Decorative film having cover film, method for manufacturing the same and method for constructing decorative film

JP2023080848A5Active Publication Date: 2024-11-223M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021194381
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2024-11-22
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

Decorative films with polyurethane surfaces often develop crater-like defects due to incomplete curing, which can lead to adhesion issues with a cover film, causing the cover film to detach during production, transportation, or use.

Method used

A decorative film design featuring a polyurethane layer with partial crosslinking, a corona-treated or plasma-treated removable cover film, and an adhesive layer, ensuring the cover film adheres well to the polyurethane layer without defects.

Benefits of technology

The solution prevents crater defects and maintains high surface quality by ensuring the cover film adheres properly, preventing detachment during production, transportation, and use, while allowing easy removal when applied to a substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a decorative film having a cover film, including a polyurethane layer as a surface layer, having less defects, such as a crater and having high surface quality.SOLUTION: A decorative film having a cover film includes: (a) a polyurethane layer having a first surface and a second surface on the side opposite to the first surface and including polyurethane at least partially crosslinked, where the polyurethane at least partially crosslinked includes at least one of polyester based polyurethane and polycarbonate based polyurethane, (b) a removable cover film having a surface subjected to corona treatment or plasma treatment and contacting the surface subjected to corona treatment or plasma treatment of removable cover film to the first surface of the polyurethane layer; (c) a base layer having a first surface contacting the second surface of the polyurethane layer and a second surface on the side opposite to the first surface; and (d) an adhesive layer contacting the second surface of the base layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to a decorative film with a cover film, and a manufacturing method and application method thereof. [Background technology]

[0002] BACKGROUND ART It is known to apply a decorative film to the body or parts of an automobile instead of painting to decorate the exterior of the automobile.

[0003] Patent Document 1 (JP 2013-039724 A) describes "a vehicle paint replacement film including a transparent material layer and a colored adhesive layer, wherein the colored adhesive layer includes: (i) a colorant premix including (a) an acrylic polyol; and (b) a colorant dispersed in the acrylic polyol, the colorant premix including a colorant selected from the group consisting of a combination of an organic pigment and an inorganic pigment, a combination of an organic pigment and an aluminum luster material, a combination of an organic pigment and a mica luster material, a combination of an inorganic pigment and an aluminum luster material, a combination of an inorganic pigment and a mica luster material, and a combination of an aluminum luster material and a mica luster material, and combinations thereof; and (ii) an adhesive polymer, wherein the solids mass ratio expressed as adhesive polymer / (adhesive polymer + acrylic polyol) is 25% or more."

[0004] Patent Document 2 (JP 2007-297569 A) describes a decorative layer-forming film having a top coat layer made of a polyurethane resin and a carrier film provided on the surface side of the top coat layer, wherein the polyurethane resin is made of a polyurethane resin composition containing (1) a polyisocyanate containing an isocyanurate or an adduct of isophorone diisocyanate, or both, in an amount of 0.5 equivalents or more relative to the total polyisocyanate, and (2) a polyol consisting of caprolactone diol, polycarbonate diol, or a mixture thereof, and containing a polyester polyol having an average molecular weight of 1000 or less in an amount of 0.4 equivalents or more relative to the total polyol, wherein the equivalent ratio of the polyisocyanate to the polyol is 0.7 to 2.0. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2013-039724 [Patent Document 2] Japanese Patent Application Laid-Open No. 2007-297569 Summary of the Invention [Problem to be solved by the invention]

[0006] Cured products of reactive polyurethane compositions have excellent durability and can therefore be advantageously used as the surface layer (top layer) of decorative films for exterior applications. However, forming a surface layer using a reactive polyurethane composition can result in problems with the appearance of the decorative film, such as the occurrence of crater-like defects (dents). Reactive polyurethane compositions generally do not completely cure by the heat treatment alone during the process of forming the surface layer of the decorative film; the polyurethane curing reaction continues and progresses gradually even after the heat treatment. When the decorative film or an intermediate member having a surface layer is wound into a roll after the heat treatment, air may become trapped between the decorative film or intermediate member. It is believed that the trapped air presses against the soft surface layer, which is not completely cured, resulting in crater-like defects in the surface layer.

[0007] The mechanism by which crater defects occur in the production of decorative films will be described with reference to Figures 3A to 3D. Figure 3A shows a schematic cross-sectional view of an intermediate member for decorative films. The intermediate member 30a is a laminate including a cover film 12a, a polyurethane layer 14a that forms the surface layer of the decorative film, a base layer 16a, and a processing film 32a that supports the base layer 16a. The cover film 12a is laminated to protect the polyurethane layer 14a, which has a soft surface that has not yet fully hardened.

[0008] The intermediate member 30a is temporarily wound onto a roll and stored until the next process. Figure 3B shows a schematic cross-sectional view of the overlapping intermediate members wound onto the roll. During the winding onto the roll, air 40 is trapped between the process film 32b of the upper intermediate member 30b and the cover film 12a of the lower intermediate member 30a. The polyurethane layer 14a, which has a soft surface and is not completely cured, is compressed by the air 40 through the cover film 12a, deforming it and forming craters 42 in the polyurethane layer 14a.

[0009] After forming the adhesive layer in a separate process, the intermediate member is unwound from the roll, the process film is removed, and the adhesive layer is laminated onto the base layer. Figure 3C shows a schematic cross-sectional view of a decorative film with a cover film laminated with an adhesive layer. The decorative film with a cover film 10a has an adhesive layer 18a laminated on the underside of the base film 16a of the intermediate member. The adhesive layer 18a is protected by a liner 20a. In the decorative film with a cover film 10a, the cover film 12a is rigid and has restored to its original shape, but the polyurethane layer 14a has fully hardened in its deformed state, leaving the crater 42 intact.

[0010] During application, the cover film is then removed from the decorative film with the cover film. Fig. 3D shows a schematic cross-sectional view of the decorative film after the cover film has been removed. Craters 42 formed in the polyurethane layer 14a of the decorative film are visible as defects on the surface of the decorative film.

