Multi-layer co-extrusion barrier film and preparation method thereof

By using a combination of modified kaolin and copolymer in a multi-layer coextruded barrier membrane, a five-layer structure is formed, which solves the problem of poor barrier properties in the prior art, and achieves higher barrier properties and thermal stability. It is suitable for Food and pharmaceutical packaging.

CN118876536APending Publication Date: 2024-11-01CHONGZHOU JUNJIAN PLASTIC CO LTD

Patent Information

Application Number
CN202411072119.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing multi-layer coextruded barrier film has poor barrier properties and cannot meet the barrier requirements of oxygen and water vapor in food and drug packaging.

Method used

Adopting a five-layer structure from the outside to the inside, the middle layer is made of ethylene-vinyl alcohol copolymer, polyamide and DDAB modified kaolin blend, the outer layer is made of homopolymer polypropylene and cycloolefin copolymer, the sub-external layer and the second layer The inner layer is blended with polypropylene and polypropylene by maleic anhydride, and the inner layer is blended with binary/tere copolymer and elastomer. By modifying the combination of kaolin and copolymer, the barrier properties are improved.

Benefits of technology

It achieves better barrier properties, significantly reduces oxygen, carbon dioxide permeability and water vapor permeability, improves thermal bonding strength, and the membrane material is resistant to heat pressing, cooking and sterilization without deformation, and the production process is environmentally friendly and has low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876536A_ABST
    Figure CN118876536A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of flexible packaging, and provides a multi-layer co-extrusion barrier film and a preparation method thereof. According to the method, an outer layer, a secondary outer layer, a middle layer, a secondary inner layer and an inner layer are sequentially arranged from outside to inside by adopting a multi-layer co-extrusion barrier film structure; wherein the middle layer is prepared from a blend of an ethylene-vinyl alcohol copolymer, polyamide and DDAB modified kaolin; the ethylene-vinyl alcohol copolymer accounts for 30-70 parts by weight, the polyamide accounts for 10-40 parts by weight, and the DDAB modified kaolin accounts for 1-5 parts by weight. The barrier film is prepared through simultaneous and respective film blowing of a five-layer co-extrusion film blowing machine, the film material is not sticky before and after hot-pressing sterilization, the production process is environment-friendly, the production cost is low, and the raw material cost is low due to localization of raw materials. Therefore, the high-performance barrier film has a wide heat sealing temperature window, high heat sealing strength and high barrier performance, does not deform at high temperature, fills the blank of the high-performance barrier film in the current market, and has great application value in the aspects of medicine and food packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flexible packaging, and in particular, relates to a multi-layer co-extruded barrier film and a preparation method thereof. Background Art

[0002] In recent years, my country's plastic packaging industry has developed rapidly, with output increasing at a rate of more than 10% per year. Functionality, especially high barrier properties, has become an important research direction for plastic packaging to meet the requirements of diversification and functionalization. Food and medicine are the most widely used fields for barrier film materials, mainly to prevent oxygen and water vapor in the air from entering the packaging and causing the medicine or food to deteriorate, thereby reducing its shelf life. According to the production process, barrier films can be mainly divided into composite films and co-extruded films. Composite films refer to films with different functions bonded together by adhesives, and co-extruded films refer to two or more materials that are compositely welded together in a die head in a molten state. Compared with composite films, co-extruded films have the advantages of low cost, high production efficiency, and environmentally friendly production process.

[0003] Food and medicine are sensitive to small gas molecules such as oxygen and water vapor; the urgent need to extend their shelf life has put forward higher requirements for packaging materials. However, the barrier properties of barrier films in the prior art are poor and cannot meet the needs of food and medicine packaging. For example, the patent with publication number CN112721377A discloses a multi-layer co-extruded high-barrier film, including an integrated composite layer structure, the integrated composite layer structure has no stratification phenomenon, a multi-layer co-extrusion process, and a double PE structure to increase the puncture resistance of the product. The middle layer uses LDPE-EVOH (-LDPE as a barrier layer to reduce the entry of gas and keep the inert gas in the bag from leaking out. The addition of elastomer improves the flexibility of the rice bag. The outer layer adopts an independent support structure and a transparent PP material, and has better sealing and body-fitting properties. However, its barrier properties are poor. Therefore, based on the above description, how to improve the barrier properties of the multi-layer co-extruded barrier film is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The present application is used to solve the technical problem of poor barrier performance of barrier films existing in the prior art.

