Additive mixture for non-aqueous battery electrolytes
Patent Information
- Application Number
- JP2023527087
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-04
- Filing Date
- 2021-10-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing rechargeable lithium-ion batteries face challenges in achieving improved cycle life and stability, particularly at high voltages, due to the adverse effects of electrolyte decomposition and parasitic reactions.
A non-aqueous battery electrolyte comprising a primary lithium salt, a primary non-aqueous solvent, and an additive mixture containing vinylene carbonate, fluoroethylene carbonate, a sulfur-containing compound, and lithium difluorophosphate, used in amounts less than 10% by weight, enhances the performance of high-voltage rechargeable lithium-ion batteries.
The additive mixture forms a robust solid electrolyte interfacial layer, reducing parasitic reactions and electrolyte oxidation, thereby extending the cycle life and improving stability of high-voltage lithium-ion batteries without significant adverse effects.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to an additive mixture for use in battery electrolytes, particularly in the electrolytes of high-voltage rechargeable lithium-ion batteries. [Background technology]
[0002] The development of rechargeable high-energy-density batteries, such as lithium-ion (Li-ion) batteries, is of paramount importance from a technological standpoint. Conventional Li-ion batteries have been widely used in numerous commercial applications for many years. Such batteries use one or more lithium insertion compounds in each of the cathode and anode electrodes. During battery discharge, lithium is extracted from the anode material and inserted into the cathode material. During charging, this process is reversed. The voltage difference between the two electrodes when lithium is removed from one electrode and inserted into the other determines the overall voltage of the battery. The lifespan of such batteries is limited by the number of times this can be achieved without significant lithium loss due to parasitic reactions or other failures.
[0003] Typically, in a lithium-ion battery, one or more lithium transition metal oxides are used as the cathode material, and one or more carbonaceous materials, such as graphite, are used as the anode material. A suitable non-aqueous electrolyte containing one or more lithium salts and a mixture of non-aqueous solvents is also used. Such an electrolyte must react favorably with lithium during the initial lithification of the anode in order to create a stable solid electrolyte interface ("SEI") layer on the anode that allows for subsequent desirable ion transport through it while preventing further reactions with the electrolyte. Furthermore, a suitable electrolyte preferably possesses numerous other properties, including high ionic conductivity of lithium and high thermal and electrochemical stability at the cathode. Solvents suitable for commercial use typically contain ethylene carbonate to create the desired SEI layer and are mixed with other suitable non-aqueous solvents, including other carbonate solvents, to provide other desirable properties. Various lithium salts or salt mixtures may be used in commercially available products.
[0004] While current lithium-ion batteries generally perform well in a wide range of applications, improvements in cell capacity and lifespan remain desirable. However, while the former can be achieved, for example, by using high-voltage cathode materials and / or operating the battery at higher voltages, such approaches generally have a negative impact on the latter. This is because higher voltages typically increase the rate of electrolyte decomposition. Such trade-offs are commonly encountered in the development of better battery products.
[0005] A common approach used to improve battery performance in some way without causing other unacceptable effects is the use of electrolyte additives. Certain additives or additive mixtures can, in principle, be used to improve desired battery characteristics or reduce undesirable ones. In this regard, much research has been conducted over the years, and numerous chemical species and combinations have been identified and tested as potentially suitable electrolyte additives.
[0006] For example, U.S. Patent Application Publication No. 2018 / 0102570 discloses a lithium secondary battery containing a disulfonate additive and a method for manufacturing the same. In one embodiment, fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinylethylene carbonate (VEC), phosphine compounds (e.g., triphenylphosphine), phosphite compounds, phosphate compounds, propanesultone (PS), or combinations thereof may further be included in the non-aqueous solvent within the battery. Furthermore, the electrolyte used in the experimental example contained MMDS, as well as LiDFOB and LiFSI salts. Such electrolytes were found to reduce the impedance increase during cycling, but did not lead to an improvement in lifespan.
[0007] Furthermore, International Publication No. 2019 / 025980 discloses a non-aqueous electrolyte for a lithium-ion battery comprising a lithium salt, a first non-aqueous solvent, and an additive mixture comprising a first active additive of lithium difluorophosphate and a second active additive of either fluoroethylene carbonate or vinylene carbonate. The lithium-ion battery comprises a negative electrode, a positive electrode comprising NMC having micrometer-scale particles, a non-aqueous electrolyte having lithium ions dissolved in the first non-aqueous solvent, and an additive mixture comprising a first active additive of either fluoroethylene carbonate or vinylene carbonate, and a second active additive of either 1,3,2-dioxathiolane-2,2-dioxide, another sulfur-containing additive, or lithium difluorophosphate.
[0008] Furthermore, International Publication No. 2018 / 198742 discloses a lithium-ion secondary battery that includes a positive electrode containing a lithium nickel composite oxide as a positive electrode active material, and uses a cyclic sulfonic acid ester having at least two sulfonyl groups in its molecule, and a compound having only one sulfonyl group and whose highest occupied orbital energy level, calculated by the PM3 method, is -11.2 eV or lower, in the electrolyte. In addition, when such a battery is charged, a film containing sulfur atoms is formed on at least a portion of the surface of the positive electrode active material.
