agent to the initial grout results in a grout with increased fluidity, i.e., a yield stress of less than 1000 Pa, preferably less than 250 Pa. This means that the amount of water needed to achieve a consistent yield stress compared to a grout without a dispersing agent is reduced. When the yield stress is below 1000 Pa, the grout becomes easier to work, mold, form, and pump. The yield stress below 1000 Pa can be achieved by adding less than 2% by weight, preferably 0.1 to 0.5% by weight of dispersing agent relative to the total dry weight of mineral material or 0.4 to 2% by weight of dispersing agent relative to the total weight of dry clays. In particular, the dispersing agent may be selected from sodium polyphosphate, sodium hexametaphosphate, sodium silicate, sodium polyacrylate, and ammonium polyacrylate. In a preferred embodiment of the present invention, the dispersing agent consists of a mixture of at least one phosphate and at least one silicate, more preferably a mixture of sodium hexametaphosphate and sodium silicate.

[0016] The addition of a coagulating agent capable of causing the clay particles to agglomerate to the second grout to obtain an aqueous construction material grout is preferably carried out when the second aqueous grout has reached a yield stress of less than 1000 Pa and more preferably when the second aqueous grout has reached a yield stress of less than 1000 Pa and before the formwork of the aqueous construction material grout.

[0017] The addition of a coagulant accelerates the setting of aqueous construction material grout by releasing divalent ions, such as calcium, which can form precipitations such as crystals that can increase mechanical properties, such as compressive strength, in the final construction material. The solubility of the coagulant can be used to control the setting rate of the construction material grout in order to optimize the progress of the construction process. When rapid setting, i.e., within one hour, is desired, the coagulant is preferably chosen from halides and nitrates, such as chlorides of alkaline earth metals, for example, magnesium or calcium chloride, or calcium nitrate or magnesium nitrate. However, when prolonged workability, i.e.,beyond one hour and preferably more than 4 hours is desired, the coagulant agent is preferably chosen from among the oxides, hydroxides and carbonates, and sulfates of alkaline earth metals such as for example magnesium or calcium oxide, magnesium or calcium hydroxide, magnesium or calcium carbonate.

[0018] For example, if the dispersing agent is a silicate such as sodium silicate and the coagulant is an alkaline earth metal salt such as calcium oxide, the precipitation occurs as hydrated calcium silicate crystals such as plomberite. If the dispersing agent is a phosphate such as hexametaphosphate and the coagulant is an alkaline earth metal salt such as calcium oxide, the precipitation occurs as hydrated calcium silicate crystals such as apatite. Similarly, when the dispersing agent is a phosphate such as hexametaphosphate and the coagulant is an alkaline earth metal salt such as magnesium oxide, the precipitation occurs as magnesium silicate crystals.Without favoring any particular theory, it is estimated that the rapid increase in compressive strength observed in aqueous construction material grouts shortly after the addition of the coagulant and during drying results from the formation of precipitation. This precipitation consumes the dispersing agent present in the aqueous construction material grout and eliminates the electrostatic repulsion generated by the adsorption of the dispersing agent onto the clay particles. This rapid increase in compressive strength in aqueous construction material grouts shortly after the addition of the coagulant and during drying allows for a reduction in the time required to manufacture a construction material component.

[0019] Generally, the coagulant is preferably chosen from inorganic salts containing a divalent metallic cation, such as iron or alkali-earth metals, or from carbonate, chloride, nitrate, sulfate, oxide, or hydroxide, and more preferably from salts of alkaline earth metals, such as calcium or magnesium, or from carbonate, chloride, nitrate, sulfate, oxide, or hydroxide. In particular, the coagulant may be chosen from calcium carbonate, calcium chloride, calcium nitrate, calcium sulfate, calcium hydroxide, magnesium oxide, magnesium hydroxide, magnesium carbonate, magnesium sulfate, cement, or calcium sulfoaluminate cement.

[0020] In a preferred embodiment of the present invention, the dispersing agent consists of at least one phosphate, at least one silicate, or mixtures thereof, more preferably of sodium hexametaphosphate, sodium silicate or a mixture of sodium hexametaphosphate and sodium silicate and / or the coagulant consists of magnesium oxide, calcium hydroxide or a mixture of magnesium oxide and calcium hydroxide.

[0021] The coagulant may be added either in solid form or as a dispersion or aqueous solution, and when a rapid setting, i.e. within less than one hour is desired, the coagulant is added as an aqueous solution in the case of halides or in the case where the coagulant is preferably chosen from oxides, hydroxides and carbonates, and sulfates in the form of solid particles having a specific surface area of ​​at least 20 m² / g or as an aqueous dispersion of the same solid particles.

