Manufacturing process for a composite profile and the resulting profile
The described process addresses the limitations of existing methods by using pre-formed cords and reinforcing layers to create composite profiles with high fiber density and mechanical resistance, enhancing productivity and design flexibility.
Patent Information
- Application Number
- FR2022000390
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-18
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-01-18
AI Technical Summary
Existing methods for manufacturing composite profiles with thermoplastic matrices face challenges such as high tooling costs, limited productivity, and the inability to achieve complex sections and high fiber densities, often requiring dedicated tools for each profile section.
A process involving the use of pre-formed cords with reinforcing fibers coated in a first thermoplastic material, which are assembled around a mandrel, fused with a reinforcing layer, and calibrated to form a profile with high fiber density and mechanical resistance, using simple and shareable tooling.
This process enables high productivity and the production of profiles with complex sections and high mechanical resistance, allowing for a high fiber density and flexibility in profile design, suitable for various thermoplastic materials.
Smart Images

Figure 00000015_0000 
Figure 00000015_0001 
Figure 00000015_0002
Abstract
Description
Title of the invention: Method for manufacturing a composite profile and profile thus obtained Technical field
[0001] The invention relates to a method for manufacturing a composite profile comprising continuous fibers and a thermoplastic matrix. It also relates to a profile obtained by this manufacturing method. Prior art
[0002] It is known to produce profiles from composite material comprising continuous fibers coated in a matrix of synthetic material. The fibers are, for example, glass fibers, carbon fibers, synthetic material or plant fibers. Such profiles are known to be light and have good strength. The use of a thermoplastic matrix makes it possible to benefit from specific physical or chemical properties of thermoplastic materials, for example to subsequently transform the profiles by softening or melting the material and giving them a new shape. It also makes it easier to recycle objects constructed with these profiles.
[0003] One of the known methods for manufacturing such profiles is pultrusion, which consists of pulling a bundle of unidirectional fibers through a die making it possible to impregnate said fibers with a polymerizable resin and to polymerize the resin in the die to form a composite profile at the outlet of said die, consisting of the reinforcing fibers and a matrix incorporating the fibers. The resins used are mainly of the thermosetting type but can also be of the thermoplastic type. The bundle of fibers is typically a grouping of strands, each strand being composed of a multitude of fibers, for example glass fibers, placed side by side without intersecting. A strand is also called a "roving" in the case of glass or designated by the English term "roving".
[0004] In a particular case, the polymerization of the thermoplastic precursors (monomers and oligomers) takes place in situ in the pultrusion tooling. The precursors used are generally of low viscosity, which has the advantage of allowing the use of very high reinforcement rates while having an excellent and very homogeneous impregnation of the fibers. The existing reactive systems for pultrusion are mainly based on anionic polymerization mechanisms of monomers such as for polyamide 6, from ε-caprolactam, polyamide 12, from lauryl-lactam, radical polymerizations such as with PMMA, from methyl methacrylate or polycondensations such as with polybutylene te- polybutylene terephthalate (PBT) or polyethylene terephthalate (PET) from aromatic polybutylene terephthalate, respectively aromatic polyethylene terephthalate. In the rest of the document, the mixture of precursors that will form the polymer and the matrix after the polymerization reaction will be called resin.
[0005] The profile is formed in a pultrusion die which incorporates an impregnation zone followed by the polymerization zone which also acts as a calibration zone since it gives the desired shape to the profile, so that the profile generally comes out in the solid state, that is to say at a temperature below the melting point of the material which composes it. These tools are extremely expensive due to their dimensions and the fact that they incorporate components to control the evolution of the temperature. In addition, each tool is specific to a section of profile. Productivity is limited by the polymerization speed and by the compromise which it is necessary to make between the length of the die and the tensile forces generated in the die on the profile.Although the polymerization rate can be controlled by the addition of dedicated components, it is limited by the need to transfer the resin mixture into the tooling and wet the fiber bundle.
