A method for preparing a sustainable multifunctional synthetic slag and the multifunctional synthetic slag thereof
Patent Information
- Application Number
- IN202641033830
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-03-20
- Publication Date
- 2026-10-26
- Estimated Expiration
- 2046-03-20
AI Technical Summary
Existing steelmaking processes face challenges with slag disintegration, boron micro alloying, inclusion modification, steel desulphurization, and high melting temperatures, leading to environmental pollution and inefficiencies, while transitioning to green steelmaking is not cost-effective.
A method for preparing a sustainable multifunctional synthetic slag composed of CaO-Al2O3-B2O3, with optimized weight percentages, which serves as a boron micro alloying agent, inclusion modifier, and slag stabilizer, reducing melting point and viscosity, and improving desulphurization kinetics.
The developed slag reduces slag disintegration, lowers melting point by 30%, enhances boron recovery, and improves desulphurization efficiency, while reducing synthetic slag consumption and environmental impact.
Abstract
Description
FIELD OF THE INVENTION:[1] The present invention is in the field of steel manufacturing, more particularly in thetechnical field of premelting and refining slag. To be specific, the invention relates to amethod for preparing a sustainable multifunctional synthetic slag and themultifunctional synthetic slag thereof.BACKGROUND OF THE INVENTION:[2] The properties of refining slags play a crucial role in steelmaking, such asdesulphurization, inclusion removal, preventing re-oxidation of steel,dephosphorisation etc. The refining slag should have optimum sulphide capacity,viscosity, basicity, and melting temperature. CaF2 and CaO-Al2O3-based fluxes arewidely used in secondary steelmaking to achieve the optimal LF (Ladle furnace) slagcomposition required for steel refining.[3] Basic oxygen Furnace (BOF) is one of the methods of primary steelmaking, used forrefining pig iron to steel. Steel obtained from BOF is further refined in secondarymetallurgy using a Ladle Furnace (LF). Synthetic slags are added during tapping steelfrom BOF to the Ladle and further treated in the Ladle Furnace. Steels can be broadlyclassified depending on the deoxidation process as Si-Killed and Al-Killed steels. Mostof the ladles used for steelmaking are lined with MgO-C refractory bricks. The steelfrom BOF is further treated by the addition of ferro alloys to get the desired chemicalcomposition. During tapping steel from BOF to the ladle, some amount of oxidizingBOF slag is carried over from BOF to ladle. The composition of top slags formed duringLadle Furnace (LF) refining plays a major role in desulphurisation, inclusionabsorption, preventing heat loss, preventing reoxidation of steel, etc. Around 5-10 kgof synthetic slag / ton of steel is added in ladle, depending on the composition andproperties of synthetic slags. Calcium aluminate synthetic slags, CaF2 have wideapplicability in secondary steelmaking as fluxes. The high alumina in calciumaluminate slag helps achieve a refractory-friendly CaO-MgO-Al2O3 LF slag systemrather than a CaO-SiO2-MgO slag system, particularly in Si-Killed steels. CaF2 isobsolete due to associated health risks. Ladle Furnace slags generated after the additionof conventional fluxing agents such as CaO-Al2O3 based slags are highly basic and havedi-Calcium silicate (C2S-2CaO.SiO2) as one of the major phases. LF slag disintegratesor pulverizes during cooling due to volume expansion, leading to landfilling problems,environmental pollution, and poor valorisation potential. Ferro Boron (FeB) is widelyused for boron micro alloying in low and medium carbon steels to improve themechanical properties. Production of high purity FeB is a challenge and an energyintensive process. Conventional boron containing ferro alloys contain 5-20 % of boron.With growing environmental concerns, there is a need for the development ofsustainable boron microalloying practice. B2O3 emerged as a promising fluxingmaterial in iron making and steelmaking to improve overall process efficiency. B2O3 aslow as 0.5wt% of LF slag is used as slag stabilizer for ferro alloy, iron, and steel makingslags. Usage of boron-based material in ferro alloy production resulted in a reductionof furnace clogging and overall process efficiency. B2O3 addition may increase ordecrease the melting point and viscosity of slag systems. Hence, optimisation of slagchemistry is done to develop a low-melting synthetic slag with B2O3. The novelty ofinvention lies in optimising wt% B2O3 in CaO-Al2O3 slag to achieve multifunctionallow melting synthetic slag.[4] Reference is made to IN202441016268A, which discloses the use of recycled Al killedLF slag stabilized with B2O3 as a flux in Ladle Furnace refining. 0-4 wt% H3BO3 wasadded as Al killed LF slag stabilizer. However, only Al -Killed LF slag can be recycledin the provided method. B2O3 source may not dissolve uniformly as addition was donein slag containers.[5] Reference is further made to IN202441008179A which discloses the use of 70-80 %lime, 3-8 wt% B2O3, and 10-20 wt% CaO-Al2O3 synthetic slag for treating Si-killedsteels in LF. The ladle flux comprised 60-80 wt% CaO, 1-3wt% SiO2, 5-15 wt% Al2O3,2-8 wt% B2O3 as major constituents. However, H3BO3 used in the citation mayevaporate during addition at steelmaking temperatures, leading to less recovery.[6] Reference is also made to CN103849712A which describes the use of CaO-Al2O3-B2O3 flux as a replacement to CaF2. The flux comprised of 55-60 wt% of CaO, 15-20wt% of Al2O3, and 5-10% of B2O3. However, the method disclosed in the citationdoes not mention the use of recycled LF slag as a source of CaO and Al2O3.[7] With growing environmental concerns, there is an urgent need to reduce specific CO2emissions. However, the transition to green steel making is not cost-effective yet.Recycling LF slag to replace calcined fluxes will reduce specific CO2 emissions per tonof crude steel produced. In the prior art, it is found that there is a need for developmentof premelted CaO-Al2O3-B2O3 synthetic slag for steelmaking to solve the problem ofslag disintegration, boron micro alloying, inclusion modification, steel desulphurisationand low melting properties. To address all the above problems, a multifunctional,sustainable, low-melting synthetic slag which serves the purpose of flux, boron microalloying agent, and LF slag stabilizer is developed.OBJECT OF THE INVENTION:[8] The principal object of the present invention is to provide a method for preparing asustainable multifunctional synthetic slag and multifunctional synthetic slag thereof.[9] Another object of the present invention is to provide a method for preparing asustainable CaO-Al2O3-B2O3 synthetic slag that has a low melting point, acts as a boronmicro alloying agent, inclusion modifier, and a slag stabilizer in secondary steelmaking.
