RUBBER COMPOSITION
Eugenol derivatives in rubber compositions address oxidation issues in tires by enhancing aging resistance and mechanical properties, providing a sustainable solution to fossil-based anti-oxidants.
Patent Information
- Application Number
- FR2021006816
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-25
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-06-25
AI Technical Summary
Rubber articles, particularly tires, are susceptible to oxidation during aging, and existing anti-oxidants often rely on fossil-based compounds, necessitating the development of eco-friendly alternatives.
Incorporating eugenol or its derivatives as a phenolic antioxidant in rubber compositions comprising a diene elastomer, reinforcing filler, and crosslinking system, which are derived from natural sources like cloves, to protect against oxidation and enhance composition properties.
Eugenol derivatives effectively improve the rubber composition's resistance to oxidation, maintaining mechanical properties during aging, offering a sustainable alternative to fossil-based anti-oxidants.
Abstract
Description
Title of the invention: RUBBER COMPOSITION
[0001] The field of the present invention is that of rubber compositions, the rubber compositions being particularly intended for use in rubber articles such as, for example, tires.
[0002] Rubber articles are sensitive to oxidation, particularly during their aging, and require protection systems against this oxidation. Certain antioxidants exist and are used by those skilled in the art.
[0003] Nevertheless, it is interesting today to look for antioxidants that can be of natural origin in order to limit compounds of fossil origin in rubber articles, and in particular in tires.
[0004] Eugenol and its possible derivatives are known to be easily obtained from plants such as cloves. Eugenol is mainly used today in cosmetic and dental care applications.
[0005] Continuing its research, the Applicant discovered that the use of eugenol or a eugenol derivative in a rubber composition comprising a diene elastomer, a reinforcing filler and a crosslinking system, makes it possible to protect this composition against oxidation and thus to improve the properties of this composition after aging.
[0006] Thus, a first subject of the invention is a rubber composition based on at least one diene elastomer, a reinforcing filler, a crosslinking system and a phenolic antioxidant of general formula [Chem 1] below, in which the radical RI represents a hydrogen atom, an alkyl group comprising from 1 to 18 carbon atoms, or an alkoxy group comprising from 1 to 18 carbon atoms, and the radicals R2 to R7 each represent, independently of one another, a hydrogen atom or a hydrocarbon group comprising from 1 to 18 carbon atoms.
[0007] [Chem.l] Ri
[0008] Another subject of the invention is a pneumatic or non-pneumatic tire comprising a composition according to the invention. I- DEFINITIONS
[0009] The expression "composition based on" means a composition comprising the mixture and / or the in situ reaction product of the different constituents used, some of these constituents being able to react and / or being intended to react with each other, at least partially, during the different phases of manufacture of the composition; the composition thus being able to be in a totally or partially crosslinked state or in a non-crosslinked state.
[0010] By the expression "part by weight per hundred parts by weight of elastomer" (or pce), it is meant, within the meaning of the present invention, the part, by mass per hundred parts by mass of elastomer.
[0011] In this document, unless expressly indicated otherwise, all percentages (%) indicated are percentages (%) by mass.
[0012] On the other hand, any interval of values designated by the expression "between a and b" represents the range of values from more than a to less than b (i.e., excluding limits a and b), while any interval of values designated by the expression "from a to b" means the range of values from a to b (i.e., including the strict limits a and b). In the present document, when an interval of values is designated by the expression "from a to b", the interval represented by the expression "between a and b" is also and preferably designated.
[0013] When a "majority" compound is referred to, within the meaning of the present invention, this compound is the majority among the compounds of the same type in the composition, that is to say that it is the one which represents the largest quantity by mass among the compounds of the same type. Thus, for example, a majority elastomer is the elastomer representing the largest mass relative to the total mass of the elastomers in the composition. In the same way, a so-called majority filler is the one representing the largest mass among the fillers in the composition. For example, in a system comprising a single elastomer, this is the majority within the meaning of the present invention; and in a system comprising two elastomers, the majority elastomer represents more than half of the mass of the elastomers. On the contrary, a "minority" compound is a compound which does not represent the largest mass fraction among the compounds of the same type.Preferably by majority, we mean present at more than 50%, preferably more than 60%, 70%, 80%, 90%, and more preferably the “majority” compound represents 100%.
