Method of preventing discoloration and corrosion

JP2023143790A5Active Publication Date: 2024-10-03DUPONT ELECTRONIC MATERIALS INT LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023039494
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-14
Publication Date
2024-10-03
Estimated Expiration
2043-03-14

AI Technical Summary

Technical Problem

Silver tarnishes and gold corrodes due to sulfide reactions, leading to discoloration and impaired electrical performance, with existing organic and precious metal coatings having drawbacks such as volatility, thermal instability, and high costs.

Method used

A bismuth electroplating method is applied to create a thin layer (up to 20 nm) on silver or gold surfaces to prevent tarnishing and corrosion, using a bismuth electroplating solution comprising bismuth ions, acid, and optional additives like surfactants, brighteners, and antifoam agents.

Benefits of technology

The bismuth layer effectively inhibits tarnishing and corrosion, maintaining low contact resistance and electrical performance even after thermal aging, as demonstrated by accelerated sulfidation and corrosion tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a method of preventing discoloration and corrosion.SOLUTION: A method of preventing discoloration of silver or a silver alloy and corrosion of gold or a gold alloy is performed by depositing a thin coating of bismuth on the silver, silver alloy, gold, or gold alloy. The thin bismuth coating does not spoil the electric performance of the silver, silver alloy, gold, or gold alloy even after thermal aging.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preventing discoloration of silver and corrosion of gold. More specifically, the present invention relates to a method for preventing discoloration of silver and corrosion of gold by depositing a bismuth layer on the surface of silver or gold to a thickness sufficient to prevent discoloration of silver and corrosion of gold and to maintain good electrical performance even after thermal aging.

Background Art

[0002] Silver is used as a metal finish for applications in the electronics industry. Connector and lead frame components may include silver finishes due to their excellent electrical properties. There is also a financial incentive for using silver, as it is much less expensive than gold. A major drawback of silver is its tendency to discolor, resulting in the formation of a layer on the surface that impairs the appearance, which is not visually acceptable and has insulating properties, so the electrical performance of silver when applied as a finish for electrical components is impaired. The main product of silver discoloration is silver sulfide, which is generated through the semi-reactions 8Ag + 4HS - ⇔4Ag2S + 2H2 + 4e - and O2 + 2H2O + 4e - ⇔4OH - due to the presence of sulfides such as hydrogen sulfide present in the atmosphere. In dry air, discoloration does not occur. When water is present (relative humidity of 5 - 50% or more), oxygen functions as a cathode species and consumes electrons as shown in the equations. As the concentration of silver sulfide increases, the discoloration increases. The discoloration rate gradually decreases with an increase in the thickness of the discolored layer, but this reaction proceeds even on a significantly discolored surface. Silver sulfide does not form a protective layer for preventing surface corrosion due to its rough structure.

[0003] Therefore, silver deposition requires the use of a post-treatment to prevent tarnishing of the silver surface. Traditionally, organic tarnishing treatments for silver consisted of fatty acid thiols. These molecules form a dense, self-assembled monolayer due to the high enthalpy of the silver-sulfur bond and van der Waals interactions of the hydrocarbon tails of the long-chain fatty acid thiol molecules. The hydrophobicity of the resulting monolayer prevents interaction between water and the silver surface, thus preventing tarnishing. However, this method has drawbacks, such as the long process time required for monolayer formation and the need for a flammable organic solvent to dissolve the long-chain thiols. Another major drawback of using organic molecules for tarnishing treatment is their thermal instability. Organic molecules evaporate or decompose when heated to temperatures above 100°C. The aliphatic carbon-hydrogen bonds of the long hydrocarbon chains also oxidize and thus decompose in a high-temperature, oxygen-containing atmosphere, rendering them ineffective as a post-treatment for silver.

[0004] As an alternative to organic post-treatment, metallic or inorganic treatments have also been disclosed. Unlike typical organic post-treatments, metallic coatings do not volatilize even at high temperatures. Metal oxides of zinc, titanium, or aluminum have been used to prevent tarnishing. Chromium(VI) is also a conventionally used coating component, but has not been widely used due to its toxicity. In addition, precious metals can also protect the surface of silver. Such thin coatings are typically electroplated as an inert topcoat to prevent silver from interacting with sulfur and moisture, and therefore no tarnishing of the silver is observed, as disclosed in (Patent Document 1), (Patent Document 2), (Patent Document 3), and (Patent Document 4). These thin metallic coatings can also preserve the lustrous appearance of silver. The main drawback of these treatments is the cost associated with precious metal coatings. In addition, intermetallic compounds can be formed by heating. Thus, thermal instability is not related to the evaporation of the post-treatment, but rather to diffusion into the silver, which impairs electrical performance (i.e., increases contact resistance).

[0005] Hard silver or gold alloys of cobalt and nickel are widely used as contact materials for electrical connectors in high-reliability applications. Connectors with a hard gold final layer are often electroplated over a nickel substrate, such as nickel plating on copper. Generally, selective plating techniques such as spot plating significantly reduce the material cost of connectors by limiting the plating area of ​​gold and other precious metals, such as palladium and palladium-nickel alloys. Although hard gold does not tarnish like silver, it often has a thin, porous surface through which the underlying nickel layer can corrode, potentially impairing the performance of the electrical connector. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] European Patent No. 2196563 [Patent Document 2] U.S. Patent Application Publication No. 20020185716 [Patent Document 3] U.S. Patent Application Publication No. 20170253983 [Patent Document 4] U.S. Patent No. 10,056,707B2 [Overview of the project] [Problems that the invention aims to solve]

[0007] Therefore, there is a need for a method to prevent silver discoloration and porosity corrosion of the underlying nickel layer by applying a gold or silver alloy topcoat. [Means for solving the problem]

[0008] A method for electroplating bismuth, comprising the steps of: providing a substrate containing silver, a silver alloy, gold, or a gold alloy; providing a bismuth electroplating solution containing a bismuth ion source, an acid, a salt of an acid, or a combination thereof; bringing the substrate into contact with the bismuth electroplating solution; applying an electric current to the bismuth electroplating solution and the substrate; and electroplating bismuth onto the silver, silver alloy, gold, or hard gold substrate to a thickness of more than 0 nm and less than or equal to 20 nm.