[0009] Furthermore, the disclosure in U.S. Patent Application Publication No. 2017 / 0301952 relates to an electrolyte and a lithium-ion battery comprising the electrolyte. The electrolyte comprises a lithium salt, an organic solvent, and additives comprising additive A, additive B, additive C, and at least one of additive D; where additive A is a cyclic sultone; additive B is a cyclic sulfate; additive C is a silane phosphate compound and / or silane borate compound; and additive D is a fluorophosphate. Due to the synergistic function of the additives, the battery has low gas generation at high temperatures, a high capacity retention rate, and high power at low temperatures.
[0010] It is generally known in the art that adding small amounts of MA additives is a method to improve charging speed and low-temperature performance. Such additives are disclosed, for example, in U.S. Patent No. 6,492,064 relating to organic solvents, electrolytes, and lithium-ion cells having good low-temperature performance. However, MA is highly reactive at high voltages, and this high reactivity reduces lifespan performance. Therefore, further additives are required to be effective. Furthermore, it is generally known in the art that the addition of very small amounts of sulfur additives helps improve battery performance at high voltages. In particular, sulfur additives such as DTD have been shown to improve performance in the presence of MA, as disclosed, for example, in U.S. Patent Application Publication No. 2019 / 0036171.
[0011] Furthermore, it is generally known and accepted in the art that solvents VC and FEC are essentially functionally interchangeable in lithium secondary battery applications. This is exemplified, for example, in International Publication 2019 / 025980, which discloses a non-aqueous electrolyte for lithium-ion batteries comprising a lithium salt, a first non-aqueous solvent, and an additive mixture comprising a first working additive of lithium difluorophosphate and a second working additive of either fluoroethylene carbonate or vinylene carbonate. The lithium-ion battery comprises a negative electrode, a positive electrode comprising NMC having micrometer-scale particles, a non-aqueous electrolyte having lithium ions dissolved in the first non-aqueous solvent, and an additive mixture comprising a first working additive of either fluoroethylene carbonate or vinylene carbonate and a second working additive of either 1,3,2-dioxathiolane-2,2-dioxide, another sulfur-containing additive, or lithium difluorophosphate. In particular, the example in International Publication No. 2019 / 025980 includes the use of VC or FEC, from which it is clear that they are essentially interchangeable in terms of the results obtained. [Prior art documents] [Patent Documents]
[0012] [Patent Document 1] U.S. Patent Application Publication No. 2018 / 0102570 [Patent Document 2] International Publication No. 2019 / 025980 [Patent Document 3] International Publication No. 2018 / 198742 [Patent Document 4] U.S. Patent Application Publication No. 2017 / 0301952 [Patent Document 5] U.S. Patent No. 6492064 [Patent Document 6] U.S. Patent Application Publication No. 2019 / 0036171 [Summary of the Invention] [Problems to be Solved by the Invention]
[0013] Despite continuous and extensive worldwide efforts towards improving rechargeable batteries, further improvements are still desired in all areas. The present invention addresses these needs and provides additional advantages as disclosed below. [Means for Solving the Problems]
[0014] An electrolyte solution containing a specific additive mixture has been found to result in improved performance of non-aqueous batteries, particularly rechargeable lithium-ion batteries, and in particular, to improve the lifespan of high-voltage rechargeable lithium-ion batteries (e.g., those with a maximum operating voltage limit of 4.2 V or higher).
[0015] Specifically, the non-aqueous battery electrolyte of the present invention contains a main lithium salt, a main non-aqueous solvent, and an additive mixture of less than 10% by weight. The additive mixture is characterized by containing an additive solvent selected from the group consisting of vinylene carbonate and fluoroethylene carbonate, a sulfur-containing compound selected from the group consisting of methylene methanedisulfonate and ethylene sulfate, and lithium difluorophosphate.
[0016] The main solvent in the electrolyte can include at least one solvent selected from the group consisting of ethylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, dimethyl carbonate, propylene carbonate, diethyl carbonate, and methyl acetate. The main lithium salt in the electrolyte can include at least one salt selected from the group consisting of LiPF6, LiBF4, lithium bis(oxalato)borate, and lithium difluoro(oxalato)borate.
[0017] In one embodiment of the present invention, the main solvent includes ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate. Further, in one embodiment of the present invention, the main lithium salt is LiPF6. Further, in certain embodiments, the main non-aqueous solvent is different from the additive solvent, and the main lithium salt is different from lithium difluorophosphate.
[0018] Most commonly, the electrolyte contains less than 10 wt% of an additive mixture. Among them, typically, the electrolyte contains 0.1 wt% - 5 wt% of an additive solvent, 0.1 wt% - 3 wt% of a sulfur-containing compound, and 0.1 wt% - 5 wt% of lithium difluorophosphate. The electrolyte may further contain 0 wt% - 2 wt% of a sultone compound such as 1,3-propene sultone.
[0019] The improved non-aqueous battery electrolyte is particularly advantageous for use in high-voltage rechargeable lithium-ion batteries, which further include a cathode electrode and an anode electrode together with an advanced non-aqueous battery electrolyte. In this regard, a typical high-voltage rechargeable lithium-ion battery has a cathode electrode having a stoichiometry of about Li y , z , x Mn 0.2 Co 0.2 O2, such as lithium nickel manganese cobalt oxide, of the formula Li x M y O <The compound contains the following: where 0 ≤ x, y ≤ 2, 2 ≤ z ≤ 4, and M contains one or more of the following elements: Ni, Al, Mn, Co, Fe, P, Mg, Ti, Zr, Ga, Cr, Ru. Such a cathode electrode may optionally include a surface coating. Furthermore, in this regard, a typical high-voltage rechargeable lithium-ion battery has an anode electrode containing graphite.
