AI Technical Summary
Current optical devices struggle to achieve optimal anti-reflective and mirror effects across a wide range of wavelengths and angles of incidence, particularly in the infrared spectrum, with existing multilayer constructions and structuring methods being limited in their ability to control refractive indices and improve transmission efficiency.
The development of an optical device featuring a textured coating layer and substrate, where the texturing creates cavities that pass through the coating layer and partially hollow out the substrate, allowing for controlled variation of effective refractive indices and improved transmission and reflection properties across specific wavelength ranges.
This approach enhances transmission and reflection performance, particularly in the infrared range, by expanding the angle of incidence validity and improving spectral width and maximum transmission, while maintaining simplicity in manufacturing and surface tension.
Description
TECHNICAL FIELD
[0001] The present invention relates to an optical device, suitable for the transmission or reflection of radiation in a predetermined wavelength range, for example of the ultraviolet, visible, infrared or microwave type.
[0002] The field of the invention is that of optical devices, designed for example to equip imaging systems. In practice, the applications depend on the wavelength range. PREVIOUS ART
[0003] As is known, anti-reflective or mirror effects can be obtained by multi-layer construction and / or by structuring optical devices.
[0004] The following documents describe different examples of optical devices. EP3206059A1 describes a broadband diffractive device, comprising a plurality of elementary zones and microstructures arranged to form an artificial material having an effective index variation at the surface of the device. BRUYNOOGHE (2016), "Broadband and wide-angle hybrid antireflection coatings prepared by combining interference multilayers with subwavelength structures", Journal of Nanophotonics, SPIE, International Society for Optics and Photonics. This document describes a multilayer construction combined with stochastic structures made by dry etching. KUBOTA (2014), "Optimization of hybrid antireflection structure integrating surface texturing and multi-layer interference coating", Thin Films for Solar and Energy Technology VI, Graduate School of Science and Engineering, Yamagata University, Japan. This document describes the theoretical study of the combination of a multilayer construction and a moth-eye grating.CAMARGO (2012), "Multi-scale structured, superhydrophobic and wide-angle, antireflective coating in the near-infrared region", Chem. Commun., 2012, 48, 4992-4994, Royal Society of Chemistry, United Kingdom. This paper describes the structuring of multiple layers, with a focus on improving certain surface behaviors. RALCHENKO (1999), "Fabrication of CVD Diamond Optics with Antireflective Surface Structures", phys. stat. sol., General Physics Institute, Moscow, Russia. This paper describes the structuring of CVD-deposited diamond to achieve an antireflective effect. WO 2011 / 021752 A1 EP 1 785 748 A1 WO 2010 / 056500 A2 US 2008 / 074748 A US 2015 / 103396 A1. STATEMENT OF THE INVENTION
[0005] The aim of the present invention is to propose an optical device, of the anti-reflective or mirror type, exhibiting improved properties.
[0006] For this purpose, the invention relates to an optical device according to claim 1.
[0007] Thus, the invention makes it possible to modify the front of an electromagnetic wave in a controlled manner.
[0008] Texturing allows for the variation of the effective refractive index across the surface of the textured device. Specifically, texturing enables the controlled achievement of lower effective refractive indices in both the textured coating layer and the textured area of the substrate. Texturing makes it possible to obtain effective indices that are unattainable directly using multilayers. These indices vary depending on the wavelength of the radiation.
[0009] Also, the invention makes it possible to increase the range of incidence angle for which the validity of the optical function is interesting.
[0010] The device structure forms at least one bi-layer system, comprising the textured coating layer and the textured substrate layer, overlying the non-textured portion of the substrate.
[0011] According to a first application, the optical device has an anti-reflective function.
[0012] Advantageously, the invention makes it possible to improve the transmission of the device, in terms of spectral width and maximum transmission (therefore minimum absorption), compared to an untextured and uncoated substrate; a textured and uncoated substrate; a substrate coated with an untextured coating layer; and even a substrate coated with a textured coating layer, but whose texturing does not penetrate the substrate. This improvement depends on the configuration of the device, in particular the characteristics of the substrate-coating pair and the texturing.
[0013] Compared to a textured, uncoated substrate, the textured coating layer improves transmission by forming shallower cavities. This makes texturing easier and faster to achieve.
[0014] Compared to a substrate coated with a non-textured coating layer, the surface behavior of the device is changed.
[0015] In practice, the device does not improve transmission across the entire electromagnetic spectrum, but is configured for transmission over a wavelength range in the infrared (IR) dependent on the characteristics of the substrate-coating pair and the texturing.
[0016] Wavelength ranges are defined according to the subdivisions recommended by the International Commission on Illumination (CIE): Gamma rays: less than 10 pm; X-rays: 10 pm to 10 nm; Ultraviolet: 10 nm to 380 nm; Visible: 380 nm to 780 nm; IR-A (near-infrared): 0.78 µm to 1.4 µm; IR-B (mid-infrared): 1.4 µm to 3 µm; IR-C (far-infrared): 3 µm to 1 mm; Radio waves: greater than 1 mm
[0017] For the IR range, the following subdivisions can also be used: NIR (near IR): 0.75 µm to 1.4 µm SWIR: 1.4 µm to 3 µm MWIR: 3 µm to 8 µm LWIR: 8 µm to 15 µm FIR (far IR): 15 µm to 1 mm
[0018] In terms of transmission, the different variants of the device are not necessarily more efficient than prior art devices. However, the device according to the invention offers other advantages: simplicity of manufacture, surface tension, etc.
[0019] According to a second application, the optical device has a mirror function.
[0020] Thus, the invention makes it possible to improve the reflection of the device, compared to an untextured and uncoated substrate, a textured and uncoated substrate, or a substrate coated with an untextured coating layer.
[0021] Alternatively (or in combination with the reflectance and transmittance functions), the optical device may have a function of modifying the wavefront of optical surfaces, different from the anti-reflection and mirror functions.
