Polarizer protection film, polarizing plate and image display device

JP2023171426A5Active Publication Date: 2024-11-11TOYOBO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023165229
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-02-22
Filing Date
2023-09-27
Publication Date
2024-11-11
Estimated Expiration
2038-03-29

AI Technical Summary

Benefits of technology

【0010】 本発明の偏光子保護フィルム、偏光板及び画像表示装置(液晶表示装置や有機ELディスプレイ等)は、いずれの観察角度においても虹状の色斑(以下、虹斑と同じ)が抑制された良好な視認性を確保することができる。また、本発明の偏光板および偏光子保護フィルムは、薄膜化に適した機械強度を備えており、良好な加工特性を確保することができる。本発明によれば、フィルムを薄膜化した際にも虹状の色斑による視認性の悪化が有意に抑制された偏光子保護フィルム、偏光板および画像表示装置を提供することができる。

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a polarizer protection film, a polarizing plate and an image display device, capable of accommodating the thinning of an image display device and suppressing deterioration in visibility due to iridescent spots.SOLUTION: A polarizer protection film includes a polyester film, where the slow axis direction of the polyester film is approximately parallel to an MD direction, and the in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.20 or less, the polarizer protection film further satisfying the following (A) or (B): (A) the refractive index in the fast axis direction of the polyester film is 1.580 or more and 1.630 or less; and (B) the smaller value out of tear strengths by a right angle tear method in the slow axis direction and the fast axis direction of the polyester film is 250 N / mm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to polarizer protective films, polarizing plates, and image display devices such as liquid crystal displays and organic EL displays. More specifically, it relates to polarizer protective films, polarizing plates, and image display devices (such as liquid crystal displays and organic EL displays) that offer good visibility and are suitable for thinning. [Background technology]

[0002] Polarizing plates used in liquid crystal displays (LCDs) typically consist of a polarizer, made of polyvinyl alcohol (PVA) or similar material impregnated with iodine, sandwiched between two polarizer protective films. Triacetylcellulose (TAC) film is commonly used as the polarizer protective film. In recent years, with the miniaturization and cost reduction of LCDs, there has been a demand for thinner polarizing plates. However, reducing the thickness of the TAC film used as the protective film results in insufficient mechanical strength and poor moisture permeability. Furthermore, TAC film is very expensive, creating a strong need for inexpensive alternative materials.

[0003] Polyester film offers superior durability compared to TAC film, but unlike TAC film, it possesses birefringence. Therefore, when used as a polarizer protective film, it suffers from a problem of reduced image quality due to optical distortion. Specifically, because birefringent polyester film has a certain optical anisotropy (retardation), when used as a polarizer protective film, it produces rainbow-like color spots when viewed from an oblique direction, resulting in reduced image quality. To address this, Patent Document 1 describes a solution to the rainbow-like color spots by controlling the in-plane retardation of the polyester film within a specific range. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] WO2011-162198 [Overview of the project] [Problems that the invention aims to solve]

[0005] However, the market demands even thinner image display devices such as liquid crystal displays, and as polarizer protective films become thinner, it becomes difficult to ensure sufficient retardation to adequately suppress iridescent color variations. Furthermore, the reduced film thickness leads to insufficient mechanical strength for processing, making it difficult to meet the demand for thinner films.

[0006] In one embodiment of the present invention, the objective is to provide a polarizer protective film, a polarizing plate, and an image display device (such as a liquid crystal display or an organic EL display) that can accommodate the thinning of image display devices such as liquid crystal displays and organic EL displays (i.e., has sufficient mechanical strength) and suppresses deterioration of visibility due to rainbow-like color spots. [Means for solving the problem]

[0007] Typical examples of the present invention are as follows: Section A1. A polarizer protective film containing a polyester film, The slow phase axis direction of the polyester film is substantially parallel to the MD direction. The in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.20 or less. The refractive index of the polyester film in the phase-advancing axis direction is 1.580 or more and 1.630 or less. Polarizer protective film. Section A2. The polarizer protective film according to item A1, wherein the smaller of the tear strengths of the polyester film measured by a right-angle tear test in the slow-phase axis direction and the fast-phase axis direction is 250 N / mm or more. Section A3. The polarizer protective film according to item A1 or A2, wherein the NZ coefficient of the polyester film is 1.5 or more and 2.5 or less. Section A4. A polarizer protective film according to any one of items A1 to A3, wherein the retardation of the polyester film is between 1500 nm and 30000 nm. Section A5. A polarizer protective film according to any of items A1 to A4, wherein the thickness of the polyester film is 25 to 60 μm. Section A6. A polarizer protective film according to any of items A1 to A5, wherein the angle between the slow phase axis direction and the MD direction of the polyester film is 3 degrees or less. Section A7. A polarizer protective film according to any of items A1 to A6, wherein the elastic modulus of the polyester film in the MD direction is 3000 MPa or more. Section A8. A polarizing plate in which a polarizer protective film described in any of items A1 to A7 is laminated on at least one surface of the polarizer. Section A9. A polarizing plate in which a polarizer protective film described in any of items A1 to A7 is laminated on one side of the polarizer, and no film is laminated on the other side of the polarizer. Section A10. A polarizer having a polarizer protective film described in any of items A1 to A7 laminated on one side of the polarizer, and a quarter-wave plate laminated on the other side of the polarizer. Section A11. An image display device including a polarizing plate as described in any of items A8 to A10. Section A12. A liquid crystal display device including a polarizing plate as described in item A8 or A9. Section A13. An organic EL display including a polarizing plate as described in any of items A8 to A10. Section A14. A QLED display including a polarizing plate as described in any of items A8 to A10.

[0008] Section B1. A polarizer protective film containing a polyester film, The slow phase axis direction of the polyester film is substantially parallel to the MD direction. The in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.2 or less, The smaller value of the tear strength by the right-angle tear method in the slow axis direction and the fast axis direction of the polyester film is 250 N / mm or more, Polarizer protection film. Item B2. The polarizer protection film according to Item B1, wherein the NZ coefficient of the polyester film is 1.5 or more and 2.5 or less. Item B3. The polarizer protection film according to Item B1 or B2, wherein the retardation of the polyester film is 1500 nm or more and 30000 nm or less. Item B4. The polarizer protection film according to any one of Items B1 to B3, wherein the thickness of the polyester film is 25 to 60 μm. Item B5. The polarizer protection film according to any one of Items B1 to B4, wherein the angle formed by the slow axis direction of the polyester film and the MD direction is within 3 degrees. Item B6. The polarizer protection film according to any one of Items B1 to B5, wherein the elastic modulus in the MD direction of the polyester film is 3000 MPa or more. Item B7. A polarizing plate in which the polarizer protection film according to any one of Items B1 to B6 is laminated on at least one surface of the polarizer. Item B8. A polarizing plate in which the polarizer protection film according to any one of Items B1 to B6 is laminated on one surface of the polarizer, and no film is laminated on the other surface of the polarizer. Item B9. A polarizing plate in which the polarizer protection film according to any one of Items B1 to B6 is laminated on one surface of the polarizer, and a quarter-wave plate is laminated on the other surface of the polarizer. Item B10. An image display device including the polarizing plate according to any one of Items B7 to B9. Item B11. A liquid crystal display device including the polarizing plate according to Item B7 or B8. Item B12. An organic EL display including a polarizing plate as described in any of items B7 to B9. Section B13. A QLED display including a polarizing plate as described in any of items B7 to B9.

