Biodegradable coatings based on aqueous PHA dispersions

JP2021535238A5Active Publication Date: 2024-10-08MEREDIAN INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021507584
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-08-13
Filing Date
2019-08-12
Publication Date
2024-10-08
Estimated Expiration
2039-08-12
Patent Text Reader

Abstract

A biodegradable aqueous dispersion is disclosed, which is comprised of about 35 to about 75% by weight of water and about 25 to about 65% by weight of a polyhydroxyalkanoate. A biodegradable food service product is also disclosed, which includes a biodegradable substrate having at least one food contact surface. A coating formed from the biodegradable aqueous dispersion is applied to the at least one food contact surface.
Need to check novelty before this filing date? Find Prior Art

Description

[Technology Field]

[0001] field This disclosure relates to biodegradable polymer compositions. More specifically, this disclosure relates to biodegradable coatings for food service items made from aqueous dispersions of polyhydroxyalkanoates ("PHAs"). [Background technology]

[0002] background Consumers frequently use disposable catering supplies such as plates, bowls, cups, and utensils for convenience. Disposable catering supplies are particularly convenient for serving food at large gatherings and outdoor dining events.

[0003] Disposable food service supplies can sometimes be easily reprocessed from base materials such as cardboard, which decompose relatively quickly after landfill disposal. However, simple, uncoated cardboard base materials readily absorb water and / or oil, which compromises the strength of the cardboard. Consequently, food service supplies made from cardboard are typically coated with a thin polymer layer to improve water and oil resistance.

[0004] Coatings made from polymers such as polyethylene (PE), polypropylene (PP), or polyethylene terephthalate (PET) can significantly improve the resistance of cardboard to water and / or oil absorption; however, such polymers do not readily degrade or decompose after landfill disposal. Thus, cardboard coated with such polymers may remain in landfills for centuries after disposal.

[0005] Thus, it is desirable to provide a novel coating for school lunch supplies that is completely biodegradable. Furthermore, it is desirable that this biodegradable coating provides excellent water and oil resistance—that is, water and oil resistance comparable to that provided by conventional non-biodegradable coatings. [Overview of the project]

[0006] The above and other requirements are met by a biodegradable aqueous dispersion for coating food-contact substrates. According to one embodiment, this dispersion consists of about 35 to about 75% by weight of water and about 25 to about 65% by weight of polyhydroxyalkanoate.

[0007] In one embodiment, the dispersion preferably comprises about 25 to about 65% by weight of poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)"). Furthermore, in one embodiment, this P(3HB-co-3HHx) is then preferably comprised of about 75 to about 99 mole percent of hydroxybutyrate and about 1 to about 25 mole percent of hydroxyhexanoate. More preferably, P(3HB-co-3HHx) comprises about 85 to about 95 mole percent of hydroxybutyrate and about 5 to about 15 mole percent of hydroxyhexanoate.

[0008] In some embodiments, the dispersion preferably consists of about 1 to about 25% by weight of at least one polyhydroxyalkanoate, including hydroxyvalerate, hydroxyhexanoate, hydroxyoctanoate and / or hydroxydecanoate, in a range of about 25 to about 50 mole percent.

[0009] Furthermore, in some cases, polyhydroxyalkanoate polymers may be terpolymers composed of at least three types of hydroxyalkanoate monomer residues. These terpolymers may contain, for example, hydroxybutyrate in about 75 to about 99 mole percent, hydroxyvalerate in about 0.1 to about 15 mole percent, and a third hydroxyalkanoate such as hydroxyhexanoate in about 1 to about 25 mole percent.

[0010] In one embodiment, the polyhydroxyalkanoate in the dispersion preferably has a weight-average molecular weight ranging from about 50,000 daltons to about 2,500,000 daltons. More preferably, the weight-average molecular weight is ranging from about 150,000 daltons to about 600,000 daltons, and even more preferably from about 150,000 daltons to about 500,000 daltons.

[0011] In one embodiment, the dispersion is preferably composed of particles having an average particle size of about 10 nm to about 50 μm. Furthermore, in some embodiments, the dispersion preferably has an average solid content of about 25 percent to about 65 percent solid. More preferably, the average solid content is about 40 percent to about 55 percent solid, and even more preferably about 40 percent to about 50 percent solid.

[0012] In addition to water and PHA, the dispersion may optionally contain further components. For example, in one embodiment, the dispersion preferably contains at least one surfactant selected from the group consisting of polysorbates, aromatic polyethylene oxides, sorbitan derivatives, block copolymers of poly(ethylene oxide) and poly(propylene oxide), poly(glycol ethers), poly(vinyl alcohol), alkyl sulfates, alkyl phosphates, stearates, and mixtures thereof, in an amount of about 0.01% to about 5.0% by weight. More preferably, the dispersion contains at least one surfactant in an amount of about 0.5% to about 5.0% by weight, and even more preferably, at least one surfactant in an amount of about 0.5% to about 2.0% by weight.

