Compound, method for forming metal-containing film, and method for producing compound
Patent Information
- Application Number
- JP2022008360
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-01-24
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for forming metal-containing films, such as niobium and vanadium nitrides, face challenges in controlling thickness and composition, particularly at high temperatures and low melting points, which affect their stability and deposition efficiency.
The development of precursor compounds represented by specific formulas, including alkyl groups and ligands, allows for the formation of metal-containing films through vapor deposition processes like atomic layer deposition, ensuring high temperature stability and low melting points, enabling precise control over film thickness and composition.
These compounds provide vapor phase compatibility and high temperature stability, enabling efficient formation of metal films with controlled thickness and composition, suitable for applications in microelectronic devices and energy storage.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure relates to compounds, methods for forming metal-containing films, and methods for producing compounds. [Background technology]
[0002] Metal oxides such as niobium oxide (Nb₂O₅) and niobium oxide (V₂O₅) are widely used in various technological fields. Typically, these oxides are applied as high-k materials in insulating films.
[0003] On the other hand, niobium nitride and vanadium nitride (NbN x , VN x Metal nitride films like the one shown (where the value of x is approximately 1 in both cases) have recently been used as diffusion barrier layers and adhesive layers in microelectronic devices.
[0004] Mixed oxides containing Nb are attracting considerable interest in energy storage applications, such as thin, highly ionically conductive interface layers between the positive electrode active material and electrolyte in all-solid-state batteries and lithium-ion batteries. For example, lithium niobate is of particular interest as an interface layer due to its remarkably high ion conductivity.
[0005] As a feasible technique for depositing the aforementioned interfacial layer onto a material, vapor deposition methods such as atomic layer deposition are being investigated. Various compounds have been proposed as niobium, vanadium, and tantalum sources for vapor deposition of metal nitrides (Chem. Mater. 1993, 5, 614-619; German Patent Application Publication No. 102006037955). [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] German Patent Application Publication No. 102006037955 Specification [Non-patent literature]
[0007] [Non-Patent Document 1] Chem. Mater. 1993, 5, 614-619 [Overview of the project] [Problems that the invention aims to solve]
[0008] The present disclosure aims to provide precursor compounds containing niobium, vanadium, or tantalum that are suitable for controlling thickness and composition in film formation by vapor deposition at high temperatures, and that are liquid or have a low melting point (50°C or less at atmospheric pressure) and are stable at high temperatures. [Means for solving the problem]
[0009] According to this disclosure, certain precursor compounds have been found to be suitable for the deposition of Nb, V, or Ta-containing thin films by vapor deposition processes, including atomic layer deposition (ALD).
[0010] This disclosure describes, in one embodiment, This invention relates to a compound, represented by the following formula (1), for forming a metal-containing film by gas-phase deposition. [ka] (In the formula, M is either V or Nb, R 1 , R 2 and R 3 Each of these is independently H or a C1-C10 alkyl group. L is a ligand derived from a substituted or unsubstituted C3 or greater alkene structure, a C4 or greater alkadiene structure, a C5 or greater cycloalkadiene structure, or a condensed aromatic ring structure. The value of e is either 0 or 1; or M is Ta, R 1 , R 2 and R 3 Each of these is independently H or a C1-C10 alkyl group. L is a ligand derived from a substituted or unsubstituted alkene structure having 3 or more carbon atoms, an alkadiene structure having 4 or more carbon atoms, a cycloalkadiene structure having 6 or more carbon atoms, or a condensed aromatic ring structure, The value of e is 0 or 1.)
[0011] In one embodiment, the present disclosure an introduction step of introducing the compound into a reactor having a substrate disposed therein, a deposition step of depositing at least a part of the compound on the substrate and relates to a method for forming a metal-containing film including
[0012] In one embodiment, the present disclosure a method for producing the compound, comprising a step of reacting a precursor compound represented by the following formula (i) with at least one of an alcohol represented by the following formula (α-1) and an alcohol represented by the following formula (α-2). The present disclosure relates to a method for producing a compound.
Chemical formula
Chemical formula
[0013] Hereinafter, definitions of terms will be described.
[0014] Standard abbreviations for elements from the periodic table are used herein. Thus, elements may be represented by these abbreviations (for example, Nb means niobium, V means vanadium, Ta means tantalum, N means nitrogen, C means carbon, and H means hydrogen; the same applies to other elements).
[0015] In this specification, the abbreviation "Me" means a methyl group; "Et" means an ethyl group; "Pr" means a propyl group; "nPr" means a normal or linear propyl group; "iPr" means an isopropyl group; "Bu" means a butyl group; "nBu" means a normal or linear butyl group; "tBu" means a tert-butyl group, also known as 1,1-dimethylethyl; "sBu" means a sec-butyl group, also known as 1-methylpropyl; "iBu" means an isobutyl group, also known as 2-methylpropyl; the term "amyl" means an amyl group or pentyl group; the term "t-amyl" means a tert-amyl group, also known as 1,1-dimethylpropyl; "Cp" means a cyclopentadienyl group; and "amd" means an amide group.