[0009] A bismuth electroplating solution comprising a bismuth ion source, an acid, a salt of an acid, or a combination thereof, water, optionally a surfactant, optionally a brightener, optionally an antibacterial agent, and optionally an antifoaming agent.

[0010] An article comprising a layer of silver, a silver alloy, gold, or a gold alloy, and having a bismuth layer adjacent to a monolayer of silver, a silver alloy, or hard gold with a thickness of 20 nm or less.

[0011] A bismuth layer on silver, silver alloys, gold, or gold alloys prevents discoloration of silver and corrosion of gold, and provides low contact resistance that enables good electrical performance even after thermal aging. [Brief explanation of the drawing]

[0012] [Figure 1] This is a schematic diagram of the metal layer continuum of the present invention, comprising a brass base, a nickel barrier layer adjacent to the brass base, a silver layer adjacent to the nickel barrier layer, and a bismuth layer adjacent to the silver layer. [Figure 2] This is a schematic diagram of the metal layer continuum of the present invention, comprising a brass base, a silver layer adjacent to the brass base, and a bismuth layer adjacent to the silver layer. [Figure 3] This is a schematic diagram of the metal layer continuum of the present invention, comprising a brass base, a nickel barrier layer adjacent to the brass base, a silver alloy layer adjacent to the nickel barrier layer, and a bismuth layer adjacent to the silver alloy layer. [Figure 4] This is a schematic diagram of the metal layer continuum of the present invention, comprising a brass base, a nickel barrier layer adjacent to the brass base, a hard gold layer adjacent to the nickel barrier layer, and a bismuth layer adjacent to the hard gold layer. [Figure 5] Schematic of the metal layer continuum of the present invention by a copper-iron-phosphite-zinc base (copper-C-194), a silver layer adjacent to the copper-iron-phosphite-zinc base, and a bismuth layer adjacent to the silver layer.

Embodiments for Carrying Out the Invention

[0013] The following abbreviations have the following meanings, unless otherwise clearly interpreted in the context: °C = degrees Celsius, g = gram, mL = milliliter, L = liter, A = ampere, dm = decimeter, ASD = ampere / dm 2 , mΩ = milliohm, nm = nanometer, μm = micrometer, cm = centimeter, eN = centinewton, sec = second, DI = deionized, DC = direct current, XRF = X-ray fluorescence, bismuth ion = bismuth (III) = Bi 3+ , wt% = weight percent, ASTM = American Society for Testing and Materials, NA = not available or not applicable.

[0014] All percentages and ratios are by weight, unless otherwise expressly stated. All ranges are inclusive and can be combined in any order, except when it is inevitable that the sum of such numerical ranges must be 100%.

[0015] Throughout this specification, the terms "plating" and "electroplating" are used interchangeably. The indefinite articles (a, an) are taken to include both singular and plural. The term "adjacent" means adjacent or joined so as to have a common interface. The term "contact resistance" means the contribution that can be made to the overall resistance of a system by the contact interfaces of electrical leads and connections. The term "additional vertical force" means the force applied to an object by a person or another object, i.e., gravity or weight. The term "centinewton" is a unit of measurement of force. The term "ohm" is the SI coherent unit of electrical resistance. The term "monolayer" means a layer one molecule thick.

[0016] The bismuth electroplating solution of the present invention contains water, a bismuth (III) ion source, an acid, optionally a brightener, and optionally a surfactant (preferably consisting of these). The plating solution does not contain alloy metals, and therefore, the deposit plated from the plating solution of the present invention is substantially 100% bismuth.

[0017] The bismuth source provides bismuth (III) (Bi 3+ ) ions and corresponding neutralization. Preferably, the bismuth (II) ion source is water-soluble. Examples of the bismuth (III) ion source include bismuth salts of alkanesulfonic acids such as bismuth methanesulfonate, bismuth ethanesulfonate, bismuth propanesulfonate, 2-bismuth propanesulfonate, and bismuth p-phenolsulfonate; bismuth salts of alkanolsulfonic acids such as bismuth hydroxymethanesulfonate, bismuth 2-hydroxyethane-1-sulfonate, and bismuth 2-hydroxybutane-1-sulfonate; bismuth salts such as bismuth nitrate, bismuth sulfate, and bismuth chloride, but are not limited thereto. Mixtures of bismuth (III) ion sources can also be included in the bismuth electroplating solution of the present invention. More preferably, the bismuth (III) ion source is selected from the group consisting of bismuth methanesulfonate, bismuth ethanesulfonate, bismuth propanesulfonate, and mixtures thereof. Most preferably, the bismuth (III) ion source is bismuth methanesulfonate.

[0018] Preferably, the bismuth salt is included in the plating solution to provide bismuth (III) ions in an amount of 1 to 200 g / L, more preferably 1 to 150 g / L, even more preferably 1 to 100 g / L, far more preferably 1 to 50 g / L, still more preferably 1 to 25 g / L, and most preferably 1 to 10 g / L. Such bismuth salts may be commercially available or produced according to the disclosure of chemical literature. These are generally commercially available from various suppliers including Aldrich Chemical Company in Milwaukee, Wisconsin.

