Manufacturing of parts in MgB2
Additive manufacturing with laser sintering and densification techniques address the challenges of shaping MgB2 ceramics, enabling complex-shaped parts with reduced material costs and tool wear, suitable for magnetic field applications.
Patent Information
- Application Number
- FR2022005332
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-02
- Publication Date
- 2024-09-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
MgB2 superconducting ceramics are difficult to shape and machine due to their high hardness, brittleness, and chemical instability, making it challenging to produce complex-shaped parts necessary for applications requiring significant magnetic fields.
A process involving additive manufacturing techniques, specifically powder bed additive manufacturing with laser sintering, followed by densification under load, to create preformed MgB2 parts with complex shapes.
Enables the production of complex-shaped MgB2 parts with reduced material usage and tool wear, maintaining mechanical strength and superconductivity, suitable for applications in magnetic fields and on-board systems.
Smart Images

Figure 00000016_0000 
Figure 00000016_0001 
Figure 00000017_0000
Abstract
Description
Title of the invention: Production of MgB2 parts
[0001] The present invention relates to a method for manufacturing a preformed part, in particular of complex shape, in superconducting ceramic of magnesium diboride or MgB2 by an additive manufacturing technique. Prior art
[0002] Superconducting materials are increasingly present in our daily lives. Superconducting parts find their applications in medicine, such as superconducting MRI coils in industry, magnets and magnetic shields in transportation, or engine parts and potential levitation transportation systems, and in many other fields.
[0003] Among these materials, MgB2 is one of the most promising materials. MgB2 is an intermetallic material whose structure consists of a stack of magnesium planes alternating with boron planes along its c axis. While this compound has been known since the 1950s, its superconductivity was discovered only a few years ago. While thin films and powders exhibit anisotropic superconducting properties, sintered ceramics are isotropic.
[0004] Nevertheless, MgB2 superconducting ceramics are very difficult to shape and machine because the material is extremely hard (Hv = 18 GPa and Young's Modulus = 400 MPa), brittle (K = 2 MPam1 / 2), difficult to sinter since only Spark Plasma Sintering allows its optimal sintering, and its chemical composition is easily decomposed with temperature.
[0005] This material is of great interest in the context of superconducting applications (motors, magnetic screens, bending elements, electricity storage, electromagnetic thrusters, etc.) in order to generate significant magnetic fields thanks to its high critical current density capacity. These current densities are greater than those of the high critical temperature superconducting oxides usually used, such as YBa2Cu3O7 (ReYBCO) with identical passage sections.
[0006] However, obtaining massive parts, particularly with complex shapes, is not possible to date. This is one of the major problems encountered to date in the use of MgB2 which is slowing down its development.
[0007] Furthermore, MgB2 is a very light material (2.5 g / cm3) and is therefore interesting for on-board applications, such as in electric aircraft motors, unlike ReBCO.
[0008] Applications involving large magnetic fields increasingly require the ability to produce complex magnetic field maps, which requires the parts of the superconducting material to also have shapes. complex. Such applications in the case of MgB2 are made extremely difficult because it is not possible to machine it due to its high hardness (GPa) and brittleness.
[0009] There is therefore a need to have a method for manufacturing a part in MgB2 which makes it possible to avoid the winding of ribbons, as used in the case of oxides such as ReBCO, which is a very delicate technical operation, and above all to have a complete superconducting current passage section corresponding to the true section of the material.
[0010] There is also a need to have such a manufacturing method so as to be able to reduce the size of the devices for the same magnetic performances and to avoid the loss of material due to machining or even the wear of the machining tools. Summary of the invention
[0011] The invention meets this need using a method for manufacturing a part of MgB2 comprising: a) producing a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, comprising exposing the MgB2 powder to laser radiation, and b) a step of densification of the preform, until obtaining the MgB2 part.
[0012] In the context of the present invention, the method thus makes it possible, in particular from a commercial MgB2 powder, preferably previously deagglomerated, to spread it in a bed and then to expose it using a laser under an inert atmosphere. The method is additive and makes it possible to build a preform layer by layer.
[0013] By this method, the amount of material used can be reduced, thereby reducing raw material costs.