[0022] According to a first embodiment, the device comprises a single substrate layer supporting one or more coating layers. The substrate preferably has a thickness of between 0.1 and 30 mm, for example of the order of 1 or 2 mm. The coating layer preferably has a thickness of between 0.01 and 50 µm, for example of the order of 0.5 µm or 2 µm for the IR range. The material of the substrate is for example silicon Si, germanium Ge, zinc sulfide ZnS, zinc selenide ZnSe, etc., for IR applications. The substrate generally has a crystalline structure. The coating may have an amorphous or crystalline structure. The material of the coating layer is for example silicon Si, germanium Ge, zinc sulfide ZnS, zinc selenide ZnSe, tantalum pentoxide Ta2O5, hafnium dioxide HfO2, alumina Al2O3. The device comprises at least one back layer. The device may comprise a single substrate and a single coating layer.In this case, preferably, the substrate has a refractive index higher than the refractive index of the coating before texturing. The device may comprise a single substrate and several textured coating layers. In this case, preferably, the substrate has a refractive index higher than the refractive index of the coatings before texturing. Alternatively, the substrate may have a refractive index lower than at least one of the coating layers.
[0023] According to a second embodiment, the structure of the device forms a stack of layers comprising more than one coating layer and one substrate layer. In this case, each substrate is defined as a support layer for a coating layer. The substrates and the coating layers preferably have a thickness of between 0.01 and 50 µm, for example of the order of 0.5 µm or 2 µm for the IR range. The substrate may have an amorphous or crystalline structure. The coating may have an amorphous or crystalline structure. The device comprises at least one rear layer. The rear layer disposed against the last substrate preferably has a thickness of between 0.1 and 30 mm, for example of the order of 1 or 2 mm. The rear layer disposed against the last substrate may have a crystalline structure. If the device comprises several rear layers, the second rear layer preferably has a thickness of between 0.01 and 50 µm, for example of the order of 0.5 µm or 2 µm for the IR range. The back layer material can be silicon Si, germanium Ge, zinc sulfide ZnS or zinc selenide ZnSe.The device may comprise a stack of several alternating substrates and coating layers, including at least a first combination of a first coating layer and a first substrate, oriented on the upper side, receiving the incident radiation, and a last combination of a last coating layer and a last substrate. The cavities may be formed only in the first combination, oriented on the upper side, receiving the incident radiation. The cavities may pass entirely through the stack except for the last substrate, which is partially hollowed out. Preferably, these cavities have a strictly decreasing area section in the direction of the last substrate. The cavities may pass entirely through the coating layer and partially hollow out the substrate for each combination forming the stack.The stack may include at least one intermediate combination between the first combination and the last combination. The device may include a back layer for each substrate-coating combination. In this case, the back layer may optionally be traversed by the cavities, penetrating into the next coating layer. Alternatively, the device may include a single back layer for the last combination. In this case, the back layer is not traversed by the cavities.
[0024] According to other advantageous characteristics of the invention, taken in isolation or in combination: The cavities are formed in the substrate to a depth preferably between 0.5 and 10 µm, for example of the order of 1 µm, for the far IR range, beyond 3 µm. The cavities are formed in the substrate to a depth preferably between 0.08 µm and 3 µm, for example of the order of 200 nm, for the near IR or mid IR range between 780 nm and 3 µm. The cavities are formed in the substrate to a depth preferably between 1 nm and 600 nm, for example of the order of 80 nm, for the visible range. Preferably for IR applications, the substrate and the coating layer are transparent / reflective for the entire wavelength range between 1 µm and 50 µm. Preferably for the far IR range between 8 µm and 12 µm, the device allows a transmittance / reflectance of at least 90% of the incident infrared radiation for the diopter considered.The characteristics of the cavities (shape, dimensions, distribution, etc.) depend on the texturing technique and the parameters used. Preferably, the cavities have a larger width or diameter between 0.02 and 3 µm, especially between 1 and 2 µm. The coating layer can be made by a thin film deposition technique, such as PVD or CVD. Texturing can be carried out by any type of technique suitable for passing through the coating layer and partially digging the substrate, for example laser ablation, photolithography, nano-imprinting, etc. Laser texturing is relatively economical and well controlled. Texturing can be carried out by an ultra-short laser, with a pulse duration in the femtosecond or picosecond regime. The laser wavelength, which typically varies between 200 and 16000 nm, is to be chosen according to the desired texturing characteristics (shape and dimensions of the cavities, patterns, etc.).The optomechanical environment of the laser includes motorized stages, a microscope objective (and / or galvano scanner, and / or micro-sphere monolayer), an in-line viewing unit, etc. Preferably, the cavities have a continuous profile at the transition between the coating layer and the substrate. This continuous profile can be obtained by forming the cavities in the coating layer and in the substrate during the same texturing operation, for example laser texturing. A continuous profile improves control of the desired wavefront shape. Indeed, discontinuities can generate diffraction or other unwanted effects. The cavities can have a circular cross-section. The cavities have a strictly decreasing area cross-section towards the last substrate. The cavities can have a concave profile in an axial plane, with a decreasing area cross-section with depth.The cavities may have a symmetrical concave profile in an axial plane. The cavities may have an asymmetrical concave profile in an axial plane. The cavities may have different dimensions, including different diameters, widths, and / or depths. The dimensions of the cavities may vary periodically. The dimensions of the cavities may have a variable periodicity, evolving according to a defined rule and not randomly. The cavities may be randomly distributed over the surface of the device. The cavities may be distributed in a regular pattern over the surface of the device. The cavities may be distributed in a pattern having a triangular, square, hexagonal, etc. mesh. The cavities may be distributed with a variable periodicity over the surface of the device. The variable periodicity evolves according to a defined rule and not randomly. The variable periodicity evolves regularly.The cavities may have a different periodicity between the center and the edges of the device. The cavities may be closer together in the center of the device. In the cladding layer, the cavities have a density of between 20 and 91%, i.e., a space filling rate of between 20 and 91%. The rate of 91% corresponds to the cavities arranged hexagonally and which touch each other. The device may comprise at least one back layer made of a material different from the substrate and the cladding, the cladding being formed on a first side of the substrate, the back layer being formed on a second side of the substrate opposite the first side. The device may comprise two faces, each with a cladding layer and surface texturing forming cavities passing through the cladding layer and partially penetrating the substrate or one of the substrates.The device may comprise a first face with a coating layer and surface texturing forming cavities passing through the coating layer and partially penetrating the substrate or one of the substrates, and a second face with a coating layer which may be devoid of texturing in accordance with the invention, or may receive a treatment different from the texturing of the first face, or may not receive any treatment. The coating layers of the two faces may be different (material, thickness, etc.). The faces of the device may or may not be parallel. For example, the faces may be arranged in inclined planes. According to another example, the faces may be concave or convex.
