Low-cost, energy-efficient, and environmentally friendly synthesis of plasma-induced N-doped NVOPF cathode for Sodium-ion batteries

IN606039BActive Publication Date: 2026-10-14INDIAN INST OF TECH HYDERABAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202641040619
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-03-31
Publication Date
2026-10-14
Estimated Expiration
2046-03-31

AI Technical Summary

Technical Problem

Existing nitrogen-doping methods for NVOPF cathodes in sodium-ion batteries require wet-chemical conditions that are difficult to control, leading to variations in total N content and N-bonding, which hinder electrochemical performance.

Method used

A hydrothermal synthesis method using water as a solvent, followed by non-thermal plasma treatment under nitrogen gas flow, to achieve controlled nitrogen functionalization of NVOPF cathodes, reducing reaction time and eliminating the need for wet-chemical conditions.

Benefits of technology

Enhances electronic conductivity, accelerates sodium ion kinetics, and improves electrochemical performance by producing a surface N-doped NVOPF cathode with higher capacity and stability, suitable for sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

ABSTRACT Low-cost, energy-efficient, and environmentally friendly synthesis of plasma-induced N-doped NVOPF cathode for Sodium-ion batteries The present subject matter comprises at least two aspects: (i) developing a one-pot hydrothermal synthesis of NVOPF utilizing water as a solvent and resulting in NVOPF microparticle cathode material, (ii) developing high-capacity and better electrochemical performance surface nitrogen-doped NVOPF cathode materials through non-thermal plasma treatment. This dual strategy will yield advanced electrode materials for sodium-ion batteries and other energy storage systems. [To be accompanied with Figure 2]
Need to check novelty before this filing date? Find Prior Art

Description

FIELD OF INVENTION

[001] The present invention relates to the field of Sodium-ion batteries, and more particularly to a method for synthesis of plasma-induced N-doped NVOPF cathode.BACKGROUND OF THE INVENTION

[002] The rising demand for portable electronics, EVs, and grid energy storage positions sodium-ion batteries (SIBs) as a promising alternative to lithium-ion batteries (LIBs), given their cost-effectiveness and the abundance of sodium resources. Unlike lithium, sodium has a larger ionic radius and a higher mass, which hinders ionic diffusion and reduces energy density. NASICON-based polyanionic compounds stand out among various cathodes due to their structural stability, fast Na+-ion mobility, and high working potential (>3.4 V). The Na3V2O2(PO4)2F (NVOPF) is a class of polyanionic compounds that demonstrate high operating voltage (~3.8 V vs. Na+ / Na), a robust three-dimensional structure, and good thermal stability (~400-600°C). This NVOPF cathode material undergoes reversible sodiation and desodiation during charge-discharge cycles, enabling electrochemical energy storage. Having moderate capacity and high voltage, poor electronic conductivity and restricted ion mobility result in a limited energy density for the NVOPF cathode materials in SIBs. To overcome the intrinsic issues associated with the NVOPF cathode, carbon coating, surface doping, cationic / anionic doping, and architectural design can be attempted. Among them, doping engineering can intrinsically enhance electronic conductivity, modify the crystal lattice, accelerate sodium diffusion kinetics, and improve the structural stability of the NVOPF cathode material.

[003] Nitrogen doping has been widely recognized as an effective strategy to enhance the electrochemical performance of Na3V2(PO4)2F3 / NVOPF cathodes, because N-containing functional groups improve electronic conductivity, enrich defect sites for charge transport, and promote the formation of a stable cathode-electrolyte interphase. Although traditional N-doping approaches offer benefits such as improved electronic conductivity, structural stability, and facilitate faster ion diffusion kinetics. They usually require wet-chemical conditions that are difficult to control, as both total N content and N-bonding have been shown to be sensitive to these reaction conditions. Non-thermal plasma (NTP)-assisted surface treatment has emerged as an appealing alternative, as it enables controllable nitrogen incorporation, cleaner reaction pathways,and more uniform functionalization of surfaces, with less variance compared to traditional wet-chemical methods. NTP is a dry technology that eliminates the need for solvents and subsequent treatment of hazardous liquid effluents, reduces costs and energy efficiency, and minimizes waste disposal costs. It enables rapid, continuous processing and is often faster than traditional wet-chemistry methods. The invention aims to produce a hydrothermal method to synthesize NVOPF microparticles, followed by non-thermal plasma-assisted nitrogen surface treatment at various exposure times, including delayed controlled N-functionalization, as a cleaner and tuneable method to enhance electrochemical performance compared to traditional N-doping techniques.