[0014] To date, no production of MgB2 material by additive manufacturing techniques has been reported in the literature. Brief description of the drawings
[0015] The invention may be better understood by reading the detailed description which follows, non-limiting examples of its implementation, and by examining the figures:
[0016] [Fig-1] represents a diagram of the successive steps of an embodiment of the method according to the invention.
[0017] [Fig.2] represents the curve obtained in the example representing the mass fraction of the MgB2 phase as a function of the cumulative energy dose for the plate with a powder bed of 100 pm.
[0018] [Fig.3] represents XRD diagrams of samples A and B of the example after implementation of the method, namely step a) implementing the SLS technique and step b) implementing the SPS technique.
[0019] [Fig.4] shows magnetic moment versus temperature curves of samples obtained in the example. The insets show a photograph of sample A after step a) using the SLS technique and then after step b) using the SPS technique, and the transition region for sample B in more detail (right).
[0020] [Fig.5] represents a diagram of more complex shaped parts in MgB2 to be printed (scale in mm) and corresponding preforms, obtained experimentally. Detailed description
[0021] The invention relates to a method for manufacturing a part, in particular a preformed part, in particular of complex shape, of the superconducting ceramic MgB2 according to the invention, the method comprising the production of said part by shaping a powder using an additive manufacturing technique.
[0022] Preferably, the additive manufacturing technique is a powder bed additive manufacturing technique.
[0023] Preferably, the additive manufacturing technique, commonly referred to as 3D printing techniques, implements a partial or complete melting of powder particles by means of a light beam or electrons, in particular a light beam. Preferably, the light beam is a laser beam. In the context of the present invention, the additive manufacturing technique used is preferably the additive manufacturing of direct metal laser sintering, translation of Direct Metal Laser Sintering (DMLS).
[0024] The technique of additive manufacturing by laser fusion on a powder bed comprises the deposition of at least one layer of powder then the partial or complete fusion of at least a part of the particles of the powder, preferably of all the particles of the layer deposited by a selective supply of energy under the action of a laser beam.
[0025] In the context of the present invention, such a step allowing the production of a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique is called step a), and is followed by a densification step b).
[0026] According to the terms of the invention, “densification” designates the possibility of manually extracting a preform via an increase in the density of the material, expressed in relation to the theoretical density of the material without porosity.
[0027] According to a variant, step a) and / or step b) is carried out under an inert atmosphere, in particular under argon.
[0028] The different aspects of the method according to the invention, and different embodiments are detailed below. Powder bed additive manufacturing - step a)
[0029] Step a) of the method according to the invention comprises the production of a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, comprising the exposure of the MgB2 powder with laser radiation.
[0030] In one variant, the MgB2 powder may be that marketed as boron powder from Pavezyum, Advanced Chemicals (Istanbul, Türkiye).
[0031] As regards the quality of this starting powder, the purity may be in particular greater than 90%, or even 95%, for example 97%.
[0032] As traces present in this powder, we can cite traces of MgO (for example 2%) and MgB4 (for example 0.1%).
[0033] In a variant, the median equivalent diameter of the particles of the MgB 2 powder varies from 1 pm to 50 pm, in particular varies from 2 pm to 30 pm, preferably varies from 5 pm to 20 pm.
[0034] In a variant, the method comprises, prior to step a), a step of deagglomeration of the powder of MgB2 particles.
[0035] Typically, this deagglomeration step can be carried out by placing the powder in a mixer and / or centrifuge, for example as marketed under the name Centrifugal Mixer SK-300SII by the company Kakuhanter Planetary. Typically, the rotation speed can be between 800 rpm and 1500 rpm, in particular between 1000 rpm and 1400 rpm, for example at 1200 rpm.
[0036] The powder can be spread in a bed of different thicknesses. The thickness of the powder bed can in particular influence the way in which the sintering of the powder occurs. In fact, within the framework of the present invention, it may be sought to aim for a temperature which avoids the degradation of the MgB2 phase, in particular into Mg and B.
[0037] According to a variant, the thickness of the powder bed in step a) varies from 50 μm to 800 μm, in particular varies from 75 μm to 500 μm, preferably varies from 100 μm to 300 μm.
[0038] According to a variant, step a) is implemented by selective laser sintering (SLS or DMLS).