[0025] The invention also relates to a method for manufacturing an optical device adapted for the transmission / reflection of electromagnetic radiation within a wavelength range of the electromagnetic spectrum, said method comprising at least the following steps to form at least one combination of a substrate made of a first material, and a coating layer made of a second material different from the first material, then to perform a surface texturing forming cavities in the device, characterized in that the cavities pass through the coating layer and partially hollow out the substrate.
[0026] The invention can find numerous applications in the field of optical devices: IR applications: camera, lens, optical window, camouflage surface, decoy, etc. Near-IR applications: optical windows, lenses, mirrors, for cameras, imaging devices, laser lines, beam shaping, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The invention will be better understood on reading the description which follows, given solely as a non-limiting example and made with reference to the appended drawings in which: [ Fig 1 ] is a schematic cross-sectional representation of a device comprising a silicon substrate (Si), a DLC amorphous carbon coating layer, and a textured surface forming cavities within the device, with the cavities extending through the coating layer and partially excavating the substrate. Fig 2 ] is a cut analogous to the figure 1 , showing a device consisting of an untextured Si substrate and DLC coating. [ Fig 3 ] is a cut analogous to the figure 1 showing a device consisting of a textured, uncoated Si substrate. Fig 4 ] is a cut analogous to the figure 1 showing a device consisting of an untextured Si substrate and a textured DLC coating. Fig 5 ] is a cut analogous to the figure 1 showing a device consisting of an untextured and uncoated Si substrate. Fig 6 ] is a schematic top-view representation of the device of the figure 1 . [ Fig 7 ] is a graph showing the evolution of transmission (T from 0 to 1) as a function of wavelength (WL from 3 to 15 µm), for each of the devices of the figures 1 à 5 . [ Fig 8 [ ] is a graph showing the evolution of the transmission (T in %) as a function of the angle of incidence (angle from 0 to 80°) of the radiation on the surface of the device, for the devices of the figures 1 et 2 . [ Fig 9 ] is a graph analogous to the figure 8 showing the evolution of transmission (T in %) as a function of the angle of incidence (angle from 0 to 60°) for the devices of figures 1 et 2 . [ Fig 10 ] is a diagram showing the evolution of the transmission (T in %) as a function of the wavelength (WL from 3 to 15 µm) and the angle of incidence (Angle from 0 to 80°), for the device of the figure 1 , in accordance with the invention. [ Fig 11 ] is a diagram analogous to the figure 10 , for the device of the figure 2 . [ Fig 12 ] is a graph analogous to the figure 7 showing the evolution of transmission (T from 0.7 to 1) as a function of wavelength (WL from 0.8 to 3 µm), for five different devices, configured as shown in the figures 1 à 5 , with a zinc selenide (ZnSe) substrate and, for some, a silicon dioxide (SiO2) coating layer. Fig 13 ] is a graph analogous to the figure 9 , for two devices whose transmission is represented on the figure 12 , namely a device according to the invention comprising a textured substrate and coating, and a device comprising a non-textured substrate and coating. Fig 14 ] is a graph analogous to the figure 7 , showing the evolution of the transmission (T from 0.96 to 1) as a function of the wavelength (WL from 0.3 to 1 µm), for five different devices, configured as in the figures 1 à 5 , with a silicon dioxide SiO2 substrate and for some a magnesium fluoride MgF2 coating layer. [ Fig 15 ] is a graph analogous to the figure 9 , for two devices whose transmission is represented on the figure 14 , namely a device according to the invention comprising a textured substrate and coating, and a device comprising a non-textured substrate and coating. Fig 16 ] is a graph analogous to the figure 7 , showing the evolution of the transmission (T from 0.966 to 1) as a function of the wavelength (WL from 0.3 to 1 µm), for five different devices, configured as in the figures 1 à 5 , with an alumina Al2O3 substrate and for some a silicon dioxide SiO2 coating layer. [ Fig 17 ] is a schematic top-view representation of a variant of the device according to the invention, in which the cavities have a variable periodicity on the surface of the device, being closer together in the center than at the edges of the device. Fig 18 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, the cavities having a symmetrical concave profile, with a cross-section decreasing with depth, and not a cylindrical profile. Fig 19 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, the cavities having an asymmetrical concave profile. Fig 20 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, the cavities having variable depths. Fig 21 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, the cavities having variable diameters. Fig 22 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, comprising a stack of two substrates and two alternating coating layers, the cavities being formed only in the first coating layer and the first substrate. Fig 23 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, comprising a stack of two substrates and two alternating coating layers, the cavities passing completely through the stack except for the last substrate, which is partially hollowed out. Fig 24 ] is a cut analogous to the figure 2 , showing a variant of the device according to the invention, comprising a rear layer made of a material different from the substrate and the coating. Fig 25 ] is a cut analogous to the figure 2 , showing a variant of a device according to the invention, with two faces each comprising a substrate, a coating layer and a surface texturing forming cavities passing through the coating layer and partially penetrating the substrate. Fig 26 ] is a cut analogous to the figure 2 , showing a variant of a device according to the invention, with a first face comprising a coating layer and a surface texturing forming cavities passing