Clear binder containing plastic waste particles and its applications

A clear binder composition combining vegetable oil esters, plant-origin resin, and plastic waste particles addresses the thermal and sustainability issues of existing binders, effectively managing urban heat islands and maintaining mechanical resistance.

FR3139577B1Inactive Publication Date: 2024-09-20TOTALENERGIES ONETECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022009051
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-09-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing clear binders, both petroleum-based and biosourced, fail to effectively limit and prevent urban heat islands due to insufficient thermal properties and sustainability issues, particularly in urban construction materials like road surfaces, and they degrade quickly, reducing their environmental benefits.

Method used

A clear binder composition comprising a vegetable oil ester derived from tall oil with specific acidity and solidification properties, a plant-origin resin, a polymer based on conjugated diene and monovinyl aromatic hydrocarbon units, and plastic waste particles, which enhances thermal management and mechanical resistance.

Benefits of technology

The binder composition effectively limits and prevents urban heat island phenomena while maintaining mechanical properties comparable to traditional binders, offering improved thermal performance and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Clear binder comprising plastic waste particles and its applications. The invention relates to a clear binder composition comprising (i) a plasticizing agent comprising at least one vegetable oil including an ester compound derived from tall oil, (ii) a structuring agent comprising at least one vegetable resin selected from natural rosins, modified rosins, rosin esters, and any mixture thereof, (iii) at least one polymer based on conjugated diene units and aromatic monovinyl hydrocarbon units, (iv) plastic waste particles comprising a polymeric portion including polypropylene, optionally mixed with polyethylene. Figure for abstract: None
Need to check novelty before this filing date? Find Prior Art

Description

Description Title of the invention: Clear binder comprising particles of plastic waste and its applications Technical field

[0001] — The present invention relates to a clear binder composition incorporating particles of plastic, in particular recycled plastic particles. The invention relates to also a method of preparing a clear binder composition according to the invention. The invention further relates to various uses of a clear binder composition. according to the invention for road and / or industrial applications, in particular for the production of colored surface coating compositions. State of the prior art

[0002] The phenomenon of urban heat islands is defined as localized elevations temperatures, particularly daytime and nighttime maximum temperatures, recorded in urban areas, compared to neighboring rural or forest areas or compared to regional average temperatures. Significant differences in temperature can thus be recorded according to the nature of land use (forest, bodies of water, suburbs, dense city, etc.), relief, exposure or even the season.

[0003] — Urban heat islands have an environmental, meteorological but also also on public health. These harmful effects are accentuated during periods of high heat.

[0004] — The origins of this phenomenon are multiple. They are partly natural, linked directly with the geographical area in which the city is located and the climate associated (range of temperature, humidity, wind exposure, precipitation, etc.). These temperature increases are also linked to human activities res- responsible on the one hand for localized heat emissions (due in particular to the func- operation of cars, construction machinery, various household appliances such as air conditioners but also industrial activity), and on the other hand the emission of greenhouse gases, in particular carbon dioxide or methane, contributing to the phenomenon of global warming.

