Three-way conversion catalyst compositions containing platinum-rhodium bimetallic components
Patent Information
- Application Number
- JP2023521719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-09
- Filing Date
- 2021-09-23
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional three-way conversion (TWC) catalysts face challenges with platinum group metal (PGM) stability and cold start performance, particularly due to the use of palladium, which is expensive and has lower thermal stability compared to platinum, necessitating a more cost-effective and thermally stable catalyst solution.
A catalyst composition comprising platinum, rhodium, and a ceria-alumina or zirconia composite support, with specific mass ratios, to enhance the synergistic effect and improve CO, NO, and HC conversion rates, while maintaining thermal stability.
The proposed catalyst composition significantly improves cold start performance and conversion efficiency of CO, NO, and HC, offering a cost-effective alternative to traditional TWC catalysts by leveraging the synergistic effect of platinum and rhodium on ceria-alumina or zirconia composites.
Abstract
Description
Technical Field
[0001] Field of the Invention The invention described in the claims relates to a catalyst composition useful for treating exhaust gas and reducing pollutants contained therein. In particular, the invention described in the claims relates to a catalyst composition suitable for a three-way conversion catalyst and a catalyst article containing the catalyst composition.
Background Art
[0002] Background of the Invention Three-way conversion (TWC) catalysts are well known for having catalytic activity to reduce pollutants such as NO, CO, and HC using platinum group metals. Conventional TWC catalysts use Pd and Rh as catalytic active components. Considering the current PGM market price, replacing a part of the more expensive Pd with the cheaper Pt in the TWC catalyst will help significantly reduce costs for catalyst product manufacturers and automobile manufacturers. However, since platinum has lower thermal stability than palladium, it becomes a major problem in TWC applications that must withstand severe changes over time. Therefore, it is desired to provide a TWC catalyst that can not only solve the problems related to the stability of PGM but also improve cold start performance.
Summary of the Invention
Problems to be Solved by the Invention
[0003] An object of the present invention is to provide a catalyst capable of realizing an improvement in cold start performance.
[0004] The present invention solves the cold start problem by providing a TWC catalyst based on a platinum-rhodium bimetal component that exhibits a synergistic effect between Pt and Rh by selecting an appropriate carrier material. This synergistic effect significantly improves the conversion of CO, NO, and HC compared to the individual metals (Pt, Rh).
Means for Solving the Problems
[0005] Summary of the Invention The invention described in these claims is as follows: a) Platinum, b) Rhodium, c) Ceria-alumina composite, zirconia composite, or mixture thereof Includes, Here, platinum is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, rhodium is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, the amount of CeO2 in the ceria-alumina composite is 1.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. A catalyst composition is provided.
[0006] Furthermore, the present invention provides a method for producing a catalyst composition. Moreover, the present invention provides a catalyst article comprising a catalyst composition according to the claims described herein deposited on a substrate, and a method for producing the same. Furthermore, the present invention provides an exhaust gas treatment system for an internal combustion engine comprising a catalyst article according to the claims described herein. [Brief explanation of the drawing]
[0007] To aid in understanding embodiments of the present invention, refer to the accompanying drawings. However, the accompanying drawings are not necessarily drawn to an exact scale. Reference numerals indicate components of exemplary embodiments of the present invention. The drawings are illustrative only and should not be construed as limiting the present invention. The above-mentioned and other features, characteristics, and various advantages of the invention described in these claims will become more apparent when considered in conjunction with the accompanying drawings and the following detailed description. [Figure 1] This figure shows the light-off characteristics of a Pt-Rh catalyst supported on CeO2 / Al2O3 for the conversion rates of CO, NO, and HC. [Figure 2] This figure shows the light-off characteristics of a Pt-Rh catalyst supported on La2O3 / ZrO2 for the conversion rates of CO, NO, and HC. [Figure 3] This figure shows the light-off characteristics for CO, NO, and HC conversion rates of Pt-Rh catalysts supported on CeO2 / Al2O3 and La2O3 / ZrO2. [Figure 4] This figure shows the light-off characteristics of a Pt-Rh catalyst supported on Al2O3 for the conversion rates of CO, NO, and HC. [Figure 5] This figure shows the light-off characteristics of the Pt-Rh catalyst supported on OSC1 for the conversion rates of CO, NO, and HC. [Figure 6] This figure shows the light-off characteristics of the Pt-Rh catalyst supported on OSC2 for the conversion rates of CO, NO, and HC. [Figure 7] This figure shows the light-off characteristics of the Pt-Rh catalyst supported on OSC3 for the conversion rates of CO, NO, and HC. [Figure 8] This figure shows the light-off characteristics of a Pt-Rh catalyst supported on a support mixture, for the conversion rates of CO, NO, and HC. [Figure 9A] This is a perspective view of a honeycomb-type substrate carrier that may include a catalyst composition according to one embodiment of the invention described in these claims. [Figure 9B] This is an enlarged partial cross-sectional view of Figure 9A, which is a cross-sectional view cut along a plane parallel to the end face of the substrate carrier in Figure 9A, and shows an enlarged view of the multiple gas flow paths shown in Figure 9A. [Figure 10] This is an enlarged cross-sectional view of Figure 9A, where the honeycomb-shaped substrate in Figure 9A represents the wall flow filter substrate monolith. [Modes for carrying out the invention]
[0008] Detailed explanation The invention described in these claims will be described in detail below. However, the invention described in these claims can be embodied in many different forms and should not be construed as being limited to the embodiments described herein. Rather, these embodiments provide a thorough and complete understanding of the invention described in these claims and fully convey the scope of the invention to those skilled in the art. Nothing in this specification should be construed as indicating that non-claimed elements are essential for carrying out the disclosed materials and methods.
[0009] All methods described herein may be performed in any suitable order, unless otherwise specified herein or unless the context clearly contradicts it. The use of any specific examples or illustrative expressions (e.g., "etc.") described herein is intended solely to better illustrate the materials and methods and is not intended to limit their scope unless otherwise stated.
[0010] Definition: In relation to the descriptions of materials and methods discussed herein (particularly in connection with the claims), the use of the terms “a,” “an,” “the,” and similar references should be interpreted as encompassing both the singular and plural forms unless otherwise indicated herein or unless it is clearly inconsistent with the context.
[0011] The term "approximately" as used throughout this specification is used to express and describe small fluctuations. For example, the term "approximately" can refer to ±5%, such as ±2% or less, ±1% or less, ±0.5% or less, ±0.2% or less, ±0.1% or less, or ±0.05% or less. All numerical values used in this document, whether explicitly stated or not, are modified with the term "approximately." Of course, numerical values modified with the term "approximately" encompass their specifically identified value. For example, "approximately 5.0" must include 5.0.
[0012] In the context of the present invention, the term "first layer" is used interchangeably with "bottom layer" or "bottom coat" or "bottom wash coat", while the term "second layer" is used interchangeably with "top layer" or "top coat" or "top wash coat". The first layer is deposited on at least a part of the substrate, and the second layer is deposited on at least a part of the first layer.
[0013] The term "three-way conversion catalyst" refers to a catalyst that simultaneously promotes a) reducing nitrogen oxides to nitrogen and oxygen, b) oxidizing carbon monoxide to carbon dioxide, and c) oxidizing unburned hydrocarbons to carbon dioxide and water.
[0014] Also, the term "NOx" refers to nitrogen oxide compounds such as NO and / or NO2.
[0015] As used herein, the term "wash coat" has its ordinary meaning in the art and refers to a coating of a catalyst material or other material applied to a substrate material, which is thin and adherent. Generally, a wash coat is formed by preparing a slurry containing particles with a certain solid content (e.g., 15 - 60% by mass) in a liquid vehicle, applying this to the substrate, and drying it to provide a wash coat layer.
[0016] The term "oxygen storage component (OSC)" refers to a substance having multiple valence states that can actively react with a reducing agent such as carbon monoxide (CO) and / or hydrogen under reducing conditions and can also react with an oxidizing agent such as oxygen or nitrogen oxides under oxidizing conditions.
[0017] In this context, OSC refers to ceria - zirconia that can be optionally stabilized by rare earth elements such as at least lanthanum, yttrium, neodymium, and praseodymium.
[0018] In terms of functionality, the hydrothermal stability of a catalyst can be defined as maintaining sufficient catalytic function even after high-temperature aging. Specifically, in this context, hydrothermal stability means that after aging at a temperature in the range of 950°C to 1050°C using 10% water vapor for approximately 5 hours, the catalyst has a NOx watt-off temperature below 280°C and a hydrocarbon watt-off temperature below 290°C.
[0019] Platinum group metals, also known as "PGMs," include ruthenium, rhodium, palladium, osmium, iridium, and platinum. It is preferable to select platinum, rhodium, or mixtures thereof from the platinum group metals.
[0020] The term "flow," as used herein, broadly refers to a combination of fluid gases that may contain solid or liquid particulate matter.