[0020] Accordingly, the present invention also includes a method for improving the cycle life and stability of a high-voltage rechargeable lithium-ion battery. In this regard, the battery in question comprises a cathode electrode, an anode electrode, and a non-aqueous electrolyte, the electrolyte comprising a main lithium salt and a main non-aqueous solvent. The method then comprises the step of adding less than 10% by weight of the aforementioned additive mixture to the electrolyte. [Brief explanation of the drawing]
[0021] [Figure 1] Figure 1 shows the normalized capacity against the number of cycles for a typical cell during the LTC test in Experiment 1 in the experimental example. [Figure 2] Figure 2 shows the delta-V as a function of the number of cycles of a typical cell during the LTC test in Experiment 1 in the experimental example. [Figure 3] Figures 3a and 3b show the normalized capacity against the number of cycles for a typical battery without LFO in the electrolyte and a battery containing LFO, respectively, during the LTC test of Experiment 1 in the experimental example. [Figure 4] Figures 4a and 4b show the delta-V as a function of cycle count for a representative battery without LFO in the electrolyte and a battery containing LFO, respectively, during the LTC test of Experiment 1 in the experimental example. [Figure 5] Figure 5 shows the storage test results of representative cells in the experimental example. [Modes for carrying out the invention]
[0022] Unless otherwise specified in the context, terms such as “comprise” and “comprising” should be interpreted in an open, comprehensive sense throughout this specification and the claims. Words such as “a” and “an” should be considered to mean at least one, but not limited to one.
[0023] Furthermore, the following definitions apply throughout this specification.
[0024] The term "lithium-ion battery" refers to both individual lithium-ion cells or arrays of such cells interconnected in series and / or parallel. Each such cell contains anode and cathode electrode materials that allow for the reversible insertion and removal of lithium ions.
[0025] The term "anode" refers to the electrode in an alkali metal ion battery that undergoes oxidation during discharge. In a lithium-ion battery, the anode is the electrode that is delithified during discharge and lithified during charging.
[0026] The term "cathode" refers to the electrode in an alkali metal ion battery where reduction occurs during discharge. In a lithium-ion battery, the cathode is the electrode that is lithiumized during discharge and delithified during charging.
[0027] In a quantitative context, the term "approximately" should be interpreted as being within a range of plus 10% to minus 10%.
[0028] In this invention, certain additive mixtures advantageous for use in electrolytes for non-aqueous battery electrolytes comprising at least one (main) lithium salt and at least one (main) non-aqueous solvent have been identified. The additive mixtures are used in amounts of less than 10% by weight in such electrolytes, and they are particularly suitable for use in rechargeable lithium batteries, such as high-voltage rechargeable lithium-ion batteries. Life advantages are obtained, particularly with respect to cycle life and stability. The additive mixtures are characterized by comprising an additive solvent selected from the group consisting of vinylene carbonate and fluoroethylene carbonate, a sulfur-containing compound selected from the group consisting of methylene methane disulfonate and ethylene sulfate, and lithium difluorophosphate.
[0029] In typical embodiments, the main solvent in the electrolyte is one of ethylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, dimethyl carbonate, propylene carbonate, diethyl carbonate, or methyl acetate. However, generally, the electrolyte contains a mixture of several of these solvents and / or other solvents. In the exemplary embodiment shown in the following experimental example, the electrolyte contains a mixture of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate. The main lithium salt in the electrolyte is one of LiPF6, LiBF4, lithium bis(oxalato)borate, and lithium difluoro(oxalato)borate. In the exemplary embodiment shown in the following experimental example, the electrolyte contains a LiPF6 salt. However, here again, the electrolyte may contain several such salts.
[0030] A suitable additive mixture for use in progressive electrolytes contains vinylene carbonate and / or fluoroethylene carbonate. For clarity, the main non-aqueous solvent in the electrolyte is different from the additive solvent and therefore neither vinylene carbonate nor fluoroethylene carbonate. Furthermore, again for clarity, the main lithium salt is different from lithium difluorophosphate.
[0031] The aforementioned components in this additive mixture may have been proposed for use in the prior art, either individually or in smaller subcombinations, but each use brings certain undesirable drawbacks or disadvantages. However, the inventors have found that this selection of components unexpectedly provides performance advantages without the unacceptable trade-offs seen in the prior art additive mixtures.
[0032] In particular, embodiments in which the electrolyte comprises an additive solvent between 0.1% and 5% by weight, a sulfur-containing compound between 0.1% and 3% by weight, and lithium difluorophosphate between 0.1% and 5% by weight, benefit the present invention. Furthermore, the additive mixture may optionally contain a sultone compound (e.g., 1,3-propenesultone) in an amount of 0% to 2% by weight to obtain additional beneficial results.
[0033] Recently, there are numerous available options for components that can be used in rechargeable batteries in general, particularly lithium-ion batteries, and these are well known to those skilled in the art. Furthermore, numerous structures or designs (including coin-type, cylindrical, and prismatic embodiments), along with manufacturing methods well known to those skilled in the art, are available for such batteries. Based on this disclosure and the following experimental examples, it is expected that those skilled in the art will be able to readily make appropriate selections regarding the types and amounts of components to be used in progressive additive mixtures to suit a given application in such non-aqueous rechargeable batteries.