[10] Another objective of the invention is to use the CaO-Al2O3-B2O3 synthetic slag for steelrefining, such as for treating both Si-killed and Al-Killed steels.
[11] Another objective of the invention is to improve the recycling potential of SecondarySteelmaking slags.
[12] Another objective of the invention is to replace ferro boron (FeB) with CaO-Al2O3-B2O3 synthetic slag for boron micro alloying.
[13] Another objective of the invention is ease of adding B2O3 source in pre-melted form tomaximise recovery.
[14] Another objective of the invention is to reduce the consumption of synthetic slags insteelmaking.
[15] Another objective of the invention is to reduce steel production cost.SUMMARY OF THE INVENTION:
[16] The invention relates to a method for preparing a sustainable multifunctional syntheticslag and multifunctional synthetic slag thereof.
[17] The present invention provides a method for preparing a sustainable multifunctionalsynthetic slag that serves the purpose of slag stabilisation, boron micro alloying,inclusion modifier and slag fluxing in steelmaking. The prepared synthetic slag is addedduring tapping steel from BOF / EAF into the ladle for slag fluxing effect, in secondarysteelmaking processes after deoxidizing steel for the purpose of boron micro alloyingin presence of Si or Al in steel and in Ladle Furnace or any other secondary steelmakingunits after finish of treatment for slag stabilization. Hence, it is added in ladle duringtapping steel and at LF during reefing for achieving all three functions i.e., slag fluxing,boron micro alloying and slag stabilization. Moreover, the prepared synthetic slagimproves desulphurisation kinetics by lowering slag viscosity and improving limedissolution. The sustainable synthetic slag is prepared from a mixture of CaO (35-50wt%), Al2O3 (30-45 wt%), B2O3 (2-6 wt%), MgO (4-10 wt%) and SiO2 (2-5wt%).The melting temperature of the CaO-Al2O3-B2O3 synthetic slag is 1200-1300°C whichis 30% lower than Calcium Aluminate synthetic slag and due to its ultra-low meltingpoint, the specific synthetic slag consumption is reduced in steel industries.
[18] In an aspect of the present invention, there is provided a method for preparing amultifunctional synthetic slag, comprising: (i) mixing at least one source of calciumoxide (CaO), aluminium oxide (Al2O3) and boron oxide (B2O3) to form a mixture; (ii)grinding the mixture obtained in step (i) to form a homogenous slag mixture; and (iii)feeding the slag mixture obtained in step (ii) into graphite crucibles and melting thesame to form a multifunctional synthetic slag.
[19] In another aspect of the present invention, there is provided a multifunctional syntheticslag for steel refining, comprising: (a) CaO; (b) Al2O3; (c) B2O3; and (d) MgO.DESCRIPTION OF THE ACCOMPANYING DRAWINGS:
[20] The accompanying drawings constitute a part of the description and are used to providefurther understanding of the present invention. Such accompanying drawings illustratethe embodiments of the present invention, which are used to describe the principles ofthe present invention together with the description.
[21] Figure 1 illustrates a detailed flowsheet for preparing sustainable CaO-Al2O3-B2O3synthetic slag, in accordance with an implementation of the present invention.
[22] Figure 2 depicts raw materials used for melting experiments i.e., (a) calcium aluminatesynthetic slag, (b) B2O3 source, in accordance with an implementation of the presentinvention.
[23] Figure 3 depicts graphite crucibles used for melting experiments, in accordance withan implementation of the present invention.
[24] Figure 4 depicts the high temperature (1800°C ) muffle furnace used for meltingexperiments, in accordance with an implementation of the present invention.
[25] Figure 5 illustrates the layout of melting experiments at lab scale, in accordance withan implementation of the present invention.
[26] Figure 6 depicts visual appearance / macroscopic image of air-cooled slags samples (a)0 wt% B2O3 (b) 2 wt% B2O3 (c) 4 wt% B2O3 (d) 6 wt% B2O3 (e) 8 wt% B2O3 in calciumaluminate synthetic slag, in accordance with an implementation of the presentinvention.
[27] Figure 7 illustrates inclined Plane setup for measuring slag fluidity: (a) Line Diagram(b) Experimental setup, in accordance with an implementation of the present invention.
[28] Error! Reference source not found. illustrates (a) Image of slag ribbons obtained fromInclined Plane test; (b) Effect of temperature and wt% B2O3 on slag fluidity; and (c) theeffect of B2O3 addition on fluidity of calcium aluminate slag measure from InclinedPlane test, in accordance with an implementation of the present invention.
[29] Error! Reference source not found. illustrates Ash Fusion determinator used formeasuring slag melting temperature, in accordance with an implementation of thepresent invention.
[30] Figure 10 illustrates high temperature microscopy images of slag samples measuredusing the Ash Fusion determinator, in accordance with an implementation of the presentinvention.
[31] Figure 11 illustrates the effect of B2O3 addition on calcium aluminate slag meltingtemperature measured from Ash Fusion Determinator, in accordance with animplementation of the present invention.
[32] Figure 12 illustrates the effect of B2O3 addition on viscosity of calcium aluminate slagcalculated from empirical models, in accordance with an implementation of the presentinvention.
[33] Error! Reference source not found. illustrates the effect of B2O3 addition on mineralogyof air cooled calcium aluminate slag from X-Ray Diffraction analysis (XRD)(1:12CaO.7Al2O3, 2:2CaO.Al2O3, 3:3CaO.B2O3), i.e. (a) XRD analysis of 0 wt% B2O3synthetic slag, (b) XRD analysis of 2 wt% B2O3 synthetic slag, (c) XRD analysis of 4wt% B2O3 synthetic slag, (d) XRD analysis of 6 wt% B2O3 synthetic slag, and (e) XRDanalysis of 8 wt% B2O3 synthetic slag, in accordance with an implementation of thepresent invention.
[34] Figure 14 illustrates effect of 0-6 wt% B2O3 on depolymerisation and 8 wt% B2O3 onpolymerisation of CaO-Al2O3-B2O3 synthetic slag, in accordance with animplementation of the present invention.
[35] Error! Reference source not found. illustrates the effect of B2O3 on meltingtemperature of different LF slag systems, in accordance with an implementation of thepresent invention.
[36] Error! Reference source not found. illustrates the effect of B2O3 in LF slag on boronmicro alloying for different steel and slag compositions from FactSage 8.4, inaccordance with an implementation of the present invention.
[37] Figure 17 illustrates the effect of B2O3 addition on liquid slag region in CaO-SiO2-Al2O3 0.1 mass fraction MgO LF slag system at 1500°C, in accordance with animplementation of the present invention.
