Laminated tube
Patent Information
- Application Number
- JP2021202598
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-14
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-12-14
AI Technical Summary
The interlayer adhesion between polypropylene resin and polyamide resin layers in laminated tubes is low, leading to potential tube rupture under internal pressure and decreased adhesion after annealing, and the use of adhesives complicates the bonding process.
A laminated tube structure with a maleic anhydride-modified polypropylene resin layer containing organic particles and a polyamide resin layer with a specific amine value, forming protrusions at the interface to enhance chemical bonding and anchoring effect, thereby improving interlayer adhesion without adhesives.
The laminated tube exhibits excellent interlayer adhesion and maintains strength and heat resistance, preventing tube rupture and adhesion loss during annealing, while eliminating the need for adhesives.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to a laminated tube used for piping in a cooling system inside a vehicle such as an automobile.
Background Art
[0002] Conventionally, polyamide resin has been adopted as the piping material for the cooling system inside a gasoline vehicle because of its excellent strength and heat resistance. Also, conventionally, the same polyamide resin as that used in gasoline vehicles has been adopted as the piping material for the cooling system inside an electric vehicle. In recent years, as the electrification of vehicles such as automobiles progresses, the need to cool the inside of electric vehicles has been increasing more and more.
[0003] However, tubes made of polyamide resin still have problems in terms of price. Therefore, the use of tubes made of inexpensive polypropylene resin has also been considered to solve the above problems. Also, laminated tubes that utilize the characteristics of both layers and are low-cost and highly functional by laminating a polyamide resin layer and a polypropylene resin layer have been considered (see Patent Documents 1 and 2).
Prior Art Documents
Patent Documents
[0004]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0005] However, the interlayer adhesion between the polypropylene resin layer and the polyamide resin layer is low. Without sufficient interlayer adhesion, the outer layer of the tube is not protected, leading to problems such as the tube being prone to bursting due to the internal pressure of the fluid flowing through it. Furthermore, when bending such laminated tubes, annealing (heat treatment) is performed near the melting point of each layer's resin, which can easily reduce interlayer adhesion.
[0006] Therefore, bonding the polyamide resin layer and the polypropylene resin layer by applying an adhesive is being considered, but there are drawbacks in terms of the labor costs associated with this bonding process. Furthermore, in the tube disclosed in Patent Document 2, the polypropylene resin layer is made of maleic anhydride-modified polypropylene resin, thereby improving adhesion with the polyamide resin layer. However, problems remain, such as the tendency for interlayer adhesion to decrease due to annealing (heat treatment) performed when bending the laminated tube. Therefore, there is still room for improvement in this respect.
[0007] This invention has been made in view of these circumstances, and aims to provide a laminated tube that is excellent in strength and heat resistance, exhibits excellent interlayer adhesion without adhesive, and also has good interlayer adhesion after annealing. [Means for solving the problem]
[0008] The inventors diligently conducted research to solve the aforementioned problems. In the course of this research, they investigated improvements to interlayer adhesion and other properties for tubes having a laminated structure of a maleic anhydride-modified polypropylene resin layer and a polyamide resin layer through various experiments. As a result, we conceived of using a polyamide resin with an amine value of 15 to 100 mmol / kg as the polyamide resin in the polyamide resin layer, and further adding organic particles with a specific particle size to the material of the polypropylene resin layer, and through improvements in the manufacturing method, causing numerous convex ridges to appear on the polypropylene resin layer side at the interface between the polyamide resin layer and the polypropylene resin layer due to the organic particles. In this manner, we discovered that the chemical bonding between the amino groups of the polyamide resin and the maleic anhydride-modified groups of the polypropylene resin improves the interlayer adhesion between the two layers. Furthermore, the anchoring effect of the convex ridges increases the contact area between the two layers and improves the frictional force, leading to more effective interlayer adhesion. Therefore, we found that it is possible to further improve the interlayer adhesion between the two layers even without adhesive, and that problems such as the decrease in interlayer adhesion due to annealing and the resulting tube rupture can be resolved.