[0005] — Another factor contributing to the phenomenon of urban heat islands is urbanization, due to the disappearance of natural soils in favor of in- industrial or building. Part of the vegetation participating in thermal management is thus replaced by construction materials such as cement or coated. These coatings are however waterproof and thus block the natural cooling phenomena such as evapotranspiration of the water contained in soils and in plants. Urban morphology, as such, is Also a key element: a dense city with tall, closely spaced buildings creates trapped areas that reduce air circulation that could help with cooling. In addition, some of the solar radiation is reflected by buildings and sent back to the city, thus contributing to a further increase in temperature. Finally, buildings absorb a significant amount of heat, much greater than that absorbed by natural environments. This stored energy is then retransmitted to the urban environment by thermal radiation. There is therefore a need for construction materials, particularly for urban construction, capable of limiting and / or preventing the phenomenon of urban heat islands. In particular, there remains a need for materials with improved thermal properties, in order to prevent and / or limit and / or reduce the increase in urban ambient temperature. In particular, there remains a need for materials with reduced thermal emissivity and / or thermal capacity and / or thermal conductivity. Urban surfaces, particularly road surfaces, are now mostly prepared from bituminous binders or colored coatings, known as light binders. Due to the presence of asphaltenes, bituminous binders are black in color and are therefore difficult to color. Colored coatings are increasingly used because, among other things, they improve road user safety by clearly identifying specific routes such as pedestrian paths, cycle paths, and bus lanes. They also help to mark certain danger zones such as city entrances or dangerous bends. Colored coatings improve visibility in low-light conditions, for example at night or in specific locations such as tunnels.Finally, they simply improve the aesthetic appearance of urban roads and can be used for public squares, courtyards of buildings and schools, sidewalks, pedestrian streets, garden and park paths, parking and rest areas. Therefore, for all the above applications, it is preferred to use clear synthetic binders, which do not contain asphaltenes and can be colored. The clear binders of the prior art generally consist of a plasticizing agent, for example an oil of petroleum origin, a structuring agent, for example a hydrocarbon resin, and a polymer. Application WO2018 / 046838 discloses a cold-solid clear binder. In particular, it describes a clear binder containing a synthetic oil from deasphalting unit cuts (DAO) and a copolymer based on butadiene and styrene units, for example an SB or SBS copolymer. Application WO2018 / 115729 discloses a cold solid binder composition. In particular, the composition may be a clear binder and the plasticizing agent is in particular an oil of petroleum origin. Application WO2018 / 115730 describes a similar composition for the preparation of poured asphalts and the production of coatings. Document US2002 / 052431 discloses aqueous emulsions comprising on the one hand a clear synthetic binder and on the other hand a latex. During manufacture, and then in implementation, these binders are subjected to different types of external factors which modify their structure and cause their properties to evolve. Clear binders with a reduced environmental footprint compared to the clear binders discussed above have also been developed by seeking to at least partially substitute the plasticizing agent and / or the structuring agent with constituents of plant origin. Application EP3081599 describes in this sense a binder of plant origin based on modified tall oil pitch, a modified resin and possibly a polymer. However, these clear binders are not entirely satisfactory. None of these plant-based binders has in fact been shown to be capable of sufficiently limiting and / or preventing the urban heat island phenomena discussed above. Furthermore, although they do indeed have a reduced environmental footprint compared to traditional clear binders, these plant-based binders present sustainability issues. Indeed, currently available clear binders incorporating a plasticizing agent and / or a structuring agent of plant origin have significantly reduced aging resistance compared to traditional clear binders prepared from petroleum-based products. In particular, these binders prepared from plant-based compounds have significantly reduced resistance to aging of cold properties compared to traditional clear binders prepared from petroleum-based products. More regular replacement of road surfaces is therefore to be expected, which significantly reduces their environmental value. There is therefore still a need for bio-sourced clear binders (prepared from at least one plasticizing agent of plant origin and / or at least one structuring agent of plant origin) with improved mechanical properties, compared to existing bio-sourced clear binders. In particular, there remains a need for bio-sourced clear binders (prepared from at least one plasticizing agent of plant origin and / or at least one structuring agent of plant origin) with properties equivalent to traditional clear binders prepared from oil and resin of petroleum origin. There is also a need for clear bio-sourced binders (prepared from at least one plasticizing agent of plant origin and / or at least one structuring agent of plant origin) capable of limiting and / or preventing the phenomenon of urban heat islands. In particular, there remains a need for clear bio-sourced binders (prepared from at least one plasticizing agent of plant origin and / or at least one structuring agent of plant origin) with improved thermal properties, so as to limit and / or prevent and / or reduce the increase in urban ambient temperature. In particular, there remains a need for bio-sourced clear binders (prepared from at least one plasticizing agent of plant origin and / or at least one structuring agent of plant origin) with reduced thermal emissivity and / or thermal capacity and / or thermal conductivity. Surprisingly, it was found that the combination of (i) a vegetable oil comprising an ester derived from tall oil having a solidification temperature of less than 30°C and whose acidity index, determined according to the ASTM D465 method, is less than or equal to 150 mg KOH / g, (ii) a resin of vegetable origin chosen from natural rosins, modified rosins, rosin esters, and mixtures thereof and whose acidity index, determined according to the ASTM D465 method, is less than 8 mg KOH / g, (iii) a polymer based on conjugated diene units and monovinyl aromatic hydrocarbon units, and (iv) plastic waste particles comprising a polymeric part chosen from polypropylene and a mixture of propylene and polyethylene, made it possible to obtain a bio-sourced clear binder capable of limiting and / or preventing the phenomena urban heat islands. In particular, the clear binder according to the invention allows the preparation of an urban surface, in particular a road surface, making it possible to prevent and / or limit and / or reduce the increase in urban ambient temperature. In addition, the clear binder according to the invention has properties similar to those of traditional clear binders, obtained from compounds of petroleum origin. Summary of the invention For the purposes of the invention, the term “bio-sourced clear binder” means a clear binder comprising at least one plasticizing agent of plant origin and / or at least one structuring agent of plant origin. For the purposes of the invention, "urban ambient temperature" means the average temperature measured in the outdoor spaces of a city, particularly in the street. For the purposes of the invention, "surface temperature" means the average temperature measured on the surface of a material present in an urban environment, in particular on the surface of a construction material such as a coating. In the remainder of the application, any reference to a standard (e.g. ASTM D1982) refers to the version of said standard in force on the date of filing of this application. The invention firstly relates to a clear binder composition comprising: (i) a plasticizing agent comprising at least one oil of vegetable origin comprising an ester compound derived from tall oil, said oil of vegetable origin having a solidification temperature, determined according to the ASTM D1982 method, of less than 30°C and an acidity index, determined according to the ASTM D465 method, of less than or equal to 150 mg KOH / g, (ii) a structuring agent comprising at least one resin of plant origin chosen from natural rosins, modified rosins, rosin esters, and any of their mixtures, said resin of plant origin having an acidity index, determined according to the ASTM D465 method, of less than 8 mg KOH / g, (ii) at least one polymer based on conjugated diene units and monovinyl aromatic hydrocarbon units, (iv) plastic waste particles comprising a polymeric part comprising polypropylene, optionally in admixture with polyethylene, and (v) possibly an adhesive dope. Preferably, the ester compound is selected from derivatives of a tall oil fatty acid. More preferably, the ester