[0019] The acids included in the bismuth plating solution are organic, inorganic, or a mixture thereof. Salts of organic and inorganic acids can also be included in the bismuth electroplating solution of the present invention. Mixtures of acids and salts can also be included in the bismuth electroplating solution of the present invention. Preferably, organic acids and their salts are included in the bismuth electroplating solution of the present invention. Preferably, organic acids include, but are not limited to, alkanesulfonic acids, alkanolsulfonic acids, and aromatic sulfonic acids. Alkanesulfonic acids include, but are not limited to, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, 1-butanesulfonic acid, 2-butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, decanesulfonic acid, and dodecanesulfonic acid. Alkanol sulfonic acids include, but are not limited to, 1-hydroxypropane-2-sulfonic acid, 3-hydroxypropane-1-sulfonic acid, 4-hydroxybutane-1-sulfonic acid, 2-hydroxyhexane-1-sulfonic acid, 2-hydroxydecane-1-sulfonic acid, 2-hydroxy-dodecane-1-sulfonic acid, 2-hydroxyethane-1-sulfonic acid, 2-hydroxypropane-1-sulfonic acid, 2-hydroxybutane-1-sulfonic acid, and 2-hydroxypentane-1-sulfonic acid. Aromatic sulfonic acids include, but are not limited to, benzenesulfonic acid, alkylbenzenesulfonic acid, phenolsulfonic acid, cresolsulfonic acid, sulfosalicylic acid, nitrobenzenesulfonic acid, sulfobenzoic acid, and diphenylamine-4-sulfonic acid. Preferably, the organic acid is an alkanesulfonic acid. More preferably, the alkanesulfonic acid is selected from the group consisting of methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, their salts, and mixtures thereof. Most preferably, the alkanesulfonic acid is methanesulfonic acid or a salt thereof.

[0020] Preferably, the organic acid is water-soluble. Preferably, the organic acid and its salt are included in the plating solution in an amount of 1 to 1000 g / L, more preferably 5 to 500 g / L, even more preferably 10 to 250 g / L, much more preferably 10 to 100 g / L, and most preferably 10 to 60 g / L. The acids described above may be commercially available or may be manufactured according to disclosures in chemical literature. These are generally commercially available from various distributors, including Aldrich Chemical Company in Milwaukee, Wisconsin.

[0021] Inorganic acids include, but are not limited to, sulfuric acid, nitric acid, hydrochloric acid, sulfamic acid, and their salts. Preferably, the inorganic acid is sulfuric acid and its salts. Preferably, the inorganic acid and its salts can be included in the plating solution in an amount of 10 to 200 g / L, more preferably 20 to 100 g / L, and even more preferably 30 to 70 g / L.

[0022] The pH of the bismuth electroplating solution of the present invention is 7 or less, preferably less than 7, more preferably 0 to 6, even more preferably 0 to 2, and most preferably less than 0 to 2.

[0023] Optionally, but preferably, the bismuth electroplating solution of the present invention contains a surfactant. Preferably, the surfactant is polyoxymethylene acrylic ether, e.g., commercially available from ADEKA Corporation, ADEKA® TOL PC-8; amine oxide, e.g., commercially available from Evonik Operation GmbH, TOMAMINE® AO-455; branched alcohol alkoxylate nonionic surfactant, e.g., commercially available, TERGITOL® CA; polyether polyol, e.g., commercially available, TERGITOL® L-64; secondary alcohol ethoxylate, e.g., commercially available, TERGITOL® 15-S-7; nonionic low-foaming surfactant, e.g., poly(oxy-1,2-ethanosyl), alpha-(phenylmethyl)-omega-(1,1,3,3-tetramethylbutyl)phenoxy, polyethylene glycol octylphenyl ether, and decanoic acid in a mixture, TRITON® CF-87 (all available from Dow Chemical Company in Midland, Michigan); a mixture of organic and inorganic components, e.g., sodium dodecylphenylsulfonate in a wetting solution. The surfactant is selected from the group consisting of Agent W and Wetting Agent NAW-4 (also available from DOW Chemical Company), which contains a mixture of 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-2H-isothiazole-3-one. Preferably, the surfactant is a nonionic surfactant.

[0024] The surfactant can be included in the bismuth electroplating solution in conventional amounts. Preferably, the surfactant is included in an amount of 0.1 to 2 g / L, more preferably 0.5 to 2 g / L, and even more preferably 0.5 to 1 g / L.

[0025] An antifoaming agent can be optionally included in the bismuth plating solution. Conventional antifoaming agents can be used and included in conventional amounts. The antifoaming agent is preferably included in an amount of 10 to 100 mg / L. An example of a preferred commercially available antifoaming agent is FOAM BAN® MS-293 antifoaming agent, available from Inwoo Corporation of Gobiz Korea, which contains a mixture of 5-decine 4,7-diol,2,4,7,9-tetramethyl (less than 2.5 wt%) and ethylene glycol (less than 2.5 wt%).

[0026] The bismuth electroplating solution of the present invention may optionally contain a brightener. Conventional brighteners can be included in the bismuth electroplating solution. Preferably, the brightener is selected from the group consisting of 5-sulfosalicylic acid, cysteine, 1,6-hexanediol, thiodiethanol, 4,5-dihydroxy-1,3-benzenedisulfonic acid, 2,2-bis(hydroxymethyl)propionic acid, thiodiglycolic acid, its salts, and combinations thereof. More preferably, the brightener is selected from the group consisting of 5-sulfosalicylic acid, 4,5-dihydroxyl-1,3-benzenedisulfonic acid, thiodiglycolic acid, its salts, and mixtures thereof.

[0027] The brightener can be included in conventional amounts. Preferably, the brightener is included in the bismuth electroplating solution in an amount equivalent to 0.5 to 20 molar equivalents of bismuth(III) ions in the bismuth electroplating solution. More preferably, the brightener is included in an amount equivalent to 0.5 to 15 molar equivalents of bismuth(III) ions in the bismuth electroplating solution, and even more preferably, the brightener is included in an amount equivalent to 0.5 to 10 molar equivalents of bismuth(III) ions in the bismuth electroplating solution.

[0028] Optionally, the bismuth electroplating solution may contain one or more antimicrobial agents. Conventional antimicrobial agents typically included in electroplating solutions may be used. Such antimicrobial agents are well known in the industry. They are used in conventional amounts.

[0029] Bismuth can be plated onto the surfaces of silver, silver alloys, hard gold, and soft gold using the electroplating solution of the present invention at a current density of 0.1 ASD or higher. Preferably, bismuth can be plated at a current density of 0.1 to 5 ASD, more preferably 0.1 to 3 ASD, and most preferably 0.1 to 1 ASD.