[0009] In other words, the gist of the present invention is as follows: [1] to [6]. [1] A laminated tube having a layer structure in which a polypropylene resin layer and a polyamide resin layer are laminated in close contact, The polypropylene resin in the aforementioned polypropylene resin layer is maleic anhydride-modified polypropylene, and the polypropylene resin layer contains organic particles with an average particle size of 0.1 to 10 μm. The polyamide resin in the aforementioned polyamide resin layer is a polyamide resin with an amine value of 15 to 100 mmol / kg. At the interface between the polypropylene resin layer and the polyamide resin layer, the polypropylene resin layer side has numerous convex ridges formed by the organic particles, Laminated tube. [2] The laminated tube according to [1], wherein the height of the convex ridge is in the range of 0.1 to 10 μm. [3] The laminated tube according to [1] or [2], wherein the number of convex ridges in a straight line distance at the interface between the polypropylene resin layer and the polyamide resin layer is 2 to 20 per 100 μm. [4] The laminated tube according to any one of [1] to [3], wherein the proportion of organic particles in the polypropylene resin layer is 5 to 20% by mass. [5] The laminated tube according to any one of [1] to [4], wherein the organic particles consist of at least one of polyethylene and an ethylene-propylene copolymer. [6] The laminated tube according to any one of [1] to [5], wherein the polypropylene resin layer is an inner layer and the polyamide resin layer is an outer layer. [Effects of the Invention]
[0010] Based on the above, the laminated tube of the present invention exhibits excellent strength and heat resistance, as well as excellent interlayer adhesion even without adhesive, and can maintain good interlayer adhesion even after annealing. Therefore, it is possible to eliminate problems such as the decrease in interlayer adhesion due to annealing and the resulting tube rupture. [Brief explanation of the drawing]
[0011] [Figure 1] This is an explanatory diagram showing an example of a laminated tube according to the present invention. [Figure 2] This is a schematic diagram showing the stacked state of the laminated tube according to the present invention. [Modes for carrying out the invention]
[0012] Next, embodiments of the present invention will be described in detail. However, the present invention is not limited to these embodiments. In this invention, when "X~Y" (where X and Y are any numbers) is used, unless otherwise specified, it means "X or greater and Y or less," and also includes the meaning of "preferably greater than X" or "preferably less than Y."
[0013] A laminated tube (hereinafter referred to as "this laminated tube"), which is an embodiment of the present invention, is a tube having a structure in which a polypropylene resin layer and a polyamide resin layer are laminated in an adhered state (directly). And, the polypropylene resin in the polypropylene resin layer is maleic anhydride-modified polypropylene, and organic particles having an average particle diameter of 0.1 to 10 μm are contained in the polypropylene resin layer. The polyamide resin in the polyamide resin layer is a polyamide resin having an amine value of 15 to 100 mmol / kg. Further, the laminated tube has a large number of convex ridges formed by the organic particles on the side of the polypropylene resin layer at the interface between the polypropylene resin layer and the polyamide resin layer.
[0014] Here, FIG. 2 schematically shows the interface between the polypropylene resin layer and the polyamide resin layer. That is, in FIG. 2, 1 is a polypropylene resin layer, 2 is a polyamide resin layer, and 3 is an organic particle. As shown in the figure, on the side of the polypropylene resin layer 1 at the interface between the polypropylene resin layer 1 and the polyamide resin layer 2, there are a large number of convex ridges 1a formed by the organic particles 3. As described above, the average particle diameter of the organic particles 3 in the polypropylene resin layer 1 is in the range of 0.1 to 10 μm, preferably in the range of 0.1 to 5 μm, and more preferably in the range of 0.3 to 3 μm. That is, by showing such an average particle diameter, a large number of convex ridges 1a of a desired size can be formed on the side of the polypropylene resin layer 1 at the interface. Due to the anchoring effect, the contact area between the two layers increases and the frictional force also improves, so that the interlayer adhesion between the two layers can be improved. The average particle diameter of the organic particles 3 is obtained by cutting the laminated tube in half, photographing the laminated cross-section with a scanning electron microscope (SEM) at a magnification of 5000 times, and measuring the particle diameters of any 10 organic particles 3 confirmed in the polypropylene resin layer 1 based on the image, and then calculating the average.