[0034] The electrolyte of the present invention has been demonstrated to provide excellent performance advantages in rechargeable lithium-ion batteries. Generally, such batteries include a cathode electrode, an anode electrode, and a non-aqueous battery electrolyte, where both electrodes are lithium-inserted compounds and the electrolyte includes the non-aqueous electrolyte outlined above. A typical cathode electrode material is of the formula Li x M yIt contains one or more compounds with Oz. Here, 0≦x,y≦2, 2≦z≦4, and M contains one or more of the following elements: Ni, Al, Mn, Co, Fe, P, Mg, Ti, Zr, Ga, Cr, Ru. To obtain functional benefits known to those skilled in the art, these cathode materials may optionally have a surface coating applied thereto. Typical anode electrode materials contain carbonaceous compounds, preferably graphite, but coke and disordered carbon are also acceptable.
[0035] However, in particular, the electrolyte of the present invention has been specifically demonstrated to address problems encountered when high-voltage cathodes are used in such batteries (for example, cathodes containing nickel-containing lithium transition metal oxide materials such as lithium nickel manganese cobalt oxide materials having a stoichiometry of LiNi 0.6 Mn 0.2 Co 0.2 O2). Such batteries typically feature a maximum operating voltage limit of 4.2V or higher. Therefore, the use of the additive mixture of the present invention corresponds to a method of improving the lifespan, specifically, a method of improving the cycle life and stability of such high-voltage rechargeable lithium-ion batteries.
[0036] The present selection of components in the additive mixture of the present invention has been experimentally found to provide such possible improvements without significantly or adversely affecting other performance aspects of rechargeable lithium batteries unexpectedly. This is clearly demonstrated in the following experimental examples for additive mixtures containing VC. And as is well known to those skilled in the art, FEC is not only chemically similar to VC but has also been shown to function similarly to VC in other prior art embodiments. Therefore, it would be expected that FEC can be used in place of VC in the present invention.
[0037] The following experimental examples illustrate certain aspects of the present invention, but should not be interpreted as limiting the invention. Those skilled in the art will readily understand that batteries other than high-voltage rechargeable lithium-ion batteries can also enjoy certain advantages by using the electrolyte of the present invention.
[0038] [Example of experiment] Preparation and analysis methods Several series of experimental lithium-ion batteries were fabricated and tested using various electrolytes to determine and compare the performance results obtained with the electrolyte of the present invention and other conventional or prior art electrolytes. In all cases, the batteries used were individual pouch cells fabricated in an in-house pilot manufacturing facility using commercially available materials. The cathode electrode was 19.4 ± 0.4 mg·cm². -2 During loading, it is coated onto an aluminum foil substrate, with a weight of 3.3±0.1 g·cm². -3 Compressed to a density of approximately LiNi 0.6 Mn 0.2 Co 0.2 The anode electrode was fabricated using the single crystal "NMC622" (EASpring ME6SC), a lithium nickel manganese cobalt oxide with O2 stoichiometry. -2 Coated with loading, 1.55±0.03g·cm -3 These cells were fabricated from synthetic graphite (Kaijin AML400) compressed to a specific density. The cells were assembled with an anode-to-cathode capacitance ratio of 1.08 and a nominal capacitance of approximately 300mAh balanced for 4.4V operation.
[0039] The test electrolytes were mixed in-house in a glove box (MBraun) filled with argon. The electrolyte in all cells contained 1.2 M LiPF6 (Soulbrain) in a solvent mixture (Capchem) consisting of ethylene carbonate ("EC"), ethyl methyl carbonate ("EMC"), and dimethyl carbonate ("DMC") in a mass ratio of 25 wt% EC:5 wt% EMC:70 wt% DMC (hereinafter referred to as "25EC:5EMC:70DMC"). Additive mixtures were added thereto according to the weight percentage of the total electrolyte and included vinylene carbonate ("VC", Capchem), methylene methane disulfonate ("MMDS", TCI Chemicals), ethylene sulfate ("DTD", Capchem), also known as 1,3,2-dioxathiolane-2,2-dioxide, and lithium difluorophosphate ("LFO", Capchem). In this specification, cells are indicated according to abbreviated names that describe the weight percentage of additive components in a particular cell (for example, "2VC 1MMDS" refers to a test cell using a 1.2M LiPF625EC:5EMC:70DMC electrolyte containing an additive mixture of 2 wt% VC and 1 wt% MMDS). In some cases, certain test cells contained a solvent mixture containing methyl acetate ("MA", Capchem) in a mass ratio of 20MA:80 (25EC:5EMC:70DMC). Such cells include "20MA" in their abbreviated name (e.g., "2VC 1MMDS 20MA"). Furthermore, in some cases, certain test cells contained an amount of additive components less than 1%. In this case, "05MMDS" indicates 0.5 wt% MMDS, "05DTD" indicates 0.5 wt% DTD, and so on.
[0040] Before filling with electrolyte, the cells were dried overnight in a vacuum oven at 90°C. Then, in a drying chamber (dew point <-55°C), 1.20 ± 0.05 g of electrolyte was filled using a pipette and placed under vacuum at -90 kPa for 30 seconds to remove trapped air from the electrode stack and moisten the electrodes. The cells were then transferred to a vacuum sealer (MSK-115, MTI Corporation) and sealed at 165°C for 5 seconds.