[0006] Document US 5,310,600 shows a technique for manufacturing a composite based on a polyamide matrix and continuous fibers, according to which a bundle of fibers is first impregnated with reactive resin and then coated in a thermoplastic sheath. The polymerization reaction occurs in the sheath by bringing it to a temperature sufficient for the polymerization reaction. The bead thus formed is then cut into granules, with or without removal of the sheath to serve as an injection molding material. This technique has the advantage of simplifying the tooling since it is no longer necessary to calibrate the bead during the polymerization phase. The sheath serves as mechanical support and as a barrier against the risk of evaporation of the resin monomers during the polymerization phase.This approach allows for simpler tooling, not dedicated to a section, and to increase the production rate by allowing larger dimensions since the size of the tooling can be enlarged without increasing the pulling forces.
[0007] Document WO 2011 / 156693 A2 shows a method for producing profiles comprising mainly two steps. In a first step, ribbons are produced from continuous fibers which are coated with molten thermoplastic material. These ribbons are then assembled in a stack and the assembly passes through a die while the thermoplastic material is melted again. This produces a profile with a rectangular section. The technique of coating fibers with molten thermoplastic material has never been convincing, because the material remains too viscous and can only impregnate a small section of fibers and with a low fiber density.
[0008] Document FR3053912A1 shows the manufacture of a thermoplastic matrix composite profile with reactive pultrusion curvature, for the production of particular structural elements. An intermediate material comprising longitudinal fibers and a malleable thermoplastic matrix is prepared in a straight die, then extracted through a curved calibrator which cools the profile to harden it. Pulling means accompany the curvature imparted to the profile. This technique requires dedicated tooling for each section.
[0009] Document US 4,202,718 shows a method for manufacturing a rectilinear profile comprising longitudinal reinforcing cords deposited on a tubular core and reinforced by at least one winding layer. A calibrator determines the final section. The addition of the winding layer makes it possible to increase the resistance of the profile to stresses other than axial stress. This technique does not allow for a high fiber density. Statement of the invention
[0010] The invention aims to provide a method for manufacturing profiles made of thermoplastic matrix composite material which allows high productivity and good mechanical properties, with simple tooling. It also aims at profiles obtained by this method.
[0011] With these objectives in mind, the invention relates to a method for manufacturing a continuous profile made of thermoplastic composite material, characterized in that it comprises the steps consisting of: - sliding in a pulling direction in shaping means comprising a mandrel a plurality of cords comprising a core with reinforcing fibers coated in a first matrix made of a first thermoplastic material, the cords being distributed around the periphery of the section of the mandrel; - depositing by winding around the plurality of cords a system of at least one reinforcing layer comprising fibers, - assembling by fusion in an agglomeration step the plurality of cords and the system of at least one reinforcing layer, and - with a calibrator, calibrate and cool the section to give a predetermined section to the profile and obtain the profile after hardening.
[0012] The use of already produced cords makes it possible to manufacture profiles with a high fiber density to provide high mechanical strength, and with high productivity. Indeed, the constitution of the profile only requires a melting phase of the thermoplastic material to agglomerate the cords and hardening by cooling, without a temperature maintenance phase as in the reactive pultrusion process. The fibers in the cords are for example longitudinal. shaping means allow the plurality of cords and the reinforcing layer to be compacted. The mechanical strength is considerably improved with the addition of at least one reinforcing layer for stresses other than pure traction. The use of thermoplastic material allows the section of the profile to be determined with a tool that can be partly shared with a tool for other profile sections. In addition, the shaping of the section downstream of the application of the reinforcing layer allows sections to be obtained, in particular with re-entrant angles, which would be impossible to obtain directly by winding. The process is suitable for any thermoplastic material. Examples include polycarbonate (PC), polypropylene (PP), polystyrene (PPS), polyetheretherketone (PEEK).
[0013] According to a constructive arrangement, in the agglomeration step, the shaping means comprises a die which surrounds the mandrel, the sections of the mandrel and the die evolving in the pulling direction to constrain the system of at least one reinforcing layer against the plurality of cords. The plurality of cords are thus compacted together and against the reinforcing layer in order to obtain the desired section and a good bond between them.