through the coating layer and partially penetrating the substrate, and a second face comprising a coating layer devoid of texturing, devoid of treatment, or receiving a treatment different from the texturing of the first face. Fig 27 ] is a cut analogous to the figure 2 , showing a variant of a device according to the invention, with two faces each comprising a substrate, a coating layer and a texturing, and an intermediate layer formed between the two substrates. Fig 28 ] is a diagram illustrating the reversibility of the device. [ Fig 29 ] is a diagram illustrating the optical equivalence of a complex device and two simple devices. [ Fig. 30 ] is a cut analogous to the figure 2 , showing a variant of a device according to the invention, comprising a stack of two substrates and two alternating coating layers as well as a back layer, the cavities being formed only in the first coating layer and the first substrate. Fig 31 ] is a graph analogous to the figure 7 , showing the evolution of transmission (T) as a function of wavelength (WL from 340 to 840 nm), for three different devices, including two devices with a stack of two HfO2 substrate layers, two SiO2 coating layers and an amorphous carbon back layer. Fig 32 ] is a graph analogous to the figure 7 , showing the evolution of transmission (T) as a function of wavelength (WL from 1 to 2.4 µm), for three different devices, namely a device consisting of a single layer of amorphous carbon, and two devices with a stack of two Si3N4 substrate layers, two SiO2 coating layers and a ZnSe back layer, one textured device and one untextured device. Fig 33 ] is a graph analogous to the figure 9 , for the two multilayer devices whose transmission is shown on the figure 32 . [ Fig 34 ] is a graph analogous to the figure 7 , showing the evolution of transmission (T) as a function of wavelength (WL from 7 to 15 µm), for three different devices, namely a device consisting of a single layer of amorphous carbon, and two devices with a stack of two TiO2 substrate layers, two DLC coating layers, and a Si back layer, one textured device and one untextured device. Fig 35 ] is a graph analogous to the figure 9 , for the two multilayer devices whose transmission is shown on the figure 34 . [ Fig 36 ] is a graph analogous to the figure 7 , showing the evolution of transmission (T) as a function of wavelength (WL from 7 to 15 µm), for three different devices, namely a device consisting of a single layer of amorphous carbon, and two devices with a stack of two TiO2 substrate layers, two DLC coating layers, and a Si back layer, one textured device and one untextured device. Fig 37 ] is a graph analogous to the figure 9 , for the two multilayer devices whose transmission is shown on the figure 36 . DETAILED DESCRIPTION OF THE INVENTION
[0028] On the figures 1 et 2 an anti-reflective optical device (1) is shown.
[0029] The device (1) is well suited for the transmission of electromagnetic radiation in a far IR wavelength range, between 7 and 15 µm (LWIR).
[0030] The device (1) comprises a substrate (10) made of silicon Si, with for example a thickness (E10) of 1 or 2 mm. The substrate (10) has a refractive index n = 3.43 and is transparent in the aforementioned wavelength range.
[0031] The device (1) comprises a coating layer (20) of amorphous carbon, also called DLC, with a thickness (E20) of 1425 nm. The DLC has a refractive index n = 1.8 and is transparent in the aforementioned wavelength range.
[0032] The device (1) comprises a surface texturing (30) forming distinct cavities (31), which pass through the coating layer (20) and partially hollow out the substrate (10). The cavities (31) are distributed in a regular network on the surface of the device (1). The cavities (31) have a periodicity (L31) of 2 µm, a diameter (D31) of 1.6 µm, and a depth (P31) of the order of 2.34 µm. The cavities (31) penetrate into the substrate (10), in a textured layer (11) having a depth (P11) of 915 nm, much less than the thickness (E10) of the substrate (10). The texturing (30) makes it possible to lower the effective refractive index in the textured layer (11) of the substrate (10), in a controlled manner.
[0033] Texturing (30) can be achieved using any suitable technique to penetrate the coating layer (20) and partially etch the substrate (10), for example, laser ablation, photolithography, nanoprinting, etc. Laser texturing is relatively inexpensive and well-established. In particular, texturing (30) can be performed using an ultrashort laser with a pulse duration in the femtosecond or picosecond range. The laser wavelength, which typically ranges from 200 to 16,000 nm, is selected according to the desired texturing characteristics (30), such as the shape and dimensions of the cavities (31), patterns, periodicity, etc.
[0034] The following references can be consulted to configure the laser system: YU (2013), “Femtosecond laser nanomachining initiated by ultraviolet multiphoton ionization”, Optics Express. SEDAO (2012), “Large area laser surface micro / nanopatterning by contact microsphere lens arrays”, Applied Physics A.
[0035] On the figures 3 à 6 different devices (2, 3, 4, 5) not in accordance with the invention are shown. Apart from the differences detailed below, the substrate (10), the coating layer (20) and the texturing (30) have the same characteristics as for the device (1) described above.
[0036] On the figure 3 , the device (2) is constituted by a substrate (10) in silicon Si and a coating (20) in DLC, not textured.
[0037] On the figure 4 , the device (3) consists of a substrate (10) made of textured, but uncoated, silicon Si. The substrate (10) of the device (3) has the same thickness as the device (1). The cavities (31) have the same depth (P31) for both devices (1, 3).
[0038] On the figure 5 , the device (4) consists of a substrate (10) made of untextured silicon Si and a coating (20) made of textured DLC. The cavities (31) pass through the coating (20), but do not penetrate the substrate (10).
[0039] On the figure 6 , the device (5) is constituted by a substrate (10) made of untextured and uncoated Si.
[0040] The substrate (10) of the device (3) has the same thickness as the substrate (10) of the device (1).