[0021] In this specification, the terms “upstream” and “downstream” refer to the relative directions corresponding to the flow of engine exhaust gases from the engine to the tailpipe, with the engine being upstream and the tailpipe and pollution mitigation items such as filters and catalysts being downstream from the engine.
[0022] As used herein, the term "wash coat" has the common meaning in the art of a thin, adhesive coating of a catalyst material or other material applied to a substrate material. Generally, a wash coat is formed by preparing a slurry containing a certain amount of solid particles (e.g., 15-60% by mass) in a liquid vehicle, applying it to a substrate, and drying it to create a wash coat layer.
[0023] Catalyst composition according to the present invention: According to the present invention, a) Platinum, b) Rhodium, c) Ceria-alumina composite, zirconia composite, or mixture thereof Includes, Here, platinum is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, rhodium is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, the amount of CeO2 in the ceria-alumina composite is 1.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. A catalyst composition is provided.
[0024] The term "catalyst composition" refers to a composition comprising at least one catalytically active metal and at least one support, or carrier. The catalytically active metal is deposited on the carrier. The catalyst composition may also contain other components such as stabilizers, accelerators, and / or binders, which are also deposited on the carrier. The catalytically active metal is preferably selected from PGMs, more preferably from platinum, rhodium, or mixtures thereof.
[0025] The expressions "deposited" and "supported" are used interchangeably. The deposition of catalytically active metals onto a support can be carried out by various methods known to those skilled in the art. These methods include coating techniques, impregnation techniques such as induce wetness impregnation, precipitation techniques, and atomic deposition techniques such as chemical vapor deposition. In these techniques, a suitable precursor containing the catalytically active metal is brought into contact with the support, thereby chemically or physically bonding with the support. In this way, the precursor containing the catalytically active metal is deposited onto the support. Through interaction with the support, the precursor containing the catalytically active metal may transform into another species containing the catalytically active metal. Different treatment steps, such as chemical fixation and / or thermal fixation, can be performed to enhance the chemical or physical bonding between the deposited species and the support.
[0026] The term "thermal fixation" refers to the process of depositing catalytically active metals onto their respective supports, for example, via an induced wetness impregnation method, and then thermally calcining the resulting catalytically active metal / support mixture. In one embodiment, this mixture is calcined at 400-700°C for 1.0-3.0 hours at a ramp rate of 1-25°C / min.
[0027] "Chemical fixation" refers to the process of depositing catalytically active metals onto their respective supports, and then, depending on the properties of the metal precursor, fixing them using additional reagents such as barium hydroxide or acetic acid, thereby chemically bonding the precursor to the support material. As a result, the catalytically active metals are chemically fixed as insoluble components into the pores of the support and onto the support surface.
[0028] The term "inducient wetness impregnation," also known as capillary impregnation or dry impregnation, refers to a process in which a precursor of a catalytically active metal is dissolved in an aqueous or organic solution, and the resulting solution containing the catalytically active metal is added to a carrier. This solution is drawn into the pores of the carrier by capillary action. The resulting composition can then be dried and calcined to remove volatile components from the solution, allowing the metal to be deposited on the surface of the carrier.
[0029] The term "support" refers to a solid material on which catalytically active metals(s) are deposited. The support may be inert or may participate in the catalytic reaction. Preferably, the support has a high BET surface area that is maintained under reaction conditions and is mechanically stable. "BET surface area" has its usual meaning and refers to the surface area determined by the Brunauer, Emmett, and Teller methods, which are determined by N2 adsorption.
[0030] The support of the present invention is a ceria-alumina composite, a zirconia composite, or a mixture of a ceria-alumina composite and a zirconia composite. The total amount of the ceria-alumina composite and the zirconia composite is 10 to 90% by mass based on the total mass of the catalyst composition.
[0031] Ceria-alumina composite: Ceria-alumina composites, also known as ceria-doped alumina, are composites in which CeO2 is distributed as particles, nanoclusters, or monatoms on the surface or within the bulk of alumina. In one embodiment, the composite is a mixed oxide, where each oxide has a different chemical and physical state, but the oxides can interact through their interfaces. CeO2 can be present on the alumina surface or bulk in any physical state, or in combinations of various states. Surface CeO2 modification of alumina can take the form of discontinuous portions (multiple particles or clusters), or this modification can form a layer of ceria that partially or completely covers the surface of the alumina.
[0032] The amount of CeO2 (cerium oxide) in the ceria-alumina composite is 1.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Preferably, the amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Furthermore, it is more preferable that the amount of CeO2 in the ceria-alumina composite is 10 to 40% by mass, based on the total mass of the ceria-alumina composite. Even more preferably, the amount of CeO2 in the ceria-alumina composite is 10 to 30% by mass, based on the total mass of the ceria-alumina composite. Even more preferably, the amount of CeO2 in the ceria-alumina composite is 15 to 35% by mass, based on the total mass of the ceria-alumina composite. Even more preferably, the amount of CeO2 in the ceria-alumina composite is 20 to 30% by mass, based on the total mass of the ceria-alumina composite.
[0033] The amount of Al2O3 (aluminum oxide) in the ceria-alumina composite is 50 to 99% by mass, based on the total mass of the ceria-alumina composite. Preferably, the amount of Al2O3 in the ceria-alumina composite is 50 to 95% by mass, based on the total mass of the ceria-alumina composite. More preferably, the amount of Al2O3 in the ceria-alumina composite is 70 to 90% by mass, based on the total mass of the ceria-alumina composite.
[0034] The average particle size of ceria in the ceria-alumina composite is less than 50 nm, as measured by a transmission electron microscope. Preferably, the average particle size of ceria in the ceria-alumina composite is less than 20 nm. More preferably, the particle size is in the range of 5 nm to 20 nm. The particle size is measured by a transition electron microscope.
[0035] The ceria-alumina composite further comprises a dopant selected from zirconia, lantana, titania, hafnia, magnesia, calcia, strontian, barrier, or a combination thereof. The dopant is incorporated into the lattice structure of the ceria-alumina composite. The total amount of dopants in the ceria-alumina is preferably in the range of 0.001 to 15% by mass based on the total mass of the ceria-alumina composite. More preferably, the total amount of dopants in the ceria-alumina is in the range of 0.01 to 10% by mass based on the total mass of the ceria-alumina composite. Furthermore, it is even more preferable that the total amount of dopants in the ceria-alumina is in the range of 0.01 to 5.0% by mass based on the total mass of the ceria-alumina composite.
[0036] Ceria-alumina composites can be produced by methods known to those skilled in the art, such as coprecipitation or surface modification. These methods involve contacting a suitable cerium-containing precursor with a suitable aluminum-containing precursor to convert the resulting mixture into a ceria-alumina composite. Suitable cerium-containing precursors include, for example, water-soluble cerium salts and colloidal ceria suspensions. Ceria-alumina can also be produced by atomic layer deposition, in which a ceria compound selectively reacts with the alumina surface, forming ceria on the alumina surface after calcination. This deposition / calcination process can be repeated until a layer of the desired thickness is reached. Suitable aluminum-containing precursors include, for example, aluminum oxides such as gamma-alumina, delta-alumina, or theta-alumina, or combinations thereof. The resulting mixture can be converted into a ceria-alumina composite by a calcination process.
[0037] Zirconia composite: The zirconia composite is a ZrO2-containing solid solution and can form a single phase as detected by XRD. The amount of ZrO2 (zirconium oxide) in the zirconia composite is 50 to 99% by mass based on the total mass of the zirconia composite. The zirconia composite preferably contains one or more rare earth metals in their oxide form. The rare earth metals are incorporated into the lattice structure of the zirconia composite in their oxide form. The rare earth metals are preferably selected from lanthanum, praseodymium, yttrium, neodymium, and mixtures thereof. The amount of rare earth metals in oxide form in the zirconia composite is preferably 1.0 to 15% by mass based on the total mass of the zirconia composite. The amount of rare earth metals in oxide form in the zirconia composite is more preferably 5.0 to 15% by mass based on the total mass of the zirconia composite. Some ZrO2 composites doped with rare earth composites undergo slight phase separation after high-temperature (>1000°C) aging.
[0038] The zirconia composite most preferably contains 85-99% by mass of ZrO2 and 1.0-15% by mass of La2O3, based on the total mass of the zirconia composite. Furthermore, the amount of CeO2 in the zirconia composite is preferably less than 0.001% by mass, based on the total mass of the zirconia composite.
[0039] The zirconia composite may contain other dopants selected from alumina, titania, hafnia, magnesia, calcia, strontian, barrier, or combinations thereof. The total amount of dopants in the zirconia is preferably in the range of 0.001 to 15% by mass based on the total mass of the zirconia composite.
[0040] Zirconia composites can be manufactured by methods known to those skilled in the art, such as coprecipitation or surface modification.
[0041] A mixture of ceria-alumina composite and zirconia composite: A mixture of ceria-alumina composites and zirconia composites refers to a physical mixture of the components. These mixtures can be prepared by methods known to those skilled in the art. The mixtures can be prepared before or after depositing platinum and / or rhodium onto the ceria-alumina composites and / or zirconia composites.