[0014] According to a constructive arrangement, the mandrel comprises at least one groove extending in the pulling direction in order to guide at least one of the cords. This controls the way in which the cords are assembled together. In general, each cord is guided by a groove. The grooves may have a V-shaped, rectangular, circular or other section.
[0015] According to an improvement, the mandrel comprises at least two grooves, a first groove of which is less deep than a second groove at the inlet of the shaping means, the second groove being of the same depth as the first groove at the outlet of the shaping means. The cord in the second groove is thus forced to insert itself next to the cord in the first groove, which puts the cords under pressure against the reinforcing layer. Good compaction is thus obtained.
[0016] According to an improvement, the mandrel is curved and makes it possible to obtain a curved profile. Obtaining curved profiles is particularly interesting for obtaining structural elements such as arches, portions of frames or vehicle structural elements. The curved mandrel makes it possible to form the profile in its curved shape before it hardens. The reinforcing layer is also deposited following the curvature of the profile.
[0017] According to another improvement, during the agglomeration step, shaping means, including the mandrel, evolve in the drawing direction to change the section of the assembly formed by the plurality of cords and the system of at least one reinforcing layer from an initial section at the level of the winding to the predetermined section of the profile. Once a base is formed, the section of this base, in particular by bringing together, or even joining, opposite parts of the base wall. In the extreme, it is possible to make the cavity disappear and obtain a section with a wall covered on each of these faces with the reinforcement layer. In principle, the perimeter of the reinforcement layer does not change and it is necessary to plan for an evolution of the section while maintaining the same perimeter.
[0018] According to one embodiment, at least a portion of the cords comprise a sheath made with the second thermoplastic material, which is melted at least in the agglomeration step to agglomerate the cores of the cords. Most of the material that allows the cords to be joined is directly brought with them. The second thermoplastic material may be the same as the first, which ensures continuity between the core and the second matrix. It may also be distinct to provide other properties, in particular protection against humidity if the first thermoplastic material is sensitive to humidity, or by providing surface functionalities, such as ultraviolet protection or sufficient electrical conductivity for the use of powder coating.
[0019] According to an improvement, the system of at least one reinforcing layer is formed by a reinforcing strip previously coated with a third thermoplastic material. Thus, the reinforcing strip is pre-impregnated and forms a composite layer after cooling and solidification. The reinforcing strip is for example heated before winding to melt the third thermoplastic material. The layer is for example formed by a ribbon of continuous fibers coated by reactive pultrusion.
[0020] According to one embodiment, during the agglomeration step, the plurality of cords are heated to a temperature above the melting temperature of the first thermoplastic material, the cross-section of the cores being deformed during the agglomeration step. It is thus possible to use cords having, for example, a round cross-section, and to shape them so that the cores best fill the cross-section of the profile to be obtained. It will thus be possible to have a high fiber density, for example more than 50% by volume, or even more than 60% or 70%. The cords preferably provide all, or at least most of the material of the final profile. Any additional material may be provided under pressure to fill the variations in volume of the cords while ensuring good compaction and the reduction of any hollows or cracks. This contribution is less than 5% of the cross-section, or even less than 2%.
[0021] According to an improvement, the number of winding layers is at least two, with a first winding layer wound in a first direction and a second winding layer wound in a second direction opposite to the first direction. A single winding may have a tendency, depending on its mass, to induce twisting of the profile. The addition of a second winding in the opposite direction makes it possible to balance this trend and cancel it out. In addition, due to the crossing of the fiber directions between the winding layers, an even more solid assembly is obtained.
[0022] According to an improvement, a sliding layer comprising reinforcing fibers extending in the pulling direction is deposited after the winding layer and upstream of the shaping means. The sliding layer has a dragging effect for the underlying reinforcing layer. This avoids pushing back and destructuring the reinforcing layer, in particular if the latter has a pronounced winding angle, when it enters the shaping means, in particular in a die.