[0041] On the figure 7 , the graph includes five curves showing the evolution of the transmission (T1, T2, T3, T4, T5) as a function of the wavelength (WL), for the devices (1, 2, 3, 4, 5). On the abscissa, the wavelength (WL) varies between 3 and 15 µm. On the ordinate, the transmission (T) varies from 0 to 1. The transmission curve (T1) corresponds to the device (1) shown in figures 1 et 2 . The transmission curve (T2) corresponds to the device (2) shown in the figure 3 . The transmission curve (T3) corresponds to the device (3) shown in the figure 4 . The transmission curve (T4) corresponds to the device (4) shown in the figure 5 . The transmission curve (T5) corresponds to the device (5) shown in the figure 6 .
[0042] As shown in the graph of the figure 7 , the transmission (T1) of the device (1) is improved compared to each of the devices (2, 3, 4, 5), at the level of the spectral width and the maximum transmission (therefore minimum absorption).
[0043] The transmissions (T1, T3) show a cut-off around 3 to 5 µm, possibly linked to the depth of the cavities (31) penetrating the substrate (10).
[0044] On the figures 8 And 9 , the graphs include two curves showing the evolution of the transmission (T1, T2) as a function of the angle of incidence (Angle), for the devices (1, 2). We note that the angular transmission width is greater for the device (1) than for the device (2).
[0045] On the figures 10 et 11 , the diagrams show the evolution of the transmission (T1, T2) as a function of the wavelength (WL) and the angle of incidence (Angle). The evolution of the transmission (T1, T2) is represented in two dimensions, by shades of color. It can be seen that the transmission range is larger for device (1) than for device (2), except for wavelengths (WL) around 3 to 5 µm.
[0046] The structure of the device (1) forms a two-layer system, comprising a textured coating layer (20) and a textured layer (11) of the substrate (10), overlying the untextured part of the substrate (10).
[0047] By means of the texturing (30), the structure of the device (1) makes it possible to obtain improved anti-reflective performance compared to the devices (2, 3, 4, 5).
[0048] The anti-reflective performance of the device (1) is comparable to that of multi-layer systems comprising several superimposed coating layers (20). The implementation of the texturing (30) is particularly advantageous when the application of multi-layer coatings is not possible, practical or desirable.
[0049] On the figure 12 is represented a graph analogous to the figure 7 , showing the evolution of the transmission (T1, T2, T3, T4, T5), for five devices (1, 2, 3, 4, 5) configured as in the figures 1 à 5 , with a coating layer (20) of silicon dioxide SiO2 deposited on a substrate (10) of zinc selenide ZnSe. On the abscissa, the wavelength (WL) varies from 0.8 to 3 µm, in the near and mid IR range. On the ordinate, the transmission (T) varies from 0.7 to 1.
[0050] For devices (1, 2, 3, 4, 5), the zinc selenide ZnSe substrate (10) has a refractive index n = 2.46.
[0051] For devices (1, 2, 4), the silicon dioxide SiO2 coating layer (20) has a thickness (E20) of 230 nm and a refractive index n = 1.44.
[0052] For devices (1, 3, 4), the cavities (31) have a periodicity (L31) of 320 nm and a diameter (D31) of 265 nm.
[0053] For devices (1, 4), the cavities (31) have a depth (P31) of the order of 400 nm.
[0054] The device (1) is well suited to the transmission of electromagnetic radiation in a near and mid IR wavelength range, between 0.8 and 3 µm.
[0055] As shown in the graph of the figure 12 , the transmission (T1) of the device (1) is improved compared to each of the devices (2, 3, 4, 5), at the level of the spectral width and the maximum transmission (therefore minimum absorption).
[0056] On the figure 13 , the graph includes two curves showing the evolution of the transmission (T1, T2) as a function of the angle of incidence (Angle), for the devices (1, 2) described above in line with the figure 12 . It is observed that the angular transmission width is greater for device (1) than for device (2).
[0057] On the figure 14 is represented a graph analogous to the figure 7 , showing the evolution of the transmission (T1, T2, T3, T4, T5), for five devices (1, 2, 3, 4, 5) configured as in the figures 1 à 5 , with a coating layer (20) of magnesium fluoride MgF2 deposited on a substrate (10) of silicon dioxide SiO2. On the abscissa, the wavelength (WL) varies from 0.3 to 1 µm, in the visible, near and mid-IR range. On the ordinate, the transmission (T) varies from 0.96 to 1.
[0058] For devices (1, 2, 3, 4, 5), the substrate (10) made of silicon dioxide SiO2 has a refractive index n = 1.44.
[0059] For devices (1, 2, 4), the coating layer (20) of magnesium fluoride MgF2 has a thickness (E20) of 57 nm and a refractive index n = 1.38.
[0060] For devices (1, 3, 4), the cavities (31) have a periodicity (L31) of 202 nm and a diameter (D31) of 160 nm.
[0061] For devices (1, 4), the cavities (31) have a depth (P31) of the order of 94 nm.
[0062] The device (1) is well suited for the transmission of electromagnetic radiation in a visible wavelength range, between 0.38 and 0.78 µm.
[0063] As shown in the graph of the figure 14 The transmission (T1) of device (1) is improved compared to the transmissions (T2, T5) of devices (2, 5) in terms of spectral width and maximum transmission (and therefore minimum absorption). However, the transmission (T1) of device (1) is relatively close to the transmissions (T3, T4) of devices (3, 4).
[0064] On the figure 15 , the graph includes two curves showing the evolution of the transmission (T1, T2) as a function of the angle of incidence (Angle), for the devices (1, 2) described above in line with the figure 14 . It is observed that the angular transmission width is greater for device (1) than for device (2).