[004] Existing production protocols utilise conventional approaches for nitrogen-doping / incorporation into cathode materials to produce surface-N-doped NVOPF cathode material via solvothermal synthesis, followed by high-temperature treatment. Synthesized nitrogen doped-NVOPF cathode such as N / P-dual-doped carbon-coated Na3V2O2(PO4)2F (Zhang, Lu-Lu, et al., ACS applied materials & interfaces 12.3 (2019) 3670-3680), Na3V2(PO4)3 / N-doped carbon composites (Zhao, Lina, et al., ACS applied materials & interfaces 13.7 (2021) 8445-8454), N-doped Na3V2(PO4)2F3 / C cathode (Yi, Guo-dong, et al., Electrochimica Acta 383 (2021) 138370), and Nitrogen-doped carbon-coated Na3V2O2(PO4)2F (Mao, Yuezhen, et al., Journal of Electroanalytical Chemistry 975 (2024) 118763), etc, were widely developed and utilizes longer reaction duration of 20 h to 65 h to achieve the high performance surface N-doped NVOPF cathode. All these processes rely on wet-chemical conditions that are difficult to control, as both the total N content and the N-bonding.

[005] Other aspects and advantages of the present disclosure will become apparent from the following description, taken in connection with the accompanying drawings which by way of example illustrate exemplary embodiments of the present invention.OBJECTS OF THE INVENTION

[006] Some of the objects of the present disclosure, which at least one embodiment herein satisfy, are listed herein below.

[007] The primary object of the present invention is to produce a hydrothermal method to synthesize NVOPF microparticles, followed by non-thermal plasma-assisted nitrogen surface treatment at various exposure times, including delayed controlled N-functionalization, as a cleaner and tuneable method to enhance electrochemical performance compared to traditional N-doping techniques.

[008] Another object of the invention is non-thermal plasma treatment under nitrogen gas flow to surface-dope the NVOPF cathode material with N.

[009] A further object of the invention is (i) Hydrothermal synthesis of NVOPF cathode material using water as a solvent, (ii) treating the NVOPF material under an inert atmosphere for crystallinity, and (iii) non-thermal plasma treatment under nitrogen gas flow to get the surface nitrogen-doped NVOPF cathode material.

[010] These and other objects and advantages will become more apparent when reference is made to the following description and accompanying drawings.SUMMARY OF THE INVENTION

[011] This summary is provided to refer synthesis of plasma-induced N-doped NVOPF cathode . This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter

[012] The present subject matter refers at least two aspects: (i) developing a one-pot hydrothermal synthesis of NVOPF utilizing water as a solvent and resulting in NVOPF microparticle cathode material, (ii) developing high-capacity and better electrochemical performance surface nitrogen-doped NVOPF cathode materials through non-thermal plasma treatment. This dual strategy will yield advanced electrode materials for sodium-ion batteries and other energy storage systems.

[013] Water as a solvent for the NVOPF synthesis via a hydrothermal approach, and avoid the usage of organic solvents such as ethylene glycol, ethanol, dimethyl formamide, etc.

[014] Performing a shorter reaction duration of 12 h for the hydrothermal synthesis, unlike existing reaction conditions, which utilizes 20 h to 65 h.