[0014] The compounds mentioned in the description may be of fossil or biosourced origin. In the latter case, they may be, partially or totally, derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, the compounds mentioned may also come from the recycling of materials already in use, i.e. they may be, partially or totally, derived from a recycling process, or obtained from raw materials themselves derived from a recycling process. This includes polymers, plasticizers, fillers, etc.
[0015] Unless otherwise indicated, the glass transition temperature values "Tg" described herein are measured in a known manner by DSC (Differential Scanning Calorimetry) according to ASTM D3418 (1999). II- DESCRIPTION OF THE INVENTION
[0016] II-1 Elastomeric matrix
[0017] By "diene" elastomer (or indistinctly rubber), whether natural or synthetic, must be understood in a known manner an elastomer consisting at least in part (i.e., a homopolymer or a copolymer) of diene monomer units (monomers carrying two carbon-carbon double bonds, conjugated or not).
[0018] The term diene elastomer capable of being used in the compositions in accordance with the invention is particularly understood to mean:
[0019] (a) - any homopolymer of a diene monomer, conjugated or not, having from 4 to 18 carbon atoms;
[0020] (b) - any copolymer of a diene, conjugated or not, having from 4 to 18 carbon atoms and at least one other monomer.
[0021] The other monomer may be ethylene, an olefin or a diene, conjugated or not.
[0022] Suitable conjugated dienes are conjugated dienes having from 4 to 15 atoms. of carbon, in particular 1,3-dienes, such as 1,3-butadiene and isoprene.
[0023] Suitable non-conjugated dienes are non-conjugated dienes having 6 to 12 carbon atoms, such as 1,4-hexadiene, ethylidene norbornene, dicyclopentadiene. Suitable olefins are vinylaromatic compounds having from 8 to 20 carbon atoms and aliphatic α-monoolefins having from 3 to 12 carbon atoms.
[0025] Suitable vinylaromatic compounds include, for example, styrene, ortho-, meta-, para-methylstyrene, the commercial mixture "vinyl-toluene", para-tert-butylstyrene.
[0026] Suitable aliphatic α-monoolefins include, in particular, acyclic aliphatic α-monoolefins having from 3 to 18 carbon atoms.
[0027] More particularly, the diene elastomer is:
[0028] (a') - any homopolymer of a conjugated diene monomer, in particular any homopolymer obtained by polymerization of a conjugated diene monomer having from 4 to 12 carbon atoms;
[0029] (b') - any copolymer obtained by copolymerization of one or more dienes conjugated with each other or with one or more vinylaromatic compounds having from 8 to 20 carbon atoms;
[0030] (c') - a copolymer of isobutene and isoprene (butyl rubber), as well as the halogenated versions, particularly chlorinated or brominated, of this type of copolymer.
[0031] (d') - any copolymer obtained by copolymerization of one or more dienes, conjugated or not, with ethylene, an α-monoolefin or their mixture such as for example elastomers obtained from ethylene, propylene with a non-conjugated diene monomer of the aforementioned type.
[0032] Preferably, the diene elastomer is chosen from the group consisting of polybutadienes (BR), natural rubber (NR), synthetic polyisoprenes (IR), butadiene copolymers, isoprene copolymers, and mixtures of these elastomers. The butadiene copolymers are particularly chosen from the group consisting of butadiene-styrene copolymers (SBR).
[0033] The diene elastomer can be modified, i.e. either coupled and / or star-shaped, or functionalized, or coupled and / or star-shaped and simultaneously functionalized.
[0034] Thus, the diene elastomer can be coupled and / or star-shaped, for example by means of a silicon or tin atom which links the elastomer chains together.
[0035] The diene elastomer may be simultaneously or alternatively functionalized and comprise at least one functional group. By functional group is meant a group comprising at least one heteroatom chosen from Si, N, S, O, P. Particularly suitable functional groups are those comprising at least one function such as: silanol, an alkoxysilane, a primary, secondary or tertiary amine, cyclic or not, a thiol, an epoxide.
[0036] The rubber composition of the invention may contain a single diene elastomer or a mixture of several diene elastomers.