[0042] The mass ratio of the ceria-alumina composite to the zirconia composite in this mixture is preferably 1:4 to 4:1. More preferably, the mass ratio of the ceria-alumina composite to the zirconia composite in this mixture is 1:1. For clarity, the amount of platinum and / or rhodium that may be supported in each composite is not considered when determining the mass ratio.
[0043] The total amount of ceria-alumina composite and / or zirconia composite in the catalyst composition is 10 to 90% by mass, based on the total mass of the catalyst composition.
[0044] Platinum group metals: In the present invention, the catalytically active metals supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof are platinum and rhodium. In addition to platinum and rhodium, other PGMs may also be supported on each of the supports. The total amount of platinum in the catalyst composition is in the range of 0.1 to 10% by mass based on the total mass of the catalyst support. Preferably, the total amount of platinum in the catalyst composition is in the range of 0.1 to 5.0% by mass based on the total mass of the catalyst support. More preferably, the total amount of platinum in the catalyst composition is in the range of 0.1 to 3.0% by mass based on the total mass of the catalyst support. The total amount of rhodium in the catalyst composition is in the range of 0.1 to 10% by mass based on the total mass of the catalyst support. Preferably, the total amount of rhodium in the catalyst composition is in the range of 0.1 to 5.0% by mass based on the total mass of the catalyst support. More preferably, the total amount of rhodium in the catalyst composition is in the range of 0.1 to 3.0% by mass based on the total mass of the catalyst support.
[0045] Preferably, the catalyst composition of the present invention does not contain additional PGM metals such as palladium. That is, the catalyst composition of the present invention is essentially palladium-free. The expression "essentially palladium-free" means that palladium is present as an impurity in an amount of less than 0.01%, preferably less than 0.001%.
[0046] Alternatively, additional PGM metals, such as palladium, may optionally be present in the catalyst composition of the present invention.
[0047] It is preferable to support platinum on a ceria-alumina composite, a zirconia composite, or a mixture thereof. Furthermore, it is preferable that the total amount of platinum supported on the ceria-alumina composite and / or zirconia composite be 0.1 to 10% by mass based on the total mass of the ceria-alumina composite and / or zirconia composite. More preferably, the platinum is supported on the ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.5 to 2.0% by mass based on the total mass of the zirconia composite and / or ceria-alumina composite.
[0048] Rhodium is preferably supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. Furthermore, the total amount of rhodium supported on the ceria-alumina composite and / or zirconia composite is preferably 0.1 to 10% by mass based on the total mass of the ceria-alumina composite and / or zirconia composite. More preferably, rhodium is supported on the ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.5 to 2.0% by mass based on the total mass of the zirconia composite and / or ceria-alumina composite.
[0049] More preferably, platinum is supported on the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the ceria-alumina composite, and rhodium is supported on the zirconia composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite; or, Platinum is supported on the zirconia composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite, and rhodium is supported on the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the ceria-alumina composite; or, platinum is supported on both the zirconia composite and the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite and the ceria-alumina composite, and rhodium is supported on the zirconia composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite; or, Platinum is supported on the zirconia composite and the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite and the ceria-alumina composite, and rhodium is supported on the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the ceria-alumina composite; or, Platinum is supported on the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the ceria-alumina composite, and rhodium is supported on the zirconia composite and the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite and the ceria-alumina composite; or, platinum is supported on the zirconia composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite, and rhodium is supported on the zirconia composite and the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite and the ceria-alumina composite; or, Platinum is supported on the zirconia composite and the ceria-alumina composite in an amount of 0.1 to 10% by mass based on the total mass of the zirconia composite and the ceria-alumina composite, and rhodium is supported on the ceria-alumina composite and the zirconia composite in an amount of 0.1 to 10% by mass based on the total mass of the ceria-alumina composite and the zirconia composite; or platinum and rhodium are supported on a mixture of the ceria-alumina composite and the zirconia composite. The mass ratio of the ceria-alumina composite to the zirconia composite in the mixture is preferably 1:4 to 4:1. It is more preferable that the mass ratio of the ceria-alumina composite to the zirconia composite in the mixture is 1:1.
[0050] The present invention will be further described by the following embodiments. The features of each embodiment can be combined with any of the other embodiments where appropriate and practical.
[0051] Embodiment 1: the below described: a) Platinum, b) Rhodium, c) Ceria-alumina composite, zirconia composite, or mixture thereof Includes, Here, platinum is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, rhodium is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, the amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. Catalyst composition.
[0052] Embodiment 2: A catalyst composition according to a prior or subsequent embodiment, wherein the amount of CeO2 in the zirconia composite is <0.001% by mass based on the total mass of the zirconia composite. Embodiment 3: A catalyst composition according to either the earlier or later embodiment, wherein platinum is supported on a ceria-alumina composite and rhodium is supported on a zirconia composite.
[0053] Embodiment 4: A catalyst composition according to either the earlier or later embodiment, wherein platinum is supported on a zirconia composite and rhodium is supported on a ceria-alumina composite.
[0054] Embodiment 5: A catalyst composition according to any of the preceding or subsequent embodiments, wherein platinum and rhodium are supported on a mixture of a ceria-alumina composite and a zirconia composite.
[0055] Embodiment 6: the below described, a) Platinum, b) Rhodium, c) A mixture of ceria-alumina composite and zirconia composite. Includes, Here, platinum and rhodium are supported on a mixture of ceria-alumina composite material and zirconia composite material. Here, the amount of platinum is 0.1 to 5.0 mass%, based on the total mass of the mixture of ceria-alumina composite and zirconia composite. Here, the amount of rhodium is 0.1 to 5.0 mass%, based on the total mass of the mixture of ceria-alumina composite and zirconia composite. Here, the amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. A catalyst composition according to either a prior or subsequent embodiment.
[0056] Embodiment 7: A catalyst composition according to any of the preceding or subsequent embodiments, wherein the mass ratio of the ceria-alumina composite to the zirconia composite in a mixture of the ceria-alumina composite and the zirconia composite is 1:4 to 4:1.
[0057] Embodiment 8: A catalyst composition according to any of the preceding or subsequent embodiments, wherein the mass ratio of the ceria-alumina composite to the zirconia composite in a mixture of the ceria-alumina composite and the zirconia composite is 1:1.
[0058] Embodiment 9: A catalyst composition according to any of the preceding or subsequent embodiments, wherein the zirconia composite comprises 85% by mass or more of ZrO2 and 15% by mass or less of rare earth metals in oxide form, based on the total mass of the zirconia composite.
[0059] Embodiment 10: A catalyst composition according to any of the preceding or subsequent embodiments, wherein the rare earth metal in oxide form is selected from lanthanum, praseodymium, yttrium, neodymium, and combinations thereof.
[0060] Embodiment 11: A catalyst composition according to any of the preceding or subsequent embodiments, wherein the zirconia composite comprises 85-95% by mass of ZrO2 and 5.0-15% by mass of lanthanum oxide, based on the total mass of the zirconia composite.
[0061] Embodiment 12: The ceria-alumina composite is a catalyst composition according to either the earlier or later embodiment, characterized in that the average ceria particle diameter measured by a transmission electron microscope is less than 50 nm.
[0062] Embodiment 13: The ceria-alumina composite is a catalyst composition according to either the earlier or later embodiment, characterized in that the average ceria particle diameter measured by a transmission electron microscope is less than 20 nm.
[0063] Embodiment 14: The ceria-alumina composite is a catalyst composition according to either the earlier or later embodiment, characterized in that the average ceria particle size measured by a transmission electron microscope is less than 10 nm.
[0064] Embodiment 15: The catalyst composition according to either the preceding or succeeding embodiment, characterized in that the ceria-alumina composite has an average ceria particle diameter of 1.0 to 10 nm as measured by a transmission electron microscope.
[0065] Embodiment 16: The catalyst composition according to any of the preceding or subsequent embodiments, wherein the total amount of ceria-alumina composites and / or zirconia composites is 10 to 90% by mass, based on the total mass of the catalyst composition.
[0066] Embodiment 16: A catalyst composition according to either the preceding or subsequent embodiment, wherein the amount of CeO2 in the ceria-alumina composite is 10 to 40% by mass, based on the total mass of the ceria-alumina composite.
[0067] Embodiment 17: A catalyst composition according to either the preceding or succeeding embodiment, wherein the amount of CeO2 in the ceria-alumina composite is 15 to 35% by mass, based on the total mass of the ceria-alumina composite.
[0068] Embodiment 18: A catalyst composition according to either the preceding or succeeding embodiment, wherein the amount of CeO2 in the ceria-alumina composite is 20 to 30% by mass, based on the total mass of the ceria-alumina composite.