[015] Nitrogen doping performed via non-thermal plasma treatment under nitrogen gas flow, resulting in the surface N-doped NVOPF cathode material, and avoid usage of wet-chemical conditions and chemical vapor deposition based plasma methods. This N-modified NVOPF composite enhances electronic conductivity, lowers charge-transfer impedances, accelerates Na-ion kinetics, and improves electrochemical performance for sodium-ion battery applications.

[016] It is to be understood that the aspects and embodiments of the disclosure described above may be used in any combination with each other. Several of the aspects and embodiments may be combined to form a further embodiment of the disclosure.

[017] The foregoing summary is illustrative only and is not intended to be in any way limiting. In addition to the illustrative aspects, embodiments, and features described above, further aspects, embodiments, and features will become apparent by reference to the drawings and the following detailed description.BRIEF DESCRIPTION OF THE ACCOMPANIED DRAWINGS

[018] The features of the invention believed to be novel are set forth with particularity in the appended claims. The invention itself, however, both as to organization and method of operation, together with further objects and advantages thereof, may best be understood by reference to the following description in conjunction with the accompanying drawings in which like characters represent like parts throughout the drawings, and in which:

[019] FIG. 1 illustrates schematic representation of the surface nitrogen-doped NVOPF cathode material, in accordance with an embodiment of the present subject matter.

[020] FIG. 2 illustrates step-by-step synthesis procedure of the NVOPF cathode material, in accordance with an embodiment of the present subject matter.

[021] FIG. 3 illustrates X-ray diffractograms (XRD) of NVOPF, NVN30, NVN45, and NVN60 composite samples.

[022] FIG. 4 illustrates (a) Scanning electron micrograph (SEM) image, (b) Transmission electron micrograph (TEM) image, and (c-f) STEM-EDX images of NVN30 composite.

[023] FIG. 5 illustrates electrochemical analysis. (a) Galvanostatic charge-discharge profiles at 0.1 C rate, (b) Rate capacity at 0.1, 0.2, 0.5, 1, 2, 5, 10, 20, 50 and 100 C current, and (c) Cyclic stability at 1 C of NVOPF, NVN30, NVN45, and NVN60 composite samples.

[024] The figures depict embodiments of the present subject matter for the purposes of illustration only. A person skilled in the art will easily recognize from the following description that alternative embodiments of the structures and methods illustrated herein may be employed without departing from the principles of the disclosure described herein.DETAILED DESCRIPTION OF THE INVENTION

[025] While the embodiments of the disclosure are subject to various modifications and alternative forms, a specific embodiment thereof has been shown by way of example in the figures and will be described below. It should be understood, however, that it is not intended to limit the disclosure to the particular forms disclosed, but onthe contrary, the disclosure is to cover all modifications, equivalents, and alternatives falling within the scope of the disclosure.

[026] The terms "comprise", "comprising", or any other variations thereof used in the disclosure, are intended to cover a non-exclusive inclusion, such that a device, system, assembly that comprises a list of components does not include only those components but may include other components not expressly listed or inherent to such system, or assembly, or device. In other words, one or more elements in a system or device proceeded by "comprises... a" does not, without more constraints, preclude the existence of other elements or additional elements in the system or device.

[027] Referring to FIG. 1, the present subject matter aims at two aspects: (i) developing a one-pot hydrothermal synthesis of NVOPF utilizing water as a solvent and resulting in NVOPF microparticle cathode material, (ii) developing high-capacity and better electrochemical performance surface nitrogen-doped NVOPF cathode materials through non-thermal plasma treatment. This dual strategy will yield advanced electrode materials for sodium-ion batteries and other energy storage systems.

[028] Referring to FIG. 2, as a part of synthesis of surface N-doped NVOPF cathode, following steps are important. (i) Hydrothermal synthesis of NVOPF cathode material using water as a solvent, (ii) treating the NVOPF material under an inert atmosphere for crystallinity, and (iii) non-thermal plasma treatment under nitrogen gas flow to get the surface nitrogen-doped NVOPF cathode material.

