Electrophotographic photoreceptor, electrophotographic device having electrophotographic photoreceptor, and process cartridge

JP2023066793A5Active Publication Date: 2024-10-31CANON KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021177593
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-31
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing electrophotographic photoreceptors with durable surface layers suffer from ghost phenomena due to potential differences between exposed and non-exposed areas, exacerbated by the omission of static elimination processes in simplified processes, and there is a need for a photoreceptor that suppresses ghost images without requiring such processes.

Method used

The photoreceptor incorporates a second hole transport layer with specific hole-transporting compounds having a chain polymerizable functional group, formulated to maintain good electrical properties and durability, where the energy difference in the highest occupied molecular orbitals of these compounds is controlled within a specific range to moderate charge migration and reduce potential fluctuations.

Benefits of technology

This configuration effectively suppresses ghost phenomena and maintains durability, even without static elimination processes, by ensuring proper charge transport and potential uniformity across the photoreceptor surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023066793000001
    Figure 2023066793000001
  • Figure 2023066793000002
    Figure 2023066793000002
  • Figure 2023066793000003
    Figure 2023066793000003
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor with which the occurrence of a ghost is suppressed even when used in an electrophotographic device not having neutralization means, and which has a curable hole transport layer.SOLUTION: Provided is an electrophotographic photoreceptor comprising a support medium, a charge generation layer, a first hole transport layer, and a second hole transport layer, wherein the second hole transport layer contains a hole transportable compound (mass W1, energy value of highest occupied molecular orbital, CTM1HOMO) expressed by formula (1), a hole transportable compound (mass W2) expressed by formula (2) and / or a hole transportable compound (mass W3)(energy value of highest occupied molecular orbital, CTM2HOMO) repressed by formula (3), the value calculated by formula (I) is 0.05 mass% to 5.0 mass% and satisfies formula (II). Formula (I): (W2+W3) / (W1+W2+W3)×100 (mass%), formula (II): 0.05(eV)≤|CTM2HOMO|-|CTM1HOMO|≤0.30(eV).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrophotographic photoreceptor, an electrophotographic apparatus having the electrophotographic photoreceptor, and a process cartridge.

Background Art

[0002] In the surface layer of an electrophotographic photoreceptor, stress due to a series of electrophotographic processes such as charging, exposure, development, transfer, and cleaning is repeatedly applied, so durability and stability are required. As a means for improving durability, a method of containing a curable resin in the surface layer of the electrophotographic photoreceptor can be mentioned. However, when a highly durable surface layer is provided, there is a problem that the potential difference between the exposed portion and the non-exposed portion at the time of the previous image output affects the next image output and may deteriorate the so-called ghost phenomenon that appears as an image density difference. Usually, a countermeasure is taken by providing a discharging process such as light irradiation after each cycle of the electrophotographic process.

[0003] On the other hand, in recent years, there has been a high demand for simplification and cost reduction of electrophotographic apparatus processes, and a design that can omit existing modules and the like is required. For this reason, an electrophotographic photoreceptor that can suppress ghost images without providing a discharging process is demanded. Patent Document 1 describes that the ghost phenomenon is suppressed by devising the material composition of the surface layer of an electrophotographic photoreceptor. However, it is not a configuration for a highly durable electrophotographic photoreceptor containing a curable resin in the surface layer.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] In recent years, there has been a demand not only for increased durability of electrophotographic photoreceptors, but also for technologies that can suppress image defects even in simplified processes. The object of the present invention is to provide an electrophotographic photoreceptor that has a ghosting suppression effect even in a highly durable electrophotographic photoreceptor and also has good electrical properties, as well as an electrophotographic apparatus and process cartridge having the electrophotographic photoreceptor. [Means for solving the problem]

[0006] In other words, according to one aspect of the present invention, In an electrophotographic photoreceptor having a support, a charge generation layer on the support, a first hole transport layer on the charge generation layer, and a second hole transport layer on the first hole transport layer, wherein the second hole transport layer is a surface layer, The second hole transport layer, A hole-transporting compound represented by the following formula (1), At least one hole transport compound selected from the group consisting of hole transport compounds represented by the following formula (2) and hole transport compounds represented by the following formula (3), It contains a copolymer of a composition containing, Let W1 be the mass of the hole-transporting compound represented by the following formula (1) contained in the composition. Let W2 be the mass of the hole-transporting compound represented by the following formula (2) contained in the composition. When the mass of the hole-transporting compound represented by the following formula (3) contained in the composition is denoted as W3, the value calculated by the following formula (I) is between 0.05% by mass and 5.0% by mass. (W2+W3) / (W1+W2+W3)×100(mass%)...Formula (I) and, The energy value of the highest occupied orbital of the hole transporting compound, obtained from the energy calculation using the density functional theory B3LYP / 6-31G* after structural optimization of the hole transporting compound represented by the following formula (1), is defined as CTM1HOMO. When the energy value of the highest occupied molecular orbital of at least one hole transporting compound selected from the group consisting of a hole transporting compound represented by the following formula (2) and a hole transporting compound represented by the following formula (3) obtained by energy calculation by density functional method B3LYP / 6-31G* after structural optimization of the hole transporting compound is defined as CTM2HOMO, the CTM1HOMO and the CTM2HOMO satisfy the following formula (II) an electrophotographic photoreceptor is provided. 0.05 (eV) ≦ |CTM2HOMO| - |CTM1HOMO| ≦ 0.30 (eV) ··· (II)

[0007]

Chemical formula

[0008] (In formula (1), R 11 and R 12 each independently represent an alkylene group having 2 to 5 carbon atoms. R 13 and R 14 each independently represent a hydrogen atom or a methyl group. n 1 is 0 or 1. R 15 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a substituted or unsubstituted phenyl group. x 11 is an integer of 0 to 5. When x 11 is an integer of 2 to 5, x 11 number of R 15 may be the same or different. R 16 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. x 12 is an integer of 0 to 4. When x 12 is an integer of 2 to 4, x 12 number of R 16 may be the same or different.)

[0009]

Chemical formula

[0010] (In formula (2), R 21 and R 22 Each of these independently represents an alkylene group having 2 to 5 carbon atoms. 23 and R 24 Each of these independently represents either a hydrogen atom or a methyl group. 2 It is either 0 or 1. 25 This represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 21 x is an integer between 0 and 5. 21 If x is an integer between 2 and 5, 21 Individual R 25 They may be the same or they may be different. 26 This represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 22 x is an integer between 0 and 4. 22 If x is an integer between 2 and 4, 22 Individual R 26 They may be the same or they may be different.