compound is chosen from the group consisting of: trimethylolpropane tallates, ethylene glycol monomers, neopentyl glycol monomers, 2-ethylhexyl monomers, glycerol monomers, and any of their mixtures. Advantageously, the clear binder composition has a plasticizing agent content ranging from 1% to 40% by mass, relative to the total mass of the composition, preferably from 5% to 30% by mass, more preferably from 10% to 20% by mass. Preferably, the resin of plant origin is chosen from natural rosin esters, more preferably from pentaerythritol esters of natural rosins, in particular from pentaerythritol esters of tall oil rosins. Advantageously, the clear binder composition has a structuring agent content ranging from 50% to 95% by mass, relative to the total mass of the composition, preferably from 60% to 90% by mass, more preferably from 75% to 85% by mass. Advantageously, the polymer is a copolymer of styrene and butadiene, preferably chosen from a styrene / butadiene / styrene block copolymer of radial structure, a butadiene / styrene block copolymer of radial structure and their mixtures. According to a preferred embodiment, the plastic waste particles (introduced into the clear binder composition) have: - a thickness less than or equal to | mm, preferably ranging from 0.1 mm to 0.5 mm, and / or - a length less than or equal to 10 cm, preferably ranging from 0.1 cm to 10 cm, and / or - an area less than 20 cm”, preferably ranging from 5 to 20 cm2. Preferably, the clear binder composition according to the invention has a content of plastic waste particles ranging from 0.1% to 5% by mass, relative to the total mass of the composition, preferably from 0.5% to 3% by mass, more preferably from 0.7% to 1.5% by mass. The invention also relates to a process for preparing a clear binder composition as defined above, comprising the steps: a) bringing the plasticizing agent and the structuring agent into contact, and heating to a temperature between 140°C and 200°C, b) mixing with stirring the plasticizing agent and the structuring agent at a temperature between 140°C and 200°C, c) adding the polymer, mixing and heating to a temperature ranging from 140°C to 200°C. (d) adding the plastic waste particles, mixing and heating to a temperature ranging from 140°C to 200°C, e) adding the possible adhesive dope, mixing and heating to a temperature ranging from 140°C to 200°C. The invention also relates to an emulsion comprising a clear binder composition as defined above and described in detail below, water, and an emulsifying agent. The invention also relates to a coating comprising (i) a clear binder composition as defined above and described in detail below or an emulsion as defined above and described in detail below, (ii) aggregates and / or mineral fillers, and optionally (iii) one or more pigments. According to one embodiment, the coating according to the invention further comprises plastic waste particles comprising a polystyrene polymeric part. Preferably, the coating defined below and in detail below is a draining coating. The invention finally relates to the use of a clear binder composition as defined above and described in detail below, of an emulsion as defined above and described in detail below or of a coating as defined above and described in detail below, for: - limit and / or prevent and / or reduce an increase in urban ambient heat, and / or - limit and / or prevent and / or reduce the surface temperature of construction materials used in urban environments. Detailed description The essential constituents of a clear binder composition are: - a plasticizing agent, for example an oil free of asphaltenes, - a structuring agent, - at least one polymer, - where appropriate, doping agents, or dopes, or adhesiveness dopes. The clear binder of the invention is characterized by the combination of a particular oil of plant origin and a specific resin of plant origin. This selection of components makes it possible to obtain a clear binder with a reduced environmental footprint, compared to clear binders prepared from an oil of petroleum origin and a resin of petroleum origin, while having similar properties, particularly in terms of mechanical strength. For the purposes of the invention, the terms “clear binder” and “clear binder base” are used equivalently. The invention relates to a clear binder comprising: (i) a plasticizing agent comprising at least one oil of vegetable origin comprising an ester compound derived from tall oil, said oil of vegetable origin having a solidification temperature, determined according to the ASTM D1982 method, of less than 30°C and an acidity index, determined according to the ASTM D465 method, of less than or equal to 150 mg KOH / g, (ii) a structuring agent comprising at least one resin of plant origin chosen from natural rosins, modified rosins, rosin esters, and any of their mixtures, said resin of plant origin having an acidity index, determined according to the ASTM D465 method, of less than 8 mg KOH / g (ii) at least one polymer based on conjugated diene units and monovinyl aromatic hydrocarbon units, (iv) plastic waste particles comprising a polymeric portion selected from polypropylene and a mixture of polypropylene and polyethylene, and (iv) possibly an adhesive agent. The plasticizing agent For the purposes of the invention, the term "plasticizing agent" means a chemical constituent making it possible to fluidify and reduce the viscosity and modulus of the binder in which it is incorporated. According to the invention, the plasticizing agent comprises, preferably consists of, at least one oil of plant origin whose characteristics are stated above. The plant-derived oil typically includes at least one plant-derived ester compound derived from tall oil. For the purposes of the invention, the term "tall oil derivative" means a chemical compound obtained at least in part from one of the components of crude tall oil (or CTO). Components of crude tall oil include, for example, tall oil fatty acids (or TOFA), tall oil heads, tall oil rosins and tall oil pitch (also called tall oil pitch). Suitable tall oil derivatives of the invention include acid-functional derivatives such as monomeric, dimeric and trimeric acids made from tall oil fatty acids, dimerized rosin acids and refined fatty acids obtainable from tall oil. The ester compound has a solidification temperature, determined according to the ASTM D1982 method, of less than 30°C. Preferably, the ester compound is selected from C4-Cas, typically C1-Cn, fatty acid esters. In a known manner, an ester compound results from the reaction between a carboxylic acid and an alcohol with elimination of water. In the remainder of the application, the ester compound of the invention is described from the carboxylic acid and the alcohol whose esterification reaction would lead to the production of said ester. According to one embodiment, the carboxylic acid is in a polymerized form, in particular in the form of dimerized fatty acids. Preferably, the fatty acid is selected from the group consisting of: oleic acid, linoleic acid, linolenic acid, palmitic acid and any mixture thereof. Alternatively, the fatty acid is selected from monomeric acids (defined below), dimeric acids, tall oil heads, and the like, and mixtures thereof. The alcohol can be primary, secondary, or tertiary. In particular, it can be a monool, a diol, or a polyol. The alcohol can also come from polyethers such as triethylene glycol or polyethylene glycols. Phenolic esters are also suitable. Preferably, the alcohol is chosen from: methanol, ethanol, 1-propanol, isobutyl alcohol, 2-ethylhexanol, octanol, isodecyl alcohol, benzyl alcohol, cyclohexanol, ethylene glycol monobutyl ether, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, neopentyl glycol, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, dipentaerythritol, sorbitol, sucrose and the like, and any mixture thereof. More preferably, the alcohol is chosen from alcohols comprising a quaternary carbon atom located in the beta position relative to the oxygen of any of their hydroxyl groups. By way of example, mention may in particular be made of trimethylolpropane, neopentyl glycol, trimethylolethane, pentaerythritol, dipentaerythritol, benzyl alcohols and others. As stated above, the ester compound is a derivative of tall oil. Preferably, it is obtained from a tall oil fatty acid (also called TOFA for "Tall Oil fatty acid" in English) or from a derivative of a tall oil fatty acid, for example from a dimer acid of tall oil fatty acid. Tall oil fatty acid is obtained from crude tall oil (or CTO for "Crude Tall Oil" in English) by distillation. Crude tall oil is a by-product of the process of converting wood into paper pulp, also called the Kraft process. Distillation of crude tall oil gives, in addition to tall oil fatty acid, a more volatile and highly saturated fraction of long-chain fatty acids (mainly palmitic acid), called "tall oil heads".Tall oil fatty acid is the next cut, which contains mainly C1g and C16 fatty acids with varying degrees of unsaturation (e.g., oleic acid, linoleic acid, linolenic acid, and various isomers thereof). Another cut, known as distilled tall oil (DTO), is a mixture composed mainly of tall oil fatty acids and a smaller proportion of tall oil rosin. Tall oil rosin (TOR), isolated next, consists largely of a C19-C16 tricyclic monocarboxylic acid. The lower cut from the distillation is known