[0016] In this specification, a combination of C and a number, such as "C1," represents the number of carbon atoms that make up the group or structure. For example, a C1 alkyl group represents an alkyl group with 1 carbon atom (i.e., a methyl group), a C2 alkyl group represents an alkyl group with 2 carbon atoms (i.e., an ethyl group), and a C3 alkene structure represents an alkene structure with 3 carbon atoms (i.e., a propene structure). [Effects of the Invention]
[0017] The compounds described herein are suitable for forming metal films containing niobium, vanadium, or tantalum by vapor deposition because they possess vapor deposition compatibility, high-temperature stability, and a low melting point (or liquid state). Furthermore, the method for forming metal-containing films described herein uses specific compounds as precursors for vapor deposition, enabling efficient formation of metal-containing films. [Brief explanation of the drawing]
[0018] [Figure 1] This is a thermogravimetric analysis (TGA) graph showing the weight percentage of bis(ethoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OEt)2 as the temperature rises. [Figure 2] This is a thermogravimetric analysis (TGA) graph showing the weight percentage of bis(tert-butoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OtBu)2 as the temperature rises. [Figure 3] This is a thermogravimetric analysis (TGA) graph showing the weight percentage of bis(sec-butoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OsBu)2 as the temperature rises. [Figure 4] This is a differential scanning calorimetry (DSC) measurement of bis(ethoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OEt)2. [Figure 5] This is differential scanning calorimetry (DSC) of bis(tert-butoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OtBu)2. [Figure 6] This is differential scanning calorimetry (DSC) of bis(sec-butoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OsBu)2. [Figure 7] This is a thermogravimetric analysis (TGA) graph showing the mass percentage of bis(dimethylamide)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(NMe2)2 as the temperature rises. [Figure 8] This shows the ozone-induced ALD window for bis(ethoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OEt)2. [Figure 9] These are images (SEM measurements) of patterned wafers coated with Nb2O5 films deposited with Nb(=NtBu)(Cp)(OEt)2 at 250°C and 300°C. [Figure 10] This shows the ozone-induced ALD window for bis(tert-butoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OtBu)2. [Modes for carrying out the invention]
[0019] Embodiments of this disclosure are described below. This disclosure is not limited to these embodiments. Preferred combinations of embodiments are also preferred.
[0020] 《Compound》 The compound according to this embodiment is represented by the following formula (1) and is used to form a metal-containing film by gas-phase deposition. The compound is liquid at room temperature or has a melting point of 50°C or lower. Furthermore, since the compound is thermally stable, it can be directly introduced into the reactor as a gas or liquid during gas-phase deposition, and it can provide a wide ALD window in which it exhibits a constant growth rate with respect to temperature increases. [ka]
[0021] In one embodiment (hereinafter also referred to as the "first embodiment"), in formula (1), M is either V or Nb, R 1 , R 2 and R 3 Each of these is independently H or a C1-C10 alkyl group. L is a ligand derived from a substituted or unsubstituted C3 or greater alkene structure, a C4 or greater alkadiene structure, a C5 or greater cycloalkadiene structure, or a condensed aromatic ring structure. The value of e is either 0 or 1.
[0022] In another embodiment (hereinafter also referred to as the "second embodiment"), in formula (1), M is Ta, R 1 , R 2 and R 3 Each of these is independently H or a C1-C10 alkyl group. L is a ligand derived from a substituted or unsubstituted C3 or greater alkene structure, a C4 or greater alkadiene structure, a C6 or greater cycloalkadiene structure, or a condensed aromatic ring structure. The value of e is either 0 or 1.
[0023] (First Embodiment) In the first embodiment, the central metal M of the compound represented by formula (1) is V (vanadium) or Nb (niobium). M is preferably Nb.
[0024] R 1 , R 2 and R 3 The C1-C10 alkyl groups represented by include, independently, linear or branched alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl, n-propyl, i-propyl, n-butyl, s-butyl, and t-butyl groups. 1 A branched alkyl group having 3 to 5 carbon atoms is preferred, and a tert-butyl group is even more preferred. 2 and R 3 These are preferably linear or branched alkyl groups having 2 to 5 carbon atoms, and more preferably ethyl, tert-butyl, or sec-butyl groups.
[0025] Examples of alkene structures with 3 to 10 carbon atoms that provide the ligand represented by L include linear or branched propene structures, butene structures, pentene structures, and hexene structures, regardless of the position of the unsaturated bond. Among the alkene structures with 3 or more carbon atoms, linear C3-C6 alkene structures are preferred, and propene is even more preferred.