[0015] Further, the height of the convex ridge 1a (the distance between the valley and the peak at the interface of the unevenness) is preferably in the range of 0.1 to 10 μm, more preferably in the range of 0.1 to 5 μm. Furthermore, the number of the convex ridges 1a in the linear distance at the interface between the polypropylene resin layer 1 and the polyamide resin layer 2 is preferably 2 to 20 per 100 μm, more preferably 3 to 15 per 100 μm. That is, by satisfying these regulations, the anchoring effect and the like due to the convex ridge 1a become higher, and the interlayer adhesion between the two layers can be improved, which is preferable. These measurements are performed by splitting the laminated tube in half, photographing the laminated cross-section with a scanning electron microscope (SEM) at a magnification of 5000 times, and measuring based on an image obtained by connecting 10 images thereof.
[0016] Next, the materials of the polypropylene resin layer 1 and the polyamide resin layer 2 will be described.
[0017] 《Material for the polypropylene resin layer 1》 As described above, the polypropylene resin used as the forming material of the polypropylene resin layer 1 is maleic anhydride-modified polypropylene. Note that 50% by mass or more of the material for the polypropylene resin layer 1 is occupied by maleic anhydride-modified polypropylene, including the case where the forming material of the polypropylene resin layer 1 other than the organic particles 3 consists only of maleic anhydride-modified polypropylene. And, the maleic anhydride-modified polypropylene preferably has a modification amount of 0.05 to 7% by mass, more preferably 0.1 to 5% by mass. That is, if the modification amount is too low, the interlayer adhesion tends to deteriorate, and conversely, if the modification amount is too high, the heat resistance tends to be inferior. Also, the maleic anhydride-modified polypropylene preferably has a melting point of 130 to 180°C, more preferably 140 to 170°C. That is, if the melting point is too low, the heat resistance tends to be inferior, and conversely, if the melting point is too high, the interlayer adhesion tends to deteriorate.
[0018] The organic particles 3 contained in the polypropylene resin layer 1 include particles made of organic materials such as rubber (ethylene-propylene copolymer, ethylene octene, ethylene butene, ethylene hexene, ethyl acrylate, etc.) and resin (polyethylene, etc.). These can be used alone or in combination of two or more. Among these, organic particles made of at least one of polyethylene and ethylene-propylene copolymer are preferred from the viewpoint of compatibility. The organic particles 3 may be pre-granulated to satisfy the specific average particle size described above and added to the material for the polypropylene resin layer 1. Alternatively, the resin or rubber that will be the material for the organic particles 3 may be melt-kneaded with maleic anhydride-modified polypropylene under specific conditions (melt-kneading in a twin-screw wrench at 200-250°C for 1-10 minutes) to form pellets, and then melt-extruded according to the conditions described below, so that the organic particles 3 appear in the polypropylene resin as a result.
[0019] The proportion of organic particles 3 in the polypropylene resin layer 1 is preferably 5 to 20% by mass, and more preferably 10 to 15% by mass. This is because including organic particles 3 in this proportion allows for good interlayer adhesion after annealing. Here, the proportion of organic particles 3 in the polypropylene resin layer 1 can be determined before the production of the laminated tube by the proportion of organic particles 3 (or the resin or rubber that makes up the organic particles 3) blended into the material for the polypropylene resin layer 1. After the production of the laminated tube, it can be determined by photographing the polypropylene resin layer 1 with a scanning electron microscope (SEM) at a magnification of 1000x and performing binarization processing, etc.
[0020] Furthermore, in addition to maleic anhydride-modified polypropylene and organic particles 3, the material for the polypropylene resin layer 1 may also contain weather stabilizers, lubricants, pigments, dyes, antistatic agents, plasticizers, heat-resistant anti-aging agents, etc., as needed. Furthermore, the material for the polypropylene resin layer 1 may be made by melting and kneading these materials together and then forming them into pellets, as needed.
