PVDF-BASED PROTON EXCHANGE MEMBRANE IN THE FORM OF CRYO-GROWN GRANULES
A proton exchange membrane using irradiated PVDF powder from ground granules, grafted with vinyl monomers, addresses the limitations of existing membranes by enhancing thermal resistance and conductivity/gas permeability, enabling effective high-temperature fuel cell operation.
Patent Information
- Application Number
- FR2022012492
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-29
AI Technical Summary
Existing proton exchange membranes, particularly those based on non-fluorinated polymers and perfluorinated polymers, suffer from rapid degradation, low durability, and inadequate conductivity/gas permeability ratios, limiting their effectiveness in fuel cells operating above 80°C.
A proton exchange membrane composed of irradiated PVDF powder, derived from ground granules with a specific particle size and high apparent packed density, is grafted with vinyl monomers to enhance thermal resistance, hydroxide radical resistance, and conductivity/gas permeability ratios.
The membrane exhibits improved thermal resistance up to 120°C, enhanced resistance to hydroxide radicals, and increased conductivity/gas permeability ratios, with ion exchange capacity exceeding 0.65 mmol/g, suitable for high-temperature fuel cell applications.
Smart Images

Figure 00000018_0000
Abstract
Description
Title of the invention: PVDF-BASED PROTON EXCHANGE MEMBRANE IN GRANULE FORM CRYOCROWDERS FIELD OF THE INVENTION
[0001] The present invention relates to a proton exchange membrane based on PVDF in the form of cryogenically ground granules, the method for preparing said membrane, and the application of said membrane in fields requiring ion exchange, such as electrochemistry or in the energy fields. In particular, this membrane is used in the design of fuel cell membranes, such as proton-conducting membranes for fuel cells operating with H2 / air or H2 / O2 (these cells being known under the abbreviation PEMFC for "Proton Exchange Membrane Fuel Cell") or operating with methanol / air (these cells being known under the abbreviation DMFC for "Direct Methanol Fuel Cell"). TECHNICAL BACKGROUND
[0002] A fuel cell is an electrochemical generator, which converts the chemical energy of an oxidation reaction of a fuel in the presence of an oxidant into electrical energy, heat and water. Generally, a fuel cell comprises a plurality of electrochemical cells connected in series, each cell comprising two electrodes of opposite polarity separated by a proton exchange membrane acting as a solid electrolyte. The membrane ensures the passage to the cathode of the protons formed during the oxidation of the fuel at the anode.
[0003] The membranes structure the core of the cell and must, consequently, have good performance in terms of proton conduction, as well as low permeability to reactant gases (H2 / air or H2 / O2 for PEMFC cells and methanol / air for DMFC cells). The properties of the materials constituting the membranes are essentially thermal stability, resistance to hydrolysis and oxidation as well as a certain mechanical flexibility.
[0004] Commonly used membranes that meet these requirements are membranes obtained from polymers belonging, for example, to the family of polysulfones, polyetherketones, polyphenylenes, polybenzimidazoles. However, it has been found that these non-fluorinated polymers degrade relatively quickly in a fuel cell environment and their lifetime remains, for the moment, insufficient for the PEMFC application.
[0005] Most proton exchange membranes are based on the chemistry of perfluorinated polymers having long or short branches carrying sulfonate functions. These different polymers have, in addition to their high cost, a low resistance to hydroxide radicals, which limits their durability in a fuel cell type environment and a low mechanical resistance. These membranes also have an ionic conductivity / hydrogen permeability ratio which does not allow the production of thin membranes combining high impermeability and high conductivity. Furthermore, perfluorinated membranes have a temperature limitation which does not allow them to be operated at temperatures above 80°C for long periods.
[0006] To obtain long-term efficiency in proton conduction at temperatures above 80°C, some authors have proposed more complex materials comprising, in addition to a polymer matrix, proton-conducting particles, the conductivity thus no longer being solely devolved to the constituent polymer(s) of the membranes. This is the case of application WO 2014 / 173885, which describes composite materials comprising a polymer matrix and a filler consisting of inorganic ion-exchange particles, said particles being synthesized in situ within the fluorinated polymer matrix. These membranes have a more homogeneous distribution of the inorganic particles within the polymer matrix.However, this type of membrane has weaker mechanical properties compared to a membrane made from a polymer matrix alone, a risk of cavitation at the particle-matrix interface due to dimensional variations during battery operation, and is difficult to manufacture on an industrial scale.
[0007] Ion-conducting membranes produced by radiation-induced grafting are another option to improve their chemical stability. The radiation grafting reaction is controlled by the diffusion of monomers into the film and the polymerization reactions of the monomers. The reaction starts at the surface of the irradiated film and gradually moves into the bulk of the film. Films based on ethylene tetrafluoroethylene (ETFE), fluorinated ethylene-propylene (FEP), ethylene-chlorotrifluoroethylene (ECTFE) have been described, especially for amphoteric ion exchange membranes.