[0005] Therefore, in view of the above-mentioned deficiencies in the prior art, the first object of the present invention is to provide a multi-layer co-extruded barrier film, wherein the structure of the multi-layer co-extruded barrier film is sequentially provided with an outer layer, a sub-outer layer, a middle layer, a sub-inner layer and an inner layer from the outside to the inside; wherein the middle layer is made of a blend of ethylene-vinyl alcohol copolymer, polyamide and DDAB modified kaolin; in parts by weight, the ethylene-vinyl alcohol copolymer accounts for 30 to 70 parts, the polyamide accounts for 10 to 40 parts, and the DDAB modified kaolin accounts for 1 to 5 parts.

[0006] Furthermore, the outer layer is made by blending homopolypropylene and cycloolefin copolymer; in parts by weight, the homopolypropylene accounts for 40-70 parts, and the cycloolefin copolymer accounts for 30-60 parts; the melt index of the blend of homopolypropylene and cycloolefin copolymer is 2-6g / 10min.

[0007] Furthermore, the sub-outer layer and the sub-inner layer are made of maleic anhydride grafted polypropylene or a blend of maleic anhydride grafted polypropylene and polypropylene; in parts by weight, the polypropylene accounts for 0 to 60 parts, and the maleic anhydride grafted polypropylene accounts for 40 to 100 parts; the melt index of the polypropylene or the blend of polypropylene and maleic anhydride grafted polypropylene is 2 to 8 g / 10min.

[0008] Furthermore, the inner layer is made of a binary / ternary copolymer polypropylene and an elastomer blend; in parts by weight, the binary / ternary copolymer polypropylene accounts for 60-80 parts, and the elastomer accounts for 20-40 parts; the melt index of the binary / ternary copolymer polypropylene and elastomer blend is 1-8g / 10min.

[0009] Furthermore, the elastomer includes one or more of styrene-ethylene-butylene-styrene block copolymer, styrene-ethylene-propylene-styrene copolymer and polyolefin elastomer.

[0010] Furthermore, the total thickness of the barrier film is 180-200 μm; the thickness of the outer layer is 10-30 μm; the thickness of the sub-outer layer and the sub-inner layer are both 10-20 μm; the thickness of the middle layer is 100-130 μm; and the thickness of the inner layer is 20-40 μm.

[0011] Furthermore, the barrier film satisfies at least one of the following properties: oxygen and carbon dioxide permeability is 0.1 to 0.4 cm 3 / (m 2 ·d), water vapor transmission rate is 0.4~1.0g / (m 2 ·d), heat sealing strength is 35~45N / 15mm.

[0012] The technical mechanism is:

[0013] (1) Kaolin has a layered silicate structure. Kaolin is modified with DDAB, and the quaternary ammonium ions of DDAB are exchanged with the interlayer ions of kaolin to obtain DDAB-modified kaolin. DDAB is inserted into the interlayer of kaolin, which increases the interlayer spacing of kaolin, improves the compatibility of kaolin and polymer molecules, and is also conducive to the entry of polymer molecules into the kaolin lamellae in subsequent processing. Therefore, through modification, the interlayer spacing of kaolin is increased while its compatibility with organic molecules is enhanced.

[0014] (2) By adding DDAB-modified kaolin nanoparticles to the high-barrier material and the matrix to reduce the solubility of the permeating molecules, extend the permeation path of the permeating molecules, and reduce the diffusion rate of the permeating molecules, the barrier properties of the polymer are increased, and the barrier properties of the barrier film are further improved.