[0009] Section C1. A polarizer protective film containing a polyester film, The slow phase axis direction of the polyester film is substantially parallel to the MD direction. The in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.2 or less. The thickness of the polyester film is 15 to 60 μm. Polarizer protective film. Section C2. The polarizer protective film according to item C1, wherein the NZ coefficient of the polyester film is 1.5 or more and 2.5 or less. Section C3. The polarizer protective film according to item C1 or C2, wherein the retardation of the polyester film is 1500 nm or more and 30000 nm or less. Section C4. A polarizer protective film according to any of items C1 to C3, wherein the angle between the slow phase axis direction and the MD direction of the polyester film is 3 degrees or less. Section C5. A polarizer protective film according to any of items C1 to C4, wherein the elastic modulus of the polyester film in the MD direction is 3000 MPa or more. Section C6. A polarizing plate in which a polarizer protective film described in any of items C1 to C5 is laminated on at least one surface of the polarizer. Section C7. A polarizing plate in which a polarizer protective film described in any of items C1 to C5 is laminated on one side of the polarizer, and no film is laminated on the other side of the polarizer. Section C8. A polarizer having a polarizer protective film described in any of items C1 to C5 laminated on one side of the polarizer, and a quarter-wave plate laminated on the other side of the polarizer. Section C9. An image display device including a polarizing plate as described in any of items C6 to C8. Section C10. A liquid crystal display device comprising a polarizing plate as described in item C6 or C7. Section C11. An organic EL display including a polarizing plate as described in any of items C6 to C8. Section C12. A QLED display including a polarizing plate as described in any of items C6 to C8. [Effects of the Invention]

[0010] The polarizer protective film, polarizer plate, and image display device (such as a liquid crystal display device or an organic EL display) of the present invention can ensure good visibility with suppressed iridescent color spots (hereinafter the same as iridescence) at any observation angle. Furthermore, the polarizer plate and polarizer protective film of the present invention have mechanical strength suitable for thinning and can ensure good processing characteristics. According to the present invention, it is possible to provide a polarizer protective film, polarizer plate, and image display device in which deterioration of visibility due to iridescent color spots is significantly suppressed even when the film is thinned. [Modes for carrying out the invention]

[0011] 1. Polarizer protective film In one embodiment, the polarizer protective film of the present invention is a polarizer protective film comprising a polyester film, wherein the slow phase axis direction of the polyester film is substantially parallel to the MD direction, the in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.20 or less, and the refractive index of the polyester film in the phase-advancing axis direction is 1.580 or more and 1.630 or less.

[0012] In one embodiment, the polarizer protective film of the present invention is a polarizer protective film comprising a polyester film, wherein the slow phase axis direction of the polyester film is substantially parallel to the MD direction, the in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.2 or less, and the smaller of the tear strengths of the polyester film measured by a right-angle tear test in the slow phase axis direction and the fast phase axis direction is 250 N / mm or more.

[0013] In one embodiment, the polarizer protective film of the present invention is a polarizer protective film comprising a polyester film, wherein the slow phase axis direction of the polyester film is substantially parallel to the MD direction, the in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.20 or less, and the thickness of the polyester film is 15 to 60 μm. The objective of this embodiment is to provide a polarizer protective film in which deterioration of visibility due to rainbow-like color spots is significantly suppressed even when the film is made into a thin film, and to provide a thin polarizer plate and an image display device (such as a liquid crystal display device or an organic EL display).

[0014] The slow phase axis of the polyester film used as the polarizer protective film of the present invention is preferably substantially parallel to the MD direction (the direction of travel during film formation) from the viewpoint of suppressing iridescent color spots. Here, substantially parallel means that the angle between the slow phase axis direction of the polyester film and the MD direction (the direction of travel during film formation) is preferably within 10 degrees, more preferably within 7 degrees, even more preferably within 5 degrees, particularly preferably within 3 degrees, and most preferably within 2 degrees.

[0015] The direction of the slow axis can be determined using a molecular orientation meter (MOA-6004 molecular orientation meter, manufactured by Oji Instruments Co., Ltd.).

[0016] In this specification, the MD direction refers to the direction of travel during film formation and is sometimes called the longitudinal direction. The TD direction refers to the width direction during film formation and is sometimes called the transverse direction.

[0017] When industrially producing image display devices (such as liquid crystal displays and organic EL displays) using polarizers with polyester film as a polarizer protective film, the direction of the polarizer's absorption axis and the slow phase axis of the polyester film are usually positioned perpendicular to each other. This is due to the following circumstances: The polyvinyl alcohol film used as the polarizer is manufactured by MD uniaxial stretching. Therefore, the polyvinyl alcohol film used as the polarizer is usually a film that is long in the stretching direction and has its absorption axis in the MD direction. On the other hand, the polyester film used as its protective film is usually manufactured by MD stretching followed by TD stretching, so the orientation principal axis direction (slow phase axis direction) of the polyester film is in the TD direction. From the viewpoint of manufacturing efficiency, these films are usually laminated roll to roll so that their longitudinal directions are parallel to each other to manufacture the polarizer. In this case, the slow phase axis of the polyester film and the absorption axis of the polarizer are usually perpendicular to each other.

[0018] On the other hand, in the present invention, it is preferable that the orientation principal axis direction (slow phase axis direction) of the polyester film is in the MD direction. Such a polyester film is obtained by strongly stretching the polyester film in the MD direction. When a polarizer is manufactured by laminating this polyester film and a polarizer manufactured by uniaxial stretching in the MD direction using a roll-to-roll method with their longitudinal directions parallel, the absorption axis of the polarizer and the slow phase axis of the polyester film are parallel. The inventors have discovered that when the absorption axis of the polarizer and the slow phase axis of the polyester film are laminated in a state where they are parallel, the iridescence suppression effect is superior to when the absorption axis of the polarizer and the slow phase axis of the polyester film are perpendicular. In order to efficiently manufacture a polarizer with excellent iridescence suppression effect using an industrially advantageous roll-to-roll method, it is preferable to use a polyester film in which the MD direction and the slow phase axis direction are substantially parallel, by strongly stretching the polyester film in the MD direction.

[0019] The in-plane birefringence ΔNxy of the polyester film used in the polarizer protective film of the present invention is preferably 0.06 or more and 0.2 or less, more preferably 0.07 or more and 0.19 or less, and even more preferably 0.08 or more and 0.18 or less. If ΔNxy is less than 0.06, iridescent color spots are more likely to be observed when viewed from an oblique direction. Furthermore, while iridescent color spots do not occur in films with ΔNxy greater than 0.2, the mechanical strength in the direction parallel to the orientation direction decreases significantly because it approaches perfect uniaxiality (uniaxial symmetry). The in-plane birefringence ΔNxy is the absolute value of the difference between the refractive index (nx) in the slow phase axis direction and the refractive index (ny) in the fast phase axis direction. The measurement wavelength for the refractive index is 589 nm.

[0020] In one embodiment, the refractive index (ny) in the phase-advancing axis direction of a polyester film used in the polarizer protective film of the present invention, in which the slow phase axis direction is substantially parallel to the MD direction, is preferably 1.58 or more and 1.63 or less, more preferably 1.584 or more and 1.625 or less, and even more preferably 1.588 or more and 1.62 or less. If the refractive index (ny) in the phase-advancing axis direction falls below 1.58, it approaches perfect uniaxiality (uniaxial symmetry), and the mechanical strength (tear strength) in the direction parallel to the orientation direction decreases significantly. In addition, in films where the refractive index (ny) in the phase-advancing axis direction exceeds 1.63, iridescent color spots are more easily observed when viewed from an oblique direction.

[0021] The smaller of the tear strengths measured by right-angle tearing in the slow axis direction and the fast axis direction of the polyester film used in the polarizer protective film of the present invention is preferably 250 N / mm or more, more preferably 280 N / mm or more, and even more preferably 300 N / mm or more. In films with a high ΔNxy value, the tear strength in the slow axis direction tends to be smaller than that in the fast axis direction. Conventionally, it has been difficult to meet the demand for thin films because the mechanical strength required for processing becomes insufficient as the film thickness decreases. However, if the smaller of the tear strengths measured by right-angle tearing in the slow axis direction and the fast axis direction of the film is 250 N / mm or more, the above problem can be solved. If it is less than 250 N / mm, the film will tear easily, and the stability during film formation and processing will decrease. On the other hand, while higher tear strength increases stability during film formation and processing, it also increases biaxiality (biaxial symmetry), resulting in iridescent color variations. Therefore, it is preferable to increase the tear strength to a level that does not produce iridescent color variations, and in practice, 500 N / mm or less is preferable. The tear strength is measured according to the right-angle tear test method (JIS K-7128-3), and the tear strength per unit film thickness (N / mm) is determined.