[0026] Examples of the C4 or higher alkadien structures include linear or branched butadiene structures, pentadiene structures, hexadiene structures, heptadiene structures, and other alkadien structures having 4 to 10 carbon atoms, regardless of the position of the unsaturated bond. Among the C4 or higher alkadien structures, linear alkadien structures having 4 to 6 carbon atoms are preferred, and linear butadiene structures and pentadiene structures are even more preferred.
[0027] Examples of the cycloalkadiene structures with 5 or more carbon atoms include cyclopentadiene structures, cyclohexadiene structures, cycloheptadiene structures, and cyclooctadiene structures, which have 5 to 10 carbon atoms and whose positions are not restricted by the position of the unsaturated bond. Among these, cycloalkadiene structures with 5 to 7 carbon atoms are preferred, and cyclopentadiene structures are even more preferred.
[0028] The aforementioned condensed aromatic ring structure is not particularly limited in that it includes a structure in which an aromatic ring is condensed with another ring. Condensation refers to a polycyclic structure in which two adjacent rings share an edge (a bond between two adjacent carbon atoms). The other ring may be the same or different aromatic ring as the aforementioned aromatic ring, or it may be an alicyclic structure.
[0029] Aromatic rings include aromatic hydrocarbon rings or aromatic heterocycles with 5 to 30 members, such as aromatic hydrocarbon rings like benzene, naphthalene, anthracene, phenalene, phenanthrene, pyrene, fluorene, perylene, and coronene rings; aromatic heterocycles like furan, pyrrole, thiophene, phosphole, pyrazole, oxazole, isoxazole, thiazole, pyridine, pyrazine, pyrimidine, pyridazine, and triazine rings; or combinations thereof.
[0030] Examples of alicyclic structures include aliphatic cyclic hydrocarbon structures with 5 to 20 ring members, such as cycloalkanes like cyclopentane and cyclohexane; cycloalkenes like cyclopropene, cyclopentene, and cyclohexene; bridged ring saturated hydrocarbons like norbornane, adamantane, and tricyclodecane; and bridged ring unsaturated hydrocarbons like norbornene and tricyclodecene.
[0031] The aforementioned condensed aromatic ring structure is preferably an aromatic hydrocarbon ring structure with 6 to 12 members, and more preferably an indene structure.
[0032] Examples of substituents that substitute for some or all of the hydrogen atoms in L include halogen atoms such as fluorine, chlorine, bromine, and iodine, alkyl groups, alkylsilyl groups, alkylgermyl groups, alkylamide groups, alkylsilylamide groups, hydroxyl groups, carboxyl groups, cyano groups, nitro groups, alkoxy groups, alkoxycarbonyl groups, alkoxycarbonyloxy groups, acyl groups, and acyloxy groups.
[0033] The value of e is preferably 1.
[0034] (Second Embodiment) In the second embodiment, the central metal M of the compound represented by formula (1) is Ta (tantalum). In the first embodiment, the number of carbon atoms in the cycloalkadiene structure that gives the ligand represented by L is 5 or more (C5 or more), whereas in the second embodiment, the number of carbon atoms in the cycloalkadiene structure is 6 or more (C6 or more). For other structures and substituents, the same structures and substituents as in the first embodiment can be suitably adopted.
[0035] (Other embodiments) The following lists preferred embodiments of the compound.
[0036] The aforementioned compound is preferably represented by the following formula (1-1). [ka] (In formula (1-1), M is either V or Nb, R 4 , R 5 , R 6 , R 7 and R 8 Each of these is independently H, a C1-C10 alkyl group, a halogen atom, an alkylsilyl group, an alkylgermyl group, an alkylaminocarbonyl group, or an alkylsilylamide group. R 1 , R 2 and R 3 This is equivalent to equation (1) above.
[0037] R 4 , R 5 , R 6 , R 7 and R 8 The C1-C10 alkyl group represented by is R of formula (1) above. 1 , R 2 and R 3 C1 to C10 alkyl groups represented by can be preferably used.
[0038] Examples of the halogen atoms include fluorine, chlorine, bromine, and iodine atoms. Among these, fluorine atoms are preferred.
[0039] Examples of the alkylsilyl group include trimethylsilyl group and triethylsilyl group.
[0040] Examples of the alkylgelmyl group include trimethylgelmyl group and triethylgelmyl group.
[0041] Examples of the alkylaminocarbonyl group include a dimethylaminocarbonyl group and a diethylaminocarbonyl group.
[0042] Examples of the alkylsilylamide group include trimethylsilylamide group and triethylsilylamide group.