[0023] In a particular arrangement, the sliding layer is itself made up of cords. In this case, the die may include grooves to guide the cords of the sliding layer.
[0024] According to an improvement, at least a second plurality of cords is deposited over the system of at least one reinforcing layer, then at least a second system of at least one reinforcing layer upstream of the shaping means. It is thus possible to produce a complex profile with several successive layers having crossed or non-crossed reinforcing fibers.
[0025] According to a particular arrangement, the cords of the plurality of cords have a section whose perimeter to area ratio is less than or equal to 4 mm '. The perimeter to area ratio makes it possible to characterize the shape and size of the cords. With a value of 4 mm ', cords of rather massive section, not very thin, are selected. For a cord of round section and diameter 1 mm, the value is 4 mm '. The criterion makes it possible to select round cords of diameter greater than or equal to 1 mm. For a cord of rectangular section of 6 x 0.6 mm, the ratio is 3.7. The selection of cords according to this criterion makes it possible to obtain the desired sections by limiting the stresses at the interfaces of the cords between them and the flows of molten material, and therefore by limiting the risks of fiber breakage or creation of cracks trapping air.The limitation of constraints comes from limiting the number of cords, by using cords of significant section, and by limiting the contact surface between them, with a compact shape. Cords of this size are also easier to guide on the mandrel, by allowing deeper, therefore more efficient, guide grooves.
[0026] According to one embodiment, the final section of the profile is greater than the sum of the sections of the plurality of cords and, during the agglomeration step, a fourth thermoplastic material is provided to complete the profile up to the final section. This guarantees that a profile is obtained without a lack of material in the section. It is not necessary for the final section to be significantly greater.
[0027] According to an improvement, an extrusion die is provided downstream of the shaping means and into which the fourth thermoplastic material is injected at the periphery of the section of the profile to obtain the final section of the profile. It is thus possible to cover the reinforcing layer and add specific properties to the surface of the profile.
[0028] Preferably, the cords are produced in a reactive pultrusion step, the core comprising continuous fibers. This technique makes it possible to obtain cores with a high fiber density. In addition, the cords can be produced with a sheath, as in the technique disclosed by document US 5,310,600 with high productivity.
[0029] For example, reactive pultrusion produces the first thermoplastic material selected from a group comprising polyamide-6, polyamide-12, polymethyl methacrylate and polybutylene terephthalate.
[0030] The invention also relates to a composite profile, obtained with a method as defined above, and comprising a constant section with a plurality of cores with reinforcing fibers coated in a first matrix of a first thermoplastic material, the cores being coated in a second matrix of a second thermoplastic material and covered by at least one reinforcing layer comprising fibers oriented at least non-longitudinally. The reinforcing layer combined with a high density of longitudinal fibers gives such a profile a high capacity mechanical behavior, which allows it to be used as a structural element in numerous applications, in particular in the transport, automotive, railway or aeronautical industry, or in the construction industry.
[0031] According to a characteristic of the profile, the average rate of fibers by volume is greater than 40%, preferably greater than 55%.
[0032] According to a characteristic of the profile, the fiber content of the cores in volume is greater than 50%, preferably greater than 60%.