[0011] [ka]

[0012] (In formula (3), R 31 and R 32 Each of these independently represents an alkylene group having 2 to 5 carbon atoms. 33 and R 34 Each of these independently represents either a hydrogen atom or a methyl group. 3 It is either 0 or 1. 35 This represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 31 x is an integer between 0 and 5. 31 If x is an integer between 2 and 5, 31 Individual R 35 They may be the same or they may be different. 36 This represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 32x is an integer between 0 and 4. 32 If x is an integer between 2 and 4, 32 Individual R 36 They may be the same or they may be different. [Effects of the Invention]

[0013] As described above, the present invention provides an electrophotographic photoreceptor, an electrophotographic apparatus, and a process cartridge having an electrophotographic photoreceptor that have a ghosting effect, good durability, and excellent electrical properties. [Brief explanation of the drawing]

[0014] [Figure 1] This is a schematic diagram showing an example of a process cartridge having an electrophotographic photoreceptor. [Figure 2] This is a schematic diagram showing an example of an electrophotographic apparatus having an electrophotographic photoreceptor. [Figure 3] This is a schematic diagram showing an example of an apparatus for pressure-contact shape transfer processing on the surface of an electrophotographic photoreceptor. [Figure 4] This is a schematic diagram showing an example of a stamper mold used for crimping. [Figure 5] This figure shows the image used in the example to evaluate the ghosting phenomenon. [Figure 6] This figure shows the "halftone image of the 1-dot knight pattern" in Figure 5. [Modes for carrying out the invention]

[0015] The embodiments for carrying out the present invention will be described below with reference to the drawings, but the scope of this disclosure is not limited to these embodiments, and modifications that do not impair the spirit of this disclosure are also included in the present invention. This invention applies when the surface layer of an electrophotographic photoreceptor contains a hole-transporting compound having a chain-polymerizable functional group. To increase the durability of electrophotographic photoreceptors, it is required to use a surface layer with a highly cross-linked structure. Furthermore, in recent years, there has been a demand to reduce and simplify various processes in order to simplify electrophotographic devices.

[0016] In electrophotographic photoreceptors with a cross-linked structure in the surface layer, an interface is formed between the surface and the underlying layer, resulting in incomplete charge transport between layers and the occurrence of ghost images. This problem is usually improved by performing a static elimination process on the photoreceptor after the electrophotographic process is complete, thereby removing the potential difference on the photoreceptor. Typically, the static elimination process is performed by irradiating the entire surface with static elimination light for uniform exposure.

[0017] As described above, due to the recent demand for process simplification, there is a need for electrophotographic photoreceptors that are highly durable yet can suppress the occurrence of ghosting even when the static elimination process is omitted. As a result of diligent research, the inventors discovered that this problem can be improved by including a hole transport compound having specific differences in physical properties, in a specific proportion, in a hole transport compound that has a main chain polymerizable functional group.

[0018] Specifically, the present invention is In an electrophotographic photoreceptor having a support, a charge generation layer on the support, a first hole transport layer on the charge generation layer, and a second hole transport layer on the first hole transport layer, wherein the second hole transport layer is a surface layer, The second hole transport layer, A hole-transporting compound represented by the following formula (1), At least one hole transport compound selected from the group consisting of hole transport compounds represented by the following formula (2) and hole transport compounds represented by the following formula (3), It contains a copolymer of a composition containing [the specified substance].

[0019] Let W1 be the mass of the hole-transporting compound represented by the following formula (1) contained in the composition. Let W2 be the mass of the hole-transporting compound represented by the following formula (2) contained in the composition. When the mass of the hole-transporting compound represented by the following formula (3) contained in the composition is denoted as W3, the value calculated by the following formula (I) is between 0.05% by mass and 5.0% by mass. (W2+W3) / (W1+W2+W3)×100(mass%)...Formula (I) and, Let CTM1HOMO be the energy value of the highest occupied orbital of the hole-transporting compound represented by the following formula (1). When the energy value of the highest occupied orbital of at least one hole transport compound selected from the group consisting of hole transport compounds represented by the following formula (2) and hole transport compounds represented by the following formula (3) is denoted as CTM2HOMO, The CTM1HOMO and the CTM2HOMO satisfy the following equation (II). 0.05(eV)≦|CTM2HOMO|-|CTM1HOMO|≦0.30(eV) ···(II) The energy values ​​of the highest occupied orbitals of the hole-transporting compounds represented by the general formulas (1) to (3) above are all obtained as a result of energy calculations using the density functional theory B3LYP / 6-31G* after structural optimization. As described later, it is preferable that the CTM1HOMO and the CTM2HOMO satisfy the following formula (II)'. 0.15(eV)≦|CTM2HOMO|-|CTM1HOMO|≦0.25(eV) ···(II)'

[0020] [ka] (In formula (1), R 11 and R 12 Each of these independently represents an alkylene group having 2 to 6 carbon atoms. 13 and R 14 Each of these independently represents either a hydrogen atom or a methyl group. 1 It is either 0 or 1. 15This represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 11 x is an integer between 0 and 5. 11 If x is an integer between 2 and 5, 11 Individual R 15 They may be the same or they may be different. 16 This represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 12 x is an integer between 0 and 4. 12 If x is an integer between 2 and 4, 12 Individual R 16 They may be the same or they may be different.

[0021] [ka] (In formula (2), R 21 and R 22 Each of these independently represents an alkylene group having 2 to 6 carbon atoms. 23 and R 24 Each of these independently represents either a hydrogen atom or a methyl group. 2 It is either 0 or 1. 25 This represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 21 x is an integer between 0 and 5. 21 If x is an integer between 2 and 5, 21 Individual R 25 They may be the same or they may be different. 26 This represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 22 x is an integer between 0 and 4. 22 If x is an integer between 2 and 4, 22 Individual R 26 They may be the same or they may be different.

[0022] [ka] (In formula (3), R 31 and R32 each independently represents an alkylene group having 2 to 6 carbon atoms. R 33 and R 34 each independently represents a hydrogen atom or a methyl group. n 3 is 0 or 1. R 35 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. x 31 is an integer from 0 to 5. x 31 When x is an integer from 2 to 5, 31 the x number of R 35 may be the same or different. R 36 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. x 32 is an integer from 0 to 4. x 32 When x is an integer from 2 to 4, 32 the x number of R 36 may be the same or different.)

[0023] The ghost phenomenon that occurs when the charge removal process is not provided is caused by carrying over the surface potential difference of the electrophotographic photoreceptor generated between the exposed portion and the non-exposed portion by the previous process into the next process and outputting it as image density unevenness during the next image output in a series of processes such as exposure - development - transfer, etc.

[0024] When the hole transporting compound existing only on the surface layer side contains, in an appropriate ratio, a substance having a slightly higher energy value of the highest occupied molecular orbital (HOMO) than the main hole transporting compound, as in the present invention, the effects of the present invention are considered to be exhibited. Although the exact mechanism of ghost image suppression is not understood, it is considered as follows. By containing another hole transporting compound having an energy value of the hole transport level slightly higher than that of the main hole transporting compound contained in the surface layer, a moderate delay in hole movement occurs in the second hole transport layer, and the density difference due to potential unevenness is homogenized during development.

[0025] Because of its good compatibility and affinity with the main hole-transporting compound, we believe that the optimal combination is with positional isomers that have the same main skeletal structure but differ in the substitution positions of the substituents. The energy value of the highest occupied orbital in hole-transporting compounds can be calculated using molecular orbital calculations based on the chemical structure. Computational chemistry software such as Gaussian 16 from Gaussian, Inc., or Spartan 16 from WaveFunction, Inc. can be used for these calculations.

[0026] The numerical value can be determined by inputting the structure of the compound to be calculated, performing structural optimization using methods such as semi-empirical molecular orbital methods, and then calculating the energy using density functional theory. The energy value of the highest occupied orbital is preferably in the range of 0.05 (eV) to 0.30 (eV), and more preferably in the range of 0.15 (eV) to 0.25 (eV), compared to that of the main hole-transporting compound. If the difference is too small, the effect of the present invention will be reduced, and if the difference is too large, the hole transport performance will decrease, and the potential fluctuation of the photoreceptor will tend to decrease.