as tall oil pitch or tall oil pitch (or simply "pitch"). In general, any fraction which contains at least one tall oil fatty acid is preferred for the preparation of an ester compound suitable for the invention. As previously stated, polymerized fatty acids can be used to make the tall oil-derived ester compounds of the invention. Unsaturated fatty acids are generally polymerized using acidic clay catalysts. Fatty acids with high levels of mono- or polyunsaturation are preferred. In this high-temperature process, the unsaturated fatty acids undergo intermolecular addition reactions, e.g., the "Alder-ene reaction," to form polymerized fatty acids. The mechanism is complex and not well understood. However, the product comprises primarily dimerized fatty acids and a unique mixture of monomeric fatty acids. Distillation yields a fraction highly enriched in dimerized fatty acid, commonly referred to as "dimer acid." These dimer acids can be used to make skin rejuvenating agents. ester function. Distillation of polymerized tall oil fatty acid provides a fraction enriched in monomeric fatty acids, known as the "Monomer" (with a capital "M") or "Monomeric Acid." The Monomer, a unique composition, is a preferred starting material for the preparation of the ester compound of the invention. While tall oil fatty acid derived from a natural source consists largely of linear Cys unsaturated carboxylic acids, primarily oleic and linoleic acids, the Monomer contains relatively small amounts of oleic and linoleic acids, and instead contains significant amounts of branched and cyclic, saturated and unsaturated C,5 acids, as well as elaidic acid. The more diverse and significantly branched composition of the Monomer results from the catalytic treatment performed on the tall oil fatty acid during polymerization.It is believed that the reaction of Monomer with alcohols to make esters “Monomers” will yield unique derivatives that differ from the corresponding tall oil fatty acid esters. The “Monomer” has been assigned CAS No. 68955-98-6. Examples of Monomer are Century® MOS and MO6 fatty acids, produced by Arizona Chemical Company. Further information on the composition of Monomer and its conversion to various esters is given in U.S. Patent 7,256,162. The ester compounds of the invention include, for example, ethylene glycol tallate (i.e., tall oil fatty acid ethylene glycol ester), propylene glycol tallate, trimethylolpropane tallate, neopentyl glycol tallate, methyl tallate, ethyl tallate, glycerol tallate, oleyl tallate, octyl tallate, benzyl tallate, 2-ethylhexyl tallate, polyethylene glycol tallates, tall oil pitch esters, ethylene glycol monomerate, glycerol monomerate, trimethylolpropane monomerate, neopentyl glycol monomerate, 2-ethylhexyl monomerate, ethylene glycol dimerate, 2-ethylhexyl dimerate, 2-ethylhexyl trimerate, and derivatives thereof. Particularly preferred ester compounds are tallates and monomerates, including trimethylolpropane tallate, ethylene glycol monomerate, glycerol monomerate, and any mixtures thereof. The ester compounds are typically non-crystalline, i.e., they have a solidification temperature, determined according to the ASTM D1982 method, of less than 30°C, preferably less than 20°C, more preferably less than 10°C, and most preferably less than 0°C. Preferably, the ester compounds have a cloud point below 0°C, more preferably below -10°C, even more preferably below -20°C, and most preferably below -25°C. The cloud point is determined by cooling gradually a pure, molten sample and observing the temperature at which the clear sample just becomes cloudy. Preferably, the plasticizing agent has a Gardner color index, determined according to standard ASTM D6166, of less than or equal to 10, more preferably less than or equal to 8. Preferably, the plasticizing agent has a flash point, determined according to the ASTM D92 method, greater than or equal to 200°C, preferably greater than or equal to 250°C, even more preferably greater than or equal to 280°C. Preferably, the plasticizing agent has an acidity index, determined according to the ASTM D465 method, less than or equal to 150 mg KOH / g, more preferably less than or equal to 100 mg KOH / g, even more preferably less than or equal to 50 mg KOH / g. Advantageously, the plasticizing agent has an acidity index, determined according to the ASTM D465 method, less than or equal to 20 mg KOH / g, preferably less than or equal to 15 mg KOH / g, typically between 0.1 mg KOH / g and 15 mg KOH / g. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at 40°C, measured according to the ASTM D445 method, greater than or equal to 30 cSt, more preferably between 30 cSt and 100 cSt, even more preferably between 35 cSt and 50 cSt. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at -20°C, measured according to the ASTM D445 method, greater than or equal to 1000 cSt, more preferably between 1000 cSt and 2000 cSt, even more preferably between 1500 cSt and 1800 cSt, typically 1600 cSt. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at 0°C, measured according to the ASTM D445 method, greater than or equal to 200 cSt, more preferably between 200 cSt and 500 cSt, even more preferably between 300 cSt and 400 cSt, typically 350 cSt. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at 20°C, measured according to the ASTM D445 method, greater than or equal to 50 cSt, more preferably between 50 cSt and 200 cSt, even more preferably between 75 cSt and 150 cSt, typically 100 cSt. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at 40°C, measured according to the ASTM D445 method, greater than or equal to 10 cSt, more preferably between 10 cSt and 100 cSt, even more preferably between 15 cSt and 50 cSt, typically 40 cSt. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at 60°C, measured according to the ASTM D445 method, greater than or equal to 10 cSt, more preferably between 15 cSt and 50 cSt, even more preferably between 20 cSt and 30 cSt. cSt, typically 23 cS$t. Preferably, the plasticizing agent has a Cannon-Fenske kinematic viscosity at 100°C, measured according to the ASTM D445 method, greater than or equal to S cSt, more preferably between 5 cSt and 50 cSt, even more preferably between 5 cSt and 20 cSt, typically 10 cSt. In particular, in a preferred embodiment, the plasticizing agent according to the invention consists solely of one or more ester compound(s) derived from tall oil. For example, an oil that can be used in the clear binder compositions according to the invention may be a product marketed by the company KRATON under the name: SYLVAROAD® RP1000. Advantageously, the clear binder of the invention has a plasticizing agent content ranging from 1% to 40% by mass, relative to the total mass of the clear binder, preferably from 5% to 30% by mass, more preferably from 10% to 20% by mass, typically from 14% to 17% by mass. Advantageously, in the clear binder compositions of the invention, the oils of plant origin, as defined above, represent at least 90% by mass relative to the total mass of the plasticizing agent, preferably at least 95%, even more advantageously at least 98%, and even more advantageously at least 99%. The structuring agent By “structuring agent” we mean any chemical constituent conferring mechanical properties and satisfactory cohesiveness to said binder. The structuring agent used in the composition of the invention is a resin chosen from resins of plant origin. Resins of plant origin can be said to be harvested, that is, harvested from the living plant. They can be used as is, in which case we speak of natural resins, or they can be chemically transformed, in which case we speak of modified natural resins. Harvesting resins include natural rosins, modified rosins, and rosin esters. These can be used alone or in a mixture. Natural rosins include gem and wood rosins, especially pine rosins, and / or tall oil rosins. These natural rosins can be used alone or in a mixture. Modified rosins include hydrogenated rosins, disproportionated rosins, polymerized rosins, and / or maleated rosins. These modified natural rosins can be taken alone or in a mixture, and undergo a or several disproportionation, polymerization and / or maleization treatments. Preferably, the resin is chosen from rosin esters, optionally modified. More preferably, the resin is chosen from modified rosin esters. Even more preferably, the resin is chosen from tall oil rosin esters, possibly modified. Advantageously, the resin is chosen from modified tall oil rosin esters. Rosin esters include natural rosin methyl esters, hydrogenated rosin methyl esters, natural rosin glycerol esters, hydrogenated rosin glycerol esters, disproportionated rosin glycerol esters, polymerized rosin glycerol esters, maleated rosin glycerol esters, natural rosin pentaerythritol esters, and hydrogenated rosin pentaerythritol esters. These rosin esters may be taken alone or as a mixture and may be derived from rosins that have undergone one or more disproportionation, polymerization, and / or maleization treatments. Advantageously, the resin is chosen from pentaerythritol esters of natural rosins, pentaerythritol esters of hydrogenated rosins and any of their mixtures, more advantageously from pentaerythritol esters of natural rosins. According to a preferred embodiment, the resin is chosen from pentaerythritol esters of tall oil rosins. For more information on the plant-based resins that can be