[0039] Any DMLS / SLS device known to those skilled in the art can be used, such as the M ProXLS 200 device marketed by the company 3D System.
[0040] The type of laser that can be used in the exposure carried out in step a) of the method is in particular a 300 W laser. Typically, a laser with a wavelength of 1064 nm can be used.
[0041] According to an alternative embodiment, the production of a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, comprises exposing the MgB2 powder with laser radiation, with a local cumulative energy density varying from 18 mJ / pm2 to 265 mJ / pm2, or a non-cumulative global macroscopic dose varying from 4 J / cm2 / pass to 70 J / cm2 / pass, so as to obtain the preform based on an insolated MgB2 powder.
[0042] The insolation makes it possible to achieve densification of the preform.
[0043] Thus, the densification of the MgB2 powder at the end of step a) can vary from 30% to 45%, preferably vary from 35% to 45%, expressed relative to the theoretical density of the material without porosity.
[0044] The optimization of laser exposure (dose, thickness) has in particular made it possible to provide the possibility of having preforms (35% densification) which can be handled and which can then be sintered under load and in an inert atmosphere during step b) detailed below.
[0045] The power of the laser radiation can in particular vary from 28 W to 115 W, in particular from 40 W to 95 W, even more particularly from 50 W to 85 W.
[0046] In terms of doses or energy density of the laser radiation, they can vary from 4 J / cm2 / pass to 70 J / cm2 / pass, in particular vary from 4.5 J / cm2 / pass to 70 J / cm2 / pass, more particularly vary from 5 J / cm2 / pass to 70 J / cm2 / pass, preferably vary from 6 J / cm2 / pass to 60 J / cm2 / pass, and more preferably from 7 J / cm2 / pass to 50 J / cm2 / pass.
[0047] In terms of cumulative dose, it can vary from 18 mJ / pm2 to 265 mJ / pm2, in particular vary from 31 mJ / pm2 to 188 mJ / pm2, and even more particularly from 53 mJ / pm2 to 144 mJ / pm2.
[0048] The inventors have notably been able to observe that laser doses that are too low, for example less than 4 J / cm2 / pass, can lead to ineffective sintering, in other words manifesting itself by the fact that the powder remains in powder form whereas a higher dose, for example greater than 100 J / cm2 / pass, leads to the degradation of the MgB2 phase, typically by the formation of impurity phases such as MgB4, Mg2B2, MgO or Mg, which leads to undesirable properties in the samples obtained, in particular the loss of superconductivity. Furthermore, the cumulative energy dose can be adjusted by a person skilled in the art as a function of the thickness of the selected powder bed.
[0049] According to one variant, the laser beam is moved at a speed varying from 100 mm / s to 1000 mm / s, in particular from 100 mm / s to 800 mm / s, in particular varying from 120 mm / s to 800 mm / s, more particularly varying from 120 mm / s to 500 mm / s, preferably varying from 150 mm / s to 300 mm / s, and more preferably varying from 150 mm / s to 250 mm / s.
[0050] According to a variant, the vector deviation of the laser beam varies from 50 pm to 250 pm, in particular varies from 75 pm to 175 pm, preferably varies from 100 pm to 150 pm.
[0051] According to a variant, the focusing of the laser beam varies from -50 mm to -20 mm, in particular varies from -50 mm to -30 mm, preferably varies from -50 mm to -40 mm.
[0052] According to another variant embodiment, step a) of the method according to the invention comprises the production of a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, comprising the insolation of the MgB2 powder with laser radiation, with a macroscopic energy dose varying from 50 J / cm2 / pass to 90 J / cm2 / pass, so as to obtain a counterform based on an MgO powder and the preform based on a non-insulated MgB2 powder contiguous to the MgO powder.
[0053] According to a variant of this embodiment, the energy dose of the laser radiation in step a) varies from 50 J / cm2 / pass to 90 J / cm2 / pass, in particular varies from 50 J / cm2 / pass to 80 J / cm2 / pass, preferably varies from 50 J / cm2 / pass to 70 J / cm2 / pass.
[0054] According to a variant of this embodiment, the power of the laser radiation in step a) varies from 70 W to 150 W, in particular varies from 70 W to 130 W, preferably varies from 70 W to 120 W.