[0069] Manufacturing of catalyst compositions: The present invention also relates to a method for producing a catalyst composition according to the present invention, i) Impregnating a ceria-alumina composite, a zirconia composite, or a mixture thereof with platinum to obtain a first mixture, ii) Impregnating a ceria-alumina composite, a zirconia composite, or a mixture thereof with rhodium to obtain a second mixture, and iii) Mix the first mixture and the second mixture to obtain a catalyst composition. This provides a method that includes this.
[0070] Alternatively, a method for producing the catalyst composition includes sequentially impregnating a mixture of ceria-alumina composite and zirconia composite with rhodium and platinum to obtain the catalyst composition.
[0071] Furthermore, the present invention provides a catalyst article comprising a catalyst composition according to the claims of this invention deposited on a substrate.
[0072] The catalyst article is preferably a single-layer catalyst article or a double-layer catalyst article that has hydrothermal stability at an aging temperature in the range of 950°C to 1050°C.
[0073] The above double-layer article comprises a) a first layer, b) a second layer, and c) a base material.
[0074] First layer (bottom coat) The bottom coat is deposited on the substrate. Preferably, the bottom coat covers 90-100% of the substrate surface. More preferably, the bottom coat covers 95-100% of the substrate surface, and even more preferably, the bottom coat covers the entire accessible surface of the substrate. The term "accessible surface" refers to the surface of the substrate that can be covered by conventional coating techniques used in catalyst manufacturing fields, such as impregnation techniques.
[0075] The first layer preferably contains platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. The amount of platinum in the first layer is 0.1 to 10% by mass, based on the total mass of the first layer. Alternatively, the amount of platinum in the first layer is preferably 0.3 to 5.0% by mass, based on the total mass of the first layer.
[0076] Alternatively, the first layer contains rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. The amount of rhodium in the first layer is preferably 0.1 to 10% by mass, based on the total mass of the first layer. More preferably, the amount of rhodium in the first layer is 0.1 to 1.0% by mass, based on the total mass of the first layer.
[0077] The amount of CeO2 in the ceria-alumina composite is 5.0–50% by mass, based on the total mass of the ceria-alumina composite. Similarly, the amount of ZrO2 in the zirconia composite is 50–99% by mass, based on the total mass of the zirconia composite.
[0078] Second layer (top court) The top coat is deposited on top of the bottom coat. Preferably, the top coat covers 90-100% of the surface of the bottom coat. More preferably, the top coat covers 95-100% of the surface of the substrate, and even more preferably, the top coat covers the entire accessible surface of the bottom coat.
[0079] The second layer preferably contains rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof.
[0080] The amount of rhodium in the second layer is preferably 0.1 to 10% by mass, based on the total mass of the second layer. More preferably, the amount of rhodium in the second layer is 0.1 to 1.0% by mass, based on the total mass of the second layer.
[0081] Alternatively, the second layer contains platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. The amount of platinum in the second layer is 0.1 to 10% by mass, based on the total mass of the second layer. Preferably, the amount of platinum in the second layer is 0.3 to 5.0% by mass, based on the total mass of the second layer.
[0082] The amount of CeO2 in the ceria-alumina composite is 5.0–50% by mass, based on the total mass of the ceria-alumina composite. Similarly, the amount of ZrO2 in the zirconia composite is 50–99% by mass, based on the total mass of the zirconia composite.
[0083] It is more preferable to support platinum and rhodium in a mixture of ceria-alumina composite and zirconia composite. The mass ratio of the ceria-alumina composite to the zirconia composite in this mixture is preferably 1:4 to 4:1. Furthermore, it is more preferable that the mass ratio of the ceria-alumina composite to the zirconia composite in this mixture is 1:1.
[0084] Platinum and / or rhodium are preferably fixed thermally or chemically onto a ceria-alumina composite, a zirconia composite, or a mixture thereof.
[0085] The catalyst article further comprises an oxygen storage component in the first layer and / or the second layer. Preferably, the oxygen storage component is ceria-zirconia, ceria-zirconia-lantana, ceria-zirconia-yttria, ceria-zirconia-lantana-yttria, ceria-zirconia-neodymia, ceria-zirconia-praseodymia, ceria-zirconia-lantana-neodymia, ceria-zirconia-lantana-praseodymia, ceria-zirconia-lantana-neodymia-praseodymia, or a combination thereof.
[0086] Zone (area division) configuration: Catalyst articles, such as single-layer or double-layer articles, may have a zone configuration comprising a first zone and a second zone. In a double-layer catalyst article, the first layer and / or the second layer comprises a first zone and a second zone. It is preferable that the first and second zones together cover 50-100% of the length of the substrate. More preferably, the first and second zones together cover 90-100% of the length of the substrate, and even more preferably, the first and second zones together cover the entire length of the substrate. It is also preferable that the first zone covers 10-90% of the total length of the substrate from the inlet, the second zone covers 10-90% of the total length of the substrate from the outlet, and the first and second zones together cover 20-100% of the total length of the substrate. Furthermore, it is preferable that the first zone covers 30-70% of the total length of the substrate from the entrance, and the second zone covers 30-70% of the total length of the substrate from the exit, while the first and second zones together cover 60-100% of the total length of the substrate. Moreover, it is preferable that the first zone covers 40-60% of the total length of the substrate from the entrance, and the second zone covers 40-60% of the total length of the substrate from the exit, while the first and second zones together cover 80-100% of the total length of the substrate.
[0087] The first zone and / or the second zone preferably contain platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. The amount of platinum in the first layer is preferably 0.1 to 10% by mass, based on the total mass of the first layer, and also preferably 0.3 to 5.0% by mass, based on the total mass of the first layer. Alternatively, the first zone and / or the second zone may contain rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. The amount of rhodium in the first layer is preferably 0.1 to 10% by mass, based on the total mass of the first layer. It is more preferably 0.1 to 1.0% by mass, based on the total mass of the first layer. The amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Furthermore, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite.
[0088] It is more preferable to support platinum and rhodium in a mixture of ceria-alumina composite and zirconia composite. The mass ratio of the ceria-alumina composite to the zirconia composite in this mixture is preferably 1:4 to 4:1. Furthermore, it is more preferable that the mass ratio of the ceria-alumina composite to the zirconia composite in this mixture is 1:1.
[0089] Base material: The substrate of the catalyst article of the invention described in these claims may be made of any of the materials commonly used to manufacture automotive catalysts. In one embodiment, the substrate is a ceramic substrate, a metal substrate, a ceramic foam substrate, a polymer foam substrate, or a woven fiber substrate. In one embodiment, the substrate is a ceramic or metal monolithic honeycomb structure.
[0090] The substrate provides multiple walls for applying and adhering a wash coat containing the catalyst composition described in this document, thereby functioning as a carrier for the catalyst composition.
[0091] Examples of metal substrates include heat-resistant metals and metal alloys, such as titanium and stainless steel, and other alloys in which iron is a substantial or major component. Such alloys may contain one or more of nickel, chromium, and / or aluminum, with the total amount of these metals constituting at least 15% by mass of the alloy, preferably, for example, 10-25% by mass of chromium, 3-8% of aluminum, and up to 20% by mass of nickel. The alloy may also contain small or trace amounts of one or more metals, such as manganese, copper, vanadium, or titanium. The surface of the metal substrate may be oxidized at a high temperature, for example, above 1000°C, to form an oxide layer on the substrate surface, thereby improving the corrosion resistance of the alloy and promoting adhesion of the wash coat layer to the metal surface.
[0092] Examples of suitable refractory materials that can be used to construct the base material include, for example, cordierite, mullite, cordierite-alumina, silicon nitride, zircon mullite, spodumene, alumina silica-magnesia, zircon silicate, sillimanite, magnesium silicate, zircon, petalite, alumina, and aluminosilicate.
[0093] As the substrate, any suitable substrate can be used, such as a monolithic flow-through substrate having multiple fine, parallel gas channels extending from the inlet to the outlet surface of the substrate so that the channels are open to the fluid flow. The substantially straight channels from inlet to outlet are defined by walls coated with a catalyst material as a wash coat so that the gas flowing through the channels comes into contact with the catalyst material. The channels in the monolithic substrate are thin-walled channels that can have any suitable cross-sectional shape, such as trapezoidal, rectangular, square, sinusoidal, hexagonal, elliptical, or circular. Such structures have about 60 to about 1200 or more gas inlet openings (i.e., "cells") (cpsi) per square inch of cross-sectional area, and more commonly about 300 to 900 cpsi. The wall thickness of the flow-through substrate can vary, typically ranging from 0.002 to 0.1 inches. Typical commercially available flow-through substrates are cordierite substrates with 400 cpsi and a wall thickness of 6 mils, or 600 cpsi and a wall thickness of 4 mils. However, it is understood that the present invention is not limited to a specific substrate type, material, or geometric arrangement. In another embodiment, the substrate may be a wall-flow substrate, where each passage is blocked at one end of the substrate body by a non-porous plug, in which case the passages are alternately blocked at both end faces. This allows the gas flow to reach the outlet through the porous walls of the wall-flow substrate. Such monolithic substrates can have a pressure of up to about 700 cpsi or more, for example, about 100 to 400 cpsi, more typically about 200 to about 300 cpsi. The cross-sectional shape of each cell may vary as described above. The wall thickness of the wall-flow substrate is typically 0.002 to 0.1 inches. Typical commercially available wall-flow substrates are made of porous cordierite, one example having a wall thickness of 10 mils at 200 cpsi or 8 mils at 300 cpsi, and a wall porosity of 45 to 65%. Other ceramic materials such as aluminum titanate, silicon carbide, and silicon nitride are also used as wall-flow filter substrates. However, the present invention is understood to be not limited to a specific substrate type, material, or geometric arrangement.It should be noted that, when the substrate is a wall-flow substrate, the catalyst composition can not only be placed on the surface of the wall, but can also penetrate into the pore structure of the porous wall (i.e., partially or completely block the pore openings). In one embodiment, the substrate has a flow-through ceramic honeycomb structure, a wall-flow ceramic honeycomb structure, or a metal honeycomb structure.