[0022] Generally, the coagulant can be obtained from the extraction of the corresponding ore from a quarry. Although ores contain the majority of the coagulant, they also contain impurities that can interfere with the coagulating action. Therefore, it is preferable to use coagulants with increased purity, i.e., a purity of at least 85% by weight, and preferably 95% by weight or more. It has been found that using coagulants with increased purity also leads to higher mechanical properties in the hardened construction material, as well as faster setting. Conversely, using coagulants with reduced purity, i.e., a purity of less than 85% by weight, leads to a longer workable time for the grout.

[0023] In a particular embodiment of the process according to the present invention, the coagulant agent in the building material is present in at least 0.1% by weight, preferably from 0.1 to 0.5% by weight, relative to the total weight of dry mineral material or at least 1% by weight, preferably from 1% to 2% by weight, relative to the dry clay content.

[0024] In a particular embodiment of the process according to the present invention where the dispersing agent is chosen from phosphates and the coagulating agent is chosen from inorganic salts having a divalent metal cation, the molar ratio [Me 2+< / PO 4 3-< ] between the metal cation of the inorganic salt and the phosphate in the aqueous construction material grout is preferably greater than 1 and more preferably greater than 2 or between 2 and 5, i.e. that generally the metal cation of the inorganic salt is present in a molar excess relative to the phosphate.

[0025] In a preferred embodiment of the present invention, where the dispersing agent consists of at least one aqueous solution of silicate such as, for example, sodium silicate, i.e., soda silicate, the sodium silicate is present in a Na₂O:SiO₂ ratio greater than 1, more preferably in the range between 1 and 2.8. In particular, where sodium silicate having a Na₂O:SiO₂ ratio greater than 1, more preferably in the range between 1 and 2.8, is used as a coagulant, the dispersing agent is preferably a polyacrylate and more preferably chosen from sodium polyacrylate, ammonium polyacrylate, or mixtures thereof.

[0026] In a particular embodiment of the process according to the present invention, the building material is a building block, preferably in the shape of a parallelepiped such as bricks, in particular load-bearing bricks or other load-bearing elements such as a wall, a slab or a pillar.

[0027] The present invention further provides a solid building material obtained by any of the aforementioned variations of the process, having a compressive strength of at least 1.4 MPa, and more particularly of at least 3 MPa or from 3 to 10 MPa, and substantially free of hydraulic binders. A compressive strength in this range makes it possible to manufacture building blocks or vertical walls suitable for constructing houses or buildings of up to four stories without resorting to materials such as hydraulic binders and using a small amount of additives such as dispersing and coagulating agents. It is important to note that a compressive strength of at least 1.4 MPa can be achieved after 24 hours of drying, allowing construction progress at essentially the same rate as when using cement or concrete as the building material.Compressive strength is measured using a Unitronic Compression 50kN / tensile 25kN device manufactured by Matest on 4×4×16 cm samples which are broken at 3 bending points and then tested in uniaxial compression using a 10kN cell.

[0028] Thus, the resulting construction material is substantially free of hydraulic binders such as cement, lime, or pozzolana; that is, it comprises less than 2% by weight, and less than 1% by weight, of hydraulic binders such as cement, lime, or pozzolana, relative to the total weight of dry mineral material contained in the mineral fraction. In a preferred embodiment, the resulting construction material comprises less than 1% by weight of cement relative to the total weight of dry mineral material contained in the mineral fraction.

[0029] In a particular embodiment of the process according to the present invention, the addition of the dispersing agent and the coagulating agent to finally obtain a grout of aqueous construction material can be done by first adding the dispersing agent and the coagulating agent.

[0030] In the case where the dispersing agent and the coagulating agent are added sequentially, i.e. first the dispersing agent and then the coagulating agent, it is preferable to add the dispersing agent, the coagulating agent or both in the form of an aqueous solution or dispersion in order to better control over the working time or the triggering of the setting of the construction material grout. EXAMPLES

[0031] 1325 kg of sand, 509.33 kg of clay and 305.59 kg of water were mixed to obtain 1 m³ of grout in which the water / clay ratio is 0.6 and the sand / clay volume ratio is approximately 1.0.

[0032] The amount of additives added was varied to evaluate the effect of the dispersant and coagulant on the rheology and setting of the grout. In the case discussed, the dispersant used was sodium hexametaphosphate (NaHMP).