[0043] R 4 , R 5 , R 6 , R 7 and R 8 It is preferable that it is H (hydrogen atom).
[0044] The aforementioned compound is preferably represented by the following formula (1-2). [ka] (In the formula, M is V, Nb, or Ta. R 9 , R 10 , R 11 , R 12 , R 13 , R 14 and R 15 Each of these is independently H, a C1-C10 alkyl group, or a halogen atom. R 1 , R 2 and R 3 This is equivalent to equation (1) above.
[0045] R 9 , R 10 , R 11 , R 12 , R 13 , R14 and R 15 The C1-C10 alkyl group represented by is R of formula (1) above. 1 , R 2 and R 3 C1 to C10 alkyl groups represented by can be preferably used.
[0046] As the halogen atom, the same halogen atom as in formula (1-1) can be used.
[0047] R 9 , R 10 , R 11 , R 12 , R 13 , R 14 and R 15 It is preferable that it is H (hydrogen atom).
[0048] The aforementioned compound is preferably represented by the following formula (1-3). [ka] (In the formula, M is V, Nb, or Ta. R 16 and R 17 Each of these is independently H, a C1-C10 alkyl group, or a halogen atom. R 1 and R 2 This is equivalent to equation (1) above.
[0049] R 16 and R 17 The C1-C10 alkyl group represented by is R of formula (1) above. 1 , R 2 and R 3 C1 to C10 alkyl groups represented by can be preferably used.
[0050] As the halogen atom, the same halogen atom as in formula (1-1) can be used.
[0051] R 16 and R17 is preferably H (a hydrogen atom).
[0052] The compound is preferably represented by the following general formula (1-4). [Chemical formula] (In the formula, M is V, Nb or Ta, R 18 , R 19 and R 20 are each independently H, a C1-C10 alkyl group or a halogen atom, R 1 , R 2 and R 3 have the same meanings as in the above formula (1).)
[0053] R 18 , R 19 and R 20 As the C1-C10 alkyl group represented by, the C1-C10 alkyl group represented by R 1 , R 2 and R 3 in the above formula (1) can be preferably employed.
[0054] As the halogen atom, the same halogen atom as in the above formula (1-1) can be employed.
[0055] R 18 , R 19 and R 20 are preferably H (a hydrogen atom).
[0056] The compound is preferably liquid at 25°C or the temperature at which the vapor pressure shows 133.3 Pa is 130°C or lower. The temperature at which the vapor pressure shows 133.3 Pa is more preferably 120°C or lower. Thereby, the compound can exist as a liquid at room temperature or a solid with a low melting point, and the vapor deposition process for forming a metal-containing film can be efficiently carried out.
[0057] In the thermogravimetric analysis of the compound, it is preferable that there is a region where the weight loss is 20% or less at 150°C or above, more preferably a region where the weight loss is 20% or less at 180°C or above, and even more preferably a region where the weight loss is 20% or less at 200°C or above. This allows the compound to exhibit excellent thermal stability.
[0058] The aforementioned compounds can be suitably used for thin-film vapor deposition due to the above-described properties. Suitable vapor deposition methods include, but are not limited to, atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PE-ALD), chemical vapor deposition (CVD), pulsed chemical vapor deposition (P-CVD), and thermal, plasma, or remote plasma processes in low-pressure chemical vapor deposition (LPCVD), or combinations thereof.
[0059] Methods for producing compounds The method for producing the compound includes a step of reacting a precursor compound represented by the following formula (i) with at least one of the alcohols represented by the following formula (α-1) and the following formula (α-2). According to this production method, the desired compound can be efficiently produced simply by carrying out a ligand exchange reaction between the precursor compound and a predetermined alcohol. [ka] (In formula (i), M, R 1 L and e are equivalent to those in equation (1) above. R a and R b Each of these is independently a C1-C5 alkyl group. [ka] (In equations (α-1) and (α-2), R 2 and R 3 This is equivalent to equation (1) above.
[0060] R a and R bExamples of C1-C5 alkyl groups represented by include methyl groups and ethyl groups. Among these, methyl groups are preferred.
[0061] The precursor compound can be synthesized, for example, by the method described in U.S. Patent No. 8,460,989.
[0062] The precursor compound is dissolved in a suitable solvent such as toluene to obtain a starting solution. The target compound can be produced by mixing and stirring the starting solution with alcohol to carry out a ligand exchange reaction. It is preferable to mix 1 to 3 moles of alcohol for every 1 mole of precursor compound. The reaction temperature may be room temperature or heated to about 50°C. The reaction time is preferably 1 to 24 hours, and more preferably 2 to 16 hours.
[0063] After the reaction, the product may be purified as needed by removing the solvent using an evaporator, heating and drying under reduced pressure, distillation, sublimation, column chromatography, etc.