[0022] The NZ coefficient of the polyester film used in the polarizer protective film of the present invention is preferably 1.5 to 2.5, more preferably 1.6 to 2.3, and even more preferably 1.7 to 2.1. The smaller the NZ coefficient, the less likely rainbow-like color variations will occur depending on the observation angle. Furthermore, while the NZ coefficient is 1.0 for a perfectly uniaxial (uniaxially symmetric) film, the mechanical strength in the direction parallel to the orientation tends to decrease as the film approaches perfect uniaxiality (uniaxial symmetry).

[0023] The NZ coefficient can be determined as follows: The orientation principal axis direction (slow phase axis direction) of the film is determined using a molecular orientation meter (MOA-6004, manufactured by Oji Instruments Co., Ltd.). The refractive indices in the two axes perpendicular to the orientation principal axis direction (fast phase axis direction) (refractive index nx in the slow phase axis direction, refractive index ny in the fast phase axis direction, where nx > ny), and the refractive index in the thickness direction (nz) are determined using an Abbe refractometer (NAR-4T, manufactured by Atago, measurement wavelength 589 nm). The NZ coefficient can then be determined by substituting the obtained nx, ny, and nz into the formula |nx-nz| / |nx-ny|. The measurement wavelength for the refractive index is 589 nm.

[0024] From the viewpoint of further reducing iridescence, the polyester film used in the polarizer protective film preferably has a retardation of 1500 nm to 30000 nm. The lower limit of the retardation is preferably 2500 nm, and the next preferred lower limit is 3000 nm.

[0025] On the other hand, the upper limit of retardation is 30,000 nm. Even if a polyester film with a retardation greater than this is used, not only is no further improvement in visibility not substantially obtained, but the film thickness also becomes considerably thicker, which is undesirable because it reduces the ease of handling as an industrial material. In one embodiment, the preferred upper limit of retardation is 8,000 nm, the more preferred upper limit is 6,000 nm, the even more preferred upper limit is 5,500 nm, and the particularly preferred upper limit is 5,000 nm.

[0026] Birefringence can be determined by measuring the refractive index in two axes, or by using a commercially available automatic birefringence measuring device such as the KOBRA-21ADH (Oji Instruments Co., Ltd.). The measurement wavelength for the refractive index is 589 nm.

[0027] The elastic modulus in the MD direction of the polyester film used in the polarizer protective film of the present invention is preferably 3000 MPa or higher. In recent years, with the thinning of LCDs, the thinning of components has progressed. In this context, with the thinning of the glass substrate used in liquid crystal panels, the problem of warping of liquid crystal panels caused by the shrinkage of the polarizer has become apparent. The shrinkage of the polarizer is caused by the shrinkage of the PVA film, which is the polarizer (mainly shrinkage in the direction of the absorption axis), and it is preferable to control the shrinkage of the polarizer by the rigidity of the protective film. If the elastic modulus in the running direction of the protective film is 3000 MPa or higher, sufficient control force will act against the shrinkage of the polarizer, and it is possible to prevent warping of the liquid crystal panel. However, if it is significantly below 3000 MPa, there is a risk that the warping of the liquid crystal panel will become apparent. The preferred lower limit of the elastic modulus in the MD direction is 3500 MPa, the more preferred lower limit is 4000 MPa, and the still more preferred lower limit is 4500 MPa.

[0028] The polyester used in the polarizer protective film of the present invention can be polyethylene terephthalate or polyethylene naphthalate, but may also contain other copolymer components. These resins have excellent transparency as well as excellent thermal and mechanical properties, and their in-plane birefringence can be easily controlled by stretching. In particular, polyethylene terephthalate has a large intrinsic birefringence, and a large in-plane birefringence can be obtained relatively easily, making it the most suitable material.

[0029] Furthermore, in order to suppress the degradation of optically functional dyes such as iodine dyes, it is desirable that the polarizer protective film of the present invention has a light transmittance of 20% or less at a wavelength of 380 nm. A light transmittance of 15% or less at 380 nm is more preferable, 10% or less is even more preferable, and 5% or less is particularly preferable. If the light transmittance is 20% or less, the deterioration of optically functional dyes due to ultraviolet light can be suppressed. The transmittance in the present invention is measured perpendicular to the plane of the film and can be measured using a spectrophotometer (for example, Hitachi U-3500).

[0030] To achieve a transmittance of 20% or less at a wavelength of 380 nm in the polarizer protective film of the present invention, it is desirable to appropriately adjust the type and concentration of the ultraviolet absorber and the thickness of the film. The ultraviolet absorber used in the present invention is a known substance. Examples of ultraviolet absorbers include organic ultraviolet absorbers and inorganic ultraviolet absorbers, but organic ultraviolet absorbers are preferred from the viewpoint of transparency. Examples of organic ultraviolet absorbers include benzotriazole-based, benzophenone-based, cyclic iminoester-based, and combinations thereof, but are not particularly limited as long as they fall within the absorbance range defined by the present invention. However, from the viewpoint of durability, benzotriazole-based and cyclic iminoester-based are particularly preferred. When two or more ultraviolet absorbers are used in combination, ultraviolet light of different wavelengths can be absorbed simultaneously, thereby further improving the ultraviolet absorption effect.

[0031] Examples of benzophenone-based UV absorbers, benzotriazole-based UV absorbers, and acrylonitrile-based UV absorbers include 2-[2'-hydroxy-5'-(methacryloyloxymethyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxyethyl)phenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(methacryloyloxypropyl)phenyl]-2H-benzotriazole, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,4-di-tert-butyl-6-(5-chlorobenzotriazole-2-yl)phenol, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, and 2-(5-chloro(2H)-benzotriazole-2-yl)-4-methyl-6-(tert-butyl)pheno Examples include 2,2'-methylenebis(4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole-2-yl)phenol. Examples of cyclic iminoester-based UV absorbers include 2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazinone-4-one), 2-methyl-3,1-benzoxazin-4-one, 2-butyl-3,1-benzoxazin-4-one, and 2-phenyl-3,1-benzoxazin-4-one. However, the list is not limited to these.

[0032] Furthermore, in addition to the ultraviolet absorber, it is also preferable to include various additives other than catalysts, to the extent that they do not hinder the effects of the present invention. Examples of additives include inorganic particles, heat-resistant polymer particles, alkali metal compounds, alkaline earth metal compounds, phosphorus compounds, antistatic agents, light-resistant agents, flame retardants, heat stabilizers, antioxidants, gelation inhibitors, and surfactants. In addition, in order to achieve high transparency, it is preferable that the polyester film is substantially free of particles. "Substantially free of particles" means, for example, in the case of inorganic particles, that the content is 50 ppm or less, preferably 10 ppm or less, and particularly preferably below the detection limit when inorganic elements are quantified by fluorescence X-ray analysis.

[0033] In the polarizer protective film of the present invention, it is also preferable to apply various hard coatings to the surface for purposes such as preventing reflections, suppressing glare, and preventing scratches.

[0034] Furthermore, in the present invention, the polyester film may be subjected to corona treatment, coating treatment, flame treatment, etc., in order to improve adhesion with polarizers and various hard coat layers.

[0035] In the present invention, in order to improve adhesion to the polarizer, it is preferable that at least one side of the film of the present invention has an easy-adhesion layer mainly composed of at least one of polyester resin, polyurethane resin, or polyacrylic resin. Here, "main component" refers to a component that accounts for 50% by mass or more of the solid components constituting the easy-adhesion layer. The coating liquid used to form the easy-adhesion layer of the present invention is preferably an aqueous coating liquid containing at least one of water-soluble or water-dispersible copolymer polyester resin, acrylic resin, and polyurethane resin. Examples of these coating liquids include water-soluble or water-dispersible copolymer polyester resin solutions, acrylic resin solutions, polyurethane resin solutions, etc., disclosed in Japanese Patent Publication No. 3567927, Japanese Patent Publication No. 3589232, Japanese Patent Publication No. 3589233, Japanese Patent Publication No. 3900191, Japanese Patent Publication No. 4150982, etc.