[0037] 11-2 Specific antioxidant
[0038] According to the invention, the rubber composition is based on at least one phenolic antioxidant of general formula [Chem 1] below,
[0039] [Chem.l]
[0040] in which:
[0041] - the radical RI represents a hydrogen atom, an alkyl group comprising from 1 to 18 carbon atoms, or an alkoxy group comprising from 1 to 18 carbon atoms,
[0042] - the radicals R2 to R7 each represent, independently of one another, a hydrogen atom or a hydrocarbon group comprising from 1 to 18 carbon atoms.
[0043] Preferably, the RI group is a hydrogen atom, a methyl, ethyl, isopropyl, tert-butyl group or a methoxy group.
[0044] Also preferably, the radicals R2 to R7 each represent, independently of one another, a hydrogen atom, an alkyl group comprising from 1 to 18 carbon atoms, or an aryl group comprising from 6 to 18 carbon atoms. More preferably, the radicals R2 to R7 each represent, independently of one another, a hydrogen atom, a methyl, ethyl, isopropyl, or tert-butyl group.
[0045] Very preferably, the phenolic antioxidant of general formula [Chem 1] is eugenol of formula [Chem 2] below.
[0046] [Chem.2]
[0047] Eugenol and its derivatives of general formula [Chem 1] above have the advantage of being able to be biosourced since eugenol can be easily extracted from plants and in particular from cloves, and its derivatives can be obtained by simple chemical modifications within the reach of any chemist.
[0048] Preferably for the purposes of the invention, the phenolic antioxidant of general formula [Chem 1] is present in the composition at a level within a range ranging from 0.2 to 10 pce, preferably from 0.5 to 8 pce and more preferably from 0.8 to 5 pce.
[0049] 11-3 Reinforcing charge
[0050] The rubber composition in accordance with the invention has the other essential characteristic of comprising a reinforcing filler.
[0051] Any type of so-called reinforcing filler, known for its ability to reinforce a rubber composition which can be used in particular for the manufacture of tires, can be used, for example an organic filler such as carbon black, an inorganic filler such as silica or even a mixture of these two types of fillers.
[0052] Suitable carbon blacks are all carbon blacks, in particular the blacks conventionally used in tires or their treads. Among the latter, mention will be made more particularly of the reinforcing carbon blacks of the 100, 200, 300 series, or the blacks of the 500, 600 or 700 series (ASTM D-1765-2017 grades), such as for example blacks NI 15, N134, N234, N326, N330, N339, N347, N375, N550, N683, N772). These carbon blacks can be used in the isolated state, as commercially available, or in any other form, for example as a support for certain of the rubber additives used. Carbon blacks could, for example, already be incorporated into the diene elastomer, in particular isoprene, in the form of a masterbatch (see, for example, applications WO97 / 036724-A2 or WO99 / 016600-Al).
[0053] As an example of organic fillers other than carbon blacks, mention may be made of functionalized polyvinyl organic fillers as described in applications WO2006 / 069792-A1, WO2006 / 069793-A1, WO2008 / 003434-A1 and WO2008 / 003435-A1.
[0054] By "reinforcing inorganic filler" is meant here any inorganic or mineral filler, whatever its color and origin (natural or synthetic), also called "white" filler, "clear" filler or even "non-black" filler as opposed to carbon black, capable of reinforcing on its own, without any other means than an intermediate coupling agent, a rubber composition intended for the manufacture of tires. In a known manner, certain reinforcing inorganic fillers can be characterized in particular by the presence of hydroxyl groups (OH) on their surface.
[0055] Suitable reinforcing inorganic fillers include, in particular, mineral fillers of the siliceous type, preferably silica (SiO2) or of the aluminous type, in particular alumina (A12O3). The silica used may be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenic silica having a BET specific surface area and a CTAB specific surface area, both less than 450 m2 / g, preferably within a range of 30 to 400 m2 / g, in particular 60 to 300 m2 / g.