[0030] Preferably, bismuth electroplating is carried out at a liquid temperature of room temperature to 60°C, more preferably room temperature to 50°C, even more preferably 30 to 50°C, and most preferably 35 to 45°C.

[0031] The bismuth layer adjacent to silver, silver alloys, hard gold, and soft gold is in the range of greater than 0 nm to 20 nm, or the bismuth is 20 nm, more preferably greater than 1 nm to 20 nm, more preferably greater than 1 nm to 10 nm, even more preferably greater than 1 nm to 7 nm, and most preferably the thickness of the bismuth layer is 1 to 5 nm. In addition to the bismuth metal deposited adjacent to silver, silver alloys, hard gold, and soft gold, the deposit may contain bismuth(III).

[0032] A bismuth layer adjacent to silver or a silver alloy prevents discoloration of the surface of the silver or silver alloy, and a bismuth layer adjacent to hard gold or soft gold prevents corrosion of the gold. As a result, silver, silver alloys, hard gold, and soft gold can maintain low contact resistance even under an additional vertical force of 100 cN, resulting in good conductivity. Furthermore, the bismuth layer of the present invention prevents discoloration of silver and silver alloys, as demonstrated by conventional accelerated sulfidation tests by immersing the substrate in a 2 wt% potassium polysulfide aqueous solution. The bismuth layer also prevents discoloration after thermal aging, as demonstrated by conventional thermal aging tests. The bismuth layer also prevents corrosion of hard gold, even after thermal aging, as demonstrated by conventional thermal aging tests, which is demonstrated by conventional nitric acid vapor (NAV) and sulfur dioxide vapor tests.

[0033] Preferably, the silver is substantially about 98-99.9 wt% silver, and the silver can be deposited on a substrate or article surface by conventional methods known in the industry. Preferably, the silver is deposited by electroplating from a silver electroplating solution.

[0034] Silver plating solutions contain silver ions, which can be provided as silver salts, including but not limited to silver cyanide, silver oxide, silver hydantoin, silver succinate, silver halides, silver gluconate, silver citrate, silver lactate, silver nitrate, silver sulfate, silver alkanesulfonate, silver alkanolsulfonate, or combinations thereof. When silver halides are used, preferably the halides are chlorides. Mixtures of silver salts can also be included in the composition. Silver salts are generally commercially available or can be prepared by methods described in the literature and are included in conventional amounts in water-soluble silver electroplating compositions, and are well known to those skilled in the art. Silver plating solutions may contain conventional additives such as electrolytes, complexing agents, buffers, and brighteners. Such additives are included in conventional amounts and are well known to those skilled in the art. Commercially available silver electroplating solutions include SILVERON® GT-101 Bright Silver or SILVERGLO® 3K Bright Silver (both available from Dupont Electronic & Industrial in Marlborough, Massachusetts).

[0035] Preferably, the current density for electroplating the silver layer can be in the range of 0.1 ASD to 50 ASD, or for example, 1 ASD to 5 ASD. Preferably, the temperature of the silver plating solution can be room temperature to 50°C. Preferably, the silver layer is 0.1 μm to 20 μm thick.

[0036] Silver alloys include, but are not limited to, silver-tin, silver-indium, silver-nickel, and silver-gold. Preferably, the silver alloy is a silver-tin alloy. Preferably, the silver content of the silver-tin alloy is about 70-95 wt%, with the remainder being tin and trace amounts of impurities.

[0037] Silver-tin alloys can be deposited on a substrate using conventional methods known in the industry. Preferably, the silver-tin alloy is electroplated from a silver-tin electroplating solution. Such an electroplating solution contains one or more sources of silver ions. The ion sources include, but are not limited to, silver salts such as silver halides, silver gluconate, silver citrate, silver lactate, silver nitrate, silver sulfate, silver alkanesulfonate, and silver alkanolsulfonate. Silver salts are generally commercially available or can be prepared by methods described in the literature. Preferably, the concentration of silver salt in the plating solution can be in the range of 1 g / L to 100 g / L.

[0038] Preferably, the tin ion source includes, but is not limited to, salts such as tin halides, tin sulfides, tin alkanesulfonic acids, tin alkanolsulfonic acids, and acids. Tin salts are generally commercially available or can be prepared by methods known in the literature. Preferably, the tin salt can be in the range of 0.1 g / L to 80 g / L. The silver / tin alloy electroplating solution may also contain one or more conventional plating solution additives, which are included in conventional amounts known in the industry. Preferably, the current density for electroplating the silver-tin layer can be in the range of 0.1 ASD to 50 ASD, for example, 1 ASD to 5 ASD. Preferably, the temperature of the silver-tin plating solution can be in the range of room temperature to 50°C. An example of a commercially available hard gold alloy electroplating solution is SILVERON® GT-820 Silver-Tin (available from Dupont Electronic & Industrial, Marlborough, Massachusetts). Preferably, the silver-tin layer is 0.1 μm to 20 μm thick.

[0039] Hard gold is either gold-cobalt or gold-nickel alloy. Gold-cobalt alloys preferably have a gold content of about 98-99.95 wt% and a cobalt content of about 0.01-2 wt%. Gold-nickel alloys preferably have a gold content of about 98-99.95 wt% and a nickel content of about 0.01-2 wt%. Most preferably, hard gold alloys consist of 0.1 wt% to 0.4 wt% cobalt and the remainder gold.

[0040] Hard gold can be deposited on a substrate by conventional methods known in the industry. Preferably, hard gold is electroplated onto the substrate using a gold-cobalt alloy electroplating solution. Gold ion sources for the plating solution include, but are not limited to, potassium gold cyanide, sodium gold dicyano(I), ammonium gold dicyano(I), and other dicyanoano(I) salts, potassium gold tetracyano(III), sodium gold tetracyano(III), ammonium gold tetracyano(III), and other tetracyanoano(III) salts, gold cyanide, gold cyanide, dichloroauroate(I), tetrachloroauroate(III), sodium gold tetrachloro(III), and other tetrachloroauroate(III) compounds, ammonium gold sulfide, potassium gold sulfide, sodium gold sulfide, and other gold sulfite compounds, gold oxide, gold hydroxide, and other alkali metal salts thereof, and nitrosulfito gold complexes. Preferably, the gold ion source is included in a conventional amount, such as 3 g / L to 8 g / L.