[38] Error! Reference source not found.8 illustrates effect of B2O3 content on plastic area ofinclusions in CaO-MnO-SiO2 at 1200°C (B is wt% B2O3), in accordance with animplementation of the present invention.
[39] Error! Reference source not found.9 illustrates the process flow of an integrated steelPlant, in accordance with an implementation of the present invention.
[40] Figure 20 illustrates possibilities of CaO-Al2O3-B2O3 synthetic slag addition atdifferent stages of steel refining (a) During tapping steel from BOF into the ladle (b)During Ladle Furnace refining (c) After the finish of steel refining in Ladle Furnace, inaccordance with an implementation of the present invention.
[41] Error! Reference source not found.21 illustrates the multiple functions of CaO-Al2O3-B2O3 synthetic slag in Ladle Furnace refining, in accordance with an implementationof the present invention.
[42] Figure 22 illustrates a summary of the advantages of multifunctional CaO-Al2O3-B2O3synthetic slag, in accordance with an implementation of the present invention.
[43] Figure 23 illustrates triple role of B2O3 in LF after addition of developed premeltedCaO-Al2O3-B2O3 synthetic slag, in accordance with an implementation of the presentinvention.DETAILED DESCRIPTION OF THE INVENTION:
[44] While the invention is susceptible to various modifications and alternative forms, aspecific embodiment thereof will be described in detail below. It should be understood,however, that it is not intended to limit the invention to the particular forms disclosed,but on the contrary, the invention is to cover all modifications, equivalents, andalternatives falling within the scope of the invention as defined by the appended claims.
[45] Although one or more features and / or elements may be described herein in the contextof only a single embodiment, or alternatively in the context of more than oneembodiment, or further alternatively in the context of all embodiments, the featuresand / or elements may instead be provided separately or in any appropriate combinationor not at all. Conversely, any features and / or elements described in the context ofseparate embodiments may alternatively be realized as existing together in the contextof a single embodiment.
[46] The terminology used herein is for the purpose of describing particular variousembodiments only and is not intended to be limiting of various embodiments. As usedherein, the singular forms "a," "an" and "the" are intended to include the plural formsas well, unless the context clearly indicates otherwise.
[47] In addition, as used herein, the term "or" is an inclusive "or" operator, and is equivalentto the term "and / or" unless the context clearly dictates otherwise. The term "based on"is not exclusive and allows for being based on additional factors not described, unlessthe context clearly dictates otherwise.
[48] As discussed in the background section of the present invention, the existing methodsreported in the references or literature show that there is an urgent need to reducespecific CO2 emissions, but the transition to green steel making is not cost-effectiveyet. Recycling LF slag to replace calcined fluxes will reduce specific CO2 emissionsper ton of crude steel produced. In the prior art, it is found that there is a need fordevelopment of pre-melted CaO-Al2O3-B2O3 synthetic slag for steelmaking to solve theproblem of slag disintegration, boron micro alloying, inclusion modification, steeldesulphurisation and low melting properties.
[49] Therefore, to overcome the existing problems in the art, the present invention providesa method for preparing a sustainable multifunctional synthetic slag and themultifunctional synthetic slag thereof.
[50] In another embodiment, the present invention provides a method for preparing amultifunctional synthetic slag, comprising: (i) mixing at least one source of calciumoxide (CaO), aluminium oxide (Al2O3) and boron oxide (B2O3) to form a mixture; (ii)grinding the mixture obtained in step (i) to form a homogenous slag mixture; and (iii)feeding the slag mixture obtained in step (ii) into graphite crucibles and melting thesame to form a multifunctional synthetic slag.
[51] In another embodiment, the present invention, provides a method as described herein,wherein CaO is present in a range of 35-50wt%.
[52] In another embodiment, the present invention, provides a method as described herein,wherein Al2O3 is present in a range of 30-45wt%.
[53] In another embodiment, the present invention, provides a method as described herein,wherein B2O3 is present in a range of 2-8wt%.
[54] In another embodiment, the present invention, provides a method as described herein,wherein the melting is performed at a temperature of 1500°C.
[55] In another embodiment, the present invention, provides a method as described herein,wherein the slag having a chemical composition comprising 35-50wt% of CaO, 30-45wt% of Al2O3, 2-6 wt% of B2O3, 4-10 wt% of MgO, 2-5wt% of SiO2.
[56] In another embodiment, the present invention provides a multifunctional synthetic slagfor steel refining, comprising: (a) CaO; (b) Al2O3; and (c) B2O3 (d) MgO.
[57] In another embodiment, the present invention provides a slag as described herein,wherein the source of CaO is selected from Limestone, Calcined lime, Recycled LFslag and Calcium Aluminate synthetic slag.
[58] In another embodiment, the present invention provides a slag as described herein,wherein the source of Al2O3 is selected from Calcium Aluminate synthetic slag,Calcined Bauxite and Recycled LF slag.
[59] In another embodiment, the present invention provides a slag as described herein,wherein the source of B2O3 is selected from a group consisting of Boron Oxide (B2O3),Boric acid (H3BO3), Borax (Na2O.2B2O3.10H2O), Kernite (Na2O.2B2O3.5H2O),Colemanite (2CaO.3B2O3.5H2O), Ulexite (Na2O. 2CaO.5B2O3.16H2O), Datolite(2CaO.B2O3.2SiO2.H2O), Danburite (CaO.B2O3.2SiO2), Ludwigite (Mg2Fe3+BO5) andSuanite (Mg2B2O5(OH)2.
[60] In another embodiment, the present invention provides a slag as described herein,wherein the source of MgO is selected from a group consisting of dolomite and calcineddolomite.
[61] In another embodiment, the present invention provides a slag as described herein,wherein the slag comprises 35-50wt% of CaO, 30-45 wt% of Al2O3, 4-10 wt% MgOand 2-6 wt% of B2O3.
[62] In another embodiment, the present invention provides a slag as described herein,wherein the CaO and Al2O3 are present in a ratio in the range of 1.1-1.16.
[63] In another embodiment, the present invention provides a slag as described herein,wherein the slag exhibits a melting temperature in a range of 1200-1300°C.
[64] In another embodiment, the present invention provides a slag as described herein,wherein the slag has a viscosity in a range of 0.17-0.25 Pa.s at 1500°C due to theformation of 2D-BO33-units and low-melting compounds.
[65] In another embodiment, the present invention provides a slag as described herein,wherein the slag is used for silicon (Si) and aluminium (Al) killed steel refining, steelmaking, slag fluxing, boron micro alloying, slag stabilisation and inclusionmodification.