[0027] The configuration of the second charge transport layer according to the present invention can improve the ghosting phenomenon. In the configuration of the second charge transport layer according to the present invention, the amount of hole transporting compounds represented by formulas (2) and (3) is preferably 0.05% to 5.0% by mass. 0.1% to 2.0% by mass is more preferable, and 0.2% to 1.0% by mass is even more preferable. If the amount added is too small, the effects of the present invention will not be easily realized. On the other hand, adding too many charge transporting compounds with different hole transport levels may cause other problems. If there are many substances with different charge transport levels, the charge transport performance will be impaired, and the problem of reduced potential fluctuation during the durable use of the photoreceptor will occur. When the amount is generally greater than 5% by mass, the potential fluctuation in a low-humidity environment will decrease.

[0028] In this invention, a polymerizable functional group refers to a functional group that can form covalent bonds between molecules when a reaction occurs between molecules having polymerizable functional groups. From the viewpoint of improving the film strength and abrasion resistance of the surface layer, acryloyloxy groups and methacryloyloxy groups are suitable as chain polymerizable functional groups. As means of inducing the polymerization reaction of chain polymerizable functional groups, methods can be used to impart energy such as ultraviolet light, electron beams, or heat, or to introduce auxiliary agents such as polymerization initiators, or compounds such as acids, alkalis, or complexes.

[0029] The second hole transport layer can be formed by creating a coating film of a surface layer coating solution containing the charge transport compound of the present invention, and then drying and / or curing this coating film to form the surface layer. As the solvent used for the coating solution for the second hole transport layer, alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, aliphatic halogenated hydrocarbon-based solvents, aliphatic hydrocarbon-based solvents, aromatic hydrocarbon-based solvents, etc., can be used. The thickness of the second hole transport layer is preferably 0.1 μm or more and 15 μm or less.

[0030] Methods for curing the coating film of the surface layer coating liquid (polymerizing the surface layer of the present invention) include polymerization using heat, light (such as ultraviolet light), or radiation (such as electron beams). Among these, radiation is preferred, and electron beams are more preferred. Polymerization using electron beams is preferable because it yields a three-dimensional network structure, improving wear resistance. Furthermore, the polymerization reaction is rapid and efficient, resulting in high productivity. Examples of accelerators used for electron beam irradiation include scanning, electrocurtain, broadbeam, pulsed, and laminar types.

[0031] When using an electron beam, the acceleration voltage of the electron beam is preferably 150kV or less, from the viewpoint of suppressing the degradation of material properties due to the electron beam without impairing polymerization efficiency. Furthermore, the electron beam absorbed dose at the surface of the coating film of the surface layer coating liquid is preferably 1kGy or more and 50kGy or less, and more preferably 5kGy or more and 10kGy or less. Furthermore, when polymerizing the hole transport material of the present invention using an electron beam, it is preferable to irradiate with an electron beam in an inert gas atmosphere and then heat in an inert gas atmosphere in order to suppress polymerization inhibition by oxygen. Examples of inert gases include nitrogen, argon, and helium. Next, the overall configuration of the electrophotographic photoreceptor of the present invention will be described.

[0032] <Electrophotographic photoconductor> A preferred configuration for the electrophotographic photoreceptor in this invention is one in which a charge generation layer, a first hole transport layer, and a second hole transport layer are laminated on a support in this order. A conductive layer or undercoat layer may be provided between the charge generation layer and the support as needed. In this invention, the charge generation layer, the first hole transport layer, and the second hole transport layer are collectively referred to as the photosensitive layer.

[0033] <Support> The support used in this invention is preferably a conductive support made of a conductive material. Examples of support materials include metals or alloys such as iron, copper, gold, silver, aluminum, zinc, titanium, lead, nickel, tin, antimony, indium, chromium, aluminum alloys, and stainless steel. Metal supports or resin supports having a coating formed by vacuum deposition of aluminum, aluminum alloys, indium oxide-tin oxide alloys, etc., can also be used. Supports made by impregnating plastic or paper with conductive particles such as carbon black, tin oxide particles, titanium oxide particles, and silver particles, or supports containing conductive resins, can also be used. Examples of support shapes include cylindrical, belt-shaped, sheet-shaped, or plate-shaped, but cylindrical is the most common.

[0034] The surface of the support may be subjected to treatments such as cutting, roughening, or anodizing, from the viewpoint of suppressing interference fringes caused by the scattering of laser light, improving surface defects of the support, and improving the conductivity of the support. A conductive layer may be provided between the support and the undercoat layer or charge generation layer described later, for the purpose of suppressing interference fringes caused by scattering from lasers, controlling resistance, or covering scratches on the support.

[0035] A conductive layer can be formed by applying a coating solution for a conductive layer, obtained by dispersing carbon black, conductive pigments, electrical resistance-modulating pigments, etc., together with a binder resin, and then drying the resulting coating film. Compounds that cure by heating, ultraviolet irradiation, or radiation irradiation may be added to the coating solution for the conductive layer. Conductive layers formed by dispersing conductive pigments or electrical resistance-modulating pigments tend to have a roughened surface.

[0036] The thickness of the conductive layer is preferably 0.1 μm or more and 50 μm or less, more preferably 0.5 μm or more and 40 μm or less, and even more preferably 1 μm or more and 30 μm or less.

[0037] Examples of binder resins used in conductive layers include: polymers and copolymers of vinyl compounds such as styrene, vinyl acetate, vinyl chloride, acrylic acid esters, methacrylic acid esters, vinylidene fluoride, and trifluoroethylene; polyvinyl alcohol resins; polyvinyl acetal resins; polycarbonate resins; polyester resins; polysulfone resins; polyphenylene oxide resins; polyurethane resins; cellulose resins; phenolic resins; melamine resins; silicon resins; epoxy resins; and isocyanate resins.

[0038] Examples of conductive pigments and electrical resistance modulating pigments include particles of metals (alloys) such as aluminum, zinc, copper, chromium, nickel, silver, and stainless steel, or particles of these metals deposited on the surface of plastic particles. Alternatively, particles of metal oxides such as zinc oxide, titanium oxide, tin oxide, antimony oxide, indium oxide, bismuth oxide, tin-doped indium oxide, and antimony or tantalum-doped tin oxide may also be used. These may be used individually or in combination of two or more types.

[0039] An underlay layer (intermediate layer) may be provided between the support or conductive layer and the charge generation layer for purposes such as improving the adhesion of the charge generation layer, improving hole injection from the support, and protecting the charge generation layer from electrical breakdown. The undercoat can be formed by applying an undercoat coating solution obtained by dissolving a binder resin in a solvent, and then drying the resulting coating film.

[0040] Examples of binder resins used in the undercoat include: polyvinyl alcohol resin, poly-N-vinylimidazole, polyethylene oxide resin, ethylcellulose, ethylene-acrylic acid copolymer, casein, polyamide resin, N-methoxymethylated nylon 6 resin, copolymerized nylon resin, phenolic resin, polyurethane resin, epoxy resin, acrylic resin, melamine resin, or polyester resin.