[0094] Figures 9A and 9B show an exemplary substrate 2 in the form of a flow-through substrate coated with the wash-coat composition described herein. Referring to Figure 9A, the exemplary substrate 2 has a cylindrical shape and has a cylindrical outer surface 4, an upstream end surface 6, and a corresponding downstream end surface 8 identical to the end surface 6. The substrate 2 has a plurality of fine, parallel gas channels 10 formed therein. As can be seen from Figure 9B, each channel 10 is formed by a wall 12 and extends through the substrate 2 from the upstream end surface 6 to the downstream end surface 8, and each channel 10 is not blocked so that a fluid flow, such as a gas flow, can flow longitudinally through the substrate 2 via the gas channels 10. As can be seen more clearly in Figure 9B, the wall 12 is dimensioned and constructed so that the gas channels 10 have a substantially regular polygonal shape. As illustrated, the wash-coat composition can be applied as a plurality of separate layers, if desired. In the illustrated embodiment, the washcoat composition comprises a separate first washcoat layer 14 attached to the wall 12 of the base material member, and a second washcoat layer 16 applied to the surface of the first washcoat layer 14. In one embodiment, the invention described in the claims may be carried out using two or more (e.g., three or four) washcoat layers, and is not limited to the illustrated two-layer embodiment.
[0095] Figure 10 illustrates an exemplary substrate 2 of a wall flow filter substrate coated with the washcoat composition described herein. As shown in Figure 10, the exemplary substrate 2 has a plurality of channels, or passages 52. These passages are tubularly surrounded by the inner wall 53 of the filter substrate. The substrate has an inlet end 54 and an outlet end 56. These passages are alternately blocked by inlet plugs 58 at the inlet ends and by outlet plugs 60 at the outlet ends, forming a checkerboard pattern of opposing channels at the inlet 54 and outlet 56. The gas flow 62 enters through the unblocked channel inlet 64, is stopped by the outlet plugs 60, and diffuses through the (porous) channel wall 53 to the outlet side 66. The gas does not flow back to the inlet side of the wall due to the presence of the inlet plugs 58. The porous wall flow filter used in the present invention is catalytic in that the wall of the filter has one or more catalytic materials on it or contains one or more catalytic materials within it. The catalyst material may be present only on the inlet side of the element wall, only on the outlet side, or on both the inlet and outlet sides, or the wall itself may be made entirely or partially of the catalyst material. The present invention also includes methods of using one or more layers of catalyst material on the inlet and / or outlet walls of the element.
[0096] Manufacturing of catalyst articles: In another aspect of the present invention, a method for producing the catalyst articles described herein is provided. This method comprises the following steps: First, a slurry is prepared consisting of platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof, and rhodium supported on ceria-doped alumina, a zirconia composite, or a mixture thereof. In the next step, the prepared slurry is deposited onto a substrate to obtain a catalyst article, which is then calcined at a temperature in the range of 400 to 700°C. The steps for preparing the slurry include techniques selected from induce-wetness impregnation, induce-wetness co-impregnation, and post-addition.
[0097] Preferably, the method for manufacturing the catalyst article consists of the following steps: - To prepare a slurry in which platinum and rhodium are supported on a mixture of ceria-alumina composite material and zirconia composite material. - After depositing the slurry onto the substrate to obtain the catalyst, it is calcined at a temperature in the range of 400 to 700°C. Includes, Here, the process of preparing the slurry includes techniques selected from induce-wetness impregnation, induce-wetness co-impregnation, and post-addition.
[0098] This method may include a preliminary step of thermally or chemically fixing platinum, rhodium, or both onto a support.
[0099] Substrate coating: The catalyst compositions described above are typically prepared in the form of catalyst particles. These catalyst particles are mixed with water to form a slurry for coating catalyst substrates, such as honeycomb-type substrates. In addition to the catalyst particles, the slurry may optionally contain binders in the form of alumina, silica, zirconium acetate, zirconia, or zirconium hydroxide, associative thickeners, and / or surfactants (including anionic, cationic, nonionic, or amphoteric surfactants). Other examples of binders include boehmite, gamma-alumina, or delta / theta-alumina, and silica sol. If present, the binder is typically used in an amount of about 1-5% by mass of the total washcoat load. Acidic or basic species are also added to the slurry to adjust the pH as appropriate. For example, in some embodiments, the pH of the slurry is adjusted by adding ammonium hydroxide, aqueous nitric acid solution, or acetic acid. The typical pH range of the slurry is about 3-12.
[0100] The slurry can be pulverized to reduce particle size and facilitate particle mixing. This pulverization can be carried out using a ball mill, continuous mill, or other similar apparatus, and the solid content of the slurry may be, for example, about 20-60% by mass, more specifically about 20-40% by mass. In one embodiment, the pulverized slurry is characterized by a D90 particle size of about 3-40 microns, preferably 10-30 microns, and more preferably 10-15 microns. 90 This is determined using a dedicated particle size analyzer. In this example, a device was used that measures the particle size in a small amount of slurry using laser diffraction. 90 This usually refers to a unit called microns, meaning that 90% of the particles have a diameter smaller than that value, based on the number of particles.
[0101] The slurry is applied to the catalyst substrate using a wash-coat technique known in the art. In one embodiment, the catalyst substrate is immersed in the slurry once or multiple times, or the slurry is used to coat the substrate. The coated substrate is then dried at a high temperature (e.g., 100-150°C) for a set period of time (e.g., 10 minutes to 3 hours), and then calcined by heating at, for example, 400-700°C for about 10 minutes to about 3 hours. After drying and calcining, the final wash-coat coating layer is considered essentially solvent-free. After calcining, the catalyst load obtained by the wash-coat technique described above can be determined by calculating the difference between the mass of the substrate with and without coating. As will be apparent to those skilled in the art, the catalyst load can be changed by altering the rheology of the slurry. Furthermore, the coating / drying / calcining process for producing the wash-coat can be repeated as needed to build up the coating to a desired load level or thickness. In other words, multiple wash-coats can be applied.
[0102] In certain embodiments, the coated substrate is aged by heat treatment. In one embodiment, aging is carried out by alternating hydrocarbon / air supply for 50 to 75 hours at a temperature of about 850°C to about 1050°C in an environment containing 10% by volume of water. Thus, in certain embodiments, an aged catalyst article is provided. In certain embodiments, particularly effective materials include metal oxide-based carriers (including, but not limited to, substantially 100% ceria carriers) that maintain their pore volume at a high percentage (e.g., about 95 to 100%) during aging (e.g., aging at about 850°C to about 1050°C, 10% by volume of water, alternating hydrocarbon / air supply, 50 to 75 hours).
[0103] The present invention will be further described by the following embodiments. The features of each embodiment can be combined with any of the other embodiments where appropriate and practical.
[0104] Embodiment 19: A. The following: a) Platinum, b) Rhodium, c) Ceria-alumina composite, zirconia composite, or mixture thereof Includes, Here, platinum is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, rhodium is supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof in an amount of 0.1 to 10.0% by mass, based on the total mass of the ceria-alumina composite and / or the zirconia composite. Here, the amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. Catalyst composition, and B. Base material A catalyst article comprising the following features.
[0105] Embodiment 20: A catalyst article according to either the earlier or later embodiment, wherein the catalyst article is a single-layer catalyst article and has hydrothermal stability at an aging temperature in the range of 950°C to 1050°C.
[0106] Embodiment 21: The catalyst article, a) The first layer, b) The second layer, and c) Base material A double-layered article comprising, Here, the first layer comprises platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. Here, the second layer comprises rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. Here, the first layer is at least partially deposited on the substrate, and the second layer is at least partially deposited on the first layer. Here, the amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. Here, the amount of platinum in the first layer is 0.3 to 5.0 mass%, based on the total mass of the first layer. Here, the amount of rhodium in the second layer is 0.1 to 1.0 mass%, based on the total mass of the second layer. A catalyst article as described in either the preceding or subsequent embodiment.