[0036] The easy-adhesion layer can be obtained by applying the coating solution to at least one side of the film surface during any step in the polyester film manufacturing process, followed by drying at 100-150°C. The final amount of the easy-adhesion layer applied is 0.05-0.2 g / m². 2 It is preferable to manage the amount to 0.05 g / m². 2 If the amount is significantly lower than the specified value, the adhesion to the resulting polarizer may be insufficient. On the other hand, if the coating amount is 0.2 g / m² 2If this value is significantly exceeded, the blocking resistance may decrease. When an easy-adhesion layer is provided on both sides of the polyester film, the amount of easy-adhesion layer applied to both sides may be the same or different, and can be set independently within the above range.

[0037] It is preferable to add particles to the easy-adhesion layer to provide slipperiness. It is preferable to use particles with an average particle size of 2 μm or less. If the average particle size significantly exceeds 2 μm, the particles tend to fall off the coating layer. Examples of particles to be included in the easy-adhesion layer include inorganic particles such as titanium dioxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, and calcium fluoride, as well as organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles. These may be added to the easy-adhesion layer individually, or two or more may be added in combination.

[0038] Furthermore, known methods can be used for applying the coating solution. Examples include the reverse roll coating method, gravure coating method, kiss coating method, roll brush method, spray coating method, air knife coating method, wire bar coating method, and pipe doctor method, and these methods can be used individually or in combination.

[0039] The average particle size of the above-mentioned particles is measured by the following method: A scanning electron microscope (SEM) is used to photograph the particles, and the maximum diameter (distance between the two furthest points) of 300 to 500 particles is measured at a magnification such that the size of the smallest particle is 2 to 5 mm. The average value of these measurements is then taken as the average particle size.

[0040] Polyester films can be manufactured according to general polyester film manufacturing methods. For example, one method involves melting polyester resin, extruding it into a sheet, stretching the unoriented polyester in the longitudinal and transverse directions at a temperature above the glass transition temperature, and then heat-treating it.

[0041] The polyester film of the present invention may be either a uniaxially oriented film or a biaxially oriented film. However, when a biaxially oriented film is used as a polarizer protective film, rainbow-like color spots may not be visible when viewed from directly above the film surface, but they may be visible when viewed from an oblique angle, so caution is necessary.

[0042] This phenomenon occurs because a biaxially oriented film is composed of refractive index ellipsoids with different refractive indices in the running direction, width direction, and thickness direction, and there is a direction in which retardation becomes zero (the refractive index ellipsoid appears as a perfect circle) depending on the direction of light transmission within the film. Therefore, when the display screen is observed from a specific oblique direction, a point where retardation becomes zero may occur, and rainbow-like color spots will appear concentrically around that point. If we let θ be the angle from directly above the film surface (normal direction) to the position where the rainbow-like color spots are visible, this angle θ increases as the birefringence within the film surface increases, and the rainbow-like color spots become less visible. Since biaxially oriented films tend to have a smaller angle θ, uniaxially oriented films are preferable because the rainbow-like color spots are less visible.

[0043] However, a perfectly uniaxial (uniaxially symmetrical) film is undesirable because its mechanical strength in the direction parallel to the orientation direction is significantly reduced. The present invention preferably has biaxiality (biaxial symmetry) in a range where rainbow-like color spots do not occur substantially, or in a range where rainbow-like color spots do not occur within the viewing angle range required for the display screen.

[0044] The film-forming conditions for the polyester film of the present invention may be sequential biaxial stretching or simultaneous biaxial stretching. However, in general sequential biaxial stretching, the longitudinal stretching is roll stretching, which makes the film prone to scratches. Therefore, from the viewpoint of preventing scratches during stretching, simultaneous biaxial stretching without rolls is preferable. Specifically, the film-forming conditions are as follows: The longitudinal stretching temperature and transverse stretching temperature are preferably 80 to 150°C, and particularly preferably 90 to 140°C. The longitudinal stretching ratio is preferably 5.5 to 7.5 times, more preferably 6.0 to 7.0 times, and particularly preferably 6.5 to 7.0 times. The transverse stretching ratio is preferably 1.5 to 3.0 times, and particularly preferably 1.8 to 2.8 times. In order to control the direction of the slow axis, ΔNxy, the refractive index value in the fast axis direction, the NZ coefficient, and the tear strength within the above ranges, it is preferable to control the respective ratios of the longitudinal stretching ratio and the transverse stretching ratio. If the difference in the stretch ratio between the longitudinal and transverse directions is too small, it becomes difficult to increase ΔNxy, which is undesirable. Setting a lower stretching temperature is also a desirable approach for increasing ΔNxy.

[0045] To achieve high tear strength while keeping the refractive index in the phase-advancing axis direction within the aforementioned range, it is preferable that the film has a moderate degree of biaxiality under conditions where ΔNxy satisfies the range specified in this application, rather than being a perfectly uniaxial film. In the subsequent heat treatment, the treatment temperature is preferably 100 to 250°C, and particularly preferably 180 to 245°C.

[0046] As mentioned above, controlling ΔNxy and the NZ coefficient within a specific range can be achieved by appropriately setting the stretching ratio and stretching temperature. For example, a higher stretching ratio and a lower stretching temperature make it easier to obtain a higher ΔNxy. Conversely, a lower stretching ratio and a higher stretching temperature make it easier to obtain a lower ΔNxy. In addition to controlling ΔNxy and the NZ coefficient, it is preferable to set the final film formation conditions by considering the physical properties required for processing.

[0047] The thickness of the polyester film used as the polarizer protective film of the present invention is arbitrary, but is preferably in the range of 15 to 200 μm, and more preferably in the range of 15 to 150 μm. With films thinner than 15 μm, the mechanical properties of the film deteriorate significantly, making it prone to tearing and ripping, and significantly reducing its practicality as an industrial material. The lower limit of the preferred thickness is 25 μm, the lower limit of the more preferred lower limit is 30 μm, and the lower limit of the still more preferred lower limit is 35 μm. On the other hand, the upper limit of the thickness of the polarizer protective film is undesirable if it exceeds 200 μm, as this makes the polarizer plate too thick. From the viewpoint of practicality as a polarizer protective film, the upper limit of the thickness is preferably 150 μm, the upper limit of the more preferred upper limit is 80 μm, the upper limit of the still more preferred upper limit is 60 μm, the upper limit of the still more preferred upper limit is 55 μm, the upper limit of the still more preferred upper limit is 50 μm, and the upper limit of the still more preferred upper limit is 45 μm. In order to control the ΔNxy, NZ coefficients and tear strength within the range of the present invention, polyethylene tarephthalate is preferred as the polyester used as the film substrate, even within the thickness range described above.

[0048] Furthermore, while known methods can be used in combination to incorporate the ultraviolet absorber into the polyester film in the present invention, for example, a masterbatch can be prepared by first blending the dried ultraviolet absorber with the polymer raw material using a kneading extruder, and then mixing the predetermined masterbatch with the polymer raw material during film formation.

[0049] At this time, the concentration of the UV absorber in the masterbatch is preferably 5 to 30% by mass in order to uniformly disperse the UV absorber and to formulate it economically. The conditions for preparing the masterbatch are preferably using a kneading extruder, with an extrusion temperature above the melting point of the polyester raw material and below 290°C for 1 to 15 minutes. Above 290°C, the amount of UV absorber decreases significantly, and the viscosity of the masterbatch also decreases significantly. Below 1 minute, uniform mixing of the UV absorber becomes difficult. At this time, stabilizers, color adjusters, and antistatic agents may be added as needed.

[0050] Furthermore, in the present invention, it is preferable to have a multilayer structure of at least three layers, and to add an ultraviolet absorber to the intermediate layer of the film. Specifically, a three-layer film containing an ultraviolet absorber in the intermediate layer can be manufactured as follows: Polyester pellets alone are used for the outer layer, and a masterbatch containing an ultraviolet absorber and polyester pellets are mixed in a predetermined ratio for the intermediate layer. After drying, the mixture is supplied to a known melt lamination extruder, extruded into a sheet from a slit-shaped die, and cooled and solidified on a casting roll to produce an unstretched film. That is, two or more extruders and a three-layer manifold or confluence block (for example, a confluence block having a square confluence section) are used to laminate the film layers constituting both outer layers and the film layer constituting the intermediate layer, the three-layer sheet is extruded from a die, and cooled on a casting roll to produce an unstretched film. In addition, in the present invention, it is preferable to perform high-precision filtration during melt extrusion in order to remove foreign matter contained in the raw polyester that causes optical defects. The filtration particle size (initial filtration efficiency of 95%) of the filter material used for high-precision filtration of the molten resin is preferably 15 μm or less. If the filtration particle size of the filter media significantly exceeds 15 μm, the removal of foreign matter larger than 20 μm tends to be insufficient.