[0041] Gold alloy electroplating solutions may also contain conventional additives, such as surfactants, brighteners, smoothing agents, complexing agents, chelating agents, buffering agents, organic and inorganic acids, and biocides, but are not limited to these. Such additives are included in conventional amounts and are well known in the industry. An example of a commercially available hard gold alloy electroplating solution is RONOVEL® CM Cobalt-Alloyed Electrolytic Gold (available from Dupont Electronic & Industrial, Marlborough, Massachusetts).

[0042] Hard gold alloy electroplating can be performed at a current density of preferably 0.1 ASD to 10 ASD, more preferably 0.5 ASD to 3 ASD, and at a temperature of 30°C to 60°C. The pH of the hard gold alloy electroplating solution can be in the range of 4 to 8.

[0043] Preferably, soft gold or gold is approximately 98-99.9 wt% gold, with the remainder being unavoidable impurities. Soft gold or gold can be deposited onto a substrate using conventional methods known in the art. Preferably, soft gold or gold is electroplated onto the substrate. The gold ion source is the same as that described above for hard gold. The gold ion source can be included in conventional amounts in the plating solution. Plating solutions for soft gold and gold may also contain surfactants, brighteners, smoothing agents, complexing agents, chelating agents, buffering agents, organic and inorganic acids, and biocides. Such additives are included in conventional amounts and are well known among those skilled in the art. A commercially available soft gold plating solution is AURONAL® BGA LF gold electroplating solution (available from Dupont Electronic & Industrial, Marlborough, Massachusetts).

[0044] A substrate containing silver, silver alloy, hard gold, or soft gold is brought into contact with the bismuth electroplating solution of the present invention by any suitable method known in the art, such as immersing the substrate in the solution or spraying the plating solution onto the substrate. An insoluble electrode, such as an insoluble platinum-plated titanium electrode, can serve as the anode. Bismuth plating is carried out according to the parameters described above for depositing a bismuth layer adjacent to the silver, silver alloy, hard gold, or soft gold.

[0045] The bismuth electroplating solution of the present invention can also be used to plate bismuth onto any suitable substrate, including silver, silver alloys, hard gold, or soft gold layers. Preferably, the method of the present invention is used to deposit bismuth adjacent to silver, silver alloys, or hard gold on lead frames or similar electronic components. Such electronic components preferably include a brass base of a copper-zinc alloy, optionally comprising a nickel barrier layer and a silver or silver alloy surface layer. The nickel barrier layer, silver layer, and silver alloy layer are deposited using conventional plating compositions and methods well known in the industry, such as electroplating.

[0046] The nickel barrier layer can be deposited by conventional methods known in the art. Preferably, the nickel barrier layer is deposited by electroplating from a nickel plating solution. Nickel ion sources for the nickel electroplating solution include, but are not limited to, nickel sulfate or its hydrated form, nickel sulfamate or its hydrated form, nickel chloride hexahydrate, nickel methanesulfonate, or nickel acetate or its hydrated form. One or more nickel ion sources are included in conventional amounts in aqueous nickel electroplating compositions and are well known to those skilled in the art. The nickel plating solution may contain conventional additives, which include, but are not limited to, surfactants, brighteners, smoothing agents, complexing agents, chelating agents, buffering agents, and biocides. Such additives are included in conventional amounts and are well known to those skilled in the art. Examples of commercially available nickel electroplating solutions are NIKAL® PC-3 BrightNickel and NIKAL® SC Nickel (both available from Dupont Electronic & Industrial in Marlborough, Massachusetts).

[0047] Preferably, the current density for electroplating the nickel layer is 0.5 ASD to 20 ASD, or for example, 1 ASD to 10 ASD. Preferably, the nickel plating solution is electroplated at a temperature of room temperature to 60°C.

[0048] The article of the present invention includes a brass base 10, as shown in Figure 1. The brass base preferably includes a copper-zinc alloy. Adjacent to the base 10 is an optional nickel barrier layer 12. Preferably, the thickness of the nickel barrier is 0 to 2 μm. Adjacent to the nickel barrier layer is a silver layer 14, preferably with a thickness of 0.5 to 7 μm. Adjacent to the silver layer 14 is a bismuth layer 16, preferably with a thickness of 1 to 20 nm.

[0049] Figure 2 shows an article of the present invention that does not include a nickel barrier layer. The brass base 20 preferably contains a copper-zinc alloy. Adjacent to the brass base 20 is a silver layer 22, and adjacent to the silver layer 22 is a bismuth layer 24. The thickness of the metal layers is substantially the same as in Figure 1.

[0050] Figure 3 shows an article of the present invention, preferably including a brass base 30 made of a copper-zinc alloy. Adjacent to the brass base 30 is a nickel barrier layer 32. Adjacent to the nickel barrier layer 32 is a silver-tin alloy layer 34. A bismuth layer 36 is adjacent to the silver-tin alloy layer.

[0051] Figure 4 shows an article of the present invention, preferably including a brass base 40 made of a copper-zinc alloy. A nickel barrier layer 42 is adjacent to the brass base 40. A hard gold layer 44 is adjacent to the nickel barrier layer 42. A bismuth layer 46 is adjacent to the hard gold layer 44.

[0052] Another article of the present invention is shown in Figure 5. The base comprises brass of a copper-iron-phosphite-zinc alloy (copper-C194) 50. Adjacent to the brass base is a layer of silver 52, and adjacent to the silver layer 52 is a layer of bismuth 54.