used according to the invention, please refer to article K340 by Bernard Delmond published in “Techniques de l'ingénieur”. Preferably, the resin of plant origin has a softening temperature, determined according to the AQCM 003 method, of between 60°C and 200°C, preferably between 80°C and 150°C, more preferably between 90°C and 110°C. Plant-based resin typically has an acidity index, determined according to ASTM D465, of less than 8 mg KOH / g. Preferably, the resin of plant origin has an acidity index, determined according to the ASTM D465 method, of between 0.1 and 8 mg KOH / g, preferably between 0.2 and 7 mg KOH / g, more preferably between 0.5 mg and 6 mg KOH / g. Advantageously, the plant-based resin has an acidity index, determined according to the ASTM D465 method, less than or equal to 5 mg KOH / g. Preferably, the resin has a Gardner color index, determined according to the ASTM D6166 standard, less than or equal to 10, more preferably less than or equal to 5, even more preferably less than or equal to 1, typically 0.9. Preferably, the resin of plant origin has a glass transition temperature, measured according to the AQCM 218 method, of between 10°C and 80°C, preferably between 20°C and 60°C, more preferably between 40°C and 50°C. Preferably, the resin of plant origin has a Brookfield viscosity at 125°C, measured according to the AQCM 004 method, greater than or equal to 5,000 mPa.s, preferably between 7,500 mPa.s and 15,000 mPa.s, more preferably between 10,000 mPa.s and 11,000 mPa.s. Preferably, the resin of plant origin has a Brookfield viscosity at 150°C, measured according to the AQCM 004 method, greater than or equal to 500 mPa.s, preferably between 750 mPa.s and 1500 mPa.s, more preferably between 900 mPa.s and 1000 mPa.s. Preferably, the resin of plant origin has a Brookfield viscosity at 177°C, measured according to the AQCM 004 method, greater than or equal to 80 mPa.s, preferably between 100 mPa.s and 500 mPa.s, more preferably between 150 mPa.s and 200 mPass. For example, a resin usable in the clear binder compositions according to the invention may be a product marketed by the company KRATON under the name: SYLVALITE® 2100 Rosin Ester. Preferably, the weight ratio between the structuring agent and the plasticizing agent used for the preparation of the clear binder composition according to the invention is between 2 and 10, for example between 4 and 6. In a specific embodiment, the content of structuring agent in the clear binder composition of the invention ranges from 50% to 95% by mass, relative to the total mass of the composition, preferably from 60% to 90% by mass, more preferably from 75% to 85% by mass, typically from 76% to 83% by mass. The polymer The polymer used in the process for preparing the clear binder according to the invention is a copolymer based on conjugated diene units and monovinyl aromatic hydrocarbon units. The conjugated diene is preferably chosen from those comprising 4 to 8 carbon atoms per monomer, for example butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene and 1,2-hexadiene, chloroprene, carboxylated butadiene, carboxylated isoprene, in particular butadiene and isoprene, and mixtures thereof. The monovinyl aromatic hydrocarbon is preferably selected from styrene, o-methyl styrene, p-methyl styrene, p-tert-butylstyrene, 2,3 dimethyl styrene, vinyl naphthalene, vinyl toluene, vinyl xylene, and the like or mixtures thereof, especially styrene. Advantageously, the polymer is chosen from copolymers of styrene and conjugated diene. More particularly, the polymer consists of one or more copolymers chosen from block copolymers of styrene and butadiene, of styrene and isoprene, of styrene and chloroprene, of styrene and carboxylated butadiene or of styrene and carboxylated isoprene. Preferably, the polymer consists of one or more copolymers chosen from copolymers of styrene and butadiene. For example, the polymer may be selected from one or more of the following copolymers: SB copolymers (styrene and butadiene block copolymers), SBS (styrene-butadiene-styrene block copolymers), SIS (styrene-isoprene-styrene), SBS* (styrene-butadiene-styrene star block copolymer), SBR (styrene-b-butadiene-rubber). Advantageously, the polymer is chosen from block copolymers. A preferred polymer is a copolymer based on butadiene units and styrene units, in particular such as a styrene / butadiene SB block copolymer or a styrene / butadiene / styrene SBS block copolymer, or a mixture of such copolymers. More preferably, the polymer is a blend of a styrene / butadiene / styrene SBS block copolymer and a styrene / butadiene SB block copolymer. Advantageously, the polymer is a blend of a styrene / butadiene / styrene SBS block copolymer and a styrene / butadiene SB block copolymer in a SB / SBS mass ratio ranging from 0.1:99.9 to 30:70, advantageously from 1:99 to 20:80, even more advantageously from 5:95 to 15:85. The styrene-conjugated diene block copolymer, in particular the styrene-butadiene copolymer, advantageously has a styrene content by weight ranging from 5 to 50%, preferably from 20 to 40%, even better from 25 to 35%. The copolymer of styrene and conjugated diene, in particular the copolymer of styrene and butadiene, advantageously has a weight content of styrene ranging from 20 to 40%, preferably from 25 to 35% by mass relative to the total mass of the copolymer. According to one embodiment, the average molecular mass of the copolymer of styrene and conjugated diene, and in particular that of the copolymer of styrene and butadiene, may be, for example, between 10,000 and 700,000, preferably between 50,000 and 500,000 and more preferably from 200,000 to 400,000 daltons. According to a variant, the average molecular mass of the copolymer of styrene and conjugated diene, and in particular that of the copolymer of styrene and butadiene, may be, for example, between 10,000 and 500,000, preferably between 20,000 and 100,000, more preferably from 30,000 to 75,000 daltons, advantageously between 50,000 and 60,000. The polymer may have a linear, branched or radial structure. Preferably, the copolymer of styrene and conjugated diene, in particular the copolymer of styrene and butadiene, used in the clear binder composition according to the invention, has a radial structure. In a preferred embodiment, the total quantity of the polymer used in the process for preparing the clear binder of the invention is between 0.5 and 20% by mass, preferably between 1 and 10%, preferably between 1.5 and 7.5%, for example between 2.5% and 5%, even more preferably between 3.5% and 4.5% by mass relative to the total mass of the clear binder composition. Polypropylene-based plastic waste particles present in the clear binder composition The clear binder according to the invention further comprises plastic waste particles comprising a polymeric part comprising polypropylene. The plastic waste particles present in the clear binder composition include a polymeric part. The polymeric portion of the plastic waste particles incorporated into the clear binder typically represents at least 80% by mass of the total mass of the plastic waste particles, preferably at least 90% by mass, more preferably at least 95% by mass, advantageously at least 99% by mass. Preferably, the polymeric portion of the plastic waste particles incorporated in the clear binder represents from 80% to 100% by mass of the total mass of the plastic waste particles, more preferably from 85% to 99.9% by mass, even more preferably from 90% to 99% by mass. According to a first embodiment, the polymeric part of the plastic waste integrated into the clear binder consists solely of polypropylene. According to a second embodiment, the polymeric part of the plastic waste integrated into the clear binder comprises a mixture of polypropylene and polyethylene. Preferably, the polymeric part of the plastic waste integrated into the clear binder comprises, preferably consists of: - from 95% to 99.9% by mass of polyethylene, and - from 0.1% to 5% polypropylene. Advantageously, the polymeric part of the plastic waste integrated into the clear binder comprises, preferably consists of, a mixture of polypropylene, low-density polyethylene and halogenated polyethylene, in particular chlorinated polyethylene. More advantageously, the polymeric part of the plastic waste integrated into the clear binder comprises, preferably consists of: - from 90% to 99.8% by mass of low density polyethylene, - from 0.1% to 5% polypropylene, - from 0.1% to 5% by mass of halogenated polyethylene, in particular chlorinated polyethylene. Preferably, the plastic waste particles incorporated into the clear binder have a thickness less than or equal to | mm, more preferably less than or equal to 0.5 mm. More preferably, the plastic waste particles integrated into the clear binder have a thickness ranging from 0.1 mm to 0.5 mm. Preferably, the plastic waste particles incorporated into the clear binder have a length less than or equal to 10 cm, more preferably ranging from 1 mm to 10 cm. Preferably, the plastic waste particles incorporated into the clear binder have a surface area of ​​less than or equal to 20 cm, more preferably ranging from Sem? to 20 cm?. The surface area of ​​the particles is typically determined by multiplying the average particle length by the average particle width. The size of the particles, including their thickness, length and width, is determined by simple