[0021] Materials for polyamide resin layer 2 As mentioned earlier, the polyamide resin used as the forming material for the polyamide resin layer 2 is a polyamide resin with an amine value of 15 to 100 mmol / kg. Preferably, it is a polyamide resin with an amine value of 20 to 80 mmol / kg, and more preferably, a polyamide resin with an amine value of 25 to 60 mmol / kg. Using a polyamide resin with such an amine value results in superior interlayer adhesion to the polypropylene resin layer 1. If the amine value is too low, the interlayer adhesion tends to be poor, and conversely, if the amine value is too high, the extrusion moldability tends to be poor. Here, the amine value of the polyamide resin indicates the number of mmol of amine contained in 1 kg of solid content of the polyamide resin.
[0022] Examples of polyamide resins exhibiting the aforementioned amine value include aliphatic polyamide resins such as polyamide 46 (PA46), polyamide 410 (PA410), polyamide 6 (PA6), polyamide 66 (PA66), polyamide 610 (PA610), polyamide 612 (PA612), polyamide 11 (PA11), polyamide 12 (PA12), and polyamide 1010 (PA1010), as well as aromatic polyamide resins such as polyamide 6T (PA6T), polyamide 9T (PA9T), and polyamide 10T (PA10T). These can be used individually or in combination of two or more. Among these, aliphatic polyamide resins are preferred due to their superior interlayer adhesion with the polypropylene resin layer 1.
[0023] Furthermore, the polyamide resin preferably has a melting point of 160 to 280°C, and more preferably 170 to 270°C. This is because if the melting point is too low, the heat resistance tends to be poor, and conversely, if the melting point is too high, the interlayer adhesion tends to be poor.
[0024] Furthermore, 50% by mass or more of the material for the polyamide resin layer 2 is comprised of the polyamide resin with the specified amine value, preferably 70% by mass or more of the material for the polyamide resin layer 2 is comprised of the polyamide resin with the specified amine value, and more preferably 100% by mass of the material for the polyamide resin layer 2 is comprised of the polyamide resin with the specified amine value.
[0025] Furthermore, in addition to the polyamide resin of the amine value, the material for the polyamide resin layer 2 may also contain weather stabilizers, lubricants, pigments, dyes, antistatic agents, plasticizers, heat-resistant anti-aging agents, etc., as needed. Furthermore, the material for the polyamide resin layer 2 may be made by melting and kneading these materials together and then forming them into pellets, as needed.
[0026] In this laminated tube, it is preferable to form both layers by co-extrusion molding in order to bond the polypropylene resin layer 1 and the polyamide resin layer 2 together without adhesive.
[0027] Furthermore, in this laminated tube, it is preferable from the viewpoint of hydrolysis resistance that the polypropylene resin layer 1 is the inner layer and the polyamide resin layer 2 is the outer layer. For example, in a laminated tube with a two-layer structure in which an outer layer 12 is directly formed on the outer surface of an inner layer 11, as shown in Figure 1, the inner layer 11 is the same layer as the polypropylene resin layer 1, and the outer layer 12 is the same layer as the polyamide resin layer 2. Alternatively, a layer identical to the polypropylene resin layer 1 may be formed on the outer circumferential surface of the outer layer 12 to create a three-layer laminated tube. Furthermore, other resin layers, rubber layers, or reinforcing layers (layers formed by braiding reinforcing threads such as PET yarn) may be laminated onto the outer surface of these laminated tubes.
[0028] Method for manufacturing this laminated tube Next, we will explain the manufacturing method of this laminated tube. Specifically, first, the material for the inner layer 11 (the material for the polypropylene resin layer 1) is pelletized as appropriate according to the conditions described above. Similarly, the material for the outer layer 12 (the material for the polyamide resin layer 2) is also prepared in pelletized form. Next, using an extrusion molding machine, the materials for the inner layer 11 and the outer layer 12 are melt-extruded (co-extruded) onto a mandrel to form a tube, thereby forming the outer layer 12 on the outer surface of the inner layer 11. Note that the mandrel may be omitted if necessary. The extrusion molding of each layer by the extruder at this time is carried out at a temperature of 200 to 350°C (preferably 220 to 280°C) and a take-up speed of 1 to 15 m / min (preferably 3 to 5 m / min). In particular, it is desirable to perform melt extrusion molding (co-extrusion molding) at a temperature 20 to 100°C higher (preferably 20 to 80°C higher) than the melting point of the polyamide resin used for the outer layer 12. That is, by manufacturing under these conditions, the organic particles in the inner layer 11 can be unevenly distributed near the interface with the outer layer 12, and as a result, a large number of convex ridges of the desired size can be generated on the inner layer 11 side at the interface.