[0033] As can be seen in the graph in Figure 1, increasing the amount of dispersant added to the grout leads to a decrease in the grout flow threshold, which was also confirmed by an increase in spread from 10 cm (0.2% by weight of NaHMP relative to the weight of clays) to 40 cm (0.8% by weight of NaHMP relative to the weight of clays) in an Abrams cone slump test.

[0034] As can be seen in Figure 2, increasing the amount of coagulant added to the fluidized grout with 0.8% by weight of dispersant, relative to the weight of clays, accelerates the grout setting. It is worth noting that in Figure 2, a penetration depth of 0 corresponds to the maximum penetration in the direction where the Vicat needle reaches the bottom of the sample, i.e., to depth 0 of the sample. In this case, the coagulant used is magnesium oxide. Without the addition of magnesium oxide (Mg / P molar ratio = 0), no solidification occurs. Conversely, if a magnesium oxide-based coagulant is added, setting is initiated and accelerated as the magnesium-to-phosphate molar ratio increases.

[0035] As can be seen in the photograph in drawing 3, without the addition of magnesium oxide-based coagulant, a sample of fluidized grout with 0.8% by weight of demolded dispersant collapses even after 24 hours, whereas in the presence of magnesium oxide-based coagulant, the sample stays in place.

[0036] As can be seen in the graph in Figure 4, the compressive strength of 1 MPa, sufficient for demolding a self-supporting wall, is reached after 24 or 48 hours when the fluidized grout, containing 0.8% by weight of dispersant, includes a magnesium oxide-based coagulant. Without the addition of a magnesium oxide-based coagulant, the grout requires at least one week to reach a compressive strength of 1 MPa. In practice, this means that grouts obtained by the process according to the present invention can be demolded after 24 hours, which is approximately the same time required to demold a conventional cement grout. This therefore allows for the substitution of conventional cement grouts without any loss of time during construction.

[0037] In conclusion, the addition of coagulant leads to an increase in compressive strength which allows for the rapid construction of self-supporting vertical walls because sufficient strength is reached after 24 hours in order to demold a self-supporting wall.

Claims

1. A process for the manufacture of a solid building material substantially free of hydraulic binder, comprising the steps of: a. extracting a mineral fraction comprising clay particles from a soil, b. optionally adjusting the particle size of the extracted mineral fraction, in particular with respect to its clay, sand, gravel or silt content, c. preparing a first aqueous slurry from at least a part of the extracted mineral fraction and optionally adjusted as to the particle size, d. adding a dispersing agent capable of dispersing the clay particles to the first aqueous slurry to obtain a second aqueous slurry, e. adding a coagulating agent capable of causing the clay particles to agglomerate to the second aqueous slurry to obtain an aqueous building material slurry, f. introducing the aqueous building material slurry into a formwork, and g. allowing the water contained in the material slurry to evaporate to obtain a solid building material, characterized in that the solid building material is a load-bearing element having a compressive strength of at least 1.4 MPa, wherein when the dispersing agent is selected from phosphates and polyacrylate salts such as monovalent salts thereof, and the coagulating agent is selected from inorganic salts having a divalent metal cation of carbonate, chloride, nitrate, sulfate, oxide, or hydroxide, more preferably from alkaline earth metal salts of carbonate, chloride, nitrate, sulfate, oxide, or hydroxide.

2. The process according to claim 1, wherein load-bearing element is a wall, a brick, a slab or a pillar.

3. The process according to any one of claims 1 to 2, wherein the building material comprises at least 5% by weight, preferably from 5 to 30% by weight of clay particles, relative to the total dry weight of the mineral material contained in the mineral fraction.

4. The process of any one of claims 1 to 3, wherein the building material comprises 0.4 to 2% by weight of dispersing agent, relative to the total dry weight of clays.

5. The process according to any one of claims 1 to 4, wherein the building material comprises at least 1% by weight of coagulating agent, preferably from 1% to 2% by weight, relative to the total dry weight of clays.

6. The process of any one of claims 1 to 5, wherein the slurry of building material, at the time of introduction into the mold, contains from 5 to 30% water.

7. The process according to any one of claims 1 to 6, wherein when the dispersing agent is selected from phosphates and the coagulating agent is selected from alkaline earth metal salts, wherein the molar ratio [Me2+ / PO43-] between the metal cation of the salt and the phosphate in the aqueous building material slurry is greater than 1 and preferably between 2 and 5.

8. A solid building material obtained by the process according to any to any one of the preceding claims, characterized in that the solid building material is a load-bearing element having a compressive strength of at least 1.4 MPa.