[0051] 2. Polarizing plate The polarizer plate has a structure in which a polarizer protective film is laminated on at least one side of a polarizer made of PVA or the like that is dyed with iodine. In the polarizer plate of the present invention, it is preferable to use the polarizer protective film of the present invention having the above-mentioned specific polyester film as at least one of the polarizer protective films constituting the polarizer plate. In one preferred embodiment, the polarizer protective film of the present invention having the above-mentioned specific polyester film is laminated on one side of the polarizer, and a non-birefringent polarizer protective film or optical compensation film such as a TAC film, norbornene film, or acrylic film is laminated on the other side of the polarizer. In another preferred embodiment, the polarizer protective film of the present invention containing the above-mentioned specific polyester film is laminated on one side of the polarizer, and no film is laminated on the other side of the polarizer (no film is attached to the polarizer on the other side of the polarizer in an independent state). In the above other preferred embodiment, a coating layer (hard coat layer, anti-glare layer, anti-reflective layer, low-reflection layer, moisture-resistant layer (which may be made of organic or inorganic material), or a layer combining these functions) may be provided on the side of the polarizer opposite to the side on which the specific polyester film is laminated.

[0052] As described above, in order to suppress iridescence and to suppress warping of the liquid crystal panel, it is preferable that the polarizer's absorption axis and the polyester film's slow axis are laminated in a substantially parallel relationship. Here, substantially parallel means that a slight deviation is permitted. The angle between the polarizer's absorption axis and the polyester film's slow axis is preferably within 10 degrees, more preferably within 7 degrees, even more preferably within 5 degrees, particularly preferably within 3 degrees, and most preferably within 2 degrees.

[0053] 3. Image display device Image display devices include liquid crystal displays, organic EL displays, QLED displays, and other devices that contain polarizing plates inside.

[0054] 4.Liquid crystal display device Generally, a liquid crystal panel consists of a rear module, liquid crystal cells, and a front module, arranged in the order from the side facing the backlight source to the side displaying the image (viewing side). The rear module and front module generally consist of a transparent substrate, a transparent conductive film formed on its surface facing the liquid crystal cells, and a polarizing plate positioned on the opposite side. In this case, the polarizing plate is positioned on the side facing the backlight source in the rear module, and on the side displaying the image (viewing side) in the front module.

[0055] A liquid crystal display device comprises at least a backlight source and a liquid crystal cell placed between two polarizing plates. It may also include other components as appropriate, such as a color filter, lens film, diffusion sheet, and anti-reflective film.

[0056] The arrangement of the polarizer protective film of the present invention having a specific polyester film is not particularly limited, but in the case of a liquid crystal display device in which a polarizer plate arranged on the incident light side (light source side), a liquid crystal cell, and a polarizer plate arranged on the output light side (viewing side) are arranged, it is preferable that the polarizer protective film on the incident light side of the polarizer plate arranged on the incident light side and / or the polarizer protective film on the output light side of the polarizer plate arranged on the output light side are the polarizer protective film of the present invention having the specific polyester film. A particularly preferred embodiment is in which the polarizer protective film on the incident light side of the polarizer plate arranged on the incident light side is the specific polyester film. If the polyester film is arranged in a position other than those mentioned above, it may change the polarization characteristics of the liquid crystal cell. Since it is not preferable to use the polarizer protective film of the present invention in a location where polarization characteristics are required, it is preferable to use it as a protective film for polarizer plates in such specific positions.

[0057] The backlight configuration can be either an edge-lit system, which uses light guide plates and reflectors as components, or a direct-lit system.

[0058] It is preferable to use a white light-emitting diode (white LED) as the backlight source for a liquid crystal display device. In this invention, a white LED refers to a phosphor-type element, that is, an element that emits white light by combining a light-emitting diode that emits blue light or ultraviolet light using a compound semiconductor with a phosphor. Examples of phosphors include yttrium-aluminum-garnet-based yellow phosphors and terbium-aluminum-garnet-based yellow phosphors. In particular, a white light-emitting diode consisting of a light-emitting element combining a blue light-emitting diode using a compound semiconductor and a yttrium-aluminum-garnet-based yellow phosphor has a continuous and broad emission spectrum and excellent luminous efficiency. Here, a continuous emission spectrum means that there is no wavelength at which the light intensity is zero, at least in the visible light region. Furthermore, since the method of this invention makes it possible to widely use white LEDs with low power consumption, it is also possible to achieve energy saving effects.

[0059] Furthermore, as a backlight light source, a white light source having peaks in the emission spectrum in each wavelength region of 400nm to less than 495nm (B region), 495nm to less than 600nm (G region), and 600nm to 780nm (R region) is also preferred. For example, a white light source utilizing quantum dot technology, a phosphor-type white LED light source using a phosphor with emission peaks in the R (red) and G (green) regions respectively depending on the excitation light and a blue LED, a three-wavelength white LED light source, a white LED light source combining a red laser, and others, for example, a material with the composition formula K2SiF6:Mn 4+Examples include white LED light sources using fluoride phosphors (also known as "KSF") and blue LEDs. These white light sources are attracting attention as backlight light sources for wide-color-gamut liquid crystal display devices, and all of them have a narrower peak full width at half maximum compared to light sources consisting of white light-emitting diodes made of light-emitting elements combining blue light-emitting diodes and yttrium-aluminum-garnet-based yellow phosphors, which have been used conventionally. When using backlight light sources consisting of these white light sources, there was a problem that iridescence tended to occur more easily when a retarded polyester film was used as a polarizer protective film, which is a component of the polarizer plate, compared to the case of a backlight light source consisting of white light-emitting diodes made of light-emitting elements combining blue light-emitting diodes and yttrium-aluminum-garnet-based yellow phosphors. However, with the polarizer protective film of the present invention, iridescence can be significantly suppressed.

[0060] 5. Organic EL displays and QLED displays Organic EL elements can be appropriately selected and used from organic EL elements known in the art. The use of organic EL elements is preferred in terms of wide viewing angle, high contrast, and fast response. Organic EL elements are typically light-emitting bodies (organic electroluminescent light-emitting bodies) having a structure in which a transparent electrode anode, an organic light-emitting layer, and a metallic electrode cathode are stacked in this order on a transparent substrate. Organic EL cells emit light when a voltage is applied between the anode and the cathode, by the recombination of holes (positive ions) injected from the anode and electrons injected from the cathode in the organic light-emitting layer.

[0061] Any transparent substrate can be used as the transparent substrate. For example, the transparent substrate can be selected from the group consisting of glass substrates, ceramic substrates, semiconductor substrates, metal substrates, and plastic substrates. A specific example of a plastic substrate is a conventionally used transparent resin film. The transparent substrate may be provided with a surface treatment layer as needed. Examples of surface treatment layers include a moisture-proof layer, a gas barrier layer, a hard coat layer, and an undercoat layer.

[0062] Materials constituting the anode and cathode include metals, metal oxides, alloys, electrically conductive compounds, and mixtures thereof. More specific materials for the anode include conductive transparent materials such as gold, silver, chromium, nickel, copper iodide, indium tin oxide (ITO), tin oxide, and zinc oxide. More specific materials for the cathode include magnesium, aluminum, indium, lithium, sodium, cesium, silver, magnesium-silver alloys, magnesium-indium alloys, and lithium-aluminum alloys.

[0063] The thicknesses of the anode and cathode can be arbitrarily set depending on the materials constituting the anode and cathode. For example, the thickness of the anode can be appropriately set from the range of 10 nm to 200 nm, preferably from 10 nm to 100 nm. The thickness of the cathode can be appropriately set from the range of 10 nm to 1000 nm, preferably from 10 nm to 200 nm.

