Ultra-low heat storage coating material

A dark polymer composition with multiple IR transparent dyes and a thermoplastic matrix addresses high heat storage in dark coatings by achieving ultra-low heat accumulation and opacity, ensuring low L values and reduced substrate warping.

JP2022539530A5Inactive Publication Date: 2024-10-09ARKEMA FRANCE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021576946
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2020-06-22
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing dark-colored thermoplastic coatings exhibit high heat storage capacity, leading to warping of substrates like PVC in window and door frames, and there is a need for visually opaque, dark-colored structures with low heat storage temperatures and low L values.

Method used

A dark polymer composition using two or more types of IR transparent dyes, combined with a thermoplastic polar polymer matrix, achieves opacity and NIR transparency, with heat retention below 55°F, 50°F, or even 42°F, and L values less than 50, 40, or 30.

Benefits of technology

The composition provides visually opaque, dark-colored structures with ultra-low heat accumulation, maintaining desired color intensity and reducing substrate warping risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a dark-colored thermoplastic polymer composition that, when formed into a film, has ultra-low heat buildup, is visually opaque, and has high NIR transparency. The dye system includes two or more IR-transparent dyes that combine to produce a color with an L value of less than 40, preferably less than 30, and a heat buildup of less than 50°F, preferably less than 45°F. In one embodiment, the composition is jet black. The composition may be a free-standing film or a capstock applied over a substrate, preferably a white substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dark thermoplastic polymer composition that has ultra-low heat build-up when formed into a film, and is visually opaque and NIR transparent when extruded or laminated onto a light-colored substrate. dye which in combination produce a color with an L value of less than 40, preferably less than 30, and a heat retention of less than 50° F., preferably less than 45° F. dye In one embodiment, the composition is jet black. The composition may be a free-standing film or a coating used on a substrate, preferably a white substrate. [Background technology]

[0002] Many structural plastics exhibit attractive mechanical properties when extruded, molded, or shaped into various products. Such articles include, for example, sports and recreational equipment; decorative exterior trim; molding side trim; quarter trim panels; fenders and fender extensions; louvers; rear end panels; pickup truck bed covers; rearview mirror housings; accessories for trucks, buses, campers, vans, mass transit vehicles; B-pillar extensions, and the like; bathtubs; shower stalls; countertops; appliance housings and liners; building materials; doors; windows; siding; decks; handrails; and shutters; lawn and garden applications; marine applications; aerospace applications; pool applications; and storage facilities. Although these structural plastics are strong, tough, and relatively inexpensive, their exposed surface properties are less than ideal. That is, the surfaces of structural plastics can be degraded by light, easily scratched, and attacked by common solvents.

[0003] As a result, it has become common practice in the industry to coat structural plastics with a resinous material to protect the structural material underneath and provide a surface that can withstand the abuse associated with the service environment. Such surface materials are called "capstocks."

[0004] The covering material is generally much thinner than the structural plastic, typically about 5 to about 25% of the total thickness of the multilayer structure including the covering material and the structural plastic layer. For example, the thickness of the structural plastic layer may be about 1.0 to about 50 mm, preferably 2.5 to 30 mm, while the thickness of the covering material may be about 0.025 to about 2.5 mm.

[0005] Dark cladding materials such as dark red, dark green, dark gray, and even jet black are often desired for siding, banisters, verandas, and window and door frames. The problem with dark cladding materials is that they have a high thermal mass, which can lead to warping of the underlying substrate, such as the PVC substrate often used for window and door frames.

[0006] US8,632,868, US2006 / 0255496, and 2017 / 0361517 describe three factors that affect the level of heat retention in a substrate coated with a dark coating: 1) the thickness of the dark coating must be selected to minimize IR absorbance as NIR passes through the dark coating, reflects off the substrate, and returns through the dark coating. This selection must be made in a manner that maintains the visual color of the coating. 2) the substrate is selected to reflect IR, most commonly by manipulating the loading of TiO2. 3) the pigment in the dark coating required to impart a particular color must be optimized to minimize the NIR absorbance of the pigment. In practice, all three measures must be optimized for a particular coating / color / substrate combination to obtain a functional end product. These references describe IR-transparent coatings with black base colorants in thin coating layers. dyeThey show that using a 100% IR reflective substrate with high levels of TiO2, dark colors such as hunter green and bronze with L values ​​ranging from 13 to 40 can be achieved while maintaining heat build-up below 58°F and even below 52°F.