[0065] On the figure 16 is represented a graph analogous to the figure 7 , showing the evolution of the transmission (T1, T2, T3, T4, T5), for five devices (1, 2, 3, 4, 5) configured as in the figures 1 à 5 , with a coating layer (20) of silicon dioxide SiO2 deposited on a substrate (10) of alumina Al2O3. On the abscissa, the wavelength (WL) varies from 0.3 to 1 µm, in the visible, near and medium IR range. On the ordinate, the transmission (T) varies from 0.96 to 1.
[0066] For devices (1, 2, 3, 4, 5), the substrate (10) made of alumina Al2O3 has a refractive index n = 1.69.
[0067] For devices (1, 2, 4), the coating layer (20) of silicon dioxide SiO2 has a thickness (E20) of 83 nm and a refractive index n = 1.44.
[0068] For devices (1, 3, 4), the cavities (31) have a periodicity (L31) of 176 nm and a diameter (D31) of 159 nm.
[0069] For devices (1, 4), the cavities (31) have a depth (P31) of the order of 156 nm.
[0070] The device (1) is well suited for the transmission of electromagnetic radiation in a visible, near and mid-IR wavelength range, between 0.3 and 1 µm.
[0071] As shown in the graph of the figure 16 , the transmission (T1) of the device (1) is improved compared to each of the devices (2, 3, 4, 5), at the level of the spectral width and the maximum transmission (therefore minimum absorption), in particular for a near and medium IR wavelength range.
[0072] Other variants of a device (1) according to the invention are shown in figures 17 à 37 . For the sake of simplification, the constituent elements comparable to those of the first embodiment described above bear the same numerical references.
[0073] On the figure 17 , the cavities (31) are distributed on the surface of the device (1) with a variable periodicity. This variable periodicity evolves according to a defined rule and not randomly. The cavities (31) are distinct and not in communication with each other. The variations are controlled, they are not due to an irregular surface state of the device (1) and / or to the inaccuracies of the texturing process. The periodicity is different between the center and the edges of the device (1). The cavities (31) are closer together in the center than on the edges.
[0074] On the figure 18 , the cavities (31) have a symmetrical concave profile in an axial plane, with a diameter (D31) and a section of area decreasing with depth (P31).
[0075] On the figure 19 , the cavities (31) have an asymmetrical concave profile in an axial plane, with a larger dimension (D31) and a decreasing area section with depth (P31). If the section is circular, the larger dimension (D31) is a diameter, otherwise for a non-circular section, the larger dimension (D31) is a length. In practice, the texturing (30) produces different optical effects depending on the orientation of the incident radiation. This phenomenon is reinforced by the asymmetry of the cavities (31).
[0076] On the figure 20 , the cavities (31) have different depths (P31a, P31b).
[0077] On the figure 21 , the cavities (31) have different diameters (D31a, D31b).
[0078] On the figure 22 The device (1) comprises a stack of two substrates (10) and two alternating coating layers (20). The cavities (31) are formed only in the first combination (10+20) of a substrate (10) and a coating layer (20), oriented with the upper side facing upward, receiving the incident radiation. In the case of a multilayer broadband antireflective device (1), this solution improves wavefront correction compared to a non-textured multilayer device. This solution also represents a time saving compared to a multilayer device in which all layers (20, 30) are traversed by the cavities (31), as described below.
[0079] On the figure 23 , the device (1) also comprises a stack of two substrates (10) and two coating layers (20) alternating. The cavities (31) pass entirely through the stack except for the last substrate (10), which is partially hollowed out.
[0080] On the figure 24 , the device (1) according to the invention comprises a rear layer (40) made of a material different from the substrate (10) and the coating layer (20). The coating (20) is formed on a first side of the substrate (10), while the rear layer (40) is formed on a second side of the substrate (10) opposite the first side. The rear layer (40) has a different function from the coating layer (20). For example, in the case of an anti-reflective device (1), this rear layer (40) can provide anti-reflective and mechanical functions on the rear face, while the coating layer (20) has a broadband anti-reflective function. According to another example, in the case of a mirror device (1), this rear layer (40) can be designed to reflect part of the radiation.
[0081] On the figure 25 , the device (1) comprises two faces configured according to the invention, with a central substrate (10). Each face comprises a coating layer (20) and a texturing (30), forming cavities (31) which pass through the coating layer (20) and partially penetrate the substrate (10). The two coating layers (20) may be identical or different (materials, thicknesses, etc.).
[0082] As illustrated in the figure 28 , in the case where there is no diffraction order, the behavior of a surface of the device (1) does not depend on the direction of the optical path. That is, the direction of passage of light from air to the device (1) or from the device (1) to air does not change the reflection and transmission rates of the device (1). The figure 28 shows schematically that under these conditions, whatever the direction of the device (1), then for an incident optical radiation (I), the reflected (R) and transmitted (T) optical radiation are the same.
[0083] Additionally, as illustrated in the figure 29 , if the coherence length of light does not exceed the thickness of the device (1), then the device (1) shown in the figure 25 can be considered as the assembly of two independent simple devices (1a, 1b) that have been juxtaposed. The transmission rate of the device (1) illustrated is then the multiplication of the transmission rates of these two independent simple devices.
[0084] This configuration increases the performance of the device (1), since the optical system is thus equipped with a double wavefront correction device. This solution is advantageous for improving wavefront correction, because it allows the use of both sides of the same device (1) to correctly correct the wavefront twice, instead of adding a second device in addition to the first. The overall size remains moderate.