[0008] Application PCT / FR2022 / 051032 describes a material consisting of an irradiated PVDF, in the form of a powder formed of particles having a volume average diameter (Dv50) ranging from 10 to 50 pm, onto which a styrene monomer and a nitrile monomer are grafted, said irradiated and grafted PVDF carrying proton exchange sulfonate groups. In this document, said powder is obtained by emulsion polymerization, leading to the production of a latex of particles of approximately 200 nm, which after drying, for example, by spraying, leads to the production of particles having an apparent compacted volume mass strictly less than 0.4 g / ml.
[0009] There is a real need for proton exchange membranes with improved properties, including improved thermal resistance and a higher conductivity / gas permeability ratio. Summary of the invention
[0010] To overcome the aforementioned drawbacks, the inventors have developed a membrane having a very particular morphology obtained by starting from a vinylidene fluoride (PVDF) based polymer in the form of irradiated PVDF powder, said powder being obtained from the grinding of granules.
[0011] According to a first aspect, the invention relates to a material consisting of an irradiated PVDF, in powder form, onto which at least one vinyl monomer is grafted, said irradiated and grafted PVDF carrying proton exchange sulfonate groups.
[0012] Typically, the bulk density of said powder is greater than 0.4 g / ml.
[0013] This PVDF powder is produced by grinding granules having a particle size with a D50 between 30 and 80 pm.
[0014] Said PVDF is chosen from poly(vinylidene fluoride) homopolymers and copolymers of vinylidene difluoride with at least one comonomer chosen from the list: vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropene, 2,3,3,3-tetrafluoropropene, 1,3,3,3-tetrafluoropropene, hexafluoroisobutylene, perfluorobutylethylene, 1,1,3,3,3-pentafluoropropene, 1,2,3,3,3-pentafluoropropene, perfluoropropylvinylether, perfluoromethylvinylether, bromotrifluoroethylene, chlorofluoroethylene, chlorotrifluoroethylene, chlorotrifluoropropene, ethylene, and mixtures thereof.
[0015] According to a second aspect, the invention relates to a process for preparing said material, said process comprising the grafting of an irradiated PVDF powder with at least one vinyl monomer chosen from styrenic monomers and nitrile monomers or with a mixture of styrenic and nitrile monomers, followed by a post-treatment of the PVDF powder thus irradiated and grafted, by sulfonation.
[0016] According to a third aspect, the invention relates to a proton exchange polymer electrolyte membrane, said membrane consisting of a film obtained from said PVDF material.
[0017] According to a fourth aspect, the invention relates to a method for manufacturing the proton exchange polymer electrolyte membrane from said irradiated, grafted and functionalized PVDF material in powder form, said method comprising transforming the PVDF powder into film form.
[0018] According to another aspect, the invention relates to a proton exchange polymer composite membrane, said membrane consisting of a porous polymer support impregnated with said PVDF material by solvent and / or aqueous route.
[0019] According to another aspect, the invention relates to a proton exchange polymer composite membrane, said membrane being at least partly made of the fibers of said PVDF material, the remainder being a polymer, and being manufactured by electrospinning. This membrane is then impregnated with said PVDF material by solvent or aqueous means.
[0020] According to another aspect, the invention relates to the applications of the proton exchange polymer electrolyte membrane in the following fields:
[0021] - fuel cells, for example, fuel cells operating with H2 / air or H2 / O2 or methanol / air powered;
[0022] - electrolysers;
[0023] - lithium batteries, said membranes being able to be used in the constitution of electrolytes.
[0024] The present invention makes it possible to overcome the drawbacks of the state of the art. More particularly, it provides a technology which makes it possible to:
[0025] - improve the thermal resistance of the film with no flow for a temperature below 120°C;
[0026] - improve resistance to hydroxide radicals compared to conventional membranes NAFION type commercial vehicles;
[0027] - improve the conductivity / hydrogen permeability ratio compared to the state of art.
[0028] Surprisingly, the use of a powder obtained from granules ground between 30 and 80 μm having a packed bulk density greater than 0.4 g / ml promotes the diffusion of the monomers within the powder and thus leads to grafting rates of between 10 and 100%. The use of a powder whose particles have a packed bulk density greater than 0.4 g / ml also makes it possible to have a better grafting yield, namely greater than 0.8, compared to the powder resulting from synthesis having a packed bulk density less than 0.4 g / ml. The grafting yield is defined as being the ratio between the mass of product obtained after grafting and the mass of product to be obtained theoretically.