[0041] The undercoat layer may further contain metal oxide particles. Examples of metal oxide particles include those containing titanium oxide, zinc oxide, tin oxide, zirconium oxide, and aluminum oxide. The metal oxide particles may also be metal oxide particles whose surfaces have been treated with a surface treatment agent such as a silane coupling agent. The thickness of the undercoat layer is preferably 0.05 μm or more and 30 μm or less, and more preferably 1 μm or more and 25 μm or less. The undercoat layer may further contain organic resin fine particles and a leveling agent.

[0042] <Charge generation layer> Next, the charge generation layer will be described. The charge generation layer can be formed by applying a coating solution for the charge generation layer, obtained by dispersing a charge generation material together with a binder resin and a solvent, to form a coating film, and then drying the resulting coating film. Alternatively, the charge generation layer may be a vapor-deposited film of the charge generation material.

[0043] Examples of charge-generating materials used in the charge-generating layer include: azo pigments, phthalocyanine pigments, indigo pigments, perylene pigments, polycyclic quinone pigments, squalylium dyes, pyrylium salts, thiapyrillium salts, triphenylmethane dyes, quinacridone pigments, azulenium salt pigments, cyanine dyes, anthanthrone pigments, pyrantrone pigments, xanthene dyes, quinoneimine dyes, styryl dyes, etc. Only one of these charge-generating materials may be used, or two or more may be used. Among these charge-generating materials, phthalocyanine pigments and azo pigments are preferred from the viewpoint of obtaining excellent sensitivity, and phthalocyanine pigments are particularly preferred.

[0044] Among phthalocyanine pigments, oxytitanium phthalocyanine, chlorogallium phthalocyanine, and hydroxygallium phthalocyanine exhibit particularly excellent charge generation efficiency. Furthermore, among hydroxygallium phthalocyanines, the following hydroxygallium phthalocyanine crystals are more preferable from the viewpoint of obtaining even better sensitivity. A hydroxygallium phthalocyanine crystal with peaks at Bragg angles 2θ of 7.4°±0.3° and 28.2°±0.3° in CuKα characteristic X-ray diffraction.

[0045] Examples of binder resins used in the charge generation layer include: polymers of vinyl compounds such as styrene, vinyl acetate, vinyl chloride, acrylic acid esters, methacrylic acid esters, vinylidene fluoride, and trifluoroethylene; and polyvinyl alcohol resin, polyvinyl acetal resin, polycarbonate resin, polyester resin, polysulfone resin, polyphenylene oxide resin, polyurethane resin, cellulose resin, phenolic resin, melamine resin, silicon resin, epoxy resin, etc.

[0046] The mass ratio of the charge-generating material to the binder resin is preferably in the range of 1:0.3 to 1:4. The thickness of the charge generation layer is preferably 0.05 μm or more and 1 μm or less, and more preferably 0.1 μm or more and 0.5 μm or less.

[0047] <First hole transport layer> Next, the first hole transport layer will be described. The first hole transport layer can be formed by creating a coating film of a hole transport layer coating solution, which is a mixture of a hole transport material and a binder resin in a solvent, and then drying this coating film. The hole transport material and binder resin used in the hole transport layer will be described below.

[0048] Examples of hole-transporting substances include: carbazole compounds, hydrazone compounds, N,N-dialkylaniline compounds, diphenylamine compounds, triphenylamine compounds, triphenylmethane compounds, pyrazoline compounds, styryl compounds, stilbene compounds, etc.

[0049] Examples of binder resins include acrylic acid esters, methacrylic acid esters, polyvinyl alcohol resins, polyvinyl acetal resins, polycarbonate resins, and polyester resins. Curable resins such as curable phenolic resins, curable urethane resins, curable melamine resins, curable epoxy resins, curable acrylic resins, and curable methacrylic resins can also be used.

[0050] Solvents used in the coating solution for the first hole transport layer include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, aliphatic halogenated hydrocarbon-based solvents, and aromatic hydrocarbon-based solvents. The thickness of the first hole transport layer is preferably 1 μm or more and 100 μm or less, more preferably 3 μm or more and 50 μm or less, and even more preferably 5 μm or more and 40 μm or less.

[0051] Various additives can be added to each layer of the electrophotographic photoreceptor of the present invention. Specifically, these include organic pigments, organic dyes, coating surface modifiers, electron transport agents, oils, waxes, antioxidants, light absorbers, polymerization initiators, radical deactivators, organic resin fine particles, and inorganic particles. The surface of each layer of the electrophotographic photoreceptor may be treated using abrasive sheets, shape transfer materials, glass beads, zirconia beads, etc. Alternatively, irregularities may be formed on the surface using the constituent materials of the coating solution.

[0052] When applying the coating solution for each of the above layers, any known coating method can be used, such as immersion coating, spray coating, circular volume control (ring) coating, spin coating, roller coating, Meyer bar coating, or blade coating. Next, a process cartridge equipped with the electrophotographic photoreceptor of the present invention and an image forming process will be described.

[0053] <Process cartridges and image forming processes> Figure 1 shows an example of the configuration of a process cartridge. In Figure 1, the cylindrical electrophotographic photoreceptor 1 is driven to rotate at a predetermined peripheral speed in the direction of the arrow. The peripheral surface of the rotating electrophotographic photoreceptor 1 is uniformly charged to a predetermined positive or negative potential by the charging means 2. Next, the charged peripheral surface of the electrophotographic photoreceptor 1 receives exposure light (image exposure light) 3 output from an exposure means (not shown), such as slit exposure or laser beam scanning exposure. In this way, an electrostatic latent image corresponding to the desired image is sequentially formed on the peripheral surface of the electrophotographic photoreceptor 1. The voltage applied to the charging means (charging roller, etc.) 2 may be either a voltage with an AC component superimposed on a DC component, or a voltage with only a DC component.

[0054] The electrostatic latent image formed on the circumferential surface of the electrophotographic photoreceptor 1 is developed by the toner contained in the developer of the developing means 4 to form a toner image. Next, the toner image formed and supported on the circumferential surface of the electrophotographic photoreceptor 1 is sequentially transferred to the transfer material (paper, intermediate transfer material, etc.) 6 by the transfer bias from the transfer means (transfer roller, etc.) 5. The transfer material 6 is fed in synchronization with the rotation of the electrophotographic photoreceptor 1.

[0055] After toner image transfer, the surface of the electrophotographic photoreceptor 1 is treated to remove static electricity by pre-exposure light 7 from a pre-exposure means (not shown), and then cleaned by a cleaning means 8 to remove any remaining toner. The electrophotographic photoreceptor 1 is then repeatedly used for image formation. The pre-exposure means may be performed before or after the cleaning process. In the process cartridge according to the present invention, a pre-exposure means is not required.

[0056] The electrophotographic photoreceptor 1 may be mounted in an electrophotographic device such as a copier or a laser beam printer. Alternatively, a process cartridge 9 may be constructed by housing and supporting multiple components, such as the electrophotographic photoreceptor 1, charging means 2, developing means 4, and cleaning means 8, in a container, and making it detachable from the electrophotographic device body. In Figure 1, the electrophotographic photoreceptor 1, charging means 2, developing means 4, and cleaning means 8 are supported as a single unit, forming a process cartridge 9 that is detachable from the electrophotographic device body. Next, an electrophotographic apparatus equipped with the electrophotographic photoreceptor of the present invention will be described.