[0085] On the figure 26 , the device (1) comprises a first face configured according to the invention, with a coating layer (20) and a texturing (30) partially penetrating into the substrate (10), and a second face with a coating layer (20) which is devoid of texturing, or devoid of treatment, or receives a treatment different from the texturing of the first face. In accordance with the explanations given above, with reference to the figures 25 , 28 et 29 , this configuration makes it possible to have the equivalent of two complementary devices (1). The second face being adapted in terms of treatment or texturing, this solution makes it possible to choose the effect(s) that one wishes to have, for one or more wavelength ranges. In a first example, different treatments can be applied in the same wavelength range, for example a V-shaped anti-reflection treatment and a broadband anti-reflection treatment. According to a second example, different treatments can be applied in different wavelength ranges. According to a third example, the same treatment can be applied in two separate, juxtaposed or overlapping wavelength ranges. If the two wavelength ranges treated by each of the faces are juxtaposed or overlapping, the device (1) can be used to treat a larger range than with a single-sided device.Alternatively, if the two wavelength ranges processed by each of the faces are disjoint, the device (1) can perform the role of a filter. According to a particular application, there can be a first wavefront correction processing for a first wavelength range associated with a first detector, and a second wavefront correction processing for a second wavelength range associated with a second detector.
[0086] On the figure 27 , the device (1) comprises two faces configured according to the invention, with a central layer (20 / 40). Each face comprises a coating layer (20) and a texturing (30), forming cavities (31) which pass through the coating layer (20) and partially penetrate the substrate (10). The substrate (10) and coating layers (20) of the two faces may be identical or different (materials, thicknesses, etc.).
[0087] On the figure 30 , the device (1) comprises two stacks of substrate (10) and coating (20), as well as a back layer (40). The cavities (31) are formed only in the first combination (10+20) of a substrate (10) and a coating layer (20), oriented on the upper side, receiving the incident radiation. From such a configuration, several tests were carried out.
[0088] The first test concerns wavelengths in the visible range, between 350nm and 750nm. The device (1) is configured as follows: the substrate (10) is HfO2, the coating (20) is SiO2, and the back layer (40) is amorphous carbon; the first coating thickness (E201) measures 98 nm; the first substrate thickness (E101) measures 409 nm; the second coating thickness (E202) measures 174 nm; the second substrate thickness (E102) measures 73 nm; the thickness of the back layer (40) is not imposed; the cavities (31) of the texturing (30) have a depth of 377 nm, thus passing through the first coating layer (20) and partially digging the first substrate layer (10). They are circular with a diameter of 138 nm, and regularly distributed according to a square matrix with a pitch of 174 nm.
[0089] There figure 31 shows the transmission curve (T3) of this device (1), compared: with the transmission curve (T2) of a device comprising the same stacks of substrate (10) and coating (20) and back layer (40), but without texturing (30); with the transmission curve (T1) of a device comprising only a layer of amorphous carbon.
[0090] It is clearly seen that the device (1) according to the above configuration makes it possible to obtain improved transmission compared to the other two configurations, and over a much larger wavelength range.
[0091] The second test concerns wavelengths in the near-infrared range, between 1 and 2 µm. The device (1) is configured as follows: the substrate (10) is Si3N4, the coating (20) is SiO2, and the back layer (40) is ZnSe; the first coating thickness (E201) measures 228 nm; the first substrate thickness (E101) measures 452 nm; the second coating thickness (E202) measures 461 nm; the second substrate thickness (E102) measures 166 nm; the thickness of the back layer (40) is not imposed; the cavities (31) of the texturing (30) have a depth of 351 nm, thus passing through the first coating layer (20) and partially digging the first substrate layer (10). The cavities (31) are circular with a diameter of 255 nm, and regularly distributed according to a square matrix with a pitch of 320 nm.
[0092] THE figures 32 et 33 show the transmission curve (T3) of this device (1), compared: with the transmission curve (T2) of a device comprising the same stacks of substrate (10) and coating (20) and backing layer (40), but without texturing (30); with the transmission curve (T1) of a device comprising only one layer of amorphous carbon (only on the figure 32 ).
[0093] We can clearly see on the figure 32 that the device (1) according to the above configuration makes it possible to obtain improved transmission compared to the other two configurations, and over a much larger wavelength range.
[0094] We see on the figure 33 that depending on the angle of incidence of the optical radiation on the device (1), the transmission (T3) of the device (1) is improved compared to the transmission (T2).
[0095] The third test concerns wavelengths in the mid-infrared range, between 7 and 15 µm. The device (1) is configured as follows: the substrate (10) is TiO2, the coating (20) is DLC, and the back layer (40) is Si; the first coating thickness (E201) measures 1393 nm; the first substrate thickness (E101) measures 541 nm; the second coating thickness (E202) measures 2843 nm; the second substrate thickness (E102) measures 838 nm; the thickness of the back layer (40) is not imposed; the cavities (31) of the texturing (30) have a depth of 1934 nm, thus passing through the first coating layer (20) and partially digging the first substrate layer (10). The cavities (31) are circular with a diameter of 1600 nm, and regularly distributed according to a square matrix with a pitch of 2000 nm.
[0096] THE figures 34 et 35 show the transmission curve (T3) of this device (1), compared: with the transmission curve (T2) of a device comprising the same stacks of substrate (10) and coating (20) and backing layer (40), but without texturing (30); with the transmission curve (T1) of a device comprising only one layer of amorphous carbon (only on the figure 34 ).
[0097] We can clearly see on the figure 34 that the device (1) according to the above configuration makes it possible to obtain improved transmission compared to the other two configurations, and over a much larger wavelength range.
[0098] We see on the figure 35 that depending on the angle of incidence of the optical radiation on the device (1), the transmission (T3) of the device (1) is improved compared to the transmission (T2).
[0099] The fourth test also concerns wavelengths in the mid-infrared range, between 7 and 15 µm. The device (1) is configured as follows: The substrate (10) is TiO2, the coating (20) is DLC, and the back layer (40) is Si; the first coating thickness (E201) is 1054 nm; the first substrate thickness (E101) is 2160 nm; the second coating thickness (E202) is 142 nm; the second substrate thickness (E102) is 1293 nm; the thickness of the back layer (40) is not specified; the cavities (31) of the texture (30) are 1968 nm deep, thus penetrating the first coating layer (20) and partially cutting into the first substrate layer (10). The cavities (31) are circular with a diameter of 1600 nm and are regularly distributed in a square matrix with a 2000 nm spacing.
