Lithium ion secondary battery, assembly for preparing lithium ion secondary battery, preparation method and electric device

By setting up a multi-layer structure of the negative electrode active material layer in the negative electrode sheet of the lithium-ion secondary battery and performing negative electrode lithium supplementation treatment, the problem of insufficient cycle life and battery life of the lithium-ion secondary battery is solved by using the fast-embedded lithium material. Achieve higher lithium embedded rate and lithium supplement efficiency, extending battery life and improving energy density and kinetic performance.

CN119069644APending Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411566361.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The cycle life and battery life of existing lithium-ion secondary batteries are insufficient, making it difficult to meet high-demand application scenarios.

Method used

By providing a multi-layer structured negative electrode active material layer in the negative electrode sheet, including the first negative electrode active layer and the second negative electrode active layer, and performing negative electrode lithium supplementation treatment on its surface, fast-embedded lithium materials such as artificial graphite and hard carbon are used to use. , soft carbon, silicon oxide and silicon carbon composites, improve lithium embedded rate and lithium replenishment efficiency, and extend battery life.

Benefits of technology

It significantly improves the cycle life and battery life of lithium-ion secondary batteries, reduces the enrichment of lithium ions on the surface of the negative electrode active material and lithium-ion production, and improves the energy density and kinetic performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069644A_ABST
    Figure CN119069644A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium ion secondary battery, a component for preparing the lithium ion secondary battery, a preparation method and an electric device. The lithium ion secondary battery comprises a positive pole piece, a negative pole piece, an isolating membrane and electrolyte, wherein the isolating membrane is arranged between the positive pole piece and the negative pole piece; the negative electrode plate comprises a negative electrode current collector, and a second negative electrode active layer and a first negative electrode active layer which are sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active layer comprises a first negative electrode active material, and the second negative electrode active layer comprises a second negative electrode active material; the lithium intercalation rate of the first negative electrode active material is higher than that of the second negative electrode active material, and the negative electrode plate is subjected to negative electrode lithium supplementing treatment. The lithium ion secondary battery has a significantly improved cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion secondary batteries, and further to a lithium-ion secondary battery, a component for preparing the same, a preparation method and an electrical device. Background Art

[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0003] With the development of lithium-ion secondary battery technology, lithium-ion batteries are widely used in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields, and are also widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations. The demand for the cycle life and endurance of lithium-ion secondary batteries is also increasing. Summary of the invention

[0004] According to various embodiments and examples of the present application, the present application provides a lithium ion secondary battery, a component for preparing the same, a preparation method and an electric device. The lithium ion secondary battery has a significantly improved cycle life.

[0005] In a first aspect of the present application, a lithium ion secondary battery is provided.

[0006] In some embodiments, a lithium-ion secondary battery is provided, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the separator is arranged between the positive electrode plate and the negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the negative electrode plate is treated with negative lithium supplementation.

[0007] In the present application, unless otherwise specified, in a lithium-ion secondary battery, "the negative electrode plate has been treated with negative electrode lithium supplementation" means that "the negative electrode plate includes lithium pre-embedded by negative electrode lithium supplementation", which means that the negative electrode plate of the lithium-ion secondary battery has been treated with negative electrode lithium supplementation, so that the negative electrode plate includes not only the lithium embedded in the negative electrode during the formation process, but also the lithium additionally introduced by the negative electrode lithium supplementation treatment. During the negative electrode lithium supplementation process, the lithium supplementation material carried by the negative electrode plate releases active lithium ions, and the released active lithium ions are embedded in the negative electrode active material, thereby obtaining a negative electrode plate treated with negative electrode lithium supplementation, and the lithium embedded in the negative electrode during the negative electrode lithium supplementation process can be called "pre-embedded lithium"; after the negative electrode plate treated with negative electrode lithium supplementation is introduced into the lithium-ion secondary battery, the negative electrode plate can release the pre-embedded lithium during the charge and discharge process of the lithium-ion secondary battery, thereby replenishing the lithium continuously consumed by the battery system. Compared with the case where the negative electrode plate has not been treated with lithium supplementation, the lithium-ion secondary battery provided in the first aspect of the present application has a significantly extended cycle life.

[0008] In the present application, unless otherwise specified, the negative electrode lithium replenishment material used in the negative electrode lithium replenishment treatment process undergone by the negative electrode pole piece is provided by the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer, that is, "the negative electrode pole piece undergoes negative electrode lithium replenishment treatment" means that the negative electrode pole piece undergoes lithium replenishment treatment with the lithium replenishment layer located on the surface of the first negative electrode active layer away from the second negative electrode active layer; accordingly, "the negative electrode pole piece includes lithium pre-embedded by negative electrode lithium replenishment" means that the negative electrode pole piece includes lithium pre-embedded by the lithium replenishment treatment of the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0009] In this application, unless otherwise specified, "lithium insertion rate (rate)" can reflect the amount of lithium inserted per unit time, and "lithium replenishment efficiency (efficiency)" can reflect the ratio of the amount of lithium inserted effectively into the negative electrode active material to the total amount of lithium supplied by the negative electrode lithium replenishment material. The lithium replenishment efficiency of the negative electrode active material is mainly related to factors such as the lithium insertion potential and gram capacity of the negative electrode active material. The "lithium insertion potential" of the negative electrode active material indicates the potential difference for the insertion and extraction of lithium ions in the negative electrode active material, which can reflect the ease of lithium ion insertion. The "gram capacity" of the negative electrode active material can reflect the ability of the negative electrode active material to store and release lithium ions.

[0010] In some embodiments, a lithium-ion secondary battery is provided, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the separator is arranged between the positive electrode plate and the negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the lithium insertion rate of the first negative electrode active material is higher than the lithium insertion rate of the second negative electrode active material, and the negative electrode plate is subjected to negative electrode lithium supplementation treatment.

[0011] By arranging a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer (the direction away from the surface of the negative electrode current collector is regarded as the upper layer, and the direction toward the surface of the negative electrode current collector is regarded as the lower layer) on the negative electrode active layer of the negative electrode plate, the first negative electrode active material located on the upper layer can further have a higher lithium insertion rate, which is beneficial for the active lithium ions provided by the negative electrode lithium replenishing material to be efficiently embedded in the first negative electrode active layer, which can reduce the probability of active lithium being deactivated due to lack of time to be embedded, and can significantly improve the lithium replenishment efficiency; thereby, a negative electrode plate treated with efficient negative electrode lithium replenishment can be obtained, and the negative electrode plate includes lithium pre-embedded by negative electrode lithium replenishment through the lithium replenishing layer. By introducing the aforementioned negative electrode plate that has undergone high-efficiency negative electrode lithium replenishment treatment into a lithium-ion secondary battery, the higher lithium replenishment efficiency is conducive to storing more lithium in the negative electrode, thereby permanently replenishing active lithium and continuously replenishing capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is conducive to reducing the enrichment of lithium ions on the surface of the negative electrode active material, which in turn is conducive to reducing the generation of lithium plating; through the synergy of the aforementioned multiple effects, the lithium-ion secondary battery can have a significantly improved cycle life.

[0012] The effects described in any part of this application are not intended to be limited by any theory.

[0013] The lithium insertion potential of natural graphite is usually lower than that of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon carbon composite. The specific capacity of natural graphite is usually lower than that of hard carbon, soft carbon, silicon oxide and silicon carbon composite. The lithium insertion potential of natural graphite is usually low, for example, it can be between 0.01V ~ 0.2 V vs. Li / Li +Within this range, natural graphite has structural defects and uneven surface morphology, which leads to anisotropy in the diffusion of lithium ions, making the overall lithium replenishment efficiency of natural graphite relatively low. The lithium insertion potential of artificial graphite can be slightly higher than that of natural graphite, and the gram capacity of artificial graphite may be slightly lower than that of natural graphite. However, the morphology and structure of artificial graphite are more regular than those of natural graphite, and the internal defects are relatively few, which makes the transmission of lithium ions more stable, and overall can achieve a faster lithium insertion rate than natural graphite. The lithium insertion potential of hard carbon is usually higher than that of natural graphite, and the capacity of hard carbon is also higher than that of natural graphite. The crystal arrangement inside hard carbon is disordered and there are many pores, which can provide abundant lithium insertion sites and fast transmission channels, and can provide a faster lithium insertion rate. The lithium insertion potential of soft carbon is also usually higher than that of natural graphite. The carbon layers in soft carbon are disorderly stacked, so that lithium ions can be transmitted relatively quickly in it. Soft carbon can provide a higher lithium insertion rate than natural graphite overall. The lithium insertion potential of silicon oxide and silicon-carbon composites is higher than that of natural graphite, and the capacity is much higher than that of natural graphite. The large amount of lithium insertion per unit time makes the lithium insertion rate of silicon oxide and silicon-carbon composites higher than that of natural graphite.

[0014] In summary, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite have higher lithium insertion rates than natural graphite. In this application, "artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite" can be collectively referred to as fast lithium insertion materials.

[0015] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0016] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite;

[0017] The negative electrode plate satisfies one or both of the following characteristics (t1) and (t2):

[0018] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0019] (t2) The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 The negative electrode sheet satisfies one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 ;

[0020] The negative electrode plate is treated with negative electrode lithium supplementation.

[0021] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0022] The first negative electrode active material and the second negative electrode active material independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material, and the negative electrode plate has been treated with negative electrode lithium supplementation.

[0023] By controlling the first negative electrode active material located in the upper layer to have a higher lithium insertion potential, it is beneficial to quickly embed active lithium ions into the first negative electrode active layer. When preparing the negative electrode plate, it is beneficial to embed more active lithium provided by the negative electrode lithium replenishment material into the first negative electrode active layer faster, which can reduce the probability of active lithium being deactivated due to lack of time to embed, and can significantly improve the lithium replenishment efficiency. By introducing the negative electrode plate treated with efficient negative electrode lithium replenishment into the lithium-ion secondary battery, more lithium can be stored in the negative electrode, thereby replenishing active lithium and continuously replenishing capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reducing the enrichment of lithium ions on the surface of the negative electrode active material, which is beneficial to reducing the generation of lithium precipitation; through the synergy of the aforementioned multiple effects, the lithium-ion secondary battery can have a significantly improved cycle life.

[0024] In some embodiments, the lithium insertion potential of the first negative electrode active material is 0.08 V to 0.5 V vs. Li / Li + , selectable from 0.1 V ~ 0.5 V vs. Li / Li + .

[0025] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0026] The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is 10 is higher than the proportion of the sum of the masses of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material. 20 , where f 10 >f 20 ≥0, or, f 10 ≥f 20 The sum of the mass of the hard carbon, the soft carbon, the silicon oxide and the silicon-carbon composite accounts for a proportion of the total mass of the first negative electrode active material. 19 is higher than the proportion of the sum of the masses of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material. 29 (That is, f 10 ≥f 20 And f 19 >f 29 );

[0027] The proportion of natural graphite in the total mass of the first negative electrode active material is 15 is lower than the proportion of natural graphite in the total mass of the second negative electrode active material 21 , where 0≤f 15 <f 21 ; or, 0≤f15 ≤f 21 The sum of the mass of the hard carbon, the soft carbon, the silicon oxide and the silicon-carbon composite accounts for a proportion of the total mass of the first negative electrode active material. 19 is higher than the proportion of the sum of the masses of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material. 29 (That is, 0≤f 15 ≤f 21 And f 19 >f 29 ).

[0028] In some embodiments, a lithium ion secondary battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet comprises a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector; the first negative electrode active layer comprises a first negative electrode active material, and the second negative electrode active layer comprises a second negative electrode active material;

[0029] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite;

[0030] The proportion of the sum of the masses of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is denoted as f. 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 ;

[0031] The negative electrode plate meets one or more of the following characteristics:

[0032] f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ;

[0033] 0≤f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 .

[0034] By controlling the first negative electrode active layer to have a higher sum of the mass fractions of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite (such as f 10 >f 20 ≥0), controlling the first negative electrode active layer located on the upper layer to have a lower natural graphite content (such as 0≤f 15 <f 21 ) and controlling the first negative electrode active layer to have a higher sum of the mass fractions of hard carbon, soft carbon, silicon oxide and silicon-carbon composite (such as f 10 ≥f 20 And f 19 >f 29 , or if 0≤f 15 ≤f 21 And f 19 >f 29 ) at least one control method is adopted to make the first negative electrode active layer contain more fast-insertion lithium materials and / or contain less natural graphite, so that the first negative electrode active layer can have a higher lithium insertion rate, and the lithium ions provided by the negative electrode lithium supplement material can be more efficiently embedded in the negative electrode, which is beneficial to improve the lithium supplement efficiency and improve the battery cycle life. As one of the exemplary theories, by making the first negative electrode active layer have a higher lithium insertion rate, it is beneficial to make the active lithium ions embed into the first negative electrode active layer faster and more, which can reduce the probability of active lithium being deactivated due to lack of time to embed, and can significantly improve the lithium supplement efficiency. By introducing the negative electrode pole piece treated with efficient negative electrode lithium supplement into the lithium ion secondary battery, the higher lithium supplement efficiency is beneficial to store more lithium in the negative electrode, so as to replenish the active lithium persistently and continuously replenish the capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reduce the enrichment of lithium ions on the surface of the negative electrode active material, which is beneficial to reduce the generation of lithium precipitation; through the synergy of the above-mentioned multiple effects, the lithium ion secondary battery can have a significantly improved cycle life.

[0035] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0036] 50%≤f 10 ≤100%, optionally, 80%≤f 10 ≤100%, further optionally, 90%≤f 10 ≤100%;

[0037] 50%≤f20 ≤100%, optionally, 80%≤f 10 ≤100%, further optionally, 90%≤f 10 ≤100%;

[0038] 0≤f 15 ≤50%, optionally, 0≤f 15 ≤30%, further optionally, 0≤f 15 ≤20%;

[0039] 0≤f 21 ≤50%, optionally, 1≤f 21 ≤30%, further optionally, 10≤f 21 ≤30%;

[0040] 0%≤f 19 ≤50%, optionally, 1%≤f 19 ≤40%, further optionally, 5%≤f 19 ≤30%;

[0041] 0%≤f 29 ≤50%, optionally, 0%≤f 29 ≤40%, further optionally, 1%≤f 29 ≤30%.

[0042] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0043] 80%≤f 10 ≤100%;

[0044] 80%≤f 20 ≤100%;

[0045] 0≤f 15 ≤30%;

[0046] 1≤f 21 ≤30%;

[0047] 1%≤f 19 ≤40%;

[0048] 0%≤f 29 ≤40%.

[0049] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0050] 90%≤f 10 ≤100%;

[0051] 90%≤f 20 ≤100%;

[0052] 0≤f 15 ≤20%;

[0053] 10≤f 21 ≤30%;

[0054] 5%≤f 19 ≤30%;

[0055] 1%≤ f29 ≤30%.

[0056] By adding f 10 、f 20 、f 15 、f 21 、f 19 、f 29 One or more parameters in are controlled within the aforementioned range, which is conducive to making the negative electrode sheet as a whole have a faster lithium insertion rate, which is conducive to better improving the lithium replenishment efficiency and better extending the battery cycle life. In some embodiments, the first negative electrode active material includes one or more of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite.

[0057] In some embodiments, the first negative electrode active material includes artificial graphite.

[0058] In some embodiments, the proportion of artificial graphite in the total mass of the first negative electrode active material is denoted as f. 11 , satisfying 50%≤f 11 ≤100%, optionally, 70%≤f 11 ≤95%.

[0059] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0060] The proportion of artificial graphite in the total mass of the first negative electrode active material is 11 Higher than the proportion of artificial graphite in the total mass of the second negative electrode active material 22 , where f 11 >f 22 ≥0;

[0061] The proportion of natural graphite in the total mass of the second negative electrode active material is 21 is higher than the proportion of natural graphite in the total mass of the first negative electrode active material 15 , where f 21 >f 15 ≥0.

[0062] By controlling the negative electrode to meet the 11 >f 22 ≥0 and f21 >f 15 One or both of ≥0 are beneficial to making the first negative electrode active layer have a higher lithium insertion rate, which is beneficial to better improve the lithium replenishment efficiency.

[0063] In some embodiments, the first negative electrode active material includes artificial graphite, and the negative electrode plate satisfies f 21 >f 15 ≥0 and f 21 >f 15 ≥ 0.

[0064] In some embodiments, the first negative electrode active material includes one or more of hard carbon, soft carbon, silicon oxide, and silicon-carbon composite.

[0065] In some embodiments, the first negative electrode active material includes artificial graphite and further includes one or more of hard carbon, soft carbon, silicon oxide, and silicon-carbon composite.

[0066] By introducing one or more of hard carbon, soft carbon, silicon oxide and silicon-carbon composite into the first negative electrode active layer, it is beneficial to make the first negative electrode active layer have a higher lithium insertion rate, which is beneficial to better improve the lithium replenishment efficiency and better extend the cycle life of the battery.

[0067] In addition, by giving the first negative electrode active layer a higher lithium insertion rate, it is also beneficial to improve battery kinetics.

[0068] In some embodiments, the ratio of the sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite to the total mass of the first negative electrode active material is recorded as f. 12 , satisfying 0 <f 12 ≤50%, optionally, 5%≤f 12 ≤30%.

[0069] In some embodiments, the first negative electrode active material further includes one or more of hard carbon and soft carbon.

[0070] In some embodiments, the first negative electrode active material includes one or more of artificial graphite, silicon oxide, and silicon-carbon composite, and the first negative electrode active material further includes one or more of hard carbon and soft carbon.

[0071] By introducing one or more of hard carbon and soft carbon into the first negative electrode active layer, the hard carbon and soft carbon have a higher interlayer spacing, which is conducive to the entry of lithium ions; the hard carbon and soft carbon not only have a higher lithium insertion rate, but also have higher conductivity. Therefore, it is not only beneficial to better improve the lithium replenishment efficiency and better extend the cycle life of the battery, but also beneficial to better improve the battery dynamics.

[0072] In some embodiments, the first negative electrode active material includes artificial graphite, and the first negative electrode active material further includes one or more of hard carbon and soft carbon.

[0073] In some embodiments, the ratio of the sum of the mass of the hard carbon and the soft carbon to the total mass of the first negative electrode active material is recorded as f. 13 , satisfying 0 <f 13 ≤50%, optionally, 10%≤f 13 ≤30%.

[0074] By calculating the sum of the mass of the hard carbon and the soft carbon in the total mass of the first negative electrode active material (f 13 ) is controlled within the aforementioned range, which is beneficial to taking into account the battery dynamics, lithium replenishment efficiency and first coulombic efficiency, and is beneficial to taking into account the battery dynamics, cycle life and actual energy density.

[0075] In some embodiments, the first negative electrode active material includes artificial graphite and further includes one or more of silicon oxide and silicon-carbon composite.

[0076] By introducing one or more of silicon oxide and silicon-carbon composite into the first negative electrode active layer, the capacity of silicon oxide and silicon-carbon composite is much higher than that of carbon-based materials, and they can alloy with negative electrode lithium replenishing materials more quickly, which is beneficial to better improve battery dynamics and lithium replenishment efficiency, and is also beneficial to improve energy density.

[0077] In some embodiments, the first negative electrode active material satisfies one or more of the following characteristics:

[0078] The proportion of the sum of the mass of silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is denoted as f 14 , satisfying 0 <f 14 ≤50%, optionally, 1%≤f 14 ≤30%, further optionally, 1%≤f 14 ≤15%;

[0079] The silicon-carbon composite comprises a porous carbon matrix and simple silicon located in the cavities of the porous carbon matrix.

[0080] The ratio of the sum of the mass of silicon oxide and silicon-carbon composite to the total mass of the first negative electrode active material (f 14 ) is controlled within the aforementioned range, which is beneficial to improving battery dynamics and lithium replenishment efficiency, and increasing the energy density of the negative electrode. In addition, it is also beneficial to suppress the reduction in the first coulombic efficiency and capacity attenuation caused by factors such as the volume expansion of silicon oxide and silicon-carbon composite under charge and discharge conditions.