[0064] Method for forming metal-containing films The method for forming a metal-containing film according to this embodiment includes an introduction step of introducing the compound into a reactor in which a substrate is placed, and a deposition step of depositing at least a portion of the compound onto the substrate.
[0065] (Introduction process) In this process, the compound is introduced into a reactor containing a substrate. The type of substrate on which the metal-containing film is deposited is appropriately selected according to the final application.
[0066] In some embodiments, the substrate is selected from the cathode active material or cathode in a lithium-ion battery device or an all-solid-state battery device. The cathode active material is a key component in the composition of the cathode battery cell. The cathode material is, for example, cobalt, nickel, or manganese, and its crystalline structure, such as a layered structure, forms a polymetallic oxide material with lithium inserted. The cathode active material is preferably "NMC" (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminum oxide), LNO (lithium nickel oxide), LMNO (lithium manganese nickel oxide), or LFP (lithium iron phosphate). For example, the cathode active material may be NMC622 or NMC811. The thin interfacial layer may be deposited on electrode active material powder, on electrode active material porous material, on electrode active material of different shapes, or on a pre-formed electrode where the electrode active material may be bonded to conductive carbon and / or a binder and may already be supported by a current collector foil.
[0067] In some embodiments, the substrate can be selected from oxides used as insulating materials in MIM, DRAM, or FeRam technologies (e.g., HfO2-based materials, TiO2-based materials, ZrO2-based materials, rare earth oxide-based materials, ternary oxide-based materials, etc.) or nitride-based films used as oxygen barriers between copper and low-k films (e.g., TaN). Other substrates can be used in the manufacture of semiconductors, photocells, LCD-TFTs, or flat panel devices. Examples of such substrates include, but are not limited to, solid substrates such as metal nitride-containing substrates (e.g., TaN, TiN, WN, TaCN, TiCN, TaSiN, and TiSiN); insulators (e.g., SiO2, Si3N4, SiON, HfO2, Ta2O5, ZrO2, TiO2, Al2O3, and barium strontium titanate); or other substrates containing some of these materials. The actual substrate used may also depend on the specific embodiment of the compound used.
[0068] The reactor can be any enclosed vessel or chamber in which a gas-phase deposition method is performed. Specific examples, but are not limited to, parallel-plate reactors, cold-wall reactors, hot-wall reactors, single-sheet reactors, multi-wafer reactors, or other types of deposition systems.
[0069] Next, the gas containing the vaporized compound is introduced into the reactor. A pure (single) compound or a blend of (multiple) compounds may be supplied to the vaporizer in liquid form and vaporized here before being introduced into the reactor. Alternatively, the compound can be vaporized by passing a carrier gas through a container containing the compound, or by bubbling the carrier gas through the compound. Next, the gas containing the carrier gas and the vaporized compound is introduced into the reactor. If necessary, the container may be heated to a temperature that allows the compound to have a sufficient vapor pressure. Examples of carrier gases, but not limited to, include Ar, He, N2, and mixtures thereof. Alternatively, instead of using this method of bubbling the carrier gas (i.e., the bubbling method), the compound may be vaporized using direct liquid injection (DLI).
[0070] In the introduction step, co-reactants may be further introduced into the reactor. The co-reactants are preferably selected from the group consisting of O2, O3, H2O, H2O2, NO, N2O, NO2, trimethyl phosphate, their oxygen radicals, and mixtures thereof. Other co-reactants that can be used include alcohols, ammonia, polyamines, hydrazine, dimethylethyl phosphoramide, sulfates, etc.
[0071] The container can be maintained at a temperature within a range of, for example, approximately 0°C to approximately 150°C. Those skilled in the art will see that the amount of compound vaporized can be controlled by adjusting the temperature of the container in a well-known manner.
[0072] The compounds may be supplied in pure form (e.g., liquid or low-melting-point solid) or in blends with a suitable solvent. Exemplary solvents include, but are not limited to, aliphatic hydrocarbons, aromatic hydrocarbons, heterocyclic hydrocarbons, ethers, glycans, glycols, amines, polyamines, cyclicamines, alkylated amines, alkylated polyamines, and mixtures thereof. Preferred solvents include ethylbenzene, diglymes, triglycers, tetraglycers, pyridine, xylene, mesitylene, decane, dodecane, and mixtures thereof. The concentration of the compounds is typically in the range of about 0.02 to about 2.0 M, and preferably in the range of about 0.05 to about 0.2 M.
[0073] In addition to any mixing of the compound and solvent before introduction into the reactor, a gas containing the vaporized compound may be mixed with the reactants inside the reactor. Examples of reactants, but not limited to, include metal precursors such as strontium-containing precursors, barium-containing precursors, aluminum-containing precursors such as TMA, and any combination thereof.