[0013] In some cases, the at least one surfactant preferably has a hydrophilic-lipophilic balance greater than 10. More preferably, the at least one surfactant preferably has a hydrophilic-lipophilic balance of about 12 to about 15.

[0014] In some embodiments, the dispersion preferably also contains at least one rheological modifier selected from the group consisting of polysaccharides, acrylate-based emulsion copolymers, viscosity depressants, and thickeners, in an amount from about 0.01% to about 5.0% by weight.

[0015] In some cases, the dispersion also preferably includes at least one wetting and dispersing agent in an amount ranging from about 0.01% to about 2.5% by weight.

[0016] In one embodiment, the dispersion preferably also contains at least one biocide or inhibitor in an amount from about 0.01% to about 0.5% by weight.

[0017] In one embodiment, the dispersion preferably also includes a flocculant selected from the group consisting of a bio-succinic acid-based flocculant in an amount of about 0.1% to about 5.0% by weight, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, dimethyl carbonate, methanol, ethanol, ketones, acetates and / or mixtures thereof.

[0018] In some embodiments, the dispersion preferably also includes at least one filler selected from the group consisting of clay, calcium carbonate, talc, kaolinite, montmorillonite, bentonite, silica, chitin, titanium dioxide, nanoclay, mica, or mixtures thereof, in an amount of about 1% to about 35% by weight.

[0019] In one embodiment, the dispersion preferably also contains about 0.5% to about 15% by weight of at least one plasticizer selected from the group consisting of sebacate, citrate, fatty esters of adipic acid, succinic acid and glucaric acid, lactate, alkyl diester, citrate, alkyl methyl ester, dibenzoate, propylene carbonate, caprolactone diol having a number average molecular weight of 200-10,000 g / mol, poly(ethylene) glycol having a number average molecular weight of 400-10,000 g / mol, vegetable oil ester, long-chain alkyl acid, adipate, glycerol, isosorbide derivative, or mixtures thereof.

[0020] In other embodiments, the dispersion preferably also contains about 0.1% to about 5% by weight of at least one nucleating agent selected from the group consisting of sulfur, erythritol, pentaerythritol, dipentaerythritol, artificial sweeteners, stearate, sorbitol, mannitol, polyester wax, compounds having 2:1;2:1 crystal structure chemicals, and mixtures thereof.

[0021] In some embodiments, the dispersion preferably also contains, in an amount of about 0.01% to about 5% by weight, calendula oil, and at least one crosslinking agent selected from the group consisting of stabilized ammonium zirconium carbonate, anionic hydroxylated zirconium polymer, potassium zirconium carbonate, anionic hydroxylated zirconium polymer, zinc tetraamine carbonate, and mixtures thereof.

[0022] In some embodiments, the dispersion also preferably includes at least one antifoaming agent selected from the group consisting of polyethersiloxanes, polyamide particles, and mixtures thereof, in an amount of about 0.05 to about 1% by weight.

[0023] In one preferred embodiment, in addition to water and PHA, the dispersion comprises: (1) at least one surfactant from about 0.01 wt% to about 5.0 wt%; (2) at least one rheology modifier from about 0.01 wt% to about 5.0 wt%; (3) at least one wetting and dispersing agent from about 0.01 wt% to about 2.5 wt%; and (4) may also include at least one biocide or biostatic agent from about 0.01 wt% to about 0.5 wt%.

[0024] In a second aspect, the present disclosure provides biodegradable food service articles. According to one embodiment, the biodegradable food service article includes a biodegradable substrate having at least one food contact surface. The food service article also includes a coating applied over the at least one food contact surface. The coating is applied as a biodegradable aqueous dispersion, which consists of about 35 to about 75 wt% water and about 25 to about 65 wt% polyhydroxyalkanoate.

[0025] In certain embodiments, the biodegradable substrate is preferably a biodegradable plate, cup, bowl, fiber tray or tableware.

[0026] In some embodiments, the coating is preferably applied at a coating weight of from about 2 to about 25 grams per square meter and more preferably from about 4 to about 25 grams per square meter on a dry basis over at least one food contact surface.

[0027] In one embodiment, the coating preferably has a Cobb water absorption value of less than 20 grams per square meter measured according to TAPPI Standard T441 (Cobb It shows a water absorption value (Cobb water absorption value). More preferably, the Cobb water absorption value is less than 10 grams per square meter. Further, in certain embodiments, the coating preferably exhibits a Kit Test grease resistance value greater than Kit Value 5 measured according to TAPPI Standard T559cm-12. More preferably, the Kit Value is from about 8 to about 12.

[0028] Detailed description biodegradable aqueous dispersion In accordance with the present disclosure, there is provided a biodegradable aqueous dispersion for coating food contact substrates and other substrates. The dispersion comprises at least water and a polyhydroxyalkanoate and may also include other components as will be discussed in more detail below.