[0081] By introducing silicon-carbon composites into the negative electrode active materials and designing a structure in which elemental silicon is loaded into porous carbon based on the silicon-carbon composite, the volume expansion of the negative electrode active materials and negative electrode sheets during the charge and discharge cycle is significantly suppressed, which can inhibit the generation of fresh interfaces and is beneficial to further extend the battery cycle performance.

[0082] In some embodiments, the first negative electrode active material includes coated negative electrode active particles, which include a first negative electrode active body and a coating layer located at least partially on the surface of the first negative electrode active body, and the coating layer includes one or more of soft carbon and hard carbon.

[0083] By providing a coating layer including one or more of soft carbon and hard carbon on the surface of the first negative electrode active material, a better lithium ion transmission channel can be provided for the first negative electrode active body, which is beneficial to promote lithium ion transmission, improve lithium replenishment efficiency, and further improve battery dynamics and cycle life.

[0084] In some embodiments, the coated negative electrode active particles satisfy one or more of the following characteristics:

[0085] The thickness of at least a portion of the coating layer is 1 nm to 10 nm, and may be 1 nm to 5 nm;

[0086] The average thickness of the coating layer is 1 nm to 10 nm, and can be optionally 1 nm to 5 nm;

[0087] The sum of the mass fractions of the soft carbon and the hard carbon in the coating layer in the coated negative electrode active particles is 0.5% to 10%, and can be optionally 1% to 4%;

[0088] The first negative electrode active body includes one or more of artificial graphite, silicon oxide and silicon-carbon composite; the proportion of the sum of the masses of artificial graphite, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active body is recorded as f 16 , satisfying 80%≤f 16 ≤100%, optionally, 90%≤f 16 ≤100%.

[0089] In some embodiments, the first negative electrode active body includes artificial graphite; the proportion of artificial graphite in the total mass of the first negative electrode active body is denoted as f 17 , satisfying 80%≤f 17 ≤100%.

[0090] In some embodiments, the second negative active material includes natural graphite.

[0091] By arranging natural graphite in the second negative electrode active layer located in the lower layer, lateral deformation is more likely to occur when the negative electrode plate is cold pressed, which is beneficial to provide improved compaction density and surface capacity, and further beneficial to improve energy density.

[0092] In some embodiments, the second negative electrode active material includes artificial graphite and natural graphite.

[0093] In some embodiments, the second negative electrode active layer satisfies one or more of the following characteristics:

[0094] The proportion of natural graphite in the total mass of the second negative electrode active material is denoted as f 21 , satisfying 0 <f 21 ≤50%, optionally, 10%≤f 21 ≤30%;

[0095] The proportion of artificial graphite in the total mass of the second negative electrode active material is denoted as f 22 , satisfying 50%≤f 22 <100%, optionally, 70%≤f 22 ≤90%.

[0096] By adjusting the ratio of natural graphite to the total mass of the second negative electrode active material (f 21 ) is controlled within the aforementioned range, which is beneficial to improving energy density while taking into account cycle performance.

[0097] When the second negative electrode active material includes artificial graphite and natural graphite, the ratio of natural graphite to the total mass of the second negative electrode active material (f 21 ) and the proportion of artificial graphite in the total mass of the second negative electrode active material (f 22 ) is controlled within the aforementioned range, which is beneficial to improving energy density while taking into account cycle performance.

[0098] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include carbon-coated negative electrode active particles;

[0099] The carbon-coated negative electrode active particles include a second negative electrode active body and a carbon coating layer located on at least a portion of the surface of the second negative electrode active body, wherein the carbon coating layer includes one or more of amorphous carbon, soft carbon and hard carbon;

[0100] The negative electrode plate meets one or more of the following characteristics:

[0101] The graphitization degree of the carbon coating layer in the first negative electrode active material is higher than the graphitization degree of the carbon coating layer in the second negative electrode active material;

[0102] The oxygen content of the carbon coating layer in the first negative electrode active material is lower than the oxygen content of the carbon coating layer in the second negative electrode active material.

[0103] By arranging a carbon coating layer including one or more of amorphous carbon, soft carbon and hard carbon on the surface of the first negative electrode active material, a better lithium ion transmission channel can be provided for the first negative electrode active body, which is beneficial to promote lithium ion transmission, improve lithium replenishment efficiency, and further improve battery dynamics and cycle life.

[0104] By controlling the carbon coating layer in the first negative electrode active material to have a higher degree of graphitization, it is beneficial to reduce the water content, which in turn helps to reduce the side reaction between water and the negative electrode lithium replenishing material, which helps to further improve the lithium replenishing efficiency and even more helps to extend the cycle life of the battery.

[0105] By controlling the carbon coating layer in the first negative electrode active material to have a lower oxygen content, it is beneficial to reduce water absorption, thereby reducing the side reaction between water and the negative electrode lithium replenishing material, further improving the lithium replenishing efficiency, and even more beneficial to extending the cycle life of the battery.

[0106] In some embodiments, the first negative electrode active material includes secondary particles, and the second negative electrode active material includes a single particle;

[0107] Optionally, the negative electrode plate meets one or two of the following characteristics:

[0108] The mass ratio or quantity ratio of the secondary particles in the first negative electrode active material is 60% to 100%, and can be 80% to 100%;

[0109] The mass ratio or quantity ratio of the single particle in the second negative electrode active material is 60% to 100%, and can be optionally 80% to 100%.

[0110] Primary particles can be used as the basic crystal unit in the negative electrode active material. Secondary particles refer to the agglomerates of primary particles, and single particles refer to non-agglomerated primary particles. The shape and structure of single particles are relatively simple, and often have a certain orientation. Secondary particles are aggregated from primary particles, and the secondary particles can have a relatively random or relatively disordered orientation on the whole particle. Therefore, the secondary particles are more isotropic.

[0111] By controlling one or more parameters of the mass proportion and number proportion of secondary particles in the first negative electrode active material, and the mass proportion and number proportion of single particles in the second negative electrode active material within the aforementioned range, it is beneficial to make the upper first negative electrode active material have stronger isotropy, which is beneficial to improve the lithium ion embedding path, and further beneficial to improve the lithium replenishment efficiency. In addition, it is also beneficial to improve battery dynamics.

[0112] In some embodiments, the first negative electrode active material includes graphite secondary particles, and the second negative electrode active material includes graphite single particles;

[0113] Optionally, the negative electrode plate meets one or two of the following characteristics:

[0114] The mass ratio or quantity ratio of the graphite secondary particles in the first negative electrode active material is 60% to 100%, and can be 80% to 100%;

[0115] The mass ratio or quantity ratio of the single graphite particle in the second negative electrode active material is 60% to 100%, and can be optionally 80% to 100%.

[0116] Graphite primary particles can be used as the basic crystal unit in graphite materials, graphite secondary particles refer to the agglomerates of graphite primary particles, and graphite single particles refer to non-agglomerated graphite primary particles. The isotropy of graphite secondary particles is stronger than that of graphite single particles.

[0117] By controlling one or more parameters of the mass proportion and number proportion of secondary graphite particles in the first negative electrode active material, and the mass proportion and number proportion of single graphite particles in the second negative electrode active material within the aforementioned range, it is beneficial to make the upper layer of the first negative electrode active material have stronger isotropy, which is beneficial to improving the embedding path of lithium ions, and further beneficial to improving the lithium replenishment efficiency. In addition, it is also beneficial to improve battery dynamics.

[0118] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0119] The first negative electrode active material and the second negative electrode active material each independently include a carbon-based material, and the graphitization degree of the carbon-based material in the first negative electrode active material is lower than the graphitization degree of the carbon-based material in the second negative electrode active material;

[0120] The sphericity of the first negative electrode active material is higher than the sphericity of the second negative electrode active material.

[0121] By arranging a carbon-based material with a lower degree of graphitization in the first negative electrode active layer located in the upper layer, a larger interlayer spacing can be provided, which is more conducive to lithium insertion; in addition, the carbon-based material in the second negative electrode active layer located in the lower layer has a higher degree of graphitization, which can provide a more ordered layered structure that is conducive to the insertion and extraction of lithium ions, fewer defects and stronger conductivity, which is beneficial to improving the negative electrode capacity and the battery energy density.

[0122] By controlling the sphericity of the first negative electrode active material to be higher than that of the second negative electrode active material, the first negative electrode active material is advantageously provided with a shorter lithium insertion channel, which is more advantageous for solid phase transmission, and is advantageous for better improving lithium replenishment efficiency and extending cycle life.

[0123] In some embodiments, the ratio of the thickness of the first negative electrode active layer to the sum of the thickness of the first negative electrode active layer and the second negative electrode active layer on one side of the negative electrode current collector is denoted as f. H , satisfying 20%≤f H ≤70%, optionally, 30%≤f H ≤50%.

[0124] By calculating the ratio of the thickness of the first negative electrode active layer to the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer (f H , calculated on one side of the negative electrode current collector) within the aforementioned range is conducive to better balancing the higher lithium replenishment efficiency and better battery kinetics provided by the first negative electrode active layer and the overall energy density of the negative electrode sheet. In addition, by controlling f H The aforementioned range is more conducive to processing.

[0125] Furthermore, by regulating the compaction density of the second negative electrode active layer and / or the compaction density of the powder of the second negative electrode material, the comprehensive advantages of high lithium replenishment efficiency and high energy density can be better balanced.

[0126] In some embodiments, the constituent material of the first negative electrode active layer is recorded as a first negative electrode material, and the constituent material of the second negative electrode active layer is recorded as a second negative electrode material;

[0127] The negative electrode plate meets one or two of the following characteristics:

[0128] The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer;

[0129] The powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

[0130] By adjusting the compaction density of the second negative electrode active layer to be higher than that of the first negative electrode active layer, it is beneficial to improve the energy density of the lithium-ion secondary battery, thereby facilitating both high energy density and high lithium replenishment efficiency.

[0131] By controlling the powder compaction density of the second negative electrode material to be higher than the powder compaction density of the first negative electrode active material, it is beneficial to give the second negative electrode active layer a higher compaction density during the cold pressing process of the pole piece.

[0132] By controlling the second negative electrode active layer located in the lower layer to have a higher compaction density or the second negative electrode material to have a higher powder compaction density, it is beneficial to increase the energy density of the lower layer, so that the negative electrode plate can take into account higher energy density, higher lithium replenishment efficiency and better battery dynamics.

[0133] In some embodiments, the negative electrode plate satisfies one or both of the following characteristics:

[0134] When the battery is fully discharged, the compaction density of the negative electrode sheet is 1.08 g / cm 3 ~ 1.71 g / cm 3 , optional 1.17 g / cm 3 ~ 1.52 g / cm 3 ;

[0135] When the battery is fully discharged, the surface density of the negative electrode is 10 mg / cm 2 ~ 26 mg / cm 2 , optional 15mg / cm 2 ~ 20 mg / cm 2 .

[0136] By controlling the compaction density and / or surface density of the negative electrode plate within the aforementioned range, it is also beneficial for the battery to have a higher energy density.

[0137] In some exemplary embodiments, by adjusting one or both of the compaction density and the surface density of the negative electrode sheet within the aforementioned range, it is beneficial to balance the battery kinetics and the energy density.

[0138] In some exemplary embodiments, by adjusting one or both of the compaction density and the surface density of the negative electrode sheet within the aforementioned range, it is beneficial to simultaneously achieve high energy density and high lithium replenishment efficiency.

[0139] In some embodiments, there is a lithium-replenishing residual layer on a surface of the first negative electrode active layer away from the second negative electrode active layer; the lithium-replenishing residual layer contains inactive lithium.

[0140] In some embodiments, the negative electrode plate satisfies one or both of the following characteristics:

[0141] Measured on one side of the negative electrode current collector, the thickness of the lithium supplement residual layer is less than 0.1 μm, optionally, less than 0.08 μm, and further optionally, less than 0.05 μm;

[0142] Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement residual layer relative to the first negative electrode active layer is less than or equal to 98%, and can be 50%-98% or 30%-70%, and can further be 50%-70%.

[0143] In the process of providing a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer for lithium replenishment treatment, if the active lithium provided by the negative electrode lithium replenishment material is not able to be embedded into the negative electrode active material in time and becomes inactivated, a lithium replenishment residual layer including inactive lithium may be formed at the position of the lithium replenishment layer.

[0144] By controlling one or both of the thickness of the lithium replenishment residual layer and the coverage area percentage of the lithium replenishment residual layer relative to the first negative electrode active layer within the aforementioned range, it is beneficial to achieve efficient lithium replenishment of the negative electrode while also making the lithium replenishment residual layer have a more suitable thickness and / or coverage area percentage, which is beneficial to better achieve good electrolyte infiltration performance and charge transfer performance, and is beneficial to making the battery have good battery dynamics.

[0145] Better battery kinetics is beneficial to giving the battery a lower internal resistance.

[0146] In some embodiments, a plurality of micropores are provided on a surface of the negative electrode current collector on a side close to the second negative electrode active layer.

[0147] By setting a plurality of micropores on the surface of the negative electrode current collector close to the second negative electrode active layer, it is helpful to promote the infiltration of the negative electrode plate by the electrolyte, which can increase the lithium insertion rate after the first infiltration and help improve the lithium replenishment efficiency.

[0148] In some embodiments, the negative electrode current collector satisfies one or more of the following characteristics:

[0149] The micropores penetrate the negative electrode current collector along the thickness direction of the negative electrode current collector;

[0150] The pore size of the micropores is 5 μm to 500 μm, and can be optionally 30 μm to 200 μm.

[0151] By controlling the micropores to penetrate the negative electrode current collector along the thickness direction of the negative electrode current collector, it is more conducive to promoting the infiltration of the negative electrode plate by the electrolyte, which can better improve the lithium insertion rate after the first infiltration and is more conducive to improving the lithium replenishment efficiency.

[0152] By controlling the pore size of the micropores within the aforementioned range, the lithium replenishment efficiency is improved while also taking into account the mechanical strength and processability of the negative electrode current collector.

[0153] In some embodiments, the NP ratio of the lithium ion secondary battery is 1.05-1.3, and can be optionally 1.1-1.3, and the NP ratio of the lithium ion secondary battery is equal to the ratio of the negative electrode surface capacity to the positive electrode surface capacity.

[0154] By controlling the NP ratio of the lithium-ion secondary battery within the aforementioned range, it is beneficial for the negative electrode to store more lithium ions, which is convenient for continuously releasing the supplementary capacity in the later stages of cycling or storage, and can better extend the battery cycle life.

[0155] In some embodiments, the positive electrode plate includes a positive electrode active material, and the positive electrode active material includes one or more of a ternary positive electrode material, a modified form of a ternary positive electrode material, lithium iron phosphate, a modified form of lithium iron phosphate, lithium iron manganese phosphate, and a modified form of lithium iron manganese phosphate; the modified form includes one or more of a doping modification and a coating modification.

[0156] In some embodiments, the lithium-ion secondary battery also includes a positive electrode plate, the positive electrode plate includes a positive electrode active material, the positive electrode active material includes a ternary positive electrode material, lithium iron phosphate, lithium manganese iron phosphate, and one or more modified forms of any of the foregoing positive electrode active materials; the modified forms include one or more of doping modification and coating modification.

[0157] In some embodiments, the positive electrode active material includes carbon-coated lithium iron phosphate, which includes a lithium iron phosphate body and a carbon coating layer located on at least a portion of the surface of the lithium iron phosphate body, and the carbon coating layer includes one or more of soft carbon, hard carbon and amorphous carbon.

[0158] When the positive electrode active material includes carbon-coated lithium iron phosphate, the conductivity of the surface of the lithium iron phosphate body can be improved, and the conductive network inside the positive electrode sheet can be optimized, thereby improving the battery cycle performance.

[0159] In a second aspect of the present application, there is provided a component for preparing a lithium-ion secondary battery, comprising an electrode assembly and an electrolyte, wherein the electrode assembly comprises a positive electrode sheet, a lithium-supplemented negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the lithium-supplemented negative electrode sheet;

[0160] The lithium supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active initial layer, a first negative electrode active initial layer and a lithium supplemented layer sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active initial layer comprises a first negative electrode active material, and the second negative electrode active initial layer comprises a second negative electrode active material;

[0161] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite;

[0162] The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (t1) and (t2):

[0163] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0164] (t2) The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 The lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 .

[0165] As mentioned above, when the lithium-supplemented negative electrode sheet has any one of the above characteristics (t1) and (t2), it is beneficial to give the first negative electrode active layer a higher lithium insertion rate. Such a lithium-supplemented negative electrode sheet can be provided in a component for preparing a lithium-ion secondary battery. The lithium-supplemented negative electrode sheet is provided with a lithium-supplemented layer on the surface of the negative electrode active material layer. By providing a first negative electrode active layer and a second negative electrode active layer on the negative electrode active material layer, and making the first negative electrode active layer close to the lithium-supplemented layer have a higher lithium insertion rate, when the negative electrode is subjected to lithium-supplementing treatment, it is beneficial to efficiently embed active lithium ions into the first negative electrode active layer. In the process of assembling components for preparing lithium-ion secondary batteries using the lithium-supplemented negative electrode sheet, in the process after injecting the electrolyte, it is beneficial to make the active lithium provided by the lithium-supplementing layer embed into the first negative electrode active layer faster and more, which is beneficial to inhibit the deactivation of the active lithium before embedding into the negative electrode active material, and can reduce the loss of active lithium during lithium replenishment, which is beneficial to significantly improve the lithium replenishment efficiency, and obtain components with negative electrode sheets treated with efficient lithium replenishment. The prepared lithium-ion secondary battery can persistently replenish active lithium and continuously replenish capacity during the charge and discharge cycle, and can also reduce the enrichment of lithium ions on the surface of the negative electrode active material and reduce the generation of lithium precipitation, so that the lithium-ion secondary battery can have a significantly improved cycle life.

[0166] In some embodiments, the lithium replenishing layer includes elemental lithium.

[0167] By selecting a lithium replenishing layer including single-element lithium (a non-limiting example such as a lithium film), the preparation process is more controllable and the lithium replenishing efficiency is high.

[0168] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics:

[0169] Measured on one side of the negative electrode current collector, the thickness of the lithium supplement layer is less than the sum of the thicknesses of the first negative electrode active initial layer and the second negative electrode active initial layer;

[0170] Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is less than or equal to 98%, and can be 50%-98% or 30%-70%, and can further be 50%-70%.

[0171] In some embodiments, the thickness of the lithium supplement layer on a single side of the negative electrode current collector is less than or equal to 8.5 μm, and may be 0.5 μm to 8.5 μm.

[0172] In some embodiments, based on a single side of the negative electrode current collector, the thickness of the lithium supplement layer is less than or equal to 4.8 μm, and may be 0.5 μm to 4.8 μm, and may be further 1 μm to 4.8 μm.

[0173] The thickness of the lithium replenishment layer can be adjusted according to the amount of lithium replenishment required for the negative electrode. In addition, by controlling the thickness of the single side of the lithium replenishment layer within the aforementioned range, it is helpful to control the thickness of the lithium replenishment residual layer within a more appropriate range.

[0174] In the production process, water that is difficult to completely remove usually remains in the negative electrode plate, and the water may react with the lithium replenishing material in the lithium replenishing layer to generate heat. The thicker the lithium replenishing layer, the higher the heat generation. Without being limited to any theory, by controlling the thickness of the lithium replenishing layer within the aforementioned range, it is helpful to better control the heat generation caused by the reaction of water and lithium, thereby helping to improve production safety.

[0175] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics:

[0176] The compaction density of the lithium supplemented negative electrode sheet is 1.3 g / cm 3 ~ 1.8g / cm 3 , optional 1.4 g / cm 3 ~ 1.6 g / cm 3 ;

[0177] The surface density of the lithium supplemented negative electrode sheet is 10 mg / cm 2 ~ 26 mg / cm 2 , optional 15 mg / cm 2 ~ 20 mg / cm 2 .