[0107] Embodiment 22: The catalyst article, a) The first layer, b) The second layer, and c) Base material A double-layered article comprising, Here, the first layer comprises rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. Here, the second layer comprises platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof. Here, the first layer is at least partially deposited on the substrate, the second layer is at least partially deposited on the first layer, and the amount of CeO2 in the ceria-alumina composite is 5.0 to 50% by mass, based on the total mass of the ceria-alumina composite. Here, the amount of ZrO2 in the zirconia composite is 50-99% by mass, based on the total mass of the zirconia composite. Here, the amount of platinum in the second layer is 0.3 to 5.0 mass%, based on the total mass of the second layer. Here, the amount of rhodium in the first layer is 0.1 to 1.0 mass%, based on the total mass of the first layer. A catalyst article as described in either the preceding or subsequent embodiment.
[0108] Embodiment 23: The catalyst article is a catalyst article according to either the preceding or subsequent embodiment, having a zone configuration comprising a first zone and a second zone.
[0109] Embodiment 24: The catalyst article according to any of the preceding or subsequent embodiments, further comprising an oxygen storage component, the oxygen storage component being ceria-zirconia, ceria-zirconia-lantana, ceria-zirconia-yttria, ceria-zirconia-lantana-yttria, ceria-zirconia-neodymia, ceria-zirconia-praseodymia, ceria-zirconia-lantana-neodymia, ceria-zirconia-lantana-praseodymia, ceria-zirconia-lantana-neodymia-praseodymia, or a combination thereof.
[0110] Embodiment 25: A catalyst article according to any of the preceding or subsequent embodiments, wherein platinum and / or rhodium are thermally or chemically immobilized on a ceria-alumina composite, a zirconia composite, or a mixture thereof.
[0111] Waste disposal system: In another aspect of the present invention, an exhaust gas treatment system for an internal combustion engine is provided, the system comprising a catalyst article described herein. In one example, the system comprises a platinum group metal-based ternary conversion (TWC) catalyst article and a catalyst article according to the present claims, the platinum group metal-based ternary conversion (TWC) catalyst article being located downstream of the internal combustion engine and in fluid communication with the exhaust gas from the engine. Alternatively, the catalyst article of the present invention can be used as part of an integrated exhaust system that includes one or more additional components for treating exhaust gas emissions.
[0112] For example, an exhaust system, also known as an exhaust treatment system, may further comprise a proximal coupled TWC catalyst, an underfloor catalyst, a catalytic soot filter (CSF) component, and / or a selective catalytic reduction (SCR) catalyst article. The above-mentioned components are merely illustrative and should not be construed as limiting the scope of the present invention.
[0113] The catalytic converter can be positioned in a proximal coupling location. Placing the proximal coupling catalyst close to the engine allows the catalyst to reach its reaction temperature as quickly as possible. Generally, proximal coupling catalysts are positioned within 3 feet of the engine, more specifically within 1 foot, and even more specifically less than 6 inches from the engine. Proximal coupling catalysts are often directly mounted to the exhaust manifold. Due to their proximity to the engine, high-temperature stability is required for proximal coupling catalysts.
[0114] Another aspect of the present invention provides a method for treating a gaseous exhaust flow containing hydrocarbons, carbon monoxide, nitrogen oxides, and particulate matter. This method comprises bringing the exhaust flow into contact with a catalyst article or exhaust gas treatment system according to the invention described in the claims.
[0115] The present invention also provides a method for reducing the levels of hydrocarbons, carbon monoxide, and nitrogen oxides in a gaseous exhaust stream. This method comprises bringing a gaseous exhaust stream into contact with a catalyst article or exhaust gas treatment system according to the invention described in these claims to reduce the levels of hydrocarbons, carbon monoxide, and nitrogen oxides in the exhaust gas.
[0116] Furthermore, another aspect of the present invention provides a method for using a catalyst article or exhaust gas treatment system according to the present claims to purify a gaseous exhaust stream containing hydrocarbons, carbon monoxide, and nitrogen oxides. [Examples]
[0117] The embodiments of the invention described in these claims will be further illustrated by the following examples. These examples are provided to illustrate specific embodiments of the invention and should not be construed as limiting the invention.
[0118] Example 1: Platinum supported on a ceria-alumina composite (CeO2 / Al2O3) Powder catalyst samples were prepared by impregnating CeO2 / Al2O3 with a Pt tetraamine hydroxide solution using the spontaneous wetness technique. This CeO2 / Al2O3 contained 20% by mass of CeO2 and 80% by mass of Al2O3. Before aging and testing the catalyst, the catalyst powder was prepared using the following procedure. Deionized water was added to the impregnated powder to form a slurry with a solid content of approximately 30%. The pH of the slurry was adjusted to 4-4.5 using HNO3. After drying the slurry under stirring, it was calcined in air at 590°C for 2 hours. The calcined catalyst was pulverized and sieved to a particle size of 250-500 microns.
[0119] [Table 1]
[0120] Example 2: Rhodium supported on a ceria-alumina composite A powder catalyst sample was prepared by impregnating CeO2 / Al2O3 with a nitric acid Rh solution using the spontaneous wetness technique. The CeO2 content in CeO2 / Al2O3 was 20% by mass. The Al2O3 content in CeO2 / Al2O3 was 80% by mass. The sample preparation procedure was the same as in Example 1, except that Rh / CeO2 / Al2O3 was used.
[0121] [Table 2]
[0122] Example 3: Platinum supported on a lantaner zirconia composite (La2O3 / ZrO2) A powder catalyst sample was prepared by impregnating La2O3 / ZrO2 with a Pt tetraamine hydroxide solution using the spontaneous wetness technique. The amount of La2O3 in the La2O3 / ZrO2 was 9% by mass, while the amount of ZrO2 was 91% by mass. The sample preparation procedure was the same as in Example 1, except that Pt / La2O3 / ZrO2 was used.
[0123] [Table 3]
[0124] Example 4: Rh supported on La2O3 / ZrO2 A powder catalyst sample was prepared by impregnating La2O3 / ZrO2 with a nitric acid (Rh) solution using the spontaneous wetness technique. The amount of La2O3 in the La2O3 / ZrO2 was 9% by mass, while the amount of ZrO2 was 91% by mass. The sample preparation procedure was the same as in Example 1, except that Rh / La2O3 / ZrO2 was used.
[0125] [Table 4]
[0126] Example 5: Platinum and rhodium supported on CeO2 / Al2O3 Rh was first impregnated with CeO2 / Al2O3, and then with Pt.
[0127] Deionized H2O was added to PGM-impregnated powder to obtain a slurry with a solid content of approximately 30%. The pH of the slurry was adjusted to 4.0-4.5 with nitric acid. The slurry was pulverized for 10 minutes and then dried while stirring. The dried powder was calcined in air at 590°C for 2 hours. This powder was pulverized and sieved into 250-500 mm particles.
[0128] [Table 5]
[0129] Example 6: Platinum and rhodium supported on La2O3 / ZrO2 The method of Example 5 was repeated, except that La2O3 / ZrO2 was used as the support.
[0130] [Table 6]
[0131] Example 7: Platinum and rhodium supported on CeO2 / Al2O3 and La2O3 / ZrO2 a. Preparation of Sample 15 CeO2 / Al2O3 and La2O3 / ZrO2 were first physically mixed in a 1:1 mass ratio while stirring. Rh and Pt were then sequentially impregnated into this mixture. The impregnated samples were molded according to the procedure described in Example 1.
[0132] b. Preparation of Sample 16 Pt was impregnated in CeO2 / Al2O3 and calcined in air at 450°C. Rh was separately impregnated in La2O3 / ZrO2 and calcined in air at 450°C. The two calcined powders were mixed in a 1:1 ratio. Deionized water (H2O) was added to this mixed catalyst to form a slurry with a solid content of approximately 30%. The pH of the slurry was adjusted to 4.0-4.5 with nitric acid. The slurry was pulverized for 10 minutes and then dried while stirring. The dried powder was calcined in air at 590°C for 2 hours. This powder was pulverized and sieved to 250-500 mm.
[0133] c. Preparation of Sample 17 Rh was impregnated into CeO2 / Al2O3 and calcined in air at 450°C. Pt was separately impregnated into La2O3 / ZrO2 and calcined in air at 450°C. The two calcined catalyst powders were mixed in a 1:1 ratio. Deionized water (H2O) was added to this mixed catalyst to form a slurry with a solid content of approximately 30%. The pH of the slurry was adjusted to 4.0-4.5 with nitric acid. The slurry was pulverized for 10 minutes and then dried while stirring. The dried powder was calcined in air at 590°C for 2 hours. This powder was pulverized and sieved to 250-500 mm.
[0134] [Table 7]
[0135] Example 8: Platinum supported on alumina (Al2O3) A powder catalyst sample was prepared by impregnating Al2O3 with a Pt tetraamine hydroxide solution using the induce wetness technique. The sample preparation procedure was the same as in Example 1, except that a Pt / Al2O3 catalyst was used.