[0029] The powder can then be sulfonated in order to contain proton exchange groups making it possible to obtain an ion exchange capacity (IEC) greater than 0.65 mmol / g. It is also possible to use it as a binder or membrane, after transformation, or in both forms for the manufacture of a membrane-electrode assembly, with very good compatibility between the binder and the membrane, and therefore improved efficiency.
[0030] By using a sulfonated grafted powder, it is also possible to vary the morphology of the membrane using conventional powder-to-film transformation techniques of those skilled in the art. This makes it possible to obtain a large variability in the properties, in particular proton conductivity / hydrogen permeability ratios on demand according to application needs. BRIEF DESCRIPTION OF THE FIGURES
[0031] [Fig.l] is a scanning electron microscopy image of a homopolymer PVDF powder, according to the invention, having a D50 of 50 qm and a tapped bulk density of 0.88 g / ml.
[0032] [Fig.2] is a scanning electron microscopy image of a powder of PVDF homopolymer, having a D50 of 10 mm and a tapped bulk density of 0.26 g / ml.
[0033] DESCRIPTION OF EMBODIMENTS OF THE INVENTION
[0034] The invention is now described in more detail and in a non-limiting manner in the following description.
[0035] According to a first aspect, the invention relates to a material consisting of an irradiated PVDF, in powder form, onto which at least one vinyl monomer is grafted, said irradiated and grafted PVDF carrying proton exchange sulfonate groups, characterized in that the apparent compacted density of said powder is greater than 0.4 g / ml.
[0036] According to another aspect, the invention relates to a proton exchange polymer electrolyte membrane, said membrane being obtained from said PVDF material.
[0037] According to various embodiments, said material and said membrane comprise the following characteristics, where appropriate combined. The contents indicated are expressed by weight, unless otherwise indicated. PVDF
[0038] The fluorinated polymer used in the invention, generically designated by the abbreviation PVDF, is a polymer based on vinylidene difluoride.
[0039] According to one embodiment, the PVDF is a poly(vinylidene fluoride) homopolymer or a mixture of vinylidene fluoride homopolymers. The term "VDF homopolymer" includes PVDF homopolymers comprising up to 1% by weight of a comonomer from among those cited below.
[0040] According to one embodiment, the PVDF is a poly(vinylidene fluoride) homopolymer or a copolymer of vinylidene difluoride with at least one comonomer compatible with vinylidene difluoride.
[0041] Comonomers compatible with vinylidene difluoride can be halogenated (fluorinated, chlorinated or brominated) or non-halogenated.
[0042] Examples of suitable fluorinated comonomers are: vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, trifluoropropenes and in particular 3,3,3-trifluoropropene, tetrafluoropropenes and in particular 2,3,3,3-tetrafluoropropene or 1,3,3,3-tetrafluoropropene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropenes and in particular 1,1,3,3,3-pentafluoropropene or 1,2,3,3,3-pentafluoropropene, perfluoroalkylvinylethers and in particular those of general formula Rf-O-CF-CF2, Rf being an alkyl group, preferably C1 to C4 (preferred examples being perfluoropropylvinylether and perfluoromethylvinylether).
[0043] The fluorinated comonomer may comprise a chlorine or bromine atom. It may in particular be chosen from bromotrifluoroethylene, chlorofluoroethylene, chlorotrifluoroethylene and chlorotrifluoropropene. Chlorofluoroethylene may denote either 1-chloro-1-fluoroethylene or 1-chloro-2-fluoroethylene. The 1-chloro-1-fluoroethylene isomer is preferred. Chlorotrifluoropropene is preferably 1-chloro-3,3,3-trifluoropropene or 2-chloro-3,3,3-trifluoropropene.
[0044] The VDF copolymer may also comprise non-halogenated monomers such as ethylene, and / or acrylic or methacrylic comonomers.
[0045] The fluoropolymer preferably contains at least 50 mol% vinylidene difluoride.
[0046] According to one embodiment, the PVDF is a copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (P(VDF-HFP)), having a percentage by weight of hexafluoropropylene monomer units of 1 to 35%, preferably of 2 to 23%, preferably of 4 to 20% by weight relative to the weight of the copolymer.
[0047] According to one embodiment, the PVDF is a mixture of a poly(vinylidene fluoride) homopolymer and a VDF-HFP copolymer.
[0048] According to one embodiment, the vinylidene fluoride copolymer of the invention is a heterogeneous thermoplastic copolymer transformable in the melt state, and comprises two or more co-continuous phases, said co-continuous phases comprising:
[0049] a) from 25 to 50% by weight of a first co-continuous phase comprising 90 to 100% by weight of vinylidene fluoride monomer units and 0 to 10% by weight of units of at least one other fluorinated monomer, and
[0050] b) from more than 50% by weight to 75% by weight of a second co-continuous phase comprising from 65 to 95% by weight of vinylidene fluoride monomer units and one or more co-monomers selected from the group consisting of hexafluoropropylene and perfluorovinyl ether to cause phase separation of the second phase co-continuous of the first continuous phase.