[0041] Next, the mass of each cell while suspended in water was measured using a precision digital balance with a hook attached to the bottom. Open-circuit voltage ("OCV") and AC impedance ("ACR," 10mA (<300mΩ) or 1mA (<3Ω) at 1kHz+ / -0.2Hz) were also measured using a Hioki 3561 HiTester (Hioki).
[0042] Next, a mechanical pressure of approximately 20–30 psi was applied to each cell by clamping it between the surface of the metal plate and a metal shim using toggle clamps attached to the plate.
[0043] Next, the cells were subjected to a conditioning protocol in a test chamber at 40.0 ± 0.1°C while connected to a Novonix 2A 5V High Precision Charging system (Novonix) or a Neware BTS 4000 tester (Neware). The conditioning protocol consisted of the following steps: holding a constant voltage ("CV") at 1.5V for 24 hours, charging to 4.3V at C / 20, discharging to 2.8V at C / 20, charging to 4.3V at C / 20, OCV for 48 hours, and discharging to 3.8V at C / 20. [By conventional usage, C / 20 as used herein refers to the charging and discharging rates equivalent to obtaining the cell's nominal maximum capacity in 20 hours.]
[0044] After conditioning, the mass of each cell suspended in water, their OCV and ACR were measured again. The difference in mass suspended in water before and after conditioning is equal to the change in cell volume based on Archimedes' principle and is reported below as the volume of gas produced during conditioning. Next, the cells were cut open in a drying chamber to release the gas produced during conditioning and then resealed using the same sealing procedure as above. Then, the weight of the cells was measured again in water to calculate the gas volume after the cycle test. Next, the cells were clamped again as above and subjected to various electrochemical tests, which are described in detail below. These electrochemical tests include long-term cycle ("LTC"), high-precision coulometry ("HPC"), rate test cycle ("RTC"), and storage test ("ST").
[0045] Long-term cycle: The cell for LTC testing was placed in a temperature chamber at 40.0 ± 0.1°C and connected to a Neware BTS4000 cycler. The cell underwent a protocol that included the following steps. 1. Charge to 4.3V using C / 20. 2. Discharge to 2.8V using C / 20. 3. Charge to 4.3V using C / 20. 4. Discharge to 2.8V with C / 20. 5. Charge to 4.3V with C / 5, and maintain a constant voltage (CV) of 4.3V until the current reaches C / 20. 6. Discharge to 2.8V using C / 2. 7. Repeat steps 5-7 (50 times) 8. Charge to 4.3V with C / 5, and maintain CV at 4.3V until the current reaches C / 20. 9. Return to Step 2 (until the experiment is complete).
[0046] High-precision coulometry: The cell for HPC testing was placed in a temperature chamber at 40.0±0.1℃ and connected to a Novonix 5V2A High Precision Charger. The cell underwent a protocol that included the following steps. 1. Discharge to 2.8V with C / 10. 2. Charge to 4.3V using C / 10. 3. Discharge to 2.8V with C / 10. 4. Repeat from step 2 (24 times)
[0047] Rate testing cycle: The cells for RTC testing were placed on a shelf at 21.5±0.5℃ and connected to a Neware BTS4000 cycler. The cells underwent a protocol that included the following steps. 1. Charge to 4.3V using C / 20. 2. Discharge to 2.8V using C / 20. 3. Charge to 4.3V using C / 20. 4. Discharge to 2.8V with C / 20. 5. Charge with C / 2 up to 4.3V, and maintain CV at 4.3V until the current reaches C / 20. 6. C / 2 discharge 7. Repeat steps 5-6 (10 times) 8. Repeat steps 1-4. 9. Charge at 1C up to 4.3V, and maintain CV at 4.3V until the current reaches C / 20. 10. 1C discharge 11. Repeat steps 9-10 (10 times) 12. Repeat steps 1-4. 13. Charge at 2C up to 4.3V, and maintain CV at 4.3V until the current reaches C / 20. 14. 2C discharge 15. Repeat steps 13-14 (10 times) 16. Repeat steps 1-4. 17. Charge at 3C until 4.3V, then maintain CV at 4.3V until the current reaches C / 20. 18. Discharge at 3C. 19. Repeat steps 17-18 (10 times) 20. Repeat steps 1-4.
[0048] Storage test: The cell for ST testing was placed in a temperature chamber at 40.0±0.1℃ and connected to a Novonix 5V2A High Precision Charger. The cell underwent a protocol that included the following steps. 1. Charge to 4.3V using C / 20. 2. Discharge to 2.8V using C / 20. 3. Charge to 4.3V using C / 20. 4. 12 hours of CV at 4.3V 5. Immediately transfer the cell to a temperature chamber at 60.0 ± 0.1°C. 6. Leave it in OCV for 500 hours.
[0049] Experiment 1: Performance of incremental additive mixtures Cells were fabricated and tested with various electrolytes, including additive-free electrolytes (i.e., 25EC:5EMC:70DMC), 2VC, 2VC 1LFO, 2VC 1MMDS, and 2VC 1MMDS 1LFO electrolytes. Furthermore, cells were fabricated and tested with 2VC 1LFO 20MA, 2VC 1MMDS 20MA, and 2VC 1MMDS 1LFO 20MA electrolytes. The cells underwent HPC, LTC, and RTC testing following defined conditioning protocols.