[0029] As used herein, the term "biodegradable" refers to a plastic or polymeric material coating that undergoes biodegradation by organisms (microorganisms) in anaerobic and aerobic environments (determined by ASTM D5511), in soil environments (determined by ASTM 5988), in freshwater environments (determined by ASTM D5271 (EN 29408)), or in marine environments (determined by ASTM D6691). The biodegradability of biodegradable plastics can also be determined using ASTM D6868 and European EN 13432.

[0030] The aqueous dispersion of the present disclosure is preferably also "compostable" as determined by ASTM D6400 regarding industrial or home compostability.

[0031] Water is the solvent for the dispersion and will typically constitute from about 35 wt% to about 75 wt% of the dispersion. More preferably, water constitutes from about 40 wt% to about 60 wt% of the dispersion.

[0032] The dispersion also contains polyhydroxyalkanoates ("PHAs"). Polyhydroxyalkanoates will typically constitute about 25 to about 65% by weight of the dispersion. More preferably, polyhydroxyalkanoates will constitute about 40 to about 55% by weight of the dispersion.

[0033] A preferred polyhydroxyalkanoate for use in dispersions is poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)"). In some embodiments, P3HB-co-P3HHx is the primary polyhydroxyalkanoate in the dispersion. In some cases, P(3HB-co-3HHx) may be substantially the only polyhydroxyalkanoate used in the dispersion. Thus, in some embodiments of this disclosure, the dispersion may preferably consist of about 25 to about 65% by weight of P(3HB-co-3HHx).

[0034] The aforementioned P(3HB-co-3HHx) is a copolymer composed of both hydroxybutyrate and hydroxyhexanoate, and the relative amounts of the two may vary somewhat. However, generally, P(3HB-co-3HHx) is preferably composed of about 75 to about 99 mole percent of hydroxybutyrate and about 1 to about 25 mole percent of hydroxyhexanoate. More preferably, P(3HB-co-3HHx) is composed of about 85 to about 95 mole percent of hydroxybutyrate and about 5 to about 15 mole percent of hydroxyhexanoate.

[0035] In some embodiments, the dispersion is preferably about 25 to about 50 mole percent It consists of about 1 to about 25% by weight of at least one polyhydroxyalkanoate, including hydroxyvalerate, hydroxyhexanoate, hydroxyoctanoate and / or hydroxydecanoate.

[0036] The molecular weight range of the polyhydroxyalkanoates used in the dispersion may also vary somewhat. Typically, the weight-average molecular weight of the polyhydroxyalkanoates in the dispersion ranges from about 50,000 daltons to about 2,500,000 daltons. More preferably, the weight-average molecular weight of the polyhydroxyalkanoates ranges from about 150,000 daltons to about 600,000 daltons, and even more preferably from about 150,000 daltons to about 500,000 daltons.

[0037] In one embodiment, the dispersion is preferably composed of particles having an average particle size of about 10 nm to about 50 μm. Furthermore, in some embodiments, the dispersion preferably has an average solid content of about 25 percent to about 65 percent solid. More preferably, the average solid content is about 40 percent to about 55 percent solid, and even more preferably about 40 percent to about 50 percent solid.

[0038] In addition to water and PHA, the dispersion may optionally contain further components. For example, the dispersion may also contain surfactants, rheological modifiers, wetting and dispersing agents, biocides or inhibitors, flocculants, fillers, plasticizers, nucleating agents and / or crosslinking agents.

[0039] As used herein, "surfactants" are added to a dispersion to stabilize a polymer in an aqueous medium. Surfactants typically consist of both hydrophobic and hydrophilic regions. In a dispersion, these distinct regions orient themselves at the interface between the polymer particles and the aqueous medium, lowering the surface energy between the two phase boundaries and promoting dispersion.

[0040] As used herein, "rheological modifier" is a substance that alters the fluidity of a dispersion (i.e., dilutes or concentrates the dispersion).

[0041] As used herein, “wetting and dispersing agents” are surfactants of a type that contribute to polymer stabilization and dispersion homogeneity. These materials typically contain bulky groups, which separate and maintain suspended particles through steric hindrance, thereby helping to prevent particle aggregation and sedimentation. Wetting and dispersing agents also ensure that particles are completely wetted by the aqueous medium, promoting complete and homogeneous dispersion.

[0042] As used herein, "biocide" refers to a material that kills organisms and thus protects a material from microbial growth and adhesion. "Antimicrobial" refers to a material that prevents the growth of microorganisms such as bacteria or fungi / molds, but does not kill them.

[0043] As used herein, “coagulant” is a material, usually an organic solvent, that temporarily plasticizes a material in a dispersion, thereby aiding in faster drying times. Coagulants typically have a higher boiling point than water, and therefore, upon drying, the water evaporates first, leaving the coagulant behind, which continues to plasticize the polymer as the drying process continues until the coagulant evaporates.

[0044] As used herein, “fillers” such as clay, silica, and other inorganic materials impart numerous functions to the dispersion. Firstly, these materials improve the solid content of the dispersion. Secondly, fillers may alter the brightness and gloss of the resulting film. Finally, fillers may also act as thickeners.