[029] The NVOPF material is fabricated using a single-step solvothermal method. The stoichiometric amount of oxalic acid was dissolved in desired amount of deionized water (DIW). Then, the stoichiometric amount of ammonium metavanadate (NH4VO3), sodium fluoride (NaF) and sodium phosphate monobasic dihydrate (NH2PO4.2H2O). The pH is maintained between 6 and 7 to achieve controlled nucleation and better electrochemical performance. Oxalic acid is used as a reducing agent to reduce V5+ to V4+ / 3+ and as a carbon source. The ratio of reducing agent: vanadium: fluorine: phosphorus source is 3:1:1.7:3.

[030] Ammonium metavanadate dissolves in water under hydrothermal conditions, forming vanadyl ions (VO2+), which serve as the building units of the framework. These vanadyl ions coordinate with the phosphate anions to form a vanadium-phosphate backbone. Furthermore, sodium and fluoride ions stabilize the framework and produce the final NVOPF phase. Oxalic acid is used as a reducing agent to reduce V5+ to V4+ / 3+ and as a carbon source.

[031] 2VO3- + 2H+ + C2H2O4 -> 2VO2+ + 2CO2 + 2H2O (i)

[032] 2VO2+ + 2PO43- + F- + 3Na+ -> Na3V2(PO4)2O2F (ii)

[033] Estimated overall chemical reaction:

[034] 2NH4VO3 + 2NaH2PO4 + NaF + 3H2C2O4 -> Na3V2(PO4)2O2F + 6CO2 + 2NH3 + 5H2O

[035] The dissolved solution was subjected to hydrothermal treatment at 180 °C for 12 h. During hydrothermal treatment, nucleation begins, leading to the crystal growth and formation of primary particle sizes of 2-5 μm. These primary particles aggregate, forming secondary particles micro-cuboid aggregates of 10-14 μm. The product was washed three times with de-ionized water and ethanol to remove the unwanted impurities in the resultant solution. Thereafter, the washed product was dried overnight in a hot-air oven at 80 °C. These micro-cuboids were further heated under an inert atmosphere to further crystallize the NVOPF phase particles.

[036] Non-thermal plasma is introduced on ~1.5 g NVOPF powder material under a N2 gas flow rate of 15 ml min-1 at an applied voltage of 22 kV, resulting in a surface N-enriched NVOPF cathode material. Under the strong electric field of the DBD (dielectric barrier discharge) plasma, the nitrogen molecule is activated through successive electronic excitation, followed by electron-induced ionization, producing energetic species (e-, N, N+, N2+, and N*) that subsequently bombard the NVOPF cathode material surface. The high-energy electrons, ions, and free radicals in the plasma initiate reactions without needing excessive heat. Non-thermal plasma treatment results in surface doping of the NVOPF cathode material. The NVOPF sample was exposed for 30 min, 45 min, and 60 min, abbreviated as NVN30, NVN45, and NVN60, respectively.Experimental methods:

[037] For electrochemical assessment, a working electrode slurry was prepared by mixing active cathode material, Super P C65, carbon black, and PVDF binder in a weight ratio of 70:20:10, using NMP as the dispersing solvent. The mixture was then ball-milled for at least 5 hours to achieve homogenization, before being coated onto aluminium foil using a doctor blade. The electrodes were vacuum-dried overnight at 100°C, calendared with a hot-press roll, and then cut into 10 mm diameter discs. Sodium metal was shaped into 16 mm diameter discs for use as both counter and reference electrodes. GF / D fiberglass separators were saturated with ~90 μL of electrolyte 1 M NaClO4 in a 4.5:4.5:1 volumetric ratio EC:PC: DMC with 5 wt.% FEC. The mass loading of the active material was maintained at 3-4 mg cm-2. Cell assembly was performed inside an Ar-filled glove box (mBraun, Germany) at less than 0.1 ppm O2 and H2O, and the cells were packaged into CR2032 coin cells in an NVOPF / / Na two-electrode cell configuration, with at least 5 cells tested per configuration.