[0029] Then, the laminated tubes obtained in this way are annealed (heat-treated) near the melting point of the resin in each layer, or bent during the annealing process, as needed. In this way, the laminated tube (see Figure 1) can be manufactured.
[0030] In the laminated tube obtained in this manner, the inner diameter of the tube is preferably in the range of 2 to 40 mm, and more preferably in the range of 4 to 35 mm. Furthermore, the thickness of the inner layer 11 is preferably in the range of 0.1 to 1.9 mm, and more preferably in the range of 0.2 to 1.8 mm. Furthermore, the thickness of the outer layer 12 is preferably in the range of 0.1 to 1.9 mm, and more preferably in the range of 0.2 to 1.8 mm.
[0031] This laminated tube is used in radiator hoses, heater hoses, air conditioning hoses, and cooling tubes for battery packs in electric vehicles and fuel cell vehicles. Furthermore, this laminated tube can be used not only in automobiles but also in other transportation machinery (industrial transport vehicles such as airplanes, forklifts, excavators, and cranes, as well as railway vehicles, etc.). [Examples]
[0032] Next, examples will be described together with comparative examples. However, the present invention is not limited to these examples.
[0033] First, prior to the examples and comparative examples, the inner layer material (polypropylene resin layer material) and outer layer material (polyamide resin layer material) shown below were prepared.
[0034] [Material for inner layer (A)] 100 parts by mass of maleic anhydride-modified polypropylene (Mitsui Chemicals, Admer QF500, modification amount 0.27% by mass, melting point 165°C) and 15 parts by mass of ethylene-propylene copolymer (Mitsui Chemicals, Tuffmer DF840) were mixed in a twin-screw extruder at 200°C for 1 to 5 minutes to prepare inner layer material (A) (pellets).
[0035] [Material for inner layer (B)] 100 parts by mass of maleic anhydride-modified polypropylene (Mitsui Chemicals, Admer QF500, modification amount 0.27% by mass, melting point 165°C) and 15 parts by mass of ethylene-propylene copolymer (a mixture of Mitsui Chemicals' Tuffmer DF840 and Tuffmer DF8200 in a mass ratio of Tuffmer DF840:Tuffmer DF8200 = 8:2) were mixed in a twin-screw extruder at 200°C for 1 to 5 minutes to prepare inner layer material (B) (pellets).
[0036] [Material for inner layer (C)] 100 parts by mass of maleic anhydride-modified polypropylene (Mitsui Chemicals, Admer QF500, modification amount 0.27% by mass, melting point 165°C) and 15 parts by mass of ethylene-propylene copolymer (a mixture of Mitsui Chemicals' Tuffmer DF840 and Tuffmer DF8200 in a mass ratio of Tuffmer DF840:Tuffmer DF8200 = 6:4) were mixed in a twin-screw extruder at 200°C for 1 to 5 minutes to prepare inner layer material (C) (pellets).
[0037] [Material for inner layer (D)] 100 parts by mass of maleic anhydride-modified polypropylene (Mitsui Chemicals, Admer QF500, modification amount 0.27% by mass, melting point 165°C) and 15 parts by mass of ethylene-propylene copolymer (a mixture of Mitsui Chemicals' Tuffmer DF840 and Tuffmer DF8200 in a mass ratio of Tuffmer DF840:Tuffmer DF8200 = 2:8) were mixed in a twin-screw extruder at 200°C for 1 to 5 minutes to prepare inner layer material (D) (pellets).