[0178] By adjusting the compaction density and / or surface density of the lithium-supplemented negative electrode sheet, the compaction density and / or surface density of the negative electrode sheet in the lithium-ion secondary battery can be adjusted accordingly. By controlling the compaction density and / or surface density of the lithium-supplemented negative electrode sheet within the aforementioned range, it is beneficial for the battery to have a higher energy density.

[0179] In a third aspect of the present application, a method for preparing a lithium ion secondary battery is provided, which can be used to prepare the lithium ion secondary battery of the first aspect of the present application.

[0180] In some embodiments, a method for preparing a lithium ion secondary battery is provided, comprising the following steps:

[0181] Assembling a positive electrode sheet, a separator and a lithium-supplemented negative electrode sheet into an electrode assembly, so that the separator is arranged between the positive electrode sheet and the lithium-supplemented negative electrode sheet; wherein the lithium-supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active initial layer, a first negative electrode active initial layer and a lithium-supplemented layer sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active initial layer comprises a first negative electrode active material, and the second negative electrode active initial layer comprises a second negative electrode active material;

[0182] Placing the electrode assembly in the housing cavity of the shell, injecting an electrolyte, allowing the electrolyte to infiltrate the positive electrode sheet and the lithium-supplemented negative electrode sheet, and forming them to prepare a lithium-ion secondary battery; wherein the lithium-supplemented negative electrode sheet forms a negative electrode sheet, the second negative electrode active initial layer forms a second negative electrode active layer, and the first negative electrode active initial layer forms a first negative electrode active layer;

[0183] Wherein, the first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite;

[0184] The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (t1) and (t2):

[0185] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0186] (t2) The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 The lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 .

[0187] As mentioned above, when the lithium-supplemented negative electrode sheet has any one of the above characteristics (t1) and (t2), it is beneficial to give the first negative electrode active layer a higher lithium insertion rate. By contacting the electrode assembly including the above-mentioned lithium-supplemented negative electrode sheet with an electrolyte, infiltrating, and forming, a negative electrode sheet including a negative electrode lithium-supplemented treatment can be prepared, thereby making the negative electrode sheet include lithium pre-inserted by the negative electrode lithium-supplemented treatment. The negative electrode active material layer of the negative electrode plate is provided with a first negative electrode active layer located in an upper layer and a second negative electrode active layer located in a lower layer (the direction away from the surface of the negative electrode current collector is the upper layer, and the direction toward the surface of the negative electrode current collector is the lower layer). By giving the first negative electrode active layer located in the upper layer a higher lithium insertion rate, in the process of negative electrode lithium replenishment using the above-mentioned method, based on the higher lithium insertion rate of the first negative electrode active layer, it is beneficial to make the active lithium provided by the negative electrode lithium replenishment material more efficiently embedded in the first negative electrode active layer, which is beneficial to inhibit the deactivation of the active lithium before being embedded in the negative electrode active material, and can reduce the loss of active lithium during lithium replenishment, thereby significantly improving the lithium replenishment efficiency. Therefore, the negative electrode plate treated with high-efficiency negative electrode lithium replenishment is introduced into the lithium ion secondary battery, which can replenish active lithium for a long time during the charge and discharge cycle and continuously replenish capacity; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reduce the enrichment of lithium ions on the surface of the negative electrode active material, which is beneficial to reduce the generation of lithium precipitation, thereby making the lithium ion secondary battery have a significantly improved cycle life.

[0188] In some embodiments, the lithium-supplementing layer in the lithium-supplementing negative electrode sheet satisfies the following formula:

[0189] 1.05≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3;

[0190] Among them, C N_A is the preset surface capacity of the negative electrode, C P_A is the preset surface capacity of the positive electrode, ρ A is the surface density of the lithium supplement layer on the first negative electrode active initial layer based on the total amount on both sides, C Li / g is the theoretical gram capacity of lithium.

[0191] The negative electrode preset surface capacity can be calculated based on the theoretical gram capacity of the negative electrode active material and the surface density of the negative electrode active material in the negative electrode sheet. N_A =Theoretical gram capacity of negative electrode active material × surface density of negative electrode active material in the negative electrode sheet.

[0192] The positive electrode preset surface capacity can be calculated based on the theoretical gram capacity of the positive electrode active material and the surface density of the positive electrode active material in the positive electrode sheet. P_A=Theoretical gram capacity of positive electrode active material × surface density of positive electrode active material in the positive electrode sheet.

[0193] Without being limited to any theory, by controlling the surface density of the lithium replenishing layer to satisfy the above formula, the battery cycle life can be extended by replenishing lithium, and the thickness of the lithium replenishing layer residue can be controlled to be more appropriate. In addition, it is also beneficial to better control the heat generation caused by the reaction of water and lithium, thereby improving production safety.

[0194] In some embodiments, after the step of injecting the electrolyte and before the step of allowing the electrolyte to infiltrate the positive electrode sheet and the lithium-supplemented negative electrode sheet, the component for preparing a lithium-ion secondary battery described in the second aspect of the present application is obtained.

[0195] In some embodiments, the method for preparing a lithium-ion secondary battery satisfies one or more of the following characteristics:

[0196] The lithium-supplemented negative electrode sheet is prepared by a method comprising the following steps: forming the second negative electrode active initial layer on at least one side surface of the negative electrode substrate, forming the first negative electrode active initial layer on the surface of the second negative electrode active initial layer away from the negative electrode substrate, and adding the lithium-supplemented layer on the surface of the first negative electrode active initial layer away from the second negative electrode active initial layer;

[0197] The lithium-supplemented negative electrode sheet is the lithium-supplemented negative electrode sheet described in the second aspect of the present application.

[0198] In some embodiments, the prepared lithium ion secondary battery is the lithium ion secondary battery described in the first aspect of the present application.

[0199] In a fourth aspect of the present application, an electrical device is provided, comprising at least one of the lithium ion secondary battery described in the first aspect of the present application and the lithium ion secondary battery prepared by the method for preparing the lithium ion secondary battery described in the third aspect of the present application.

[0200] The details of one or more implementations or embodiments of the present application are set forth in the following drawings and description. Other features, objects and advantages of the present application will become apparent from the description, drawings and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0201] In order to better describe and illustrate the implementation methods, embodiments or examples provided in this application, reference may be made to one or more drawings. The additional details or examples used to describe the drawings should not be considered as limitations on the scope of the disclosed application, the implementation methods, embodiments or examples currently described, and any of the best modes of these applications currently understood. Moreover, in all the drawings, the same figure numbers are used to represent the same components. It should also be noted that the drawings are all drawn in a simplified form and are only used to facilitate and clearly assist in explaining this application. The various sizes of each component shown in the drawings are arbitrarily shown and may be accurate or may not be drawn according to the actual scale. For example, in order to make the illustration clearer, the size of the components is appropriately exaggerated in some places in the drawings. Unless otherwise specified, the components in the figures are not drawn to scale. This application does not limit every size of each component.

[0202] In the attached picture:

[0203] Figure 1 1 is a schematic diagram of the structure of a lithium-supplemented negative electrode sheet in an embodiment of the present application, and corresponds to a side view showing a cross section of the lithium-supplemented negative electrode sheet.

[0204] Figure 2 yes Figure 1 A schematic diagram of the structure of the lithium-supplemented negative electrode sheet, corresponding to the top view, shows the surface of one side of the lithium-supplemented negative electrode sheet where the lithium-supplemented layer is provided.

[0205] Figure 3 It is a schematic diagram of the structure of a lithium-supplemented negative electrode sheet in another embodiment of the present application, and corresponds to a top view, showing a surface of one side of the lithium-supplemented negative electrode sheet on which a lithium-supplemented layer is provided.

[0206] Figure 4 It is a schematic diagram of the structure of a lithium-supplemented negative electrode sheet in another embodiment of the present application, and corresponds to a top view, showing a surface of one side of the lithium-supplemented negative electrode sheet on which a lithium-supplemented layer is provided.

[0207] Figure 5 It is a schematic diagram of a battery cell according to an embodiment of the present application.

[0208] Figure 6 for Figure 5 An exploded view of a battery cell according to an embodiment of the present application is shown.

[0209] Figure 7 FIG. 1 is a schematic diagram of a battery device according to an embodiment of the present application.

[0210] Figure 8 A schematic diagram of a battery pack according to an embodiment of the present application.

[0211] Fig. 9 for Figure 8 An exploded view of a battery pack according to an embodiment of the present application is shown.

[0212] Fig.10 A schematic diagram of an electrical device using a lithium-ion secondary battery according to an embodiment of the present application as a power source.

[0213] Description of reference numerals:

[0214] X is the X direction; Y is the Y direction; Z is the Z direction; 12, lithium supplement negative electrode sheet; 102, negative electrode current collector; 104, second negative electrode active initial layer; 106, first negative electrode active initial layer; 108, lithium supplement layer; 1, battery pack; 2, upper box; 3, lower box; 4, battery device; 5, battery cell; 51, shell; 52, electrode assembly; 53, cover plate; 6, power-consuming device.

[0215] Among them, the X direction corresponds to the width direction of the pole piece (which can be consistent with the height direction of the wound battery cell), the Y direction corresponds to the length direction of the pole piece, and the Z direction corresponds to the thickness direction of the pole piece. DETAILED DESCRIPTION

[0216] Below, some embodiments and examples of the lithium-ion secondary battery of the present application, the components for preparing the same, the preparation method and the electrical device are described in detail with appropriate reference to the drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0217] "Scope" disclosed in the present application can be limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or excluding end values, and any end value can be included or not included independently, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are also listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation for these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to listing the parameter as, for example, integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For example, when a parameter is expressed as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0218] In this application, when "multiple", "multiple", "multiple", "several", etc. are involved, unless otherwise specified, it means that the number is greater than 2 or equal to 2. For example, "one or more" means one or ≥ (greater than or equal to) two. It is understood that when "any number" of items are involved, it means any suitable combination of multiple items, that is, the combination of "any number" of items is performed in a way that does not conflict and can implement this application.

[0219] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0220] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment or implementation of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. The "implementation methods" mentioned herein have a similar understanding.

[0221] In the present application, in the open technical features or technical solutions described by the words "contain", "include", "include", etc., if there is no other explanation, additional members other than the listed members are not excluded, and it can be regarded as providing both closed features or solutions consisting of the listed members and open features or solutions including additional members in addition to the listed members. For example, a includes a1, a2 and a3. If there is no other explanation, it may also include other members or may not include additional members. It can be regarded as providing both the feature or solution of "a consists of a1, a2 and a3" or "a is selected from a1, a2 and a3", and the feature or solution of "a includes not only a1, a2 and a3, but also other members".

[0222] In the present application, unless otherwise specified, M (such as m1) means that m1 is a non-limiting example of M, and it can be understood that M is not limited to m1.

[0223] In this application, "optionally" and "optional" mean optional, that is, any one of the two parallel solutions of "yes" or "no". If there are multiple "optional" in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent. Unless otherwise specified, the description of "optionally including" in this application, taking "optionally including" as an example, means "may include or not include".

[0224] In the present application, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein any and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "M and / or N" means a group consisting of M, N, and "a combination of M and N". Among them, "including M and / or N" can mean "including M, including N, and including M and N", and can also mean "including M, including N, or including M and N", which can be properly understood according to the sentence in which it is located.

[0225] Herein, the word “suitable” in “suitable manner” etc. refers to the technical solution that can implement the present application.

[0226] Herein, "better", "preferable" and the like are merely used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of this application.

[0227] In the present application, “further”, “furthermore”, “particularly”, “for example”, “such as”, “example”, etc. are used for descriptive purposes to indicate differences in content, but should not be understood as limiting the scope of protection of the present application.

[0228] In the present application, the terms "first", "second", "third", "fourth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0229] In the description of the present application, it should be understood that the terms "length", "width", "thickness", "height", "up", "down", "top", "bottom", "inside", "outside", etc., indicating orientation or positional relationships, are based on the orientation or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0230] In this application, unless otherwise clearly specified and limited, the term "connection" and other terms should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection. For ordinary technicians in this field, the appropriate meanings of the above terms in this application can be understood according to the circumstances.

[0231] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean a relative positional relationship in terms of horizontal height, or may mean that there is an attachment relationship without limiting the relative positional relationship in terms of horizontal height.

[0232] In this application, the term "room temperature" generally refers to 4°C to 35°C, and may refer to 20°C ± 5°C. In some embodiments or examples of this application, room temperature refers to 20°C to 30°C.

[0233] In this application, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 3~5 μm or 3-5 μm both mean that the units of the left endpoint "3" and the right endpoint "5" are both μm (micrometers), which have the same meaning as 3 μm ~5 μm. In addition, similar descriptions of other parameters such as temperature and size are also understood in the same way.

[0234] In this application, "greater than or equal to" and "≥" have the same meaning and can be used interchangeably; "less than or equal to" and "≤" have the same meaning and can be used interchangeably; "greater than" can be equivalently expressed as ">", and "less than" can be equivalently expressed as "<". In this application, unless otherwise specified, "greater than or equal to" and "≥" can be regarded as providing two solutions of "greater than" and "equal to". In this application, unless otherwise specified, "less than or equal to" and "≤" can be regarded as providing two solutions of "less than" and "equal to".

[0235] In the present application, exemplary descriptions such as "in some implementation modes (or examples)" and "in one implementation mode (or example)" may include but are not limited to the following meanings: these solutions may be combined with other solutions in a suitable manner to form a new technical solution.

[0236] The improved effects described in this application, unless otherwise stated, are not intended to be limited to any theory.

[0237] At present, the demand for the cycle life of lithium-ion secondary batteries is getting higher and higher. The lithium replenishment technology can be used to extend the battery cycle life. As a non-limiting example, in the process of preparing the negative electrode plate, a lithium replenishment layer containing a lithium replenishment material can be provided on the surface of the negative electrode active material layer, and the active lithium ions released by the lithium replenishment material are embedded in the negative electrode active material after being infiltrated with the electrolyte, so as to replenish the negative electrode lithium. The lithium stored in the negative electrode can play a role in supplementing the capacity, thereby extending the battery cycle life. However, if the active lithium ions released by the lithium replenishment material cannot be embedded in the negative electrode active material in time, it is easy to cause the active lithium to be deactivated and unable to play the role of supplementing the capacity, affecting the efficiency of lithium replenishment, and even the lithium ion negative electrode may produce lithium precipitation on the surface of the negative electrode active material.

[0238] According to various embodiments and examples of the present application, the present application provides a lithium ion secondary battery, a component for preparing a lithium ion secondary battery, a preparation method and an electric device. The lithium ion secondary battery has a significantly improved cycle life.

[0239] In this application, unless otherwise specified, the term "lithium-ion secondary battery" refers to a secondary battery whose active ions include lithium ions, and "lithium-ion battery cell" refers to a battery cell whose active ions include lithium ions. Typically, a lithium-ion secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, the active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. In some embodiments, the active ions are lithium ions.

[0240] In the present application, unless otherwise specified, the "electrode active material layer" includes at least one of the positive electrode active material layer of the positive electrode sheet and the negative electrode active material layer of the negative electrode sheet. Depending on the detailed circumstances, the electrode active material layer may refer to the positive electrode active material layer or the negative electrode active material layer.

[0241] In the present application, the term "negative electrode sheet" includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material. The term "negative electrode active material" refers to a material used in a negative electrode sheet that can reversibly insert and remove active ions.

[0242] In this application, unless otherwise specified, "negative electrode sheet" includes a negative electrode current collector. "Negative electrode current collector" refers to a structure responsible for collecting and conducting electrons at the negative electrode. In the negative electrode sheet, the negative electrode active material layer is located on at least one side of the negative electrode current collector, which can be one side or both sides of the negative electrode current collector.

[0243] In the present application, the term "positive electrode sheet" includes a positive electrode active material layer, and the positive electrode active material layer includes a positive electrode active material. The term "positive electrode active material" refers to a material used in a positive electrode sheet that is capable of reversibly extracting and inserting active ions.

[0244] In this application, unless otherwise specified, "positive electrode sheet" includes positive electrode current collector. "Positive electrode current collector" refers to the structure responsible for collecting and conducting electrons at the positive electrode. In the positive electrode sheet, the positive electrode active material layer is located on at least one side of the positive electrode current collector, which can be one side or both sides of the positive electrode current collector.

[0245] In the present application, unless otherwise specified, "separation membrane" and "diaphragm" have the same meaning and can be used interchangeably.

[0246] In a first aspect of the present application, a lithium ion secondary battery is provided.

[0247] In some embodiments, a lithium-ion secondary battery is provided, which includes a negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the negative electrode plate has been treated with negative lithium supplementation.

[0248] In the present application, unless otherwise specified, in a lithium-ion secondary battery, "the negative electrode plate has been treated with negative electrode lithium supplementation" means that "the negative electrode plate includes lithium pre-embedded by negative electrode lithium supplementation", which means that the negative electrode plate of the lithium-ion secondary battery has been treated with negative electrode lithium supplementation, so that the negative electrode plate includes not only the lithium embedded in the negative electrode during the formation process, but also the lithium additionally introduced by the negative electrode lithium supplementation treatment. During the negative electrode lithium supplementation process, the lithium supplementation material carried by the negative electrode plate releases active lithium ions, and the released active lithium ions are embedded in the negative electrode active material, thereby obtaining a negative electrode plate treated with negative electrode lithium supplementation, and the lithium embedded in the negative electrode during the negative electrode lithium supplementation process can be called "pre-embedded lithium"; after the negative electrode plate treated with negative electrode lithium supplementation is introduced into the lithium-ion secondary battery, the negative electrode plate can release the pre-embedded lithium during the charge and discharge process of the lithium-ion secondary battery, thereby replenishing the lithium continuously consumed by the battery system. Compared with the case where the negative electrode plate has not been treated with lithium supplementation, the lithium-ion secondary battery provided in the first aspect of the present application has a significantly extended cycle life.

[0249] In the present application, unless otherwise specified, the negative electrode lithium replenishment material used in the negative electrode lithium replenishment treatment process undergone by the negative electrode pole piece is provided by the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer, that is, "the negative electrode pole piece undergoes negative electrode lithium replenishment treatment" means that the negative electrode pole piece undergoes lithium replenishment treatment with the lithium replenishment layer located on the surface of the first negative electrode active layer away from the second negative electrode active layer; accordingly, "the negative electrode pole piece includes lithium pre-embedded by negative electrode lithium replenishment" means that the negative electrode pole piece includes lithium pre-embedded by the lithium replenishment treatment of the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0250] In some embodiments, a lithium-ion secondary battery is provided, which includes a negative electrode plate; the negative electrode plate includes a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the first negative electrode active material includes a fast lithium insertion material, and the negative electrode plate is subjected to a negative electrode lithium supplementation treatment. In this case, the first negative electrode active material includes one or more of artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite.

[0251] In some embodiments, a lithium-ion secondary battery is provided, which includes a negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the lithium insertion rate of the first negative electrode active material is higher than the lithium insertion rate of the second negative electrode active material; further, the negative electrode plate undergoes a negative electrode lithium supplementation treatment.

[0252] In some embodiments, a lithium-ion secondary battery is provided, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the separator is arranged between the positive electrode plate and the negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the lithium insertion rate of the first negative electrode active material is higher than the lithium insertion rate of the second negative electrode active material; further, the negative electrode plate undergoes a negative electrode lithium supplementation treatment.

[0253] In the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector, and the negative electrode active material layer has a multilayer structure, including multiple negative electrode active layers. Further, the negative electrode active material layer includes a first negative electrode active layer and a second negative electrode active layer, and the second negative electrode active layer is located between the negative electrode current collector and the first negative electrode active layer.

[0254] In this application, unless otherwise specified, in the first negative electrode active layer, the negative electrode active material is recorded as the "first negative electrode active material"; in the second negative electrode active layer, the negative electrode active material is recorded as the "second negative electrode active material". In the context of this application, unless otherwise specified, the "first" and "second" in "first negative electrode active material" and "second negative electrode active material" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.