[038] Figure 3 shows the X-ray diffractograms of NVOPF, NVN30, NVN45, and NVN60 composite samples. The X-ray diffraction patterns of the NVN30, NVN45, and NVN60 composite samples exhibit nearly pure phase composition and high crystallinity, as shown in Figure 1. This ensures the material has been synthesized in nearly pure crystalline form, and there is no change in the bulk structure even after plasma treatment.

[039] Figure 4 (a, b) SEM images show the 2-3 μm microcuboid particle of the surface N-modified NVN30 composite sample. Figure 4(c-f) shows the TEM image and the STEM-EDX mapping confirms the existence of the N element in the surface N-modified NVN30 composite sample.

[040] Figure 5 shows the electrochemical analysis. (a) The galvanostatic charge-discharge curves of NVOPF and NVN30, NVN45, and NVN60 composite electrodes were tested at a slower current rate of 0.1 C, delivering the highest achievable capacity of 121 mAh g-1 for the NVN30 electrodes (Figure 5a). In contrast, the other composite electrodes, such as NVN45, NVN60, and NVOPF, delivered the specific capacity of 115, 110, and 109 mAh g-1, respectively, as shown in Figure 5a. The capacity contribution from both plateaus at 3.6 V and 4.1 V is almost 50%, attributed to the vanadium redox couple of V4+ / 5+. The improved capacity is attributed to the surface modification of the NVOPF cathode, which facilitates better electrolyte infiltration and sodium-ion migration. (b) The specific capacity is recorded at varying current densities, ranging from 0.1 C to 0.2, 0.5, 1, 2, 5, 10, 20, 50, and 100 C. The NVN30 sample showed a higher rate capacity of 79 mAh g-1 at 100 C, indicating that the cell underwent charging and discharging in less than a minute and still retained 65% of its initial capacity. On the other hand, the NVN45, NVN60, and NVOPF achieved specific capacities of 76, 71, and 67 mAh g-1 at a 100 C rate, respectively, as shown in Figure 5b. The higher rate capability of modified composite electrode compared to pristine NVOPF is attributed to improved reaction kinetics and minimal polarization. (c) The surface N-modified NVOPF sample tested at a 1C current rate showed 87% retention and indiscernible capacity fading over 1000 cycles of charge and discharge (Figure 5c). In contrast, the NVN45 and NVN60 samples remain 82% and 80% of their capacity after 1000 cycles, respectively. The pristine NVOPF sample retains only 70% of the initial discharge capacity after 500 cycles at a 1C rate.

[041] The higher capacity and electrochemical improvements of surface N-modified NVOPF composite obtained through these methods demonstrate the environmental benefits and technical advantages of this material. This non-thermal plasma treatment for heteroatom doping of cathode and anode materials can advance the performance of Na-ion batteries.

[042] Synthesis of surface N-modified NVOPF cathode for sodium-ion batteries through a hydrothermal method followed by plasma treatment. This process benefits from (a) environmental friendliness as it utilizes water as a solvent, (b) reducing the hydrothermal reaction time to 12 h, and (c) the surface nitrogen doping through nonthermal plasma treatment showcases enhanced electronic conductivity, lowers charge-transfer impedances, accelerates Na-ion kinetics, and improves electrochemical performance for sodium-ion battery applications.

[043] The surface N-modified NVOPF composite sample (NVN30) achieved a greater capacity of 121 mAh g-1 at a 0.1 C rate and good cycling stability of 87% at 1 C over 1000 cycles, demonstrating the efficacy of this process.

[044] It should be noted that the description and figures merely illustrate the principles of the present subject matter. It should be appreciated by those skilled in the art that conception and specific embodiment disclosed may be readily utilized as a basis for modifying or designing other structures for carrying out the same purposes of the present subject matter. It should also be appreciated by those skilled in the art that by devising various systems that, although not explicitly described or shown herein, embody the principles of the present subject matter and are included within its spirit and scope. Furthermore, all examples recited herein are principally intended expressly to be for pedagogical purposes to aid the reader in understanding the principles of the present subject matter and the concepts contributed by the inventor(s) to furthering the art and are to be construed as being without limitation to such specifically recited examples and conditions. The novel features which are believed to be characteristic of the present subject matter, both as to its organization and method of operation, together with further objects and advantages will be better understood from the following description when considered in connection with the accompanying figures.