[0055] According to a variant of this embodiment, the laser beam in step a) is moved at a speed varying from 100 mm / s to 800 mm / s, in particular varying from 120 mm / s to 500 mm / s, preferably varying from 150 mm / s to 250 mm / s.
[0056] According to a variant of this embodiment, the vector deviation of the laser beam in step a) varies from 50 pm to 250 pm, in particular varies from 75 pm to 175 pm, preferably varies from 100 pm to 150 pm.
[0057] According to a variant of this embodiment, the focusing of the laser beam in step a) varies from -50 mm to -20 mm, in particular varies from -50 mm to -30 mm, preferably varies from -50 mm to -40 mm. Preform densification step - step b)
[0058] The densification step of step b) may comprise a sintering step, in particular by densification under load, or an impregnation step, in particular with a conductive metal other than magnesium, and preferably with copper or an alloy of copper and silver.
[0059] According to a particular embodiment, step b) consists of a densification step under load.
[0060] According to one variant, the sintering step is carried out by densification under load, in particular by SPS or by hot pressing, in particular by SPS.
[0061] The objective of this densification step b) is to achieve a hardness of the formed parts compatible with the desired applications. In other words, this densification step b), in particular by SPS treatment, reduces the fragility and porosity of the samples or parts obtained by implementing a single step a) as described previously.
[0062] SPS treatment is field-assisted sintering. Field-assisted sintering Field Assisted Sintering Technology is also known by the acronym "FAST". Field-assisted sintering refers to sintering assisted by an electric or magnetic field. Electric field-assisted sintering is also known as "flash sintering" and by the acronyms "SPS" for "Spark Plasma Sintering" and "ECAS" for "Electric Current Assisted Sintering".
[0063] Powder matrices or sacrificial powders may be used in the context of the implementation of step b), in particular with a view to facilitating demolding. Among such powders, mention may in particular be made of powders such as SiC, Al2O3, MgAl2O4 and BN. Such powders may in particular be chosen so as to avoid interdiffusion and the formation of impurities due to parasitic reactions.
[0064] According to one variant, the densification step under load uses one or more sacrificial powders, and preferably at least silicon carbide.
[0065] As illustrated in the following example, it could be observed that the geometry of the part could thus be preserved.
[0066] According to one variant, the densification step under load is carried out at a temperature varying from 700°C to 1050°C, in particular varying from 750°C to 1000°C, preferably varying from 800°C to 950°C.
[0067] According to one variant, the densification step under load is carried out for a duration varying from 20 minutes to 120 minutes, in particular varying from 20 minutes to 90 minutes, preferably varying from 20 minutes to 60 minutes.
[0068] According to one variant, the densification step under load is carried out under a pressure varying from 10 MPa to 100 MPa, in particular varying from 20 MPa to 80 MPa, preferably varying from 40 MPa to 60 MPa.
[0069] According to another variant, the densification step of step b) comprises an impregnation step, in particular with a conductive metal other than magnesium, and preferably with copper or an alloy of copper and silver.
[0070] Such a step makes it possible to fill the porosity by capillarity.
[0071] According to a particular embodiment, the present invention relates to a method as described previously, characterized in that it comprises: a) the production of a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, comprising the exposure of the MgB2 powder with laser radiation, with an energy dose varying from 4 J / cm2 / pass to 70 J / cm2 / pass, so as to obtain the preform based on an exposed MgB2 powder, and b) a step of densification of the preform, by sintering the exposed MgB 2 powder, until the MgB2 part is obtained.
[0072] [Fig.l] represents a diagram of the successive stages of the embodiment of the process described above.
[0073] Furthermore, [Fig.5] represents a diagram of MgB2 parts to be printed (scale in mm) and preformed obtained experimentally with laser powers of 63-74 W, a defocus at -50 mm, a scanning speed of 200 mm / s, a spacing of 175 pm, and a powder bed thickness of 300 pm (corresponding to doses of 40 J / cm2 / pass J / cm2 / pass to 45 J / cm2 / pass).