[0074] The reactor can be maintained at a pressure in the range of about 0.5 mTorr to about 20 Torr. In addition, the temperature inside the reactor can be in the range of about 50°C to about 600°C, preferably in the range of about 80°C to about 550°C. Those skilled in the art can optimize the temperature by experience to achieve the desired results.
[0075] The substrate can be heated to a temperature sufficient to obtain the desired lithium-containing film with a sufficient growth rate and desired physical state and composition. A non-limiting exemplary temperature range in which the substrate can be heated is 50°C to 500°C. Preferably, the substrate temperature is kept below 300°C.
[0076] (deposition process) In this step, at least a portion of the compound is deposited onto the substrate. In one exemplary atomic layer deposition type process, the gas phase of the compound is introduced into a reactor and brought into contact with a suitable substrate. Excess compound can then be removed from the reactor by purging and / or evacuating it. Co-reactants are introduced into the reactor, where they react with the absorbed compound in a self-stopping manner. Excess co-reactants are removed from the reactor by purging and / or evacuating it. If the desired film is a metal oxide film, this two-step process may provide the desired film thickness, or it may be repeated until a film of the required thickness is obtained.
[0077] Alternatively, if the desired film is a metal oxide film, the introduction of a metal precursor vapor into the reactor can be continued after the two-step process described above. This metal precursor is selected based on the properties of the metal oxide to be deposited. After introduction into the reactor, the compound comes into contact with the substrate. Excess compound is removed from the reactor by purging and / or evacuating it. The co-reactants may be introduced into the reactor again and reacted with the metal precursor. Excess co-reactants are removed from the reactor by purging and / or evacuating it. Once the desired film thickness is obtained, the process may be terminated. However, if a thicker film is desired, all four steps of the process may be repeated. By alternating the supply of the compound, metal precursor, and co-reactants, films of the desired composition and thickness can be deposited.
[0078] The metal-containing film obtained from this manufacturing method may be a ternary or quaternary oxide film of niobium, such as LiNbO, LiNbO, LiNb(M)O, or NbMO. M is selected from the group consisting of Zr, Ti, Co, W, Ta, V, Sr, Ba, La, Y, Sc, Mn, Ni, and Mo. Those skilled in the art can obtain the desired film composition by appropriately selecting the appropriate compounds and reactants.
[0079] The composition of the deposited film depends on the application. For example, metal-containing films can be used in fuel cells and batteries. [Examples]
[0080] Examples are provided below to illustrate the application of the disclosures herein, but it should be understood that not all of the advantages of the processes described herein can be encompassed in any particular embodiment or group of embodiments of the present invention. While specific embodiments and examples are disclosed below, it will be understood by those skilled in the art that the present invention extends beyond the specifically disclosed embodiments and / or uses of the present invention, including obvious modifications. Therefore, it should be understood that the scope of the disclosed invention should not be limited by the specific embodiments described below.
[0081] <Example 1> Synthesis of Nb(=NtBu)(Cp)(OEt)2 and bis(ethoxy)(tert-butylimide)cyclopentadienylniobium [ka]
[0082] To a solution of Nb(=NtBu)Cp(NMe2)2 (2g, 6.3 mmol) (purchased from Air Liquide Advanced Materials Inc.) in 30 mL of toluene at -78°C, ethyl alcohol (0.58 g, 12.6 mmol) (Sigma-Aldrich) was added. The mixture was stirred at room temperature (approximately 25°C) for 12 hours, and then the solvent was removed under vacuum to obtain a yellow oily substance. This substance was then purified by distillation at 25 mTorr to 100°C to obtain 1.34 g (yield 66.6%) of the yellow oily substance. This product was subjected to NMR 1 H(π, ppm, C6D6) was characterized by 6.18(s, 5H), 4.54(q, 4H), 1.28(t, 6H), and 1.16(s, 9H).
[0083] Open-cup TGA analysis (measured using a Mettler Toledo TGA / DSC 1 STARe System) was performed on the purified product in air with a nitrogen flow of 200 mL / min and a heating rate of 10°C / min. The results showed a residual lump of 2.1%. These results are shown in Figure 1. Figure 1 is a thermogravimetric analysis (TGA) graph showing the weight percentage as the temperature rises. Differential scanning calorimetry (DSC, measured using a Mettler Toledo DSC 1 STARe System (ME-51140728)) of the product yielded the melting onset temperature (-3.8°C) and the decomposition onset temperature (317.3°C). These results are shown in Figure 4.