[0011] One method for preventing or suppressing the formation of craters is to promote the curing reaction of the reactive polyurethane composition during heat treatment, thereby increasing the hardness of the polyurethane layer. Measures for promoting the curing reaction of the reactive polyurethane composition include increasing the heat treatment temperature, lengthening the heat treatment time (e.g., reducing the line speed of a continuous oven), and increasing the amount of catalyst used.

[0012] However, when the hardness of the polyurethane layer is increased, the adhesiveness of the surface of the polyurethane layer decreases before the cover film is laminated on the polyurethane layer, and the cover film may not adhere well to the surface of the polyurethane layer. If the cover film does not adhere well, there is a risk that the cover film will fall off during production, transportation, or use of the decorative film.

[0013] The present disclosure provides a decorative film with a cover film that has a polyurethane layer as a surface layer and has high surface quality with few defects such as craters. [Means for solving the problem]

[0014] According to one embodiment of the present disclosure, (a) a polyurethane layer having a first surface and a second surface opposite the first surface, the polyurethane layer comprising an at least partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane; (b) a removable cover film having a corona-treated or plasma-treated surface, the corona-treated or plasma-treated surface of the removable cover film contacting the first side of the polyurethane layer; and (c) a base layer having a first side and a second side opposite the first side, the first side of the base layer contacting the second side of the polyurethane layer; (d) an adhesive layer in contact with the second surface of the base layer; A decorative film with a cover film is provided, comprising:

[0015] According to another embodiment of the present disclosure, (a) providing a base layer having a first side and a second side opposite the first side; (b) forming a polyurethane layer on the first surface of the base layer, the polyurethane layer having a first surface and a second surface opposite the first surface, the polyurethane layer comprising at least a partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane, and the first surface of the base layer contacting the second surface of the polyurethane layer; (c) providing a removable cover film; (d) treating the surface of the removable cover film with corona or plasma; (e) laminating the removable cover film onto the polyurethane layer such that the corona-treated or plasma-treated surface of the removable cover film contacts the first side of the polyurethane layer; and (f) forming an adhesive layer on the second surface of the base layer to obtain a decorative film with a cover film; A method for manufacturing a decorative film with a cover film is provided, comprising:

[0016] According to yet another embodiment of the present disclosure, (a) providing a base layer having a first side and a second side opposite the first side; (b) forming a polyurethane layer on the first surface of the base layer, the polyurethane layer having a first surface and a second surface opposite the first surface, the polyurethane layer comprising at least a partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane, and the first surface of the base layer contacting the second surface of the polyurethane layer; (c) providing a removable cover film; (d) treating the surface of the removable cover film with corona or plasma; (e) laminating the removable cover film onto the polyurethane layer such that the corona-treated or plasma-treated surface of the removable cover film contacts the first side of the polyurethane layer; (f) forming an adhesive layer on the second surface of the base layer; and (h) removing the removable cover film from the first side of the polyurethane layer. A method for producing a decorative film is provided, comprising:

[0017] According to yet another embodiment of the present disclosure, A method of applying a decorative film is provided that includes applying the decorative film with a cover film to a substrate, and then removing the removable cover film from the first side of the polyurethane layer.

[0018] According to yet another embodiment of the present disclosure, there is provided a method for applying a decorative film, comprising removing the removable cover film of the decorative film with cover film from the first surface of the polyurethane layer to obtain a decorative film, and applying the decorative film to a substrate. [Effects of the Invention]

[0019] According to the present disclosure, it is possible to provide a decorative film with a cover film that has a polyurethane layer as a surface layer and has high surface quality with few defects such as craters.

[0020] The above description should not be considered as a disclosure of all embodiments of the present invention and all advantages associated with the present invention. [Brief explanation of the drawings]

[0021] [Figure 1] 1 is a schematic cross-sectional view of a decorative film with a cover film according to one embodiment. [Figure 2] FIG. 10 is a schematic cross-sectional view of a decorative film with a cover film according to another embodiment. [Figure 3A] 1 is an explanatory diagram of the mechanism by which crater defects occur in the production of decorative films. FIG. [Figure 3B] 1 is an explanatory diagram of the mechanism by which crater defects occur in the production of decorative films. FIG. [Figure 3C] 1 is an explanatory diagram of the mechanism by which crater defects occur in the production of decorative films. FIG. [Figure 3D] 1 is an explanatory diagram of the mechanism by which crater defects occur in the production of decorative films. FIG. DETAILED DESCRIPTION OF THE INVENTION

[0022] Hereinafter, for the purpose of illustrating typical embodiments of the present invention, a more detailed description will be given with reference to the drawings as necessary, but the present invention is not limited to these embodiments.

[0023] In this disclosure, "(meth)acrylic" means acrylic or methacrylic, and "(meth)acrylate" means acrylate or methacrylate.

[0024] In the present disclosure, "curing" also encompasses the concept generally referred to as "crosslinking."

[0025] In the present disclosure, the term "film" also encompasses articles called "sheets."

[0026] In the present disclosure, "transparent" refers to an average transmittance of about 80% or more in the visible light region (wavelength 400 nm to 700 nm) measured in accordance with JIS K 7375: 2008, and may desirably be about 85% or more, or about 90% or more. There is no particular upper limit to the average transmittance, but it can be, for example, less than about 100%, about 99% or less, or about 98% or less.

[0027] In the present disclosure, "semi-transparent" means that the average transmittance in the visible light region (wavelength 400 nm to 700 nm) measured in accordance with JIS K 7375 is about 40% or more and less than about 80%, and desirably about 75% or less.

[0028] In one embodiment, the decorative film with a cover film is (a) a polyurethane layer having a first surface and a second surface opposite the first surface, the polyurethane layer comprising an at least partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane; (b) a removable cover film having a corona-treated or plasma-treated surface, the corona-treated or plasma-treated surface of the removable cover film contacting the first side of the polyurethane layer; and (c) a base layer having a first surface and a second surface opposite the first surface, the first surface of the base layer contacting the second surface of the polyurethane layer; (d) an adhesive layer in contact with the second surface of the base layer; Includes:

[0029] FIG. 1 shows a schematic cross-sectional view of one embodiment of a decorative film with a cover film. The decorative film with a cover film 10 includes a removable cover film 12, a polyurethane layer 14, a base layer 16, and an adhesive layer 18. The corona-treated or plasma-treated surface 122 of the removable cover film 12 contacts a first side (upper surface in FIG. 1) of the polyurethane layer 14. The first side (upper surface in FIG. 1) of the base layer 16 contacts a second side (lower surface in FIG. 1) of the polyurethane layer 14. The adhesive layer 18 contacts the second side (lower surface in FIG. 1) of the base layer 16. The decorative film with a cover film 10 may further include a liner 20 as an optional element.