[0100] THE figures 36 et 37 show the transmission curve (T3) of this device (1), compared: with the transmission curve (T2) of a device comprising the same stacks of substrate (10) and coating (20) and backing layer (40), but without texturing (30); with the transmission curve (T1) of a device comprising only one layer of amorphous carbon (only on the figure 36 ).
[0101] We can clearly see on the figure 36 that the device (1) according to the above configuration makes it possible to obtain improved transmission compared to the other two configurations, and over a much larger wavelength range.
[0102] We see on the figure 37 that depending on the angle of incidence of the optical radiation on the device (1), the transmission (T3) of the device (1) is improved compared to the transmission (T2).
[0103] Furthermore, the device (1) can be shaped differently from figures 1 à 37without departing from the scope of the invention, which is defined by the claims. Furthermore, the technical characteristics of the different embodiments and variants mentioned above can be, in whole or in part, combined with each other. Thus, the device (1) can be adapted in terms of cost, functionality and performance.
Claims
1. Optical device (1), adapted for the transmission / reflection of electromagnetic radiation in a wavelength range of the electromagnetic spectrum corresponding to infrared radiation, without diffraction order, in which the direction of light passing from air to the device (1) or from the device (1) to air does not change the reflection and transmission rates of the device (1), said device (1) comprising at least: - a substrate (10) made from a first material selected from the following: silicon Si, germanium Ge, zinc sulfide ZnS, zinc selenide ZnSe, - a coating layer (20) formed on a first side of the substrate (10) and made from a second material, different from the first material, this second material being selected from the following: silicon Si, germanium Ge, zinc sulfide ZnS, zinc selenide ZnSe, tantalum pentoxide Ta2O5, hafnium dioxide HfO2, alumina Al2O3, and - a surface texturing (30) forming cavities (31) in the device (1), varying the effective refractive index on the surface of the device, the cavities (31) passing through the coating layer (20) and partially digging into the substrate (10), - at least one backside layer (40), formed on a second side of the substrate (10) opposite the first side, with a function different from that of the coating layer (20), made from a material different from the substrate (10) and the coating (20), the material of the backside layer being selected from the following: silicon Si, germanium Ge, zinc sulfide ZnS, or zinc selenide ZnSe.
2. Device (1) according to claim 1, characterized in that the cavities (31) have a continuous profile between the coating layer (20) and the substrate (10).
3. Device (1) according to claim 1 or 2, characterized in that the cavities (31) have a circular cross-section.
4. Device (1) according to any one of claims 1 to 3, characterized in that the cavities (31) have a concave profile in an axial plane, with a cross-sectional area decreasing with depth.
5. Device (1) according to any one of claims 1 to 4, characterized in that the cavities (31) have a symmetrical concave profile in an axial plane.
6. Device (1) according to any one of claims 1 to 4, characterized in that the cavities (31) have an asymmetrical concave profile in an axial plane.
7. Device (1) according to any one of claims 1 to 6, characterized in that the cavities (31) are arranged in a regular grid pattern on the surface of the device (1).
8. Device (1) according to any one of the preceding claims, characterized in that the cavities (31) are distributed on the surface of the device (1) with variable periodicity, evolving according to a defined rule and not randomly, for example, with a different periodicity between the center and the edges of the device (1).
9. Device (1) according to any one of the preceding claims, characterized in that it comprises a stack of several substrates (10) and coating layers (20) alternately, including at least a first combination (10+20) of a first coating layer (20) and a first substrate (10), and a last combination (10+20) of a last coating layer (20) and a last substrate (10).
10. Device (1) according to claim 9, characterized in that the cavities (31) are formed only in the first combination (10+20).
11. Device (1) according to claim 9, characterized in that the cavities (31) entirely pass through the stack except for the last substrate (10), which is partially hollowed, and in that the cavities (31) have a strictly decreasing cross-sectional area toward the last substrate (10).
12. Device (1) according to any one of claims 9 to 11, characterized in that the stack includes at least one intermediate combination (10+20) between the first combination (10+20) and the last combination (10+20).
13. Device (1) according to any one of claims 1 to 12, characterized in that it comprises two faces, each with a coating layer (20) and a surface texturing (30) forming cavities (31) passing through the coating layer and partially penetrating the substrate or one of the substrates.
14. Device (1) according to any one of claims 1 to 12, characterized in that it comprises a first face with a coating layer (20) and a surface texturing (30) forming cavities (31) passing through the coating layer (20) and partially penetrating the substrate (10) or one of the substrates (10), and a second face with a coating layer (20) that is free of texturing, unprocessed, or receives a different treatment from the texturing of the first face.
15. A method for manufacturing an optical device, adapted for the transmission / reflection of electromagnetic radiation in a wavelength range of the electromagnetic spectrum corresponding to infrared radiation, in which the direction of light passing from air to the device (1) or from the device (1) to air does not change the reflection and transmission rates of the device (1), said method comprising at least the following steps: - forming at least one combination: * a substrate made from a first material selected from the following: silicon Si, germanium Ge, zinc sulfide ZnS, zinc selenide ZnSe, * a coating layer made from a second material different from the first material, this second material being selected from the following: silicon Si, germanium Ge, zinc sulfide ZnS, zinc selenide ZnSe, tantalum pentoxide Ta2O5, hafnium dioxide HfO2, alumina Al2O3, and * a backside layer, with a function different from that of the coating layer (20), made from a material different from the substrate and the coating, the material of the backside layer being selected from the following: silicon Si, germanium Ge, zinc sulfide ZnS, or zinc selenide ZnSe, the coating being formed on a first side of the substrate, the backside layer being formed on a second side of the substrate opposite the first side, then - performing surface texturing forming cavities in the device, varying the effective refractive index on the surface of the device, the cavities passing through the coating layer and partially digging into the substrate.