measurement using a graduated ruler, in particular according to ISO 7976-1 (“Methods of measurement of buildings and building products — Part!: Methods and instruments”). Advantageously, the plastic waste particles integrated into the clear binder have a glass transition temperature, measured by differential scanning calorimetry, of less than -80°C, preferably between -120°C and -90°C, Advantageously, the plastic waste particles integrated into the clear binder have a melting temperature, measured by differential scanning calorimetry, greater than 50°C, preferably between 70°C and 150°C. Advantageously, the plastic waste particles integrated into the clear binder have an initial crystallization temperature, measured by differential scanning calorimetry, of less than 150°C, preferably less than or equal to 130°C. Advantageously, the content of plastic waste particles in the clear binder composition according to the invention ranges from 0.1% to 5% by mass, relative to the total mass of the composition, preferably from 0.5% to 3% by mass, more preferably from 0.7% to 1.5% by mass. It is typically 1% by mass, relative to the total mass of the clear binder composition. Coloring agents The clear binder may also include one or more coloring agents, such as mineral pigments or organic dyes. The pigments are selected according to the desired shade or color for the coating. For example, metal oxides such as iron oxides, chromium oxides, cobalt oxides, titanium oxides will be used to obtain the colors red, yellow, gray, blue green or white. Pigments can be added, indifferently in the clear binder or in the asphalt (mixed with the aggregates for example) or in an emulsion of the clear binder. Clear binder preparation process The present invention also relates to a process for preparing the clear binder composition which has been described above. This process comprises the following steps: (a) bringing the plasticizing agent and the structuring agent into contact, and heating to a temperature of between 140-200°C, for example for 10 minutes to 1 hour, (b) mixing with stirring the plasticizing agent and the structuring agent at a temperature between 140°C and 200°C, for example from 30 minutes to 2 hours, (c) adding the polymer, for example SB and / or SBS, mixing and heating at a temperature between 140-200°C, for example, from 60 minutes to 3 hours, preferably from 60 minutes to 2 hours, (d) adding the plastic waste particles, mixing and heating at a temperature ranging from 140°C to 200°C, for example from 10 minutes to 60 minutes, and (e) optional addition of an adhesive dope, mixing and heating at a temperature between 140-200°C, for example, from 5 minutes to 30 minutes. Preferably, the process comprises between steps (d) and (e) an additional step of mixing under high shear stirring (6000 rpm), for example from 5 to 30 minutes. The order of steps (a) to (e) can be changed. Advantageously, a clear binder composition according to the invention comprises, by weight relative to the total weight of clear binder, or better still consists essentially of: - from 1% to 40% by weight of plasticizing agent, in particular of the ester compound derived from tall oil, preferably from 5 to 30% by weight, more preferably between 10% and 20% by weight, - from 50 to 90% by weight of structuring agent, in particular resin of plant origin, preferably from 60 to 85% by weight, more preferably from 70 to 85% by weight, - from 0.5 to 20% by weight of polymer, in particular copolymer of styrene and butadiene, preferably from 1 to 10%, even better from 1.5 to 7.5%, advantageously from 2.5 to 5% by weight, - from 0.1% to 5% by mass of plastic waste comprising a polymeric part comprising polypropylene, optionally mixed with polyethylene, preferably from 0.5% to 3% by mass, more preferably from 0.7% to 1.5% by mass, and - optionally from 0.05% to 0.5% by weight of dope, preferably between 0.1% and 0.3% by weight of dope, for example a dope chosen from amines. Preferably, the clear binder according to the invention has a penetrability at 25°C, measured according to standard NF EN 1426, of between 10 and 220 1 / 10 mm, preferably between 20 and 160 1 / 10 mm, more preferably between 30 and 100 1 / 10 mm. A person skilled in the art can modulate the penetrability of the clear binder, in particular by judiciously choosing the weight ratio [structuring agent / plasticizing agent] in the composition of the clear binder. Indeed, it is known that an increase in this ratio makes it possible to reduce the penetrability at 25°C. Advantageously, the clear binder according to the invention has a ring and ball softening temperature (RBT), measured according to the NF EN 1427 method, ranging from 40 to 80°C, advantageously from 45 to 70°C. Clear binder applications The clear binder composition according to the invention can be used and applied indifferently via the so-called “hot”, “warm” or “cold” techniques well known to those skilled in the art. Hot techniques are understood to mean techniques in which the clear binder composition is brought to relatively high temperatures during its application. Hot techniques lead to coatings, asphalts and so-called "hot" mixes such as bitumen gravels, high modulus mixes, bitumen sands, semi-granular bituminous concretes (BBSG), high modulus bituminous concretes (BBME), flexible bituminous concretes (BBS), thin bituminous concretes (BBM), permeable bituminous concretes (BBDr), very thin bituminous concretes (BBTM), ultra-thin bituminous concretes (BBUM). The clear binder composition according to the invention is suitable for the preparation of mixes, asphalts and coatings of all types, and in particular those mentioned above. The invention therefore also relates to coatings comprising a clear binder composition according to the invention, aggregates, optionally fillers and optionally pigments. According to a preferred embodiment, the coating according to the invention further comprises plastic waste particles comprising a polystyrene polymeric part. Plastic waste particles comprising a polystyrene polymeric portion are distinguished from polypropylene-based plastic waste particles defined above in the context of the clear binder composition. In this specific embodiment, the coating according to the invention thus comprises plastic waste particles of two different natures. The coating according to the invention firstly comprises polypropylene-based plastic waste particles, called “polypropylene-based waste particles” introduced into the binder composition. The mix according to the invention further comprises polystyrene-based plastic waste particles, hereinafter referred to as “polystyrene-based waste particles” introduced into the mix, mixed with the aggregates. Polystyrene-based waste particles typically comprise a polymeric part, and an organic part, for example fillers. Preferably, the polymeric portion of the polystyrene-based waste particles represents from 50% to 99.9% by mass of the total mass of the polystyrene-based waste particles, more preferably from 75% to 99.5% by mass, even more preferably from 80% to 99.5% by mass, advantageously from 90% to 99.5% by mass. The organic portion of polystyrene waste particles typically consists of inorganic fillers. Preferably, the polystyrene-based waste particles have an average size, determined by sieving according to standard NF P 18-560, ranging from 1 mm to 20 mm, more preferably from 1.5 mm to 10 mm, typically from 2 mm to 6 mm. More preferably, at least 90% by mass of the polystyrene-based plastic waste has an average size, determined by sieving according to standard NF P 18-560, between 2 mm and 6 mm, preferably at least 95% by mass. Advantageously, the polystyrene-based plastic waste particles have a glass transition temperature, measured by differential scanning calorimetry, of between 80°C and 120°C, preferably between 90°C and 100°C. Advantageously, the polystyrene-based plastic waste particles have a melting temperature, measured by differential scanning calorimetry, between 350°C and 500°C, preferably between 380°C and 465°C. Advantageously, the polystyrene-based plastic waste particles have a degradation temperature, measured by differential scanning calorimetry, greater than 300°C, preferably greater than 380°C. Fillers (or fines) are particles with dimensions less than 0.063 mm. Aggregates include particles of dimensions 0 / 2 (sand), 2 / 4 (gravel), 4 / 6 and 6 / 10. Preferably, the aggregates are chosen from granules of dimensions 0 / 2, 4 / 6, 6 / 10 and their mixtures. The mix generally comprises from 1 to 10% by weight of clear binder, relative to the total weight of the mix, preferably from 4 to 8% by mass, the remainder being made up of aggregates, possibly polystyrene-based plastic waste particles and / or fillers and / or pigments. Typically, the pigments represent a quantity by mass of 0 to 1% of the mix, the fillers represent a quantity by weight of 0 to 2% of the mix. Advantageously, the content of polystyrene-based plastic waste particles in the coating ranges from 0% to 10% by mass, relative to the total mass of the coating, preferably from 0.1% to 10% by mass, more preferably from 0.5% to 8% by mass, advantageously from 1% to 7.5%. It is typically 5% by mass, relative to the total mass of the coating. According to a preferred embodiment, the coating according to the invention is a draining coating. Advantageously, the coating comprises, in relation