[66] Overall, the present invention's method is different and technically advance over theconventional prior art(s) in view of the following advantages:- The present invention describes a method for preparing synthetic slag thatserves the purpose of slag stabilisation, boron micro alloying, inclusion modifierand slag fluxing in steelmaking.- The developed synthetic slag is added during tapping steel from BOF / EAF intothe ladle for slag fluxing effect.- The developed synthetic slag is added in secondary steelmaking processes afterdeoxidizing steel for the purpose of boron micro alloying in presence of Si orAl in steel.- The developed synthetic slag is added in Ladle Furnace or any other secondarysteelmaking units after finish of treatment for slag stabilization.- The developed synthetic slag is added in ladle during tapping steel and at LFduring reefing for achieving all three functions i.e., slag fluxing, boron microalloying and slag stabilization.- The developed synthetic slag improves desulphurisation kinetics by loweringslag viscosity and improving lime dissolution.- The sustainable synthetic slag is prepared from mixture of CaO is 35-50wt%,Al2O3 is 30-45 wt%, B2O3 is 2-6 wt%, MgO is 4-10 wt%, SiO2 is 2-5wt%.- The melting temperature of the CaO-Al2O3-B2O3 synthetic slag is 1200-1300°Cwhich is 30% lower than Calcium Aluminate synthetic slag.- Due to its ultralow melting point, the specific synthetic slag consumption willbe reduced in steel industries.
[67] The present invention is illustrated hereunder in greater detail in relation to non-limitingexemplary embodiments as per the following examples:EXAMPLES
[68] The following examples are put forth so as to provide those of ordinary skill in the artwith a complete disclosure and the description of how to make and use the presentinvention, and are not intended to limit the scope of what the inventors regard as theirinvention nor are they intended to represent that the experiments below are all and onlyexperiments performed. The methodology of preparing few of the preferredembodiments shall become clearer with working examples provided below.Example 1: A method for preparing a sustainable multifunctional synthetic slag
[69] A method of developing CaO-Al2O3-B2O3 synthetic slag for treating steels is shown inFigure 1. The synthetic slag is prepared by mixing CaO, Al2O3 and B2O3 where CaOis 35-50wt%, Al2O3 is 30-45 wt%, B2O3 is 2-6 wt%, MgO is 4-10 wt%, SiO2 is 2-5wt%.B2O3 forms low melting eutectics such as 12CaO.7Al2O3, Ca3B2O6, Ca11B2Si4O22,Ca2B2SiO7 in the synthetic slag and reduces melting point and viscosity of slag. B2O3forms 2D planar BO3 units and simplifies complex aluminate network by forming BO-Al linkages rather than Al-O-Al linkage. Various sources of B2O3 are listed in Table1. Various sources of Al2O3 include calcined bauxite, calcium aluminate synthetic slag,recycled LF slags which contain CaO and Al2O3 as major constituents as shown inTable 2. Various sources of CaO include recycled LF slag, limestone, calcined lime asshown in Table 3.Table 1: Various sources of B2O3Table 2: Various sources of Al2O3Table 3: Various sources of CaOTable 4: Various sources of MgO
[70] Raw materials were chosen as shown in Error! Reference source not found.. CalciumAluminate synthetic slag with composition as shown in Table 4 and boric acid areground to fine powder so as to achieve 2-8 wt% B2O3 in the mixture. The slag mixturewas fed to graphite crucibles as shown in Figure 3 and melted in muffle furnace asshown in Error! Reference source not found.. The slag mixture was melted with heatingrate of 9°C / minute and held at 1500°C for 30 minutes for homogenisation as shown inError! Reference source not found.. The macroscopic image of air-cooled slag samplesis given in Error! Reference source not found.. The appearance of slag changed toglassy structure with B2O3 addition.Table 3: Chemical Composition of the slag investigated in the present work (wt%)Example 2: Experimental tests on the prepared synthetic slag
[71] Fluidity test: The fluidity of melted slag was measured using Incline plane setup asshown in Error! Reference source not found.. The tests were carried out using a "V"-shaped stainless-steel plate and a Muffle Furnace. The slag samples (20 g in weight)were transferred to a graphite crucible and kept in the furnace at 1500°C and 1600°Cfor 20 minutes.
[72] After taking the crucible from the furnace, the liquid slag was poured over the top of a"V" shaped stainless-steel plate inclined at 14°. The molten slag flows down andsolidifies as a slag ribbon. The length of the slag ribbon was measured with a ruler. Thesteel plate was cleaned with acetone before each run. The furnace opening time topouring start time is 8±2 seconds for all the samples. There was a temperature drop ofaround 100°C during this time gap. After each test, the weight of the slag ribbon andslag remaining in the crucible was measured. The weight retained in the crucible is 0-3.8 grams. Each test is repeated 3 times, and the maximum length of ribbon observedwas considered for fluidity estimation. With B2O3 addition the length of slag ribbonincreased at 1500°C and 1600°C upto 6 wt% B2O3 and decreases with 8 wt% B2O3.This shows that fluidity of slag increased with B2O3 addition upto 6 wt% B2O3 additionand decreased with 8 wt% B2O3 as shown in Error! Reference source not found..
[73] Test for melting temperature: The melting temperature of the slag was estimatedusing Ash Fusion determinator as shown in Figure 9 and Figure 10. ASTM D1857standard was followed for the analysis. AFD is standardized by observing the meltingpoints of copper and nickel before testing. Approximately 5 g of powdered (-250 μm)slag sample was mixed with water and a dextrin (100g / l) solution to make a smoothpaste. The paste was then pressed into a stainless-steel mold to make a cone. The driedtest pieces are mounted using MgO refractory paste on a 5-position Corundum carouseland introduced into the Ash fusion determinator (AFD) as shown in Figure 5. Thesamples are then heated in H2 / CO2 atmosphere with a heating rate of 8°C / min. Thetemperatures were recorded automatically with a high-precision photographic recordcamera. Hemisphere temperature was considered as slag melting temperature.Temperature was recorded at four points:- DT (Deformation Temperature): when the rounding off of the sample tip isobserved;- ST (Softening Temperature): when the height of the sample equals the width;- HT (Hemisphere Temperature): when the height of the sample is half the width;and- FT (Flow Temperature): when the slag fuses and flows.