[0050] Table 1 shows the first-cycle Coulomb efficiency "FCCE" (i.e., first-discharge capacity divided by first-charge capacity) during conditioning. Higher FCCE typically means that a more robust solid electrolyte interface "SEI" layer has been formed, resulting in fewer side reactions during the first cycle at the anode, cathode, or both. The results in Figure 1 show that adding each additive to the electrolyte has a beneficial cumulative effect on FCCE. Higher FCCE also means that the cell completes conditioning at a more accessible capacity at the start of its service life cycle. Using 2VC 1MMDS 1LFO yielded the highest FCCE among the additive mixtures, including when MA was added to the electrolyte, suggesting that the three-component additive mixture provides better protection of the anode and cathode from parasitic reactions than the two-component combinations of 2VC 1MMDS and 2VC 1LFO.
[0051] The results in Table 1 show that the addition of MMDS and LFO does not significantly affect the gases generated during conditioning compared to 2VC, and that the addition of MMDS to the 2VC 1MMDS 1LFO mixture suppresses the excess gases generated in 2VC 1LFO.
[0052] Table 1 also shows the voltage drop during the 48-hour OCV step (step 5) during conditioning. The reaction at the NMC cathode causes a cell voltage drop due to the oxidation reaction of the electrolyte at high voltage (4.3V). A small OCV drop indicates a lower degree of electrolyte oxidation because the SEI layers on the anode and cathode are more robust. Some electrolyte oxidation may occur if reaction products from the anode reaction move through the electrolyte and cause crosstalk reactions. A decrease in OCV voltage drop may also suggest the formation of a more robust anode SEI. Using VC significantly reduces the voltage drop compared to cells without additives. The results in Table 1 show that the voltage drop can be further reduced when MMDS is combined with VC. However, the voltage drop is minimized when LFO is added to VC, or to VC with MMDS. When combined with MA, 2VC 1MMDS 1LFO 20MA performs better than both 2VC 1MMDS 20MA and 2VC 1LFO 20MA. This suggests that the unique combination of three components produces a stronger reduction in parasitic reactions at the cathode compared to other mixtures.
[0053] [Table 1]
[0054] Note: The results shown are the average of 2-3 cells produced from the same batch of ingredients. The drift and fade results are accumulated from cycle 5 to 28 due to the power interruption in cycle 4.
[0055] Figures 1 and 2 show the results of LTC tests for representative cells without MA in the additive mixture (i.e., no additive, 2VC, 2VC 1LFO, 2VC 1MMDS, and 2VC 1MMDS 1LFO), illustrating the improvement in LTC observed when additives are incrementally added to the electrolyte. Figure 1 plots the normalized cell volume, and Figure 2 plots Delta V against the number of cycles. As shown in Figure 1, performance improved after each additive component (VC, MMDS, LFO) was added to the cell. The cell containing the 2VC 1MMDS 1LFO electrolyte lost 10% of its volume in approximately 1000 cycles, showing the best volume retention compared to the 2VC 1MMDS and 2VC 1LFO cells which lost the same volume in 800 cycles, the 2VC cell which lost the same volume in 600 cycles, and the no-additive cell which lost the same volume in 400 cycles. At the fade rate of the last 500 cycles, the 2VC 1MMDS 1LFO cell reached 80% of its capacity at approximately 4200 cycles. Figure 2 shows Delta V (average charge voltage - average discharge voltage), representing the impedance increase rate within the cell, with the slope indicating the impedance increase rate. Cells without additives had the largest impedance increase rate, while the 2VC 1MMDS 1LFO cell and the 2VC 1LFO cell had the slowest impedance increase. The results suggest that cells containing 2VC 1MMDS 1LFO have a much longer lifespan than those containing other electrolytes due to the protective properties of the SEI formed on the electrodes.
[0056] Table 1 also shows a summary of the HPC test results after 28 charge-discharge cycles. Coulomb efficiency "CE" is expressed as the discharge capacity divided by the previous charge capacity. A higher CE indicates a more stable chemical property of the cell. The 2VC 1MMDS 1LFO cell had the highest CE, and adding MA to the cell resulted in a higher CE than the 2VC 1LFO cell. The slippage of the cumulative charge endpoint capacity (referred to as "slippage" in Table 1, representing the degree to which the cumulative capacity changes after repeated cycles as a result of parasitic reactions and other losses) can indicate the stability of the cell against electrolyte oxidation reactions. The HPC slippage is consistent with the results of the conditioned OCV and LTC, indicating that the amount of electrolyte oxidation reaction that occurs is much less when using 2VC 1MMDS 1LFO. The capacity "fade" indicates the amount of capacity loss since the start of the HPC test (cycle 5 of Experiment 1). The difference in capacity fade was not as dramatic as the slippage value in the HPC test. The 2VC 1MMDS 1LFO cell showed greater capacity fade than the 2VC 1LFO and 2VC 1MMDS cells, despite higher CE and drift results. This may be due to a more stable drift rate per cycle, which does not affect CE but may alter the rate of observed capacity fade.