[0051] Said heterogeneous copolymer contains two or more phases which produce a co-continuous structure in the solid state. The co-continuous phases are distinct from each other and can be observed under a scanning electron microscope (SEM). The heterogeneous copolymers according to the invention differ from homogeneous copolymers, which comprise a single phase.
[0052] According to one embodiment, the PVDF is a mixture of two or more VDF-HFP copolymers.
[0053] According to one embodiment, the PVDF comprises monomer units carrying at least one of the following functions: carboxylic acid, carboxylic acid anhydride, carboxylic acid esters, epoxy groups (such as glycidyl), amide, hydroxyl, carbonyl, mercapto, sulfide, oxazoline, phenolic, ester, ether, siloxane, sulfonic, sulfuric, phosphoric, phosphonic. The function is introduced by a chemical reaction which may be grafting, or a copolymerization of the fluorinated monomer with a monomer carrying at least one of said functional groups and a vinyl function capable of copolymerizing with the fluorinated monomer, according to techniques well known to those skilled in the art.
[0054] According to one embodiment, the functional group carries a carboxylic acid function which is a (meth)acrylic acid type group chosen from acrylic acid, methacrylic acid, hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate and hydroxyethylhexyl(meth)acrylate.
[0055] According to one embodiment, the units carrying the carboxylic acid function further comprise a heteroatom chosen from oxygen, sulfur, nitrogen and phosphorus.
[0056] According to one embodiment, the functionality is introduced via the transfer agent used during the synthesis process. The transfer agent is a polymer with a molar mass less than or equal to 20,000 g / mol and carrying functional groups chosen from the groups: carboxylic acid, carboxylic acid anhydride, carboxylic acid esters, epoxy groups (such as glycidyl), amide, hydroxyl, carbonyl, mercapto, sulfide, oxazoline, phenolic, ester, ether, siloxane, sulfonic, sulfuric, phosphoric, phosphonic. An example of a transfer agent of this type is acrylic acid oligomers.
[0057] The content of functional groups in the PVDF is at least 0.01 mol%, preferably at least 0.1 mol%, and at most 15 mol%, preferably at most 10 mol%.
[0058] The PVDF preferably has a high molecular weight. By high molecular weight, as used herein, is meant a PVDF having a melt viscosity greater than 100 Pa.s, preferably greater than 500 Pa.s, more preferably greater than 1000 Pa.s, advantageously greater than 2000 Pa.s. Viscosity is measured at 232°C, at a shear rate of 100 s 1 using a capillary rheometer or a parallel plate rheometer, according to ASTM D3825. Both methods give similar results.
[0059] The PVDF homopolymers and VDF copolymers used in the invention can be obtained by known polymerization methods such as emulsion polymerization.
[0060] According to one embodiment, they are prepared by an emulsion polymerization process in the absence of fluorinated surfactant.
[0061] Polymerization of PVDF results in a latex generally having a solids content of 10 to 60% by weight, preferably 10 to 50%, and having a weight average particle size of less than 1 micrometer, preferably less than 1000 nm, preferably less than 800 nm, and more preferably less than 600 nm. The weight average particle size is generally at least 10 nm, preferably at least 50 nm, and advantageously the average size is in the range of 100 to 400 nm. The polymer particles may form agglomerates, called secondary particles, whose weight average size is less than 5000 μm, preferably less than 1000 μm, advantageously between 1 and 80 micrometers, and preferably 2 to 50 micrometers. Agglomerates may break into discrete particles during formulation and application to a substrate.
[0062] According to certain embodiments, the PVDF homopolymer and the VDF copolymers are composed of bio-sourced VDF. The term "bio-sourced" means "derived from biomass". This makes it possible to improve the ecological footprint of the membrane. The bio-sourced VDF can be characterized by a renewable carbon content, i.e. carbon of natural origin and originating from a biomaterial or biomass, of at least 1 atomic % as determined by the 14C content according to standard NF EN 16640. The term "renewable carbon" indicates that the carbon is of natural origin and originates from a biomaterial (or biomass), as indicated below.According to certain embodiments, the bio-carbon content of the VDF may be greater than 5%, preferably greater than 10%, preferably greater than 25%, preferably greater than or equal to 33%, preferably greater than 50%, preferably greater than or equal to 66%, preferably greater than 75%, preferably greater than 90%, preferably greater than 95%, preferably greater than 98%, preferably greater than 99%, advantageously equal to 100%.