[0007] Problem: There is a need to provide visually opaque, dark multi-layer structures with low heat build-up temperature, L values ​​less than 50, less than 40, less than 30, jet black, less than 25. It is also desirable to provide these as dark coating films and multi-layer structures with reduced heat build-up below 55°F, even down to 45°F, 42°F or lower.

[0008] Solution: Now, two or more types of IR-transparent dye The combination of, especially, black dye It has been found that by using combinations containing little or no pigment, it is possible to provide a dark, visually opaque, coated white substrate that has a heat retention of less than 55° F., less than 50° F., less than 45° F., or even less than 42° F. The L values ​​of the above colors can be low, less than 50, less than 40, less than 30, or even less than 25 (including jet black). Summary of the Invention

[0009] Although the embodiments have been described herein in a manner that allows a clear and concise specification to be written, it is intended and will be understood that the embodiments can be combined or separated in various ways without departing from the invention, and for example, it will be understood that all preferred features described herein are applicable to all aspects of the invention described herein.

[0010] Aspects of the invention include the following. In a first embodiment, the dark polymer composition comprises: a) a thermoplastic polar polymer matrix; and b) from 0.01 to 1.2 weight percent, based on the weight of the polymer matrix, of two or more thermally stable polymers having a sublimation temperature greater than 200° C., preferably greater than 210° C. dye and when formed into a 0.254 mm monolayer film, has the following characteristics: 1) an L value of less than 50, preferably less than 40, more preferably less than 30, more preferably less than 25; 2) opacity to visible light; 3) a heat build-up temperature of less than 55° F., preferably less than 50° F., preferably less than 48° F., preferably less than 46° F., preferably less than 44° F., preferably less than 42° F.; and 4) a NIR transmittance at 800 nm of greater than 60%, preferably greater than 70%, more preferably greater than 80%. Satisfy all of the above.

[0011] In a second embodiment, the dark polymer composition of embodiment 1 comprises a thermoplastic polar polymer, preferably one or more acrylic polymers, selected from the group consisting of acrylic polymers, styrenic polymers, polyesters, polycarbonates, polyvinylidene fluoride (PVDF), polyamides, and thermoplastic polyurethanes (TPUs).

[0012] In a third aspect, the method according to any one of aspects 1 or 2 dye However, when added to an acrylic matrix at least 0.12 mm thick at a loading of at least 0.2%, its transmittance at 800 nm is greater than 80 percent, preferably greater than 85 percent, and preferably greater than 90 percent. dye The amount of fill is related to thickness and must be at least 0.2% when performing this test on a thickness of 5 to 6 mils (0.127 to 0.15 mm). dye is necessary.

[0013] In a fourth embodiment, the dark polymer composition of any of the preceding embodiments is jet black having an L value of 20 to 30, preferably 23 to 25, and said heat storage is less than 48°F, preferably less than 46°F, more preferably less than 44°F.

[0014] In a fifth embodiment, the multilayer dark structure comprises, from the outside to the inside, a) at least one thermoplastic polar polymer matrix polymer, and at least 0.01 to 1.2 weight percent in total of two or more thermoplastic polar polymers, based on the matrix polymer. dye an outer coating layer comprising: b) a NIR reflective substrate layer; Equipped with The heat storage temperature of the multi-layer structure is less than 55°F, preferably less than 50°F, preferably less than 48°F, preferably less than 46°F, preferably less than 44°F, preferably less than 42°F.

[0015] In a sixth embodiment, the multilayer dark structure of embodiment five comprises a thermoplastic polar polymer selected from the group consisting of acrylic polymers, styrenic polymers, polyesters, polycarbonates, polyvinylidene fluoride (PVDF), and thermoplastic polyurethanes (TPUs), preferably an acrylic polymer.