[0064] The organic light-emitting layer is a layer that, when a voltage is applied, provides a field for the recombination of holes and electrons, thereby causing it to emit light. The organic light-emitting layer contains an organic light-emitting material and may be a single-layer structure or a multilayer structure of two or more layers. In the case of a multilayer structure, each layer may emit light in a different color. The thickness of the organic light-emitting layer is arbitrary and can be appropriately set, for example, in the range of 3 nm to 3 μm.

[0065] The organic light-emitting material used in the organic light-emitting layer can be appropriately selected from any available light-emitting material. Specifically, olefin-based light-emitting materials such as 4,4'-(2,2-diphenylvinyl)biphenyl; 9,10-di(2-naphthyl)anthracene, 9,10-bis(3,5-diphenylphenyl)anthracene, 9,10-bis(9,9-dimethylfluorenyl)anthracene, 9,10-(4-(2,2-diphenylvinyl)phenyl)anthracene, 9,10'-bis(2-biphenylyl)-9,9'-bisanthracene, 9,10,9',10'-te An appropriate selection can be made from the group consisting of anthracene-based luminescent materials such as traphenyl-2,2'-bianthryl and 1,4-bis(9-phenyl-10-anthracene)benzene; spiro-based luminescent materials such as 2,7,2',7'-tetrakis(2,2-diphenylvinyl)spirobifluorene; carbazole-based luminescent materials such as 4,4'-dicarbazolbiphenyl and 1,3-dicarbazolylbenzene; and pyrene-based luminescent materials such as 1,3,5-tripyrenebenzene.

[0066] The organic EL element may include a sealing member formed to cover the organic EL element, which is composed of an anode, an organic light-emitting layer, and a cathode on the substrate, in order to isolate the organic EL element from the outside air. By including a sealing member, it is possible to prevent deterioration of the light-emitting properties of the organic light-emitting layer due to moisture and oxygen in the outside air.

[0067] The organic EL element may further include any additional components (e.g., hole injection layer, hole transport layer, electron injection layer, and / or electron transport layer) at any suitable location.

[0068] When using an organic EL cell as an image display cell, it is preferable to have a polarizer on the viewing side. Because the thickness of the organic light-emitting layer is thin, about 10 nm, ambient light is reflected by the metal electrodes and emitted again to the viewing side, and when viewed from the outside, the display surface of the organic EL display device may appear mirror-like. To block such specular reflection of ambient light, it is preferable to provide a polarizer on the viewing side of the organic EL cell, and further to provide a quarter-wave plate between the organic EL cell and the polarizer. As the polarizer, the aforementioned polarizer can be used, and it is preferable that a polarizer protective film made of the polyester film of the present invention is laminated on the viewing side of the polarizer. Alternatively, it is also preferable to laminate a quarter-wave plate onto the polarizer instead of the protective film on the organic EL element side of the polarizer. By configuring a circular polarizer with these combinations of the viewing-side polarizer and the quarter-wave plate, ambient light specularly reflected by the metal electrodes of the organic EL cell is blocked by the circular polarizer, thus suppressing a decrease in the visibility of the image display device. A half-wave plate or the like may be further laminated on the organic EL element side or the polarizer side of the quarter-wave plate. Preferably, a half-wave plate or the like is laminated on the organic EL element side of the quarter-wave plate with an inclination relative to each other's optical axes, as disclosed in Japanese Patent Application Publication No. 10-68816 and Japanese Patent Application Publication No. 2017-97379.

[0069] Furthermore, QLED displays are similar to organic EL displays in that they utilize the fact that quantum dots emit light themselves when electricity is applied, and are attracting attention as next-generation displays. [Examples]

[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited by the following examples, and can be implemented with appropriate modifications within the scope that is consistent with the spirit of the present invention, and all such modifications are included within the technical scope of the present invention. The method for evaluating the physical properties in the following examples is as follows.

[0071] (1) Evaluation of the slow axis direction of the film The slow phase axis direction of the film was evaluated using a molecular orientation meter (MOA-6004 molecular orientation meter, manufactured by Oji Instruments Co., Ltd.).

[0072] (2) ΔNxy and retardation (Re) Retardation is a parameter defined by the product of the anisotropy of the refractive indices of two orthogonal axes on a film (△Nxy=|nx-ny|) and the film thickness d (nm) (△Nxy×d), and is a measure of optical isotropy and anisotropy. The anisotropy of the refractive indices of the two axes (△Nxy) was determined by the following method: Using a molecular orientation meter (MOA-6004 molecular orientation meter manufactured by Oji Instruments Co., Ltd.), the axis direction of the slow phase was determined, and a rectangle measuring 4cm × 2cm was cut out so that the axis direction of the slow phase was parallel to the long side of the measurement sample, and this was used as the measurement sample. For this sample, the refractive indices in two orthogonal axes (refractive index in the slow axis direction: nx, refractive index in the direction perpendicular to the slow axis direction in the plane (i.e., refractive index in the fast axis direction): ny) and the refractive index in the thickness direction (nz) were determined using an Abbe refractometer (ATAGO, NAR-4T, measurement wavelength 589 nm). The absolute value of the difference in refractive index between the two axes (|nx-ny|) was defined as the refractive index anisotropy (△Nxy). The film thickness d (nm) was measured using an electric micrometer (Fineleuf, Millitron 1245D), and the unit was converted to nm. The retardation (Re) was determined from the product of the refractive index anisotropy (△Nxy) and the film thickness d (nm) (△Nxy × d).

[0073] (3) NZ coefficient The NZ coefficient was obtained by substituting the values ​​of nx, ny, and nz measured by the Abbe refractometer in (2) into |nx-nz| / |nx-ny|.

[0074] (4) Elastic modulus The modulus of elasticity of the polyester film was evaluated using a dynamic viscoelasticity analyzer (DMS6100) manufactured by Seiko Instruments Corporation, in accordance with JIS-K7244 (DMS), after standing for 168 hours in an environment of 25°C and 50% RH. The temperature dependence from 25°C to 120°C was measured under the conditions of tensile mode, drive frequency of 1 Hz, chuck distance of 5 mm, and heating rate of 2°C / min, and the average of the storage modulus from 30°C to 100°C was defined as the modulus of elasticity. Measurements were performed in the MD direction.

[0075] (5-1) Observation of iridescence (using a liquid crystal display device) A roll of polarizer made of iodine and polyvinyl alcohol film, manufactured by uniaxial stretching in the MD direction, and PET film rolls of polarizer protective films 1 to 9 (described later) were laminated roll-to-roll so that their MD directions were parallel to each other. A roll of TAC film (manufactured by Fujifilm Corporation, 40 μm thick) was similarly laminated roll-to-roll to the other side of the polarizer, creating a polarizing plate consisting of PET film / polarizer / TAC film. The resulting polarizing plates were installed on the incident and exit sides of a liquid crystal display device using a white LED (Nichia Corporation, NSPW500CS) as the light source, which consisted of a blue light-emitting diode and a yttrium-aluminum-garnet-based yellow phosphor. The polarizing plate on the incident side was installed with the polyester film facing the light source, and the polarizing plate on the exit side was installed with the polyester film facing the viewer. The polarizing plates of the liquid crystal display device were visually observed from the front and oblique directions, and the presence or absence of iridescence was determined as follows.

[0076] ○: No iridescence is observed from any direction. △: When observed from an oblique angle, faint iridescence can be observed depending on the angle. ×: When observed from an oblique angle, the iridescence is clearly visible.

[0077] (5-2) Observation of iridescence (organic EL display) A roll of polarizer made of iodine and polyvinyl alcohol film, manufactured by uniaxial stretching in the MD direction, and PET film rolls of polarizer protective films 1 to 9 (described later) were laminated roll-to-roll so that their MD directions were parallel to each other. A roll of quarter-wave plate was similarly laminated roll-to-roll to the other side of the polarizer, creating a polarizer consisting of PET film / polarizer / (quarter-wave plate). A circular polarizer (a circular polarizer positioned on the viewing side of the OLED element) was removed from a commercially available organic EL display (LG C6P 55-inch organic EL TV), and the polarizer obtained above was placed inside the organic EL display so that the PET film was positioned on the viewing side. The organic EL display was visually observed from the front and oblique directions, and the presence or absence of iridescence was determined as follows.