[0057] Figure 2 shows an example of the configuration of the electrophotographic apparatus of the present invention. A process cartridge 17 for yellow, a process cartridge 18 for magenta, a process cartridge 19 for cyan, and a process cartridge 20 for black are arranged side by side along an intermediate transfer body 10. As shown in Figure 2, the diameter of the electrophotographic photoreceptor, its constituent materials, developer, charging method, and other means do not necessarily have to be the same for each color. For example, in the electrophotographic apparatus of Figure 2, the diameter of the electrophotographic photoreceptor is larger for black than for the color (yellow, magenta, cyan). Also, while the charging method for the color colors is one in which a voltage with an AC component superimposed on a DC component is applied, the charging method for black uses corona discharge.

[0058] When the image formation operation begins, toner images of each color are sequentially superimposed on the intermediate transfer body 10 according to the image formation process described above. In parallel, the transfer paper 11 is fed from the paper tray 13, transported along the paper feed path 12, and fed to the secondary transfer means 14 in time with the rotation of the intermediate transfer body. The toner image on the intermediate transfer body 10 is transferred to the transfer paper 11 by the transfer bias from the secondary transfer means 14. The toner image transferred onto the transfer paper 11 is transported along the paper feed path 12, fixed onto the transfer paper by the fixing means 15, and then discharged from the paper discharge unit 16.

[0059] Next, examples of hole-transporting compounds having the chain-polymerizable functional group of the present invention represented by formula (1) are shown below. However, the examples below are not limited to these.

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] Furthermore, examples of compounds represented by formula (2) are shown below. However, the examples are not limited to those shown below.

[0065] [ka]

[0066] [ka]

[0067] [ka]

[0068] [ka] Furthermore, examples of compounds represented by formula (3) are shown below. However, the examples are not limited to those shown below.

[0069] [ka]

[0070] [ka]

[0071] [ka]

[0072] [ka]

[0073] Typical synthesis examples of hole-transporting compounds used in the present invention are shown below. <Synthesis Example 1> The following are examples of the synthesis of hole-transporting compounds having a bifunctional polymerizable acrylic group, as represented by example compounds No. 2-3, as shown in formula (2).

[0074] [ka]

[0075] Triarylamine compounds were synthesized using the iodine compound and amine compound shown in reaction formula (1). In a reaction vessel, 47.9 parts of the iodine compound, 36.0 parts of the amine compound from the formula, and 60 parts of o-dichlorobenzene were mixed. 18.4 parts of potassium carbonate and 9.2 parts of copper powder were added, and the reaction was carried out at an internal temperature of approximately 210°C. The reaction was stirred for approximately 16 hours. After the reaction, the mixture was filtered, washed with toluene, and concentrated to obtain the crude product.

[0076] [ka]

[0077] Next, the obtained intermediate was hydrolyzed to convert the acetate ester to a hydroxyl group. 75 parts tetrahydrofuran, 75 parts methanol, and 55 parts 24% sodium hydroxide aqueous solution were mixed and heated to an internal temperature of 60°C, stirred, and reacted for 1 hour to carry out hydrolysis. After the reaction, the reaction mixture was extracted with ethyl acetate, and the organic layer was washed with water, washed with brine, dehydrated, and concentrated. The mixture was purified by silica gel chromatography to obtain the dihydroxy intermediate. Yield: 30.5 parts, Yield (2-step): 64.5%

[0078] [ka]

[0079] 30 parts of the dihydroxy intermediate obtained by the above reaction, 340 parts of toluene, and 0.6 parts of 4-methoxyphenol were mixed, and 13.3 parts of acrylic acid were added to the reaction vessel. 1.3 parts of p-toluenesulfonic acid monohydrate were added, and the mixture was heated at 112°C under reflux conditions for 6 hours to carry out the acrylication reaction. After the reaction, the mixture was cooled, neutralized with a 10% sodium hydroxide aqueous solution, and extracted with ethyl acetate. The mixture was then washed with water, dehydrated, and concentrated to obtain the crude product.

[0080] Next, the crude product was purified by silica gel column chromatography to obtain a hole-transporting compound having polymerizable functional groups. Yield: 31.0 parts, yield 80.9% Furthermore, varnishes were obtained by adjusting the solvent type and amount of the resulting hole-transporting compound. Similarly, other hole-transporting compounds represented by formulas (2) and (3) can be synthesized. [Examples]

[0081] The present invention will be described in more detail below with reference to specific examples. In the examples, "part" refers to "part by mass." Also, the electrophotographic photoreceptor will be simply referred to as "photoreceptor" below. <Fabrication of electrophotographic photoreceptors>

[0082] [Example 1] A cylindrical aluminum cylinder with an outer diameter of 30.0 mm, a length of 357.5 mm, and a wall thickness of 0.7 mm was used as the support (conductive support). Next, zinc oxide particles (specific surface area: 19 m²) 2 / g, powder resistivity: 4.7×10 6 Ten parts of (Ω·cm) were mixed with fifty parts of toluene and stirred. 0.08 parts of a silane coupling agent were added, and the mixture was stirred for 6 hours. The toluene was then removed by distillation under reduced pressure, and the mixture was heated and dried at 130°C for 6 hours to obtain surface-treated zinc oxide particles. N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (trade name: KBM602, manufactured by Shin-Etsu Chemical Co., Ltd.) was used as the silane coupling agent.

[0083] Next, 15 parts of polyvinyl butyral resin (weight-average molecular weight: 40,000, trade name: BM-1, manufactured by Sekisui Chemical Co., Ltd.) and 15 parts of blocked isocyanate (trade name: Duranate TPA-B80E, manufactured by Asahi Kasei Chemicals Corporation) were prepared. These were dissolved in a mixed solution of 73.5 parts methyl ethyl ketone and 73.5 parts 1-butanol. To this solution, 80.8 parts of the surface-treated zinc oxide particles and 0.8 parts of 2,3,4-trihydroxybenzophenone (manufactured by Wako Pure Chemical Industries, Ltd.) were added, and the mixture was dispersed for 3 hours in a sand mill apparatus using glass beads with a diameter of 0.8 mm at an atmosphere of 23±3°C. After dispersion, the following materials were added and stirred to prepare the coating solution for the undercoat layer. Silicone oil (product name: SH28PA, manufactured by Toray Dow Corning Co., Ltd.) 0.01 part Cross-linked polymethyl methacrylate (PMMA) particles (product name: TECHPOLYMER SSX-102, manufactured by Sekisui Chemical Co., Ltd., average primary particle size 2.5 μm) 5.6 parts

[0084] This undercoating solution for the undercoat was applied to the support by immersion to form a coating film, and the resulting coating film was dried at 160°C for 40 minutes to form an undercoat with a thickness of 18 μm. Next, two parts of hydroxygallium phthalocyanine crystals (charge-generating material) in a crystalline form having peaks at 7.4° and 28.2° of the Bragg angle 2θ±0.2 in CuKα characteristic X-ray diffraction were prepared. Furthermore, 0.02 parts of a calixarene compound represented by the following formula (A), 1 part of polyvinyl butyral (trade name: S-Rec BX-1, manufactured by Sekisui Chemical Co., Ltd.), and 60 parts of cyclohexanone were prepared. These were placed in a sand mill using 1 mm diameter glass beads and dispersed for 4 hours. After that, 70 parts of ethyl acetate were added to prepare a coating solution for the charge-generating layer. This coating solution for the charge-generating layer was immersion coated onto the undercoat layer, and the resulting coating film was dried at 90°C for 15 minutes to form a charge-generating layer with a thickness of 0.18 μm.