[0016] In a seventh embodiment, in the multilayer dark structure of embodiment 5 or 6 dye However, when added to an acrylic resin matrix, its transmittance at 800 nm is a minimum of 0.2%. dye The concentration is greater than 80 percent, preferably greater than 85 percent, and preferably greater than 90 percent for a minimum thickness of 0.12 mm of said acrylic matrix polymer.

[0017] In an eighth embodiment, the multilayer dark structure of any of embodiments 5 to 7 is jet black, the L value is 20 to 30, preferably 23 to 25, and the heat storage is less than 48°F, preferably less than 46°F, and more preferably less than 44°F.

[0018] In a ninth embodiment, the multilayer dark structure of any of embodiments 5-8 has an IR reflective substrate selected from the group consisting of polystyrene (PS), high impact polystyrene (HIPS), acrylonitrile / butadiene / styrene (ABS), styrene / butadiene or isoprene / styrene (SBS / SIS), hydrogenated SBS / SIS, polyolefin derivatives such as polypropylene, polyethylene, and thermoplastic polyolefin copolymers, polyvinyl chloride (PVC), wood-polymer composites, biopolymers, pultruded polyester composites, or polyurethane composites.

[0019] In a tenth embodiment, the multilayer dark construction of any of embodiments 5-9 further comprises an intermediate highly NIR reflective layer between the coating layer and the substrate layer, the highly NIR reflective layer comprising at least 6 weight percent titanium dioxide.

[0020] In an eleventh aspect, the method for forming a multilayer structure according to any one of aspects 5 to 10 includes the steps of: a) blending the components of the coating layer together; b) coating the coating layer composition onto a substrate layer; Includes.

[0021] In a twelfth embodiment, the process of embodiment 11 is coextrusion, injection molding, insert molding, pultrusion, or extrusion lamination.

[0022] In a thirteenth embodiment, the method of any of embodiments 11 or 12 further comprises, prior to step a), dye and forming at least two different masterbatches comprising a thermoplastic carrier resin and then mixing the masterbatches with a matrix resin.

[0023] In a fourteenth embodiment, the multilayer dark structure formed by the method of any of embodiments 5-10 or any of embodiments 11-13 is an article selected from the group consisting of automobile parts, recreational vehicles, bathtubs, shower stalls, countertops, appliance enclosures and liners, building materials, doors, windows, siding, porches, banisters, shutters, lawn and garden parts, storage containers, flooring, siding with banisters, and window frames. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 shows transmission data for three polymer film samples of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present invention relates to a dark thermoplastic polymer composition, wherein a film formed from the composition is opaque to visible light, has an L value of less than 50, and has a heat storage of less than 55°F.

[0026] All references cited herein are incorporated by reference. Unless otherwise indicated, all molecular weights are weight average molecular weights as determined by gel permeation chromatography (GPC) and all percentages are weight percentages.

[0027] The term "copolymer" as used herein refers to a polymer composed of two or more different monomeric units, including two comonomers, terpolymers, and polymers having three or more different monomers. The copolymers may be random or block, heterogeneous or homogeneous, and may be synthesized by batch, semi-batch, or continuous processes.

[0028] Thermoplastic polymer matrix The thermoplastic polymer of the composition, which forms the matrix of the composition, may be any thermoplastic polymer, or a compatible mixture thereof. It is preferred that the polymer(s) is polar.

[0029] The polar polymer may be used without any additives, whereby it constitutes more than 97% of the outer layer, with the colorant making up the remainder. In the polar polymer matrix, more than 50 weight percent, preferably at least 70 weight percent, more preferably at least 85 weight percent of the matrix polymer is a polar polymer, including matrices in which the polymer is 100 weight percent of one or more polar polymers. Useful polar polymers include, but are not limited to, acrylic polymers, styrenic polymers, polyesters, polycarbonates, polyvinylidene fluoride (PVDF), and thermoplastic polyurethanes (TPUs), or compatible mixtures thereof. Preferred thermoplastic polar polymers are acrylic or styrenic polymers. Preferred polar polymers for the matrix are one or more acrylic polymer(s) or copolymer(s).