[0063] Emulsion polymerization allows the manufacture of latex particles of approximately 200 nm, which after drying, for example, by spraying, leads to the production of particles having a volume average diameter (Dv50) ranging from 10 to 50 pm.
[0064] A PVDF powder from synthesis is melted using a single-screw, twin-screw, co-rotating or counter-rotating extruder, Buss co-kneader, or a dehydrating extruder in order to obtain, via water cooling and depending on the type of cutting system, granules in lenticular or cylindrical form having a size of a few millimeters.
[0065] The granules thus obtained are then ground in a hammer mill, knife mill, air jet mill, ball mill or ball mill type grinder. The grinding can be done at room temperature or under liquid nitrogen cooling, known as cryo-grinding.
[0066] The PVDF powder has a particle size defined by a Dv50 less than or equal to 100 pm, preferably between 30 and 80 micrometers.
[0067] The Dv50 referred to herein is the volume median diameter which corresponds to the particle size value which divides the population of particles examined exactly in two. The Dv50 is measured according to ISO 9276 - parts 1 to 6. In the present description, a Malvern INSITEC System granulometer is used, and the measurement is made in the dry process by laser diffraction on the powder.
[0068] This powder has an apparent density greater than 0.4 g / ml, preferably between 0.5 and 1.2 g / ml, advantageously between 0.6 and 1.0 g / ml.
[0069] In order to measure the tamped bulk density, a known quantity of PVDF powder is introduced into a precision graduated cylinder. The mass is weighed using a precision balance to 0.1g. Said powder is then tamped in a STAV 2003 type tamping device capable of causing 220 to 250 drops per minute. After 2500 tampings, the volume Vx is measured. The bulk density (BDN), or density, is then calculated as follows: MVA w&w H
[0070] Surprisingly, it was found that the powder from the ground granules, although of a larger particle size than the powder from the synthesis output, makes it possible to obtain higher grafting rates and therefore an ion exchange capacity (IEC) greater than 0.65 mmol / g, higher than for the powder from the synthesis output. PVDF material in powder form
[0071] The material according to the invention consists of a PVDF in the form of irradiated powder, onto which at least one vinyl monomer is grafted.
[0072] According to one embodiment, said at least one vinyl monomer is chosen from styrenic monomers and nitrile monomers, said irradiated and grafted PVDF carrying proton exchange sulfonate groups.
[0073] According to one embodiment, the material according to the invention consists of a PVDF in the form of irradiated powder, onto which a styrenic monomer is grafted, said Irradiated and grafted PVDF carrying proton exchange sulfonate groups.
[0074] According to one embodiment, the material according to the invention consists of a PVDF in the form of irradiated powder, onto which a nitrile monomer is grafted, said irradiated and grafted PVDF carrying proton exchange sulfonate groups.
[0075] According to one embodiment, the material according to the invention consists of a PVDF in the form of irradiated powder, onto which a styrenic monomer and a nitrile monomer are grafted, said irradiated and grafted PVDF carrying proton exchange sulfonate groups.
[0076] This material is prepared according to a process which comprises the grafting of an irradiated PVDF with at least one monomer chosen from styrenic monomers and nitrile monomers or with a mixture of styrenic and nitrile monomers, followed by a post-treatment of the PVDF powder thus irradiated and grafted, by sulfonation.
[0077] Each step of this process is detailed below.
[0078] According to one embodiment, the PVDF powder is first exposed to ionizing radiation to introduce active sites into the PVDF polymer chain. The powder is irradiated by a source of the electron beam, gamma rays, or X-rays type, at a dose of between 25 and 150 kgray and preferably between 30 and 125 kgray. The irradiation is carried out under vacuum, in air or under nitrogen. An irradiated PVDF powder is thus obtained. The irradiated PVDF powder then undergoes a grafting step with at least one vinyl monomer chosen from styrenic monomers and nitrile monomers or with a mixture of styrenic and nitrile monomers,
[0079] According to one embodiment, said styrenic monomer is of alpha-alkyl styrene type, with the alkyl group chosen from: methyl, ethyl, propyl, butyl, pentyl, and hexyl.
[0080] According to one embodiment, said styrenic monomer is chosen from the group: α-methylstyrene, α-fluorostyrene, α-bromostyrene, α-methoxystyrene, vinyl pentafluorostyrene and α, [3, [3-trifluorostyrene.
[0081] According to one embodiment, said styrenic monomer is α-methylstyrene (AMS).
[0082] According to one embodiment, said nitrile monomer is chosen from the group: acrylonitrile, 2-methyl-2-butenenitrile, 2-methylene glutaronitrile and methylacrylonitrile.
[0083] According to one embodiment, the grafted PVDF powder is passed through a bath at 60°C containing between 30 and 50% alpha methyl styrene, between 30 and 50% methylene glutaronitrile and between 0 and 40% isopropanol before being rinsed with isopropanol.