[0030] The polyurethane layer includes an at least partially crosslinked polyurethane. The at least partially crosslinked polyurethane includes at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane. In this disclosure, "partially crosslinked" means that some of the reactive sites of the polyol and the crosslinking agent involved in the crosslinking reaction have reacted to form crosslinks, but there are still reactive sites remaining on both the polyol and the crosslinking agent that can undergo crosslinking. On the other hand, "fully crosslinked" means that at least one of the reactive sites of the polyol and the crosslinking agent involved in the crosslinking reaction has been completely consumed by the crosslinking reaction or has progressed to such a high degree that it can no longer participate in the crosslinking reaction. For example, in a reactive polyurethane composition in which the equivalent ratio (NCO / OH) of the polyol to the isocyanate crosslinking agent is less than 1, even if the hydroxyl groups of the polyol remain, the polyurethane is completely crosslinked if the isocyanato groups of the isocyanate crosslinking agent are completely consumed.

[0031] The polyurethane layer can be formed by applying a polyurethane layer composition, such as a reactive polyurethane composition, onto the first surface of the base layer or onto the liner by knife coating, bar coating, blade coating, doctor coating, roll coating, cast coating, or the like, and optionally heating. The polyurethane layer formed on the liner can be thermally laminated or transfer laminated (if the first surface of the base layer is adhesive to the polyurethane layer) onto the base layer so that the second surface of the polyurethane layer contacts the first surface of the base layer. The heating temperature can be, for example, about 40°C or higher, about 50°C or higher, or about 60°C or higher, and about 140°C or lower, about 120°C or lower, or about 100°C or lower. The heating time can be, for example, about 1 minute or higher, about 2 minutes or higher, or about 5 minutes or higher, and about 1 hour or lower, about 30 minutes or lower, or about 20 minutes or lower.

[0032] The reactive polyurethane composition may be a one-component curing type (such as a moisture-curing type or a blocked isocyanate type) or a two-component curing type. In one embodiment, the reactive polyurethane composition is a two-component curing type composition containing a polyol and an isocyanate crosslinker.

[0033] Examples of polyols include polyester polyols such as polycaprolactone diol, polycaprolactone triol, and condensates of low-molecular-weight polyols having 2 to 20 carbon atoms with aliphatic polycarboxylic acids or aromatic polycarboxylic acids (e.g., polyethylene adipate, polypropylene adipate, polybutylene adipate, polyhexamethylene adipate, and polybutylene sebacate); and polycarbonate polyols such as polybutylene carbonate, polyhexamethylene carbonate, poly(3-methyl-1,5-pentylene) carbonate, poly(1,4-dimethylcyclohexylene) carbonate, polydiethylene glycol carbonate, polytetraethylene glycol carbonate, and polydipropylene glycol carbonate. Polyester-based polyurethanes are formed from polyester polyols. Polycarbonate-based polyurethanes are formed from polycarbonate polyols.

[0034] Examples of low-molecular-weight polyols having 2 to 20 carbon atoms that constitute the polyester polyols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, glycerin, diethylene glycol, trimethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, cyclohexanedimethanol, and methylpentanediol adipate.

[0035] The polyol may further contain, as an optional component, the above-mentioned low-molecular-weight polyols having 2 to 20 carbon atoms; (meth)acrylic polyols which are copolymers of hydroxyl-free (meth)acrylates such as methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and ethylene glycol (meth)acrylic acid diester with hydroxyl-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and ethylene glycol methacrylic acid monoester; and polyether polyols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, propylene oxide adducts thereof, propylene oxide adducts of glycerin, propylene oxide adducts of sugars such as sorbitol and sucrose, and propylene oxide adducts of compounds having active hydrogen such as ethylenediamine.

[0036] The polyols may be used alone or in combination of two or more kinds.

[0037] Examples of the isocyanate crosslinking agent include aliphatic polyisocyanates such as 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate; isophorone diisocyanate, trans- and / or cis-1,4-cyclohexane diisocyanate, norbornene diisocyanate, and 4,4'-methylenebiscyclohexyl diisocyanate. Examples of suitable crosslinking agents include alicyclic polyisocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, methylenebis(4-phenylisocyanate), 2,4'-diphenylmethane diisocyanate, and 2,2'-diphenylmethane diisocyanate; and biuret-modified, isocyanurate-modified, carbodiimide-modified, or adduct-modified polyisocyanates thereof. The isocyanate crosslinking agents may be used alone or in combination of two or more.

[0038] The equivalent ratio (NCO / OH) of polyol to isocyanate crosslinker can be about 0.5 or greater, about 0.7 or greater, or about 0.9 or greater, and about 2.5 or less, about 2.0 or less, or about 1.5 or less.

[0039] The reactive polyurethane composition may contain a catalyst, such as dibutyltin dilaurate (DBTDL), zinc naphthenate, zinc octenate, and triethylenediamine. The amount of catalyst used is typically about 0.005 parts by weight or more and about 0.5 parts by weight or less, based on 100 parts by weight of the polyol and isocyanate crosslinker combined.

[0040] The reactive polyurethane composition may be water-based or organic solvent-based. In the case of a water-based composition, further crosslinking can be performed using polycarbodiimide, aziridine, oxazoline, etc. Water-based reactive polyurethane compositions preferably contain a combination of polycarbonate polyol with polycarbodiimide, 4,4'-methylenebiscyclohexyldiisocyanate, and / or aziridine. Organic solvent-based reactive polyurethane compositions preferably contain a combination of polycaprolactone diol and polycarbonate diol with isophorone diisocyanate trimer (isocyanurate).