[0084] Figure 8 shows the ozone-induced ALD window for bis(ethoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OEt)2, the compound produced in Example 1. Furthermore, Figure 9 shows the film coating images of patterned wafers with Nb2O5 films deposited with Nb(=NtBu)(Cp)(OEt)2 at 250°C and 300°C (SEM measurement, JEOL Ltd., model: FE-SEM (JEOL-6701F)). The formation conditions for the Nb2O5 films were wafer temperature: 250, 300°C, process pressure: 1 torr, Ar flow rate: 100 sccm, source introduction time / source purge time / ozone introduction time / ozone purge time: 2 / 60 / 1 / 60 (seconds).
[0085] <Example 2> Synthesis of Nb(=NtBu)(Cp)(OtBu)2, bis(tert-butoxy)(tert-butylimide)cyclopentadienylniobium [ka]
[0086] To a solution of Nb(=NtBu)Cp(NMe2)2 (2 g, 6.3 mmol) (purchased from Air Liquide Advanced Materials Inc.) in 30 mL of toluene at -78 °C, tert-butyl alcohol (0.93 g, 12.6 mmol) (Sigma-Aldrich) was added. The mixture was stirred at room temperature (approximately 25 °C) for 12 hours, and the solvent was removed under vacuum to obtain a yellow oily substance. This substance was then purified by distillation at 25 mTorr to 100 °C to obtain 2.0 g (yield 84.6%) of yellow oily substance. This product was NMR 1 H(π, ppm, C6D6) was characterized by 6.17 (s, 5H), 1.32 (s, 18H), and 1.21 (s, 9H).
[0087] Open-cup TGA analysis (measured using a Mettler Toledo TGA / DSC 1 STARe System) was performed on the purified product in air with a nitrogen flow of 200 mL / min and a heating rate of 10°C / min. The results showed that 0.6% of the product remained as a residual mass. These results are shown in Figure 2. Figure 2 is a thermogravimetric analysis (TGA) graph showing the weight percentage as the temperature rises. Differential scanning calorimetry (DSC, measured using a Mettler Toledo DSC 1 STARe System (ME-51140728)) of the product yielded the melting onset temperature (34.5°C) and the decomposition onset temperature (285.1°C). These results are shown in Figure 5.
[0088] Figure 10 shows the ozone-induced ALD window for bis(tert-butoxy)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(OtBu)2, the compound produced in Example 2.
[0089] <Example 3> Synthesis of Nb(=NtBu)(Cp)(OsBu)2, bis(sec-butoxy)(tert-butylimide)cyclopentadienylniobium [ka]
[0090] To a solution of Nb(=NtBu)Cp(NMe2)2 (2g, 6.3 mmol) (purchased from Air Liquide Advanced Materials Inc.) in 30 mL of toluene at -78°C, sec-butyl alcohol (0.93 g, 12.6 mmol) (Sigma-Aldrich) was added. The mixture was stirred at room temperature (approximately 25°C) for 12 hours, and then the solvent was removed under vacuum to obtain a yellow oily substance. This substance was then purified by distillation at 25 mTorr to 125°C to obtain 1.75 g (yield 74%) of the yellow oily substance. This product was analyzed by NMR. 1 H(π, ppm, C6D6) was characterized by 6.19(s, 5H), 4.49(m, 2H), 1.61(m, 2H), 1.49(m, 2H), 1.31(d, 3H), 1.26(d, 3H), 1.18(s, 9H), and 0.99(t, 6H).
[0091] Open-cup TGA analysis (measured using a Mettler Toledo TGA / DSC 1 STARe System) was performed on the purified product in air with a nitrogen flow of 200 mL / min and a heating rate of 10°C / min. The results showed that 1.3% of the product remained as a residual mass. These results are shown in Figure 3. Figure 3 is a thermogravimetric analysis (TGA) graph showing the weight percentage as the temperature rises. Differential scanning calorimetry (DSC, measured using a Mettler Toledo DSC 1 STARe System (ME-51140728)) of the product yielded the decomposition onset temperature (318.6°C). These results are shown in Figure 6.
[0092] <Synthesis Example 1> Compound V(=NtBu)(Cp)(OEt)2 can be synthesized by the following method. [ka]
[0093] Ethanol is added dropwise to a solution of V(=NtBu)(Cp)(NMe2)2 in toluene at -78°C. The mixture is stirred at room temperature for 12 hours, after which the solvent is removed under vacuum. The substance is then purified by distillation or sublimation to obtain the final product.
[0094] <Synthesis Example 2> The compound Ta(=NtBu)(Cp)(OEt)2 can be synthesized by the following method. [ka]
[0095] Ethanol is added dropwise to a solution of Ta(=NtBu)(Cp)(NMe2)2 in toluene at -78°C. The mixture is stirred at room temperature for 12 hours, after which the solvent is removed under vacuum. The substance is then purified by distillation or sublimation to obtain the final product.