[045] It will be further appreciated that functions or structures of a plurality of components or steps may be combined into a single component or step, or the functions or structures of one-step or component may be split among plural steps or components. The present invention contemplates all of these combinations. Unless stated otherwise, dimensions and geometries of the various structures depicted herein are not intended to be restrictive of the invention, and other dimensions or geometries are possible. In addition, while a feature of the present invention may have been described in the context of only one of the illustrated embodiments, such feature may be combined with one or more other features of other embodiments, for any given application. It will also be appreciated from the above that the fabrication of the unique structures herein and the operation thereof also constitute methods in accordance with the present invention. The present invention also encompasses intermediate and end products resulting from the practice of the methods herein. The use of "comprising" or "including" also contemplates embodiments that "consist essentially of' or "consist of' the recited feature.

Claims

1. A method for synthesis of plasma-induced N-doped NVOPF cathode for Sodium-ion batteries comprising: Performing a one-step hydrothermal synthesis of NVOPF utilizing water as a solvent, treating the NVOPF material under an inert atmosphere for crystallinity, and developing a surface nitrogen-doped NVOPF cathode material through nonthermal plasma treatment of crystallized NVOPF material.

2. The method as claimed in claim 1, wherein the performing of one-step hydrothermal synthesis comprises dissolving stoichiometric amount of oxalic acid in deionized water (DIW); and further dissolving a stoichiometric amount of ammonium metavanadate (NH4VO3), sodium fluoride (NaF) and sodium phosphate monobasic dihydrate (NH2PO4.2H2O).

3. The method as claimed in claim 2, wherein during the synthesis, pH is maintained between 6 and 7 to achieve controlled nucleation and better electrochemical performance.

4. The method as claimed in claim 2, wherein the oxalic acid is used as a reducing agent to reduce V5+ to V4+ / 3+ and as a carbon source, the reducing agent comprising vanadium: fluorine: phosphorus source in a ratio of 3:1:1.7:3.

5. The method as claimed in claim 2, wherein the synthesis comprises: Subjecting the dissolved solution of claim 2 to hydrothermal treatment at 180 °C for 12 h to trigger: a. nucleation and crystal growth and formation of primary particles, wherein the primary particles are 2-5 μm in size; and b. aggregation of primary particles to form secondary particles micro-cuboid aggregates of 10-14 μm in size.

6. The method as claimed in claim 5, wherein the micro cuboids are washed three times with de-ionized water and ethanol to remove the unwanted impurities in the resultant solution, followed by drying overnight in a hot-air oven at 80 °C.

7. The method as claimed in claim 6, wherein micro-cuboids were further heated under the inert atmosphere to further crystallize the NVOPF phase particles.

8. The method as claimed in claim 1, wherein the non-thermal plasma treatment comprises: introducing non-thermal plasma on about 1.5 g synthesized NVOPF under a N2 gas flow rate of 15 ml min-1 at an applied voltage of 22 kV, resulting in a surface N-enriched NVOPF cathode material.

9. The method as claimed in claim 8, wherein the non-thermal plasma treatment further comprises: activating nitrogen molecule under an electric field of the DBD (dielectric barrier discharge) plasma through successive electronic excitation, followed by electron-induced ionization, producing species (e-, N, N+, N2+, and N*) to bombard the NVOPF cathode material surface to produce the surface N-enriched NVOPF cathode material.

10. The method as claimed in claim 1, wherein the non-thermal plasma treatment comprises subjecting treatment to the synthesized NVOPF material for 30 min, 45 min, and 60 min to produce a plurality of variants of the surface N-enriched NVOPF cathode material as NVN30, NVN45, and NVN60, respectively.