[0015] (3) The middle layer material is made by melt blending ethylene-vinyl alcohol copolymer and polyamide. Thanks to the advantage of the small free volume in the polyamide high barrier material, it can improve the barrier performance to a certain extent while reducing the cost. Therefore, the method of blending the high barrier material with the matrix has a wide range of application scenarios and good modification effect.

[0016] (4) The blending of cycloolefin copolymers and polyolefin materials can not only solve the molding problem when using pure cycloolefin copolymers, but also improve the thermal stability, water vapor barrier and other properties of the blended materials without adding a barrier layer.

[0017] (5) Using binary and / or ternary copolymer polypropylene and elastomer blends, the elasticity and toughness are enhanced by adding elastomers to polypropylene for blending and modification, thereby forming an inner layer; using ethylene-vinyl alcohol copolymer, polyamide and DDAB modified kaolin blend to form a middle layer. Ethylene vinyl alcohol copolymer combines the processability of ethylene polymer with the barrier effect of vinyl alcohol polymer, not only showing excellent processability, but also showing excellent blocking effect on gas, odor, fragrance, solvent, etc., thereby making the middle layer have a good barrier effect; using homopolymer polypropylene and cycloolefin copolymer, utilizing their good impact resistance to form an outer layer, enhancing durability and playing a certain protective role for the internal layers; using maleic anhydride grafted polypropylene or maleic anhydride grafted polypropylene and polypropylene blends, by adding polypropylene grafted maleic anhydride to polypropylene for blending and modification, utilizing the characteristics of maleic anhydride grafted polypropylene to enhance the adhesion and compatibility of polar materials and non-polar materials, forming a sub-inner layer and a sub-outer layer that play a bonding role, and bonding the inner layer, middle layer and outer layer together.

[0018] The second object of the present invention is to provide a method for preparing a multilayer co-extruded barrier film as described in any one embodiment of the first object, the method comprising the following steps:

[0019] S1, mixing kaolin dispersion with DDAB to modify kaolin to obtain DDAB-modified kaolin;

[0020] S2, extruding and granulating the DDAB-modified kaolin, ethylene-vinyl alcohol copolymer and polyamide in a twin-screw extruder at a set temperature to obtain a middle-layer material;

[0021] S3, placing the inner layer material, the sub-inner layer material, the middle layer material, the sub-outer layer material and the outer layer material into the corresponding extruder hoppers of the five-layer co-extrusion film blowing machine respectively for five-layer co-extrusion film blowing, followed by water cooling, shaping, winding and slitting to obtain a barrier film.

[0022] Furthermore, the set temperature of the extrusion granulation is 180-240°C.

[0023] Furthermore, the extrusion temperature of the outer layer is 190-220°C; the extrusion temperature of the sub-outer layer and the sub-inner layer is 180-220°C; the extrusion temperature of the middle layer is 180-220°C; the extrusion temperature of the inner layer is 190-210°C; and the die head temperature is 180-230°C.

[0024] The beneficial effects of the present invention are:

[0025] (1) Compared with conventional packaging films, the barrier film of the present invention has better barrier properties, with oxygen and carbon dioxide permeation rates of 0.1 to 0.4 cm 3 / (m 2 ·d), water vapor transmission rate is 0.4~1.0g / (m 2 ·d).

[0026] (2) The barrier film of the present invention has a relatively high heat-sealing strength, which can reach 35 to 45 N / 15 mm;

[0027] (3) The barrier film of the present invention is resistant to autoclave sterilization and the film material does not deform.