[0074] The inventors have furthermore developed a particular embodiment of the method using laser radiation with a high cumulative energy density in step a) making it possible to obtain a counterform in the form of a powder of degraded MgB2 and / or decomposed MgO. In other words, the preform and the counterform are then contiguous during this step a). The part thus obtained at the end of step a), comprising the preform and the counterform, can then be subjected to step b) to obtain the densified MgB2 preform.
[0075] Thus, the present invention also relates to a method as described previously, characterized in that it comprises: a) producing a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, in an environment with oxygen, comprising exposing the MgB2 powder with laser radiation, with an energy dose varying from 50 J / cm2 / pass to 90 J / cm2 / pass, preferably varying from 60 J / cm2 / pass to 80 J / cm2 / pass, so as to obtain a counterform based on an MgO powder and the preform based on a non-exposed MgB2 powder contiguous to the MgO powder, and b) a step of densification of the preform, by sintering the non-insulated MgB2 powder in step a), in a sintering furnace under an inert atmosphere, followed by a step of depowdering the MgO powder, until the MgB2 part is obtained.
[0076] According to a variant of this embodiment, the sintering step is carried out at a temperature varying from 700°C to 1050°C, in particular varying from 750°C to 1000°C, preferably varying from 800°C to 950°C.
[0077] At the end of step b), the method may also comprise a subsequent step of demolding the MgB2 part.
[0078] The MgB2 part may be a superconductor, the critical temperature of which may be between 35 K and 39 K. Preforms or parts obtained and their use
[0079] The inventors have shown that the method according to the present invention makes it possible to produce complex shapes. Typically, the size of the parts or patterns can advantageously be greater than 0.5 x 0.5 x 0.5 cm3 to obtain good mechanical strength of the preforms. The method according to the present invention can thus be particularly suitable for the manufacture of solid objects of multicenti- metrics.
[0080] The inventors have further demonstrated that the method according to the present invention allows the manufacture of preforms, in particular densified to 35%, with good mechanical strength for large parts, without significant degradation of the MgB 2 phase. The successive step of densification under load (SPS), in particular using a sacrificial powder such as a SiC powder, for the purpose of avoiding diffusion coupled with an undesirable reaction and for demolding purposes, makes it possible to increase the densification of the preforms while maintaining the initial geometry of the preform. Due to a shrinkage which may be significant, in particular 65%, in particular visible along the axis of application of the force, as illustrated in the example which follows, it may be advantageous to take this into account to satisfy the final dimensions of the parts.
[0081] Furthermore, as shown in [Fig.4], the inventors were able to show that samples had the MgB2 phase and that the latter were superconductors with a critical temperature similar to that of samples obtained by the conventional route (38 K).
[0082] The method according to the present invention allows the obtaining of complex 3D shapes.The preforms or parts obtained by the method according to the present invention can in particular be used for all types of applications using superconductors such as motors or alternators, in particular in the field of aeronautics, wind power, satellite trajectory correctors, magnetic levitation systems, thrusters, in particular for in the field of magnetohydrodynamics or for launchers, magnetic shields and screens (MAGLEV), energy storage systems (SMES), bending magnets and magnetic confinement systems, for example for particle accelerators, fusion reactors (ITER), maritime propulsion systems for submarines and boats, high-power electricity systems (superconducting shunts), magnetic field generation systems (IRM) or even electromagnetic launchers (S3EL).
[0083] The invention is not limited to the embodiments described above.
[0084] For example, MgB2 parts may be different from those illustrated. Examples MATERIALS AND METHODS
[0085] A commercial powder (Pavezyum) with a purity greater than 95% and an agglomerate size less than 500 pm (particles from 1 pm to 50 pm) was used for the manufacture of the superconducting parts.
[0086] The purity of said powder, as well as the phase distribution in the produced samples, were verified using the Bruker D8 diffractometer in the configuration Bragg-Brentano (30 < 20 < 65°, 0.01° step) and CuKa wavelength radiation (40 kV, 40 mA). During acquisition, a nickel filter was used to eliminate K[3 radiation and reduce fluorescence.
[0087] Mixing of the raw powder was carried out for deagglomeration of the powder several days before the start of the implementation of the process by means of the Kakuhanter Planetary Centrifugal Mixer SK-300SII apparatus.
[0088] Mixing conditions: 1100 rpm, for a duration of 6 minutes for a maximum of 180 g of powder at one time.