[0033] According to a characteristic of the profile, the reinforcing fibers of the core of the cords are chosen from a group comprising glass fibers, carbon fibers, vegetable fibers and aramid fibers. Brief description of the figures
[0034] The invention will be better understood and other features and advantages will appear on reading the description which follows, the description making reference to the appended drawings among which:
[0035] - [Fig.l] is a schematic view of a part of a manufacturing installation implementing implements a method according to a first embodiment of the invention;
[0036] - [Fig.2] is a view of another part of the installation of [Fig.l];
[0037] - [Fig.3] is a sectional view of a cord produced in an intermediate manner with the installation of [Fig.l];
[0038] - [Fig.4] is a longitudinal sectional view of the shaping means of the [Fig.2] ;
[0039] - [Fig.5] is a perspective view of a mandrel of the installation of [Fig.2];
[0040] - [Fig.6] is a perspective view of the mandrel of [Fig.4] from another angle of view;
[0041] - [Fig.7] is a sectional view along plane VI of [Fig.4] with a plurality of cords and a reinforcing layer shown on the mandrel to manufacture a profile according to a first example;
[0042] - [Fig.8] is a sectional view of a tubular base being manufactured according to a second example;
[0043] - [Fig.9] is a view similar to [Fig.8] further downstream;
[0044] - [Fig. 10] is a view similar to [Fig.8] further downstream;
[0045] - [Fig.l 1] is a view similar to [Fig.8] with the final section of the profile;
[0046] - [Fig.12] is a perspective view of a mandrel for the manufacture of a third profile example;
[0047] - [Fig. 13] is an end view of the mandrel of [Fig. 12]. Detailed description
[0048] A method for manufacturing composite parts with a thermoplastic matrix according to the invention is described in connection with an installation shown diagrammatically in Figures 1 and 2.
[0049] A first part of the installation, shown schematically in [Fig.l], comprises a spinning device 1 for manufacturing cords 30 in a spinning step, while a second part, shown in [Fig.2], concerns an agglomeration device 2 for implementing an agglomeration step. The spinning device 1 is in practice a pultrusion device 1 which successively comprises: a first reel support 10 for storing and unwinding reels of rovings 3010 of continuous fibers, a preheating unit 11 for the fibers 3010 which makes it possible to bring the glass fibers to a temperature close to the melting temperature of reactive monomers, i.e. approximately 80°C in the case of e-caprolactam. The fibers 3010 are heated by infrared ramps, not shown, under a nitrogen flow.The pultrusion device 1 further comprises an impregnation unit 12 receiving from an injection unit 13 reactive monomers or pre-polymers which form, after polymerization, a first thermoplastic material 3011. As illustrated, the monomers and the reactive system are metered separately and mixed just at the inlet of the impregnation unit 12, for example in a static mixer 14. A unit of . 15 comprises a first extruder 150 and an extrusion die 151 placed after the impregnation unit 12 which makes it possible to deposit a sheath 302 made of a second thermoplastic material around the impregnated strands, in a sheathing step. The spinning device 1 then comprises a polymerization oven 16 in which the bead 30 is maintained at temperature to allow the polymerization of the resin into the first thermoplastic material 3011, so that the impregnated strands become a core 301 forming with the sheath 302 the bead 30. The pultrusion device 1 further comprises a first pulling unit 17 which makes it possible to simultaneously advance the bead 30 hardened by cooling and to unwind the strands 3010 by the propagation of the movement through the pultrusion device 1.
[0050] The cords 30 thus produced are wound onto other reels 18 in order to accumulate a sufficient number of cords 30 for the agglomeration step. The section of such a cord 30 is shown in [Fig.3].
[0051] The agglomeration device 2, shown in [Fig. 2], comprises a second reel support 20 on which the reels 18 of cords 30 are placed to unwind the cords 30. A plurality of cords 30 is thus directed towards an oven 21 to heat the cords 30 to a temperature higher than the melting temperature of the second thermoplastic material 302. The agglomeration device 2 further comprises a winding station 24 between the oven 21 and shaping means 22 shown in [Fig. 4]. The winding station 24 is fed by one or more reels 240 to provide a ribbon of fibers 330 and deposit it by forming a winding around the plurality of cords 30 to form a reinforcing layer 33 on the outside of the profile.
[0052] Downstream of the winding station 24, a sliding layer 38 is inserted over the reinforcing layer 33. The shaping means 22 assemble the plurality of cords 30 so that the sheaths 302 come into contact with each other and fuse. In this example, the shaping means 22 comprise a mandrel 220, as shown in FIGS. 5, 6 and 7, and an agglomeration die 22 which determine the section of the profile 3 at the outlet.