[0255] For the negative electrode plate, the negative electrode plate includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material. It can be understood that the first negative electrode active material and the second negative electrode active material are both contained in the negative electrode active material.

[0256] In the present application, unless otherwise specified, the "first" and "second" in "first negative electrode active layer" and "second negative electrode active layer" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.

[0257] In this application, unless otherwise specified, "lithium insertion rate (rate)" can reflect the amount of lithium inserted per unit time, and "lithium replenishment efficiency (efficiency)" can reflect the ratio of the amount of lithium inserted effectively into the negative electrode active material to the total amount of lithium supplied by the negative electrode lithium replenishment material. The lithium replenishment efficiency of the negative electrode active material is mainly related to factors such as the lithium insertion potential and gram capacity of the negative electrode active material. The "lithium insertion potential" of the negative electrode active material indicates the potential difference for the insertion and extraction of lithium ions in the negative electrode active material, which can reflect the ease of lithium ion insertion. The "gram capacity" of the negative electrode active material can reflect the ability of the negative electrode active material to store and release lithium ions.

[0258] By arranging a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer (the direction away from the surface of the negative electrode current collector is regarded as the upper layer, and the direction toward the surface of the negative electrode current collector is regarded as the lower layer) on the negative electrode active layer of the negative electrode plate, the first negative electrode active material located on the upper layer can further have a higher lithium insertion rate, which is beneficial for the active lithium ions provided by the negative electrode lithium replenishing material to be efficiently embedded in the first negative electrode active layer, which can reduce the probability of active lithium being deactivated due to lack of time to be embedded, and can significantly improve the lithium replenishment efficiency; thereby, a negative electrode plate treated with efficient negative electrode lithium replenishment can be obtained, and the negative electrode plate includes lithium pre-embedded by negative electrode lithium replenishment through the lithium replenishing layer. By introducing the aforementioned negative electrode plate that has undergone high-efficiency negative electrode lithium replenishment treatment into a lithium-ion secondary battery, the higher lithium replenishment efficiency is conducive to storing more lithium in the negative electrode, thereby permanently replenishing active lithium and continuously replenishing capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is conducive to reducing the enrichment of lithium ions on the surface of the negative electrode active material, which in turn is conducive to reducing the generation of lithium plating; through the synergy of the aforementioned multiple effects, the lithium-ion secondary battery can have a significantly improved cycle life.

[0259] The effects described in any part of this application are not intended to be limited by any theory.

[0260] The lithium insertion potential of natural graphite is usually lower than that of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon carbon composite. The specific capacity of natural graphite is usually lower than that of hard carbon, soft carbon, silicon oxide and silicon carbon composite. The lithium insertion potential of natural graphite is usually low, for example, it can be between 0.01V and 0.2V vs. Li / Li. + Within this range, natural graphite has structural defects and uneven surface morphology, which leads to anisotropy in the diffusion of lithium ions, making the overall lithium replenishment efficiency of natural graphite relatively low. The lithium insertion potential of artificial graphite can be slightly higher than that of natural graphite, and the specific capacity of artificial graphite may be slightly lower than that of natural graphite. However, the morphology and structure of artificial graphite are more regular than those of natural graphite, and the internal defects are relatively few, which makes the transmission of lithium ions more stable, and overall can achieve a faster lithium insertion rate than natural graphite. The lithium insertion potential of hard carbon is usually higher than that of natural graphite, and the capacity of hard carbon is also higher than that of natural graphite. The crystal arrangement inside hard carbon is disordered and there are many pores, which can provide abundant lithium insertion sites and fast transmission channels, and can provide a faster lithium insertion rate. The lithium insertion potential of soft carbon is also usually higher than that of natural graphite. The carbon layers in soft carbon are stacked disorderly, so that lithium ions can be transmitted relatively quickly in it. Soft carbon can provide a higher lithium insertion rate than natural graphite overall. The lithium insertion potential of silicon oxide and silicon-carbon composites is higher than that of natural graphite, and the capacity is much higher than that of natural graphite. The large amount of lithium insertion per unit time makes the lithium insertion rate of silicon oxide and silicon-carbon composites higher than that of natural graphite.

[0261] In summary, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite have higher lithium insertion rates than natural graphite. In this application, "artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite" can be collectively referred to as fast lithium insertion materials.

[0262] In this application, unless otherwise specified, the sum of the masses of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is denoted as f. 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is recorded as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 .

[0263] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0264] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; the negative electrode plate satisfies one or both of the following characteristics (t1) and (t2):

[0265] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0266] (t2) The negative electrode sheet meets one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f29 .

[0267] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0268] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite;

[0269] The negative electrode sheet satisfies one or both of the following characteristics (t1) and (t2):

[0270] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0271] (t2) The negative electrode sheet meets one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 ;

[0272] Furthermore, the negative electrode plate undergoes negative electrode lithium replenishment treatment.

[0273] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0274] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0275] Furthermore, the negative electrode plate undergoes negative electrode lithium replenishment treatment.

[0276] By controlling the first negative electrode active material located in the upper layer to have a higher lithium insertion potential, it is beneficial to quickly embed active lithium ions into the first negative electrode active layer. When preparing the negative electrode plate, it is beneficial to embed more active lithium provided by the negative electrode lithium replenishment material into the first negative electrode active layer faster, which can reduce the probability of active lithium being deactivated due to lack of time to embed, and can significantly improve the lithium replenishment efficiency. By introducing the negative electrode plate treated with efficient negative electrode lithium replenishment into the lithium-ion secondary battery, more lithium can be stored in the negative electrode, thereby replenishing active lithium and continuously replenishing capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reducing the enrichment of lithium ions on the surface of the negative electrode active material, which is beneficial to reducing the generation of lithium precipitation; through the synergy of the aforementioned multiple effects, the lithium-ion secondary battery can have a significantly improved cycle life.

[0277] The lithium insertion potential of the negative electrode active material can be tested by any suitable known method in the art, non-limiting examples of which include constant current intermittent titration technique (GITT), cyclic voltammetry (CV), potentiometric titration, electrochemical impedance spectroscopy (EIS) combined with other methods, etc.

[0278] In this application, unless otherwise specified, the constituent materials of the negative electrode active material layer are recorded as negative electrode materials, the constituent materials of the first negative electrode active layer are recorded as first negative electrode materials, and the constituent materials of the second negative electrode active layer are recorded as second negative electrode materials. The "first" and "second" in "first negative electrode material" and "second negative electrode material" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. The first negative electrode material in the first negative electrode active layer and the second negative electrode material in the second negative electrode active layer can be obtained by the following method: disassemble the battery cell to obtain the negative electrode sheet, scrape the powder at the thickness position of the first negative electrode active layer and the second negative electrode active layer in the negative electrode sheet respectively, and obtain the first negative electrode material (taken from the first negative electrode active layer) and the second negative electrode material (taken from the second negative electrode active layer) respectively after drying. The first negative electrode material includes the first negative electrode active material, and the second negative electrode material includes the second negative electrode active material. Those skilled in the art can further extract the first negative electrode active material and the second negative electrode active material by existing methods. The corresponding negative electrode active materials can be extracted from different negative electrode active layers of the negative electrode sheet by using methods such as solvent washing, ultrasonic dispersion, and graded sedimentation, and the samples can be obtained by drying. Taking the extraction of the first negative electrode active material from the first negative electrode material as an example, the following method can be used, but is not limited to: use a solvent (such as dimethyl carbonate) to fully soak the first negative electrode material, so that the organic components such as binders and thickeners therein are dissolved in the solvent (ultrasonic dispersion can also be combined to promote dissolution), and after washing and filtering, the collected solid phase is used as the powder to be tested for the negative electrode active material. It should be noted that the small amount of conductive agent that may be contained in the test sample does not affect the comparative analysis of the types of negative electrode active materials in the first negative electrode active layer and the second negative electrode active layer and the lithium insertion potential.

[0279] In the present application, unless otherwise specified, the "lithium insertion potential" of the negative electrode active material refers to the intrinsic lithium insertion potential at a rate of 0.05C to 0.1C.

[0280] In the present application, unless otherwise specified, the following method may be used to test and compare the lithium insertion potentials of the first negative electrode active material and the second negative electrode active material in the lithium ion secondary battery.

[0281] Taking the first negative electrode active material as an example, a certain mass m1 of the first negative electrode active material to be tested is placed in an agate mortar, an appropriate amount of deionized water is added, and the powder is evenly ground and then scraped on the single side surface of the copper foil, and then dried and punched into small discs of a certain diameter (such as a diameter of 14 mm). The lithium sheets are assembled into a button battery, and the battery is charged and discharged at a voltage of 0.005V~2V at a rate of 0.1C for one week and then charged to 0.005V. The lithium insertion potential V1 of the first negative electrode active material can be calculated according to the following formula: lithium insertion potential V1=charging energy / capacity. Similarly, a certain mass m2 of the second negative electrode active material can be used to prepare a button battery, and the lithium insertion potential V2 of the second negative electrode active material can be measured. Control m1=m2, when V1>V2, it can be considered that "the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material".

[0282] In the present application, the characteristics of negative electrode lithium replenishment technology can be combined. For example, the coverage area and uncovered area of ​​the lithium replenishment residue can be detected to determine whether the negative electrode plate has been treated with negative electrode lithium replenishment and to identify the lithium replenishment area. Taking the use of metal lithium foil for negative electrode lithium replenishment as a non-limiting example, the lithium foil and the negative electrode active material are reacted under the action of the electrolyte, so that the lithium ions released by the lithium foil are embedded in the negative electrode active material, and lithium replenishment can be achieved. After lithium replenishment using this type of method, a residue area with the same shape as the lithium foil coverage area is usually formed at the position where the lithium foil is initially set. The residue area may contain inactive substances such as lithium oxide (Li2O) and other by-products. In addition, unreacted metal lithium may also exist in the residue area. SEM and EDS can be used in combination to distinguish the residue area from the area not covered by the lithium foil. For example, the distribution difference of carbon elements and / or silicon elements can be used to distinguish the residue area from the area not covered by the lithium foil.

[0283] In the present application, the cross section of the negative electrode sheet can be subjected to microscopic morphology observation to observe the microscopic morphology of each negative electrode active layer in the negative electrode active material layer in the negative electrode sheet and the boundary between different negative electrode active layers, and then the thickness of different negative electrode active layers can be determined. "The cross section of the negative electrode sheet" refers to the cross section perpendicular to the thickness direction of the negative electrode sheet. Furthermore, the cross section of the negative electrode sheet can also be subjected to microscopic morphology observation and combined with component analysis (such as energy dispersive spectroscopy (EDS), X-ray diffraction (XRD) analysis, etc.) to identify the type of elements, so as to confirm the composition of different negative electrode active layers in the negative electrode active material layer. Non-limitingly, the cross section of the negative electrode sheet can be obtained by using instruments or equipment including but not limited to focused electron beam (FIB) electron microscope (non-limiting examples such as FEIScios 2HiVac equipment, etc.), ion cross-section polisher (non-limiting examples such as IB-09010 CP argon ion cross-section polisher, IB-19500CP ion cross-section polisher, etc. of JEOL, Japan), or plasma quenching method. The cross section of the negative electrode sheet can be obtained by using instruments or equipment including but not limited to scanning electron microscope (SEM) technology, non-limitingly, a high-resolution field emission scanning electron microscope can be used; non-limiting examples of SEM instruments include Sigma 300 scanning electron microscope, Apreo 2 SEM field emission scanning electron microscope, etc. of ZEISS, Germany.

[0284] In the SEM microscopic morphology image of the cross section of the negative electrode sheet, the boundaries between different negative electrode active layers and the thickness of each negative electrode active layer can be confirmed based on the obvious discontinuous changes in the microscopic morphology.

[0285] In the present application, unless otherwise specified, the “section of the negative electrode sheet” refers to the cross section of the negative electrode sheet.

[0286] In some embodiments, the lithium insertion potential of the first negative electrode active material is greater than or equal to 0.08 V vs. Li / Li + , optionally, greater than or equal to 0.1 V vs. Li / Li + .

[0287] In some embodiments, the lithium insertion potential of the first negative electrode active material is 0.08 V to 0.5 V vs. Li / Li + , selectable from 0.1 V ~ 0.5 V vs. Li / Li +Without limitation, the lithium insertion potential of the first negative electrode active material may be any of the following values ​​or a range consisting of any two of the following values: 0.08, 0.09, 0.1, 0.10, 0.12, 0.13, 0.14, 0.15, 0.16, 0.18, 0.2, 0.20, 0.25, 0.3, 0.30, 0.35, 0.4, 0.40, 0.45, 0.5, etc., in units of Vvs. Li / Li + .

[0288] Those skilled in the art can identify the components in the negative electrode active material layer, the first negative electrode active layer, and the second negative electrode active layer by one or more of the following detection methods known in the art, including but not limited to: Fourier transform infrared (FT-IR) spectroscopy, ultraviolet spectroscopy, nuclear magnetic resonance spectroscopy (NMR), and hydrogen spectroscopy. 1 H NMR) method, gel permeation chromatography (GPC) method, high performance liquid chromatography (HPLC) method, mass spectrometry, X-ray diffraction (XRD) method, Raman spectroscopy (Raman) method, single crystal X-ray diffraction (SCXRD) method, inductively coupled plasma spectroscopy (ICP) method, energy dispersive spectroscopy (EDS) instrument (abbreviated as spectrometer) analysis, etc. The sample preparation methods and test methods of these test methods are known to those skilled in the art, and the test parameters can be appropriately adjusted according to the structure of the material or substance and the sample characteristics.

[0289] As a non-limiting example, Si and C can be distinguished using EDS.

[0290] Taking the distinction between natural graphite and artificial graphite in the negative electrode active material as a non-limiting example, natural graphite and artificial graphite can be distinguished by the appearance morphology of the particles; X-ray diffraction (XRD) analysis test can be further performed. In the XRD spectrum, if the characteristic peak near 2θ 26.5° is very sharp and has a high intensity, it is natural graphite; if the characteristic peak near 2θ 26.5° is relatively wide and has a weak intensity, it is artificial graphite.

[0291] Taking the distinction between graphite and amorphous carbon as an example, Raman spectroscopy can be used for testing and analysis. The characteristic peak information of the carbon component in the spectrum (such as the intensity ratio of D peak / G peak, I D / G ) to analyze amorphous carbon. Both D peak and G peak are Raman characteristic peaks of carbon atom crystals. D peak represents the defects of carbon atom crystals. The more defects there are, the greater the intensity of D peak. The intensity of D peak can reflect the content of amorphous (turbostratified stacking) area. G peak represents the in-plane stretching vibration of sp2 hybridization of carbon atoms. The intensity of G peak can reflect the content of graphitized (layered structure) area. As the degree of disorder of carbon atoms increases, the intensity ratio of D peak to G peak also increases. You can also compare Raman spectra I D / G Standard Raman spectrum of graphite ID / G The difference between the D peak and the G peak of the Raman spectrum can be used to distinguish natural graphite from artificial graphite.

[0292] As non-limiting examples, FT-IR, UV spectroscopy, 1 One or more methods such as H NMR can be used to detect the type and content of the binder, but it is not limited thereto. For another example, EDS can be used to detect the type and content of the conductive agent, but it is not limited thereto. In addition, the conductive agent can also be identified or distinguished by combining the scanning electron microscope (SEM) and transmission electron microscope (TEM) test images.

[0293] In the present application, the sample to be tested of the "negative electrode active material" in the negative electrode sheet of the lithium-ion secondary battery can be obtained by disassembling the battery to obtain a powder sample to be tested. For the particle components in different negative electrode active layers, energy spectrometer (EDS, Energy Dispersive Spectrometer), inductively coupled plasma (inductively coupled plasma, ICP) method, XRD test analysis and other methods can be used for identification and test analysis. In a non-limiting manner, EDS, XRD, ICP and other methods can be used to identify different types of particles and perform quantitative test analysis of component content. Samples of different negative electrode active layers can be extracted from different positions of the negative electrode sheet, and different types of solid particles can be collected by methods including but not limited to solvent washing, ultrasonic dispersion, graded sedimentation, etc., and then the types of different solid particles can be identified by component analysis methods. For example, a reagent (such as aqua regia, reverse aqua regia, a combination of aqua regia and hydrogen fluoride, etc.) can be used to digest the negative electrode active material layer, and the composition of the negative electrode active material can be tested and analyzed by methods such as inductively coupled plasma emission spectrometer. For another example, a solvent (such as dimethyl carbonate) can be used to fully soak the powder material extracted from the corresponding negative electrode active layer, so that the organic components such as binder, thickener, etc. are dissolved in the solvent (it can also be combined with ultrasonic dispersion to promote dissolution), and after washing and filtering, the collected solid phase is used as the powder to be tested for the negative electrode active material. It should be noted that the small amount of conductive agent that may be contained in the test sample does not affect the analysis of the type, content, agglomeration morphology, etc. of the negative electrode active material in the first negative electrode active layer and the second negative electrode active layer.

[0294] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0295] f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ;

[0296] 0≤f 15 <f 21 ; or, 0≤f 15 ≤f 21 And f 19 >f 29 .

[0297] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0298] The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite;

[0299] The negative electrode sheet meets one or more of the following characteristics:

[0300] f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ;

[0301] 0≤f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 .

[0302] By controlling the first negative electrode active layer to have a higher sum of the mass fractions of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite (such as f 10 >f 20 ≥0), control the first negative electrode active layer located on the upper layer to have a lower natural graphite content (such as 0≤f 15 <f 21 ) and controlling the first negative electrode active layer to have a higher sum of the mass fractions of hard carbon, soft carbon, silicon oxide and silicon-carbon composite (such as f 10 ≥f 20 And f 19 >f 29 , or if 0≤f 15 ≤f 21 And f 19 >f 29) at least one control method is adopted to make the first negative electrode active layer contain more fast-insertion lithium materials and / or contain less natural graphite, so that the first negative electrode active layer can have a higher lithium insertion rate, and the lithium ions provided by the negative electrode lithium supplement material can be more efficiently embedded in the negative electrode, which is beneficial to improve the lithium supplement efficiency and improve the battery cycle life. As one of the exemplary theories, by making the first negative electrode active layer have a higher lithium insertion rate, it is beneficial to make the active lithium ions embed into the first negative electrode active layer faster and more, which can reduce the probability of active lithium being deactivated due to lack of time to embed, and can significantly improve the lithium supplement efficiency. By introducing the negative electrode pole piece treated with efficient negative electrode lithium supplement into the lithium ion secondary battery, the higher lithium supplement efficiency is beneficial to store more lithium in the negative electrode, so as to replenish the active lithium persistently and continuously replenish the capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reduce the enrichment of lithium ions on the surface of the negative electrode active material, which is beneficial to reduce the generation of lithium precipitation; through the synergy of the above-mentioned multiple effects, the lithium ion secondary battery can have a significantly improved cycle life.

[0303] In some embodiments, 50%≤f 10 ≤100%, optionally, 80%≤f 10 ≤100%, further optionally, 90%≤f 10 ≤100%. Without limitation, f 10 It can also be any of the following percentages or a range consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc. In some embodiments, 95%≤f 10 ≤100%.

[0304] In some embodiments, 50%≤f 20 ≤100%, optionally, 80%≤f 10 ≤100%, further optionally, 90%≤f 10 ≤100%. Without limitation, f 20 It can also be any of the following percentages or a range consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc. In some embodiments, 95%≤f 10 ≤100%.

[0305] In some embodiments, 0≤f 15 ≤50%, optionally, 0≤f 15 ≤30%, further optionally, 0≤f 15 ≤20%. Non-restrictive, non-restrictive, f 15It can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 1%, 2%, 4%, 5%, 6%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, 35%, 30%, 35%, 40%, 45%, 50%, etc.

[0306] In some embodiments, 0≤f 21 ≤50%, optionally, 1≤f 21 ≤30%, further optionally, 10≤f 21 ≤30%. Without limitation, f 21 It can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 1%, 2%, 4%, 5%, 6%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, 35%, 30%, 35%, 40%, 45%, 50%, etc.