[74] With 6 wt% B2O3 addition the melting temperature of calcium aluminate slag reducedfrom 1331 to 1248°C. For every 2 wt% increase in B2O3, the temperature decreased by30°C upto 6 wt% B2O3 addition as shown in Figure 11. With 8 wt% B2O3 addition themelting temperature increased due to self-polymerisation of BO3 and BO4 units in slag.In addition to that, B2O3 forms low melting point eutectics with CaO and MgO anddecreases the overall melting point and viscosity of LF slags upto 6 wt% B2O3 addition.Due to the addition of a small quantity of B2O3 low melting and highly basic slags areachieved which will improve the desulphurization capability of top slags. As B2O3 isa surface-active component, it increases the electrical conductivity which is beneficialfor arcing in LF. The energy of B-O bonds is very large and B3+ ions destroy [SiO4]4-- [SiO4]4- and form will form [SiO4]4-- [BO3]3- structures. The bond energy of B-O (787kJ / mol) is much larger than that of Si-O (600 kJ / mol) and Al-O (485 kJ / mol). Thebigger the bond energy, the more unstable it is. This might increase the probability thatthe B-O bond will be destroyed and the polymerization degree of the system willdecrease. B2O3 forms low-melting components (such as CaO-B2O3, CaO-2B2O3, andBaO-B2O3) with CaO, thus reducing the liquidus temperature of systems. First, the lowmelting temperature of B2O3, which is 450°C, is favourable for the high meltingtemperature components such as CaO and Al2O3 fusing into slag, so the meltingtemperature of the system is decreased. B2O3 forms low melting eutectics such asCa3B2O6, Ca11B2Si4O22, Ca2B2SiO7 in steelmaking slags and reduces melting point andviscosity of slag systems. The addition of B2O3 simplifies the complex networkstructure in slag by forming 2D-BO3 units, thus reducing slag viscosity and meltingtemperature. Because the melting temperatures of these eutectics are low, the formingof eutectics is also favourable for decreasing the melting temperature of slag. Theviscosity of the slag was calculated using empirical models. The viscosity of slagreduced from 0.4 Pa.s to 0.17 Pa.s with 6 wt% B2O3 addition at 1500°C as shown inFigure 12. To achieve synthetic slag with ultra low melting point and viscosity, B2O3content is limited to 6 wt% in the developed synthetic slag with CaO / Al2O3 ratio in therange of 1.1-1.16.
[75] X-ray Diffraction (XRD) analysis: To identify mineralogical phases, XRD analysiswas carried out for air-cooled slag samples. Powdered slag samples were characterizedusing Rigaku Ultima IV with 2θ between 10-90°, Cu Kα radiation with a wavelengthof 1.54 A, and a step size of 0.02. The structure of slag changed from crystalline toamorphous with 8 wt% B2O3 addition. With B2O3 addition low melting phase3CaO.B2O3 was formed in the slag as shown in Figure 13.
[76] Structural changes: Even though a larger number of BO33- units are formed, theymight have undergone self-polymerisation with 8 wt% B2O3 addition by forming B-OB linkages instead of attaching to the aluminate network as shown in Figure 14. Hence,there is a saturation limit to realize the fluxing effect of B2O3 in CaO-Al2O3 slagsystems. This might be the reason for increased slag melting temperature and reducedslag fluidity beyond 6 wt% B2O3 addition. In the studied slag system, B2O3 showedbasic behavior till 6wt% B2O3 addition and acidic behavior at 8 wt%.
[77] Equilibrium phase test: Computational thermodynamics software FactSageTM 8.4(developed by GTT-technologies) with FToxid , FSStel, and FactPS was used for theanalysis. Equilibrium phases were calculated in the temperature range of 600-1500°C(with a heating step of 25°C) for the studied calcium aluminate slag as shown in Table5.Table 4: Equilibrium phases in calcium aluminate slag with B2O3 addition
[78] The effect of 0-6 wt% B2O3 on the melting temperature of LF slag, as shown in Table5 with different CaO / Al2O3 and CaO / SiO2 ratios, was estimated with a step size of25°C. The melting temperature of all the slag systems decreased with B2O3 addition asshown in Error! Reference source not found.13.Table 5: Different LF slag compositions studied using FactSage
[79] The equilibrium boron picks up by liquid steel with B2O3 addition in slag (Slag is 2%of steel weight) was studied by conducting equilibrium calculation in the FactSageusing FSstel, FactPS, and FToxid databases. Equilibrium slag-metal reactions wereconsidered at 1600°C for different steel grades and LF slag compositions, as shown inTable 6. Four different grades of steel were considered for FactSage simulations:LCAK (Low carbon Al Killed), HCSK (High Carbon Si / Mn Killed), BS (Boron steel),and TS (Tire Cord steel).Table 6: Composition of steel and slag for FactSage simulations (wt %)
[80] Boron micro alloying: The boron requirement in BS grade is 18 to 30 ppm, whereasthere is no boron requirement is other grades considered. The slag composition forLCAK, HCSK, and BS grades was considered based on the slag samples collected froman integrated steel plant. The slag composition for TS grade was taken from theliterature. Equilibrium calculations revealed that, boron pickup in all the steel gradesincreased with wt% B2O3 in slag, Si or Al wt% in steel, as shown in Figure 16. WithB2O3 addition, LF slag is maintained in a higher basicity range even with a low meltingpoint, as shown in the isothermal ternary projection presented in Figure 17. It isnoteworthy to mention that boron pickup is <10 ppm with 4 wt% B2O3 addition inLCAK steel, whereas boron pickup was>30 ppm in HCSK and TS steel grades with4wt% B2O3 in slag at 1600°C as shown in Figure 16. Maximum boron pickup wasobserved in TS grade steel, which has a higher Si range. For boron steel, even 6 wt%B2O3 in slag resulted <22 ppm boron. The boron steel grade has both Al and Si as perthe grade requirement. As B2O3 has more affinity to Al in steel, varying Si content didnot have much effect on boron recovery. The kinetics of boron recovery may dependon Si and Al range in the steel grades considered. Therefore, boron steels are developedusing B2O3 by partially replacing costlier FeB.