[0053] Optionally, second thermoplastic material is supplied by the extruder 25 via a feed duct 2240 into the chamber 224 so as to supplement any missing quantity over the sliding layer 38. The agglomeration die 22 is followed by a calibrator 222 provided with cooling means in order to obtain the hardening of at least a portion of the profile 3 thus formed. A second pulling unit 23 exerts traction on the hardened profile 3 and causes the cords 30 to unwind from the reels 18 by the propagation of the movement through the agglomeration device 2. In the embodiment as shown, the mandrel 220, the agglomeration die 22 and the calibrator 222 are curves. The pulling unit 23 is also adapted to the curvature which is thus imparted to the profile 3.
[0054] In a variant not shown, the pultruded cords 30 could directly feed the agglomeration device without going through a winding step. In a variant also not shown, the mandrel, the agglomeration die and the calibrator are rectilinear so as to produce a profile that is also rectilinear.
[0055] In a first example, cords 30 were manufactured by pultrusion with a first matrix formed by the first thermoplastic material 3011, which is polyamide-6 obtained by the polymerization of ε-caprolactam monomer, and as fibers glass fibers. The cross-section of the cores 301 of the cords 30 was circular and 3 mm in diameter, as shown in [Fig. 3]. The cores 301 were covered with a sheath 302 made of polypropylene with a thickness of 0.2 to 0.5 mm. The melting temperature of polyamide-6 is 220 °C while that of polypropylene is 170 °C. Such cords 30 could be produced at a speed of the order of 2 m / min on a pilot plant limited in size.
[0056] In the agglomeration device 2, forty cords 30 were used by passing them through the oven 21 to raise the temperature of the cords 30 to 150°C, then to 200°C in the shaping means 22. At this latter temperature, the sheath 302 was melted, but not the cores 301. The plurality of cords 30 was grouped on the mandrel 220 as shown in FIGS. 5 and 6 to form a square section, as shown in [Fig. 7], in which the cores 301 are coated in a second matrix 32 formed by the second thermoplastic material from the sheaths 302. The mandrel 220 has a groove 2201, 2202 for each cord 30 extending in the pulling direction in order to guide each of the cords 30. On each face, two of the grooves, called second grooves 2202, are deeper than the first grooves 2201 at the level of the inlet of shaping means 22, as shown in the sectional view in [Fig.7], where the reinforcing tape 330 is deposited by the winding means 24, as symbolized by the arrow FL. The second grooves 2202 are of the same depth as the first grooves 2201 at the outlet of the shaping means 22. The fiber content of the cores 301 of the cords 30 by volume was 70%. The average fiber content by volume over the entire section varied from 44 to 49%. Such profiles 3 could be produced at a speed of the order of 0.5 m / min.
[0057] In a second example, the mandrel, not shown, has a rectangular section at the entrance to the shaping means 22, so as to prepare a tubular base 35 of rectangular section covered by a reinforcing layer 33, as shown in [Fig. 8]. The section of the mandrel and the die evolves in the drawing direction by first creating a hollow on one of the faces ([Fig. 9]), by joining the walls to make dis appear the cavity ([Fig. 10]) by interrupting the mandrel and finally calibrating the profile 3' according to a U-shaped section ([Fig. 11]).
[0058] In a third example, shown in Figures 12 and 13, the cords 3 are initially gathered in a rectangular section covered by a reinforcing layer 33 as in the second example ([Fig.8]). The section of the mandrel 220" and of the die evolve in the drawing direction by first creating a hollow on the two largest faces 31, by joining the walls on their middle part to form a web 34 by maintaining two cavities 36 delimited by tubular soles 37 and finally by calibrating the profile 3” according to an I-shaped section, as shown in [Fig. 13].
[0059] The invention is not limited to the embodiments described solely by way of example. The cords may be obtained by mixing the fibers with molten thermoplastic material.