[0307] In some embodiments, 0%≤f 19 ≤50%, optionally, 1%≤f 19 ≤40%, further optionally, 5%≤f 19 ≤30%. Without limitation, f 19 It can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 1%, 2%, 4%, 5%, 6%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, 35%, 30%, 35%, 40%, 45%, 50%, etc.

[0308] In some embodiments, 0%≤f 29 ≤50%, optionally, 0%≤f 29 ≤40%, further optionally, 1%≤f 29 ≤30%. Without limitation, f 29 It can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 1%, 2%, 4%, 5%, 6%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, 35%, 30%, 35%, 40%, 45%, 50%, etc.

[0309] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0310] 50%≤f 10 ≤100%, optionally, 80%≤f 10 ≤100%, further optionally, 90%≤f 10≤100%;

[0311] 50%≤f 20 ≤100%, optionally, 80%≤f 10 ≤100%, further optionally, 90%≤f 10 ≤100%;

[0312] 0≤f 15 ≤50%, optionally, 0≤f 15 ≤30%, further optionally, 0≤f 15 ≤20%;

[0313] 0≤f 21 ≤50%, optionally, 1≤f 21 ≤30%, further optionally, 10≤f 21 ≤30%;

[0314] 0%≤f 19 ≤50%, optionally, 1%≤f 19 ≤40%, further optionally, 5%≤f 19 ≤30%;

[0315] 0%≤f 29 ≤50%, optionally, 0%≤f 29 ≤40%, further optionally, 1%≤f 29 ≤30%.

[0316] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0317] 80%≤f 10 ≤100%;

[0318] 80%≤f 20 ≤100%;

[0319] 0≤f 15 ≤30%;

[0320] 1≤f 21 ≤30%;

[0321] 1%≤f 19 ≤40%;

[0322] 0%≤f 29 ≤40%.

[0323] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0324] 90%≤f 10 ≤100%;

[0325] 90%≤f 20 ≤100%;

[0326] 0≤f 15 ≤20%;

[0327] 10≤f 21 ≤30%;

[0328] 5%≤f 19 ≤30%;

[0329] 1%≤f 29 ≤30%.

[0330] By adding f 10 、f 20 、f 15 、f 21 、f 19 、f 29 Controlling one or more parameters in the above range is beneficial to making the negative electrode sheet as a whole have a faster lithium insertion rate, which is beneficial to better improve the lithium replenishment efficiency and better extend the battery cycle life.

[0331] In some embodiments, the first negative electrode active material includes one or more of artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite; the second negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite;

[0332] The negative electrode sheet meets one or more of the following characteristics:

[0333] f 10 >f 20 ≥0;

[0334] 0≤f 15 <f 21 .

[0335] At this time, the first negative electrode active layer has a higher lithium insertion rate and a better lithium replenishment efficiency.

[0336] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include one or more of artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite, and satisfy f 10 >f 20 >0.

[0337] In some embodiments, 0 <f 15 <f 21At this time, both the first negative electrode active layer and the second negative electrode active layer are provided with natural graphite, but the natural graphite content of the first negative electrode active layer is lower, so that the first negative electrode active layer has a higher lithium insertion rate and better lithium replenishment efficiency.

[0338] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include one or more of artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite, satisfying f 19 >f 29 At this time, the first negative electrode active layer has a higher lithium insertion rate and a better lithium replenishment efficiency.

[0339] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite, satisfying f 19 >f 29 And 0≤f 15 ≤f 21 At this time, the first negative electrode active layer has a higher lithium insertion rate and a better lithium replenishment efficiency.

[0340] In some embodiments, 0≤f 15 ≤f 21 And f 19 >f 29 And f 19 >f 29 In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include one or more of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite. In this case, the first negative electrode active layer contains a lower content or an equal amount of natural graphite than the second negative electrode active layer, and the sum of the mass of the hard carbon, soft carbon, silicon oxide and silicon-carbon composite accounts for a smaller proportion of the total mass of the first negative electrode active material. 19 is higher than the proportion of the sum of the masses of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material. 29 , that is, the total content of hard carbon, soft carbon, silicon oxide and silicon-carbon composite is higher in the first negative electrode active layer, so that the first negative electrode active layer has a higher lithium insertion rate and better lithium replenishment efficiency.

[0341] In some embodiments, f 10 ≥f 20 And f 19 >f 29 At this time, the first negative electrode active layer contains an equal amount or more of fast lithium insertion material relative to the second negative electrode active layer, and the total content of hard carbon, soft carbon, silicon oxide and silicon-carbon composite is further controlled to be higher in the first negative electrode active layer, so that the first negative electrode active layer has a higher lithium insertion rate and better lithium replenishment efficiency.

[0342] In some embodiments, 0≤f 15 <50% and 0 <f 21 ≤50%. Furthermore, 0≤f 15 <f 21 ≤50%.

[0343] In some embodiments, the first negative electrode active material includes one or more of artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite. In some embodiments, 50%≤f 10 ≤100%. 10 is the ratio of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite to the total mass of the first negative electrode active material. 10 It can also be any of the following percentages or a range consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc. In some embodiments, 80%≤f 10 ≤100%, optionally, 90%≤f 10 ≤100%, further optionally, 95%≤f 10 ≤100%.

[0344] In some embodiments, the first negative active material includes artificial graphite.

[0345] Artificial graphite refers to the process of treating graphitizable materials under high temperature and other conditions to form a regular graphitized lamellar structure. Artificial graphite is significantly different from natural graphite in morphology. Through the observation of the graphite cross section under a scanning electron microscope, it is found that natural graphite has more layered structures and a large number of pores between the lamellar structures; while the crystals of artificial graphite are more strictly arranged in an ABAB manner, with a dense interior and no gaps or only a small number of gaps. Artificial graphite and natural graphite also differ in their crystal structures. Natural graphite not only has a hexagonal phase, but also an orthorhombic hexahedral phase (3R phase); while artificial graphite can only have a hexagonal phase. Artificial graphite has fewer defects and higher capacity, which can reduce the degree of side reactions with the electrolyte, give full play to the high capacity characteristics of graphite, reduce gas production, and enable battery cells to have both high energy density and good cycle performance.

[0346] In this application, the proportion of artificial graphite in the total mass of the first negative electrode active material is denoted as f 11 .

[0347] In some embodiments, 50%≤f 11 ≤100%, optionally, 70%≤f 11 ≤95%. Without limitation, f 11It can also be any of the following percentages or a range consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0348] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0349] The proportion of artificial graphite in the total mass of the first negative electrode active material is f 11 Higher than the proportion of artificial graphite in the total mass of the second negative electrode active material 22 , where f 11 >f 22 ≥0;

[0350] The proportion of natural graphite in the total mass of the second negative electrode active material is f 21 Higher than the proportion of natural graphite in the total mass of the first negative electrode active material 15 , where f 21 >f 15 ≥0.

[0351] By controlling the negative electrode to meet the 11 >f 22 ≥0 and f 21 >f 15 One or both of ≥0 are beneficial to making the first negative electrode active layer have a higher lithium insertion rate, which is beneficial to better improve the lithium replenishment efficiency.

[0352] In some embodiments, the first negative electrode active material includes artificial graphite, and the negative electrode sheet satisfies f 21 >f 15 ≥0 and f 21 >f 15 ≥ 0.

[0353] In some embodiments, the first negative electrode active material includes one or more of hard carbon, soft carbon, silicon oxide, and silicon-carbon composite.

[0354] In some embodiments, the first negative electrode active material includes artificial graphite and further includes one or more of hard carbon, soft carbon, silicon oxide, and silicon-carbon composite.

[0355] By introducing one or more of hard carbon, soft carbon, silicon oxide and silicon-carbon composite into the first negative electrode active layer, it is beneficial to make the first negative electrode active layer have a higher lithium insertion rate, which is beneficial to better improve the lithium replenishment efficiency and better extend the cycle life of the battery.

[0356] In addition, by giving the first negative electrode active layer a higher lithium insertion rate, it is also beneficial to improve battery kinetics.

[0357] In the present application, the proportion of the sum of the masses of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is denoted as f. 12 .

[0358] In some embodiments, 0 <f 12 ≤50%, optionally, 5%≤f 12 ≤30%. Without limitation, f 12 It can also be any of the following percentages or a range consisting of any two of the following percentages: 1%, 2%, 4%, 5%, 6%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.

[0359] In some embodiments, the first negative electrode active material further includes one or more of hard carbon and soft carbon.

[0360] In some embodiments, the first negative electrode active material includes one or more of artificial graphite, silicon oxide, and silicon-carbon composite, and the first negative electrode active material further includes one or more of hard carbon and soft carbon.

[0361] By introducing one or more of hard carbon and soft carbon into the first negative electrode active layer, the hard carbon and soft carbon have a higher interlayer spacing, which is conducive to the entry of lithium ions; the hard carbon and soft carbon not only have a higher lithium insertion rate, but also have higher conductivity. Therefore, it is not only beneficial to better improve the lithium replenishment efficiency and better extend the cycle life of the battery, but also beneficial to better improve the battery dynamics.

[0362] In some embodiments, the first negative electrode active material includes artificial graphite, and the first negative electrode active material further includes one or more of hard carbon and soft carbon.

[0363] In this application, the ratio of the sum of the mass of the hard carbon and the soft carbon to the total mass of the first negative electrode active material is denoted as f. 13 .

[0364] In some embodiments, 0 <f 13 ≤50%, optionally, 10%≤f 13 ≤30%. Without limitation, f 13 It can also be any of the following percentages or a range consisting of any two of the following percentages: 1%, 2%, 4%, 5%, 6%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.

[0365] By calculating the sum of the mass of the hard carbon and the soft carbon in the total mass of the first negative electrode active material (f 13) is controlled within the aforementioned range, which is beneficial to taking into account the battery dynamics, lithium replenishment efficiency and first coulombic efficiency, and is beneficial to taking into account the battery dynamics, cycle life and actual energy density.

[0366] In some embodiments, the first negative electrode active material includes artificial graphite and further includes one or more of silicon oxide and silicon-carbon composite.

[0367] By introducing one or more of silicon oxide and silicon-carbon composite into the first negative electrode active layer, the capacity of silicon oxide and silicon-carbon composite is much higher than that of carbon-based materials, and they can alloy with negative electrode lithium replenishing materials more quickly, which is beneficial to better improve battery dynamics and lithium replenishment efficiency, and is also beneficial to improve energy density.

[0368] In the present application, the ratio of the sum of the mass of silicon oxide and silicon-carbon composite to the total mass of the first negative electrode active material is denoted as f. 14 .

[0369] In some embodiments, 0 <f 14 ≤50%, optionally, 1%≤f 14 ≤30%, further optionally, 1%≤f 14 ≤15%. Without limitation, f 14 It can also be any of the following percentages or a range consisting of any two of the following percentages: 1%, 2%, 4%, 5%, 6%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.

[0370] The ratio of the sum of the mass of silicon oxide and silicon-carbon composite to the total mass of the first negative electrode active material (f 14 ) is controlled within the aforementioned range, which is beneficial to improving battery dynamics and lithium replenishment efficiency, and increasing the energy density of the negative electrode. In addition, it is also beneficial to suppress the reduction in the first coulombic efficiency and capacity attenuation caused by factors such as the volume expansion of silicon oxide and silicon-carbon composite under charge and discharge conditions.

[0371] In some embodiments, the silicon-carbon composite includes a porous carbon matrix and elemental silicon located in cavities of the porous carbon matrix.

[0372] By introducing silicon-carbon composites into the negative electrode active materials and designing a structure in which elemental silicon is loaded into porous carbon based on the silicon-carbon composite, the volume expansion of the negative electrode active materials and negative electrode sheets during the charge and discharge cycle is significantly suppressed, which can inhibit the generation of fresh interfaces and is beneficial to further extend the battery cycle performance.

[0373] In some embodiments, the first negative electrode active material includes coated negative electrode active particles, which include a first negative electrode active body and a coating layer located at least partially on the surface of the first negative electrode active body, and the coating layer includes one or more of soft carbon and hard carbon.

[0374] By providing a coating layer including one or more of soft carbon and hard carbon on the surface of the first negative electrode active material, a better lithium ion transmission channel can be provided for the first negative electrode active body, which is beneficial to promote lithium ion transmission, improve lithium replenishment efficiency, and further improve battery dynamics and cycle life.

[0375] In some embodiments, in the coated negative electrode active particles, the thickness of at least a portion of the coating layer can be 1 nm to 10 nm, optionally 1 nm to 5 nm, or any of the following thicknesses or within the range consisting of any two of the following thicknesses: 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.

[0376] In some embodiments, in the coated negative electrode active particles, the average thickness of the coating layer can be 1 nm to 10 nm, optionally 1 nm to 5 nm, or any of the following thicknesses or within the range consisting of any two of the following thicknesses: 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.

[0377] In the present application, unless otherwise specified, the following method can be used to test and analyze the thickness of the coating layer in the coated negative electrode active particles.

[0378] The test sample of the coated negative electrode active particles can be obtained by the following method: the negative electrode sheet obtained by disassembling the battery cell is soaked and cleaned with a solvent (such as dimethyl carbonate (DMC)), and powder is scraped from different thickness positions to obtain powder samples of the first negative electrode material and the second negative electrode material respectively; after cutting the powder with FIB (focused ion beam), the particle cross-sectional morphology is observed under TEM (transmission electron microscope), and a clear boundary can be observed at the coating interface. Based on the TEM image, the thickness and average thickness of the coating layer can be analyzed and calculated;

[0379] Further combining one or more methods such as energy dispersive spectroscopy (EDS) analysis, Raman spectroscopy, X-ray diffraction (XRD) and the like, the material types of the coating layer and the active body can be confirmed.

[0380] The element composition and component types of the coating layer in the coated negative electrode active particles can be analyzed by using or referring to the above-mentioned method.

[0381] In some embodiments, in the coated negative electrode active particles, the sum of the mass fractions of soft carbon and hard carbon in the coating layer in the coated negative electrode active particles is 0.5%~10%, which can be optionally 1%~4%, or any of the following percentages or a range selected from any two of the following percentages: 0.5%, 1%, 2%, 3%, 3.5%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.

[0382] In some embodiments, the first negative electrode active body includes one or more of artificial graphite, silicon oxide, and silicon-carbon composite.

[0383] In the present application, the proportion of the sum of the mass of artificial graphite, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active body is denoted as f 16 .

[0384] In some embodiments, 80%≤f 16 ≤100%, optionally, 90%≤f 16 ≤100%. Without limitation, f 16 It can also be any of the following percentages or a range consisting of any two of the following percentages: 80%, 85%, 90%, 95%, 100%, etc.

[0385] In some embodiments, the coated negative electrode active particles satisfy one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0386] The thickness of at least a portion of the coating layer is 1 nm to 10 nm, and may be 1 nm to 5 nm;

[0387] The average thickness of the coating layer is 1nm~10nm, and can be optionally 1nm~5nm;

[0388] The sum of the mass fractions of the soft carbon and the hard carbon in the coating layer in the coated negative electrode active particles is 0.5% to 10%, and can be optionally 1% to 4%;

[0389] The first negative electrode active body includes one or more of artificial graphite, silicon oxide and silicon-carbon composite; the proportion of the sum of the mass of artificial graphite, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active body is recorded as f 16 , satisfying 80%≤f 16 ≤100%, optionally, 90%≤f 16 ≤100%.

[0390] In some embodiments, the first negative electrode active body includes artificial graphite.

[0391] In this application, the proportion of artificial graphite in the total mass of the first negative electrode active body is denoted as f 17 .

[0392] In some embodiments, 80%≤f 17 ≤100%. Without limitation, f 17 It can also be any of the following percentages or a range consisting of any two of the following percentages: 80%, 85%, 90%, 95%, 100%, etc.

[0393] In some embodiments, the second negative active material includes natural graphite.

[0394] By arranging natural graphite in the second negative electrode active layer located in the lower layer, lateral deformation is more likely to occur when the negative electrode plate is cold pressed, which is beneficial to provide improved compaction density and surface capacity, and further beneficial to improve energy density.

[0395] In some embodiments, the second negative active material includes artificial graphite and natural graphite.

[0396] In some embodiments, 0 <f 21 ≤50%, optionally, 10%≤f 21 ≤30%. 21 is the proportion of natural graphite in the total mass of the second negative electrode active material. Without limitation, f 21 It can also be any of the following percentages or a range consisting of any two of the following percentages: 1%, 2%, 4%, 5%, 6%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.

[0397] In this application, the proportion of artificial graphite in the total mass of the second negative electrode active material is denoted as f 22 .

[0398] In some embodiments, 50%≤f 22 ≤100%, optionally, 70%≤f 22 ≤95%. Without limitation, f 22 It can also be any of the following percentages or a range consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0399] In some embodiments, 50%≤f 22 <100%, optionally, 70%≤f 22 ≤90%. Without limitation, f 22It can also be any of the following percentages or a range consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, etc.

[0400] In some embodiments, the second negative electrode active layer satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0401] 0 <f 21 ≤50%, optionally, 10%≤f 21 ≤30%;

[0402] 50%≤f 22 <100%, optionally, 70%≤f 22 ≤90%.

[0403] By adjusting the proportion of natural graphite in the total mass of the second negative electrode active material (f 21 ) is controlled within the aforementioned range, which is beneficial to improving energy density while taking into account cycle performance.

[0404] When the second negative electrode active material includes artificial graphite and natural graphite, the ratio of natural graphite to the total mass of the second negative electrode active material (f 21 ) and the proportion of artificial graphite in the total mass of the second negative electrode active material (f 22 ) is controlled within the aforementioned range, which is beneficial to improving energy density while taking into account cycle performance.

[0405] In some embodiments, 0≤f 15 <50%, optionally, 0≤f 15 ≤30%, further optionally, 0≤f 15 ≤10%. 15 is the proportion of natural graphite in the total mass of the first negative electrode active material. In a non-limiting manner, f 15 It can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 1%, 2%, 4%, 5%, 6%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, 35%, 30%, 35%, 40%, 45%, etc.

[0406] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include carbon-coated negative electrode active particles;

[0407] The carbon-coated negative electrode active particles include a second negative electrode active body and a carbon coating layer located at at least a portion of the surface of the second negative electrode active body, and the carbon coating layer includes one or more of amorphous carbon, soft carbon and hard carbon.

[0408] In this application, unless otherwise specified, "amorphous carbon" refers to a transitional carbon material with a very low degree of graphitization and crystallization, which is close to an amorphous state (or has no fixed shape and periodic structural regularity). In this application, "amorphous carbon" refers to the product of carbonization treatment of an organic carbon source.

[0409] The definitions of "soft carbon" and "hard carbon" can be found above.

[0410] By arranging a carbon coating layer including one or more of amorphous carbon, soft carbon and hard carbon on the surface of the first negative electrode active material, a better lithium ion transmission channel can be provided for the first negative electrode active body, which is beneficial to promote lithium ion transmission, improve lithium replenishment efficiency, and further improve battery dynamics and cycle life.

[0411] Those skilled in the art can prepare carbon-coated negative electrode active particles using existing methods.

[0412] Without limitation, the carbon source precursor can be mixed with the negative electrode active body (which can be recorded as the second negative electrode active body), and then carbonized under conditions far below the graphitization temperature to form a carbon coating on the surface of the negative electrode active body. During the carbonization process, the organic components in the carbon source precursor undergo pyrolysis reaction and molecular rearrangement, so the temperature for carbonization treatment can also be called pyrolysis temperature. Non-limiting examples of carbon source precursors include asphalt, phenolic resin, etc. Typically, the graphitization temperature is greater than or equal to 2800°C, for example, 2800°C to 3200°C.