to the total mass of the coating: - from 1% to 10% by mass of binder, preferably 4% to 8% by mass, more preferably from 3 to 6% by mass: - from 80% to 98% by mass of aggregates, preferably from 84% to 97% by mass; - from 0 to 2% by mass of fillers, preferably from 0.5 to 1.5% by mass; and - 0.1% to 10% by mass of polystyrene-based plastic waste, preferably 2.5% to 7.5% by mass. Another subject of the invention is poured asphalts comprising a clear binder composition according to the invention, mineral fillers and optionally pigments. The asphalt comprises from 1 to 20% by weight of clear binder, relative to the total weight of the asphalt, preferably from 5 to 10% by weight, the remainder being made up of the fillers and optionally the pigments (the pigments representing a quantity by mass of 0 to 1% of the asphalt). Cold techniques are understood to mean techniques based on the use of clear binder emulsions in aqueous phase, at lower temperatures. Cold techniques lead to surface coatings, grouts, cold-cast asphalt mixes, cold asphalt mixes, cold bituminous concretes, emulsion-gravel, storable cold asphalt mixes. The clear binder composition according to the invention is suitable for the preparation of the products mentioned above. The invention therefore also relates to a clear binder emulsion comprising a clear binder composition according to the invention, water and an emulsifying agent. The clear binder comprises at least one plasticizing agent, at least one structuring agent and at least one polymer, as defined above. The invention therefore also relates to a process for preparing a clear binder emulsion comprising: (i) the preparation of a clear binder composition by mixing at least one plasticizing agent, at least one structuring agent and at least one polymer, as defined above, (ii) preparing an emulsifying solution by mixing the water and the emulsifying agent, (iii) dispersing the clear binder of step (1) in the emulsifying solution of step (ii). The clear binder emulsion according to the invention preferably comprises from 50% to 80% by weight of the clear binder composition, preferably from 60% to 70%, relative to the total weight of the clear binder emulsion. The invention further relates to the use of a clear binder composition, an emulsion or a coating according to the invention, to limit and / or prevent and / or reduce a For the purposes of the invention, the term "increase in urban heat" means the difference between ambient temperatures recorded in urban areas, compared to neighboring rural or forest areas or compared to regional average temperatures. The invention finally relates to the use of a clear binder composition, an emulsion or a coating according to the invention, to limit and / or prevent and / or reduce the surface temperature of construction materials used in urban environments. The various embodiments, variations, preferences and advantages described above for the plasticizing agent, the structuring agent and the other components of the clear binder composition apply to the use according to the invention. Surprisingly, it has been observed that the combination of a plant-based oil comprising an ester compound derived from tall oil and a particular rosin resin in a clear binder composition allows, in comparison with other plant-based oils and resins, to obtain improved cold aging resistance properties. This improvement was observed using a standardized test called BBR for determining the flexural rigidity modulus (NF ENI4771: 2012), this test being carried out before and after an aging protocol applied to the sample. This improved cold aging resistance makes it possible to formulate surface coatings, particularly in the road sector, which deteriorate less under the effect of time and / or climatic conditions. The invention is illustrated by the following examples given without limitation. Examples In the examples below, parts and percentages are by weight unless otherwise indicated. Materials and methods: Plasticizer: The oil available under the trade name SYLVAROAD® RP1000 from KRATON was used. This is a vegetable oil obtained from tall oil. Resin: the resin available under the trade name SYLVALITE® was used 2100 Rosin ester from KRATON. This is a plant-based resin comprising a blend of pentaerythritol esters of tall oil rosin. Styrene and butadiene copolymer: a mixture of thermoplastic SB and SBS block copolymers was used, having a content of constituent units derived from 70 / 30 Butadiene / Styrene monomers, of radial structure, obtained by solution polymerization, with a molecular mass of approximately 330,000 daltons polystyrene equivalent (PS), commercially available under the name Calprene 411 from the company Dynasol. Plastic waste particles embedded in the binder (A particles): plastic waste particles comprising at least 80% by mass of low-density polyethylene, at least 0.5% by mass of chlorinated polyethylene and at least 0.5% by mass of polypropylene. The particles have a thickness of less than 0.5 mm, a length of less than 10 cm and a surface area of ​​less than 20 cm?. The glass transition temperature of the particles is between -120°C and -90°C. The melting temperature of the particles is between 70°C and 150°C. The crystallization temperature is less than 130°C. Plastic waste particles incorporated into the asphalt (mixed with aggregates, particles B): plastic waste particles comprising at least 90% by mass of polystyrene and between 0.5% and 10% by mass of inorganic fillers. The particles have an average size ranging from 2 mm to 6 mm. The glass transition temperature of the particles is between 90°C and 100°C. The melting temperature of the particles is between 380°C and 465°C. The degradation temperature is above 380°C. Aggregates for asphalt: mixtures comprising 13% by mass of sand (dimensions 0 / 2), 86% by mass of gravel (dimensions 6 / 10) and 1% by mass of fillers. 1) Pre-mixture of binder according to the i jon (C1 The clear binder is prepared according to the following process: The oil and resin are brought into contact and the whole thing is heated to a temperature of 175°C + - The heated oil and resin are mixed for 2 hours at a stirring speed of 200 rpm, while maintaining the mixture at a temperature of 175°C; - The powdered styrene-butadiene copolymer is added and mixed for 1 hour at 180°C at a stirring speed of 250 rpm. - The plastic waste particles are added gradually, then high shear mixing (6000 rpm) is applied for 15 minutes. - Reduce the stirring to 250 rpm and continue mixing at 180°C for 4 hours. Mé rise ; ; jai ; Jai [Tables 1] Abbreviation | Unit Measurement standard [Steps | 110 mm [NF EN 1426 TBA °CC|NF EN 1427 vi60 Needle-point property at 25€ Softening temperature - ball and ring Viscosity at 160°C - Elastic return measurement ° mPa.S a NF EN 13302 NF EN 13398 Clear binder compositions The clear binder composition according to the invention CI is prepared according to the protocol described in the previous paragraph with the constituents and proportions (in percentage by weight relative to the total weight of clear binder) reported in table 2. [Tables 2] Composition Plasticizing agent Structuring agent SB / SBS copolymer Particles A Homogeneity Homogeneity after reheating Penetrability at 25°C (dmm) TBA (°C) Elastic return (%) Viscosity at 160°C (mPa.s) The composition is formulated at a grade of 50 / 70. Results It is found that the composition according to the invention C1 has good mechanical properties, suitable for use as a clear binder for both road applications and industrial applications. vi ion (C2) The C2 coating is prepared according to the following protocol: The aggregates are preheated to a temperature of mixing equal to 170°C; Separately, the clear binder composition is heated to a mixing temperature equal to 170°C; The hot aggregates are then introduced into a mixer, set at 170°C, and mixed for a few minutes: The following two steps are then carried out, the order of the steps being able to to change : A) The clear binder is added hot to the mixer and mixed with the aggregates for 90 seconds; B) The polystyrene waste particles, not previously heated, are added and the final mixture is left to stir for 30 seconds at 170°C. Methods for determining the properties of the asphalt mix [Tables 3] Abbreviation | Unit Measurement standard | MPa NF EN 12697-12 Property lAbbreviation Unit Measurement standard Crushing strength | MPa NF EN 12697-12 (Duriez) Water sensitivity (Duriez) [vC | NF EN 12697-12 Actual density MVR g / em* NF EN 12697-5 Void content of the asphalt | |PCG % NF EN12697-8 Coated The C2 coating is prepared according to the protocol described in the previous paragraph with the constituents and proportions (in percentage by weight relative to the total weight of coating) reported in table 4. [Tables 4] [10.8 67.1 2.272 23.5 Results It is found that the C2 coating according to the invention has crushing resistance values ​​suitable for use as an urban surface (low traffic). These values ​​are higher (more than 2 times higher) than the conventional values ​​for coatings based on light binders known to those skilled in the art. I / C ratio values ​​close to 70% are satisfactory for a level 0 asphalt mix, i.e. suitable for low traffic roads. The C2 asphalt mix is ​​also advantageous in that it has a low density. Finally, the void content of the material (equal to 23.5%) demonstrates the draining nature of the coating.