[0038] [Materials for the inner layer (E)] 100 parts by mass of maleic anhydride-modified polypropylene (Mitsui Chemicals, Admer QF500, modification amount 0.27% by mass, melting point 165°C) and 15 parts by mass of ethylene-propylene copolymer (Mitsui Chemicals, Tuffmer DF8200) were mixed in a twin-screw extruder at 200°C for 1 to 5 minutes to prepare inner layer material (E) (pellets).
[0039] [Material for inner layer (F)] 100 parts by mass of maleic anhydride-modified polypropylene (Mitsui Chemicals, Admer QF500, modification amount 0.27% by mass, melting point 165°C) and 15 parts by mass of ethylene-propylene copolymer (Mitsui Chemicals, Tuffmer XM-7070) were mixed in a twin-screw extruder at 200°C for 1 to 5 minutes to prepare inner layer material (F) (pellets).
[0040] [Outer layer materials (a) to (e)] The commercially available polyamide resins shown in Table 1 below were prepared as outer layer materials (a) to (d). Furthermore, polyphthalamide (PPA), which is outer layer material (e) shown in Table 1 below, was prepared as described below.
[0041] [Table 1]
[0042] [Preparation of outer layer material (e) (PPA)] 14.9 mol of terephthalic acid, 25 mol of 1,6-hexanediamine, 10 mol of adipic acid, 0.6 mol of benzoic acid, sodium hypophosphate monohydrate, and distilled water were placed in a 13.6 L autoclave, purged with nitrogen, and the internal temperature was raised from 190°C to 250°C over 3 hours, and the internal pressure was increased to 3.0 MPa. The reaction was continued for one hour in that state, after which the low condensate was released into the atmosphere through a spray nozzle at the bottom of the autoclave. The low condensate was then pulverized in a pulverizer and dried at 100°C for 48 hours. The low condensate was then subjected to nitrogen purging. The nitrogen-purged low-condensate was then heated to 220°C in an autoclave over 1 hour and 30 minutes, followed by a solid-phase polymerization reaction for 1 hour, after which it was cooled to room temperature. The resulting prepolymer was then melt-polymerized in a twin-screw extruder with a screw diameter of 30 mm and a screw diameter-to-screw length ratio (L / D) of 54, at a cylinder temperature of 330°C, a screw rotation speed of 170 rpm, and a discharge rate of 5 kg / H to obtain polyphthalamide (PPA) with a melting point of 320°C and an amine value of 110.0 mmol / g.
[0043] Examples 1-6, Comparative Examples 1-4 Using the combinations shown in Table 2 below, the inner layer material and outer layer material were melt-extruded into a tubular shape (co-extruded) at a temperature 20°C higher than the melting point of each outer layer material (each polyamide resin) using a multilayer extrusion molding machine (a multilayer extrusion molding machine manufactured by Plastics Engineering Research Institute Co., Ltd.) capable of co-extrusion molding, and laminated tubes (inner layer thickness: 0.6 mm, outer layer thickness: 0.4 mm, inner diameter: 12 mm) were fabricated at a take-up speed of 3 m / min.
[0044] The laminated tube obtained in this way was cut in half, and its laminated cross-section was photographed at a magnification of 5000x using a scanning electron microscope (SEM), and 10 of these images were stitched together. Then, based on the aforementioned image, the particle sizes of 10 arbitrary ethylene-propylene copolymer particles (organic particles) found in the inner layer were measured, and their average particle size (μm) was determined. Furthermore, in the images, for those in which numerous convex ridges (ridges with a height of 0.1 μm or more from the interface) caused by the organic particles were observed on the inner layer side at the interface between the inner and outer layers, the number of convex ridges (ridges / 100 μm) along the straight-line distance at the interface was counted. These results are also shown in Table 2 below.
[0045] The laminated tubes of the examples and comparative examples were evaluated according to the following criteria. These results are also shown in Table 2 below.
[0046] <Extruderability> The appearance of the laminated tubes produced by co-extrusion molding as described above was visually observed and evaluated according to the following evaluation criteria. <Evaluation Criteria> ○: There was no disorder between the inner and outer layers, and it was possible to collect tubes with the specified wall thickness. ×: Layer disorder occurred between the inner and outer layers, making it impossible to collect a tube with the specified wall thickness.