[0136] [Table 8]
[0137] Example 9: Rhodium supported on alumina A powder catalyst sample was prepared by impregnating Al2O3 with a nitric acid (Rh) solution using the inducer wetness technique. The sample preparation procedure was the same as in Example 1, except that Rh / Al2O3 was used.
[0138] [Table 9]
[0139] Example 10: Platinum and rhodium supported on alumina The method of Example 5 was repeated, except that alumina was used as the support. The sample molding procedure was the same as in Example 1, except that a Pt_Rh / Al2O3 catalyst was used.
[0140] [Table 10]
[0141] Example 11: Platinum and rhodium supported on an oxygen storage component (OSC1) OSC1 is composed of 11% CeO2, 74% ZrO2, 2% La2O3, 8% Y2O3, and 5% Nd2O3.
[0142] The PGM deposition procedure was the same as in Example 1 (for Pt), Example 2 (for Rh), and Example 5 (for Pt and Rh), except that OSC1 was used as the support. The sample molding procedure was the same as in Example 1, except that an OSC1-supported catalyst was used.
[0143] [Table 11]
[0144] Example 12: Platinum and rhodium supported on OSC2 OSC2 is composed of 20% CeO2, 70% ZrO2, 5% La2O3, and 5% Y2O3.
[0145] The PGM deposition procedure is the same as in Example 1 (for Pt), Example 2 (for Rh), and Example 5 (for Pt and Rh), except that OSC2 was used as the support. The sample molding procedure is the same as in Example 1, except that an OSC2-supported catalyst was used.
[0146] [Table 12]
[0147] Example 13: Platinum and rhodium supported on OSC3 OSC3 is composed of 40% CeO2, 50% ZrO2, 5% La2O3, and 5% Y2O3.
[0148] The PGM deposition procedure is the same as in Example 1 (for Pt), Example 2 (for Rh), and Example 5 (for Pt and Rh), except that OSC3 was used as the support. The sample molding procedure is the same as in Example 1, except that an OSC3-supported catalyst was used.
[0149] [Table 13]
[0150] Example 14: Platinum and rhodium supported on a mixed support Prior to PGM impregnation, two types of carriers were mixed in a 1:1 mass ratio. The PGM deposition procedure was the same as in Example 7 (Sample 15), except that a mixture of La2O3 / ZrO2 and OSC3 or a mixture of CeO2 / Al2O3 and OSC2 was used instead of a mixture of CeO2 / Al2O3 and La2O3 / ZrO2. The sample molding procedure was the same as described in Example 1.
[0151] [Table 14]
[0152] Example 15: CeO2 loading amount dependence of platinum and rhodium supported on ceria-alumina composites (CeO2 / Al2O3) For samples 36, 37, and 38, the method of Example 5 was repeated, except that CeO2 / Al2O3 composites containing 10%, 30%, and 50% CeO2, respectively, were used.
[0153] [Table 15]
[0154] Example 16: Catalyst performance measurement: All catalysts were aged at 1050°C for 5 hours using 10% H2O with alternating lean / rich feed (10 minutes 4% air / 10 minutes 4% H2 / N2). The aged catalysts were then subjected to 70,000 h. -1 The system was evaluated in a light-off test using a monolith-equivalent GHSV with an l=1 oscillating feed (l=0.95 / 1.05 circulating at 1Hz) at 175-450°C. In the light-off test, the lean feed (l=1.05) consisted of 0.7% CO, 0.22% H2, 3000 ppm HC(C1) (propene:propane = 2:1), 1500 ppm NO, 14% CO2, 10% H2O, and ~1.8% O2, while the rich feed (l=0.95) contained 2.33% CO, 0.77% H2, 3000 ppm HC(C1), 1500 ppm NO, 14% CO2, 10% H2O, and ~0.7% O2. The precise lambda value was fine-tuned by adjusting the O2 level based on the upstream λ-sensor.
[0155] In the case of CeO2 / Al2O3-supported catalysts, the degree of performance improvement of the Pt / Rh composition compared to the Rh standard differs depending on whether it is CO, NO, or HC. The improvement in CO conversion rate is slight. However, significant improvements in activity are observed in both the low and high temperature ranges for NO and HC conversion rates. For example, the HC T50 (temperature at 50% conversion rate) is 55°C lower for 2%Pt / 0.5%Rh / CeO2 / Al2O3 than for the Rh standard. The difference in HC conversion rate at 325°C is 61%. Figure 1 shows a comparison of the light-off performance of CO, NO, and HC conversion rates for samples 1-7 (containing CeO2 / Al2O3 as the support).
[0156] Figure 2 shows a comparison of the light-off performance of CO, NO, and HC conversion rates for samples 8-14 (containing La2O3 / ZrO2 as a support). The performance improvement of the Pt / Rh catalyst relative to the Rh standard is proportional to the amount of Pt loaded. In the case of 2%Pt_0.5%Rh, the light-off T50 is 22°C, 27°C, and 19°C lower for CO, NO, and HC conversion rates, respectively.
[0157] Figure 3 shows a comparison of the light-off performance of CO, NO, and HC conversion rates for samples 15, 16, and 17 (containing two types of supports: CeO2 / Al2O3 and La2O3 / ZrO2). These three samples showed similar efficiency for CO conversion. Samples 15 and 17 were found to be active for NOx conversion, while samples 15 and 16 were optimal for HC conversion. Overall, sample 15 was found to improve the conversion rates of CO, NO, and HC.
[0158] Figure 4 shows the light-off performance of the Al2O3-supported catalyst. The Pt reference catalyst exhibits significantly lower activity for CO, NO, and HC compared to the Rh reference catalyst. The difference in light-off T50 between 2%Pt and 0.5%Rh is 58, >100, and 29°C for CO, NO, and HC, respectively. When Pt and Rh are combined, they exhibit significantly higher activity than the sum of the individual components, and it was found that the activity of the Pt / Rh composition is proportional to the amount of Pt loaded in the catalyst. For example, the HC conversion rates at 325°C were 31%, 62%, and 68% for 0.5%Pt / 0.5%Rh, 1%Pt / 0.5%Rh, and 2%Pt / 0.5%Rh, respectively, while the conversion rate was zero for all individual component catalysts.
[0159] Figures 5 to 7 show the performance results when OSC1 (samples 25-27), OSC2 (samples 28-30), and OSC3 (samples 31-33) were supported with 2% Pt, 0.5% Rh, and 2% Pt / 0.5% Rh, respectively. For each OSC support, the Pt / Rh composition (2% Pt and 0.5% Rh) showed significantly lower light-off temperatures for CO, NO, and HC conversion compared to the Rh-based composition. Furthermore, the Pt / Rh composition improved the conversion rate of NO and HC at high temperatures. The degree of improvement appears to be proportional to the ceria content in the OSC support.
[0160] Figure 8 shows the performance of Pt / Rh compositions (2% Pt and 0.5% Rh) supported on a mixed support. Compared to OSC-supported Pt / Rh catalysts (samples 30 and 33), CeO2 / Al2O3 and La2O3 / ZrO2-supported Pt / Rh catalysts (samples 7 and 14) show lower light-off temperatures and lower conversion rates at high temperatures. Pt / Rh supported on a 1:1 mixture of La2O3 / ZrO2 and OSC3 (sample 34) exhibits similar performance characteristics to Pt / Rh on OSC3 (high light-off temperature and high high-temperature conversion). However, when the Pt / Rh composition is supported on a 1:1 mixture of CeO2 / Al2O3 and OSC2 (sample 35), the catalyst exhibits both a low light-off temperature and a high high-temperature conversion rate.
[0161] The table below shows a comparison of the conversion rates of Pt / Rh (2% Pt and 0.5% Rh) compositions supported on various single and mixed supports at light-off temperatures T50 and 400°C.
[0162] [Table 16]
[0163] Catalysts with Pt / Rh supported on CeO2 / Al2O3 and La2O3 / ZrO2 have lower light-off temperatures (T50s) compared to Pt / Rh catalysts with OSC supported on Al2O3.
[0164] OSC-supported Pt / Rh catalysts exhibit higher high-temperature conversion rates. Pt / Rh catalysts supported on a mixture of CeO2 / Al2O3 and OSC2 yield high catalytic activity at both low and high temperatures.
[0165] The following table shows a comparison of the light-off temperatures (T50) of Pt / Rh (2% Pt and 0.5% Rh) compositions supported on CeO2 / Al2O3 composites with various CeO2 loading amounts.
[0166] [Table 17]
[0167] The results show that Pt / Rh catalysts supported on CeO2 / Al2O3 composites containing 20% and 30% CeO2 exhibited the lowest light-off temperatures (T50s) for CO, NO, and HC. Increasing the CeO2 content in the composite beyond 30% or decreasing it below 20% tended to increase the light-off temperature. Sample 24, a catalyst on an undoped support (pure Al2O3), showed the lowest activity.