[0085] [ka]

[0086] Next, the following materials were prepared to form the first hole transport layer. • 6 parts of the compound represented by the following formula (B) • Three parts of the compound represented by the following formula (C) • One part of the compound represented by the following formula (D) • Bisphenol Z-type polycarbonate resin (product name: Yupiron Z400, manufactured by Mitsubishi Engineering Plastics Corporation) 10 parts

[0087] A coating solution for the charge transport layer was prepared by dissolving these in a mixed solvent consisting of 35 parts o-xylene, 35 parts dimethoxymethane, and 30 parts methyl benzoate. This coating solution for the charge transport layer was applied to the charge generating layer by immersion, and the resulting coating film was dried at 110°C for 50 minutes to form a charge transport layer with a thickness of 18 μm.

[0088] [ka]

[0089] <Formation of the second hole transport layer> 1.5 parts of a fluorine atom-containing acrylic resin having repeating structural units represented by the following formula (F1) and repeating structural units represented by the following formula (F2) (weight-average molecular weight: 83,000, copolymerization ratio (F1) / (F2) = 1 / 1 (molar ratio))

[0090] [ka] It was dissolved in a mixed solvent of 45 parts 1-propanol and 45 parts Zeolora® H (manufactured by Nippon Zeon Co., Ltd.). Then, 30 parts of fluoroethylene resin powder (product name: Lebron L-2, manufactured by Daikin Industries, Ltd.) were added and dispersed using a high-pressure disperser (product name: Microfluidizer M-110EH, manufactured by Microfluidics, Inc., USA) to obtain a fluoroethylene resin dispersion.

[0091] Next, the following materials were stirred and uniformly dispersed to prepare a protective coating solution. 9.90 parts of hole-transporting compounds represented by example compounds No. 1-3 Compounds shown as example compounds No. 2-3: 0.08 parts Compound No. 3-3 (example compound): 0.02 parts 16.60 parts of the aforementioned fluoroethylene resin dispersion. 1-Propanol 7.20 parts Zeolora H (cyclic HFC c-C5F7H3) 7.20 parts

[0092] This protective coating solution was applied to the charge transport layer by immersion, the resulting coating film was dried at 50°C for 10 minutes, and polymerization curing treatment was performed by electron beam irradiation and heating under the following conditions. In an atmosphere with an oxygen concentration of 50 ppm or less, an aluminum cylinder was rotated at a speed of 300 rpm while being irradiated with an electron beam using an electron beam irradiation device under the following conditions: irradiation distance of 30 mm, acceleration voltage of 70 kV, beam current of 8 mA, and irradiation time of 3.0 seconds. After electron beam irradiation, the oxygen concentration was maintained at 50 ppm or less, and the surface of the protective coating was allowed to reach 135°C over 24 seconds.

[0093] Next, the aluminum cylinder was removed to an atmospheric environment and heated at 100°C for a further 12 minutes to form a protective layer with a thickness of 5 μm. The energy value of the highest occupied orbital of the hole-transport compound used in the second charge transport layer was calculated as follows.

[0094] WaveFunction's Spartan 16 was used as the computational chemistry application. After inputting the chemical structure and adjusting the conformation, structural optimization was performed using the semi-empirical molecular orbital method (PM3). Next, the energy values ​​were calculated by density functional theory for each molecular structure. B3LYP 6-31G* was used as the basis set. When the second hole transport layer of the present invention contains two or more hole transport compounds represented by formulas (2) and (3), the values ​​were determined by performing a weighted average of the individual physical properties of each compound, taking into account the mass ratio of the materials used. The calculated energy values ​​are shown in Table 1.

[0095] Next, a mold was placed in the pressure-welding shape transfer processing apparatus, and surface processing was performed on the electrophotographic photoreceptor before the recess was formed. Figure 3 is a schematic diagram showing an example of an apparatus for pressure-contact shape transfer processing on the surface of an electrophotographic photoreceptor. As shown in Figure 3, the device includes a mold 22, a pressurizing member 23, and a support member 24. Figure 4 shows the molds used in the examples and comparative examples. The mold shown in Figure 4 was placed in the pressure-contact shape transfer processing apparatus shown in Figure 3, and surface processing was performed on the electrophotographic photoreceptor 21 before the formation of the recesses. Figure 4(a) is a top view showing a schematic of the mold. Figure 4(b) is a schematic cross-sectional view of the electrophotographic photoreceptor 21 in the axial direction of the protrusion of the mold (cross-sectional view in the SS' section of Figure 4(a)). Figure 4(c) is a cross-sectional view of the electrophotographic photoreceptor 21 in the circumferential direction of the protrusion of the mold (cross-sectional view in the T-T' section of Figure 4(a)).

[0096] The mold shown in Figure 4 has a protrusion with a maximum width X: 50 μm, a maximum length Y: 75 μm, an area ratio of 56%, and a height H: 4 μm. The maximum width X is the maximum width in the axial direction of the electrophotographic photoreceptor 21 when the protrusions on the mold are viewed from above. The maximum length Y is the maximum circumferential length of the electrophotographic photoreceptor 21 when the protrusions on the mold are viewed from above. Area ratio refers to the ratio of the area of ​​the protrusions to the total surface area when the mold is viewed from above. During processing, the temperatures of the electrophotographic photoreceptor 21 and the mold were controlled so that the surface temperature of the electrophotographic photoreceptor 21 reached 120°C. Then, while pressing the electrophotographic photoreceptor 21 against the mold at a pressure of 7.0 MPa, the electrophotographic photoreceptor 21 was rotated in the circumferential direction to form recesses across the entire surface layer (circumferential surface) of the electrophotographic photoreceptor 21. In this way, the electrophotographic photoreceptor 21 was manufactured.

[0097] The surface of the obtained electrophotographic photoreceptor 21 was observed using a laser microscope (product name: X-100, manufactured by Keyence Corporation) with a 50x lens to observe the recesses on the surface of the electrophotographic photoreceptor 21. During observation, adjustments were made to ensure that the electrophotographic photoreceptor 21 was not tilted in the longitudinal direction, and that the focus was on the vertices of the arcs of the electrophotographic photoreceptor 21 in the circumferential direction. The magnified images were stitched together using an image stitching application to obtain a square area with sides of 500 μm. The obtained results were then filtered using the included image analysis software, selecting the image processing height data and filtering with the filter type median.

[0098] Based on the observations described above, the depth of the recess is 2 μm, the axial width of the opening is 50 μm, the circumferential length of the opening is 75 μm, and the area is 140,000 μm. 2 This was the case. The area refers to the area of ​​the recesses when the surface of the electrophotographic photoreceptor 21 is viewed from above, and represents the total area of ​​the openings of the recesses. The photoreceptor according to Example 1 was prepared in the manner described above.

[0099] [Examples 2-17] Instead of the hole-transporting compound used in Example 1, a protective coating solution was prepared using the materials shown in Table 1A, in the same manner as in Example 1. Otherwise, the photoreceptor was prepared in the same manner as in Example 1.

[0100] [Example 18] A protective coating solution was prepared in the same manner as in Example 1, using the materials shown in Table 1A and 2.5 parts of a polymerizable compound that does not possess hole-transporting properties, represented by formula (G) below, instead of the hole-transporting compound used in Example 1. Otherwise, a photoreceptor was prepared in the same manner as in Example 1.