[0041] The polyurethane layer may optionally contain additives such as benzotriazole, ultraviolet absorbers such as Tinuvin® 99-2 (BASF Japan Ltd., Chuo-ku, Tokyo, Japan) and Tinuvin® 1130 (BASF Japan Ltd.), and hindered amine light stabilizers (HALS) such as Tinuvin® 292 (BASF Japan Ltd.). The use of ultraviolet absorbers or hindered amine light stabilizers can effectively prevent discoloration, fading, deterioration, and other problems when the base layer contains a decorative layer or colorant. The polyurethane layer may also contain a hard coat material, a gloss-imparting agent, and the like. The polyurethane layer may be transparent or translucent to achieve the desired appearance. It is advantageous for the polyurethane layer to be transparent.

[0042] The thickness of the polyurethane layer may vary, but is generally about 1 μm or more, about 5 μm or more, or about 10 μm or more, and about 100 μm or less, about 80 μm or less, or about 60 μm or less. When applying a decorative film to an article with a complex shape, a thinner polyurethane layer is advantageous in terms of shape conformability, and for example, a thickness of about 80 μm or less or about 60 μm or less is desirable. On the other hand, when imparting high light resistance or weather resistance to the article, a thicker polyurethane layer is advantageous, and for example, a thickness of about 5 μm or more or about 10 μm or more is desirable.

[0043] In a decorative film with a cover film, a balance is required between the adhesion of the removable cover film to the polyurethane layer, i.e., the cover film does not fall off during production, transportation, or operation, and the peelability of the removable cover film, i.e., the cover film can be easily removed during or after application. In the present disclosure, a corona treatment or plasma treatment is performed on the surface of the removable cover film as a means to achieve such a balance.

[0044] The removable cover film protects the surface of the polyurethane layer until the polyurethane contained in the polyurethane layer is completely crosslinked, and also during production, transportation, or use of the decorative film, or contributes to improving the surface quality of the polyurethane layer by transferring the smooth surface of the removable cover film to the polyurethane layer. The removable cover film can also be used as a support for the decorative film during production, transportation, or use.

[0045] The removable cover film may be a resin film made of polyvinyl chloride, polyolefin such as polyethylene or polypropylene, acrylic resin, polyester such as polyethylene terephthalate or polybutylene terephthalate, or a fluorine-based polymer.

[0046] The removable cover film is preferably a polyethylene terephthalate film, which can effectively prevent damage to the polyurethane layer and maintain or improve the surface quality of the polyurethane layer.

[0047] The polyethylene terephthalate film is advantageously a biaxially oriented polyethylene terephthalate film, which has high elongation at break and tensile strength, thereby effectively preventing damage to the polyurethane layer and maintaining or improving the surface quality of the polyurethane layer.

[0048] The surface of the removable cover film that comes into contact with the first side of the polyurethane layer is subjected to corona treatment or plasma treatment. Corona treatment and plasma treatment can impart to the removable cover film sufficient adhesion to the polyurethane layer, even when the polyurethane layer contains polyurethane in which crosslinking has progressed relatively well during formation, so that the removable cover film will not fall off during production, transportation, or use of the decorative film with cover film, and will be removable when the decorative film with cover film is installed.

[0049] In one embodiment, corona treatment and plasma treatment can clean the surface of the removable cover film, thereby reducing or eliminating foreign matter that gets caught between the removable cover film and the polyurethane layer, resulting in a higher surface quality of the polyurethane layer.

[0050] In one embodiment, the corona treatment and plasma treatment can remove static electricity that has accumulated on the surface of the removable cover film when it is unwound from the roll, thereby preventing foreign matter such as dust and dirt from adhering to the surface of the removable cover film, thereby reducing or eliminating foreign matter that gets caught between the removable cover film and the polyurethane layer, and as a result, the surface quality of the polyurethane layer can be improved.

[0051] Corona treatment can be carried out using a corona treatment device commonly used for surface modification of resin films. Examples of corona treatment devices include GXR50 (Sherman Treaters Ltd., Thame, Oxfordshire, UK) and TEG-4AX (Kasuga Electric Co., Ltd., Kawasaki, Kanagawa Prefecture, Japan). The conditions for corona treatment are not particularly limited, but examples include an applied power of 1 kW to 5 kW, a corona treatment time of 0.05 seconds to 5 seconds, and a frequency of 10 kHz to 20 kHz. Discharge during corona treatment may be continuous or intermittent.

[0052] The plasma treatment can be carried out using a plasma treatment device commonly used for surface modification of resin films. Examples of plasma treatment devices include atmospheric pressure plasma treatment devices and low-pressure plasma treatment devices. The conditions for the plasma treatment are not particularly limited, but can be, for example, nitrogen gas or a rare gas such as helium or argon as the plasma gas, power of 0.5 kW to 4 kW, plasma gas supply rate of 50 liters per minute to 150 liters per minute, atmospheric pressure inside the plasma treatment device, and plasma treatment time of 0.05 seconds to 5 seconds.

[0053] The corona- or plasma-treated surface of the removable cover film preferably has a surface tension of about 40 mN / m or greater. More preferably, the surface tension is about 44 mN / m or greater, or about 46 mN / m or greater. The corona- or plasma-treated surface of the removable cover film generally has a surface tension of about 60 mN / m or less. More preferably, the surface tension is about 58 mN / m or less, or about 56 mN / m or less.

[0054] The surface of the removable cover film opposite the corona- or plasma-treated surface may not have a corona or plasma treatment. In one embodiment, the surface tension of the removable cover film opposite the corona- or plasma-treated surface is less than about 40 mN / m, about 39 mN / m or less, or about 38 mN / m or less.

[0055] The corona-treated or plasma-treated surface of the removable cover film may be subjected to a surface treatment for transferring a shape to the surface of the polyurethane layer. Examples of surface treatments include matte finish, embossing, and sandblasting. The surface opposite to the corona-treated or plasma-treated surface of the removable cover film may be subjected to a surface treatment for imparting lubricity, releasability, etc.

[0056] The thickness of the removable cover film can be about 5 μm or more, about 10 μm or more, or about 25 μm or more, and about 150 μm or less, about 100 μm or less, or about 80 μm or less.