[0096] Figure 7 is a thermogravimetric analysis (TGA, measured using a Mettler Toledo TGA / DSC 1 STARe System) graph showing the mass percentage of bis(dimethylamide)(tert-butylimide)cyclopentadienylniobium, Nb(=NtBu)(Cp)(NMe2)2 as the temperature rises, which is the starting material for the production of the compound in Example 1.
[0097] Table 1 below shows a comparison of the vapor pressures of the disclosed compound and several existing compounds.
[0098] [Table 1]
Claims
1. A compound for forming a metal-containing film by vapor deposition, represented by the following formula (1): 【Chemistry 1】 (In formula (1), M is V or Nb; R 1 , R 2 and R 3 are each independently H or a C1-C10 alkyl group; L is a ligand derived from a substituted or unsubstituted C3 or higher alkene structure, C4 or higher alkadiene structure, C5 or higher cycloalkadiene structure or fused aromatic ring structure, The value of e is 0 or 1; or M is Ta; R 1 , R 2 and R 3 are each independently H or a C1-C10 alkyl group; L is a ligand derived from a substituted or unsubstituted C3 or higher alkene structure, C4 or higher alkadiene structure, C6 or higher cycloalkadiene structure or fused aromatic ring structure, The value of e is 0 or 1.
2. 2. The compound of claim 1, wherein M is V or Nb and L is a ligand derived from a substituted or unsubstituted cyclopentadiene.
3. 3. The compound of claim 1 or 2, wherein the value of e is 1.
4. The compound according to any one of claims 1 to 3, wherein M is Nb.
5. R 1 The compound according to any one of claims 1 to 4, wherein is a tert-butyl group.
6. R 2 and R 3 The compound according to any one of claims 1 to 5, wherein each independently represents an ethyl group, a tert-butyl group, or a sec-butyl group.
7. The compound according to claim 1, represented by the following general formula (1-1): 【Chemistry 2】 (In formula (1-1), M is V or Nb; R 4 , R 5 , R 6 , R 7 and R 8 are each independently H, a C1-C10 alkyl group, a halogen atom, an alkylsilyl group, an alkylgermyl group, an alkylamide group, or an alkylsilylamide group, R 1 , R 2 and R 3 has the same meaning as the formula (1).
8. The compound according to claim 1, represented by the following general formula (1-2): 【Transformation 3】 (In formula (1-2), M is V, Nb or Ta; R 9 , R 10 , R 11 , R 12 , R 13 , R 14 and R 15 are each independently H, a C1-C10 alkyl group, or a halogen atom; R 1 , R 2 and R 3 has the same meaning as the formula (1).
9. The compound according to claim 1, represented by the following general formula (1-3): 【Chemistry 4】 (In formula (1-3), M is V, Nb or Ta; R 16 and R 17 are each independently H, a C1-C10 alkyl group, or a halogen atom; R 1 and R 2 has the same meaning as the formula (1).
10. The compound according to claim 1, represented by the following general formula (1-4): 【Transformation 5】 (In formula (1-4), M is V, Nb or Ta; R 18 , R 19 and R 20 are each independently H, a C1-C10 alkyl group, or a halogen atom; R 1 , R 2 and R 3 has the same meaning as the formula (1).
11. an introduction step of introducing the compound according to any one of claims 1 to 10 into a reactor having a substrate disposed therein; depositing at least a portion of the compound onto the substrate; A method for forming a metal-containing film comprising:
12. The method for forming a metal-containing film according to claim 11 , wherein the introducing step further comprises introducing a co-reactant into the reactor.
13. The coreactant is O 2 , O 3 , H 2 O, H 2 O 2 , NO, N 2 O, NO 2 13. The method of forming a metal-containing film of claim 12, wherein the metal-containing compound is selected from the group consisting of trimethyl phosphate, trimethyl phosphate, oxygen radicals thereof, and mixtures thereof.
14. The method for forming a metal-containing film according to any one of claims 11 to 13, wherein the depositing step is carried out by atomic layer deposition.
15. The method for forming a metal-containing film according to any one of claims 11 to 14, wherein the substrate comprises a cathode active material powder.
16. The method for forming a metal-containing film according to any one of claims 11 to 14, wherein the substrate comprises a cathode active material powder, conductive carbon, and a binder material.
17. A method for producing the compound of claim 1, comprising the steps of: A method for producing a compound, comprising a step of reacting a precursor compound represented by the following formula (i) with at least one of an alcohol represented by the following formula (α-1) and an alcohol represented by the following formula (α-2): 【Transformation 6】 (In formula (i), M.R. 1 , L and e are the same as in formula (1). R a and R b are each independently a C1 to C5 alkyl group. 【Transformation 7】 (In formulas (α-1) and (α-2), R 2 and R 3 has the same meaning as in formula (1).