[0057] Table 1 also shows the summarized results of the RTC test. After 10 cycles each of CCCV charge and CC discharge cycles at C / 2, 1C, 2C, and 3C at room temperature, two C / 20 CC cycles were performed. Table 1 shows the discharge capacities of the second C / 20 cycle (step 16) after the 2C rate test and the second C / 20 cycle (step 20) after the 3C rate test, normalized to the second C / 20 cycle (step 4) of the RTC test. Any differences correspond to capacity lost due to electrode active material loss or lithium metal plating in the cell, due to the rate limits of the material, SEI, and electrolyte. Table 1 shows that adding 1LFO to 2VC degrades rate performance, while adding 1MMDS improves rate performance. In combination, the 2VC 1MMDS 1LFO cell achieved better rate capability than the 2VC 1LFO cell, especially after the 3C cycle, and maintained 91.4% capacity throughout the RTC protocol. When MA was added to the electrolyte, the 2VC 1MMDS 1LFO 20MA cell showed performance similar to that of cells with 2VC 1MMDS 20MA and 2VC 1MMDS 1LFO 20MA, maintaining 94.3% capacity throughout the entire RTC protocol.
[0058] Figure 3a shows the LTC capacity retention rate (nominal capacity as a percentage of cycles) for cells with electrolytes that do not contain LFO, and Figure 3b shows the capacity retention rate for cells with electrolytes that contain LFO, highlighting the effect of MA in long-term cycles. Figures 4a and 4b plot the delta-V of the same cell group, respectively. Figures 3a and 4a show that a 2VC 1MMDS additive mixture containing 20MA is effective in mitigating the impedance increase typically associated with MA addition during long-term high-voltage cycles. Figures 3b and 4b show that cells containing 2VC 1LFO 20MA have faster capacity loss and increased delta-V (impedance increase), suggesting that MMDS is more effective than LFO in protecting the cathode from electrolyte oxidation. However, cells containing 2VC 1MMDS 1LFO 20MA exhibit the best overall capacitance retention and lowest impedance increase, demonstrating a dramatic improvement compared to 2VC 1MMDS 20MA and especially the 2VC 1LFO 20MA additive mixture, and further demonstrating a favorable synergistic effect in the VC-MMDS-LFO additive mixture.
[0059] Experiment 2: Performance comparison of sulfur-containing additives In Experiment 2, the same tests as in Experiment 1 were performed on cells with the same electrolyte but containing different sulfur-containing compounds in the additive mixture. Cells containing 2VC, 2VC 1PS, 2VC 1PS 1LFO, 2VC 0.5MMDS, 2VC 0.5MMDS 1LFO, 2VC 1DTD, 2VC 1DTD 1LFO, 2VC 1PES, and 2VC 1PES 1LFO were prepared and tested. The results of these tests are summarized in Table 2.
[0060] Table 2 shows that in all additive mixtures including PS, MMDS, DTD, and PES, the addition of LFO increased FCCE and reduced the cell voltage drop. In all cases except the 2VC 1PES 1LFO cell, which had very low gas generation during conditioning, the addition of LFO increased gas during conditioning. The 2VC 1DTD 1LFO cell had a large amount of gas during conditioning. Experiment 3 below demonstrates the effect of combining PES with MMDS and DTD to reduce gas generation during conditioning.
[0061] Table 2 also shows that the 2VC 0.5MMDS 1LFO cell and the 2VC 1DTD 1LFO cell had the best CE in the HPC test, and also exhibited low levels of both drift and fade.
[0062] In RTC testing, cells containing all additive mixtures without LFO performed well up to 3C cycles, achieving at least 94.2% (2VC 1PS) to a maximum of 97.3% (2VC 1DTD) of the original cell capacity at C / 20 after 3C cycles. However, with the addition of LFO, the 2VC 1PS 1LFO cell and the 2VC 1PES 1LFO cell lost significant capacity after 2C cycles (88.1% and 74.2%, respectively) and after 3C cycles (75.5% and 65%, respectively). The 2VC 0.5MMDS 1LFO cell achieved 96.6% and 91.1% after 2C and 3C cycles, respectively, while the 2VC 1DTD 1LFO cell achieved 96.4% and 91.3%. The dramatic improvement in rate performance indicates a further favorable and remarkable synergy between VC, MMDS / DTD, and LFO.
[0063] Figure 5 shows the ST test results for cells containing 2VC, 2VC 1PS 1LFO, 2VC 1MMDS 1LFO, 2VC 1DTD 1LFO, and 2VC 1PES 1LFO electrolytes. The voltage drop during the 500-hour OCV, 60°C test indicates the cell's stability against electrolyte oxidation at the cathode. The advantage of the sulfur-containing additive component in the additive mixture is clear, as VC alone exhibits a rapid voltage drop and a very high reaction rate. The sulfur-containing additive creates a robust SEI on the cathode surface that protects against electrolyte oxidation. Figure 5 also demonstrates that the 2VC 1MMDS 1LFO cell had the lowest voltage drop during the high-temperature storage test, followed by the 2VC 1PES 1LFO and 2VC 1DTD 1LFO cells.
[0064] [Table 2]
[0065] Note: The displayed results are the average of 2-3 cells produced from the same batch of ingredients. Shift and fade results are accumulated over cycles 1-24.
[0066] Experiment 3: Gas reduction during conditioning In Experiment 3, PES was combined with DTD-containing additive mixtures and MMDS-containing additive mixtures to reduce the amount of gas generated in the cell during conditioning. Cells containing 1VC, 1VC 1PES 1LFO, 1VC 1MMDS 1LFO, 1VC 0.5MMDS 0.5PES 1LFO, 1VC 1DTD 1LFO, and 1VC 0.5DTD 0.5PES 1LFO were prepared and tested. The results of these tests are summarized in Table 3.
[0067] The results in Table 3 show that replacing 1MMDS with 0.5MMDS and 0.5PES in the additive mixture resulted in a 48% gas reduction. Using 0.5PES and 0.5DTD instead of 1DTD resulted in a dramatic 72% gas reduction.