[0045] As used herein, "plasticizer" is a material that works to disrupt the interactions between polymer chains, allowing the polymer chains to become more flexible. The introduction of a plasticizer lowers the glass transition temperature (T) of the polymer. g ) significantly reduces.

[0046] As used herein, "nucleating agent" is a material that acts to promote the crystallization of a polymer in a dispersion after drying. The nucleating agent provides sites where crystals can form, thereby shortening the crystallization time for the film. The faster the crystallization, the shorter the waiting time before the coating is ready for use.

[0047] As used herein, “crosslinking agent” is a material that forms strong chemical bonds between the polymer coating and the substrate, as well as within the polymer coating itself. Crosslinking forms a stronger and harder film coating, which will be more resistant to abrasion and wear.

[0048] As used herein, “defoaming agent” is a material that reduces or removes foam in a dispersion. Often, foam in a dispersion results in a film with imperfections or defects that affect the barrier properties of the coating during application.

[0049] For example, in one embodiment, the dispersion preferably contains at least one surfactant selected from the group consisting of polysorbates (such as TWEEN), aromatic polyethylene oxides (such as TRITON), sorbitan derivatives (such as SPAN), block copolymers of poly(ethylene oxide) and poly(propylene oxide) (such as PLURONIC), poly(glycol ethers) (such as TERGITOL), poly(vinyl alcohol), alkyl sulfates, alkyl phosphates, stearates, and mixtures thereof, in an amount of about 0.01% to about 5.0% by weight. More preferably, the dispersion contains at least one surfactant in an amount of about 0.5% to about 2.0% by weight.

[0050] In some cases, the at least one surfactant preferably has a hydrophilic-lipophilic balance greater than 10. More preferably, the at least one surfactant preferably has a hydrophilic-lipophilic balance of about 12 to about 15.

[0051] In some embodiments, the dispersion may also preferably contain at least one rheological modifier selected from the group consisting of polysaccharides (such as starch, xanthan gum, guar gum, cellulose fiber, and seaweed extracts), acrylate-based emulsion copolymers, viscosity depressants (such as VISCOBYK 5120 or a blend containing carboxylic acid esters and wetting and dispersing components), and thickeners (solutions of modified polyurethanes containing derivatives of ethyl acrylate and methacrylic acid copolymers, such as the BYK 400 family or ALCOGUM), in an amount of about 0.01% to about 5.0% by weight.

[0052] In some cases, the dispersion may preferably contain at least one wetting and dispersing agent (such as BYK 190, BYK 184, TEGO 755, or TEGO 761, but not limited to those that appear to be nonionic or slightly anionic copolymers) in an amount from about 0.01% to about 2.5% by weight.

[0053] In one embodiment, the dispersion may also contain at least one biocide or microbial agent (such as ethylenediaminetetraacetic acid (EDTA) or benzisothiazolinone) in an amount ranging from about 0.01% to about 0.5% by weight.

[0054] Furthermore, the dispersion contains approximately 0.1% to 5.0% by weight of a bio-succinic acid-based coagulation solvent (such as MYRIFILM), 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (such as Eastman TEXANOL), and benzoate. The formulation may also include at least one flocculant selected from the group consisting of esters or alkyl benzoate esters (such as Eastman BENZOFLEX or VELATE), dimethyl carbonate, methanol, ethanol, ketones, acetates, and / or mixtures thereof.

[0055] In some embodiments, the dispersion may preferably contain at least one filler selected from the group consisting of clay, calcium carbonate, talc, kaolinite, montmorillonite, bentonite, silica, chitin, titanium dioxide, nanoclay, or mixtures thereof, in an amount of about 1% to about 35% by weight.

[0056] In one embodiment, the dispersion may also contain, in an amount of about 0.5% to about 15% by weight, at least one plasticizer selected from the group consisting of sebacate, citrate, fatty esters of adipic acid, succinic acid and glucaric acid, lactate, alkyl diester, citrate, alkyl methyl ester, dibenzoate, propylene carbonate, caprolactone diol having a number average molecular weight of 200-10,000 g / mol, polyethylene glycol having a number average molecular weight of 400-10,000 g / mol, vegetable oil ester, long-chain alkyl acid, adipate, glycerol, isosorbide derivatives, or mixtures thereof.

[0057] In other embodiments, the dispersion preferably also contains about 0.1% to about 5% by weight of at least one nucleating agent selected from the group consisting of sulfur, erythritol, pentaerythritol, dipentaerythritol, artificial sweeteners, stearate, sorbitol, mannitol, polyester wax, compounds having a 2:1;2:1 crystalline structure, and mixtures thereof.

[0058] In some embodiments, the dispersion preferably also contains, in an amount of about 0.01% to about 5% by weight, calendula oil, stabilized ammonium zirconium carbonate, anionic hydroxylated zirconium polymer (such as BACOTE), potassium zirconium carbonate, anionic hydroxylated zirconium polymer (such as ZIRMEL and ZIRMEL XL), zinc tetraamine carbonate (such as ZINPLEX), and mixtures thereof, at least one crosslinking agent selected from the group.