[0053] The following examples are included for illustrative purposes only and are not intended to limit the scope of the present invention. [Examples]

[0054] Example 1 Multiple 3cm x 4cm copper-zinc alloy brass substrates were electroplated with a 1μm nickel barrier layer using nickel electroplating solution, NIKAL® PC-3 Bright Nickel, or NIKAL® SC Nickel. The current density for electroplating the nickel layer was 4 ASD. The nickel plating solution temperature was 50°C.

[0055] A 2 μm silver layer was plated onto a nickel layer using silver electroplating solution, SILVERON® GT-101 Bright Silver, or SILVERGLO® 3K Bright Silver electroplating solution. The current density for electroplating the silver layer was 2 ASD at 50°C.

[0056] The thickness of the nickel and silver layers was measured by XRF using a BOWMAN® P-Series fluorescence analyzer. The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN. The applied force was controlled using a Starrett DFC-20 force meter. The resistance was measured using a Keithley 2010 Multimeter with a gold reference probe contact.

[0057] Subsequently, the substrate was immersed in a 2 wt% aqueous potassium polysulfide sulfidation test solution at room temperature for 5 minutes. The substrate was removed from the sulfidation test solution, rinsed with DI water, and air-dried. The silver turned dark blue. Contact resistance was measured under an applied vertical force of 0 to 100 cN. The contact resistance of the discolored silver was significantly higher than that of the undiscolored silver. Under an applied force of 100 cN, the contact resistance of the discolored silver was approximately 8 mΩ. In contrast, the contact resistance of the undiscolored silver was only 1.5 mΩ (Table 1).

[0058] [Table 1]

[0059] Example 2 A 3cm x 4cm brass copper-zinc alloy substrate was electroplated with nickel to a thickness of 1 μm, followed by silver to a thickness of 2 μm, as described in Example 1. The thickness of the silver layer was measured by XRF using a BOWMAN® P-Series fluorescence analyzer. The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN, as described in Example 1. The results are shown in Table 3 below.

[0060] Aqueous bismuth electroplating solutions were prepared as shown in the table below.

[0061] [Table 2]

[0062] The plating solution was heated to 40°C. An insoluble platinum-plated titanium anode was immersed in the plating layer and connected to a DC power supply. A silver-plated substrate was immersed in a bismuth electroplating solution and used as the cathode. A current density of 0.2 ASD was applied for 5 seconds to plate a 10 nm bismuth layer on the silver. The current supply was cut off, the substrate was removed, washed with DI water, and air-dried. The contact resistance was measured immediately.

[0063] Next, the bismuth-plated substrate was heated in a conventional laboratory oven at 125°C for 18 hours, and the contact resistance was measured. Afterward, an accelerated sulfidation test was performed on the substrate, and the contact resistance was measured again. The substrate retained its luster and gray color. The contact resistance was 1.5 mΩ with an applied vertical force of 100 cN, which was equivalent to that of freshly plated pure silver (Table 3).

[0064] [Table 3]

[0065] Example 3 A 2.5 cm x 3.8 cm brass copper-zinc alloy substrate was electroplated with nickel to a thickness of 1 μm, followed by silver to a thickness of 2 μm, as described in Example 1. The thickness of the silver layer was measured by XRF using a BOWMAN® P-Series fluorescence analyzer. The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN, as described in Example 1, and the data is shown in Table 5 below.

[0066] Subsequently, the silver-plated substrate was heated in a conventional laboratory oven at 270°C for 10 minutes. The substrate was then cooled to room temperature. Next, the substrate was immersed in a 2 wt% potassium polysulfide accelerated sulfidation test aqueous solution at room temperature for 5 minutes. The substrate was removed from the sulfidation test solution, rinsed with DI water, and air-dried. The contact resistance was measured with an applied vertical force of 0 to 100 cN, and the results are shown in Table 5 below.

[0067] Aqueous bismuth electroplating solutions were prepared as shown in the table below.

[0068] [Table 4]

[0069] A 2.5 cm × 3.8 cm brass copper-zinc alloy substrate, having a 1 μm nickel layer and a 2 μm silver top layer, was plated with a 10 nm bismuth layer. The plating solution was heated to 40°C. A platinum-plated titanium anode was immersed in the plating solution and connected to a DC power supply as the anode. A silver-plated substrate was immersed in the plating solution and connected to a cathode wire. A current density of 0.2 ASD was applied for 5 seconds. The potential was turned off, the substrate was removed, washed with DI water, and dried. The substrate was then heat-treated in a conventional laboratory oven at 270°C for 10 minutes. After the substrate cooled to room temperature, an accelerated sulfidation test was performed and the contact resistance was measured. The data is shown in Table 5 below. The bismuth-treated substrate retained its gloss and gray color.

[0070] A comparison with octadecanethiol as a post-treatment was also performed. A 2.5 cm × 3.8 cm brass copper-zinc alloy substrate was plated with a 1 μm nickel layer and a 2 μm silver top layer, and then immersed for 30 seconds in a 30°C solution containing 0.1 M octadecanethiol and emulsified with the nonionic surfactant, TRITON (trademark) X-114 (40 g / L). The substrate was heated in a conventional laboratory oven at 270°C for 10 minutes, then subjected to an accelerated sulfidation test, rinsed with DI water, and air-dried. Contact resistance was measured with an applied vertical force of 0 to 100 cN, and the results are shown in Table 5 below.

[0071] When the substrate was heated under the same conditions, both without post-treatment and with octadecanethiol post-treatment, it turned purple after the sulfidation test. In the bismuth-containing post-treatment, a glossy appearance was maintained, and the low contact resistance after heating and sulfidation was a low 1 mΩ at an applied vertical force of 100 cN.

[0072] [Table 5]

[0073] Example 4 A 2.5 cm x 3.8 cm brass copper-zinc alloy substrate was electroplated with nickel to a thickness of 1 μm, followed by silver to a thickness of 2 μm, as described in Example 1. The thickness of the silver layer was measured by XRF using a BOWMAN® P-Series fluorescence analyzer. The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN, as described in Example 1, and is reported in Table 7 below.