Claims

Claims

1. A clear binder composition comprising: (i) a plasticizing agent comprising at least one original oil plant comprising an ester compound derived from tall oil, said oil of vegetable origin with a solidification temperature, de- finished according to ASTM D1982 method, below 30°C and an index acidity, determined according to ASTM D465 method, less than or equal to 150 mg KOH / g, (it) a structuring agent comprising at least one original resin vegetable chosen from natural rosins, rosins modified, rosin esters, and any of their mixtures, said resin of plant origin having an acidity index, determined according to ASTM D465 method, less than 8 mg KOH / g, (iii) at least one polymer based on conjugated diene units and units monovinyl aromatic hydrocarbon, (iv) plastic waste particles comprising a po- lymeric comprising polypropylene, optionally in a mixture with polyethylene, and (v) possibly an adhesive dope.

2. A composition according to claim 1, wherein the ester compound is chosen from derivatives of a fatty acid from tall oil.

3. A composition according to claim 2, wherein the ester compound is chosen from the group consisting of: trimethyl tallates lolpropane, ethylene glycol monomers, monomers of glycerol, and any mixture thereof.

4. Composition according to any one of claims 1 to 3, in in which the plasticizing agent content ranges from 1% to 40% by mass, by relative to the total mass of the composition, preferably from 5% to 30% by mass, more preferably from 10% to 20% by mass.

5. Composition according to any one of the preceding claims, in which the resin of plant origin is chosen from esters of natural rosins, more preferably among the esters of pentaerythritol of natural rosins, especially among the esters of pentaerythritol from tall oil rosin.

6. Composition according to any one of the preceding claims, in which the structuring agent content ranges from 50% to 95% by mass, relative to the total mass of the composition, preferably from 60% to 90% by mass, more preferably from 75% to 85% by mass.

7. Composition according to any one of the preceding claims, wherein the polymer is a copolymer of styrene and butadiene, preferably is chosen from a styrene / block copolymer radial butadiene / styrene structure, a butadiene / block copolymer radial structure styrene and their mixtures.

8. A composition according to any preceding claim. in which the plastic waste particles present: - a thickness less than or equal to | mm, preferably ranging from 0.1 mm to 0.5 mm, and / or - a length less than or equal to 10 cm, preferably ranging from 0.1 cm to 10 cm, and / or - a surface area of ​​less than 20 cm?, preferably ranging from 5 to 20 cm?.

9. Composition according to any one of the preceding claims, in which the content of plastic waste particles ranges from 0.1% to 5% by mass, relative to the total mass of the composition, of preferably from 0.5% to 3% by mass, more preferably from 0.7% to 1.5% by mass.

10. A process for preparing a clear binder composition according to one of any of the preceding claims, comprising the steps: a) bringing the plasticizing agent and the structuring agent into contact, and heating to a temperature between 140°C and 200°C, b) mixing with stirring of the plasticizing agent and the structuring agent at a temperature between 140°C and 200°C, c) adding the polymer, mixing and heating to a temperature ranging from 140°C to 200°C, d) adding plastic waste particles, mixing and heating at a temperature ranging from 140°C to 200°C, e) adding the possible adhesive dope, mixing and heating to a temperature ranging from 140°C to 200°C.

11. An emulsion comprising a clear binder composition according to one of any of claims | to 9, water, and an emulsifying agent.

12. A coating comprising (i) a clear binder composition according to one any of claims 1 to 9 or an emulsion according to reven- dication 11, (ii) aggregates and / or mineral fillers, and pos- (iii) one or more pigments.

13. A coating according to claim 12, further comprising particles of plastic waste comprising a polymeric part of polystyrene.

14. A coating according to claim 12 or claim 13, which is a draining coating.

15. Use of a clear binder composition according to any one of claims 1 to 9, of an emulsion according to claim 12 or of a coated according to one of claims 13 and 14, to limit and / or prevent and / or reduce an increase in ambient heat urban and / or to limit and / or prevent and / or reduce the temperature surface area of ​​building materials used in urban environments.