[0030] As used herein, acrylic polymers are intended to include polymers, copolymers, and terpolymers formed from alkyl methacrylate and alkyl acrylate monomers, as well as mixtures thereof. The alkyl methacrylate monomer is preferably methyl methacrylate, which may comprise greater than 50 to 100 weight percent, preferably at least 70 weight percent, and more preferably at least 80 weight percent of the monomer mixture. From 0 to 50 percent of other acrylate and methacrylate monomers or other ethylenically unsaturated monomers may also be present in the monomer mixture, including, but not limited to, styrene, alpha-methylstyrene, acrylonitrile, and low levels of crosslinkers. Suitable acrylate and methacrylate comonomers include, but are not limited to, methyl acrylate, ethyl acrylate and methacrylate, butyl acrylate and methacrylate, isooctyl methacrylate and acrylate, lauryl acrylate and methacrylate, stearyl acrylate and methacrylate, isobornyl acrylate and methacrylate, methoxyethyl acrylate and methacrylate, 2-ethoxyethyl acrylate and methacrylate, and dimethylaminoethyl acrylate and methacrylate monomers. Alkyl (meth)acrylic acids such as methacrylic acid and acrylic acid at levels up to 10 weight percent of the total polymer may be useful for the monomer mixture. The acrylic polymer may have 70 to 99.5 weight percent methyl methacrylate units and 0.5 to 30 weight percent of one or more C acrylic acids. 1~8 Most preferred are copolymers having linear or branched alkyl ester units of the formula:

[0031] Styrenic polymers include, but are not limited to, polystyrene, high impact polystyrene (HIPS), acrylonitrile-butadiene-styrene (ABS) copolymers, acrylonitrile-styrene-acrylic acid ester (ASA) copolymers, styrene acrylonitrile (SAN) copolymers, methacrylate-butadiene-styrene (MBS) copolymers, styrene-butadiene copolymers, styrene-butadiene-styrene block (SBS) copolymers and their partially or fully hydrogenated derivatives, styrene-isoprene copolymers, styrene-isoprene-styrene (SIS) block copolymers and their partially or fully hydrogenated derivatives, and styrene-(meth)acrylic acid ester copolymers such as styrene-methyl methacrylate copolymer (S / MMA). A preferred styrenic polymer is ASA. Styrenic polymers used in the present invention can be produced by means known in the art, including emulsion polymerization, solution polymerization, and suspension polymerization. The styrene content of the styrene copolymers used in the present invention is at least 10 weight percent, preferably at least 25 weight percent.

[0032] In one embodiment, the weight average molecular weight of the polar polymer is 50,000 to 500,000 g / mol, preferably 75,000 to 200,000 g / mol, as measured by gel permeation chromatography (GPC). The molecular weight distribution of the acrylic polymer may be monomodal or multimodal with a polydispersity index of more than 1.5. In a preferred embodiment, the T g exceeds 70°C.

[0033] In a preferred embodiment, the thermoplastic polymer composition is formed into a film that is simultaneously NIR transparent, optically opaque, has an L value of less than 50, and has a heat storage of less than 50° F. By NIR transparent, it is meant that greater than 60 percent, more preferably at least 70 percent, and more preferably at least 80 percent of near infrared radiation measured at 800 nm is transmitted through the film. Near infrared radiation is radiation in the wavelength range of 0.7 to 5 microns, and the transmission at 800 nm is at least 0.2%. dye It is measured by ASTM E1164 in the form of a 0.127 mm film containing colorant (or enough colorant to produce an opaque film). Optically opaque means the contrast ratio of the film measured with an X-Rite Color i7. The luminous reflectance (Y) of the sample film on a white substrate and on a black substrate is measured. The resulting ratio, Y on black substrate / Y on white substrate, is then calculated. This value should be ≧98%, preferably greater than 99%. If the contrast ratio is less than 98%, the substrate is visible and the film is not optically opaque.