[0089] The deagglomerated powder was introduced into the SLS apparatus.
[0090] SLS device used for step a): M ProXLS 200 marketed by the company 3D System (wavelength: 1070 nm) under an inert argon atmosphere (O2 < 800 ppm).
[0091] A thin layer of silicon was applied to the surface of the build plate to prevent slippage of the MgB2 powder during the fabrication of the first layer.
[0092] All samples obtained were studied using microscopy (KEYENCE VH-Z100R, SEM TESCAN VEGA3) and XRD techniques.
[0093] The superconductivity properties of the selected samples were investigated using magnetic susceptibility measurements with the SQUID magnetometer (Quantum design MPMS 5) in the zero field cooling (ZFC) and 20 Oe field cooling (FC) regimes in the temperature range of 20 - 40 K.
[0094] Shape of samples or nieces: Simple cubic shape. Each cube had a base area of 1 x 1 cm2 and a height of ~ 4.4 mm.
[0095] Thickness of the lightning bed: 100 pm
[0096] Laser: - hexagonal strategy of laser movement - laser power (P): {30; 129} W - laser scanning speed (v): {50; 800} mm / s - gap between two laser passes (A): {100; 250} pm - laser spot size: 1000 pm
[0097] Device used for step b): Spark Plasma Sintering SPS Dr. Sinter 2080 marketed by the company Sumitomo. RESULTS
[0098] Under the conditions identified above, the SLS manufacturing yield was ~85% (viable samples).
[0099] All synthesized samples were then studied by X-ray diffraction.
[0100] [Fig.2] shows the volume fraction of the MgB2 phase in the sample in function of the cumulative energy dose.
[0101] The highest value of the MgB2 fraction was found for laser radiation doses between 4.5 J / cm2 / pass and 60 J / cm2 / pass.
[0102] According to the microscopic study, all samples, which received an energy dose lower than 4 J / cm2 / pass, were fragile and exhibited high porosity, which indicates that the radiation energy of the laser beam is not sufficient to achieve complete sintering of the powder.
[0103] After a thorough study, two samples containing an MgB2 phase greater than 94% were selected.
[0104] These results were obtained under the following laser conditions: - P = 66 W, v = 800 mm / s, A = 100 pm (sample A, i.e. a dose of 10 J / cm2 / pass also corresponding to a cumulative dose Ed = 89 mJ / pm2), and - P = 84 W, v = 200 mm / s, A = 250 pm (sample B, i.e. a dose of 50 J / cm2 / pass, also corresponding to a cumulative dose Ed = 179 mJ / pm2).
[0105] The radiographic images of these samples are shown in [Fig.3] (a, b).
[0106] The obtained samples show a similar XRD pattern with the same compounds.
[0107] Further treatment by spark plasma sintering was carried out.
[0108] The samples were placed in graphite dies with the additional SiC powder around the cube and heated to 800 °C under 0.1 kN in the 20 mm diameter die for 8 min.
[0109] Then, a uniaxial pressure of 15.7 kN was applied for 20 minutes and this temperature and pressure were maintained for an additional 20 minutes.
[0110] Finally, the pressure and temperature were released for 16 minutes.
[0111] The obtained parallelepiped samples exhibited an undeformed geometry ([Fig.4] inset) of their base surface, but their height was extremely reduced. Despite a single difference in the SPS conditions, the X-ray diffraction pattern for sample B shows more impurity peaks ([Fig.3] c, d), which can be explained by the presence of poorly removed SiC.
[0112] Regarding the superconducting properties, magnetic susceptibility measurements show a clear transition to superconductivity at Te ~ 37.8 K in sample A, while the susceptibility curve of sample B increases again rapidly with decreasing temperature just after the transition to the superconducting state (Te ~ 37.8 K) ([Fig.4]).
[0113] Finally, the SPS conditions described above give a good result both for the composition of the phase obtained and for the preservation of the superconductivity properties. CONCLUSIONS
[0114] Cumulative energy doses of 89 rnJ / pm2 (dose 10 J / cm2 / pass) and 179 mJ / pm2 (50 J / cm2 / pass) received by the raw powder under certain SLS conditions, make it possible to obtain samples shaped with a practically non-degenerate and superconducting MgB2 phase.