[0101] [ka]

[0102] [Examples 19-27] Instead of the hole-transporting compound used in Example 1, a protective coating solution was prepared in the same manner as in Example 1, using the materials shown in Table 1A and 2.5 parts of a polymerizable compound that does not possess hole-transporting properties, represented by formula (G). Otherwise, a photoreceptor was prepared in the same manner as in Example 1.

[0103] [Example 28] In place of the hole transport compound used in Example 1, In addition to 6.93 parts of the hole-transporting compound represented by example compound No. 1-3, 0.056 parts of the compound represented by example compound No. 2-3, and 0.014 parts of the compound represented by example compound No. 3-3, Using 2.97 parts of the hole-transporting compound represented by example compounds No. 1-12, 0.024 parts of the compound represented by example compound No. 2-12, and 0.006 parts of the compound represented by example compound No. 3-12, A protective coating solution was prepared in the same manner as in Example 1. Otherwise, the photoreceptor was prepared in the same manner as in Example 1.

[0104] [Comparative Examples 1, 3, 5] A photoreceptor was prepared in the same manner as in Example 1, except that the hole-transporting compound used in Example 1 was replaced with the example compounds shown in Table 1, represented by formula (1).

[0105] [Comparative Examples 2, 4, 6] Instead of the hole-transporting compound used in Example 1, a protective coating solution was prepared in the same manner as in Example 1, using 9.90 parts of the exemplary compound represented by formula (1) and 0.10 parts of the exemplary compound represented by formula (2), as shown in Table 1. Otherwise, a photoreceptor was prepared in the same manner as in Example 1.

[0106] [Comparative Examples 7, 9, 11] Instead of the hole-transporting compound used in Example 1, a protective coating solution was prepared in the same manner as in Example 1, using 7.50 parts of the exemplary compound represented by formula (1) shown in Table 1, and 2.5 parts of the polymerizable compound that does not possess hole-transporting properties, represented by formula (G). Otherwise, the photoreceptor was prepared in the same manner as in Example 1.

[0107] [Comparative Examples 8, 10, 12] Instead of the hole-transporting compound used in Example 1, protective coating solutions were prepared in the same manner as in Example 1, using the materials listed in Table 1 below. Otherwise, the photoreceptor was prepared in the same manner as in Example 1. 7.0125 parts of the exemplary compound represented by formula (1) above. 0.4875 parts of the exemplary compound represented by formula (2) above 2.5 parts of a polymerizable compound that does not possess hole transport properties, represented by formula (G) above.

[0108] <Evaluation of the effect of suppressing ghosting phenomena> The ghost images were evaluated using the fabricated example photoreceptors 1-28 and comparative example photoreceptors 1-12 as follows. A modified Canon iR-ADVC5560 copier was used as the electrophotographic apparatus. The static elimination light was disabled during image output. The manufactured electrophotographic photoreceptor was mounted in the black process cartridge, and this process cartridge was then mounted in the black process cartridge station to output the image.

[0109] The evaluation was conducted under conditions of 23°C and 50% relative humidity. First, 5,000 full-color images (text images with 1% print density for each color) were printed on A4 size plain paper. Then, images were printed sequentially in the following order: one solid white image, five images for ghosting evaluation, one solid black image, and five images for ghosting evaluation.

[0110] As shown in Figure 5, the image used for evaluating the ghosting phenomenon was created by first outputting a square "solid image 52" within a "white image 51" at the beginning of the image, and then creating a "halftone image 53 of a 1-dot knight's mahjong pattern" as shown in Figure 6. In Figure 5, the "ghost area 54" is the part where the ghosting phenomenon caused by the "solid image 52" may appear. The ghosting phenomenon was evaluated by measuring the density difference between the image density of the halftone image of a 1-dot knight pattern and the image density of the ghosted area. Using a spectrophotometer (product name: X-Rite504 / 508, manufactured by X-Rite), the density difference was measured at 10 points in one image used for ghosting phenomenon evaluation. This procedure was performed for all 10 images used for ghosting phenomenon evaluation, and the average value of the total 100 points was calculated to evaluate the Macbeth density difference. The evaluation results are shown in Table 2.

[0111] <Evaluation: Evaluation of potential fluctuations during repeated use in low-temperature, low-humidity environments> Using the photoreceptors described in Examples 1-28 and Comparative Examples 1-12, the potential fluctuations during repeated use of the photoreceptors in a low-temperature, low-humidity environment were evaluated under the following conditions. A modified Canon iR-ADVC5560 copier was used as the electrophotographic apparatus. The modifications included adjusting the potential transferred to the photoreceptor from the charging roller and the image exposure laser power. The electrophotographic apparatus and electrophotographic photoreceptor were left undisturbed for more than 48 hours in a low-temperature, low-humidity environment of 15°C and 10% relative humidity, after which the electrophotographic photoreceptor was mounted in the cyan cartridge of the electrophotographic apparatus.

[0112] The surface potential of the electrophotographic photoreceptor was measured by removing the developing cartridge from the evaluation device and inserting a potential measuring device in its place. The potential measuring device is configured to position a potential measuring probe at the developing position of the developing cartridge. The position of the potential measuring probe relative to the electrophotographic photoreceptor was at the axial center of the cylindrical electrophotographic photoreceptor, with a gap of 3 mm from the surface of the electrophotographic photoreceptor.

[0113] The AC component of the charging roller was set to 1500 Vpp and 1500 Hz, and the initial dark area potential (VDa) was adjusted to -700 V. Then, the initial bright area potential (VLa) before endurance was adjusted to -200 V by laser exposure, and the set values ​​were recorded. These operations were performed similarly for each electrophotographic photoreceptor being evaluated. A band image with an image density of 1% was printed, and 1000 sheets were fed through the paper continuously. After the endurance test, the potential of the bright areas (VLb) after 1000 sheets was measured immediately using the potential measuring device described above. Then, the amount of change between the initial light area potential (VLa) before paper passing and the light area potential (VLb) after paper passing was confirmed, and this was defined as the light area potential fluctuation ΔVL(ab). The results are shown in Table 2.

[0114] [Table 1A]

[0115] [Table 1B]

[0116] [Table 2A]

[0117] [Table 2B] [Explanation of Symbols]

[0118] 1...Electrophotographic photoreceptor 2. Charging means 3‥‥Exposure light 4. Development methods 5. Transfer method 6. Transfer material 7...Previous exposure light 8. Cleaning methods 9... Process cartridge 10...Intermediate transfer material 11...Transfer paper 12... Paper feed path 13... Paper feed tray 14. Secondary transfer means 15... Fixing means 16... Paper output section 17... Process cartridge for yellow 18... Process cartridge for magenta 19... Process cartridge for cyan 20... Process cartridge for black color