[0084] According to one embodiment, the molar ratio of styrenic monomer to nitrile monomer in the material varies from 0.7 to 1.3.
[0085] According to one embodiment, said nitrile monomer is 2-methylene gluta-ronitrile (MGN).
[0086] Nuclear magnetic resonance (NMR) measurements, via calculation based on the ratio between the area of a specific peak of the aromatic group and / or a specific peak of the nitrile group relative to a reference peak of the PVDF, show a mass rate of grafting of the PVDF of between 10 and 100%, preferably between 15 and 30%.
[0087] The irradiated and grafted PVDF powder is then subjected to a post-functionalization reaction with chlorosulfonic acid, followed by hydrolysis in water or an alkaline solution. This makes it possible to introduce the cation exchange function -SO3H onto the PVDF. According to one embodiment, the PVDF is grafted with α-methylstyrene and 2-methylene glutaronitrile, and is functionalized with chlorosulfonic acid.
[0088] According to one embodiment, the sulfonation of the grafted powder is carried out in a dichloromethane solution containing chlorosulfonic acid at room temperature.
[0089] The grafted PVDF powder carrying the covalently bound -SO3H functions is then rinsed with distilled water until the rinsing water is at neutral pH, before being hydrolyzed at 80°C, then air-dried.
[0090] The sulfonated grafted PVDF powder thus has an ion exchange capacity (IEC) greater than 0.65 mmol / g, preferably greater than 0.7 mmol / g.
[0091] The IEC is measured as follows: a 1cm x 1cm sample is immersed in a 0.5M KCl solution overnight with stirring. The hydrogen ions present in the solution, after exchange with K+ on the sulfonated groups, are then titrated to pH = 7 with a 0.05M KOH solution. The ion exchange capacity is then calculated according to the equation below: d(H') c(KOH) X FfKQH) = —--- - -----------•—:: ---—----------- "" “ DW*) - M(H*)] k(KOH)
[0092] where n(H+) is the number of moles of protons, Wdiy is the mass of the dry membrane in its H+ form, c(KOH) the KOH concentration, V(KOH) the volume of the KOH solution added for the titration, WK the mass of the dried membrane in its K+ form, M(K+) and M(H+) the molar masses of K+ and H+, respectively. Polymer electrolyte membrane
[0093] According to another aspect, the invention relates to a method for manufacturing the proton exchange polymer electrolyte membrane from said irradiated, grafted and functionalized PVDF material in powder form, said method comprising transforming the PVDF powder into a film which constitutes the membrane. This stage of transforming the PVDF powder into film form is carried out using all the techniques known to those skilled in the art: extrusion blow molding, flat extrusion, but also, for example, solvent-based film manufacturing.
[0094] According to another aspect, the invention relates to a proton exchange polymer electrolyte membrane, said membrane consisting of a film obtained from said PVDF material.
[0095] According to another aspect, the invention relates to a method for manufacturing the proton exchange polymer electrolyte membrane from a mixture of said irradiated, grafted and functionalized PVDF material in powder form and another polymer chosen from: polymethyl methacrylate and its copolymers, fluorinated polymers, polyurethanes and polyesters. Said mixture comprises from 100% to 50% by mass of said irradiated, grafted and functionalized PVDF in powder form. The method comprises transforming the mixture into film form. This step of transforming the mixture into film form is carried out by all the techniques known to those skilled in the art: extrusion blow molding, flat extrusion but also for example solvent-based film manufacturing.
[0096] According to another aspect, the invention relates to a proton exchange polymer composite membrane, said membrane consisting of a porous support impregnated with said PVDF material by solvent and / or aqueous route, said porous support being a polymer chosen from: polymethyl methacrylate and its copolymers, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), fluorinated polymers, polyurethanes, polyesters, poly(vinylidene fluoride) (PVDF), polysulfone (PSU), polyethersulfone (PESU), polyimide (PI), the family of polyaryletherketones (PAEK) such as PEEK or PEKK. This porous support can be produced using techniques known to those skilled in the art such as phase inversion, extrusion followed by sequenced stretching, meltblown or spunbond extrusion, electrospinning.
[0097] Dynamic mechanical analysis (DMA) between -40°C and 140°C shows that the membrane does not exhibit fusion. Its elongation at break, measured at 23°C under 50% relative humidity at a speed of 20 mm / minute, for a film thickness of 20 μm, is greater than 100%.
[0098] In membrane-electrode assemblies (MEA), this powder can be used as a binder between the catalyst, other additives such as electronic conductive agents and the membrane.