[0115] The sample treated by SPS in an Ar atmosphere at 800 °C and 15.7 kN shows a sharp transition to the superconducting state at ~ 37.8 K.
[0116] These results show that the process according to the present invention allows the manufacture of superconducting parts in MgB2 with complex shapes for all types of superconducting applications.
Claims
Claims
1. Method for manufacturing a part of MgB2 comprising: a) the production of a preform by shaping a powder of MgB2 particles using a powder bed additive manufacturing technique, comprising the exposure of the MgB2 powder with laser radiation, and b) a step of densifying the preform, until the part of MgB2 is obtained.
2. Method according to claim 1, characterized in that the median equivalent diameter of the particles of the MgB2 powder varies from 1 pm to 50 pm, in particular varies from 2 pm to 30 pm, preferably varies from 5 pm to 20 pm.
3. Method according to any one of the preceding claims, characterized in that step a) is carried out by selective laser sintering.
4. Method according to any one of the preceding claims, characterized in that step b) comprises a sintering step, in particular by densification under load, or an impregnation step, in particular with a conductive metal other than magnesium, and preferably with copper or an alloy of copper and silver.
5. Method according to any one of the preceding claims, characterized in that it comprises: a) the production of a preform by shaping a powder of MgB2 particles by means of a powder bed additive manufacturing technique, comprising the insolation of the MgB2 powder with laser radiation, with an energy dose varying from 4 J / cm2 / pass to 70 J / cm2 / pass, so as to obtain the preform based on an insolated MgB2 powder, and b) a step of densification of the preform, by sintering the insolated MgB2 powder, until the MgB2 part is obtained.
6. Method according to any one of the preceding claims, characterized in that step a) is carried out in such a way that the densification of the MgB2 powder after insolation varies from 30% to 45%, preferably varies from 35% to 45%, expressed relative to the theoretical density without porosity.
7. Method according to any one of the preceding claims, characterized in that the energy dose of the laser radiation in step a) varies from 4.5 J / cm2 / pass to 70 J / cm2 / pass, in particular varies from 5 J / cm2 / pass to 70 J / cm2 / pass, even more particularly varies from 6 J / cm2 / pass to 60 J / cm2 / pass.
8. Method according to any one of the preceding claims, characterized in that the thickness of the powder bed in step a) varies from 50 pm to 800 pm, in particular varies from 75 pm to 500 pm, preferably varies from 100 pm to 300 pm.
9. Method according to any one of the preceding claims, characterized in that the sintering step is carried out by densification under load, in particular by SPS or by hot pressing, in particular by SPS.
10. Method according to any one of claims 1 to 4, characterized in that it comprises: a) the production of a preform by shaping a powder of MgB2 particles by means of an additive manufacturing technique on a powder bed, in an environment with oxygen, comprising the insolation of the MgB2 powder with laser radiation, with an energy dose varying from 50 J / cm2 / pass to 90 J / cm2 / pass, so as to obtain a counterform based on an MgO powder and the preform based on a non-insulated MgB2 powder contiguous to the MgO powder, and b) a step of densifying the preform, by sintering the non-insulated MgB2 powder in step a), in a sintering furnace under an inert atmosphere, followed by a step of depowdering the MgO powder, until obtaining the MgB2 piece.
11. Method according to the preceding claim, characterized in that the energy dose of the laser radiation in step a) varies from 50 J / cm2 / pass to 80 J / cm2 / pass, preferably varies from 50 J / cm2 / pass to 70 J / cm2 / pass.
12. Method according to any one of claims 10 or 11, characterized in that the thickness of the powder bed in step a) varies from 50 pm to 800 pm, in particular varies from 75 pm to 500 pm, preferably varies from 100 pm to 300 pm.
13. Method according to any one of claims 10 to 12, characterized in that the sintering step is carried out at a temperature varying from 700°C to 1050°C, in particular varying from 750°C to 1000°C, preferably varying from 800°C to 950°C.
14. Method according to any one of the preceding claims, characterized in that it comprises a subsequent step of demolding the MgB2 coin.
15. A method according to any preceding claim, wherein the MgB2 piece is a superconductor having a critical temperature of between 35 K and 39 K.