[0057] The base layer can be, for example, a resin film made of polyurethane, polyvinyl chloride, polyolefins such as polyethylene and polypropylene, acrylic resins, polyesters such as polyethylene terephthalate and polybutylene terephthalate, or fluorine-based polymers. The base layer preferably contains at least one thermoplastic resin selected from the group consisting of polyurethane, polyvinyl chloride, polyolefins, acrylic resins, and polyesters. In this embodiment, the decorative film can be applied to curved articles with excellent conformability by hand application, dual vacuum thermoforming (DVT), or vacuum thermoforming (VT).

[0058] The base layer may be colored. Examples of colorants include organic pigments, inorganic pigments, aluminum luster pigments, and mica luster pigments, as well as blends of two or more of these. The colorant is preferably selected from the group consisting of a combination of an organic pigment and an inorganic pigment, a combination of an organic pigment and an aluminum luster pigment, a combination of an organic pigment and a mica luster pigment, a combination of an inorganic pigment and an aluminum luster pigment, a combination of an inorganic pigment and a mica luster pigment, and a combination of an aluminum luster pigment and a mica luster pigment, and combinations thereof. Using the above combinations of colorants allows for the production of decorative films with a wide variety of color tones, thereby meeting sophisticated design requirements.

[0059] Examples of organic pigments include phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green, azo lake pigments, indigo pigments, perinone pigments, perylene pigments, quinophthalone pigments, dioxazine pigments, and quinacridone pigments such as quinacridone red. Examples of inorganic pigments include titanium dioxide, yellow lead, yellow iron oxide, red iron oxide, red iron oxide, and carbon black. Examples of aluminum luster materials include aluminum flakes, vapor-deposited aluminum flakes, metal oxide-coated aluminum flakes, and colored aluminum flakes. Examples of mica luster materials include flake-shaped mica coated with titanium dioxide, iron oxide, and other metal oxides, and synthetic mica.

[0060] The colorant content can be about 1% by weight or more, about 2% by weight or more, or about 5% by weight or more, and about 80% by weight or less, about 75% by weight or less, or about 66% by weight or less, based on the weight of the base layer.

[0061] In one embodiment, the base layer has a multi-layer structure including a decorative layer. In another embodiment of the decorative film 10 with a cover film shown in Figure 2, the base layer 16 has a multi-layer structure including a base film 162 and a decorative layer 164.

[0062] The base film may be the resin film described above for the base layer. The thickness of the base film is preferably about 10 μm or more and about 500 μm or less, more preferably about 30 μm or more and about 300 μm or less, and even more preferably about 80 μm or more and about 200 μm or less.

[0063] Examples of decorative layers include colored layers (color layers), patterned films (patterned films), and metallic layers. Specifically, the decorative layer can be a layer, coating, film, or metal-deposited film that imparts a metallic appearance (metallic, silver metallic, etc.), an automobile exterior panel paint color (paint color such as metallic, white pearl, pearl mica, solid), a pattern, a logo, a design, etc. to the decorative film.

[0064] In one embodiment, the decorative layer is a colored layer. The colored layer generally contains a binder resin and a colorant.

[0065] Examples of binder resins include acrylic resins, polyurethanes, polyvinyl chloride, and polyesters. The binder resin preferably includes a thermoplastic resin, more preferably a thermoplastic acrylic resin. In this embodiment, the decorative film can be applied to curved articles with excellent conformability by hand application, dual vacuum thermoforming (DVT), or vacuum thermoforming (VT).

[0066] The colorant may be the same as that described for the colored base layer, and the colorant content may be about 1% by weight or more, about 2% by weight or more, or about 5% by weight or more, and about 80% by weight or less, about 75% by weight or less, or about 67% by weight or less, based on the weight of the colored layer.

[0067] The colored layer can be formed by applying a colored layer composition containing a binder resin, a colorant, and, if necessary, a solvent onto a base film by knife coating, bar coating, blade coating, doctor coating, roll coating, cast coating, gravure coating, or the like, and heating if necessary.

[0068] The thickness of the color layer may vary, but is generally about 1 μm or more, about 10 μm or more, or about 20 μm or more, and about 100 μm or less, about 80 μm or less, or about 60 μm or less. A color layer thickness of about 10 μm or more can conceal the base color and provide a desired decorative appearance. When high conformability is required, a thinner color layer is advantageous, and a thickness of about 80 μm or less, or about 60 μm or less, is desirable.

[0069] The thickness of the base layer is preferably about 10 μm or more and about 500 μm or less, more preferably about 30 μm or more and about 300 μm or less, and even more preferably about 80 μm or more and about 200 μm or less. Considering the resistance to flying stones when the decorative film is used on the underside or front of a car's side, the thickness of the base layer is preferably about 80 μm or more. Except when the decorative film is temporarily applied to the surface of an adherend as a protective tape, the thickness of the base layer is preferably about 30 μm or more because it is less likely to wrinkle when applied to a curved surface. If the decorative film is too thick, its ability to conform to a curved surface tends to be impaired. Also, from an economical standpoint, it is advantageous for the thickness of the base layer to be about 300 μm or less. When the base layer has a multilayer structure, the thickness of the base layer refers to the total thickness of each layer.

[0070] The adhesive layer includes commonly used acrylic, polyolefin, polyurethane, polyester, rubber, silicone, or vinyl acetate adhesives. The adhesive layer can be formed using a solvent-based, emulsion-based, pressure-sensitive, heat-sensitive, heat-curable, or ultraviolet-curable adhesive composition. The adhesive layer may be a pressure-sensitive adhesive layer.

[0071] The adhesive layer may contain achromatic pigments such as white pigments, black pigments, or mixtures thereof, chromatic pigments such as yellow pigments, red pigments, green pigments, blue pigments, and orange pigments, or combinations thereof. An adhesive layer containing a white pigment also functions as a concealing layer that conceals the surface (base) of the adherend. Titanium dioxide is preferably used as the white pigment because of its high whiteness.

[0072] The adhesive layer can be formed using an adhesive composition. Specifically, the adhesive layer can be formed by applying the adhesive composition to the second surface of the base layer and heating it as needed. Alternatively, the adhesive composition can be applied to a separate liner and heated as needed to form an adhesive layer, which can then be transfer-laminated onto the second surface of the base layer. For example, the adhesive layer can be formed by applying the adhesive composition to the base layer or liner by knife coating, bar coating, blade coating, doctor coating, roll coating, cast coating, or the like, and heating it as needed. The liner may have a surface that has been treated with a release agent such as silicone.