[0074] Subsequently, the silver-plated substrate was heat-treated in air at 150°C for 1000 hours. The substrate was then cooled to room temperature. Next, the substrate was immersed in a 2 wt% potassium polysulfide accelerated sulfidation test aqueous solution at room temperature for 5 minutes. The substrate was removed from the sulfidation test solution, rinsed with DI water, and air-dried. The silver surface turned purple. The contact resistance was measured with an applied vertical force of 0 to 100 cN, and the results are shown in Table 7 below.

[0075] Aqueous bismuth electroplating solutions were prepared as shown in the table below.

[0076] [Table 6]

[0077] The plating solution was heated to 40°C. A platinum-plated titanium anode was immersed in the plating solution and connected to a DC power supply as the anode. A brass substrate made of copper-zinc alloy with a 1 μm thick nickel layer and a 2 μm thick silver layer was immersed in the plating solution and connected to a cathode wire. A current density of 0.3 ASD was applied for 5 seconds to deposit a 10 nm thick bismuth layer on top of the silver. The current was turned off, the substrate was removed, washed with DI water, and dried. The substrate was heated in air at 150°C for 1000 hours, after which an accelerated sulfidation test was performed and the contact resistance was measured. The appearance of the substrate retained its luster and gray color, and the contact resistance measured with an applied vertical force of 100 cN was 1.5 mΩ, which was equivalent to that of freshly plated 99.9 wt% silver, as shown in Figure 7 below.

[0078] [Table 7]

[0079] Example 5 A 2.5 cm x 3.8 cm brass copper-zinc alloy substrate was electroplated with nickel to a thickness of 1 μm, followed by silver to a thickness of 2 μm, as described in Example 1. The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN, as described in Example 1, and the results are shown in Table 9 below.

[0080] Aqueous bismuth electroplating solutions were prepared as shown in the table below.

[0081] [Table 8]

[0082] The plating solution was heated to 40°C. An insoluble platinum-plated titanium anode was immersed in the plating solution and connected to a DC power supply as the anode. A silver-plated brass substrate was immersed in the plating solution and connected to a cathode wire. A current density of 0.2 ASD was applied for 5 seconds to deposit a bismuth layer to a thickness of 10 nm on the silver. The power supply was turned off, the substrate was removed, washed with DI water, and dried. The contact resistance was measured immediately. Subsequently, the bismuth-plated substrate was heated in a conventional laboratory oven at 180°C for 48 hours, and the contact resistance was measured again. Next, an accelerated sulfidation test was performed on the substrate, and the contact resistance was measured again. The appearance of the bismuth layer on the substrate retained its luster and gray color. The contact resistance, measured with an added vertical force of 100 cN, was 1.2 mΩ, which was equivalent to that of silver plating.

[0083] [Table 9]

[0084] Example 6 A 2.5cm x 3.8cm brass copper-zinc alloy substrate was electroplated with nickel to a thickness of 1μm using NIKAL® SC Nicel electroplating solution (Dupont Electronic and Industrial, Marlborough, Massachusetts), and then with a silver-tin alloy (80wt% silver, 20wt% tin) to a thickness of 2μm using SILVERON® GT-820 Silver-Tin electroplating solution. A current density of 2 ASD was applied at 50°C for 2 minutes.

[0085] The thickness of the silver-tin layer was measured by XRF using a BOWMAN® P-Series fluorescence analyzer. The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN, as described in Example 1, and is shown in Table 11.

[0086] The silver-tin plated substrate was then heat-treated in air at 180°C for 48 hours. The substrate was cooled to room temperature and immersed in an accelerated sulfidation test solution at room temperature for 5 minutes. The substrate was removed from the sulfidation test solution, rinsed with DI water, and air-dried. The silver-tin had a dull gray appearance. Contact resistance was measured with an applied vertical force of 0 to 100 cN.

[0087] Aqueous bismuth electroplating solutions were prepared as shown in the table below.

[0088] [Table 10]

[0089] The plating solution was heated to 40°C. A platinum-plated titanium anode was immersed in the plating solution and connected to a DC power supply. A 2.5 × 3.8 cm brass substrate was electroplated with NIKAL® SC Nickel electroplating solution to a thickness of 1 μm by applying a current density of 4 ASD for 2 minutes at a plating solution temperature of 50°C. Subsequently, a silver-tin alloy (80 wt% silver, 20 wt% tin) was electroplated to a thickness of 2 μm by applying a current density of 2 ASD for 2 minutes at a plating solution temperature of 50°C using SILVERON® GT-820 Silver-Tin electroplating solution. Next, the substrate was immersed and connected to a cathode wire. A current of 0.4 ASD was applied for 5 seconds to deposit 10 nm bismuth into the silver-tin alloy layer. The electrons were turned off, the substrate was removed, washed with DI water, and dried. The substrate was heated in a conventional laboratory oven at 180°C for 48 hours, and then an accelerated sulfurization test was performed to measure the contact resistance. The substrate retained its gloss and gray color, and the contact resistance, measured with an applied vertical force of 100 cN, was <10 mΩ. [Table 11]

[0090] Example 7 Six 2.5cm x 5cm brass copper-zinc alloy test pieces were electroplated with a 1μm thick nickel layer using NIKAL® SC Nickel electroplating solution. Nickel plating was performed at 4 ASD for 2 minutes at 55°C. Hard gold alloy was then plated onto the nickel to a thickness of 0.5μm using RONOVEL® CM Cobalt-Alloyed Electrolytic Gold. The hard gold alloy was plated at 1 ASD for 4 minutes at a plating solution temperature of 50°C. The thicknesses of the nickel and hard gold layers were measured by XRF using a BOWMAN® P-Series fluorescence analyzer.

[0091] Four of the plated substrates were post-treated in PORE BLOCKER® 200 anti-tarnish corrosion agent (available from Dupont Electronic & Industrial, Marlborough, Massachusetts). The substrates were immersed in the anti-tarnish agent at room temperature for 5 minutes, removed, and rinsed with DI water. They were then air-dried at room temperature.

[0092] A aqueous bismuth electroplating solution was prepared as shown in the figure below.