[0056] Any type of precipitated silica may be used, in particular highly dispersible precipitated silicas (known as "HDS" for "highly dispersible" or "highly dispersible silica"). These precipitated silicas, whether highly dispersible or not, are well known to those skilled in the art. Examples that may be mentioned are the silicas described in applications WO03 / 016215-A1 and WO03 / 016387-A1. Among the commercial HDS silicas, we can notably use the silicas “Ultrasil ® 5000GR”, “Ultrasil ® 7000GR” from the company Evonik, the silicas “Zeosil ® 1085GR”, “Zeosil® 1115 MP”, “Zeosil® 1165MP”, “Zeosil® Premium 200MP”, “Zeosil® HRS 1200 MP” from the company Solvay.As non-HDS silica, the following commercial silicas can be used: silicas “Ultrasil ® VN2GR”, “Ultrasil ® VN3GR” from Evonik, silica “Zeosil® 175GR” from Solvay, silicas “Hi-Sil EZ120G(-D)”, “Hi-Sil EZ160G(-D)”, “Hi-Sil EZ200G(-D)”, “Hi-Sil 243LD”, “Hi-Sil 210”, “Hi-Sil HDP 320G” from PPG.
[0057] As other examples of inorganic fillers that can be used in the rubber compositions of the invention, mention may also be made of mineral fillers of the aluminous type, in particular alumina (A12O3), aluminum oxides, aluminum hydroxides, aluminosilicates, titanium oxides, silicon carbides or nitrides, all of the reinforcing type as described for example in applications WO99 / 28376-A2, WO00 / 73372-A1, WO02 / 053634-A1, WO2004 / 003067-A1, WO2004 / 056915-A2, US6610261-B1 and US6747087-B2. Examples include the aluminas “Baikalox A125” or “CR125” (Baïkowski company), “APA-100RDX” (Condéa), “Aluminoxid C” (Evonik) or “AKP-G015” (Sumitomo Chemicals).
[0058] The physical state in which the reinforcing inorganic filler is present is indifferent, whether in the form of powder, microbeads, granules, or even beads or any other suitable densified form. Of course, the term reinforcing inorganic filler also means mixtures of different reinforcing inorganic fillers, in particular silicas as described above.
[0059] Those skilled in the art will understand that, as a replacement for the reinforcing inorganic filler described above, a reinforcing filler of another nature could be used, provided that this reinforcing filler of another nature is covered with an inorganic layer such as silica, or else has functional sites on its surface, in particular hydroxyl sites, requiring the use of a coupling agent to establish the bond between this reinforcing filler and the diene elastomer. By way of example, mention may be made of carbon blacks partially or completely covered silica, or silica-modified carbon blacks, such as, but not limited to, “Ecoblack®” type fillers of the “CRX2000” series or the “CRX4000” series from Cabot Corporation.
[0060] Preferably for the invention, the reinforcing filler is chosen from the group consisting of carbon blacks, silicas and their mixtures.
[0061] A person skilled in the art will be able to adapt the total reinforcing filler rate according to the use concerned, in particular for example according to the type of tire concerned, for example a tire for a motorcycle, for a passenger vehicle or even for a utility vehicle such as a van or heavy goods vehicle. Preferably, this total reinforcing filler rate is within a range from 10 to 200 pce, more preferably from 30 to 180 pce, and even more preferably from 40 to 160 pce; the optimum being, in a known manner, different according to the particular applications targeted.
[0062] In the present disclosure, the BET specific surface area is determined by gas adsorption using the Brunauer-Emmett-Teller method described in "The Journal of the American Chemical Society" (Vol. 60, page 309, February 1938), and more precisely according to a method adapted from standard NF ISO 5794-1, appendix E of June 2010 [multipoint volumetric method (5 points) - gas: nitrogen - vacuum degassing: one hour at 160°C - relative pressure range p / po: 0.05 to 0.17].
[0063] For inorganic fillers such as silica for example, the CT AB specific surface area values were determined according to standard NF ISO 5794-1, annex G of June 2010. The process is based on the adsorption of CTAB (N-hexadecyl-N,N,N-trimethylammonium bromide) on the “external” surface of the reinforcing filler.
[0064] To couple the reinforcing inorganic filler to the diene elastomer, it is possible to use, in a well-known manner, an at least bifunctional coupling agent (or bonding agent) intended to ensure a sufficient connection, of a chemical and / or physical nature, between the inorganic filler (surface of its particles) and the diene elastomer. In particular, at least bifunctional organosilanes or polyorganosiloxanes are used. By "bifunctional", we mean a compound having a first functional group capable of interacting with the inorganic filler and a second functional group capable of interacting with the diene elastomer.For example, such a bifunctional compound may comprise a first functional group comprising a silicon atom, said first functional group being capable of interacting with the hydroxyl groups of an inorganic filler and a second functional group comprising a sulfur atom, said second functional group being capable of interacting with the diene elastomer.