[81] Research states that slag-aided boron micro alloying reduces ferro alloy consumptionand improves the mechanical properties in low and medium-carbon steels, dependingon the type of compounds formed, such as boron nitride (BN), B4C (Boron Carbide),B2O3 inclusions and iron borides (Fe2B, FeB). With an increase in wt% B2O3 in thecomplex MnO-SiO2-Al2O3 inclusions, the percentage of liquid slag region at 1200°Cincreased, as shown in Figure 18. B2O3 replaces hazardous CaF2 and costlier calciumaluminate fluxes in secondary steel making. Boron is reduced from B2O3 in slag to steelby reacting with aluminum and silicon in the steel, as shown in equations 1 and 2. Boronis reduced from B2O3 by Al and Si at steelmaking temperatures. Studies revealed thatboron recovery depends on slag composition, treatment time, temperature and B2O3content in slag. With increase in the initial Si and Al content in the steel, the boronconcentration in the steel also increases. Micro alloying with boron increases thehardenability while reducing the need for expensive alloying elements like Ni, Cr, Mo,Mn.2(B2O3) + 4 [Al] = 4 [B] + 2(Al2O3) .......... 12(B2O3) + 3 [Si] = 4 [B] + 3(SiO2) .......... 2
[82] B2O3 emerged as an inclusion modifier in tire cord steels due to its ability to form lowmelting compounds. However, B2O3 forms desirable low-melting deformable MnOSiO2-Al2O3 inclusions or detrimental non-deformable BN rings in high carbon Si / Mnkilled steels. Plasticity of inclusions is an important factor for improving the drawabilityof high carbon steels, which consist mainly of MnO-SiO2-Al2O3-CaO-MnS typeinclusions. Optimum B2O3 addition forms low melting B2O3-CaO-SiO2-Al2O3 andB2O3 -MnO-SiO2-Al2O3 inclusion systems in steels. The mechanism of slag aidedboron microalloying is depicted in Figure 6.
[83] The slag aided boron micro alloying is divided into the following kinetic steps:1. (B2O3) is transferred from molten slag to the steel / slag interface, and the[Si] / [Al] is transferred from molten steel towards the interface.2. BO33- and [Si] or [Al] are exchanged at the steel slag interface through reductionof boron from B2O3.3. Al2O3 / SiO2 and [B] are transferred from the steel / slag interface towards the slagand steel phase, respectively.
[84] From the thermodynamic analysis, it is seen that the activity of boron in steel isincreased by decreasing the activity of silica in slag. This is achieved by increasing thebasic oxides, such as CaO, in the slag. The boron content in the steel is improved byincreasing the slag basicity. Di-Calcium silicate (C2S-2CaO.SiO2) phase present inbasic slags, exhibits polymorphism during cooling leading to volume expansion andcrumbling of LF slags. These crumbled slags are very difficult to handle, store, andrecycle. In addition, they create environmental pollution and fine dust is a health hazardto people working on the shop floor.
[85] Most of the methods used by Steel industries for recycling LF slag include one or morecomplex steps, such as briquetting, adding alumina or silica-based slag stabilizers.Many researchers have tried adding B2O3 to stabilize secondary steelmaking slags.B2O3 on the other hand is an acidic oxide that exists in the form of BO33- (planartriangular structure) and BO45- (tetrahedral structure). Complex structures are formedin slag with B2O3 addition, which will affect properties such as melting point, viscosity,thermal conductivity, electrical conductivity, surface tension etc. Crumbling of LFslags is minimized by preventing C2S formation or phase transformation of C2S duringcooling. The monoclinic polymorph to the orthorhombic -polymorph is accompaniedby a volume expansion of about 12%, high internal stresses finally cause thedisintegration of the slag. It was found that B2O3 influences slag mineralogy bystabilizing C2S and preventing slag crumbling. Even 0.5 wt% B2O3 is sufficient tostabilize LF slag. The addition of such small quantities will not increase the steelproduction cost compared to other additives.
[86] Steel making: Figure 19 represents the generalised process flow for steel making.Once the steel is processed from BOF (Basic Oxygen Furnace) or EAF (Electric ArcFurnace) route, the steel is tapped into Ladle for further refining. At this stage ferroalloy and fluxes are added depending on grade requirement. The requirement ofsynthetic slags is prominent in high carbon Si killed steels due to viscous slagformation. Addition of CaO-Al2O3-B2O3 synthetic slag reduces slag crust formationand improves overall process efficiency in Ladle Furnace refining.
[87] Once the steel is tapped, it is sent to online rinsing station for homogenisation of steel.Argon is purged from bottom of the ladle to mix the steel. The ladle is then transferredto Ladle Furnace unit where further composition adjustment is done. Some Al anddeoxidizers are added to reduce the oxygen content in steel. This maximises recoveryof ferro alloys. At this stage, CaO-Al2O3-B2O3 synthetic slag is added for boron microalloying. Around 40% of boron is recovered into steel and 60% remains in slag. Boronis recovered into steel by reduction of B2O3 with Si and Al present in steel.Example 3 : Application in steelmaking
[88] Typically, steel making is performed in the following manner:A. BOF steel making:Step ParametersChargingThe furnace is tilted to load scrap 10-30% of charge)followed by molten pig iron (70-80%). Pig iron enters atroughly 1,200-1,400°C.Ignition andBlowingThe vessel is set upright. A water-cooled lance is loweredto 1.8-3.0 meters above the bath. Pure oxygen (99%) isblown at supersonic speeds (Mach 2.0-2.1).Flux Addition Lime (CaO) and Dolomite (MgO) are added early to forma basic slag (Basicity>2.8). This protects the furnace liningand absorbs impurities like phosphorus.RefiningStagesEarly Blow: Silicon and Manganese oxidize first.Temperature rises as removal completes within minutes.Main Blow: Intense decarburization occurs. Carbon dropsfrom ~4.2% to <0.5%SamplingAt the end of the blow, the furnace is tilted for temperaturemeasurement and chemical sampling. The target steeltemperature is usually 1,600-1,700°C.TappingRefined steel is poured into a ladle through a tap hole whileretaining the slag using slag arresters. Deoxidizers (Al, Si)and alloys are added to "kill" the steel and adjust grade.Fluxes such as lime and synthetic slags are added to formdesirable slag. Addition of premelted CaO-Al2O3-B2O3synthetic slag.DeslaggingThe furnace is rotated in the opposite direction to dump theremaining liquid slag.B. Rinsing online with Argon: The ladle is transferred to online rinsing stationwhere Argon gas is used for rinsing steel for homogenising a composition. Theprocess parameters are as below:Step ParametersTotal Argon Flow (Heating) 240-400 L / minTotal Argon Flow (Rinsing) 60-120 L / minAr Pressure at Header 10-15 barTreatment Time 10-30 minutesTarget Temperature 1,570-1,630°C (depending on grade)C. Ladle Furnace (LF) Refining: The typical treatment cycle for a 150-ton heatlasts 35 to 55 minutes.