[0047] <Interlayer adhesion> As described above, the laminated tubes produced by co-extrusion molding were cut in half, and strip-shaped test pieces with a width of 10 mm were prepared from the cut tubes. Then, the ends of the test pieces were peeled off with nippers, the peeled portion was grasped, and the interlayer delamination was performed by pulling it at a speed of 25 mm / min using a tensile testing machine. At this time, the average value of the adhesive strength (N / cm) when the peel strength remained stable for 30 seconds was measured and expressed as "Adhesive strength (N)". Furthermore, in the "adhesion strength (N / cm)" values expressed as described above, the value for Example 4 was set to 100 in exponential notation, and each "adhesion strength (N / cm)" value was converted to an exponent based on the value for Example 4. The interlayer adhesion was then evaluated according to the following evaluation criteria. <Evaluation Criteria> ○: The value of the aforementioned index is 70 or higher. ×: The value of the aforementioned index is less than 70.
[0048] [Table 2]
[0049] The results shown in Table 2 indicate that the laminated tubes of the examples exhibited excellent extrusion moldability and good interlayer adhesion.
[0050] In contrast, in Comparative Example 1, the average particle size of the organic particles (ethylene-propylene copolymer particles) in the inner layer was too large, which is thought to have resulted in stress concentration, and as a result, the desired interlayer adhesion could not be obtained. In Comparative Example 2, the average particle size of the organic particles (ethylene-propylene copolymer particles) in the inner layer was too small, which is thought to have resulted in insufficient anchoring effect, and as a result, the desired interlayer adhesion could not be obtained. In Comparative Example 3, a polyamide resin with a lower amine value than specified in the present invention was used as the polyamide resin material for the outer layer, which is thought to have resulted in a lower rate of chemical bond formation, and as a result, the desired interlayer adhesion could not be obtained. In Comparative Example 4, a polyamide resin with a higher amine value than specified in the present invention was used as the polyamide resin material for the outer layer, which caused molten resin residue (eye discharge) to accumulate at the tip of the extrusion molding machine head, making it impossible to obtain tubes of the specified wall thickness by extrusion molding, and abnormalities in the appearance of the tubes were also observed. [Industrial applicability]
[0051] The laminated tube of the present invention can be preferably used as a radiator hose, heater hose, air conditioner hose, etc., or as a cooling tube for battery packs in electric vehicles and fuel cell vehicles. Furthermore, the laminated tube can be used not only in automobiles but also in other transportation machinery (industrial transport vehicles such as airplanes, forklifts, excavators, cranes, etc., railway vehicles, etc.). [Explanation of symbols]
[0052] 11 Inner Layer 12 Outer layer
Claims
1. A laminated tube having a layer structure in which a polypropylene resin layer and a polyamide resin layer are laminated in a tightly contacted state, the polypropylene resin in the polypropylene resin layer is a maleic anhydride-modified polypropylene, and the polypropylene resin layer contains organic particles having an average particle size of 0.1 to 10 μm; the polyamide resin in the polyamide resin layer is a polyamide resin having an amine value of 15 to 100 mmol / kg; the organic particles are made of at least one of polyethylene and an ethylene-propylene copolymer; a polypropylene resin layer having a large number of protruding portions formed by the organic particles on the polypropylene resin layer side at the interface between the polypropylene resin layer and the polyamide resin layer; Laminated tube.
2. 2. The laminate tube according to claim 1, wherein the height of said convex protuberances is in the range of 0.1 to 10 μm.
3. 3. The laminate tube according to claim 1, wherein the number of said convex protuberances in a linear distance at the interface between said polypropylene resin layer and said polyamide resin layer is 2 to 20 / 100 μm.
4. 4. The laminate tube according to claim 1, wherein the proportion of organic particles in the polypropylene resin layer is 5 to 20% by mass.
5. 5. The laminate tube according to claim 1, wherein the polypropylene resin layer is an inner layer, and the polyamide resin layer is an outer layer.