[0065] Preferably, the organosilanes are chosen from the group consisting of polysulfurized organosilanes (symmetrical or asymmetrical) such as tetrasulfide of bis(3-triethoxy silylpropyl), abbreviated TESPT marketed under the name "Si69" by the company Evonik or bis-(triethoxysilylpropyl) disulfide, abbreviated TESPD marketed under the name "Si75" by the company Evonik, polyorganosiloxanes, mercaptosilanes, blocked mercaptosilanes, such as S-(3-(triethoxysilyl)propyl) octanethioate marketed by the company Momentive under the name "NXT Silane". More preferably, the organosilane is a polysulfurized organosilane.
[0066] Of course, mixtures of the coupling agents described above could also be used.
[0067] The content of coupling agent in the composition of the invention is advantageously less than or equal to 30 phr, it being understood that it is generally desirable to use as little as possible. Typically the level of coupling agent represents from 0.5% to 15% by weight relative to the amount of reinforcing inorganic filler. Its level is preferably within a range from 0.5 to 20 phr, more preferably within a range from 3 to 3 phr. This level is easily adjusted by a person skilled in the art according to the level of reinforcing inorganic filler used in the composition of the invention.
[0068] 11-4 Crosslinking system
[0069] The crosslinking system may be any type of system known to those skilled in the art in the field of tire rubber compositions. It may in particular be based on sulfur, and / or peroxide and / or bismaleimides.
[0070] Preferably, the crosslinking system is based on sulfur, in which case it is referred to as a vulcanization system. The sulfur can be provided in any form, in particular in the form of molecular sulfur, or a sulfur-donating agent. At least one vulcanization accelerator is also preferably present, and, optionally, also preferably, various known vulcanization activators can be used such as zinc oxide, stearic acid or equivalent compound such as stearic acid salts and transition metal salts, guanidine derivatives (in particular diphenylguanidine), or even known vulcanization retarders.
[0071] Sulphur is used at a preferential rate of between 0.2 pce and 10 pce, more preferably between 0.3 and 7 pce. The primary vulcanisation accelerator is used at a preferential rate of between 0.5 and 10 pce, more preferably between 0.5 and 5 pce.
[0072] Any compound capable of acting as an accelerator for the vulcanization of diene elastomers in the presence of sulfur may be used as an accelerator, in particular accelerators of the thiazole type and their derivatives, accelerators of the sulfenamide, thiuram, dithiocarbamate, dithiophosphate, thiourea and xanthate types. Examples of such accelerators include, in particular: the following compounds: 2-mercaptobenzothiazyl disulfide (abbreviated as "MBTS"), N-cyclohexyl-2-benzothiazyl sulfenamide ("CBS"), N,N-dicyclohexyl-2-benzothiazyl sulfenamide ("DCBS"), N-tert-butyl-2-benzothiazyl sulfenamide ("TBBS"), N-tert-butyl-2-benzothiazyl sulfenimide ("TBSI"), tetrabenzylthiuram disulfide ("TBZTD"), zinc dibenzyldithiocarbamate ("ZBEC") and mixtures of these compounds.
[0073] 11-5 Possible additives
[0074] The rubber compositions according to the invention may optionally also comprise all or part of the usual additives usually used in elastomer compositions for tires, such as, for example, pigments, protective agents such as anti-ozone waxes, chemical anti-ozonants, antioxidants other than the phenolic antioxidant of general formula [Chem 1], anti-fatigue agents, or even reinforcing resins (as described, for example, in application WO 02 / 010269).
[0075] 11-6 Preparation of rubber compositions
[0076] The compositions in accordance with the invention can be manufactured in suitable mixers, using two successive preparation phases well known to those skilled in the art:
[0077] - a first phase of thermomechanical work or mixing (so-called “phase non-productive”), which can be carried out in a single thermomechanical step during which all the necessary constituents are introduced into a suitable mixer such as a conventional internal mixer (for example of the 'Banbury' type), in particular the elastomeric matrix, the reinforcing filler, any other various additives, with the exception of the crosslinking system. The incorporation of the possible filler into the elastomer can be carried out in one or more stages by thermomechanical mixing.In the case where the filler is already incorporated in whole or in part into the elastomer in the form of a masterbatch as described for example in applications WO 97 / 036724 or WO 99 / 016600, it is the masterbatch which is directly mixed and where appropriate the other elastomers or fillers present in the composition which are not in the form of a masterbatch are incorporated, as well as any other various additives other than the crosslinking system. The non-productive phase can be carried out at high temperature, up to a maximum temperature of between 110°C and 200°C, preferably between 130°C and 185°C, for a duration generally of between 2 and 10 minutes.