[0068] Replacing MMDS or DTD with PES in the VC-MMDS / DTD-LFO three-component additive mixture not only reduces voltage drop and FCCE, but also significantly reduces gas during conditioning, suggesting equivalent or superior HPC and LTC performance. However, based on the results obtained in Experiment 2, a decrease in rate capability is expected. However, these tests were not performed in Experiment 3.
[0069] [Table 3]
[0070] Note: The results shown are the average of 2-3 cells produced from the same batch of ingredients.
[0071] All of the above-mentioned U.S. patents, U.S. patent applications, foreign patents, foreign patent applications, and non-patent publications referenced herein are incorporated herein by reference in their entirety.
[0072] While specific elements, embodiments, and applications of the present invention have been shown and described, those skilled in the art will naturally understand that the present invention is not limited thereto, as modifications can be made without departing from the spirit and scope of this disclosure, particularly in light of the teachings set forth herein. For example, while the examples focus on additive mixtures containing VC, similar advantages are expected to be obtained by using fluoroethylene carbonate instead. Such modifications should be considered within the scope and authority of the claims appended herein.
Claims
1. 1. A non-aqueous battery electrolyte comprising a primary lithium salt, a primary non-aqueous solvent, and less than 10 wt. % of an additive mixture, The additive mixture comprises: an additive solvent comprising vinylene carbonate ("VC"); a sulfur-containing compound comprising methylenemethane disulfonate ("MMDS"); and lithium difluorophosphate ("LFO"); the electrolyte solution comprises between 0.1% and 5% by weight of the additive solvent; the electrolyte comprises between 0.1% and 3% by weight of the sulfur-containing compound; 13. A non-aqueous battery electrolyte, the electrolyte comprising between 0.1% and 5% by weight lithium difluorophosphate.
2. The main lithium salt is LiPF 6 , LiBF 4 10. The electrolyte of claim 1 comprising at least one salt selected from the group consisting of lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, and lithium bis(oxalato)borate.
3. The main lithium salt is LiPF 6 The electrolyte solution according to claim 2 , 4. The electrolyte of claim 1, wherein the primary lithium salt is different from lithium difluorophosphate.
5. The electrolyte of claim 1, further comprising sultone.
6. The electrolyte of claim 1, wherein the sulfur-containing compound is MMDS.
7. The electrolyte of claim 1, wherein the primary non-aqueous solvent comprises ethylene carbonate ("EC"), ethyl methyl carbonate ("EMC"), and dimethyl carbonate ("DMC") in a mass ratio of 25 wt.% EC:5 wt.% EMC:70 wt.% DMC.
8. The electrolyte of claim 1, wherein the sulfur-containing compound comprises ethylene dithiothreitol ("DTD").
9. 13. A high voltage rechargeable lithium ion battery comprising a cathode electrode, an anode electrode, and the nonaqueous battery electrolyte of claim 1.
10. The cathode electrode has the formula Li x M y O z Compounds having the formula: In the formula, 0≦x, y≦2, and 2≦z≦4; 10. The lithium ion battery of claim 9, wherein M comprises one or more of the elements Ni, Al, Mn, Co, Fe, P, Mg, Ti, Zr, Ga, Cr, Ru.
11. The cathode electrode is about LiNi 0.6 Mn 0.2 Co 0.2 O 2 11. The lithium ion battery of claim 10 comprising lithium nickel manganese cobalt oxide having a stoichiometry of:
12. 10. The lithium ion battery of claim 9, wherein the maximum operating voltage limit of the battery is 4.2 V or greater.
13. 10. The lithium ion battery of claim 9, wherein the anode electrode comprises graphite.
14. 1. A method for improving the cycle life and stability of a high voltage rechargeable lithium ion battery comprising a cathode electrode, an anode electrode, and a non-aqueous electrolyte, the electrolyte comprising a primary lithium salt and a primary non-aqueous solvent, comprising: the method comprising providing less than 10% by weight of an additive mixture in the electrolyte; The additive mixture comprises: an additive solvent comprising vinylene carbonate ("VC"); a sulfur-containing compound comprising methylenemethane disulfonate ("MMDS"); and lithium difluorophosphate ("LFO"); the electrolyte solution comprises between 0.1% and 5% by weight of the additive solvent; the electrolyte comprises between 0.1% and 3% by weight of the sulfur-containing compound; The method of claim 1, wherein the electrolyte comprises between 0.1% and 5% by weight lithium difluorophosphate.
15. The method of claim 14, wherein the sulfur-containing compound is MMDS.
16. The method of claim 14, wherein the primary lithium salt is LiPF 6 .
17. The method of claim 14, wherein the additive mixture comprises 2 wt.% VC, 1 wt.% MMDS, and 1 wt.% LFO.
18. The method of claim 14, further comprising a sultone.
19. The method of claim 14, wherein the additive mixture comprises 2 wt.% VC, 0.5 wt.% MMDS, and 1 wt.% LFO.
20. The method of claim 14, wherein the primary non-aqueous solvent comprises ethylene carbonate ("EC"), ethyl methyl carbonate ("EMC"), and dimethyl carbonate ("DMC") in a mass ratio of 25 wt% EC:5 wt% EMC:70 wt% DMC.
21. The method of claim 14, wherein the sulfur-containing compound comprises ethylene diamine sulphate ("DTD").