[0093] [Table 12]

[0094] The plating solution was heated to 40°C. A platinum-plated titanium anode was immersed in the plating solution and connected to a DC power supply. Two of the post-treated hard gold substrates were immersed in the plating solution and electrically connected to the cathode wire. A current density of 0.2 ASD was applied for 5 seconds to deposit a 10 nm thick bismuth layer on the hard gold alloy. The current was turned off, the substrates were removed, washed with DI water, and air-dried at room temperature.

[0095] The corrosion tests performed on the plated substrates were nitric acid vapor (NAV) tests according to ASTM B735 and sulfur dioxide vapor tests according to ASTM B799. The thermal stability of the discoloration prevention post-treatment was evaluated by visually comparing the corrosion of substrates heated to 180°C for 48 hours or 125°C for 18 hours before the corrosion test with those that were not heated.

[0096] In substrates without any anti-tarnish post-treatment, the nickel underlayer of electroplated hard gold alloy substrates corroded in both tests. In substrates coated with PORE BLOCKER® 200 Anti-tarnish Formation, no corrosion of the nickel underlayer was observed in unheated substrates. However, when substrates treated with PORE BLOCKER® 200 anti-tarnish post-treatment were heated at 125°C for 18 hours before the corrosion test, substantial underlayer corrosion was observed. Substrates with bismuth plating post-treatment did not corrode under ASTM B735 or ASTM B799 conditions, whether heat-treated or unheated. These results are summarized in Table 13.

[0097] [Table 13]

[0098] Example 8 A 0.5 μm nickel barrier layer was electroplated onto a 2.5 cm x 3.8 cm brass copper-zinc alloy substrate using NIKAL® SC Nickel electroplating solution. A current density of 4 ASD was applied for 1 minute, and the plating solution temperature was 50°C. A 0.4 μm soft gold top layer (99.9% gold) was then plated on top of the nickel using AURONAL® BGA LF gold electroplating solution. Gold electroplating was performed at a current density of 1 ASD for 4 minutes at 50°C. The pH of the gold electroplating solution was 5.5 during plating.

[0099] The contact resistance of the substrate was measured with an applied vertical force of 0 to 100 cN, as described in Example 1. The contact resistance was measured again at room temperature after plating, and again after heat treatment in air at 180°C for 24 hours.

[0100] Aqueous bismuth electroplating solutions were prepared as shown in the table below.

[0101] [Table 14]

[0102] The solution was heated to 40°C. A platinum-plated titanium anode was immersed in the plating solution and connected to a DC power supply. A current of 0.2 ASD was applied for 5 seconds to deposit a bismuth layer on a 2.5cm × 3.8cm brass-copper-zinc alloy substrate having a 0.5μm nickel barrier layer and a 0.4μm thick gold layer. The current was turned off, the substrate was removed, washed with DI water, and dried. The contact resistance was measured immediately, and then the substrate was heated in air at 180°C for 24 hours. Visual evaluation of the substrate's appearance revealed luster and a golden color. There was no change in contact resistance. The contact resistance remained at approximately 2mΩ with an applied force of 100cN, as shown in Table 15 below.

[0103] [Table 15] [Explanation of symbols]

[0104] 10. Base 12 Nickel barrier layer 14 Silver layer 16 Bismuth layer 20 Brass base 22 Silver layer 24 Bismuth layer 30 Brass base 32 Nickel barrier layer 34 Silver-tin alloy layer 36 Bismuth layer 40 Brass base 42 Nickel barrier layer 44 Hard gold layer 46 Bismuth layer 50 Copper-iron zinc phosphite alloy 52 Silver layer 54 Bismuth layer

Claims

1. 1. A method for electroplating bismuth, comprising: providing a substrate comprising silver, a silver alloy, gold, or a gold alloy; providing a bismuth electroplating solution comprising a source of bismuth ions, an acid, a salt of the acid, or a combination thereof; contacting the substrate with the bismuth electroplating solution; applying an electric current to the bismuth electroplating solution and a substrate; electroplating bismuth onto the silver, silver alloy, gold, or gold alloy of the substrate to a thickness of greater than 0 nm and less than or equal to 20 nm; A method comprising:

2. The method of claim 1 , wherein the thickness ranges from greater than 1 nm to 10 nm.

3. The method of claim 2, wherein the thickness ranges from greater than 1 nm to 7 nm.

4. The method of claim 1 , wherein the current density is 0.1 ASD or greater.

5. The method of claim 4, wherein the current density ranges from 0.1 to 5 ASD.

6. A bismuth electroplating solution comprising a source of bismuth ions, an acid, a salt of an acid, or a combination thereof, water, optionally a surfactant, optionally a brightener, optionally an antibacterial agent, and optionally an antifoaming agent.

7. 7. The bismuth electroplating solution of claim 6, comprising a surfactant selected from the group consisting of secondary alcohol ethoxylates, polyether polyols, polyoxyethylene allyl ethers, amine oxides, nonionic low foaming surfactants, and mixtures thereof.

8. 7. The bismuth electroplating solution of claim 6, comprising a brightener selected from the group consisting of 5-sulfosalicylic acid, cysteine, 1,6-hexanediol, thiodiethanol, 4,5-dihydroxy-1,3-benzenedisulfonic acid, 2,2-bis(hydroxymethyl)propionic acid, taurine, diodiglycolic acid, salts thereof, and mixtures thereof.

9. An article comprising a layer of silver, a silver alloy, gold, hard gold, or a combination thereof, having a bismuth layer of more than 0 nm and not more than 20 nm adjacent to the silver, silver alloy, gold, or hard gold.

10. 10. The article of claim 9, further comprising a brass base and a nickel barrier layer, wherein the silver, silver alloy, gold, or hard gold layer is adjacent to the nickel barrier layer, and the nickel barrier layer is adjacent to the brass base.

11. 10. The article of claim 9, wherein the bismuth layer is in the range of greater than 1 nm to 10 nm.

12. 12. The article of claim 11, wherein the bismuth layer is in the range of greater than 1 nm to 7 nm.