[0034] The desired properties of opacity and NIR transparency of the film of the composition of the present invention result from a balance between film thickness and colorant concentration. To achieve this balance, the film thickness in the present invention is in the range of 0.1 to 0.5 mm, preferably 0.127 to 0.381 mm. dye Higher levels of α-methyl-2-phenyl-1,2-difluoro-1,3-difluoro-1,4-trifluoro-1,5-trifluoro-1,6-trifluoro-1,7-trifluoro-1,8-trifluoro-1,9-trifluoro-1,1-trifluoro-1,2-trifluoro-1,3-trifluoro-1,4-trifluoro-1,5-trifluoro-1,6-trifluoro-1,7-trifluoro-1,8-trifluoro-1,9-trifluoro-1,9-trifluoro-1,1-trifluoro-1,1-trifluoro-1,2-trifluoro-1,3-trifluoro-1,4-trifluoro-1,5-trifluoro-1,6-trifluoro-1,7-trifluoro-1,8-trifluoro-1,9-trifluoro-1,9-trifluoro-1 dye The level of coloring agent increases significantly, causing the composition to collapse. dye This can lead to processing problems such as the formation of lumps and defects in the film. If the film is too thick, it becomes difficult to maintain the required NIR transparency.

[0035] Additives In addition to having a polar polymer matrix and at least two colorants, the composition of the present invention may also contain additives that are typically present in coating compositions. Non-limiting examples of such additives include fillers, impact modifiers, surface modification additives, flame retardants, antioxidants, UV screening additives, heat stabilizers, and processing aids. Examples of fillers used include talc, calcium carbonate, mica, matting agents, pigments such as wollastonite, dolomite, glass fiber, boron fiber, carbon fiber, carbon black, titanium dioxide, or mixtures thereof. Other polymer additives may include polycarbonates, polyurethanes, polysulfones, polyamides, polyolefins, including copolymers and terpolymers based on these polymers, and these polymers include linear, branched, block, and grafted polymer structures. Impact modifiers include core-shell impact modifiers and block copolymer impact modifiers. Examples of matting agents include, but are not limited to, crosslinked polymer particles of various shapes. The amount of fillers and additives included in the polymer composition of each layer may vary from about 0.01% to about 70% of the combined weight of the polymer, additives, and fillers. Typical amounts include about 5% to about 60%, about 10% to about 50%. In a preferred embodiment, the impact modifier is expected to be the largest contributor to any filler added, and the impact modifier used has little or no effect on the NIR transmission. Antioxidants generally known in the art are suitable for addition to the polymers described herein at any suitable level. Non-limiting examples include sterically hindered phenols, organic phosphites, and amines. Additives known in the art for improving and enhancing UV stability are suitable for use in any layer of the present multilayer composite structure at any suitable level. Non-limiting examples include hindered amine light stabilizers (HALS), benzotriazoles, triazines, benzophenones, and cyanoacrylates.

[0036] Coloring agent The compositions of the present invention have a dark color with an L value of less than 50, less than 40, less than 35, less than 30, or less than 25. This dark color requirement must be balanced with low heat build-up, such as less than 55°F, less than 50°F, less than 45°F, or even less than 42°F. Spectroscopic data for the test specimens was obtained using an X-Rite 7000A spectrophotometer or a PerkinElmer Lambda 950 scanning spectrometer in accordance with ASTM E1164 and d-8° illumination. Color data, including L values, were then calculated using ASTM E308 and reported using CIE L*a*b*D65-10°.

[0037] The ultra-low heat storage and dark color of the films made from the compositions of the present invention are due to the presence of two or more NIR transparent films. dye The dark color is due to the combination of NIR transparency. dye At least 0.2 weight percent of the acrylic resin in the form of a 0.12 mm thick film is dye It means that the transmittance at 800 nm, as measured in accordance with ASTM E1164, of the combination of is greater than 80 percent, more preferably greater than 85 percent, and most preferably greater than 90 percent.

[0038] This is different from IR-reflecting modified carbon black pigments or metal oxides that exist in the art that exhibit heat retention of 57° F., 59° F., or greater. The present composition comprises at least two different dye As long as there exists any number of different dye This may include three, four, five, or even six or more different pigments in combination to form the desired final color. dye Includes:

[0039] In one embodiment, a black color, even a jet black color, with low heat storage was produced. L values ​​of 20 to 30, preferably 23 to 25, were obtained. This is because the black dye All dyeIt is possible to use less than 10% by weight, less than 5% by weight, less than 2% by weight, and most preferably 0% by weight, with little or no use at all.