[0099] According to another aspect, the invention relates to the applications of the proton exchange polymer electrolyte membrane in the following fields:
[0100] - fuel cells, for example, fuel cells operating with H2 / air or H2 / O2 or methanol / air powered;
[0101] - electrolysers;
[0102] - lithium batteries, said membranes being able to be used in the constitution of electrolytes.
[0103] According to one embodiment, the electrolyte polymer membrane is intended to be inserted into a fuel cell device within an electrode-membrane-electrode assembly.
[0104] These membranes are advantageously in the form of thin films, having, for example, a thickness of 10 to 200 micrometers.
[0105] To prepare such an assembly, the membrane can be placed between two electrodes. The assembly formed by the membrane placed between the two electrodes is then pressed at a suitable temperature in order to obtain good electrode-membrane adhesion.
[0106] The electrode-membrane-electrode assembly is then placed between two plates ensuring electrical conduction and the supply of reagents to the electrodes. These plates are commonly referred to as bipolar plates. EXAMPLES
[0107] The following examples illustrate the invention without limiting it.
[0108] Powder A is a PVDF homopolymer having been in powder form at the end of synthesis then extruded in a co-rotating twin-screw. The lenticular granules obtained were then ground in a cryo-hammer mill.
[0109] Powder B is a PVDF homopolymer in the form of a powder resulting from synthesis.
[0110] Both powders were analyzed by scanning electron microscopy at x400 magnification: the scanning electron microscopy image of powder A is shown in the attached [Fig.l], while the scanning electron microscopy image of powder B is shown in the attached [Fig.2].
[0111] All the PVDF powders cited in the examples were irradiated at 50KGray under electron beam and then stored at -30°C for the preservation of the radicals. The powders were then immersed in a solution of alphamethylstyrene and methylene gluta-ronitrile at a molar ratio of 1:1 at 60°C for 6 hours.
[0112] The grafting rate is obtained by gravimetry according to the following formula:
[0113] TG = mass after grafting - initial mass mass after grafting
[0114] The results obtained are presented in Table 1.
[0115] [Tables 1] Examples AB Nature of powder Ground granules Synthesis output MVA (g / mL) 0.88 0.26 D50 50 10 Type of fluorinated PVDF homopolymer PVDF homopolymer Yield 0.95 0.7 IEC (meq / g) 0.72 0.17
[0116] Sample A, obtained from ground granules, has a bulk density of 0.88 g / ml, which makes it easier to separate it from the residual monomers after grafting via centrifugation. Conversely, powder B, resulting from synthesis, has a bulk density of 0.26 g / ml. The separation of this powder and the residual monomers from synthesis after grafting results in losses of material during the washing step. The yield is therefore 0.7, whereas it is greater than 0.9 for powder A.
[0117] As observed by scanning electron microscopy in [Fig.2], the powder B resulting from synthesis is an aggregate of particles of size approximately 200nm, which results in a certain porosity, translated by an MVA of 0.26, and an enhanced access of oxygen within the powder. This aggregate also limits the physical contact between the monomers and the irradiated powder, called wettability. Due to the presence of oxygen and this low wettability, grafting is disadvantaged, resulting in a limitation in the quantity of sulfonyl groups added to the PVDF during post-modification. The IEC value of powder B is therefore only 0.17 mmol / g.
[0118] Conversely, powder A from ground granules has a denser and fuller morphology, which limits the access of oxygen to the radicals present on the PVDF, thus promoting grafting. In addition, since the particles are denser, the wettability of powder A in the monomer mixture is promoted, thus it is possible to increase the quantity of sulfonyl groups after post-modification and thus improve the ion exchange capacity of the powder, here by 0.68 mmol / g.
Claims
Claims
1. Material consisting of an irradiated PVDF, in powder form, onto which at least one vinyl monomer is grafted, said irradiated and grafted PVDF carrying proton exchange sulfonate groups, characterized in that the apparent compacted density of said powder is greater than 0.4 g / ml, preferably between 0.5 and 1.2 g / ml.
2. The material of claim 1, wherein said vinyl monomer is a styrenic monomer.
3. The material of claim 1, wherein said vinyl monomer is a nitrile monomer.
4. Material according to one of claims 1 to 3, wherein said PVDF is grafted with a mixture of styrenic and nitrile monomers, the molar ratio of styrenic monomer / nitrile monomer varies from 0.7 to
5. 1.
3. Material according to one of claims 1 to 4, in which the PVDF is chosen from poly(vinylidene fluoride) homopolymers and copolymers of vinylidene difluoride with at least one comonomer chosen from the list: vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropene, 2,3,3,3-tetrafluoropropene, 1,3,3,3-tetrafluoropropene, hexafluoroisobutylene, perfluorobutylethylene, 1,1,3,3,3-pentafluoropropene, 1,2,3,3,3-pentafluoropropene, perfluoropropylvinylether, perfluoromethylvinylether, bromotrifluoroethylene, chlorofluoroethylene, chlorotrifluoroethylene, chlorotrifluoropropene, ethylene, and mixtures thereof.