[0073] The thickness of the adhesive layer may vary, but is generally about 5 μm or more, about 10 μm or more, or about 20 μm or more, and about 100 μm or less, about 80 μm or less, or about 50 μm or less. To ensure that the adhesive layer conforms to the irregularities of the adherend surface and achieves high adhesive strength that is less likely to peel, the thickness of the adhesive layer is preferably about 20 μm or more. To reduce the phenomenon in which the decorative film shrinks in a high-temperature environment after being stretched and attached, causing the adhesive to protrude from the edges of the decorative film, the thickness of the adhesive layer is preferably about 50 μm or less.

[0074] The decorative film may have a liner to protect the adhesive layer. Examples of the liner include paper, plastic materials such as polyethylene, polypropylene, polyester, and cellulose acetate, and paper coated with such plastic materials. These liners may have a release-treated surface, such as with silicone. The thickness of the liner is generally about 5 μm or more, about 15 μm or more, or about 25 μm or more, and about 300 μm or less, about 200 μm or less, or about 150 μm or less.

[0075] The adhesive layer generally forms a flat adhesive surface, but may also form an uneven adhesive surface. This uneven adhesive surface includes an adhesive surface in which convex portions containing adhesive and concave portions surrounding the convex portions are formed on the adhesive surface of the adhesive layer, and when adhered to an adherend, a communication path defined by the concave portions is formed between the adherend surface and the adhesive surface, which communicates with the outside. An example of a method for forming an uneven adhesive surface is described below.

[0076] A liner with a release surface having a predetermined uneven structure is prepared. An adhesive composition is applied to the release surface of this liner and heated as necessary to form an adhesive layer. This transfers the uneven structure (negative structure) of the liner to the surface of the adhesive layer that contacts the liner (this becomes the adhesive surface of the decorative film), forming an uneven adhesive surface with a predetermined structure (positive structure) on the adhesive surface. As described above, the unevenness of the adhesive surface is designed in advance to include grooves that can form communication paths when the convex portions are adhered to the adherend.

[0077] The grooves in the adhesive layer may be formed by arranging grooves of a fixed shape along a regular pattern on the adhesive surface, or by arranging grooves of an indefinite shape to form an irregular pattern, as long as this prevents air bubbles from remaining when the decorative film is attached to an article. When multiple grooves are formed so as to be arranged approximately parallel to each other, the groove spacing is preferably 10 to 2000 μm. The groove depth (the distance from the adhesive surface to the bottom of the groove measured toward the base layer) is typically approximately 10 μm or more and approximately 100 μm or less. The shape of the groove is also not particularly limited as long as it does not impair the effects of the present invention. For example, the groove shape can be approximately rectangular (including trapezoidal), approximately semicircular, or approximately semielliptical in the cross section of the groove perpendicular to the adhesive surface.

[0078] The decorative film with a cover film can be produced, for example, by a method including the following steps. (a) providing a base layer having a first side and a second side opposite the first side; (b) forming a polyurethane layer on the first surface of the base layer, the polyurethane layer having a first surface and a second surface opposite the first surface, the polyurethane layer comprising at least a partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane, and the first surface of the base layer contacting the second surface of the polyurethane layer; (c) providing a removable cover film (d) treating the surface of the removable cover film with corona or plasma; (e) laminating a removable cover film onto the polyurethane layer such that the corona-treated or plasma-treated surface of the removable cover film contacts the first side of the polyurethane layer; (f) forming an adhesive layer on the second surface of the base layer to obtain a decorative film with a cover film;

[0079] The base layer provided in step (a) may be any of those described above. The base layer may be provided with a process film as a support on its second surface.

[0080] The formation of the polyurethane layer in step (b) can be carried out as described above. The polyurethane contained in the polyurethane layer is at least partially crosslinked. It is preferred that the polyurethane is not completely crosslinked upon completion of step (b). In this embodiment, the removable cover film can be more firmly attached to the polyurethane layer in step (e).

[0081] The removable cover film in step (c) can be any of those described above.

[0082] The corona or plasma treatment in step (d) can be carried out as described above. In one embodiment, the corona or plasma treatment is carried out so that the surface tension of the removable cover film is about 40 mN / m or more. After the corona or plasma treatment is completed, step (e) is carried out preferably within 1 hour, more preferably within 10 minutes. It is more preferred that steps (d) and (e) are carried out as a continuous process.

[0083] The step (e) of laminating the removable cover film is preferably carried out before the polyurethane is completely crosslinked. By laminating the removable cover film in a state where the polyurethane is partially crosslinked, the removable cover film can be more firmly adhered to the polyurethane layer.

[0084] In one embodiment, after step (e), the removable cover film has a peel strength of about 0.15 to about 2.0 N / 50 mm when peeled from the polyurethane layer after storage for 48 hours at 23° C. The peel strength is determined under the same conditions as in the method for measuring the peel strength of a decorative film with a cover film described in the examples.

[0085] The peel force measured after 48 hours of storage at 23°C following step (e) can be used as an indicator of the extent to which the crosslinking reaction of the polyurethane contained in the polyurethane layer formed in step (b) has progressed at the completion of step (e). Specifically, if the crosslinking reaction of the polyurethane is in the early stages, the cohesive strength within the polyurethane layer is low, resulting in cohesive failure of the polyurethane layer rather than interfacial peeling between the polyurethane layer and the removable cover film, resulting in an apparent low measured peel force. As the crosslinking reaction of the polyurethane progresses, the cohesive strength within the polyurethane layer exceeds the interfacial peel strength between the polyurethane layer and the removable cover film, resulting in interfacial peeling between the polyurethane layer and the removable cover film. However, the interior and surface of the polyurethane layer remain soft, and the surface of the polyurethane layer is too tacky, resulting in a high measured peel force. As the crosslinking reaction of the polyurethane progresses further, the adhesiveness of the surface of the polyurethane layer decreases, and the peel force decreases. At this point, the surface of the polyurethane layer has sufficient adhesiveness to allow a corona-treated or plasma-treated cover film to adhere well, and the hardness of the polyurethane layer is increased to a level that can suppress surface defects such as craters. As the polyurethane approaches complete crosslinking, the peel force decreases further and the removable cover film no longer adheres to the surface of the polyurethane layer with sufficient force.