[0040] In one embodiment, a non-black film is used to form a dark, even black, film. dye By mixing dye It was found that the heat storage capacity of black ink is lower than that of dark colors based on black ink. dye is any non-black color used in combination to produce an overall dark color. dye Without being bound to any particular theory, IR transparent black dye The reason why the samples containing the black IR-transmitting colorants exhibit higher heat storage than the samples containing the non-black IR-transmitting colorants used in the present invention is that the black IR-transmitting colorants in the wavelength range of 690 nm to 2220 nm are more easily absorbed by the white substrate than the non-black IR-transmitting colorants used in the present invention. dye The reason for this is believed to be that the overall IR reflectance of the colorant used in the present invention is lower than that of the colorant used in the present invention. This difference is particularly noticeable at 690 nm to 1130 nm. The high IR reflectance of the colorant used in the present invention on a white substrate results in a black substrate on the same white substrate. dye The heat storage capacity is even lower compared to

[0041] The composition is dye The level of is a function of the thickness of the film and the balance between optical opacity, NIR transmittance, and heat storage. In one embodiment, the total composition used in the injection molded part is dye The total level ranges from 0.01 to 1.2 weight percent, preferably 0.05 to 0.5 weight percent, based on the total weight of the polymer matrix. dye A low total level of does not provide the required opacity, dye Higher levels result in undesirable increases in the cost of the composition. dye When the total level of exceeds 3 weight percent, dye This can result in processing problems including lumps and surface defects.

[0042] Used in the present invention dye is preferably NIR transparent and thermally stable. dye This means that the material will not sublime for 2 minutes in the normal process window of 160 to 200°C. dye It is preferred that the sublimation temperature of each of the above is greater than 200°C, preferably greater than 210°C, and more preferably greater than 220°C.

[0043] Base material The dark thermoplastic polymer composition of the present invention can also be used as a monolayer film. In a preferred embodiment, the dark thermoplastic polymer composition is part of a multilayer structure as a thin coating on a white substrate. The substrate can be pultruded, extruded, or otherwise formed into a profile.

[0044] In a preferred embodiment, the substrate is NIR reflective, meaning that greater than 50 percent, more preferably greater than 60 percent, and most preferably greater than 70 percent of NIR radiation at 800 nm is reflected by the surface. Reflectance can be measured on the substrate or on the film alone using an X-Rite 7000A spectrophotometer according to ASTM El164 using d-8° illumination.

[0045] In one embodiment, a separate, thin, highly IR reflective layer is present between the coating layer and the substrate layer to enhance IR reflectance. This highly IR reflective layer may be a thermoplastic resin, a thermosetting polymer, or a coated metal layer. As described in US2017 / 0361517, the highly IR reflective layer includes more than 8% titanium dioxide based on the weight of the polymer resin.

[0046] In a preferred embodiment of the invention, the intermediate thin highly IR reflective layer is not required and the dark thermoplastic coating layer may be coated directly onto the substrate layer. Eliminating the optional intermediate highly IR reflective layer saves manufacturing steps and costs.

[0047] The thickness of the substrate layer is at least twice the thickness of the coating, preferably at least 5 times. The substrate layer may be 50 microns to 10 cm, preferably 0.2 mm to 10 cm. The substrate may be another polymer (thermoplastic, elastomeric, or thermosetting) such as, by way of non-limiting examples, acrylic polymers, polystyrene (PS), high impact polystyrene (HIPS), acrylonitrile / butadiene / styrene (ABS), styrene / butadiene or isoprene / styrene (SBS / SIS), hydrogenated SBS / SIS, polyolefin derivatives such as polypropylene, polyethylene, and thermoplastic polyolefin copolymers, polyvinyl chloride (PVC), biopolymers, pultruded polyester or polyurethane composites, wood-polymer composites, or a non-polymeric material, including, but not limited to, paper, metal, ceramics, glass, wood, etc.

[0048] Composite materials, such as ASN / wood composites, fiber reinforced polymer composites, or composites formed from liquid resin systems, such as Arkema's ELIUM® Liquid Resin System, may also function as the substrate.