Claims
Claims
1. Method for manufacturing a continuous profile made of thermoplastic composite material, characterized in that it comprises the steps of: - sliding, in a pulling direction in shaping means (22) comprising a mandrel (220), a plurality of cords (30) comprising a core (301) with reinforcing fibers (3010) coated in a first matrix (3011) made of a first thermoplastic material, the cords being distributed around the periphery of the section of the mandrel; - depositing by winding around the plurality of cords (30) a system of at least one reinforcing layer (33) comprising fibers, - assembling by fusion in an agglomeration step the plurality of cords (30) and the system of at least one reinforcing layer (33), and - with a calibrator (222), calibrating and cooling the section to give a predetermined section to the profile (3) and obtaining the profile (3) after hardening.
2. Manufacturing method according to claim 1, according to which, in the agglomeration step, the shaping means (22) comprises a die which surrounds the mandrel (220), the sections of the mandrel (220) and of the die evolving in the pulling direction to constrain the system of at least one reinforcing layer (33) against the plurality of cords (30).
3. Method according to one of the preceding claims, according to which the mandrel (220) comprises at least one groove (2201, 2202) extending in the pulling direction in order to guide at least one of the cords (30).
4. Manufacturing method according to claim 3, according to which the mandrel (220) comprises at least two grooves of which a first groove (2201) is less deep than a second groove (2202) at the inlet of the shaping means (22), the second groove (2202) being of the same depth as the first groove (2201) at the outlet of the shaping means (22).
5. Method according to one of the preceding claims, according to which the mandrel is curved and makes it possible to obtain a curved profile.
6. Method according to one of the preceding claims, according to which, during the agglomeration step, shaping means (22), including the mandrel (220), evolve in the pulling direction to change the section of the assembly formed by the plurality of cords and the system of at least one reinforcing layer (33) from an initial section at the level of the winding towards the predetermined section of the profile (3).
7. Method according to one of the preceding claims, according to which at least a part of the cords (30) comprise a sheath (302) made with the second thermoplastic material, which is melted at least in the agglomeration step to agglomerate the cores (301) of the cords (30).
8. Method according to one of the preceding claims, according to which, during the agglomeration step, the plurality of cords (30) are heated to a temperature higher than the melting temperature of the first thermoplastic material, the section of the cores being deformed during the agglomeration step.
9. A method according to any preceding claim, wherein the number of reinforcing layers (33) is at least two, with a first reinforcing layer wound in a first direction and a second reinforcing layer wound in a second direction opposite to the first direction.
10. Method according to one of the preceding claims, according to which, after the system of at least one reinforcing layer (33) and upstream of the shaping means, a sliding layer (38) comprising reinforcing fibers extending in the pulling direction is deposited.
11. Method according to one of the preceding claims, according to which at least a second plurality of cords is deposited over the system of at least one reinforcing layer (33) and then at least a second system of at least one reinforcing layer (33) upstream of the shaping means (22).
12. Method according to one of the preceding claims, according to which the cords (30) of the plurality of cords have a section whose perimeter to area ratio is less than or equal to 4 mm1.
13. Method according to one of the preceding claims, according to which the cords (30) are produced in a reactive pultrusion step, the core (301) comprising continuous fibers (3010).
14. The method of claim 13, wherein the reactive pultrusion produces the first thermoplastic material selected from a group consisting of polyamide-6, polyamide-12, polymethyl methacrylate and polybutylene terephthalate.
15. Composite profile, characterized in that it is obtained with a process according to one of the preceding claims, and in that it comprises a constant section with a plurality of cores (301) with reinforcing fibers (3010) coated in a first matrix (3011) made of a first thermoplastic material, the cores (301) being coated in a second matrix (302) made of a second thermoplastic material and covered by at least one reinforcing layer (33) comprising fibers oriented at least non-longitudinally.
16. Profile according to claim 15, in which the average rate of fibers by volume is greater than 40%, preferably greater than 55%.
17. Profile according to one of claims 15 to 16, in which the fiber content of the cores by volume is greater than 50%, preferably greater than 60%.
18. Profile according to one of claims 15 to 17, in which the reinforcing fibers of the core of the cords are chosen from a group comprising glass fibers, carbon fibers, plant fibers and aramid fibers.