[0028] (4) The barrier film is made by blowing films simultaneously in a five-layer co-extrusion film blowing machine. The film material does not stick together before and after hot pressing sterilization. The production process is environmentally friendly. Not only is the production cost low, but the cost of raw materials is also low due to the localization of raw materials. It can be seen that it has a wide heat-sealing temperature window and high heat-sealing strength, strong barrier properties, and does not deform at high temperatures. It fills the gap in this type of high-performance barrier film on the current market and has great application value in medicine and food packaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 A schematic cross-sectional view of a multilayer co-extruded barrier film provided in an embodiment of the present application. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] Example 1

[0033] This embodiment provides a method for preparing a multi-layer co-extruded barrier film, comprising the following steps:

[0034] S11, kaolin and deionized water are prepared into a dispersion according to a ratio (1g:20mL), and the dispersion is stirred at 500r / min in a constant temperature oil bath at 80°C for 30 minutes, DDAB is added to the evenly dispersed slurry, and the mixture is stirred at 80°C for 4 hours and then cooled to room temperature, centrifuged after standing, and washed with deionized water and anhydrous ethanol for multiple times until no precipitation is produced when 0.1M silver nitrate solution is dropped into the supernatant, and the mixture is dried in a drying oven at 60°C, and finally ground through a 200-mesh standard sieve to obtain DDAB-modified kaolin;

[0035] S21, 2 parts of DDAB modified kaolin, 58 parts of ethylene-vinyl alcohol copolymer, and 40 parts of polyamide are extruded and granulated at 200°C in a twin-screw extruder to obtain a middle layer material; 70 parts of homopolymer polypropylene and 30 parts of cycloolefin copolymer are extruded and granulated in a twin-screw extruder to obtain a melt index of 3-4 g·(10min) -1 The outer layer material; 70 parts of maleic anhydride grafted polypropylene and 30 parts of polypropylene were extruded and granulated in a twin-screw extruder to obtain a melt index of 3 to 4g·(10min) -1 The inner and outer layers of the material; 80 parts of the terpolymer polypropylene and 20 parts of the SEBS blended material were extruded and granulated in a twin-screw extruder to obtain a melt index of 4 to 5 g·(10min) -1 The inner material of the

[0036] S3. Put the inner layer material, the sub-inner layer material, the middle layer material, the sub-outer layer material and the outer layer material into the corresponding extruder hopper of the five-layer co-extrusion film blowing machine for five-layer co-extrusion film blowing, and then water-cool, shape, roll up and cut to obtain a barrier film; wherein the extrusion temperature of the outer layer is 200°C; the extrusion temperature of the sub-outer layer and the sub-inner layer is 190°C; the extrusion temperature of the middle layer is 210°C; the extrusion temperature of the inner layer is 200°C; and the die head temperature is 210°C. The total thickness of the barrier film is 180μm; wherein the thickness of the inner layer is 30μm, the thickness of the sub-inner layer is 10μm, the thickness of the sub-outer layer is 10μm, the thickness of the middle layer is 110μm, and the thickness of the outer layer is 20μm.

[0037] Example 2

[0038] The difference between this embodiment and embodiment 1 is that the total thickness of the barrier film is 190 μm, wherein the inner layer is 30 μm thick, the sub-inner layer is 10 μm thick, the sub-outer layer is 10 μm thick, the middle layer is 110 μm thick, and the outer layer is 30 μm thick.

[0039] Example 3

[0040] The difference between this embodiment and embodiment 1 is that the total thickness of the barrier film is 200 μm, wherein the inner layer is 30 μm thick, the second inner layer is 10 μm thick, the second outer layer is 10 μm thick, the middle layer is 120 μm thick, and the outer layer is 30 μm thick.

[0041] Example 4

[0042] The difference between this embodiment and embodiment 3 is that 4 parts of DDAB modified kaolin, 56 parts of ethylene-vinyl alcohol copolymer and 40 parts of polyamide are extruded and granulated at 200° C. in a twin-screw extruder to obtain a middle layer material.

[0043] Example 5

[0044] The difference between this embodiment and embodiment 3 is that 5 parts of DDAB modified kaolin, 70 parts of ethylene-vinyl alcohol copolymer and 25 parts of polyamide are extruded and granulated at 200° C. in a twin-screw extruder to obtain a middle layer material.