[0059] In other embodiments, the dispersion contains at least one silicone and / or mineral oil-free defoamer selected from the group consisting of polyethersiloxanes (such as AIRASE 5355 or 5655 or TEGO FOAMEX 825, 902 or 1488), polyamide particles (such as BYK 1640 or BYK 016), and mixtures thereof, in an amount of about 0.05 to about 1% by weight.

[0060] In one preferred embodiment, the dispersion may also contain, in addition to water and PHA: (1) at least one surfactant in an amount from about 0.01% by weight to about 5.0% by weight; (2) at least one rheological modifier in an amount from about 0.01% by weight to about 5.0% by weight; (3) at least one wetting and dispersing agent in an amount from about 0.01% by weight to about 2.5% by weight; and (4) at least one biocide or inhibitor in an amount from about 0.05% by weight to about 0.25% by weight.

[0061] Preparation of dispersion The dispersions of this disclosure may be prepared using various conventional mixing methods, such as high or low shear mixers and / or ultrasonic mixers. In a preferred embodiment, the PHA is powdered and then dispersed in water using a low to high shear mixer in the presence of a surfactant and / or wetting and dispersing agent to form initial micelles of PHA. The dispersion of the PHA particles is then preferably finished using an ultrasonic mixer / homogenizer to prepare a homogeneous emulsion / dispersion. In some cases, an ultrasonic mixer / homogenizer or In some cases, the dispersion can be prepared using only a high-shear mixer. Once the PHA is uniformly dispersed, a wetting and dispersing agent, biocide or inhibitor, and / or rheological additive may then be added and shear-mixed to complete the dispersion. After the final mixing, the viscosity of the dispersion is generally about 50 to about 2500 centipoise, more preferably about 50 to about 1000 centipoise, and most preferably about 100 to about 500 centipoise, when measured at a temperature of about 22°C.

[0062] Coated substrates for school lunch supplies Once prepared, the dispersion can be applied as a coating to a variety of substrate materials. The dispersion is particularly well-suited for use as a coating for substrates made from cardboard. Products made from wood pulp, such as paper and cardboard, are generally considered biodegradable unless coated with non-biodegradable materials. However, the application of the biodegradable dispersion of this disclosure to a substrate provides a coated substrate that remains biodegradable.

[0063] A biodegradable aqueous dispersion may be applied to one or more surfaces of cardboard or other substrates using conventional coating methods such as air knife, flexography, gravure, rod, and press coating. The dispersion is then dried on the substrate to give a final solid coating layer. The coating weight of the dispersion on the substrate may vary, but generally, the coating is applied to the surface of the substrate with a coating weight of about 2 to about 25 grams per square meter on a dry basis, and more preferably about 4 to about 25 grams per square meter.

[0064] The coated substrate may then be converted to give various final products manufactured from the coated cardboard or other substrates. In accordance with this disclosure, the coated substrate may be advantageously converted to give biodegradable feeding supplies. For example, the coated substrate may be converted to give food and drink utensils such as plates, cups, bowls, fiber trays or forks, spoons, sporks, knives, chopsticks, skewers, toothpicks, straws or beverage stirrers.

[0065] In such cases, the cardboard or other biodegradable substrate includes at least one food-contact surface, and the dispersion is applied as a coating layer on this food-contact surface. Optionally, other non-food-contact surfaces of the substrate may be similarly coated.

[0066] Thus, the provided food service supplies exhibit excellent resistance to water and oil absorption—generally comparable to cardboard coated with non-biodegradable polymers such as polyethylene (PE), polypropylene (PP), or polyethylene terephthalate (PET). At the same time, the coated cardboard substrate remains biodegradable.

[0067] In particular, resistance to water absorption may be measured using the Cobb water absorption test specified in TAPPI Standard T441. Coated substrates according to this disclosure typically exhibit a Cobb water absorption value of less than 20 grams per square meter. More preferably, the Cobb water absorption value is less than 10 grams per square meter.

[0068] Similarly, resistance to oil absorption may be measured using the Kit oil resistance test specified in TAPPI Standard T559cm-12. Coated substrates according to this disclosure typically exhibit a Kit Test oil resistance value greater than Kit Value 5. More preferably, the Kit Value is between approximately 8 and approximately 12. [Modes for carrying out the invention]

[0069] Examples Examples not limited to those described below illustrate various additional aspects of the present invention. Unless otherwise noted, temperatures are in degrees Celsius, and percentages are based on the dry weight of the preparation.