[0086] By selecting the materials and formulation of the polyurethane layer composition, the conditions for forming the polyurethane layer in step (b), and the conditions for the corona treatment or plasma treatment in step (d) so that the peel force is about 0.15 to about 2.0 N / 50 mm, it is possible to appropriately increase the hardness of the polyurethane layer while ensuring adhesion of the removable cover film to the polyurethane layer. This suppresses the occurrence of surface defects such as craters in the polyurethane layer and prevents the removable cover film from falling off during production, transportation, and use of the decorative film with a cover film.

[0087] The adhesive layer can be formed in step (f) as described above. A decorative film with a cover film may be obtained in a state where a release liner covers the adhesive layer.

[0088] The method for producing a decorative film with a cover film may optionally further include the following step (g). (g) A process of winding up the decorative film with the cover film into a roll after forming the adhesive layer.

[0089] In step (g), the decorative film with the cover film can be wound around the core using a winding device used in ordinary film production. In this embodiment, the decorative film with the cover film can be stored and transported in roll form without deteriorating the surface quality of the decorative film.

[0090] In one embodiment, the decorative film is produced by including the following step (h) after step (f). (h) removing the removable cover film from the first side of the polyurethane layer.

[0091] Step (h) involves continuously peeling the cover film using a winding device or manually peeling the cover film from the cut decorative film.

[0092] The total thickness of the decorative film, excluding the thickness of the cover film and liner, can be about 25 μm or more, about 80 μm or more, or about 150 μm or more, and about 600 μm or less, about 400 μm or less, or about 350 μm or less.

[0093] In one embodiment, the peel force of the removable cover film in the decorative film with a cover film is about 0.15 N / 50 mm or more, about 0.2 N / 50 mm or more, about 0.25 N / 50 mm or more, about 1.0 N / 50 mm or less, about 0.8 N / 50 mm or less, or about 0.5 N / 50 mm or less. The peel force is determined by the method described in the Examples.

[0094] The decorative film with cover film may be in the form of a wound roll, which allows the surface quality of the decorative film to be maintained even if air is trapped between two overlapping decorative films due to the wound film.

[0095] In one embodiment, a method for applying the decorative film includes applying the decorative film with a cover film to a substrate and then removing the removable cover film from the first surface of the polyurethane layer. In this embodiment, because the polyurethane layer is protected by the removable cover film, the decorative film can be firmly adhered to the substrate by pressing the decorative film onto the removable cover film using a crimping tool or the like while maintaining the surface quality of the decorative film.

[0096] Another embodiment of a decorative film application method includes removing the removable cover film of the cover film-attached decorative film from the first surface of the polyurethane layer to obtain a decorative film, and applying the decorative film to a substrate. In this embodiment, removing the removable cover film before applying the decorative film allows the decorative film to exhibit its inherent shape-conforming ability. Therefore, the decorative film can be applied with excellent shape-conforming ability to substrates with three-dimensional surfaces, such as corners, curved surfaces, and uneven shapes.

[0097] The decorative film of the present disclosure can be suitably used as a paint replacement film. For example, the decorative film of the present disclosure can be applied to the vehicle body (including the roof, doors, hood, etc.) or a part thereof, or to vehicle components (for example, bumpers, roof moldings, side guard moldings, pillars, etc.). Examples of vehicles include automobiles such as trucks, buses, and passenger cars, two-wheeled vehicles such as motorcycles and scooters, bicycles, trains, and ships such as pleasure boats, yachts, and motorboats. [Example]

[0098] The following examples illustrate specific embodiments of the present disclosure, but do not limit the present invention. All parts and percentages are by weight unless otherwise specified. Numerical values ​​inherently contain errors resulting from measurement principles and measuring devices. Numerical values ​​are presented to significant digits with ordinary rounding procedures.

[0099] The raw materials used in the polyurethane layer composition are shown in Table 1.

[0100] [Table 1]

[0101] Comparative Example 1 The decorative film with a cover film of Comparative Example 1 was produced in the following manner.

[0102] (1) A black pigment-containing acrylic composition having the composition shown in Table 2 was applied to a 150 μm thick thermoplastic polyurethane film (Seedam Co., Ltd., Osaka City, Osaka Prefecture, Japan) supported on an 80 μm thick polypropylene film as a process film, and heated in a continuous oven at 80°C for 5 minutes to form a colored layer with a dry thickness of 23 μm on the thermoplastic polyurethane film, thereby producing a base layer with a multilayer structure including a colored layer and a base film.

[0103] [Table 2]

[0104] (2) A polyurethane layer composition with a solids content of 76.5% by mass, prepared according to the composition shown in Table 3, was applied to the colored layer side of the base layer formed in (1) and heated in a continuous oven at 80°C for 3 minutes and 20 seconds to form a polyurethane layer with a dry thickness of 25 μm, containing at least partially crosslinked polyester-based polyurethane and polycarbonate-based polyurethane.

[0105] [Table 3]

[0106] (3) Immediately after the polyurethane layer was formed, a 50 μm thick polyethylene terephthalate cover film was laminated onto the surface of the polyurethane layer.

[0107] (4) An acrylic pressure-sensitive adhesive containing 2-ethylhexyl acrylate and acrylic acid was coated onto a silicone-coated polyethylene terephthalate release liner and heated in a continuous oven at 80°C for 5 minutes to form a pressure-sensitive adhesive layer with a dry thickness of 35 μm.

[0108] (5) The process film was removed from the laminate formed in (3), and the base film side of the base layer was laminated so that it was in contact with the pressure-sensitive adhesive layer formed in (4), to produce a decorative film with a cover film.

[0109] Comparative Example 2 A decorative film with a cover film was produced in the same manner as in Comparative Example 1, except that the heating time in the continuous oven during the formation of the polyurethane layer was changed to 8 minutes and 20 seconds.