[0413] In some embodiments, taking the use of asphalt to prepare soft carbon coating of graphite as an example, a method including the following steps can be used for preparation: using asphalt (the softening point of asphalt is such as 150°C~200°C), thermal polymerization treatment is performed at 300°C~500°C for 2h~3h to form a soft carbon precursor, and further, carbonization treatment is performed at 800°C~1200°C for 1h~3h. The heating rate for carbonization treatment can be 5~10°C / min. The prepared carbon-coated negative electrode active particles include a graphite body, and the carbon coating layer located on at least a portion of the surface of the graphite body includes soft carbon.

[0414] In some embodiments, taking the use of asphalt to prepare graphite for hard carbon coating as an example, a method including the following steps can be used for preparation: using asphalt (the softening point of asphalt is such as 200°C~300°C), carbonization treatment is performed at 1200°C~2000°C for 1h~3h. The heating rate for carbonization treatment can be 10~20°C / min. The prepared carbon-coated negative electrode active particles include a graphite body, and the carbon coating layer located on at least a portion of the surface of the graphite body includes hard carbon.

[0415] In some embodiments, taking the use of asphalt to prepare graphite for amorphous carbon coating as an example, a method comprising the following steps can be used for preparation: subjecting asphalt (the softening point of asphalt is, for example, 70°C to 150°C) to carbonization treatment at 400°C to 700°C for 1h to 3h. The heating rate for the carbonization treatment can be 1-3°C / min. The prepared carbon-coated negative electrode active particles include a graphite body, and the carbon coating layer located on at least a portion of the surface of the graphite body includes amorphous carbon.

[0416] The test samples of carbon-coated negative electrode active particles can be obtained by the following method: the negative electrode sheets obtained by disassembling the battery cells are soaked and cleaned with a solvent (such as dimethyl carbonate (DMC)), and powders are scraped from different thickness positions to obtain powder samples of the first negative electrode material and the second negative electrode material, respectively.

[0417] In the present application, taking "amorphous carbon coating" as an example, the confirmation of amorphous carbon coating can be obtained by testing the conventional method of testing the crystalline form of carbon substances in the art, such as Raman spectroscopy testing and analysis, and the characteristic peak information of the carbon component in the spectrum (such as the intensity ratio of D peak / G peak, I D / G ) to analyze whether an amorphous carbon layer is formed. Among them, the D peak and the G peak are both Raman characteristic peaks of carbon atom crystals. The D peak represents the defects of the carbon atom crystals. The more defects there are, the greater the D peak intensity is. The D peak intensity can reflect the content of the amorphous (turbostratified stacking) region. The G peak represents the in-plane stretching vibration of the sp2 hybridization of carbon atoms. The G peak intensity can reflect the content of the graphitized (layered structure) region. As the degree of disorder of carbon atoms increases, the intensity ratio of the D peak to the G peak also increases. The Raman spectrum of the specific structural layer of the particle to be tested can also be compared. D / G Standard Raman spectrum of graphite I D / G The difference between them is used to determine whether it is an amorphous carbon layer.

[0418] In addition, graphite and amorphous carbon can also be distinguished based on X-ray diffraction (XRD) pattern analysis. Graphite has a relatively strong diffraction peak near 2θ of 26.5°, corresponding to the (002) crystal plane of graphite; while amorphous carbon has no obvious crystal structure and appears as a broadened peak in the XRD pattern.

[0419] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0420] The graphitization degree of the carbon coating layer in the first negative electrode active material is higher than the graphitization degree of the carbon coating layer in the second negative electrode active material;

[0421] The oxygen content of the carbon coating layer in the first negative electrode active material is lower than the oxygen content of the carbon coating layer in the second negative electrode active material.

[0422] In some embodiments, the graphitization degree of the carbon coating layer in the first negative electrode active material is higher than the graphitization degree of the carbon coating layer in the second negative electrode active material.

[0423] In this application, unless otherwise specified, "graphitization degree" has a well-known meaning in the art and can be used to measure the degree to which the crystals of a carbon material are close to perfect graphite. The graphitization degree can be tested using instruments and methods known in the art. As a non-limiting example, an X-ray diffractometer can be used for testing. The X-ray diffractometer can be a Bruker D8 Discover, Bruker D8 advance, etc., but is not limited thereto. The test can refer to JIS K 0131-1996, JB / T 4220-2011. First, the interlayer spacing d of the (002) crystal plane of the carbon material is measured. 002 The Bragg equation can be used to calculate the interlayer spacing of the (002) crystal plane; then the Franklin formula (Mering-Maire formula) is used to calculate G = [1-(0.344-d 002 ) / (0.344-0.3354)]×100%, where G is the graphitization degree (%), 0.3440 is the interlayer spacing of non-graphitized carbon (nm), 0.3354 is the interlayer spacing of an ideal graphite crystal (half of the c-axis lattice constant of hexagonal graphite, nm), and d 002 is the interlayer spacing of the carbon material (002) crystal plane expressed in nanometers (nm). It should be noted that in order to obtain a more accurate d 002 The diffraction angle can be corrected by adding Si powder to reduce the error.

[0424] The graphitization degree of the carbon coating layer can be controlled or adjusted by known methods in the art: during the carbonization treatment, the graphitization of the carbon coating layer can be improved by increasing the pyrolysis temperature, extending the holding time, reducing the heating rate, etc.

[0425] By controlling the carbon coating layer in the first negative electrode active material to have a higher degree of graphitization, it is beneficial to reduce the water content, which in turn helps to reduce the side reaction between water and the negative electrode lithium replenishing material, which helps to further improve the lithium replenishing efficiency and even more helps to extend the cycle life of the battery.

[0426] In some embodiments, the oxygen content of the carbon coating layer in the first negative electrode active material is lower than the oxygen content of the carbon coating layer in the second negative electrode active material.

[0427] In this application, unless otherwise specified, the "oxygen content" of the carbon coating layer of the negative electrode active material can be obtained by testing using the following method:

[0428] The test samples of carbon-coated negative electrode active particles can be obtained by the following method: the negative electrode sheets obtained by disassembling the battery cells are soaked and cleaned with a solvent (such as dimethyl carbonate (DMC)), and powders are scraped from different thickness positions to obtain powder samples of the first negative electrode material and the second negative electrode material respectively;

[0429] After cutting the powder into a cross section using FIB (focused ion beam), the oxygen content in the coating layer was analyzed using TEM (transmission electron microscope) combined with EDS (Energy Dispersive Spectrometer).

[0430] By controlling the carbon coating layer in the first negative electrode active material to have a lower oxygen content, it is beneficial to reduce water absorption, thereby reducing the side reaction between water and the negative electrode lithium replenishing material, further improving the lithium replenishing efficiency, and even more beneficial to extending the cycle life of the battery.

[0431] The oxygen content of the carbon coating layer can be controlled or adjusted by methods known in the art: during the carbonization treatment, the oxygen content of the carbon coating layer can be reduced by increasing the pyrolysis temperature, extending the insulation time, etc.

[0432] In some embodiments, the carbon-coated negative electrode active particles belong to coated negative electrode active particles. In this case, the second negative electrode active body belongs to the first negative electrode active body, and the carbon coating layer in the carbon-coated negative electrode active particles belongs to the coating layer in the coated negative electrode active particles.

[0433] In some embodiments, in the carbon-coated negative electrode active particles, the amorphous carbon in the carbon coating layer includes one or more of soft carbon and hard carbon. In this case, the carbon coating layer includes one or more of soft carbon and hard carbon.

[0434] In some embodiments, the carbon-coated negative electrode active particles satisfy one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0435] The thickness of at least a portion of the carbon coating layer is 1 nm to 10 nm, and can also be any of the following thicknesses or a range consisting of any two of the following thicknesses: 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.;

[0436] The average thickness of the carbon coating layer is 1 nm to 10 nm, and can also be any of the following thicknesses or a range consisting of any two of the following thicknesses: 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.;

[0437] The carbon coating layer includes soft carbon and hard carbon. The sum of the mass fractions of the soft carbon and the hard carbon in the carbon coating layer in the carbon-coated negative electrode active particles is 0.5%~10%, which can be optionally 1%~4%, and can also be any of the following percentages or within the range consisting of any two of the following percentages: 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.

[0438] In some embodiments, the mass fraction of the carbon coating layer in the carbon-coated negative electrode active particles is 0.5% to 10%, and can be optionally 1% to 4%. It can also be any of the following percentages or a range consisting of any two of the following percentages: 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.

[0439] In some embodiments, in the carbon-coated negative electrode active particles, the second negative electrode active body includes one or more of artificial graphite, silicon oxide, and silicon-carbon composite.

[0440] In some embodiments, the ratio of the sum of the mass of artificial graphite, silicon oxide and silicon-carbon composite to the total mass of carbon-coated negative electrode active particles can be found in 16 Without limitation, the sum of the mass of artificial graphite, silicon oxide and silicon-carbon composite in the total mass of carbon-coated negative electrode active particles may account for 80% to 100%, or any of the following percentages or a range selected from any two of the following percentages: 80%, 85%, 90%, 95%, 100%, etc.

[0441] In some embodiments, the second negative electrode active body includes artificial graphite.

[0442] In some embodiments, the proportion of artificial graphite in the total mass of the second negative electrode active body can be referred to as f 17 .

[0443] In some embodiments, the proportion of artificial graphite in the total mass of the second negative electrode active body can be 80% to 100%, or any of the following percentages or a range consisting of any two of the following percentages: 80%, 85%, 90%, 95%, 100%, etc.

[0444] In some embodiments, the first negative electrode active material includes secondary particles, and the second negative electrode active material includes a single particle.

[0445] In some embodiments, the mass proportion of secondary particles in the first negative electrode active material can be 60%~100%, optionally 80%~100%, or any of the following percentages or a range consisting of any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0446] In some embodiments, the mass proportion of a single particle in the second negative electrode active material can be 60% to 100%, optionally 80% to 100%, or any of the following percentages or a range selected from any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0447] In some embodiments, the amount of secondary particles in the first negative electrode active material can be 60% to 100%, optionally 80% to 100%, or any of the following percentages or a range consisting of any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0448] In some embodiments, the amount of single particles in the second negative electrode active material can be 60% to 100%, optionally 80% to 100%, or any of the following percentages or a range selected from any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0449] In some embodiments, the negative electrode plate satisfies one or two of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0450] The mass proportion or quantity proportion of the secondary particles in the first negative electrode active material is 60% to 100%, and can be optionally 80% to 100%;

[0451] The mass proportion or quantity proportion of the single particle in the second negative electrode active material is 60% to 100%, and can be optionally 80% to 100%.

[0452] Primary particles can be regarded as the basic crystal unit in the negative electrode active material, secondary particles refer to the agglomerates of primary particles, and single particles refer to non-agglomerated primary particles. The shape and structure of single particles are relatively simple, and often have a certain orientation. Secondary particles are aggregated from primary particles, and the secondary particles can have a relatively random or relatively disordered orientation on the whole particle. Therefore, the secondary particles are more isotropic.

[0453] By controlling one or more parameters of the mass proportion and number proportion of secondary particles in the first negative electrode active material, and the mass proportion and number proportion of single particles in the second negative electrode active material within the aforementioned range, it is beneficial to make the upper first negative electrode active material have stronger isotropy, which is beneficial to improve the lithium ion embedding path, and further beneficial to improve the lithium replenishment efficiency. In addition, it is also beneficial to improve battery dynamics.

[0454] Without limitation, the "number ratio of secondary particles in the first negative electrode active material" can be obtained by statistical analysis based on the SEM scan of the first negative electrode active material. Multiple areas are randomly selected for scanning test, the number of non-agglomerated primary particles and secondary particles in each area is counted, the number ratio of non-agglomerated primary particles in each area is calculated, and then the test values ​​of the number ratio of non-agglomerated primary particles in multiple test areas are averaged as the test value of "the number ratio of non-agglomerated primary particles in the first negative electrode active material".

[0455] Without limitation, the "number ratio of a single particle in the second negative electrode active material" can be obtained by statistical analysis based on the SEM scan of the second negative electrode active material. Multiple areas are randomly selected for scanning test, the number of non-agglomerated primary particles and secondary particles in each area is counted, the number ratio of non-agglomerated primary particles in each area is calculated, and then the test values ​​of the number ratio of non-agglomerated primary particles in multiple test areas are averaged as the test value of "the number ratio of non-agglomerated primary particles in the second negative electrode active material".

[0456] In some embodiments, the first negative electrode active material includes graphite secondary particles, and the second negative electrode active material includes graphite single particles.

[0457] In some embodiments, the mass proportion of graphite secondary particles in the first negative electrode active material is 60%~100%, optionally 80%~100%, and can also be any of the following percentages or within the range of any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0458] In some embodiments, the mass proportion of single graphite particles in the second negative electrode active material is 60% to 100%, and can be optionally 80% to 100%. It can also be any of the following percentages or within the range consisting of any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0459] In some embodiments, the amount of graphite secondary particles in the first negative electrode active material accounts for 60% to 100%, and can be optionally 80% to 100%. It can also be any of the following percentages or within the range of any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0460] In some embodiments, the amount of single graphite particles in the second negative electrode active material accounts for 60% to 100%, and can be optionally 80% to 100%. It can also be any of the following percentages or a range consisting of any two of the following percentages: 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0461] In some embodiments, the negative electrode plate satisfies one or two of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0462] The mass proportion or quantity proportion of the graphite secondary particles in the first negative electrode active material is 60% to 100%, and can be optionally 80% to 100%;

[0463] The mass proportion or quantity proportion of the graphite single particles in the second negative electrode active material is 60% to 100%, and can be optionally 80% to 100%.

[0464] Graphite primary particles can be used as the basic particle unit in graphite materials, graphite secondary particles refer to the agglomerates of graphite primary particles, and graphite single particles refer to non-agglomerated graphite primary particles. The isotropy of graphite secondary particles is stronger than that of graphite single particles.

[0465] By controlling one or more parameters of the mass proportion and number proportion of secondary graphite particles in the first negative electrode active material, and the mass proportion and number proportion of single graphite particles in the second negative electrode active material within the aforementioned range, it is beneficial to make the upper layer of the first negative electrode active material have stronger isotropy, which is beneficial to improving the embedding path of lithium ions, and further beneficial to improving the lithium replenishment efficiency. In addition, it is also beneficial to improve battery dynamics.

[0466] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0467] The first negative electrode active material and the second negative electrode active material each independently include a carbon-based material, and the graphitization degree of the carbon-based material in the first negative electrode active material is lower than the graphitization degree of the carbon-based material in the second negative electrode active material;

[0468] The sphericity of the first negative electrode active material is higher than the sphericity of the second negative electrode active material.

[0469] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include a carbon-based material, and the graphitization degree of the carbon-based material in the first negative electrode active material is lower than the graphitization degree of the carbon-based material in the second negative electrode active material.

[0470] By arranging a carbon-based material with a lower degree of graphitization in the first negative electrode active layer located in the upper layer, a larger interlayer spacing can be provided, which is more conducive to lithium insertion; in addition, the carbon-based material in the second negative electrode active layer located in the lower layer has a higher degree of graphitization, which can provide a more ordered layered structure that is conducive to the insertion and extraction of lithium ions, fewer defects and stronger conductivity, which is beneficial to improving the negative electrode capacity and the battery energy density.

[0471] The degree of graphitization of the carbon-based material can be controlled or adjusted by known methods in the art: in the process of preparing the carbon-based material, the degree of graphitization of the carbon-based material can be increased by increasing the heat treatment temperature, extending the heat treatment time, etc., or the degree of graphitization of the carbon-based material can be reduced by reducing the heat treatment temperature, shortening the heat treatment time, etc. In addition, the carbon-based material can be further heat-treated to increase its degree of graphitization.

[0472] The method for preparing soft carbon and hard carbon can refer to the relevant parameters for soft carbon coating and hard carbon coating in the previous article.

[0473] The method for preparing a graphite material may include the steps of crushing, screening, pre-carbonizing, and graphitizing the carbonaceous raw material. Both pre-carbonization and graphitization are heat treatment steps. After pre-carbonization, the particles shrink and the structure becomes denser; after further graphitization, the hexagonal carbon atom plane network is transformed from a disordered arrangement in two-dimensional space (such as a chaotic layer structure or amorphous carbon) to an ordered arrangement of graphite structure in three-dimensional space. Non-limiting examples of carbonaceous raw materials include raw coke raw materials, and further include petroleum coke. The temperature for pre-carbonization can be 1050°C~1150°C, but is not limited thereto. The temperature for graphitization is generally greater than or equal to 2800°C, and can be optionally 2800°C~3200°C.

[0474] In some embodiments, the step of preparing single graphite particles may include: crushing, classifying, pre-carbonizing, graphitizing and screening a carbonaceous raw material (such as a raw coke material, further such as petroleum coke).

[0475] In some embodiments, the step of preparing graphite secondary particles may include: mixing micro-particle carbon and a binder, granulating in a molten state of the binder, pre-carbonizing, graphitizing, and screening to prepare secondary particles. Micro-particle carbon is a carbon-containing raw material of a suitable size. The step of preparing micro-particle carbon may include: crushing, grading, and screening the carbon-containing raw material (such as raw coke raw material, further such as petroleum coke).

[0476] In some embodiments, the first negative electrode active material has a higher sphericity than the second negative electrode active material.

[0477] In this application, unless otherwise specified, the "sphericity" of the negative electrode active material refers to the ratio of the longest axis dimension to the shortest axis dimension in the particle. The closer the sphericity is to 1, the higher the sphericity is considered to be.

[0478] In the present application, the obtained negative electrode plate can be cut by plasma quenching, and the cross-sectional morphology of the obtained cross section can be observed under a scanning electron microscope (SEM). The longest axis dimension and the shortest axis dimension of the particles can be measured using image analysis software, and the sphericity can be calculated. Multiple particles in multiple scanning areas can be analyzed to obtain the average value of the sphericity.

[0479] The sphericity of the negative electrode active material can be controlled or adjusted by known methods in the art: Taking carbon-based materials as an example, the carbon-based materials can be melted at high temperature and then rapidly cooled so that the molten carbon-based materials form spherical particles under the action of surface tension. In addition, the sphericity of the carbon-based materials can be improved by using high-speed airflow, which can control the size and shape of the particles. For example, the carbon-based materials can be ground into spherical particles.

[0480] By controlling the sphericity of the first negative electrode active material to be higher than that of the second negative electrode active material, the first negative electrode active material is advantageously provided with a shorter lithium insertion channel, which is more advantageous for solid phase transmission, and is advantageous for better improving lithium replenishment efficiency and extending cycle life.

[0481] In some embodiments, the ratio of the thickness of the first negative electrode active layer to the sum of the thickness of the first negative electrode active layer and the second negative electrode active layer on a single side of the negative electrode current collector is denoted as f. H , satisfying 20%≤f H ≤70%, optionally, 30%≤f H ≤50%. Without limitation, f H It can also be any of the following percentages or a range consisting of any two of the following percentages: 20%, 30%, 40%, 50%, 60%, 70%, etc.

[0482] By calculating the ratio of the thickness of the first negative electrode active layer to the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer (f H, calculated on one side of the negative electrode current collector) within the aforementioned range is conducive to better balancing the higher lithium replenishment efficiency and better battery kinetics provided by the first negative electrode active layer and the overall energy density of the negative electrode sheet. In addition, by controlling f H The aforementioned range is more conducive to processing.

[0483] Furthermore, by regulating the compaction density of the second negative electrode active layer and / or the compaction density of the powder of the second negative electrode material, the comprehensive advantages of high lithium replenishment efficiency and high energy density can be better balanced.

[0484] In some embodiments, in the negative electrode sheet of the lithium ion secondary battery, the compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer.

[0485] In the present application, unless otherwise specified, the "compacted density of the second negative electrode active layer" in the negative electrode sheet refers to the ratio of the mass to the volume of the second negative electrode active layer, and the "compacted density of the first negative electrode active layer" in the negative electrode sheet refers to the ratio of the mass to the volume of the first negative electrode active layer.

[0486] In a non-limiting manner, the compaction density of the second negative electrode active layer may be increased by adjusting the particle size of the second negative electrode active material, but is not limited thereto.