[0070] Examples 1-21: Preparation of aqueous dispersions [Examples]

[0071] In this example, an aqueous dispersion was prepared: 42.0 g of PHA (6.7 mol% hydroxyhexanoate; M) w(357,000 g / mol) was placed in 56 g of water with 1.5 g of Tween 20 and sheared at 1100 RPM for 90 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 3 minutes. 0.05 g of xanthan gum was then added to the resulting white dispersion and sheared further at 400 RPM for 30 minutes. Finally, 0.1% biocide was added to the dispersion. [Examples]

[0072] A dispersion was prepared as shown in Example 1. To this dispersion, 0.5 mL of dispersant (DISPERBYK 190) and 0.1 mL of rheological modifier (BYK 425) were added, and the mixture was sheared to ensure uniform mixing. [Examples]

[0073] A dispersion was prepared as shown in Example 2, then 3.5 g of clay (Imersys Talc) was added and sheared to obtain a homogeneous dispersion. [Examples]

[0074] In this example, 42.0 g of PHA (6.7 mol% hydroxyhexanoate; M) was used. w (357,000 g / mol) was placed in 56 g of water with 0.8 g of Tween 20 and sheared at 1100 RPM for 90 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 3 minutes. 0.05 g of xanthan gum was added to the resulting white dispersion and it was further sheared at 400 RPM for 30 minutes. Finally, 0.1% biocide was added to the dispersion. [Examples]

[0075] A dispersion was prepared as shown in Example 4. To this dispersion, 0.75 mL of dispersant (DISPERBYK 190) and 0.1 mL of rheological modifier (BYK 425) were added, and the mixture was sheared to ensure uniform mixing. [Examples]

[0076] A dispersion was prepared as shown in Example 5, then 10 g of kaolin clay was added and sheared to obtain a homogeneous dispersion. [Examples]

[0077] In this example, 35.0 g of PHA (6.0 mol% hydroxyhexanoate; M) was used. w (545,000 g / mol) was placed in 60 g of water with 2.0 g of Tween 20 and sheared at 1100 RPM for 90 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 7 minutes. 0.05 g of xanthan gum was added to the resulting white dispersion and it was further sheared at 400 RPM for 30 minutes. Finally, 0.1% biocide was added to the dispersion. [Examples]

[0078] A dispersion was prepared as shown in Example 7, and then 7.0 g of kaolin clay was added and sheared to obtain a homogeneous dispersion. [Examples]

[0079] In this example, 30.0 g of PHA (9.3 mol% hydroxyhexanoate; M) was used. w (1,458,000 g / mol) was placed in 65 g of water with 3.0 g of Tween 20 and 2.0 mL of Triton 100, and sheared at 900 RPM for 130 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 20 minutes. 0.05 g of xanthan gum was added to the resulting white dispersion, and it was further sheared at 400 RPM for 30 minutes. Finally, 0.1% biocide was added to the dispersion. [Examples]

[0080] The dispersion was prepared as shown in Example 9, then 0.75 mL of dispersant (DISPERBYK 184) was added, and the mixture was sheared to ensure uniform mixing. [Examples]

[0081] A dispersion was prepared as shown in Example 10, and then 5.0 g of PHA (28.3 mol% hydroxyhexanoate) was added and sheared to obtain a homogeneous dispersion. [Examples]

[0082] In this example, 45.0 g of PHA (6.7 mol% hydroxyhexanoate; M) was used. w(357,000 g / mol) was placed in 56 g of water with 0.8 g of Tween 20 and sheared at 1100 RPM for 60 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 5 minutes. 0.05 g of xanthan gum was then added to the resulting white dispersion and sheared further at 400 RPM for 30 minutes. Finally, 0.1% biocide was added to the dispersion. [Examples]

[0083] A dispersion was prepared as shown in Example 12, and then 0.75 mL of dispersant (DISPERBYK 190) and 0.1 mL of rheology modifier (BYK 425) were added, and the mixture was sheared to ensure uniform mixing. [Examples]

[0084] In this example, 45.0 g of PHA (6.7 mol% hydroxyhexanoate; M) was used. w (492,000 g / mol) was placed in 53 g of water with 1.5 g of Tego 755 and sheared at 10,000 RPM for 5 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 3 minutes. 0.25 g of Alcogum was added to the resulting white dispersion and sheared further at 7000 RPM for 5 minutes. Finally, 0.1% biocide was added to the dispersion. [Examples]

[0085] A dispersion was prepared as shown in Example 14. To this dispersion, 1 mL of dispersant (Tego 761) and 0.1 mL of rheology modifier (Alcogum) were added, and the mixture was sheared to ensure uniform mixing. [Examples]

[0086] A dispersion was prepared as shown in Example 15, then 10 g of kaolin clay was added and sheared to obtain a homogeneous dispersion. [Examples]

[0087] In this example, 30.0 g of PHA (9.3 mol% hydroxyhexanoate; M) was used. w: 3.0 g of Tween 20 and 2.0 mL of Triton 100 were added to 65 g of water together with 1,458,000 g / mol, and sheared at 900 RPM for 130 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 20 minutes. 0.05 g of xanthan gum was added to the resulting white dispersion, and further sheared at 400 RPM for 30 minutes. Finally, 0.1% biocide was added to the dispersion.