[0078] - a second phase of mechanical work (so-called “productive” phase), which is carried out in an external mixer such as a roller mixer, after cooling the mixture obtained during the first non-productive phase to a lower temperature, typically below 120°C, for example between 40°C and 100°C. The crosslinking system is then incorporated, and everything is then mixed for a few minutes, for example between 5 and 15 min.
[0079] Such phases have been described for example in applications EP-A-0501227, EP-A-0735088, EP-A-0810258, WO00 / 005300 or WO00 / 005301.
[0080] The final composition thus obtained is then calendered, for example, in the form of a sheet or plate, in particular for laboratory characterization, or extruded (or co-extruded with another rubber composition) in the form of a semi-finished (or profiled) rubber usable, for example, as a tire sidewall. These products can then be used for the manufacture of tires, according to techniques known to those skilled in the art.
[0081] The composition may be either in the raw state (before crosslinking or vulcanization), or in the cured state (after crosslinking or vulcanization), and may be a semi-finished product which may be used in a tire.
[0082] The crosslinking (or curing), where appropriate the vulcanization, is carried out in a known manner at a temperature generally between 130°C and 200°C, for a sufficient time which may vary for example between 5 and 90 min depending in particular on the curing temperature, the crosslinking system adopted and the crosslinking kinetics of the composition considered.
[0083] 11-7 Rubber articles
[0084] The present invention also relates to a rubber article comprising a rubber composition according to the invention.
[0085] Indeed, the interest presented by the properties of the rubber composition according to the invention makes it possible to envisage use in numerous fields involving rubber articles. In particular, mention may be made of use in various articles preferably chosen from pipes, belts, conveyor belts, tracks, pneumatic objects (and in particular tires), shoe soles, or even surgical gloves.
[0086] Preferably, the invention relates to a tire comprising a composition according to the invention. The tire according to the invention may be intended to equip motor vehicles of the passenger car, SUV ("Sport Utility Vehicles"), or two-wheeled type (in particular motorcycles), or airplanes, or even industrial vehicles chosen from vans, "Heavy Goods Vehicles" - that is to say metro, buses, road transport vehicles (trucks, tractors, trailers), off-road vehicles such as agricultural or civil engineering vehicles -, and others. III- EXAMPLES
[0087] III-1 Example 1
[0088]
[0089]
[0090]
[0091]
[0092]
[0093]
[0094]
[0095]
[0096]
[0097]
[0098]
[0099]
[0100] In a first example illustrating the interest of the invention, the polymer alone is considered, to be protected against thermo-oxidation. T0 corresponds to the case where the polymer is completely devoid of an antioxidant system. T1 is a control in which the polymer is protected by a known phenolic antioxidant: "Irganox 1520 L" marketed by the company BASF. Composition C1 illustrates the present invention and contains the polymer, protected against oxidation by eugenol, in an isomolar quantity of the 3.2 pce of "Irganox 1520 L". Oxidation resistance, “OIT” In order to compare the antioxidant activity of the invention in this particular case, the VOIT method ("Oxidation Induction Time") describes the oxidation delay measured by DSC caused by the presence of an antioxidant at high temperature (170°C) when a gas flow in contact with the composition is changed from helium to pure oxygen. The result is expressed in minutes. The details of the procedure followed for this determination are summarized in Table 1 below: [Tables 1] fîSC3*MerTdedô Temperature ramp used s » isothermal 60®C - 2 minutes (He - 40 mL / min), i « from 60°C to 170-C at 'ZO'C / min (He - 40mL.''mm}, s * isothermal 1 70'C - 1 minute- (He - 40 mL / miu). ; s isothermal 170°C - 12 hours (oxygen - 40 mL / min) Crucibles used i Crucibles in oxygen 40 pL - without cover Sample mass ( Between 10 and 11 mg Table 2 shows the tested compositions (in pce), the results obtained. [Tables2] T0 Tl [Cl MCI 'igo W | KM) """O.....j.............. 1 uyeiîol b ~ I L2 50 | 30 (1) Natural rubber (2) “Irganox 1520 L” marketed by BASF, MW = 424.8 g / mol, (3) 95% eugenol from Sigma Aldrich, Mw = 164.2 g / mol The results show that eugenol significantly improves VOIT from 18 to 30 min. III-2 Example 2 Example 2 aims to measure the ageing resistance performance of the invention subjected to a thermo-oxidative treatment by comparing a composition in accordance with the invention (C2), respectively with two control compositions (T2 and T3).