[0487] Regarding the compaction density test of the first negative electrode active layer and the second negative electrode active layer in the negative electrode sheet of a lithium-ion secondary battery, the battery can be disassembled to obtain the negative electrode sheet, dried, and punched into small discs of a certain area A0. The first negative electrode material powder of a certain thickness d1 in the first negative electrode active layer is scraped from the corresponding thickness position, and the powder mass M1 is weighed. The compaction density PD1=M1 / (A0×d1) of the first negative electrode active layer can be calculated. Multiple small discs are tested and the average value is taken. The second negative electrode material powder of a certain thickness d2 in the second negative electrode active layer is also scraped from the corresponding thickness position, and the powder mass M2 is weighed. The compaction density PD2=M2(A0×d2) of the second negative electrode active layer can be calculated. Multiple small discs are tested and the average value is taken.

[0488] By adjusting the compaction density of the second negative electrode active layer to be higher than that of the first negative electrode active layer, it is beneficial to improve the energy density of the lithium-ion secondary battery and to simultaneously achieve both high energy density and high lithium replenishment efficiency.

[0489] In this application, unless otherwise specified, the "compacted density" of an electrode sheet has a meaning well known in the art and is one of the reference indicators of material energy density. The compacted density of an electrode sheet refers to the ratio of the mass of the electrode active material layer to its volume. The compacted density of a positive electrode sheet refers to the ratio of the mass of the positive electrode active material layer to its volume, and the compacted density of a negative electrode sheet refers to the ratio of the mass of the negative electrode active material layer to its volume. The compacted density of any active layer structure in the "electrode active material layer" refers to the ratio of the mass of the active layer structure to its volume. Similarly, the compacted density of a lithium-supplemented negative electrode sheet refers to the ratio of the sum of the masses of each negative active initial layer in the lithium-supplemented negative electrode sheet to the total volume; the compacted density of any active initial layer in a lithium-supplemented negative electrode sheet refers to the ratio of the mass of the active initial layer to its volume.

[0490] In some embodiments, in the lithium-supplemented negative electrode sheet, the compaction density of the second negative electrode active initial layer is higher than the compaction density of the first negative electrode active initial layer.

[0491] Without limitation, the compaction density of the negative electrode sheet in the lithium-ion secondary battery can be tested by the following method: disassemble the battery cell, take out the negative electrode sheet, and punch it into 1540.25 mm 2 Take a small disc, measure the mass M and thickness L of the small disc, take the negative electrode sheet from another area, wipe off the negative electrode active material layer on the surface, remove the remaining negative electrode current collector foil (which can be recorded as empty negative electrode current collector foil), and also punch it into 1540.25mm 2 The mass of the empty negative electrode collector foil is weighed as M0 and the thickness is L0, then the compaction density of the negative electrode sheet is PD = (M-M0) / [1.54025 × (L-L0)]. The compaction density of the negative electrode sheet measured by disassembling the battery after the battery is fully discharged corresponds to the compaction density of the negative electrode sheet when the battery is fully discharged; the compaction density of the negative electrode sheet measured by disassembling the battery after the battery is fully charged corresponds to the compaction density of the negative electrode sheet when the battery is fully charged.

[0492] It is understandable that the negative electrode sheet in the lithium-ion secondary battery is relative to the "lithium-supplemented negative electrode sheet that has been rolled and added with a lithium-supplemented layer but has not yet been assembled into an electrode assembly". The negative electrode sheet in the battery usually rebounds after being infiltrated with the electrolyte, resulting in the compaction density of the negative electrode sheet in the battery usually being lower than the compaction density of the lithium-supplemented negative electrode sheet. Furthermore, after the formation process, the negative electrode active material reacts with the electrolyte at the interface to form a solid electrolyte interface (SEI) film on the surface of the negative electrode active material. The SEI film will also have a certain impact on the compaction density of the negative electrode active material, but the impact is relatively small. In addition, in lithium-ion secondary batteries, the compaction density of the negative electrode sheet and the negative electrode active layers it contains is also related to the charge and discharge state. The negative electrode sheet expands in the charged state, and the negative electrode sheet shrinks in the discharged state. Without limitation, based on the volume of the "lithium-supplemented negative electrode sheet that has been rolled and added with a lithium-supplemented layer but has not yet been assembled into an electrode assembly" or the volume of the negative electrode active initial layer therein, the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer therein in the fully charged state of the lithium-ion secondary battery can be 1.2-1.4, and the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer therein in the fully discharged state of the lithium-ion secondary battery can be 1.05-1.2. Without limitation, based on the volume of the "lithium-supplemented negative electrode sheet that has been rolled and added with a lithium-supplemented layer but has not yet been assembled into an electrode assembly" or the volume of the negative electrode active initial layer therein, the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer therein in the fully charged state of the lithium-ion secondary battery can also be any of the following values ​​or a range selected from any two of the following values: 1.20, 1.2, 1.25, 1.26, 1.28, 1.30, 1.3, 1.32, 1.34, 1.35, 1.36, 1.38, 1.4, 1.40, etc. Without limitation, based on the volume of the "lithium-supplemented negative electrode sheet that has been rolled and added with a lithium-supplemented layer but has not yet been assembled into an electrode assembly" or the negative electrode active initial layer therein, the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer therein in the fully discharged state of the lithium-ion secondary battery can also be any of the following values ​​or a range consisting of any two of the following values: 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, 1.2, etc. It can be understood that the compaction density of the negative electrode sheet or the negative electrode active layer therein in the lithium-ion secondary battery can be calculated by dividing the compaction density of the "lithium-supplemented negative electrode sheet that has been rolled and added with a lithium-supplemented layer but has not yet been assembled into an electrode assembly" or the negative electrode active initial layer therein by the corresponding volume expansion coefficient.

[0493] It can be understood that the "lithium-supplemented negative electrode sheet that has been rolled to add a lithium-supplemented layer but has not yet been assembled into an electrode assembly" has not yet come into contact with the electrolyte and has not yet been soaked by the electrolyte.

[0494] In some embodiments, the compaction density of the “lithium-supplemented negative electrode sheet that has been rolled to add a lithium-supplemented layer but has not yet been assembled into an electrode assembly” is 1.3 g / cm 3 ~1.8g / cm 3 , optional 1.4g / cm 3 ~1.6 g / cm 3 , can also be any of the following values ​​or a range consisting of any two of the following values: 1.3 g / cm 3 , 1.30 g / cm 3 , 1.35 g / cm 3 , 1.40 g / cm 3 , 1.45g / cm 3 , 1.50 g / cm 3 , 1.55 g / cm 3 , 1.60 g / cm 3 , 1.65 g / cm 3 , 1.70 g / cm 3 , 1.71 g / cm 3 , 1.75 g / cm 3 , 1.8 g / cm 3 , 1.80 g / cm 3 wait.

[0495] In addition, regarding the compaction density of the first negative electrode active initial layer and the second negative electrode active initial layer in the negative electrode sheet obtained by cold pressing (without the addition of the lithium supplement layer), the compaction density of the different negative electrode active initial layers can be calculated based on the coating surface density of the different negative electrode active initial layers and the thickness of the different negative electrode active initial layers after drying.

[0496] In the present application, unless otherwise specified, the term “cold pressed negative electrode sheet (without additional lithium supplement layer)” refers to a state where the first negative electrode active initial layer located on the upper layer has been cold pressed but a lithium supplement layer has not yet been added to the first negative electrode active initial layer.

[0497] In some embodiments, under the same test conditions, the powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

[0498] In this application, unless otherwise specified, "powder compaction density" has a well-known meaning in the art, and refers to the ratio of mass to volume of the powder material after compaction under a certain pressure. The "powder compaction density" of the negative electrode material can be measured using instruments and methods known in the art. For example, it can be measured using an electronic pressure testing machine (such as UTM7305) with reference to standard GB / T24533-2009. An exemplary test method is as follows: weigh a negative electrode material with a mass of M (such as 1 g), add a bottom area of ​​A (such as 1.327 cm 2 ) in a mold, pressurize to a certain pressure P (such as 3 tons (3T) to 5 tons pressure, further such as 3T, 4T, 5T, etc.), maintain the pressure for a certain time (such as 3T for 30 seconds), then release the pressure, maintain for a period of time (such as 10 seconds), and then record and calculate the powder compaction density of the negative electrode material under the pressure P. The first negative electrode material in the first negative electrode active layer and the second negative electrode material in the second negative electrode active layer can be obtained by the above method.

[0499] By controlling the powder compaction density of the second negative electrode material to be higher than the powder compaction density of the first negative electrode active material, it is beneficial to give the second negative electrode active layer a higher compaction density during the cold pressing process of the pole piece.

[0500] It can be understood that for lithium-ion secondary batteries, the relative size of the powder compaction density of the negative electrode material in different negative electrode active layers can be judged based on the relative size of the powder compaction density test values ​​obtained under the same sample parameters and test conditions. Generally, the comparison can be made based on the relative size of the powder compaction density test values ​​under the same test pressure. Similarly, for lithium-supplemented negative electrode sheets, the relative size of the powder compaction density of the negative electrode material in different negative electrode active initial layers can also be judged based on the relative size of the powder compaction density test values ​​obtained under the same sample parameters and test conditions.

[0501] For the powder compaction density of the negative electrode active material, the state in the negative electrode sheet of the lithium-ion secondary battery can be recorded as the first state, the state in the cold-pressed negative electrode sheet (without the addition of the lithium supplement layer) or the state in the lithium supplemented negative electrode sheet with the additional lithium supplement layer after rolling can be recorded as the second state, and the state of the negative electrode active material used to prepare the negative electrode sheet before being subjected to cold pressing can be recorded as the third state. The third state can include the state of powder raw materials, the state of being suspended in the negative electrode slurry, and the state of being coated on the surface of the negative electrode current collector; the powder compaction density of the negative electrode active material in the third state is equal to or close to the powder compaction density in the powder raw material state in terms of value. In the second state, after the cold pressing treatment (without the addition of the lithium supplement layer) or the addition of the lithium supplement layer after rolling, the particles of the negative electrode active material may be deformed or even broken. Therefore, after re-extracting the powder sample of the negative electrode active material and re-measuring the powder compaction density, the powder compaction density may be different in value from the powder compaction density in the powder raw material state. In the first state, the negative electrode active material is in contact with the electrolyte and is soaked by the electrolyte; after formation, the negative electrode active material is charged for the first time, and there are embedded lithium ions. In addition, an SEI film is formed on the surface of the negative electrode active material; if the battery undergoes a charge and discharge cycle, the negative electrode active material undergoes reversible insertion and extraction of lithium ions. In the charging state, the negative electrode active material is embedded with lithium ions, and in the discharging state, the lithium ions embedded in the negative electrode active material are extracted; therefore, it can be understood that in the first state and the third state, the powder compaction density of the negative electrode active material may also be different to a certain extent. The "first", "second" and "third" in the aforementioned "first state", "second state" and "third state" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.

[0502] Although the compaction density of the negative electrode active material powder may have certain numerical differences under different conditions, it does not affect the judgment of the relative size of the compaction density of the negative electrode material powder in different negative electrode active layers.

[0503] In some embodiments, the negative electrode plate satisfies one or both of the following characteristics:

[0504] The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer;

[0505] The powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

[0506] By controlling the second negative electrode active layer located in the lower layer to have a higher compaction density and / or the second negative electrode material to have a higher powder compaction density, it is beneficial to improve the energy density of the lower layer, so that the negative electrode plate can have a higher energy density and a higher lithium replenishment efficiency and better battery dynamics.

[0507] In some embodiments, when the battery is fully discharged, the compaction density of the negative electrode sheet can be 1.08 g / cm 3 ~1.71 g / cm 3 , optional 1.17g / cm 3 ~1.52 g / cm 3 Without limitation, when the battery is fully discharged, the compaction density of the negative electrode sheet can also be any of the following values ​​or a range consisting of any two of the following values: 1.08 g / cm 3 , 1.10 g / cm 3 , 1.15 g / cm 3 , 1.20 g / cm 3 , 1.25 g / cm 3 , 1.30 g / cm 3 , 1.35 g / cm 3 , 1.40 g / cm 3 , 1.45 g / cm 3 , 1.50 g / cm 3 , 1.55 g / cm 3 , 1.60 g / cm 3 , 1.65 g / cm 3 , 1.70 g / cm 3 , 1.71 g / cm 3 wait.

[0508] In some embodiments, when the battery is fully discharged, the surface density of the negative electrode sheet in the lithium-ion secondary battery can be 10 mg / cm 2 ~26mg / cm 2 , optional 15 mg / cm 2 ~20mg / cm 2 In a non-limiting manner, when the battery is fully discharged, the surface density of the negative electrode plate in the lithium-ion secondary battery can also be any of the following values ​​or a range consisting of any two of the following values: 10 mg / cm 2 , 12 mg / cm 2 , 15 mg / cm 2 , 16 mg / cm 2 , 18 mg / cm 2 , 20 mg / cm 2 , 22 mg / cm 2, 24 mg / cm 2 , 25 mg / cm 2 , 26 mg / cm 2 wait.

[0509] In this application, unless otherwise specified, the "area density" of an electrode sheet has a well-known meaning in the art, and refers to the ratio of the mass to the area of ​​the electrode active material layer in the electrode sheet. When the electrode active material layer is disposed on both sides of the current collector, the areal density of the electrode sheet is equal to the ratio of the total mass of the electrode active material layers on both sides to the area of ​​the electrode active material layers.

[0510] For the electrode sheet obtained by cold pressing (corresponding to the negative electrode, it refers to the state where the lithium supplement layer has not yet been added), the compaction density can be calculated using the following formula:

[0511] Compacted density = coating surface density / thickness of electrode active material layer, coating surface density = coating dry weight of electrode slurry / area of ​​electrode active material layer.

[0512] The thickness of the electrode active material layer on both sides corresponds to the sum of the coating surface density on both sides, and the thickness on one side corresponds to the coating surface density on one side; when the electrode active material layers on both sides of the current collector are basically the same, it can be calculated according to the following formula: compaction density = coating surface density on one side / thickness on one side of the electrode active material layer. The "one side" and "both sides" of the electrode active material layer refer to the position distribution of the current collector.

[0513] For the compaction density of the lithium-supplemented negative electrode sheet (not yet assembled into an electrode assembly) with an additional lithium-supplemented layer after rolling, the corresponding compaction density can be calculated using the following formula: compaction density = mass of the negative electrode active material layer (excluding the lithium-supplemented layer) / volume of the negative electrode active material layer, where both mass and volume are calculated based on the total amount on both sides.

[0514] For the compaction density of the negative electrode sheet (after wetting and formation) in the lithium-ion secondary battery, the corresponding compaction density can be calculated by the following formula: compaction density = mass of the negative electrode active material layer / volume of the negative electrode active material layer, mass and volume are calculated based on the total amount on both sides; after the battery is fully discharged, the battery cell can be disassembled and the electrode sheet can be taken for testing. It can be understood that the rebound degree of the negative electrode sheet has little or no effect on the surface density of the negative electrode sheet; the negative electrode SEI film formed by formation will have a certain effect on the surface density of the electrode sheet, but the effect is small; the charge and discharge state of the battery may also have a certain effect on the surface density of the electrode sheet, but in the fully discharged state, it can be considered that the surface density of the negative electrode sheet is relatively small. Therefore, it can generally be considered that the surface density of the electrode sheet in the lithium-ion secondary battery in the fully discharged state is not much different from the surface density of the lithium-supplemented negative electrode sheet (not yet assembled into an electrode assembly).

[0515] In some embodiments, the negative electrode plate in the lithium-ion secondary battery satisfies one or two of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0516] When the battery is fully discharged, the compaction density of the negative electrode is 1.08g / cm 3 ~1.71g / cm 3 , optional 1.17g / cm 3 ~1.52g / cm 3 ;

[0517] When the battery is fully discharged, the surface density of the negative electrode is 10 mg / cm 2 ~26mg / cm 2 , optional 15mg / cm 2 ~20mg / cm 2 .

[0518] By controlling the compaction density and / or surface density of the negative electrode plate within the aforementioned range, it is also beneficial for the battery to have a higher energy density.

[0519] In some exemplary embodiments, by adjusting one or both of the compaction density and the surface density of the negative electrode sheet within the aforementioned range, it is beneficial to balance the battery kinetics and the energy density.

[0520] In some exemplary embodiments, by adjusting one or both of the compaction density and the surface density of the negative electrode sheet within the aforementioned range, it is beneficial to simultaneously achieve high energy density and high lithium replenishment efficiency.

[0521] In some embodiments, in the negative electrode sheet of the lithium-ion secondary battery, a lithium supplement residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer.

[0522] In some embodiments, a lithium-ion secondary battery is provided, which includes a negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; a lithium-supplementing residual layer exists on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0523] In some embodiments, a lithium-ion secondary battery is provided, which includes a negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the lithium insertion rate of the first negative electrode active material is higher than the lithium insertion rate of the second negative electrode active material; a lithium supplement residual layer exists on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0524] In some embodiments, a lithium-ion secondary battery is provided, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the separator is arranged between the positive electrode plate and the negative electrode plate; the negative electrode plate includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer arranged in sequence on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material; the lithium insertion rate of the first negative electrode active material is higher than the lithium insertion rate of the second negative electrode active material; and a lithium supplement residual layer exists on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0525] In some embodiments, a lithium ion secondary battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector; the first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material;

[0526] The lithium insertion potential of the first negative electrode active material is higher than that of the second negative electrode active material, and a lithium supplement residual layer exists on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0527] In some embodiments, in the negative electrode sheet of the lithium-ion secondary battery, a lithium-replenishing residual layer exists on the surface of the first negative electrode active layer away from the second negative electrode active layer; further, the lithium-replenishing residual layer contains inactive lithium.

[0528] A non-limiting example of inactive lithium is lithium oxide.

[0529] In the present application, unless otherwise specified, in a lithium-ion secondary battery, the "lithium-replenishing residual layer" in the negative electrode sheet refers to a structural layer in which at least a portion of the components contained are the same as the residue after lithium replenishment using the lithium-replenishing layer. Unless otherwise specified, the "lithium-replenishing layer" refers to a structural layer containing a lithium-replenishing material. As a non-limiting example, the lithium-replenishing layer can be a lithium sheet. The lithium-replenishing material contained in the lithium-replenishing layer provided in the corresponding lithium-replenishing negative electrode sheet can also be referred to as a negative electrode lithium-replenishing material.

[0530] In some embodiments, in the negative electrode sheet of a lithium-ion secondary battery, a lithium-replenishing residual layer exists on the surface of the first negative electrode active layer away from the second negative electrode active layer, the lithium-replenishing residual layer contains inactive lithium, and the thickness of the lithium-replenishing residual layer is less than 0.1 μm (measured on a single side of the negative electrode current collector based on the lithium-replenishing residual layer).

[0531] In some embodiments, in the negative electrode sheet of the lithium-ion secondary battery, the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer is less than or equal to 98%, optionally less than or equal to 70%, calculated on a single side of the negative electrode current collector. In some embodiments, in the negative electrode sheet, the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer is greater than 0 and less than or equal to 90% calculated on a single side of the negative electrode current collector. In some of these embodiments, in the negative electrode sheet, the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer is greater than 0 and less than or equal to 70% calculated on a single side of the negative electrode current collector. Without limitation, in the negative electrode sheet, based on the single side of the negative electrode current collector, the coverage area percentage of the lithium supplement residual layer relative to the first negative electrode active layer can also be any of the following percentages, or selected from any two of the following percentages: 0.1%, 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, 98%, etc. Without limitation, based on the single side of the negative electrode current collector, the coverage area percentage of the lithium supplement residual layer relative to the first negative electrode active layer can be selected from any suitable range as follows: greater than 0 and less than or equal to 50%, 30% to 98%, 30% to 70%, 30% to 50%, 50% to 98%, 50% to 70%, etc.