Example

[0088] A dispersion was prepared as shown in Example 17, then 0.75 mL of a dispersant (Tego 755) was added and sheared to ensure uniform mixing.

Example

[0089] A dispersion was prepared as shown in Example 18, then 5.0 g of PHA (28.3 mol% hydroxyhexanoate) was added and sheared to obtain a uniform dispersion.

Example

[0090] In this example, 55.0 g of PHA (6.7 mol% hydroxyhexanoate; M w : 357,000 g / mol) was added to 53 g of water together with 2.5 g of Tego 755 and sheared at 10,000 RPM for 10 minutes. After shearing, the mixture was subjected to ultrasonic mixing for 5 minutes. Then 0.1 g of xanthan gum and 0.25 g of Alcogum were added to the resulting white dispersion, and further sheared at 4000 RPM for 3 minutes. Finally, 0.1% biocide was added to the dispersion.

Example

[0091] A dispersion was prepared as shown in Example 20, then 0.75 mL of a dispersant (Tego 761) and 1.0 mL of a rheology modifier starch were added and sheared to ensure uniform mixing.

[0092] Examples 22-24: Manufacturing and testing of coated substrates

Example

[0093] Using Mayer Rod 4, aqueous dispersions from Examples 1, 4, and 12 were coated onto solid bleached sulfate (SBS) cardboard substrates of both 14pt and 18pt thickness. The coatings were cured in a hot air dryer at 170°C until a dry coat weight of 8 grams (gsm) per square meter was achieved. Each of these dispersions yielded a Cobb water absorption value of less than 30 gsm and a Kit oil resistance value greater than 5. [Examples]

[0094] Using Mayer Rod 4, aqueous dispersions from Examples 2, 5, and 13 were coated onto solid bleached sulfate (SBS) cardboard substrates of both 14pt and 18pt thickness. The coatings were cured in a hot air dryer at 170°C until a dry coat weight of 8 gsm was achieved. Each of these dispersions yielded a Cobb water absorption value of less than 10 gsm and a Kit oil resistance value greater than 9. [Examples]

[0095] Using Mayer rods 4, 6, 8, and 9, aqueous dispersions from Examples 3, 6, 14, 15, 16, 20, and 21 were coated onto solid bleached sulfate (SBS) cardboard substrates with thicknesses of 14 pt and 18 pt, respectively. The coatings were cured in a hot air dryer at 170°C until a dry coat weight of 8 gsm was achieved. For each of these dispersions, the resulting Cobb water absorption value was less than 10 gsm, and the Kit oil resistance value was greater than 9.

[0096] The above description of preferred embodiments of the present invention is presented for illustrative and explanatory purposes. They are not exhaustive. This invention is not intended to limit the present invention to the exact form disclosed. Obvious modifications or alterations are possible in view of the foregoing. The embodiments are selected and described in an effort to best illustrate the principles and practical applications of the present invention and to enable those skilled in the art to use the invention in various forms and with various modifications suitable for the specific intended use. All such modifications and alterations are within the scope of the present invention as determined by the appended claims, if they are interpreted according to the breadth to which they are properly, legally, and fairly granted.

Claims

1. 35 to 75% by weight of water; 25 to 65 wt. % of polyhydroxyalkanoates; 0.01% to 5.0% by weight of at least one surfactant selected from the group consisting of polysorbates, aromatic polyethylene oxides, sorbitan derivatives, block copolymers of poly(ethylene oxide) and poly(propylene oxide), poly(glycol ethers), poly(vinyl alcohols), alkyl sulfates, alkyl phosphates, stearates, and mixtures thereof; 0.01 wt.% to 5.0 wt.% of at least one rheology modifier; 0.01% to 2.5% by weight of at least one wetting and dispersing agent; and 0.01% to 0.5% by weight of at least one biocide or biostat 1. A biodegradable aqueous dispersion for coating a food contact substrate comprising: The dispersion is powdering the polyhydroxyalkanoate and dispersing the powdered polyhydroxyalkanoate in water using a low to high shear mixer in the presence of at least one surfactant and at least one wetting and dispersing agent to form primary micelles of the polyhydroxyalkanoate; Finishing the dispersion of the polyhydroxyalkanoate particles using an ultrasonic mixer / homogenizer to create a uniform emulsion / dispersion, and adding at least one biocide or biostat and at least one rheological additive and shear mixing to complete dispersion; It is prepared by Biodegradable aqueous dispersion.

2. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion comprises from 25 to 65% by weight of poly-3-hydroxybutyrate-co-3-hydroxyhexanoate ("P(3HB-co-3HHx)").

3. 3. The biodegradable aqueous dispersion of claim 2, wherein P(3HB-co-3HHx) contains from 75 to 99 mole percent hydroxybutyrate and from 1 to 25 mole percent hydroxyhexanoate.

4. 2. The biodegradable aqueous dispersion of claim 1, wherein the dispersion comprises 1 to 25 weight percent of at least one polyhydroxyalkanoate comprising from 25 to 50 mole percent hydroxyvalerate, hydroxyhexanoate, hydroxyoctanoate and / or hydroxydecanoate.

5. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion comprises a polyhydroxyalkanoate having a weight average molecular weight of from 50,000 to 2.5 million daltons.

6. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion comprises particles having an average particle size of from 10 nm to 50 μm.

7. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion has an average solids content of from 25 percent to 65 percent solids.

8. 2. The biodegradable aqueous dispersion of claim 1, wherein the at least one surfactant has a hydrophilic-lipophilic balance of greater than 10.

9. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion comprises from 0.01% to 5.0% by weight of at least one rheology modifier selected from the group consisting of polysaccharides, acrylate-based emulsifying copolymers, viscosity reducers, and thickeners.

10. 2. The biodegradable aqueous dispersion of claim 1, wherein the dispersion further comprises from 0.1% to 5.0% by weight of at least one coalescent selected from the group consisting of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, dimethyl carbonate, methanol, ethanol, ketones, acetates, and / or mixtures thereof.

11. 2. The biodegradable aqueous dispersion of claim 1, wherein the dispersion further comprises from 1% to 35% by weight of at least one filler selected from the group consisting of clay, calcium carbonate, talc, kaolinite, montmorillonite, bentonite, silica, chitin, titanium dioxide, nanoclay or mixtures thereof.

12. 2. The biodegradable aqueous dispersion of claim 1, wherein the dispersion further comprises from 0.5% to 15% by weight of at least one plasticizer selected from the group consisting of sebacates, citrates, fatty esters of adipic, succinic and glucaric acid, lactates, alkyl diesters, citrates, alkyl methyl esters, dibenzoates, propylene carbonate, caprolactone diols having a number average molecular weight of 200-10,000 g / mol, poly(ethylene) glycols having a number average molecular weight of 400-10,000 g / mol, esters of vegetable oils, long chain alkyl acids, adipates, glycerol, isosorbide derivatives or mixtures thereof.

13. 2. The biodegradable aqueous dispersion of claim 1, wherein the dispersion further comprises from 0.1% to 5% by weight of at least one nucleating agent selected from the group consisting of sulfur, erythritol, pentaerythritol, dipentaerythritol, stearates, sorbitol, mannitol, polyester waxes, and mixtures thereof.

14. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion further comprises from 0.01% to 5% by weight of at least one crosslinking agent selected from the group consisting of stabilized ammonium zirconium carbonate, anionic hydroxylated zirconium polymers, potassium zirconium carbonate, anionic hydroxylated zirconium polymers, zinc tetraamine carbonate, and mixtures thereof.

15. 10. The biodegradable aqueous dispersion of claim 1, wherein the dispersion further comprises from 0.05 to 1 wt. % of at least one antifoaming agent selected from the group consisting of polyether siloxanes, polyamide particles, and mixtures thereof.

16. A biodegradable substrate having at least one food contact surface; and A coating applied onto said at least one food contact surface. A biodegradable food service product comprising: Here the coating is 35 to 75% by weight of water; 25 to 65 wt. % of polyhydroxyalkanoates; 0.01% to 5.0% by weight of at least one surfactant selected from the group consisting of polysorbates, aromatic polyethylene oxides, sorbitan derivatives, block copolymers of poly(ethylene oxide) and poly(propylene oxide), poly(glycol ethers), poly(vinyl alcohols), alkyl sulfates, alkyl phosphates, stearates, and mixtures thereof; 0.01 wt.% to 5.0 wt.% of at least one rheology modifier; 0.01% to 2.5% by weight of at least one wetting and dispersing agent; and 0.01% to 0.5% by weight of at least one biocide or biostat and applied as a biodegradable aqueous dispersion comprising The dispersion is powdering the polyhydroxyalkanoate and dispersing the powdered polyhydroxyalkanoate in water using a low to high shear mixer in the presence of at least one surfactant and at least one wetting and dispersing agent to form primary micelles of the polyhydroxyalkanoate; Finishing the dispersion of the polyhydroxyalkanoate particles using an ultrasonic mixer / homogenizer to create a uniform emulsion / dispersion, and adding at least one biocide or biostat and at least one rheological additive and shear mixing to complete dispersion; It is prepared by Biodegradable school lunch supplies.

17. 17. The biodegradable food service product of claim 16, wherein the biodegradable substrate comprises a biodegradable plate, cup, bowl, fiber tray or dishware.

18. 17. The biodegradable food service product of claim 16, wherein the coating is applied on the at least one food contact surface at a coating weight of from 2 to 25 grams per square meter on a dry basis.

19. 17. The biodegradable food service product of claim 16, wherein the coating exhibits a Cobb water absorption value of less than 20 grams per square meter measured according to TAPPI Standard T441.

20. 17. The biodegradable food service product of claim 16, wherein the coating exhibits a Kit Test oil resistance value of greater than Kit Value 5 as measured according to TAPPI Standard T559cm-12.