[0168] In this specification, the terms “one embodiment,” “a particular embodiment,” “one or more embodiments,” or “embodiment” mean that the specific features, structures, materials, or properties described in relation to that embodiment are included in at least one embodiment of the invention described in these claims. Therefore, phrases such as “in one or more embodiments,” “in a particular embodiment,” “in one embodiment,” or “in an embodiment” found in various places throughout this specification do not necessarily refer to the same embodiment of the invention described in these claims. Furthermore, specific features, structures, materials, or properties can be combined in appropriate ways in one or more embodiments. All of the various embodiments, aspects, and optional features disclosed herein can be combined in all modifications, regardless of whether such features or elements are explicitly combined in the description of a particular embodiment herein. The invention described in these claims should be considered, and should be read as a whole, to mean that the separable features or elements of the disclosed invention are intended to be combined in any of its various aspects and embodiments, unless the context explicitly indicates otherwise.
[0169] The embodiments disclosed herein, while described with reference to specific embodiments, should be understood as merely illustrative examples of the principles and applications of the invention described in these claims. It will be apparent to those skilled in the art that various modifications and variations can be made to the methods and apparatus of the present invention without departing from the spirit and scope of the invention described in these claims. Accordingly, the invention described in these claims is intended to include the modifications and variations, and equivalents thereof, within the appended claims, and the embodiments described above are presented for illustrative purposes only, not for limiting purposes. All patents and publications referenced herein are incorporated herein by reference with respect to their specific teachings unless otherwise specified. [Explanation of symbols]
[0170] 2 Base material 4 External surface 6 Upstream end face 8 Downstream end face 10 Gas flow path 12 walls 14. First Wash Coat 16. Second Wash Coat 54 Inlet end 58 Inlet Plug 62 Gas flow 53 Inner wall 56 Outlet end 60 Outlet Plugs 52 aisles 64 Channel Inlet 66 Exit side
Claims
1. a) Platinum b) rhodium, and c) Ceria-alumina composite, zirconia composite, or a mixture thereof A catalyst composition comprising: platinum is supported on the ceria-alumina composite, the zirconia composite, or a mixture thereof in an amount of 0.1 to 10 mass % based on the total mass of the ceria-alumina composite and / or the zirconia composite; Rhodium is supported on the ceria-alumina composite, the zirconia composite, or a mixture thereof in an amount of 0.1 to 10 mass % based on the total mass of the ceria-alumina composite and / or the zirconia composite; CeO in ceria-alumina composite 2 is 1.0 to 50 mass % based on the total mass of the ceria-alumina composite, ZrO in zirconia composite 2 is 50 to 99 wt. % based on the total weight of the zirconia composite.
2. The catalyst composition of claim 1, wherein the total amount of the ceria-alumina composite and / or the zirconia composite in the catalyst composition is 10 to 90 wt %, based on the total weight of the catalyst composition.
3. CeO in zirconia composite 2 A catalyst composition according to any one of claims 1 to 2, wherein the amount of is <0.001 wt.% based on the total weight of the zirconia composite.
4. 4. The catalyst composition according to claim 1, wherein platinum is supported on a ceria-alumina composite and rhodium is supported on a zirconia composite.
5. 4. The catalyst composition according to claim 1, wherein platinum is supported on a zirconia composite and rhodium is supported on a ceria-alumina composite.
6. 4. The catalyst composition according to claim 1, wherein platinum and rhodium are supported on a mixture of a ceria-alumina composite and a zirconia composite.
7. 7. The catalyst composition according to claim 1, wherein the mass ratio of the ceria-alumina composite to the zirconia composite is from 1:4 to 4:
1.
8. 8. The catalyst composition according to claim 1, wherein the mass ratio of the ceria-alumina composite to the zirconia composite is 1:
1.
9. The zirconia composite contains 85% by weight or more of ZrO based on the total weight of the zirconia composite. 2 and up to 15 wt. % of a rare earth metal in oxide form, wherein the rare earth metal in oxide form is selected from lanthanum, praseodymium, yttrium, neodymium, and combinations thereof.
10. The zirconia composite comprises 85 to 95 mass % ZrO based on the total mass of the zirconia composite. 2 and 5.0 to 15 wt. % of lanthana.
11. CeO in ceria-alumina composite 2 11. Catalyst composition according to any one of claims 1 to 10, wherein the amount is from 5.0 to 50 wt%, preferably from 15 to 35 wt%, more preferably from 20 to 30 wt%, based on the total weight of the ceria-alumina composite.
12. 12. The catalyst composition according to any one of claims 1 to 11, wherein the average particle size of the ceria in the ceria-alumina composite is less than 20 nm as measured by transmission electron microscopy.
13. - impregnating a ceria-alumina composite, a zirconia composite or a mixture thereof with platinum to obtain a first mixture; - impregnating a ceria-alumina composite, a zirconia composite or a mixture thereof with rhodium to obtain a second mixture; and - mixing the first mixture with the second mixture to obtain a catalyst composition; A method for producing the catalyst composition according to any one of claims 1 to 12, comprising:
14. A method for producing a catalyst composition according to any one of claims 1 to 12, comprising the steps of impregnating a mixture of a ceria-alumina composite and a zirconia composite with rhodium and platinum in sequence to obtain the catalyst composition.
15. A catalytic article comprising the catalytic composition of any one of claims 1 to 12 deposited on a substrate.
16. The catalyst article of claim 15, wherein the catalyst article is a single layer catalyst article and has hydrothermal stability at an aging temperature in the range of 950°C to 1050°C.
17. the catalytic article is a dual layer article comprising: a) a first layer, b) a second layer, and c) a substrate; the first layer comprises platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof; the second layer comprises rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof; the first layer is at least partially deposited on the substrate, and the second layer is at least partially deposited on the first layer; CeO in ceria-alumina composite 2 is 5.0 to 50 wt. %, based on the total weight of the ceria-alumina composite; ZrO in zirconia composite 2 is 50 to 99 weight percent based on the total weight of the zirconia composite; the amount of platinum in the first layer is 0.3 to 5.0 wt. %, based on the total weight of the first layer; The catalytic article of claim 15, wherein the amount of rhodium in the second layer is from 0.1 to 1.0 weight percent, based on the total weight of the second layer.
18. the catalytic article is a dual layer article comprising: a) a first layer, b) a second layer, and c) a substrate; the first layer comprises rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof; the second layer comprises platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof; The first layer is at least partially deposited on the substrate, and the second layer is at least partially deposited on the first layer, and the CeO 2 is 5.0 to 50 wt. %, based on the total weight of the ceria-alumina composite; ZrO in zirconia composite 2 is 50 to 99 weight percent based on the total weight of the zirconia composite; the amount of platinum in the second layer is 0.3 to 5.0 wt. %, based on the total weight of the second layer; the amount of rhodium in the first layer is 0.1 to 1.0 wt. %, based on the total weight of the first layer; 16. The catalyst article of claim 15.
19. The catalytic article of any one of claims 15 to 18, wherein the catalytic article has a zone configuration having a first zone and a second zone.
20. 20. The catalytic article of any one of claims 15 to 19, wherein the catalytic article further comprises an oxygen storage component comprising ceria-zirconia, ceria-zirconia-lanthana, ceria-zirconia-yttria, ceria-zirconia-lanthana-yttria, ceria-zirconia-neodymia, ceria-zirconia-praseodymia, ceria-zirconia-lanthana-neodymia, ceria-zirconia-lanthana-praseodymia, ceria-zirconia-lanthana-neodymia-praseodymia, or combinations thereof.
21. A method of producing a slurry comprising: preparing platinum supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof; and preparing a slurry comprising rhodium supported on a ceria-alumina composite, a zirconia composite, or a mixture thereof; - depositing the slurry on a substrate to obtain a catalyst article, which is then calcined at a temperature in the range of 400-700°C; Including, The method of making a catalyst article according to any one of claims 15 to 20, wherein the step of preparing the slurry comprises a technique selected from incipient wetness impregnation, incipient wetness co-impregnation, and post-addition.
22. - preparing a slurry comprising platinum and rhodium supported on a mixture of ceria-alumina composite material and zirconia composite material; - depositing the slurry on a substrate to obtain a catalyst article, which is then calcined at a temperature in the range of 400-700°C; Including, The method of making a catalyst article according to any one of claims 15 to 20, wherein the step of preparing the slurry comprises a technique selected from incipient wetness impregnation, incipient wetness co-impregnation, and post-addition.
23. An exhaust gas treatment system for an internal combustion engine, said system comprising a catalytic article according to any one of claims 15 to 20.
24. A method for reducing the levels of hydrocarbons, carbon monoxide, and nitrogen oxides in a gaseous exhaust stream, comprising contacting the gaseous exhaust stream with a catalytic article described in any one of claims 15 to 20 or an exhaust gas treatment system described in claim 23 to reduce the levels of hydrocarbons, carbon monoxide, and nitrogen oxides in the exhaust gas.
25. A method of using the catalytic article of any one of claims 15 to 20 or the exhaust gas treatment system of claim 23 for purifying a gaseous exhaust stream comprising hydrocarbons, carbon monoxide and nitrogen oxides.