[0110] Example 1 A decorative film with a cover film was produced in the same manner as in Comparative Example 2, except that the polyethylene terephthalate cover film was plasma treated under the following conditions immediately before lamination. Plasma treatment device: AP-T04-R1400 (Sekisui Chemical Co., Ltd., Osaka City, Osaka Prefecture, Japan) N2 flow rate: 100L / min Voltage: 360V Current: 3.5A

[0111] Example 2 A decorative film with a cover film was produced in the same manner as in Comparative Example 2, except that a corona treatment was carried out under the following conditions immediately before laminating the polyethylene terephthalate cover film. Corona treatment device: GX50R (Sherman Treaters Ltd., Thame, Oxfordshire, UK) Output: 2kW

[0112] Example 3 A decorative film with a cover film of Example 3 was produced in the same manner as in Example 2.

[0113] Example 4 A decorative film with a cover film was produced in the same manner as in Example 2, except that the output of the corona treatment was changed to 3 kW.

[0114] Surface quality (crater defects) After removing the cover film from the decorative films with cover film of Examples 1 to 4 and Comparative Examples 1 and 2, the film was visually inspected to see if it contained any particles with a size of 0.3 mm or less compared to a foreign matter measurement chart (manufactured by the National Printing Bureau, sold by Choyokai Co., Ltd., Soka City, Saitama Prefecture, Japan). 2 The number of craters equivalent to the above was counted.

[0115] Peeling force The decorative film with cover film was cut into a 50 mm wide and 200 mm long specimen. Using an Autograph AGS-X 500N (Shimadzu Corporation, Kyoto, Japan), the cover film was peeled off at a 180° angle at room temperature (23°C) at a peeling speed of 200 mm / min. The average of two measurements was used as the peel force (N / 50 mm).

[0116] surface tension Surface tension was assessed using a water-based surface tension reagent, EnerDyne® Pen (Enercon Industries Corp., Menomonee Falls, Wisconsin, USA).

[0117] Details and evaluation results of the decorative films with cover films of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 4. The number of days after lamination in Table 4 refers to how many days after lamination of the cover film the surface tension and peel force measurements were performed.

[0118] [Table 4-1]

[0119] [Table 4-2]

[0120] It will be apparent to those skilled in the art that the above-described embodiments and examples may be modified in various ways without departing from the basic principles of the present invention, and that various improvements and modifications of the present invention may be made without departing from the spirit and scope of the present invention. [Explanation of symbols]

[0121] 10, 10a Decorative film with cover film 12, 12a, 12b Removable cover film 122 Corona-treated or plasma-treated surfaces 14, 14a, 14b Polyurethane layer 16, 16a, 16b base layer 162 Base Film 164 Decorative layer 18, 18a adhesive layer 20, 20a liner 30a, 30b Intermediate member 32a, 32b Process film 40 Air 42 Crater

Claims

1. (a) a polyurethane layer having a first side and a second side opposite the first side, the polyurethane layer comprising an at least partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane; (b) a removable cover film having a corona-treated or plasma-treated surface, the corona-treated or plasma-treated surface of the removable cover film being in contact with the first side of the polyurethane layer; and (c) a base layer having a first side and a second side opposite the first side, the first side of the base layer contacting the second side of the polyurethane layer; and (d) an adhesive layer in contact with the second surface of the base layer; and Including, decorative film with cover film.

2. 2. The decorative film with cover film according to claim 1, wherein the corona-treated or plasma-treated surface of the removable cover film has a surface tension of 40 mN / m or more.

3. 3. The decorative film with a cover film according to claim 1, wherein the peel strength of the removable cover film is 0.15 to 1.0 N / 50 mm.

4. 4. The decorative film with cover film according to claim 1, wherein the surface of the removable cover film opposite the corona-treated or plasma-treated surface has a surface tension of less than 40 mN / m.

5. 5. The decorative film with a cover film according to claim 1, wherein the removable cover film is a polyethylene terephthalate film.

6. The decorative film with cover film according to any one of claims 1 to 5, wherein the base layer contains at least one thermoplastic resin selected from the group consisting of polyurethane, polyvinyl chloride, polyolefin, acrylic resin and polyester.

7. The decorative film with a cover film according to any one of claims 1 to 6, wherein the base layer has a multi-layer structure including a decorative layer.

8. (a) providing a base layer having a first side and a second side opposite the first side; (b) forming a polyurethane layer on the first side of the base layer, the polyurethane layer having a first side and a second side opposite the first side, the polyurethane layer comprising at least a partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane, the first side of the base layer contacting the second side of the polyurethane layer; (c) providing a removable cover film; (d) treating the surface of the removable cover film with corona or plasma; (e) laminating the removable cover film onto the polyurethane layer such that the corona-treated or plasma-treated surface of the removable cover film contacts the first side of the polyurethane layer; and (f) forming an adhesive layer on the second surface of the base layer to obtain a decorative film with a cover film; A method for producing a decorative film with a cover film, comprising:

9. 9. The method of claim 8, wherein the surface of the removable cover film is corona or plasma treated such that the surface tension of the removable cover film is 40 mN / m or more.

10. 10. The method according to claim 8 or 9, wherein after step (e), when the removable cover film is peeled off from the polyurethane layer after storage at 23° C. for 48 hours, the peel strength of the removable cover film is 0.15 to 2.0 N / 50 mm.

11. The method of any one of claims 8 to 10, wherein the removable cover film is a polyethylene terephthalate film.

12. (a) providing a base layer having a first side and a second side opposite the first side; (b) forming a polyurethane layer on the first side of the base layer, the polyurethane layer having a first side and a second side opposite the first side, the polyurethane layer comprising at least a partially crosslinked polyurethane, the at least partially crosslinked polyurethane comprising at least one of a polyester-based polyurethane and a polycarbonate-based polyurethane, the first side of the base layer contacting the second side of the polyurethane layer; (c) providing a removable cover film; (d) treating the surface of the removable cover film with corona or plasma; (e) laminating the removable cover film onto the polyurethane layer such that the corona-treated or plasma-treated surface of the removable cover film contacts the first side of the polyurethane layer; (f) forming an adhesive layer on the second surface of the base layer; and (h) removing the removable cover film from the first side of the polyurethane layer. A method for producing a decorative film comprising:

13. Applying the decorative film with cover film according to any one of claims 1 to 7 to a substrate; and Thereafter, removing the removable cover film from the first surface of the polyurethane layer. A method for applying a decorative film comprising: