Metallic ink for inkjet and inkjet recording method
Patent Information
- Application Number
- JP2021191254
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Existing inkjet metallic inks using flat metal particles face issues with nozzle clogging and insufficient adhesion to substrates, leading to unstable ejection and poor abrasion resistance of printed images.
A metallic ink formulation containing flat metal particles with a volume-based median diameter less than 500 nm and a thickness of 50 nm or less, along with resin particles, where the volume-based median diameter ratio of metal to resin particles is 4.0 or more, ensuring stable ejection and improved adhesion.
The ink enables stable ejection of flat metal particles, enhances adhesion to substrates, and improves the abrasion resistance of printed images, maintaining sufficient metallic luster.
Abstract
Description
[Technical Field]
[0001] The present invention relates to an inkjet metallic ink and an inkjet recording method using the ink. [Background technology]
[0002] Conventionally, inks containing metallic pigments such as brass, aluminum, and silver have been used to form images with a metallic luster on printed materials such as packages, labels, and photographs. Analog printing techniques such as offset printing, screen printing, and gravure printing have been used to form such images. Additionally, foil stamping using metal foil is also known.
[0003] In recent years, with the development of digital printing technology, inkjet printing methods have been proposed for forming images with metallic luster. Furthermore, from the viewpoint of environmental friendliness and safety for humans, inkjet printing methods have been developed to use aqueous inks containing only small amounts of organic solvents.
[0004] In the analog printing technology described above, aluminum pigments, which have a flat shape, have been used as one of the pigments that can express metallic luster. Patent Document 1 is an example of the application of a tabular aluminum pigment to an inkjet recording method. Patent Document 1 aims to provide a high metallic mirror gloss, with specular gloss values at 20 degrees, 60 degrees, and 85 degrees of 200 or more, 200 or more, and 100 or more, respectively. To achieve this, the ink uses a pigment dispersion in which, when the major axis of the flat surface of the tabular metal particles is X, the minor axis is Y, and the thickness is Z, the 50% average particle diameter R50 of the equivalent circle diameter calculated from the area of the particles in the XY plane is 0.5 to 3 μm, and R50 / Z>5 is satisfied. On the other hand, for inkjet metallic ink, a representative digital printing technology, examples have been proposed in which granular metal nanoparticles, particularly silver nanoparticles, are prepared and used for printing in order to eject the ink from fine nozzles.
[0005] Metal nanoparticles do not provide sufficient adhesion to substrates (also known as recording media), especially non-absorbent substrates, so binder resins have been used, but this has not provided sufficient metallic luster. In order to obtain a sufficient metallic luster, Patent Document 2 proposes an inkjet ink containing metal nanoparticles and emulsion resin particles, in which the average particle size of the metal nanoparticles and the average particle size of the emulsion resin particles are adjusted to have a predetermined relationship. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2020-94217 [Patent Document 2] International Publication No. 2018 / 181080 Summary of the Invention [Problem to be solved by the invention]
[0007] The flat metal particles used in Patent Document 1 have a 50% average particle diameter R50 of 0.5 to 3 μm of the equivalent circle diameter. In inkjet printing, nozzles such as ink flow paths and ejection ports in the printing device are miniaturized to form more precise images, and there are cases where printing cannot be performed with the flat metal particles described in Patent Document 1. Furthermore, in the case of flat metal particles, the adhesion to the substrate has not been fully studied, and it is unclear how the abrasion resistance, which indicates the degree of adhesion of the flat metal particles, will change when resin particles such as those in Patent Document 2 are used in combination.
[0008] An object of the present invention is to provide an inkjet metallic ink that can be stably ejected as an inkjet metallic ink containing flat metal particles together with resin particles, and that can improve the abrasion resistance of printed areas. Another object of the present invention is to provide an inkjet recording method using the metallic ink. [Means for solving the problem]
[0009] According to one aspect of the present invention, there is provided a metallic ink containing flat metal particles and resin particles, The volume-based median diameter (DP50) of the plate-like metal particles is less than 500 nm, the average thickness of the plate-like metal particles is 50 nm or less, The inkjet metallic ink is characterized in that the ratio of the volume-based median diameter (DP50) of the plate-like metal particles to the volume-based median diameter (D50) of the resin particles is 4.0 or more.
[0010] The present invention also relates to an inkjet recording method for printing on a recording medium using the inkjet metallic ink. [Effects of the Invention]
[0011] According to the present invention, it is possible to provide an inkjet metallic ink that can stably eject flat metal particles together with resin particles as an inkjet metallic ink and that can improve the abrasion resistance of printed areas. Furthermore, according to the present invention, it is possible to provide an inkjet recording method using the metallic ink. DETAILED DESCRIPTION OF THE INVENTION
[0012] The inkjet metallic ink (hereinafter also simply referred to as "ink") of the present invention contains flat metal particles and resin particles.
[0013] <Flat metal particles> The tabular metal particles used in the present invention are metal particles having flat surfaces and a thin thickness in a direction intersecting the direction of the surfaces, i.e., flat particles with a high aspect ratio in which the equivalent circle diameter of the flat surface is large relative to the thickness.
[0014] Typical pigments contained in inks are spherical. Some pigments are fixed to the recording medium by their own penetration, physical adsorption, chemical interaction, or the like, while others have a complementary effect on fixing to the recording medium, or have been processed to improve fixing properties. On the other hand, the flat metal particles contained in the metallic ink used in the present invention are characterized by their shape, which makes them less likely to fix to the recording medium.
[0015] For the flat metal particles used in the present invention, a metallic ink containing resin particles and a liquid is prepared to improve fixation. The metallic ink is then ejected onto a liquid-absorbent recording medium, such as paper, by an inkjet method. The liquid in the metallic ink that adheres to the recording medium is then absorbed by the recording medium, causing the flat metal particles and resin particles to level on the recording medium. Because the resin particles have a smaller median diameter on a volume basis than the flat metal particles, the flat metal particles are fixed on the recording medium so that the planes of the metal particles are parallel to the surface of the recording medium.
[0016] The size of the plate-like metal particles can be measured and analyzed using a wet particle image analyzer (for example, trade name: FPIA-3000, manufactured by Sysmex Corporation or trade name: IF-3200, manufactured by Jusco International Co., Ltd.). The sizes of the plate-like metal particles measured using the above-mentioned device, based on the cumulative 50% (median diameter (DP50)) and cumulative 99% (median diameter (DP99)) of the particle distribution on a volume basis of the diameter of a circle equivalent to a flat surface (circle equivalent diameter), are described below.
[0017] The flat metal particles used in the present invention preferably have a DP50 of less than 500 nm and not more than 400 nm. Furthermore, the DP99 is preferably not more than 1 μm, more preferably not more than 900 nm. If the DP50 is 500 nm or more or if the DP99 exceeds 1 μm, clogging occurs near the ink flow path or ejection port in the inkjet printing device, making stable ejection impossible. In relation to the resin particles described below, the DP50 is preferably not less than 300 nm.
[0018] The thickness of the flat metal particles of the present invention is in the range of 50 nm or less, preferably 40 nm or less. Furthermore, from the viewpoint of maintaining the flat-plate shape, a thickness of 10 nm or more is preferred, and 20 nm or more is more preferred. If the thickness of the flat metal particles is greater than 50 nm, unevenness occurs on the surface of the film formed during the film formation process, resulting in reduced light reflectivity in the flat metal particles obtained by processing the film. Furthermore, it takes time to reach the above thickness. Furthermore, if the thickness of the flat metal particles is too thin, unevenness (dots or islands) will be partially formed in the film formed. This will result in a deviation of the average particle size from the desired value when the film is processed into flat metal particles. As a result, sufficient fixation may not be achieved when the particles are ejected onto a recording medium. In other words, by keeping the thickness of the flat metal particles within the above range, good fixation can be achieved when printed by inkjet printing. The thickness of the flat metal particles can be measured, for example, by cutting the area where the flat metal particles are fixed after printing on a recording medium with a microtome at room temperature or cooled to expose the cross section, and then observing and measuring the length with an electron microscope.
[0019] The plate-like metal particles are not limited in material as long as they can be formed with the desired metallic luster by the inkjet method, but those that reflect light without coloring when reflected on a flat surface are preferred, and aluminum or its alloys are preferred from the viewpoint of cost.Other examples include single materials such as titanium, nickel, chromium, tin, zinc, platinum, and silver, or alloys and mixtures thereof.
[0020] The method for producing the flat metal particles is not particularly limited as long as it can produce flat metal particles having a substantially uniform thickness. From the viewpoint of easily obtaining metal particles with a uniform thickness, a film-forming method is preferred. For example, a release layer is formed on the surface of a sheet-like resin substrate, and a metal or alloy layer is further laminated on the release layer by vacuum deposition or sputtering. The release layer and the metal or alloy layer are then separated in an organic solvent, and the metal or alloy layer is crushed to adjust the particle size, thereby obtaining the flat metal particles of the present invention. The plate-shaped metal particles prepared by the above process are preferably subjected to the surface treatment described in the present invention before use. As described above, aluminum or its alloy is preferably used as the metal material. In this case, it is preferable to provide a surface coating layer on the surface of the aluminum or its alloy to prevent the aluminum or its alloy from reacting with moisture to aluminize and turn white. The surface coating layer may contain inorganic compounds such as phosphoric acid, silica, chromium, and carbon, or organic compounds such as silane coupling agents. The presence of a surface treatment layer on aluminum can be confirmed by methods such as X-ray diffraction.
[0021] The content of the plate-like metal particles in the ink is preferably 0.1% by mass to 20% by mass, and more preferably 0.2% by mass to 10% by mass, based on the total mass of the ink.
[0022] <Resin particles> The resin particles used in the present invention are granular materials made of resin. The resin particles used in the present invention are not limited to any particular material, and examples include acrylic resins, urethane resins, polyolefin resins, polyester resins, vinyl chloride resins, epoxy resins, polysiloxane resins, fluororesins, styrene resins, and butadiene resins. Water-soluble compounds containing flat metal particles and materials that exhibit good adhesion to recording media are particularly suitable. Examples include saturated polyester resins containing terephthalic acid, acrylic-modified polyester resins, vinyl chloride-acrylic mixed resins, urethane polyol resins, and composites or mixtures thereof. These are used in inks that are stably dispersed in the form of polymer resins, emulsions (including core-shell types), colloids, and the like. The particle size of the resin particles can be measured and analyzed using a dynamic light scattering device (e.g., Nanotrac WAV, manufactured by Microtrac, or Dynamic Light Scattering Photometer, manufactured by Otsuka Electronics). The particle size of the resin particles measured using the device at 50% cumulative (median diameter (D50)) in the volume-based particle distribution is described below. The resin particles used in the present invention have a volume-based median diameter (DP50) of the tabular metal particles / volume-based median diameter (D50) of the resin particles of 4.0 or more, preferably 5.0 or more. Furthermore, the median diameter (D50) of the resin particles is preferably 10 nm or more and 80 nm or less, and more preferably 20 nm or more and 60 nm or less. The content of the resin particles is preferably 0.1% by mass to 20% by mass, and more preferably 0.2% by mass to 10% by mass, based on the total mass of the ink.
[0023] <Components other than metal particles and resin particles> Components other than the metal particles and resin particles of the ink-jet metallic ink of the present invention will be described below.
[0024] When an aqueous ink is used as the inkjet metallic ink of the present invention, the water used in the aqueous ink is preferably pure water or ultrapure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, or distilled water. Furthermore, sterilization of such water by ultraviolet irradiation, addition of hydrogen peroxide, or the like is preferred, as this can prevent the growth of mold and bacteria. Furthermore, the amount of water used in the aqueous ink is preferably 0.2% by mass or more but 99% by mass or less, based on the total mass of the ink.
[0025] The aqueous ink of the present invention may contain a water-soluble organic solvent that is highly compatible with water. Examples of the water-soluble organic solvent include amides such as dimethylformamide and dimethylacetamide; ketones such as acetone; ethers such as tetrahydrofuran and dioxane; polyalkylene glycols such as polyethylene glycol and polypropylene glycol; alkylene glycols having an alkylene group containing 2 to 6 carbon atoms such as ethylene glycol, propylene glycol, butylene glycol, triethylene glycol, 1,2,6-hexanetriol, thiodiglycol, hexylene glycol, and diethylene glycol; glycerin; lower alkyl ethers of polyhydric alcohols such as ethylene glycol monomethyl (or ethyl) ether, diethylene glycol monomethyl (or ethyl) ether, and triethylene glycol monomethyl (or ethyl) ether; cyclic amide compounds such as N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, triethanolamine, sulfolane, dimethyl sulfoxide, 2-pyrrolidone, and ε-caprolactam; and imide compounds such as succinimide. These may be used alone or in combination of two or more as necessary. The content of the water-soluble organic solvent is preferably from 1 to 40% by mass, and more preferably from 3 to 30% by mass, based on the total mass of the ink. The ink according to the present invention may also be a water-free ink. In this case, various organic solvents, particularly polar organic solvents, may be used as the liquid medium. Examples of polar organic solvents that can be used include alcohols (e.g., methyl alcohol, ethyl alcohol, propyl alcohol, butyl alcohol, isopropyl alcohol, and fluorinated alcohol), ketones (e.g., acetone, methyl ethyl ketone, and cyclohexanone), carboxylic acid esters (e.g., methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, and ethyl propionate), and ethers (e.g., diethyl ether, dipropyl ether, tetrahydrofuran, and dioxane). In addition, for water-free inks, the liquid medium may be one or a combination of polyalkylene glycols such as polyethylene glycol and polypropylene glycol; alkylene glycols in which the alkylene group contains 2 to 6 carbon atoms, such as ethylene glycol, propylene glycol, butylene glycol, triethylene glycol, 1,2,6-hexanetriol, thiodiglycol, hexylene glycol, and diethylene glycol; glycerin; and lower alkyl ethers of polyhydric alcohols, such as ethylene glycol monomethyl (or ethyl) ether, diethylene glycol monomethyl (or ethyl) ether, and triethylene glycol monomethyl (or ethyl) ether.
[0026] The inkjet metallic ink of the present invention may contain a surfactant. For example, any of the various surfactants conventionally used in preparing inkjet inks can be used. Examples of surfactants include anionic surfactants such as dialkyl sulfosuccinates, alkyl naphthalene sulfonates, and fatty acid salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycols, and polyoxyethylene-polyoxypropylene block copolymers; cationic surfactants such as alkylamine salts and quaternary ammonium salts; and silicone-based and fluorine-based surfactants. These surfactants may be used alone or in combination of two or more. The surfactant content is preferably 0.001% by mass or more and 2% by mass or less of the total mass of the ink.
[0027] A dispersant can be used in the inkjet metallic ink of the present invention. The dispersant preferably has both hydrophobic functionality (affinity for aluminum) and hydrophilic functionality (dispersibility in water), with the hydrophilic functionality being realized by both ionic and nonionic functionality. For example, a dispersant with both hydrophobic and hydrophilic (ionic and nonionic) functionality, or a combination of a dispersant with both hydrophobic and hydrophilic (ionic) functionality and a dispersant with both hydrophobic and hydrophilic (nonionic) functionality, can be used. Specific examples of such dispersants include hydrophilic resins and surfactants that combine hydrophobic and hydrophilic functionality, or combinations of these. A representative example is JONCRYL RESIN (manufactured by BASF). The content of the dispersant is preferably 0.1% to 20% by mass, and more preferably 0.2% to 10% by mass, of the total mass of the pigment in the ink.
[0028] To improve continuous ejection, the metallic ink of the present invention can contain a linear or branched C5 to C9 alkanediol. Linear diols are particularly preferred, with 1,2-diols being more preferred. Specific examples include linear compounds such as 1,2-pentanediol, 1,2-hexanediol, 1,2-heptanediol, 1,2-octanediol, 1,2-nonanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, and 2,4-diethyl-1,5-pentanediol. The content of such alkanediols is preferably 1% by mass or more but less than 20% by mass, and more preferably 1% by mass or more but less than 10% by mass, based on the total mass of the ink.
[0029] The inkjet recording method of the present invention is a method of recording an image on a recording medium by ejecting the metallic ink described above from an inkjet recording head. In the inkjet recording method of the present invention, it is preferable to adopt a method of applying thermal energy to the ink as a method of ejecting the metallic ink. Other than using the metallic ink of the present invention, the steps of the inkjet recording method may be known.
[0030] In the inkjet recording method of the present invention, the metallic ink of the present invention can be used in combination with conventional chromatic inks. Because the metallic ink of the present invention has high hiding power due to the flat metal particles, it is preferable to apply the metallic ink of the present invention first, and then apply the chromatic ink.
[0031] <Recording Media> The recording medium is not particularly limited, and examples thereof include printing paper such as inkjet glossy paper, inkjet matte paper, inkjet raster paper, and coated paper for offset printing. In addition, resin films such as vinyl chloride and polyethylene terephthalate, glass, and printed wiring boards can also be used. The recording medium may be pretreated before image formation. The pretreatment adjusts the surface tension of the recording medium and controls the wettability of the ink, thereby adjusting the dot area per droplet of the ink ejected onto the recording medium. Examples of pretreatment include corona treatment, plasma treatment, and flame treatment. Furthermore, when using aqueous ink, it is preferable that the surface of the recording medium is moisture-absorbent. The material itself, such as paper, may be liquid (moisture)-absorbent, or a liquid-absorbent layer may be provided on a substrate that does not have liquid-absorbent properties.
[0032] The recording medium preferably has a surface roughness Ra of 2 μm or less. When the surface roughness is 2 μm or less, the flat surfaces of the plate-like metal particles on the recording medium tend to be oriented in the same direction, which increases specular reflection and tends to increase metallic luster. The surface roughness is measured by measuring the surface roughness Ra (arithmetic mean roughness) in an area of 1.4 mm x 1.1 mm using a laser microscope (product name: VK9710, manufactured by Keyence Corporation).
[0033] <Recording device> The recording apparatus used in the ink jet recording method of the present invention, particularly the structure around the recording head that ejects the ink, is not limited as long as it can stably eject the metallic ink according to the present invention.
[0034] Here, assuming that the diameter of the nozzle opening of the recording head of the inkjet recording device is Y μm and the opening size of the mesh filter provided in the ink introduction path is Z μm, it is preferable that the nozzle diameter Y μm and the opening size Z μm of the mesh filter satisfy the relationship Y≧5Z. When using the metallic ink of this embodiment in an inkjet recording device that satisfies this relationship, it is preferable that the condition Z≧2X be satisfied, where X is the median diameter (DP99) of the metal particles. This prevents clogging of the nozzle opening with the flat metal particles and ensures stable ink ejection. [Example]
[0035] The present invention will be specifically explained with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0036] [Example 1] (Preparation of a dispersion of flat metal particles) A solution containing 3% by mass of cellulose acetate butyrate (CAB, butylation rate 35-39%, manufactured by Eastman Chemical Co.) was uniformly coated onto a 100 μm thick PET film using a bar coating method and dried at 60°C for 10 minutes to form a 30 μm thick film (release layer). Next, using a vacuum deposition apparatus (product name: EME-400 type vacuum deposition apparatus, manufactured by ULVAC), aluminum was deposited onto the release layer as a raw material for plate-like metal particles to a thickness equivalent to 20 nm as measured by a film thickness meter. Thereafter, the release layer on which the aluminum had been deposited was placed in an alkylene glycol monoether solvent and subjected to ultrasonic irradiation (product name: ASU-20M type, manufactured by AS ONE Corporation) for 10 minutes to cause peeling. Next, after removing the PET from the solvent, a surface treatment agent, disodium hydrogen phosphate aqueous solution, was added to the PET to a concentration of 10% by mass, and the mixture was filtered through a SUS filter with a particle size of 10 μm to remove coarse particles. Then, an ultrasonic disperser (trade name: PR-1, manufactured by Thinky Corporation) was used to irradiate the mixture with ultrasound (24 hours, 40°C) to prepare a dispersion. Next, the dispersion was centrifuged (10,000 rpm, 30 minutes), and a precipitate consisting of aluminum flakes was collected. Pure water was then added to disperse the precipitate at 10% by mass. The above steps of centrifugation, collection of the precipitate, and dispersion by adding pure water were repeated a total of three times. The surface treatment agent was then removed and replaced with water to obtain an aqueous dispersion of aluminum flakes. At this time, a portion of the precipitate was collected separately, and X-ray diffraction of the aluminum flake surface was performed using an X-ray diffractometer (trade name: Empyrean, manufactured by Malvern Panalytical) with CuKα radiation. As a result, a diffraction peak was measured with a diffraction angle of 25° and a half-width of 6.0°, and the substance on the surface of the aluminum flake was identified as an amorphous phosphate compound. This confirmed that the surface of the aluminum flake had been surface treated with a phosphate compound. The particle size of the aluminum flakes in the aqueous dispersion was measured using a wet particle image analyzer (product name: FPIA-3000, manufactured by Sysmex Corporation).
[0037] (resin particles) The resin particles used were saturated polyester resin containing terephthalic acid (product name: PLASCOAT Z-446, manufactured by GOO Chemical Co., Ltd.) The resin particles were diluted with pure water to 0.1% by mass, and the particle size of the resin particles was measured using a dynamic light scattering device (product name: NANOTRACK WAV, manufactured by MICROTRACK).
[0038] (Preparation of metallic ink) The metallic ink of this example was prepared according to the composition shown below. 10 parts by mass of the aqueous dispersion containing 10% by mass of the aluminum flakes prepared above Resin particles (saturated polyester resin) 1 part by mass Glycerin 5 parts by mass Surfactant (acetylene glycol) 1 part by mass (Product name: Acetylenol E100, manufactured by Kawaken Fine Chemicals Co., Ltd.) Triethylene glycol 5 parts by mass Pure water 78 parts by mass
[0039] (Measurement of particle size of aluminum flakes and resin particles after ink preparation) The metallic ink prepared above was centrifuged (10,000 rpm, 30 minutes) to separate it into a precipitate consisting of aluminum flakes and a supernatant consisting of other components. The precipitate was redispersed in a solution prepared by replacing the aluminum flakes with pure water at a mass percentage equivalent to that of the aluminum flakes in the metallic ink of this example, and the particle size of the aluminum flakes was measured using the wet particle image analyzer. The result was the same as the particle size of the aluminum flakes in the aqueous dispersion before the ink was prepared. The supernatant was removed and the particle size of the resin particles was measured using the dynamic light scattering device, and the result was the same as the particle size of the resin particles in the aqueous dispersion before the ink preparation. This result indicates that the particle size of the aluminum flakes and resin particles used in this example did not change even when they were included in the ink as one component of the metallic ink using the method described in this example.
[0040] (Printing with an inkjet recording device) The metallic ink obtained in this example was used to print an A4 solid image on an A4-size recording medium (product name: Canon Photo Paper Glossy Gold, manufactured by Canon Inc.) under a room temperature and humidity environment using an inkjet recording device (product name: PIXUS Pro-10, manufactured by Canon Inc.) The nozzle diameter (discharge port diameter) of the inkjet recording device was 15 μm, and the openings of the mesh filter provided in the flow path were 3 μm.
[0041] (Measurement of the thickness of aluminum flakes contained in the printed area) A portion of the printed area was cut out, sandwiched between PET films, and its cross section was formed and exposed using a microtome. The exposed cross section was subjected to a conductive treatment according to a standard method, and then observed and measured using a high-resolution scanning electron microscope (product name: SU-8030, manufactured by Hitachi High-Technologies Corporation).
[0042] (Evaluation of abrasion resistance of printed images) The abrasion resistance of the printed image (solid image) obtained above was evaluated using a Gakushin-type abrasion tester (product name: AB-301 device, manufactured by Tester Sangyo Co., Ltd.) Specifically, the abrasion resistance was evaluated by bringing a friction element into contact with the printed image, applying a load (200 g) to the friction element, and performing a horizontal reciprocating motion (10 times). At that time, visual evaluation was carried out according to the following criteria. A: There are almost no traces of the friction element moving back and forth on the printed image, and there is no peeling. B: Traces of the friction element moving back and forth are visible in the printed image area, but there is no peeling. C: A part of the printed image peels off, and the recording medium in the peeled part is exposed. D: The entire printed image is removed, exposing the recording medium. E: Discharge is not possible and printing is not possible on the recording medium.
[0043] (Metallic gloss evaluation) The metallic gloss of the printed image obtained above was evaluated according to the following evaluation criteria: In the present invention, A and B were considered to be preferable levels, and C was considered to be an unacceptable level. A: When observed visually, a metallic luster and the outline of the reflected image can be confirmed. B: When observed visually, there is a metallic luster, but the outline of the reflected image cannot be confirmed. C: When observed visually, there is no metallic luster and the outline of the reflected image cannot be confirmed.
[0044] [Example 2] A metallic ink was prepared using the method and ink composition described in Example 1, except that Grade 701 of Vinyblan (registered trademark) manufactured by Nissin Chemical Industry Co., Ltd., which has a vinyl chloride-acrylic mixed resin as the resin particles, was used. Using the prepared ink, the particle size of the resin particles was measured and the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0045] [Example 3] A metallic ink was prepared using the method and ink composition described in Example 1, except that the resin particles used were "PESRESIN A-645GH" (trade name, manufactured by Takamatsu Oil & Fat Co., Ltd.) having an acrylic-modified saturated polyester resin skeleton. Using the prepared ink, the particle size of the resin particles was measured and the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0046] [Example 4] A metallic ink was prepared using the method, ink composition, and resin particles described in Example 1, except that the thickness of the aluminum flakes in Example 1 was changed to 40 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0047] [Example 5] A metallic ink was prepared using the method, ink composition, and resin particles described in Example 2, except that the thickness of the aluminum flakes in Example 2 was changed to 40 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0048] [Example 6] A metallic ink was prepared using the method, ink composition, and resin particles described in Example 3, except that the thickness of the aluminum flakes in Example 3 was changed to 40 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0049] [Example 7] The aluminum dispersion of Example 1 was subjected to ultrasonic irradiation using the ultrasonic disperser for 12 hours, and the median diameter (DP50) of the aluminum flakes was set to 400 nm. A metallic ink was prepared using the ink composition and resin particles described in Example 1. The prepared ink was used to evaluate the abrasion resistance of printed images in the same manner as in Example 1.
[0050] [Example 8] The aluminum dispersion of Example 2 was subjected to ultrasonic irradiation using the ultrasonic disperser for 12 hours, and the median diameter (DP50) of the aluminum flakes was set to 400 nm. A metallic ink was prepared using the ink composition and resin particles described in Example 2. The prepared ink was used to evaluate the abrasion resistance of printed images in the same manner as in Example 1.
[0051] [Example 9] The aluminum dispersion of Example 3 was subjected to ultrasonic irradiation using the ultrasonic disperser for 12 hours, and the median diameter (DP50) of the aluminum flakes was set to 400 nm. A metallic ink was prepared using the ink composition and resin particles described in Example 3. The prepared ink was used to evaluate the abrasion resistance of printed images in the same manner as in Example 1.
[0052] [Example 10] A metallic ink was prepared using the method, ink composition, and resin particles described in Example 7, except that the thickness of the aluminum flakes in Example 7 was changed to 40 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0053] [Example 11] A metallic ink was prepared using the method, ink composition, and resin particles described in Example 8, except that the thickness of the aluminum flakes in Example 8 was changed to 40 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0054] [Example 12] A metallic ink was prepared using the method, ink composition, and resin particles described in Example 9, except that the thickness of the aluminum flakes in Example 9 was changed to 40 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0055] [Example 13] (Preparation of a dispersion of flat metal particles) A solution containing 3% by mass of cellulose acetate butyrate (CAB, butylation rate 35-39%, manufactured by Eastman Chemical Co.) was uniformly coated onto a 100 μm thick PET film using a bar coating method and dried at 60°C for 10 minutes to form a 30 μm thick film (release layer). Next, using a vacuum deposition apparatus (product name: EME-400 type vacuum deposition apparatus, manufactured by ULVAC), aluminum was deposited onto the release layer as a raw material for plate-like metal particles to a thickness equivalent to 20 nm as measured by a film thickness meter. Thereafter, the release layer on which the aluminum had been deposited was placed in an alkylene glycol monoether solvent and subjected to ultrasonic irradiation (product name: ASU-20M type, manufactured by AS ONE Corporation) for 10 minutes to cause peeling. Next, after removing the PET from the solvent, the PET was filtered through a SUS filter with a particle size of 10 μm without adding a surface treatment agent to remove coarse particles, and then ultrasonically irradiated (12 hours, 40° C.) using the ultrasonic disperser to prepare a dispersion. Next, the dispersion was centrifuged (10,000 rpm, 30 minutes) to collect a precipitate consisting of aluminum flakes, and diethylene glycol monomethyl ether (manufactured by Nissin Chemical Co., Ltd.) was added to disperse the precipitate to a concentration of 10% by mass. The particle size of the aluminum flakes in the dispersion was measured using the wet particle image analyzer.
[0056] (resin particles) The resin particles used were those having a polyester resin skeleton and manufactured by GOO Chemical Co., Ltd. under the trade name "PLASCOAT RZ-105." The resin particles were diluted with diethylene glycol monomethyl ether to a concentration of 0.1% by mass, and the particle size of the resin particles was measured using the dynamic light scattering device.
[0057] (Ink Preparation) A metallic ink was prepared according to the composition shown below. Dispersion liquid containing 10% by mass of the aluminum flakes prepared above 10% by mass Resin particles 1% by mass Glycerin 5% by mass Surfactant 1% by mass (Product name: Acetinol E100, manufactured by Kawaken Fine Chemicals Co., Ltd.) Diethylene glycol monomethyl ether 40% by mass Dipropylene glycol monobutyl ether 40% by mass Triethylene glycol 3% by mass
[0058] (Measurement of the particle size of aluminum flakes and resin particles after preparing the ink) The median diameter (DP50) of the aluminum flakes and the median diameter (D50) of the resin particles of the ink prepared above were measured using the same method as in Example 1, and were found to be the same as the values before they were included in the ink as a component of the metallic ink. (Evaluation of adhesion of aluminum flakes) Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0059] [Example 14] A metallic ink was prepared using the method and ink composition described in Example 13, except that Grade 701 of Vinyblan (registered trademark) manufactured by Nissin Chemical Industry Co., Ltd., which contains vinyl chloride resin as the resin particles, was used. Using the prepared ink, the particle size of the resin particles was measured and the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0060] [Example 15] A metallic ink was prepared using the method and ink composition described in Example 13, except that the resin particles used were "PESRESIN S-180" (trade name, manufactured by Takamatsu Oil & Fat Co., Ltd.) having a saturated polyester resin skeleton. Using the prepared ink, the particle size of the resin particles was measured and the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0061] [Comparative Example 1] A metallic ink was prepared using the method and ink composition described in Example 9. However, aluminum was vapor-deposited to a thickness equivalent to 70 nm. Furthermore, ultrasonic irradiation using the ultrasonic disperser was performed for 15 hours, and the median diameter (DP50) of the aluminum flakes was 400 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0062] Comparative Example 2 A metallic ink was prepared using the method and ink composition described in Example 10, except that grade 715 of Vinyblan (registered trademark) manufactured by Nissin Chemical Industry Co., Ltd. was used as the resin particles. Using the prepared ink, the particle size of the resin particles was measured and the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0063] Comparative Example 3 The aluminum vapor-deposited film prepared by the method described in Example 1 was subjected to ultrasonic irradiation using the ultrasonic disperser described in Example 10 for 2 hours, with the median diameter (DP50) of the aluminum flakes being 600 nm. A metallic ink was prepared using the method and ink composition described in Example 1. The prepared ink was used to evaluate the abrasion resistance of the printed image in the same manner as in Example 1.
[0064] Comparative Example 4 A metallic ink was prepared using the method, ink composition, and resin particles described in Example 13. However, when aluminum was vapor-deposited, it was vapor-deposited to a film thickness equivalent to 70 nm. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0065] Comparative Example 5 A metallic ink was prepared using the method and ink composition described in Example 14, except that VB-715 manufactured by Nissin Chemical Co., Ltd., which contains vinyl chloride resin as the resin particles, was used. Using the prepared ink, the abrasion resistance of the printed image was evaluated in the same manner as in Example 1.
[0066] Comparative Example 6 For aluminum flakes, ultrasonic irradiation was performed for 2 hours using the ultrasonic disperser according to the method described in Example 13, and the median diameter (DP50) of the aluminum flakes was set to 600 nm. A metallic ink was prepared using the ink composition and resin particles described in Example 13. The prepared ink was used to evaluate the abrasion resistance of printed images in the same manner as in Example 1.
[0067] Table 1 shows the particle sizes of the aluminum and resin particles in the inks prepared in each of the Examples and Comparative Examples, and the results of evaluation of the abrasion resistance of the printed images.
[0068] [Table 1]
[0069] In Examples 1 to 15, the median diameter (DP50) of the plate-like metal particles was less than 500 nm, the average thickness was 50 nm or less, and the median diameter (DP50) of the plate-like metal particles / median diameter (D50) of the resin particles was 4.0 or more. When a metallic ink prepared to satisfy this relationship was used, the abrasion resistance of the printed image was evaluated as A or B, demonstrating that good aluminum fixation was achieved. Furthermore, the metallic gloss of the printed image was evaluated as A or B, demonstrating that sufficient gloss was achieved. On the other hand, in Comparative Examples 1 and 4, metallic inks containing flat metal particles with an average thickness of more than 50 nm were used. In these cases, the abrasion resistance of the printed image was evaluated as C, revealing a decrease in the fixability of the aluminum. This is thought to be because, when flat metal particles with an average thickness of more than 50 nm are produced by vacuum deposition, irregularities are generated on the surface, resulting in poor contact with the recording medium and resin particles. Furthermore, in Comparative Examples 2 and 5, metallic inks were used in which the ratio of the median diameter of the flat metal particles to the median diameter of the resin particles (DP50 / D50) was smaller than 4.0. In this case, the rub resistance of the printed image was evaluated as D, revealing a further deterioration in the fixation of the aluminum. This is thought to be because the particle size of the resin particles was larger than a certain level relative to the particle size of the flat metal particles, and the flat metal particles were not stably fixed so that their planes were parallel to the recording medium. Furthermore, in Comparative Examples 3 and 6, the median diameter (DP50) of the plate-like metal particles was 500 nm or more, and the median diameter (DP99) also exceeded 1 μm. In this case, even though the relationship (DP50) / (D50) was 4.0 or more, ejection was not possible due to nozzle clogging, and printing was not possible. Therefore, evaluation of metallic gloss was not performed in Comparative Examples 3 and 6. In Comparative Examples 2, 4 and 5, the metallic gloss of the printed image was evaluated as C, making it clear that the desired metallic gloss could not be obtained.
Claims
1. Contains flat metal particles and resin particles, The volume-based median diameter (DP50) of the tabular metal particles is less than 500 nm; The average thickness of the plate-like metal particles is 50 nm or less, 1. An ink-jet metallic ink, comprising: a volume-based median diameter (DP50) of said tabular metal particles / a volume-based median diameter (D50) of said resin particles being 4.0 or more.
2. A metallic ink for inkjet recording as described in claim 1, wherein the volume-based median diameter (DP50) of the flat metal particles is 400 nm or less.
3. A metallic ink for inkjet recording as described in claim 1 or 2, wherein the volume-based median diameter (DP50) of the flat metal particles is 300 nm or more.
4. 4. The ink-jet metallic ink according to claim 1, wherein the tabular metal particles have a volume-based median diameter (DP99) of 1 μm or less.
5. A metallic ink for inkjet recording as described in claim 4, wherein the volume-based median diameter (DP99) of the flat metal particles is 900 nm or less.
6. A metallic ink for inkjet recording as described in claim 4 or 5, wherein the volume-based median diameter (DP99) of the flat metal particles is 800 nm or more.
7. A metallic ink for inkjet recording described in any one of claims 1 to 6, wherein the average thickness of the flat metal particles is 10 nm or more.
8. 8. The ink-jet metallic ink according to claim 1, wherein the flat metal particles are aluminum particles.
9. A metallic ink for inkjet recording described in any one of claims 1 to 8, wherein the volume-based median diameter (D50) of the resin particles is 10 nm or more and 80 nm or less.
10. An inkjet metallic ink described in any one of claims 1 to 9, wherein the resin particles are polyester resin particles.
11. The ink-jet metallic ink according to any one of claims 1 to 10, wherein the ink-jet metallic ink is a water-based ink containing water.
12. A metallic ink for inkjet recording described in any one of claims 1 to 11, wherein the flat metal particles have been surface-treated with a phosphate compound.
13. A metallic ink for inkjet recording described in any one of claims 1 to 12, wherein the volume-based median diameter (DP50) of the flat metal particles / volume-based median diameter (D50) of the resin particles is 5.0 or more.
14. A metallic ink for inkjet recording described in any one of claims 1 to 13, wherein the volume-based median diameter (DP50) of the flat metal particles / volume-based median diameter (D50) of the resin particles is 20.0 or less.
15. 15. The ink-jet metallic ink according to claim 1, wherein the tabular metal particles account for 0.1% by mass or more and 20% by mass or less of the total mass of the ink.
16. A metallic ink for inkjet recording described in any one of claims 1 to 15, wherein the flat metal particles are 0.2 mass % or more and 10 mass % or less relative to the total mass of the ink.
17. 17. The ink-jet metallic ink according to claim 1, wherein the resin particles account for 0.1% by mass or more and 20% by mass or less of the total mass of the ink.
18. A metallic ink for inkjet recording described in any one of claims 1 to 17, wherein the resin particles are 0.2 mass % or more and 10 mass % or less relative to the total mass of the ink.
19. An inkjet recording method comprising the step of printing an image on a recording medium by using the inkjet metallic ink according to any one of claims 1 to 18.