- Heating (Arc Heating): Three graphite electrodes are lowered into theladle. Submerged arc heating is used to raise the temperature to the targetcasting level.- Slag Formation: Synthetic slag agents and fluxes such as lime are addedto create a basic white slag that absorbs sulfur and non-metallicinclusions.- Stirring and Homogenisation: Argon is injected through bottom porousplugs. This ensures uniform temperature and chemistry throughout the150-ton melt.- Alloying and Deoxidation: Ferroalloys (FeMn, SiMn, FeSi, FeCr) anddeoxidisers (Al, Si-Ca wire) are added to meet precise gradespecifications.- Addition of premelted CaO-Al2O3-B2O3 synthetic slag before or afterLF treatment as per requirement.- Soft Rinsing: A final, gentle argon blow (5-10 minutes) promotes theflotation of remaining inclusions to the slag layer.- Parameters are listed in table below:Power Rating 18-30 MW (Transformer capacity~25-35 MVA)Heating Rate3.0-5.0°C per minuteElectrode Consumption0.15-0.40 kg per ton of steelPower Consumption25-45 kWh per ton of steelArgon Flow (Strong)150-400 NL / min (foralloying / deoxidation)Argon Flow (Soft)20-60 NL / min (for inclusion removal)Slag Basicity (CaO / SiO2)>2.5 (up to 4-6 for deepdesulfurisation)Target Temperature1,580-1,650°C (depending on theContinuous Caster requirements)D. Continuous casting into blooms / rounds / billets: To cast a 150-ton heat, multistrand machines are used to ensure the entire ladle is emptied within 45-70minutes before the steel becomes too cold to flow. For 150 tons, a 4 to 6-strandmachine is standard.1. Tundish and Flow Control Parameters- The tundish acts as a buffer between the 150-ton ladle and the castingstrands.- Tundish Capacity: Typically 25-40 tons for a 150-ton heat to allow forladle changeovers without stopping the cast.- Superheat: Maintained at 25-40°C above the liquidus temperature.- Flow Control: Stopper rods or sliding gates are used to regulate the flowinto individual strands.2. Casting Speed and Throughput- The casting speed is determined by the cross-section size to matchthe 150-ton mass flow.Product Type Size Speed (m / min) Strand needsBillets 130x130 to160x1602.5-4 5 to 6Blooms 250x250 to350x4000.6-1.2 3 to 4Rounds 200 to 400diameter0.8-1.5 43. Primary & Secondary Cooling Parameters- Mold Cooling Water: For a 150-ton operation, flow is usually 1,800-2,200 L / min per strand to ensure a thick enough shell to prevent"breakouts".- Specific Water Consumption: Usually 0.6-1.2 Liters per kg of steel.- Oscillation Stroke: 5-10 mm with a frequency linked to castingspeed.4. Cutting and Handling- Billet / Bloom Length: Standard lengths are 6, 9, or 12 meters.- Cutting Method: Torch cutting (Oxy-Propane) is preferred for 150-ton bloom casts due to the thickness, while high-speed shears areused for billets.E. Slag dumping: After finish of casting the slag left over in the ladle is dumpedinto slag pots, the slag pots are then emptied by dumping slag in slag yards andleft for air cooling.- Slag Temperature: At the end of casting, the slag is typically between1,380°C and 1,450°C.- Residual Slag Volume: For a 150-ton heat, the slag volume usuallyranges from 3 to 7 tons, depending on the refining intensity and syntheticflux additions.- Slag Pot Capacity: Typically uses pots with a volume of 8 to 16.5 m3 toaccommodate the slag and any metallic skull.- Cycle Time: The complete operation-from tilting the ladle to dumpingthe pot at the yard-typically takes about 4 hours- The slag obtained after treatment with premelted CaO-Al2O3-B2O3synthetic slag is in stabilized form and can be crushed, stored, andrecycled easily.
[89] Ladle Furnace refining is a reducing process where steel desulphurisation is carried out.Desulphurisation is a kinetic phenomenon that depends on slag composition, viscosity,and melting temperature. To increase the temperature, arcing is done using graphiteelectrodes, and stirring is achieved by means of Argon bottom purging. The presenceof B2O3 in slag acts as a fluxing agent and improves arcing efficiency and steeldesulphurisation.
[90] Addition of CaO-Al2O3-B2O3 synthetic slag is carried out at different stages of refiningas depicted in Figure 20, which are as follows:- During Tapping steel from BOF to Ladle- At Online Rinsing Station- At LF entry before slag Killing- At LF after slag killing, followed by arcing and mild purging- At LF exit after final composition adjustment and mild purging
[91] (The average composition of Si killed LF slags is CaO 45-50 wt%, MgO 6-15 wt%,SiO2 10-25 wt%, Al2O3 5-15 wt%. Si killed steels are treated with Calcium aluminatesynthetic slags, to improve slag fluidity. The consumption of Calcium aluminatesynthetic slag ranges around 5-10 kg per ton of liquid steel. Addition of the developedCaO-Al2O3-B2O3 synthetic slag reduces the consumption to 3-5 kg per ton of liquidsteel due to enhanced slag fluxing effect. This will eventually reduce the steelproduction coat. The developed CaO-Al2O3-B2O3 synthetic slag is added incombination with lime to improve steel desulphurisation efficiency. Boron recoverydepends on slag basicity, deoxidation and treatment temperature. On an average 20-30% boron is recovered into steel and 70% remains in slag. LF slag which is dumpedafter casting does not cause dusting and a stabilized slag is obtained which is crushedand recycled. B2O3 also forms low melting inclusions in Si-Mn killed steels whennitrogen is <50 ppm.
[92] The developed slag is added in combination with other fluxes such as CaO and CaOAl2O3 synthetic slags in steelmaking. The slag is added in the ladle furnace afterdeoxidation for boron micro alloying and slag stabilization, where 20-30% boron isrecovered to steel and 70% remains in LF slag. For boron micro alloying, the steelshould have Si in range of 0.1-4 wt%, Al in the range of 0.1-2 wt% and basicity of LFslag (CaO / SiO2) in range of 1-5. Thereafter, the slag is added after complete treatmentof LF for slag stabilization, wherein size of the slag is approximately 20-50 mm forbetter dissolution.
[93] Further, the slag is added during tapping steel into the ladle for the fluxing effect andslag stabilization. The slag is also added during tapping steel to ladle and at LF afterdeoxidation for achieving the effect of slag fluxing, boron micro alloying and slagstabilization. The LF slag obtained after treatment with the developed synthetic slag isin stabilized form and can be used as a source of raw material for preparing the flux.
[94] The average composition of Al killed LF slag is CaO 50-60 wt%, MgO-5-10 wt%, SiO25-15 wt%, Al2O3 10-30 wt%. Al killed LF slags are more fluid compared to Si killedslags due to presence of high alumina which acts as slag fluidizer. Addition ofdeveloped CaO-Al2O3-B2O3 synthetic slag of 2-3 kg / ton of liquid steel leads to boronmicro alloying and stabilizes LF slag. The composition of Al killed LF slag iscomparable to Calcium Aluminate synthetic slag. The B2O3 stabilized slag is used as araw material to develop CaO-Al2O3-B2O3 synthetic slag.