Claims

1. An electrophotographic photoreceptor having a support, a charge generating layer on the support, a first hole transport layer on the charge generating layer, and a second hole transport layer on the first hole transport layer, the second hole transport layer being a surface layer, the second hole transport layer comprising: A hole transporting compound represented by the following formula (1): At least one hole transport compound selected from the group consisting of a hole transport compound represented by the following formula (2) and a hole transport compound represented by the following formula (3), The composition contains a copolymer of The mass of the hole transport compound represented by the following formula (1) contained in the composition is represented by W1: The mass of the hole transport compound represented by the following formula (2) contained in the composition is represented by W2: When the mass of the hole transport compound represented by the following formula (3) contained in the composition is W3, The value calculated by the following formula (I) is 0.05% by mass to 5.0% by mass, (W2+W3) / (W1+W2+W3)×100 (mass%)...(I) and, The energy value of the highest occupied molecular orbital of a hole transport compound represented by the following formula (1), which is obtained as a result of energy calculation by the density functional method B3LYP / 6-31G* after structural optimization of the hole transport compound, is defined as CTM1HOMO, When the energy value of the highest occupied molecular orbital of at least one hole transport compound selected from the group consisting of hole transport compounds represented by the following formula (2) and hole transport compounds represented by the following formula (3) after structural optimization is obtained as a result of energy calculation by the density functional method B3LYP / 6-31G*, the energy value of the highest occupied molecular orbital of the hole transport compound is defined as CTM2HOMO: The CTM1HOMO and the CTM2HOMO satisfy the following formula (II):

1. An electrophotographic photoreceptor comprising: 0.05 (eV)≦|CTM2HOMO|-|CTM1HOMO|≦0.30 (eV) ... (II) [Case 1] (In formula (1), R 11 and R 12 R each independently represents an alkylene group having 2 to 6 carbon atoms. 13 and R 14 Each of n independently represents a hydrogen atom or a methyl group. 1 is 0 or 1. 15 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 11 is an integer from 0 to 5. 11 When x is an integer from 2 to 5, 11 R 15 may be the same or different. 16 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. x 12 is an integer from 0 to 4. 12 When x is an integer from 2 to 4, 12 R 16 may be the same or different.) [chemical 2] (In formula (2), R 21 and R 22 R each independently represents an alkylene group having 2 to 6 carbon atoms. 23 and R 24 Each of n independently represents a hydrogen atom or a methyl group. 2 is 0 or 1. 25 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 21 is an integer from 0 to 5. 21 When x is an integer from 2 to 5, 21 R 25 may be the same or different. 26 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. x 22 is an integer from 0 to 4. 22 When x is an integer from 2 to 4, 22 R 26may be the same or different.) [C3] (In formula (3), R 31 and R 32 R each independently represents an alkylene group having 2 to 6 carbon atoms. 33 and R 34 Each of n independently represents a hydrogen atom or a methyl group. 3 is 0 or 1. 35 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 31 is an integer from 0 to 5. 31 When x is an integer from 2 to 5, 31 R 35 may be the same or different. 36 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 32 is an integer from 0 to 4. 32 When x is an integer from 2 to 4, 32 R 36 may be the same or different.)

2. 2. The electrophotographic photoreceptor according to claim 1, wherein the CTM1HOMO and the CTM2HOMO satisfy the following formula (II)': 0.15 (eV)≦|CTM2HOMO|-|CTM1HOMO|≦0.25 (eV) ... (II)'

3. 3. The electrophotographic photoreceptor according to claim 1, wherein the value calculated by the formula (I) is from 0.1% by mass to 2.0% by mass.

4. The electrophotographic photoreceptor according to claim 3, wherein the value calculated by the formula (I) is from 0.2% by mass to 1.0% by mass.

5. In the formula (1), n 1 is 1, and n in the formula (2) 2 is 1, and n in the formula (3) 35. The electrophotographic photoreceptor according to claim 1, wherein R is 1.

6. An electrophotographic photoreceptor described in any one of claims 1 to 5, wherein in formula (1), R 11 and R 12 are each independently an alkylene group having 2 to 5 carbon atoms, in formula (2), R 21 and R 22 are each independently an alkylene group having 2 to 5 carbon atoms, and in formula (3), R 31 and R 32 are each independently an alkylene group having 2 to 5 carbon atoms.

7. 7. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging means, an exposing means, a developing means and a transferring means.

8. 7. A process cartridge which integrally supports the electrophotographic photosensitive member according to claim 1 and at least one means selected from the group consisting of a charging means, a developing means, a transfer means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

9. A method for producing an electrophotographic photoreceptor comprising: a support; a charge generating layer on the support; a first hole transport layer on the charge generating layer; and a second hole transport layer on the first hole transport layer, the second hole transport layer being a surface layer, the method comprising the steps of: The manufacturing method comprises: forming a coating film of the coating liquid for the second hole transport layer, the coating film containing a hole transport compound represented by the following formula (1) and at least one hole transport compound selected from the group consisting of a hole transport compound represented by the following formula (2) and a hole transport compound represented by the following formula (3); copolymerizing the composition contained in the coating to form the second hole transport layer of the electrophotographic photoreceptor. having The second hole transport layer coating liquid contains The mass of the hole transport compound represented by the following formula (1) is W1: The mass of the hole transport compound represented by the following formula (2) is W2, When the mass of the hole transport compound represented by the following formula (3) is W3, The value calculated by the following formula (I) is 0.05% by mass to 5.0% by mass, (W2+W3) / (W1+W2+W3)×100 (mass%)...Formula (I) and, The energy value of the highest occupied molecular orbital of a hole transport compound represented by the following formula (1), which is obtained as a result of energy calculation by the density functional method B3LYP / 6-31G* after structural optimization of the hole transport compound, is defined as CTM1HOMO, When the energy value of the highest occupied molecular orbital of at least one hole transport compound selected from the group consisting of hole transport compounds represented by the following formula (2) and hole transport compounds represented by the following formula (3) after structural optimization is obtained as a result of energy calculation by the density functional method B3LYP / 6-31G*, the energy value of the highest occupied molecular orbital of the hole transport compound is defined as CTM2HOMO: The method for producing an electrophotographic photoreceptor, wherein the CTM1HOMO and the CTM2HOMO satisfy the following formula (II): 0.05 (eV)≦|CTM2HOMO|-|CTM1HOMO|≦0.30 (eV) ... (II) [C4] (In formula (1), R 11 and R 12 R each independently represents an alkylene group having 2 to 6 carbon atoms. 13 and R 14 Each of n independently represents a hydrogen atom or a methyl group. 1 is 0 or 1. 15 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 11 is an integer from 0 to 5. 11 When x is an integer from 2 to 5, 11 R 15 may be the same or different. 16 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. x 12 is an integer from 0 to 4. 12 When x is an integer from 2 to 4, 12 R 16 teeth, They may be the same or different.) [C5] (In formula (2), R 21 and R 22 R each independently represents an alkylene group having 2 to 6 carbon atoms. 23 and R 24 Each of n independently represents a hydrogen atom or a methyl group. 2 is 0 or 1. 25 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 21 is an integer from 0 to 5. 21 When x is an integer from 2 to 5, 21 R 25 may be the same or different. 26 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. x 22 is an integer from 0 to 4. 22 When x is an integer from 2 to 4, 22 R 26 may be the same or different.) [C6] (In formula (3), R 31 and R 32 R each independently represents an alkylene group having 2 to 6 carbon atoms. 33 and R 34 Each of n independently represents a hydrogen atom or a methyl group. 3 is 0 or 1. 35 represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a substituted or unsubstituted phenyl group. 31 is an integer from 0 to 5. 31 When x is an integer from 2 to 5, 31 R 35 may be the same or different. 36 represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 32 is an integer from 0 to 4. 32 When x is an integer from 2 to 4, 32 R 36 teeth, They may be the same or different.)