[0078] ○: No iridescence is observed from any direction. △: When observed from an oblique angle, faint iridescence can be observed depending on the angle. ×: When observed from an oblique angle, the iridescence is clearly visible.

[0079] (6) Evaluation of LCD panel warping A roll of polarizer made of iodine and polyvinyl alcohol film, manufactured by uniaxial stretching in the MD direction, and a roll of PET film for the polarizer protective film described later were laminated together roll-to-roll so that their MD directions were parallel to each other. A roll of TAC film (manufactured by Fujifilm Corporation, 40 μm thick) was similarly laminated to the other side of the polarizer using the roll-to-roll method to create a polarizing plate consisting of PET film / polarizer / TAC film. Next, two polarizing plates of the same size were laminated to both sides of a glass plate measuring 125 mm wide, 220 mm long, and 0.4 mm thick using PSA in a cross-nicol relationship (one polarizing plate having its absorption axis parallel to the width direction, and the other polarizing plate having its absorption axis parallel to the length direction). At this time, polarizers with the same shrinkage force were used for the upper and lower polarizing plates. The polarizer protective film of the present invention was laminated so that it was positioned on the outside. Next, the material was heat-treated for 30 minutes using a gear oven set to 100°C. After that, it was cooled for 10 minutes in an environment set to room temperature of 25°C. The height of each of the four corners was then measured with a tape measure, and the maximum value was recorded. A measurement of 5 mm or less was considered within the acceptable range.

[0080] (7) Tear strength Using a Shimadzu Autograph (AG-X plus), the tear strength per unit thickness (N / mm) was measured for each film according to the right-angle tear method (JIS K-7128-3). Tear strength was measured in two directions (i.e., the direction of the slow phase axis and the direction of the fast phase axis) with respect to the orientation principal axis (slow phase axis) of the film, and the smaller value was recorded as the tear strength in Table 1. The measurement in the orientation principal axis direction (slow phase axis direction) was performed using a molecular orientation meter (MOA-6004 molecular orientation meter, manufactured by Oji Keisokuki Co., Ltd.).

[0081] (8) Film forming properties The starting point was set one hour after the start of film formation. The number of fractures per hour from that point was compared, and the film-forming ability was determined as follows.

[0082] ○: Less than 3 fractures △: Number of fractures is 3 or more but less than 6 ×: Number of fractures is 6 or more.

[0083] (9) Method of evaluating scratches The film was inspected using a defect inspection device one hour after the start of film formation, and the number of defects with a maximum height Sz of 0.6 μm or more, measured with a laser microscope (Olympus Corporation, OLS4100), was determined as follows.

[0084] ○: Number of scratches is 3 per meter 2 less than △: Number of scratches: 3 / m 2 More than 6 pieces / m 2 less than ×: Number of scratches: 6 / m 2 That's all.

[0085] (Manufacturing Example 1 - Polyester A) The esterification reaction vessel was heated to 200°C, at which point 86.4 parts by mass of terephthalic acid and 64.6 parts by mass of ethylene glycol were charged. While stirring, 0.017 parts by mass of antimony trioxide, 0.064 parts by mass of magnesium acetate tetrahydrate, and 0.16 parts by mass of triethylamine were charged as catalysts. Next, the mixture was heated under pressure and the esterification reaction was carried out at a gauge pressure of 0.34 MPa and 240°C. After that, the esterification reaction vessel was returned to atmospheric pressure and 0.014 parts by mass of phosphoric acid was added. Furthermore, the temperature was raised to 260°C over 15 minutes, and 0.012 parts by mass of trimethyl phosphate was added. After 15 minutes, the mixture was dispersed using a high-pressure disperser, and after 15 minutes, the obtained esterification reaction product was transferred to a polycondensation reaction vessel and a polycondensation reaction was carried out under reduced pressure at 280°C.

[0086] After the polycondensation reaction was complete, the mixture was filtered through a Naslon filter with a 95% cut diameter of 5 μm. It was then extruded from a nozzle in strand form, cooled and solidified using pre-filtered cooling water (pore size: 1 μm or less), and cut into pellets. The resulting polyethylene terephthalate resin (A) had an intrinsic viscosity of 0.62 dl / g and contained virtually no inert particles or internally precipitated particles. (Hereafter abbreviated as PET(A).)

[0087] (Manufacturing Example 2 - Polyester B) Ten parts by mass of a dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazinon-4-one) and 90 parts by mass of particle-free PET(A) (with an intrinsic viscosity of 0.62 dl / g) were mixed, and polyethylene terephthalate resin (B) containing the ultraviolet absorber was obtained using a kneading extruder. (Hereafter, this will be abbreviated as PET(B).)

[0088] (Manufacturing Example 3 - Preparation of Adhesion Modifying Coating Solution) A water-dispersible sulfonic acid metal base-containing copolymer polyester resin was prepared by conventional transesterification and polycondensation reactions to obtain a water-dispersible sulfonic acid metal base-containing copolymer polyester resin with the following composition: dicarboxylic acid components (relative to the total dicarboxylic acid components) consisting of 46 mol% terephthalic acid, 46 mol% isophthalic acid, and 8 mol% sodium 5-sulfonaisophthalate; and glycol components (relative to the total glycol components) consisting of 50 mol% ethylene glycol and 50 mol% neopentyl glycol. Next, 51.4 parts by mass of water, 38 parts by mass of isopropyl alcohol, 5 parts by mass of n-butyl cellsolve, and 0.06 parts by mass of a nonionic surfactant were mixed, and the mixture was heated and stirred until it reached 77°C. Then, 5 parts by mass of the above water-dispersible sulfonic acid metal base-containing copolymer polyester resin was added, and stirring continued until there were no more clumps of resin. After that, the resin aqueous dispersion was cooled to room temperature to obtain a uniform water-dispersible copolymer polyester resin liquid with a solid content concentration of 5.0% by mass. Furthermore, 3 parts by mass of aggregated silica particles (Silysia 310, manufactured by Fuji Silysia Co., Ltd.) were dispersed in 50 parts by mass of water. Then, 0.54 parts by mass of the aqueous dispersion of Silysia 310 was added to 99.46 parts by mass of the above-mentioned water-dispersible copolymer polyester resin liquid, and 20 parts by mass of water was added while stirring to obtain an adhesive modification coating solution.

[0089] (Polarizer protective film 1) As raw materials for the intermediate layer of the base film, 90 parts by mass of PET (A) resin pellets containing no particles and 10 parts by mass of PET (B) resin pellets containing an ultraviolet absorber were dried under reduced pressure (1 Torr) at 135°C for 6 hours, and then supplied to Extruder 2 (for Intermediate Layer II). Also, PET (A) was dried by a conventional method and supplied to Extruder 1 (for Outer Layer I and Outer Layer III) respectively, and melted at 285°C. These two kinds of polymers were each filtered through a stainless-steel sintered filter medium (nominal filtration accuracy: 95% cut-off for 10-μm particles), laminated in a two-kind three-layer confluence block, extruded into a sheet shape from a die, and then wound around a casting drum with a surface temperature of 30°C using the electrostatic application casting method and cooled and solidified to produce an unstretched film. At this time, the discharge amounts of each extruder were adjusted so that the thickness ratio of Layer I, Layer II, and Layer III was 10:80:10.

[0090] Next, by the reverse roll method, the above-mentioned adhesive-modified coating solution was applied to both sides of this unstretched PET film so that the coating amount after drying was 0.08 g / m 2 and then dried at 80°C for 20 seconds.

[0091] The unstretched film with this coating layer formed was led into a simultaneous biaxial stretching machine, led into a hot air zone at a temperature of 125°C while gripping the ends of the film with clips, and stretched 6.5 times in the running direction and 2.2 times in the width direction. Next, while maintaining the width stretched in the width direction, it was treated at a temperature of 225°C for 30 seconds to obtain a biaxially oriented PET film with a film thickness of about 40 μm. This was wound into a roll shape to form a film roll (a film roll with a film length of 500 m in the MD direction). The slow axis of the obtained film was within 3° from the running direction. This was used as Polarizer Protection Film 1.