[0049] Formation method The compositions of the present invention are prepared by reacting a matrix thermoplastic polymer resin with the above-mentioned dye and optional additives. The components of the composition may be added in any order and may be melt blended together. Because the levels of colorants are very low, a preferred process involves first forming a masterbatch of each colorant using a polar polymeric carrier resin that is compatible with the matrix polymer, and then melt blending the desired levels of the masterbatch into the matrix polymer. In one embodiment, the T of the carrier resin is g is the T of the matrix resin g This allows for better dispersion of the masterbatch in the matrix resin.

[0050] The above matrix resin is used in the present invention. dye Once thoroughly compounded, monolayer films can be produced by means conventional in the art such as extrusion and blown film.

[0051] Multi-layer structures or profiles having the dark coating of the present invention can be formed by means known in the art, such as by coextrusion, injection molding, insert molding, pultrusion, and extrusion lamination.

[0052] In one embodiment, a multi-layer structure was produced in which the coating thickness was 0.254 mm and the overall structure thickness was 1.73 mm.

[0053] The multi-layer structure formed above may be provided in sheet form, which is thermoformed into a multi-layer article of practical use after the formation of the sheet.The multi-layer structure may also be directly coextruded into a final profile or article.Useful coated articles of the present invention include, but are not limited to, automotive parts, RVs, bathtubs, showers, countertops, appliance housings and liners, building materials, doors, windows, siding, verandas, railings and shutters, lawn and garden parts, and storage containers.The multi-layer structure may also be directly coextruded into profiles, such as, but not limited to, floor boards, railings and siding, and window frames.

[0054] characteristics The dark compositions of the present invention can be processed into monolayer films having an L value of less than 50, preferably less than 40, less than 35, or even less than 25, such as jet black, that are optically opaque and have a heat storage of less than 55° F., less than 50° F., less than 48° F., less than 46° F., less than 44° F., or even less than 42° F. Jet black films having an L value of 20-30, preferably 23-25, that are NIR transparent, and optically opaque can have a low heat storage of less than 48° F., less than 46° F., less than 44° F., or even less than 42° F.

[0055] The multilayer structure of the present invention has a coating layer having a thickness of 0.1 to 0.5 mm, preferably 0.13 to 0.38 mm, which is optically opaque, has an L value preferably less than 40, less than 30, or less than 25, is NIR transparent, and has a heat storage capacity of less than 55°F, less than 50°F, less than 48°F, less than 46°F, less than 44°F, or even less than 42°F for the entire multilayer structure including the white substrate layer. EXAMPLES

[0056] Example 1 Three coating layer polymer formulations were prepared: one containing an ultra-low heat storage colorant package according to the present invention, a second containing an IR-transmitting black colorant for comparison, and a third containing an IR-reflective black pigment. For comparison, a 1 / 8" sample containing carbon black in PVC was also prepared.

[0057] The acrylic coating formulation is prepared by melt blending the above ingredients in a twin screw extruder operating at 300-425 rpm with typical processing temperatures as shown below. TIFF2020263737000001.tif23170

[0058] The prepared acrylic coating formulation was co-extruded onto a white PVC substrate using a custom made 1 inch by 4 inch die and two extruders, one for the substrate layer and one for the coating layer.

[0059] The extruder for the white PVC substrate was a single screw extruder operating at 8 revolutions per minute (RPM) with a barrel temperature profile of 168° C. (feed zone tip) to 182° C. (die tip).

[0060] The extruder for the acrylic formulation coating layer was a single screw extruder with a barrel temperature profile of 187° C. (feed zone) to 210° C. (die tip). The coextrusion die temperatures for the profiles were set at 168° C. and 185° C. The thickness of the acrylic coating layer can range from 0.001 inch to 0.02 inch.

[0061] These acrylic compositions and their heat storage properties and L values ​​are shown in Table 1. TIFF2020263737000002.tif116170

[0062] It is clear that the ultra-low heat storage colorant in Acrylic Coating 1 shows the lowest heat storage value (44 F) and L value of 23, while the Comparative Example shows higher heat storage values ​​(53 F and 57 F). This is likely due to the combination of the highly IR-transmitting acrylic coating layer and the highly IR-reflective substrate layer (white PVC).