6. Material according to one of claims 1 to 5, in which the PVDF is a vinylidene fluoride homopolymer.
7. Material according to one of claims 1 to 5, in which the PVDF is a copolymer of vinylidene fluoride and hexafluoropropylene, having a percentage by weight of hexafluoropropylene monomer units of 1 to 35%, preferably 2 to 23%, preferably 4 to 20% by weight relative to the weight of the copolymer.
8. Material according to one of claims 1 to 5, in which the PVDF is a heterogeneous thermoplastic copolymer, and comprises two or more co-continuous phases, said co-continuous phases comprising: a) from 25 to 50% by weight of a first co-continuous phase comprising 90 to 100% by weight of vinylidene fluoride monomer units and 0 to 10% by weight of units of at least one other fluorinated monomer, and b) from more than 50% by weight to 75% by weight of a second co-continuous phase comprising from 65 to 95% by weight of vinylidene fluoride monomer units and one or more co-monomers selected from the group consisting of hexafluoropropylene and perfluorovinyl ether to cause phase separation of the second co-continuous phase from the first continuous phase.
9. Material according to one of claims 2 and 4 to 8, wherein said styrenic monomer selected from the group: a-methylstyrene, a-fluorostyrene, a-bromostyrene, a-methoxystyrene, vinyl pentafluorostyrene and a, [3, [3-trifluorostyrene.
10. Material according to one of claims 3 to 9, wherein said nitrile monomer is selected from the group: acrylonitrile, 2-methyl-2-butenenitrile, 2-methylene glutaronitrile and methylacrylonitrile.
11. Material according to one of claims 1 to 10, wherein said PVDF is grafted with α-methylstyrene and 2-methylene glutaronitrile, and is functionalized with chlorosulfonic acid.
12. Material according to one of claims 1 to 11, wherein said powder is derived from crushed PVDF granules having a particle size defined by a Dv50 less than or equal to 100 pm, preferably between 30 and 80 micrometers.
13. Process for preparing the material according to one of claims 1 to 12, said process comprising the grafting of an irradiated PVDF powder with at least one vinyl monomer chosen from styrenic monomers and nitrile monomers or with a mixture of styrenic and nitrile monomers, followed by a post-treatment of the PVDF powder thus irradiated and grafted, by sulfonation.
14. A method according to claim 13, comprising the following steps: - exposing said PVDF powder to ionizing radiation selected from electron beams, gamma rays, or X-rays; - exposing the irradiated powder to at least one vinyl monomer selected from styrenic monomers and nitrile monomers or to a mixture of styrenic and nitrile monomers, said styrenic monomer being selected from the group: α-methylstyrene, α-fluorostyrene, α-bromostyrene, α-methoxystyrene, vinyl pentafluorostyrene and α, [3, [3-trifluorostyrene, said nitrile monomer being selected from the group: acrylonitrile, 2-methyl-2-butenenitrile, 2-methylene glutaronitrile and methylacrylonitrile; - subjecting the grafted PVDF powder to a post-functionalization reaction with chlorosulfonic acid, followed by hydrolysis in water or an alkaline solution.
15. A method of manufacturing a proton exchange polymer electrolyte membrane from the PVDF material according to any one of claims 1 to 12, said method comprising transforming the PVDF powder into film form.
16. A method of manufacturing a proton exchange polymer electrolyte membrane from a mixture of the PVDF material according to any one of claims 1 to 12, and another polymer chosen from: polymethyl methacrylate and its copolymers, fluorinated polymers, polyurethanes and polyesters, said method comprising transforming said mixture into film form.
17. A proton exchange polymer electrolyte membrane, said membrane consisting of a film obtained from the PVDF material according to any one of claims 1 to 12.
18. Proton exchange polymer composite membrane, said membrane consisting of a porous support impregnated with the PVDF material according to any one of claims 1 to 12 by solvent and / or aqueous route, said porous support being a polymer chosen from: polymethyl methacrylate and its copolymers, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), fluorinated polymers, polyurethanes, polyesters, poly(vinylidene fluoride) (PVDF), polysulfone (PSU), polyethersulfone (PESU), polyimide (PI), the family of polyaryletherketones (PAEK) such as PEEK or PEKK.
19. Membrane according to one of claims 17 or 18, having an ion exchange capacity (IEC) greater than 0.65 mmol / g, preferably greater than 0.7 mmol / g, as measured by titration with a 0.05 M KOH solution.
20. Fuel cell comprising a membrane as defined in one of claims 17 to 19.