[0045] Example 6

[0046] The difference between this embodiment and embodiment 3 is that 60 parts of homopolymerized polypropylene and 40 parts of cycloolefin copolymer are extruded and granulated in a twin-screw extruder to obtain a granulated product with a melt index of 3 to 4 g·(10 min) -1 outer material.

[0047] Example 7

[0048] The difference between this embodiment and embodiment 3 is that 70 parts of binary copolymerized polypropylene and 30 parts of polyolefin elastomer blended material are extruded and granulated in a twin-screw extruder to obtain an inner layer material with a melt index of 3 to 4 g·(10 min)-1.

[0049] Example 8

[0050] The difference between this embodiment and embodiment 3 is that 60 parts of homopolymerized polypropylene and 40 parts of cycloolefin copolymer are extruded and granulated in a twin-screw extruder to obtain a granulated product with a melt index of 3 to 4 g·(10 min) -1 outer material.

[0051] Example 9

[0052] The difference between this embodiment and embodiment 3 is that 20 parts of binary copolymer polypropylene, 60 parts of ternary copolymer polypropylene and 20 parts of SEBS are blended and granulated in a twin-screw extruder to obtain an inner layer with a melt index of 4-5 g·(10 min)-1.

[0053] Example 10

[0054] The difference between this embodiment and embodiment 3 is that 50 parts of homopolypropylene and 50 parts of cycloolefin copolymer are extruded and granulated in a twin-screw extruder to obtain an outer layer material with a melt index of 3 to 4 g·(10 min)-1.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 3 is that 58 parts of ethylene-vinyl alcohol copolymer and 40 parts of polyamide are extruded and granulated at 200° C. in a twin-screw extruder to obtain a middle layer material.

[0057] Comparative Example 2

[0058] The difference between this comparative example and Example 3 is that 2 parts of DDAB-modified kaolin and 58 parts of ethylene-vinyl alcohol copolymer are extruded and granulated at 200° C. in a twin-screw extruder to obtain a middle-layer material.

[0059] Comparative Example 3

[0060] The difference between this comparative example and Example 3 is that 2 parts of kaolin, 58 parts of ethylene-vinyl alcohol copolymer and 40 parts of polyamide are extruded and granulated at 200° C. in a twin-screw extruder to obtain a middle layer material.

[0061] After the film material is produced, in the above Examples 1 to 10 and Comparative Examples 1 to 3, the water vapor transmission rate test method is: YBB00092003-2015 first method; the oxygen transmission rate test method is: YBB00082003-2015 first method; the carbon dioxide transmission rate test method is: YBB00082003-2015 first method; the heat seal strength test method is: YBB00122003-2015 first method. The properties of the multi-layer co-extruded barrier film are shown in Table 1.

[0062] Table 1 Properties of multilayer coextruded barrier films

[0063]

[0064] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A multi-layer co-extruded barrier film, characterized in that: The structure of the multi-layer co-extruded barrier film is sequentially provided with an outer layer, a sub-outer layer, a middle layer, a sub-inner layer and an inner layer from the outside to the inside; wherein the middle layer is made of a blend of ethylene-vinyl alcohol copolymer, polyamide and DDAB modified kaolin; in parts by weight, the ethylene-vinyl alcohol copolymer accounts for 30 to 70 parts, the polyamide accounts for 10 to 40 parts, and the DDAB modified kaolin accounts for 1 to 5 parts.

2. The multi-layer co-extruded barrier film according to claim 1, characterized in that: The outer layer is made by blending homopolypropylene and cycloolefin copolymer; in parts by weight, the homopolypropylene accounts for 40-70 parts, and the cycloolefin copolymer accounts for 30-60 parts; the melt index of the blend of homopolypropylene and cycloolefin copolymer is 2-6g / 10min.