[0101] The rubber compositions were produced as described in point II.6 above, using an internal mixer (non-productive phase) where most of the ingredients are incorporated. The so-called productive phase is carried out on an external tool and concerns the incorporation of the sulfur and the accelerator. The different compositions were shaped, vulcanized in the form of a plate and underwent a thermo-oxidative treatment at 77°C for 0, 7, 14, 21 and 28 days. For each of these points, the properties at break are characterized by uniaxial tensile measurements (modulus, elongation).
[0102] Limit properties, modulus and elongation at break
[0103] Tensile tests are used to determine the elastic stresses and breaking properties; carried out on cooked mixtures produced in accordance with the AFNOR-NF-T46-002 standard of September 1988.
[0104] The elongations at break (in %) are measured at 23°C, under normal hygrometry conditions (50% relative humidity), according to the French standard NF T 40-101 (December 1979), and the moduli at break (in MPa).
[0105] Table 3 presents the compositions tested (in pce), and Table 4 presents the results obtained, based on 100.
[0106] [Tables3] Composition T2 T3 C2 Natural rubber (1) 100 100 100 Irganox (2) - 3.2 - Eugenol(3) - - 1.2 Carbon black (4) 60 60 60 Stearic acid 1 1 1 Zinc oxide 8 8 8 Cobalt salt (5) 1 1 1 Accelerator (6) 1 1 1 Sulphur 5 5 5
[0107] (1) Natural rubber
[0108] (2) “Irganox 1520 L” marketed by BASF, MW = 424.8 g / mol,
[0109] (3) 95% eugenol from Sigma Aldrich, MW = 164.2 g / mol
[0110] (4) Cabot Company ASTM N375 Grade Carbon Black
[0111] (5) Cobalt acetylacetonate from Sigma Aldrich
[0112] (6) Tertiobutyl-benzothiazyl sulfenamide (“TBBS”) from the company Solutia
[0113] [T ables 4] Measured property Duration aging T2 T3 C2 Modulus (MPa) initial 26 25 25 7 days 20 23 20 14 days 15 19 17 21 days 17 19 17 28 days 18 19 19 Elongation R upture (%) initial 440 500 450 7 days 170 270 200 14 days 80 190 110 21 days 70 180 100 28 days 40 130 90
[0114] The results presented in Table 4 above show that the compositions according to the invention make it possible to preserve the mechanical properties over the course of thermo-oxidative aging. This can be seen in that the properties at break of composition C2 according to the invention contract less quickly than those of composition T2 which does not contain any protective agent. The difference is even more clear and significant from 14 days of thermo-oxidative aging.
Claims
Claims
1. Rubber composition based on at least one diene elastomer, a reinforcing filler, a crosslinking system and eugenol of formula [Chem 2] as an antioxidant. [Chem.2]
2. Rubber composition according to the preceding claim, in which the level of eugenol of formula [Chem 2] is within a range from 0.2 to 10 pce, preferably from 0.5 to 8 pce and more preferably from 0.8 to 5 pce.
3. A rubber composition according to any preceding claim, wherein the reinforcing filler is selected from the group consisting of carbon blacks, silicas and mixtures thereof.
4. Rubber composition according to any one of the preceding claims, in which the total reinforcing filler content is within a range from 10 to 200 phr, preferably from 30 to 180 phr, and more preferably from 40 to 160 phr.
5. A rubber article comprising a rubber composition defined in any one of claims 1 to 4.
6. Rubber article according to the preceding claim in which the article is chosen from pipes, belts, conveyor belts, tracks, pneumatic objects (and in particular tires), shoe soles or surgical gloves.
7. A tire comprising a rubber composition defined in any one of claims 1 to 4.