[95] The stabilized LF slags obtained after treating with developed CaO-Al2O3-B2O3synthetic slag have improved valorisation potential as the slag is easily transported. Itis recycled in Sinter making as a flux, in BOF steel making as an early slag former, inBlast furnace as a flux.
[96] Depending on the grade requirement, the developed sustainable multifunctional CaOAl2O3-B2O3 synthetic slag has various functions as shown in Figures 21, 22 and 23.The synthetic slag acts as:1. Slag stabilizer2. Boron micro alloying agent3. Inclusion modifier4. Slag fluxing agentADVANTAGES OF THE PRESENT INVENTION:
[97] The present invention provides a method for preparing a sustainable multifunctionalsynthetic slag and the multifunctional synthetic slag thereof. The present inventionprovides the following advantages:I. A low melting CaO-Al2O3-B2O3 pre-melted synthetic slag is developed. Theslag has CaO is 35-50wt%, Al2O3 is 30-45 wt%, B2O3 is 2-6 wt%, MgO is 4-10wt%, SiO2 is 2-5wt%.II. The viscosity of the CaO-Al2O3-B2O3 pre-melted synthetic slag is in the rangeof 0.17-0.25 Pa.s at 1500°C due to formation of 3D-BO33- units.III. The melting temperature and viscosity of CaO-Al2O3-B2O3 pre-melted syntheticslag are 30% lower than conventional calcium aluminate synthetic slags.IV. Sustainable multifunctional CaO-Al2O3-B2O3 synthetic slag has variousfunctions. The synthetic slag acts as:- Slag stabilizer- Boron micro alloying agent- Inclusion modifier- Slag fluxing agentV. The CaO-Al2O3-B2O3 synthetic slag is used to treat Si and Al killed steels.VI. The CaO-Al2O3-B2O3 synthetic slag acts as boron micro alloying agent ingrades which have Si and Al as alloying elements.VII. The CaO-Al2O3-B2O3 synthetic slag forms deformable low melting inclusionswhen nitrogen in steel is <50 ppm.VIII. Addition of CaO-Al2O3-B2O3 synthetic slag is carried out at different stages ofrefining depending on the requirement, which are as follows:- During Tapping steel from BOF to Ladle- At Online Rinsing Station- At LF entry before slag Killing- At LF after slag killing, followed by arcing and mild purging- At LF exit after final composition adjustment and mild purgingIX. Addition of CaO-Al2O3-B2O3 synthetic slag improves the valorisation potentialof LF slags.X. Addition of CaO-Al2O3-B2O3 synthetic slag reduces power consumption duringarcing in LF due to formation of fluid slag.XI. Addition of CaO-Al2O3-B2O3 synthetic slag prevents sticking of LF slag to ladlecover during steel refining.XII. Addition of CaO-Al2O3-B2O3 synthetic slag reduces steel production cost andoverall process efficiency compared to conventional synthetic slags.XIII. Addition of CaO-Al2O3-B2O3 synthetic slag improves steel desulphurisationefficiency due to formation of liquid slag.XIV. CaO-Al2O3-B2O3 synthetic slag is added in combination with lime and otherfluxes for steel refining.XV. Addition of CaO-Al2O3-B2O3 synthetic slag reduces the consumption of FeBused for boron micro alloying.
Claims
1. A method for preparing a sustainable multifunctional synthetic slag, comprising: i. mixing at least one source of calcium oxide (CaO), aluminium oxide (Al2O3) and boron oxide (B2O3) to form a mixture; ii. grinding the mixture obtained in step (i) to form a homogenous slag mixture; and iii. feeding the slag mixture obtained in step (ii) into graphite crucibles and melting the same to form a multifunctional synthetic slag.
2. The method as claimed in claim 1, wherein CaO is present in a range of 35-50wt%.
3. The method as claimed in claim 1, wherein Al2O3 is present in a range of 30-45wt%.
4. The method as claimed in claim 1, wherein B2O3 is present in a range of 2-8wt%.
5. The method as claimed in claim 1, wherein the melting is performed at a temperature of 1500°C.
6. The method as claimed in claim 1, wherein the slag having a chemical composition comprising 35-50wt% of CaO, 30-45 wt% of Al2O3, 2-8 wt% of B2O3, 4-10 wt% of MgO, 2-5wt% of SiO2.
7. A multifunctional synthetic slag for steel refining, comprising: a) CaO; b) Al2O3; c) B2O3; and d) MgO.
8. The slag as claimed in claim 7, wherein the source of CaO is selected from Limestone, Calcined lime, Recycled LF slag and Calcium Aluminate synthetic slag.
9. The slag as claimed in claim 7, wherein the source of Al2O3 is selected from Calcium Aluminate synthetic slag, Calcined Bauxite and Recycled LF slag.
10. The slag as claimed in claim 7, wherein the source of B2O3 is selected from a group consisting of Boron Oxide (B2O3), Boric acid (H3BO3), Borax (Na2O.2B2O3.10H2O), Kernite (Na2O.2B2O3.5H2O), Colemanite (2CaO.3B2O3.5H2O), Ulexite (Na2O. 2CaO.5B2O3.16H2O), Datolite (2CaO.B2O3.2SiO2.H2O), Danburite (CaO.B2O3.2SiO2), Ludwigite (Mg2Fe3+BO5) and Suanite (Mg2B2O5(OH)2.
11. The slag as claimed in claim 7, wherein the source of MgO is selected from a group consisting of dolomite and calcined dolomite.
12. The slag as claimed in claim 7, wherein the slag comprises 35-50wt% of CaO, 30-45 wt% of Al2O3, 4-10 wt% MgO and 2-6 wt% of B2O3.
13. The slag as claimed in claim 7, wherein CaO and Al2O3 are present in a ratio ranging from 1.1-1.16.
14. The slag as claimed in claim 7, wherein the slag exhibits a melting temperature in a range of 1200-1300°C.
15. The slag as claimed in claim 7, wherein the slag having a viscosity in the range of 0.17- 0.25 Pa.s at 1500°C due to the formation of 2D-BO33-units and low-melting compounds.
16. The slag as claimed in claim 7 is used for silicon (Si) and aluminium (Al) killed steel refining, steel making, slag fluxing, boron micro alloying, slag stabilisation and inclusion modification.