3. The multi-layer co-extruded barrier film according to claim 1, characterized in that: The sub-outer layer and the sub-inner layer are made of maleic anhydride grafted polypropylene or a blend of maleic anhydride grafted polypropylene and polypropylene; in parts by weight, the polypropylene accounts for 0 to 60 parts, and the maleic anhydride grafted polypropylene accounts for 40 to 100 parts; the melt index of the polypropylene or the blend of polypropylene and maleic anhydride grafted polypropylene is 2 to 8 g / 10 min.

4. The multi-layer co-extruded barrier film according to claim 1, characterized in that: The inner layer is made of a binary / ternary copolymer polypropylene and an elastomer blend; in parts by weight, the binary / ternary copolymer polypropylene accounts for 60-80 parts, and the elastomer accounts for 20-40 parts; the melt index of the binary / ternary copolymer polypropylene and elastomer blend is 1-8g / 10min.

5. The multi-layer co-extruded barrier film according to claim 4, characterized in that: The elastomer includes one or more of styrene-ethylene-butylene-styrene block copolymer, styrene-ethylene-propylene-styrene copolymer and polyolefin elastomer.

6. The multi-layer co-extruded barrier film according to claim 1, characterized in that: The total thickness of the barrier film is 180-200 μm, wherein the outer layer is 10-30 μm thick, the sub-outer layer and the sub-inner layer are both 10-20 μm thick, the middle layer is 100-130 μm thick, and the inner layer is 20-40 μm thick.

7. The multi-layer co-extruded barrier film according to claim 1, characterized in that: The barrier film meets at least one of the following properties: oxygen and carbon dioxide permeability is 0.1 to 0.4 cm 3 / (m 2 ·d), water vapor transmission rate is 0.4~1.0g / (m 2 ·d), heat sealing strength is 45~55N / 15mm.

8. A method for preparing a multi-layer co-extruded barrier film according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: S1, mixing kaolin dispersion with DDAB to modify kaolin to obtain DDAB-modified kaolin; S2, extruding and granulating the DDAB-modified kaolin, ethylene-vinyl alcohol copolymer and polyamide in a twin-screw extruder at a set temperature to obtain a middle-layer material; S3, placing the inner layer material, the sub-inner layer material, the middle layer material, the sub-outer layer material and the outer layer material into the corresponding extruder hoppers of the five-layer co-extrusion film blowing machine respectively for five-layer co-extrusion film blowing, followed by water cooling, shaping, winding and slitting to obtain a barrier film.

9. The method for preparing a multi-layer co-extruded barrier film according to claim 8, characterized in that: The set temperature of the extrusion granulation is 180-240°C.

10. The method for preparing a multi-layer co-extruded barrier film according to claim 8, characterized in that: The extrusion temperature of the outer layer is 190-220°C; the extrusion temperature of the sub-outer layer and the sub-inner layer is 180-220°C; the extrusion temperature of the middle layer is 180-220°C; the extrusion temperature of the inner layer is 190-210°C; and the die head temperature is 180-230°C.

Citation Information

Patent Citations

  • Encapsulated barrier for flexible films and a method of making and using the same

    CN101107120A

  • Kaolin / rubber nano compound material with strengthening and obstructing dual property

    CN101381488A

  • Co-extrusion barrier film as well as preparation method and application thereof

    CN111941980A

  • High-barrier polypropylene composite material and preparation method thereof

    CN115368670A

  • Low temperature high shrinkage and high obstruction membrane and its production process

    CN1810502A

Cited By

  • Soft multi-layer plastic hose as well as preparation method and application thereof

    CN119217797A

  • Cooking-resistant high-transparency high-barrier cycloolefin copolymer film and preparation process thereof

    CN119348264A

  • Multilayer composite barrier film and production process thereof

    CN120363567A

  • Low-temperature polyolefin packaging film and preparation method thereof

    CN120792270A

  • Multifunctional high-barrier multilayer packaging film and preparation method thereof

    CN121590108A