[0063] Example 2 This example uses transmission data obtained from a spectrophotometer to dye Spectral data was obtained using a PerkinElmer Lambda 950 scanning spectrophotometer according to ASTM E1164 using d-8° illumination.

[0064] As shown in Figure 1, both Sample A and Sample B have transmittance above 90% at 800 nm because both samples contain a combination of highly IR-transmitting organic colorants. Sample C has significantly lower transmittance at the same wavelength because this sample contains IR-reflective pigments.

[0065] The composition of the sample in this example is shown in Table 2. TIFF2020263737000003.tif102170

Claims

1. a) a thermoplastic polymer matrix; b) 0.01 to 1.2 percent by weight, based on the weight of the polymer matrix, of two or more dyes that are thermally stable and have a sublimation temperature greater than 200° C.; 1. A dark polymer composition comprising: When formed into a 0.127 mm monolayer film, the following conditions are met: 1) an L value of less than 25; 2) opacity to visible light; 3) a heat storage temperature of less than 55° F.; 4) NIR transmittance at 800 nm measured according to ASTM E1164 of greater than 90%; The composition satisfies all of the above.

2. The dark polymer composition of claim 1, wherein the thermoplastic polymer comprises one or more polymers selected from the group consisting of acrylic polymers, styrenic polymers, polyesters, polycarbonates, polyvinylidene fluoride (PVDF), and thermoplastic polyurethanes (TPU).

3. The dark polymer composition of claim 1, wherein the thermoplastic polymer comprises one or more acrylic polymers.

4. 2. The dark polymer composition of claim 1, wherein said dark color is jet black, said L value is greater than or equal to 23 and less than 25, and said heat storage temperature is less than 48°F.

5. A multi-layer dark structure, comprising from the outside to the inside: a) an outer coating layer comprising the dark polymer composition of claim 1, said outer coating layer being opaque to visible light and having a NIR transmission at 800 nm greater than 90% as measured in accordance with ASTM E1164 and an L value of less than 25; b) a NIR reflective substrate layer; Equipped with The multi-layer dark structure has a heat storage temperature of less than 55°F.

6. The multilayer dark structure of claim 5, wherein the thermoplastic polymer comprises one or more polymers selected from the group consisting of acrylic polymers, styrenic polymers, polyesters, polycarbonates, polyvinylidene fluoride (PVDF), and thermoplastic polyurethanes (TPU).

7. The multilayer dark structure of claim 5, wherein the thermoplastic polymer comprises one or more acrylic polymers.

8. 6. The multi-layer dark structure of claim 5, wherein said dark color is jet black, said L value is greater than or equal to 23 and less than 25, and said heat storage temperature is less than 48°F.

9. 6. The multilayer dark structure of claim 5, wherein the NIR reflective substrate is selected from the group consisting of polystyrene (PS), high impact polystyrene (HIPS), acrylonitrile / butadiene / styrene (ABS), styrene / butadiene or styrene / isoprene (SBS / SIS), hydrogenated SBS / SIS, polyolefin derivatives such as polypropylene, polyethylene, and thermoplastic polyolefin copolymers, polyvinyl chloride (PVC), biopolymers, pultruded polyester or polyurethane composites, and wood-polymer composites.

10. 6. The multilayer dark construction of claim 5 further comprising an intermediate highly NIR reflective layer between said coating layer and said substrate layer, said highly NIR reflective layer comprising at least 6 weight percent titanium dioxide.

11. a) blending the components of the coating layer together; b) coating the coating layer composition onto the substrate layer; 6. A method for forming the multi-layer dark structure of claim 5, comprising:

12. The method of claim 11 , wherein the method is coextrusion, injection molding, insert molding, pultrusion, or extrusion lamination.

13. 12. The method of claim 11, wherein prior to step a), at least two different masterbatches are formed, each comprising one or more dyes and a thermoplastic carrier resin, followed by mixing the masterbatches with the matrix resin.

14. 6. The multi-layer dark structure of claim 5, comprising an article selected from the group consisting of automobile parts, recreational vehicles, bathtubs, shower stalls, countertops, appliance enclosures and liners, building materials, doors, windows, siding, porches, banisters, shutters, lawn and garden parts, storage containers, flooring, siding with banisters, and window frames.