[0092] (Polarizer Protection Film 2) A biaxially oriented PET film with a film thickness of approximately 40 μm was obtained in the same manner as polarizer protective film 1, except that the thickness of the unstretched film was changed and stretched 6.0 times in the running direction and 2.2 times in the width direction. This was wound into a roll to form a film roll (a film roll with a length of 500 m in the MD direction). The slow axis of the obtained film was within 3° from the running direction. This was designated as polarizer protective film 2.

[0093] (Polarizer protective film 3) Similar to polarizer protective film 1, an unstretched film was prepared and heated to 105°C using a sequential biaxial stretcher with heated rolls and an infrared heater. It was then stretched 6.5 times in the running direction using rolls with different peripheral speeds, and then guided into a hot air zone at 125°C to stretch 2.2 times in the width direction. Next, while maintaining the width stretched in the width direction, it was processed at 225°C for 30 seconds to obtain a biaxially oriented PET film with a film thickness of approximately 40 μm. This was wound into a roll to form a film roll (a film roll with a length of 500 m in the MD direction). The slow axis of the obtained film was within 5° from the running direction. This was designated as polarizer protective film 3.

[0094] (Polarizer protective film 4) A uniaxially oriented PET film with a thickness of approximately 40 μm was obtained in the same manner as polarizer protection film 1, except that the thickness of the unstretched film was changed and stretched 1.0 times in the running direction and 4.0 times in the width direction. This was wound into a roll to form a film roll. The slow axis of the obtained film was within 4° from the width direction. This was designated as polarizer protection film 4. Because the slow axis of polarizer protection film 4 is in the width direction, when observed from an oblique direction, faint rainbow-like color spots were observed depending on the angle. In addition, it had low tear strength and tore easily. For example, when polarizer protection film 4 was laminated with a polarizer and a polarizer plate was manufactured using a roll-to-roll method, it cracked more often in the width direction than other films.

[0095] (Polarizer protective film 5) The thickness of the unstretched film was changed, and it was heated to 105°C using a heated roll group and an infrared heater. Then, it was stretched 4.0 times in the running direction using a roll group with different peripheral speeds, and then guided into a hot air zone at 125°C and stretched to 1.0 times in the width direction. Next, while maintaining the width stretched in the width direction, it was processed at 225°C for 30 seconds to obtain a uniaxially oriented PET film with a film thickness of approximately 40 μm. This was wound into a roll to form a film roll. The slow axis of the obtained film was within 8° from the running direction. This was designated as polarizer protective film 5. Although no iridescent color spots were observed in polarizer protective film 5, it had low tear strength and tore easily.

[0096] (Polarizer protective film 6) A biaxially oriented PET film with a film thickness of approximately 40 μm was obtained in the same manner as polarizer protective film 1, except that the thickness of the unstretched film was changed and stretched 4.5 times in the running direction and 2.4 times in the width direction. This was wound into a roll to form a film roll (a film roll with a length of 500 m in the MD direction). The slow axis of the obtained film was within 8° from the running direction. Because the obtained film had a low ΔNxy, iridescent color spots were observed when viewed from an oblique direction.

[0097] (Polarizer protective film 7) The thickness of the unstretched film was changed, and it was heated to 105°C using a sequential biaxial stretcher with heated rolls and an infrared heater. Then, it was stretched 2.2 times in the running direction using rolls with different peripheral speeds, and then guided into a hot air zone at 125°C to stretch 5.5 times in the width direction. Next, while maintaining the width stretched in the width direction, it was processed at 225°C for 30 seconds to obtain a biaxially oriented PET film with a film thickness of approximately 40 μm. This was wound into a roll to form a film roll (a film roll with a length of 500 m in the MD direction). The slow axis of the obtained film was within 6° from the width direction. Since the slow axis direction of the obtained film was in the width direction, iridescent color spots were observed when viewed from an oblique direction.

[0098] (Polarizer protective film 8) A biaxially oriented PET film with a film thickness of approximately 40 μm was obtained in the same manner as polarizer protective film 1, except that the thickness of the unstretched film was changed and stretched 6.0 times in the running direction and 1.5 times in the width direction. This was wound into a roll to form a film roll (a film roll with a length of 500 m in the MD direction). The slow axis of the obtained film was within 3° from the running direction. This was designated as polarizer protective film 8.

[0099] (Polarizer protective film 9) A biaxially oriented PET film with a film thickness of approximately 40 μm was obtained in the same manner as polarizer protective film 1, except that the thickness of the unstretched film was changed and stretched 6.5 times in the running direction and 2.7 times in the width direction. This was wound into a roll to form a film roll (a film roll with a length of 500 m in the MD direction). The slow axis of the obtained film was within 3° from the running direction. This was designated as polarizer protective film 9.

[0100] The results of observing iridescence and measuring tear strength for polarizer protective films 1-9 are shown in Table 1 below.

[0101] [Table 1]

[0102] As shown in Table 1, when iridescence was observed using polarizer protective films 1-3, 5, 8, and 9, no iridescence was observed when observed from the front or oblique direction. On the other hand, with polarizer protective film 4, a faint iridescence was observed in some areas when observed from an oblique direction. Furthermore, although no iridescence was observed with polarizer protective film 5, its tear strength was low and the film formation was unstable. Also, clear iridescence was observed with polarizer protective films 6 and 7 when observed from an oblique direction. In addition, when a liquid crystal display device was manufactured in the same manner as in the above item (5-1) iridescence observation, except that a polarizer consisting of a PET film / polarizer with only a PET film laminated on the polarizer without a TAC film laminated on it was used, and iridescence observation was performed in the same manner, the same results as the iridescence observation results shown in Table 1 were obtained. Furthermore, when the warpage of the liquid crystal panel was evaluated using the method described in (6) above with polarizer protective films 1-3, 5, 8, and 9, the measured values ​​were 5 mm or less, and all were good results. [Industrial applicability]

[0103] By using the polarizer protective film, polarizer plate, and image display device (such as a liquid crystal display device or an organic EL display) of the present invention, it becomes possible to contribute to the thinning and cost reduction of LCDs without reducing visibility due to rainbow-like color spots, and thus the industrial applicability is extremely high.

Claims

1. A polarizer protective film comprising a polyester film, The slow axis direction of the polyester film is approximately parallel to the MD direction, The in-plane birefringence ΔNxy of the polyester film is 0.06 or more and 0.20 or less, Further, a polarizer protective film that satisfies the following (A) or (B): (A) the refractive index of the polyester film in the fast axis direction is 1.580 or more and 1.630 or less; (B) The smaller of the tear strengths measured in the slow axis direction and the fast axis direction of the polyester film by a perpendicular tear method is 250 N / mm or more.

2. A polarizer protective film as described in claim 1, wherein the NZ coefficient of the polyester film is 1.5 or more and 2.5 or less.

3. A polarizer protective film as described in claim 1 or 2, wherein the retardation of the polyester film is 1,500 nm or more and 30,000 nm or less.

4. A polarizer protective film described in any one of claims 1 to 3, wherein the thickness of the polyester film is 15 to 60 μm.

5. A polarizer protective film described in any one of claims 1 to 4, wherein the angle between the slow axis direction of the polyester film and the MD direction is within 3 degrees.

6. A polarizer protective film described in any one of claims 1 to 5, wherein the elastic modulus in the MD direction of the polyester film is 3000 MPa or more.

7. A polarizing plate having a polarizer protective film described in any one of claims 1 to 6 laminated on at least one surface of a polarizer.

8. A polarizing plate having a polarizer protective film described in any one of claims 1 to 6 laminated on one side of a polarizer, and no film laminated on the other side of the polarizer.

9. A polarizing plate having a polarizer protective film described in any one of claims 1 to 6 laminated on one side of a polarizer and a quarter-wave plate laminated on the other side of the polarizer.

10. An image display device comprising the polarizing plate according to claim 7.

11. A liquid crystal display device comprising a polarizing plate according to claim 7 or 8.

12. An organic electroluminescence display comprising the polarizing plate according to claim 7.

13. A QLED display comprising a polarizing plate according to any one of claims 7 to 9.