[0532] In some embodiments, the thickness of the lithium supplement residual layer is less than 0.1 μm, optionally less than 0.08 μm, and further optionally less than 0.05 μm, based on the single side of the negative electrode current collector. Without limitation, the thickness of the lithium supplement residual layer (based on the single side of the negative electrode current collector) can also be any of the following values, less than any of the following values, or a range selected from any two of the following values: 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, etc.

[0533] In some embodiments, the negative electrode plate in the lithium-ion secondary battery satisfies one or both of the following characteristics:

[0534] Measured on a single side of the negative electrode current collector, the thickness of the lithium supplement residual layer is less than 0.1 μm, optionally, less than 0.08 μm, further optionally, less than 0.05 μm (can also be selected from any suitable value or range in the context);

[0535] Measured on a single side of the negative electrode current collector, the coverage area percentage of the lithium-supplemented residual layer relative to the first negative electrode active layer is less than or equal to 98%, and can be selected as 30% to 98%, further selected as 50% to 98% or 30% to 70%, and further selected as 50% to 70% (can also be selected from any suitable value or range in the context).

[0536] In the present application, unless otherwise specified, "the thickness of the lithium-replenishing residual layer" refers to the thickness on a single side of the negative electrode current collector. As an example, the cross-section of the negative electrode plate can be microscopically observed to confirm the thickness of the lithium-replenishing residual layer, for example, whether the thickness of the lithium-replenishing residual layer is less than 0.1 μm. The definition of "cross-section of the negative electrode plate" is consistent with the above. The surface of the negative electrode plate can also be microscopically observed and combined with elemental analysis (such as EDS, XRD, etc.) to confirm the percentage of coverage area of ​​the lithium-replenishing residual layer relative to the first negative electrode active layer. For example, the covered area and uncovered area of ​​the lithium-replenishing residual layer can be distinguished based on the distribution difference of carbon elements and / or silicon elements.

[0537] Taking lithium foil as an example, when the lithium foil is fully in contact with the electrolyte and reacts, the thickness of the lithium-supplemented residual layer formed may be much lower than 0.1 μm, such as less than 0.05 μm, or less than 0.02 μm.

[0538] In the process of providing a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer for lithium replenishment treatment, if the active lithium provided by the negative electrode lithium replenishment material is not able to be embedded into the negative electrode active material in time and becomes inactivated, a lithium replenishment residual layer including inactive lithium may be formed at the position of the lithium replenishment layer.

[0539] By controlling one or both of the thickness of the lithium replenishment residual layer and the coverage area percentage of the lithium replenishment residual layer relative to the first negative electrode active layer within the aforementioned range, it is beneficial to achieve efficient lithium replenishment of the negative electrode while also making the lithium replenishment residual layer have a more suitable thickness and / or coverage area percentage, which is beneficial to better achieve good electrolyte infiltration performance and charge transfer performance, and is beneficial to making the battery have good battery dynamics.

[0540] Better battery kinetics is beneficial to giving the battery a lower internal resistance.

[0541] In some embodiments, a plurality of micropores are provided on a surface of the negative electrode current collector on one side close to the second negative electrode active layer.

[0542] By setting a plurality of micropores on the surface of the negative electrode current collector close to the second negative electrode active layer, it is helpful to promote the infiltration of the negative electrode plate by the electrolyte, which can increase the lithium insertion rate after the first infiltration and help improve the lithium replenishment efficiency.

[0543] In some embodiments, the negative electrode current collector satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0544] The micropores penetrate the negative electrode current collector along the thickness direction of the negative electrode current collector;

[0545] The pore size of the micropores is 5 μm~500 μm, and can be optionally 30 μm~200 μm.

[0546] In this application, unless otherwise specified, the "pore size" of the micropores in the negative electrode current collector refers to the maximum size in each dimension along the micropore profile of the projection of the negative electrode current collector. Without limitation, the pore size of the micropores can also be any of the following sizes or a range consisting of any two of the following sizes: 5μm, 10μm, 15μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 120μm, 150μm, 160μm, 180μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm, 500μm, etc.

[0547] In the present application, the size of the micropores in the negative electrode current collector can be observed and analyzed by taking a photo under an optical microscope, or by taking a photo under a SEM to measure and analyze.

[0548] By controlling the micropores to penetrate the negative electrode current collector along the thickness direction of the negative electrode current collector, it is more conducive to promoting the infiltration of the negative electrode plate by the electrolyte, which can better improve the lithium insertion rate after the first infiltration and is more conducive to improving the lithium replenishment efficiency.

[0549] By controlling the pore size of the micropores within the aforementioned range, the lithium replenishment efficiency is improved while also taking into account the mechanical strength and processability of the negative electrode current collector.

[0550] In some embodiments, a plurality of micropores are provided on the surface of the negative electrode current collector on one side close to the second negative electrode active layer, and the shape of the micropores is not particularly limited, and can be any suitable shape such as circular, elliptical, square, etc. In some embodiments, the micropores are circular holes, in which case the pore size of the micropores corresponds to the diameter of the circular hole.

[0551] In some embodiments, on the surface of the negative electrode collector close to the second negative electrode active layer, the proportion of micropore area to the negative electrode collector area can be 30% to 80%, optionally 40% to 60%, or any of the following percentages, or selected from any two of the following percentages: 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, etc.

[0552] In some embodiments, on the surface of the negative electrode current collector close to the second negative electrode active layer, along the X direction, the total length of the micropores may account for 30% to 80% of the height of the negative electrode current collector, and may be 40% to 60%, or may be any of the following percentages, or any two of the following percentages 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, etc. The X direction corresponds to the height direction of the pole piece or the extension direction of the pole ear, and in the wound cell, the X direction is perpendicular to the winding direction.

[0553] In some embodiments, the NP ratio of the lithium ion secondary battery is 1.05-1.3, and can be optionally 1.1-1.3. The NP ratio of the lithium ion secondary battery is equal to the ratio of the negative electrode surface capacity to the positive electrode surface capacity.

[0554] Without limitation, the NP ratio of the lithium ion secondary battery can also be any of the following values ​​or a range consisting of any two of the following values: 1.05, 1.06, 1.08, 1.10, 1.12, 1.14, 1.15, 1.16, 1.18, 1.20, 1.22, 1.24, 1.25, 1.26, 1.28, 1.30, etc.

[0555] In some embodiments, the NP ratio of the lithium ion secondary battery is 1.1 to 1.2.

[0556] In this application, unless otherwise specified, the "NP ratio" of a lithium-ion secondary battery refers to the ratio of the negative electrode capacity to the positive electrode capacity, which can be expressed in English as Negative / Positive Ratio. The "NP ratio" of a lithium-ion secondary battery can be obtained by testing using conventional methods in the art.

[0557] In some embodiments, the following methods can be used to test the negative electrode capacity and the positive electrode capacity respectively:

[0558] Negative electrode capacity test: fully charge the battery, disassemble the cell, take the negative electrode sheet, and punch it into small discs with a diameter of 14 mm (corresponding to area A N ), separate the small disc from the lithium sheet with an isolation film, add electrolyte and package into 4 button-type half-cells; use a 0.1C rate to charge and discharge for 1 cycle in the voltage range of 0.005V~2V, and take the average of the discharge capacity of the 4 batteries to get the negative electrode capacity CN , negative electrode surface capacity = negative electrode capacity ÷ area A N .

[0559] Positive electrode capacity test: disassemble the battery cell, take the positive electrode sheet and punch it into small discs with a diameter of 14 mm (corresponding to area A P ), separate the small disc from the lithium sheet with an isolation film, add electrolyte and package into 4 button-type half-cells; use a 0.1C rate to charge and discharge for 1 cycle in the voltage range of 2.5V~3.65V, and take the average of the discharge capacities of the 4 batteries to get the positive electrode capacity C P , positive electrode surface capacity = positive electrode capacity ÷ area A P .

[0560] NP ratio of lithium-ion secondary battery = negative electrode surface capacity / positive electrode surface capacity; N Equal to A P In the case of , the following formula can also be used: NP ratio = C N / C P .

[0561] By controlling the NP ratio of the lithium-ion secondary battery within the aforementioned range, it is beneficial for the negative electrode to store more lithium ions, which is convenient for continuously releasing the supplementary capacity in the later stages of cycling or storage, and can better extend the battery cycle life.

[0562] It can be understood that the lithium-ion secondary battery also includes a positive electrode plate, and the positive electrode plate includes a positive electrode active material.

[0563] It will be appreciated that the positive electrode active material includes a lithium ion active material.

[0564] In some embodiments, the positive electrode active material includes one or more of lithium composite metal oxides, lithium-containing phosphates, and modified forms of any of the foregoing positive electrode active materials; the modified forms include one or more of doping modification and coating modification.

[0565] In some embodiments, the positive electrode plate includes a positive electrode active material, and the positive electrode active material may include one or more of a ternary positive electrode material, lithium iron phosphate, lithium iron manganese phosphate, and a modified form of any of the foregoing positive electrode active materials; the modified form includes one or more of doping modification and coating modification. Among them, the positive electrode active material may include one or more of a ternary positive electrode material, a modified form of a ternary positive electrode material, lithium iron phosphate, a modified form of lithium iron phosphate, lithium iron manganese phosphate, and a modified form of lithium iron manganese phosphate, and the modified form includes one or more of doping modification and coating modification.

[0566] In this application, unless otherwise specified, "lithium composite metal oxide" refers to a lithium ion active material including lithium, non-lithium metal elements and oxygen elements, which is used as a positive electrode active material. Generally, the non-lithium metal elements in the lithium composite metal oxide include transition metal elements, and therefore, the lithium composite metal oxide may also be referred to as "lithium transition metal oxide".

[0567] In the present application, unless otherwise specified, "lithium-containing phosphate" refers to a lithium ion active material including lithium, transition metal elements and phosphate, used as a positive electrode active material. Generally, the lithium-containing phosphate used as a positive electrode active material may have an olivine structure. Non-limiting examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0568] In this application, unless otherwise specified, "a modified form of a positive electrode active material" includes the positive electrode active material itself and the modified element. Furthermore, the modified element may exist in the form of a doping element, a coating element, or a combination of a doping element and a coating element. Unless otherwise specified, "a modified form of a positive electrode active material" still falls within the scope of positive electrode active materials.

[0569] In the present application, unless otherwise specified, the "doping element" involved in the positive electrode active material refers to the modified element doped in the positive electrode active material; unless otherwise specified, the "coating element" involved in the positive electrode active material refers to the positive electrode active material including the positive electrode active particle body and the coating layer located at least a part of the surface of the positive electrode active particle body, wherein the coating element is the modified element located in the coating layer. As a non-limiting example, in the positive electrode active material, "the modified element exists in a combination of the doping element and the coating element" means that the positive electrode active material includes the positive electrode active particle body and the coating layer located at least a part of the surface of the positive electrode active particle body, at least a part of the modified element is doped in the positive electrode active material body, and at least a part of the modified element is also contained in the coating layer. The positive electrode active particle body can be the positive electrode active material itself or its doped and modified form. In some embodiments, the doping element can include one or more of Na, K, Ca, Ba, Sb, Ti, Zr, W, Sr, Nb, Mo, Si, Mg, B, Cr, Ta, etc. In some embodiments, the coating element may include one or more of Ti, Mg, Nb, C, and the like.

[0570] In this application, unless otherwise specified, "ternary cathode material" refers to one or more of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. The chemical formula of the ternary cathode material can be: The ternary cathode material is a lithium ion active material.

[0571] In the present application, unless otherwise specified, "lithium ion active material" refers to a positive electrode active material that can provide active lithium ions at the positive electrode.

[0572] In the present application, unless otherwise specified, "lithium ion active material" refers to a positive electrode active material that can provide active lithium ions in the positive electrode.

[0573] In some embodiments, the positive electrode active material includes a lithium iron phosphate-based positive electrode active material. The "lithium iron phosphate-based positive electrode active material" includes at least a lithium iron phosphate body, and further may include a carbon coating layer located at least a portion of the surface of the lithium iron phosphate body, and optionally, the carbon coating layer may include one or more of soft carbon, hard carbon and amorphous carbon.

[0574] Without limitation, the lithium iron phosphate-based positive electrode active material may include carbon-coated lithium iron phosphate, which includes a lithium iron phosphate body and a carbon coating layer located on at least a portion of the surface of the lithium iron phosphate body. Optionally, the carbon coating layer may include one or more of soft carbon, hard carbon and amorphous carbon.

[0575] Those skilled in the art can use conventional techniques to select and regulate the mass proportion of the carbon coating layer in the lithium iron phosphate-based positive electrode active material (an example of the lithium iron phosphate-based positive electrode active material is carbon-coated lithium iron phosphate) and the thickness or average thickness of the carbon coating layer. Non-limitingly, the mass proportion of the carbon coating layer in the lithium iron phosphate-based positive electrode active material (such as carbon-coated lithium iron phosphate) can be 0.2%~2%, but is not limited to this. Non-limitingly, in the lithium iron phosphate-based positive electrode active material, the average thickness of the carbon coating layer can be 10nm~20nm, but is not limited to this.

[0576] The lithium-ion secondary battery provided above can flexibly select a variety of positive electrode active materials. Non-limitingly, the mass proportion of the carbon coating layer in the carbon-coated lithium iron phosphate can be 0.5%~2%, but not limited to this. Non-limitingly, in the carbon-coated lithium iron phosphate, the average thickness of the carbon coating layer can be 10nm~20nm, but not limited to this.

[0577] When the lithium iron phosphate-based positive electrode active material includes a carbon coating layer, for example, when the positive electrode active material includes carbon-coated lithium iron phosphate, the conductivity of the surface of the lithium iron phosphate body can be improved, and the conductive network inside the positive electrode sheet can be optimized, thereby improving the battery cycle performance.

[0578] In some embodiments, a lithium-ion secondary battery includes a battery cell.

[0579] In this application, unless otherwise specified, "battery cell" refers to a basic unit that can realize the mutual conversion of chemical energy and electrical energy, and further, generally includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, which mainly prevents the positive and negative electrodes from short-circuiting, and allows ions to pass through.

[0580] The following is some description about the positive electrode.

[0581] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material.

[0582] Without limitation, the mass fraction of the positive electrode active material in the positive electrode active material layer can be greater than or equal to 80%, further can be greater than or equal to 90%, and can also be any of the following percentages or a range consisting of any two of the following percentages: 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, etc.

[0583] As a non-limiting example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two surfaces facing each other of the positive electrode current collector.

[0584] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. In the positive electrode current collector, the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. In the positive electrode current collector, the composite current collector may be obtained by forming a metal material on a polymer material substrate. In the positive electrode current collector, non-limiting examples of the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. Non-limitingly, in the positive electrode current collector, the polymer material substrate may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0585] The types of positive electrode active materials can be found in the above text. The positive electrode active materials may also include other types of positive electrode active materials known in the art for lithium ion secondary batteries. The positive electrode active materials may be used alone or in combination of two or more.

[0586] As non-limiting examples, the positive electrode active material may include, but is not limited to, one or more of the following materials: olivine-structured lithium-containing phosphates, lithium transition metal oxides, and their respective modified compounds.

[0587] In some embodiments, the positive electrode active material includes one or more of a lithium-containing phosphate-based active material and a lithium composite metal oxide-based active material.

[0588] In some embodiments, the positive electrode active material includes a lithium-containing phosphate-based active material.

[0589] In the present application, unless otherwise specified, the lithium-containing phosphate active material may include at least one of lithium-containing phosphate and its modified form. The lithium-containing phosphate active material may have an olivine structure. Unless otherwise specified, "lithium-containing phosphate" refers to a material including lithium, transition metal elements and phosphate ions (PO4 3- ) positive electrode active material. Non-limiting examples of olivine-structured lithium-containing phosphates may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0590] In some embodiments, the positive electrode active material includes a lithium-containing phosphate with an olivine structure. Non-limiting examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. An example of lithium iron phosphate is LiFePO4 (also referred to as LFP). An example of lithium manganese phosphate is LiMnPO4.

[0591] In some embodiments, the positive electrode active material includes a lithium composite metal oxide-based active material.

[0592] In the present application, unless otherwise specified, lithium composite metal oxide type active materials include at least one of lithium composite metal oxides and modified forms thereof. Unless otherwise specified, "lithium composite metal oxide" refers to a positive electrode active material including lithium element, non-lithium metal element and oxygen element. Generally, the non-lithium metal elements of lithium composite metal oxides include transition metal elements, and therefore, lithium composite metal oxides may also be referred to as "lithium transition metal oxides". Lithium composite metal oxide type active materials may have a crystal structure such as a layered structure, a spinel structure, etc. suitable for positive electrode active materials. In some embodiments, the lithium composite metal oxide type active material comprises a layered structure. In some embodiments, the lithium composite metal oxide type active material is a layered structure.

[0593] In some embodiments, the positive electrode active material includes a lithium transition metal oxide. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and modified compounds thereof. Non-limiting examples of lithium cobalt oxides may include LiCoO2; non-limiting examples of lithium nickel oxides may include LiNiO2; non-limiting examples of lithium manganese oxides may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxide may include LiNi 0.80 Co 0.15 Al 0.05 O2.

[0594] It is understandable that the battery will be accompanied by lithium (Li) deintercalation and consumption during the charging and discharging process, and the content of Li in the positive electrode sheet is different when the battery is discharged to different states. In the exemplary description of the positive electrode active material in this application, unless otherwise specified, the content of Li can be the initial state of the material or the non-initial state after the charge and discharge cycle. The positive electrode active material is applied to the positive electrode in the battery system, and after the charge and discharge cycle, the content of Li in the positive electrode active material at the positive electrode usually changes. Among them, the content of Li can be measured by atomic molar content, but is not limited to this. Regarding "the content of Li is the initial state of the material", the initial state of the material refers to the state before being made into a positive electrode active material layer. It can be understood that the new material or new substance obtained by appropriately modifying the listed positive electrode active materials is also within the scope of the positive electrode active material. The aforementioned appropriate modification refers to the acceptable modification method for the positive electrode active material, and non-limiting examples include one or more of coating modification and doping modification.

[0595] In the exemplary description of the positive electrode active material in this application, the content of oxygen (O) is only a theoretical state value. The release of oxygen from the lattice will cause the atomic molar content of oxygen to change, and the actual content of O will fluctuate. Among them, the content of O can be measured by atomic molar content, but is not limited to this.

[0596] In some embodiments, the positive electrode active material layer may optionally include a binder. The binder in the positive electrode active material layer may be referred to as a positive electrode binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. Typically, the mass fraction of the binder in the positive electrode active material layer may be 0 to 10%, further 0 to 8%, and further 1% to 5%, based on the total mass of the positive electrode active material layer.

[0597] In some embodiments, the positive electrode active material layer optionally includes a conductive agent. The conductive agent in the positive electrode active material layer may be recorded as a positive electrode conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. Typically, the mass fraction of the conductive agent in the positive electrode active material layer may be 0 to 10%, further 0 to 8%, and further 0 to 5%, based on the total mass of the positive electrode active material layer.

[0598] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a positive electrode slurry. Further, the positive electrode slurry is coated on at least one side of the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained. Cold pressing can be performed by a cold rolling mill. The type of solvent in the positive electrode slurry can include but is not limited to any of the aforementioned embodiments, for example, it can include N-methylpyrrolidone (NMP), and further can be NMP. The surface of the positive electrode collector coated with the positive electrode slurry can be on a single surface of the positive electrode collector, or on both surfaces of the positive electrode collector. The solid content of the positive electrode slurry can be 40wt%~80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000mPa·s~25000mPa·s.

[0599] In the present application, "wt%" means weight percentage or mass percentage.

[0600] In some embodiments, the positive electrode active material includes a lithium-containing phosphate active material, and further, the mass proportion of the lithium-containing phosphate active material in the positive electrode active material can be greater than or equal to 50%, but is not limited thereto. When coating the positive electrode slurry, the coating surface density (based on the coating surface density on both sides) on a dry weight basis (excluding the solvent) can also be (0.2 ~1.0) g / 1540.25 mm 2 , optional: (0.4 ~ 0.8) g / 1540.25 mm 2 , but not limited to this. The compaction density of the positive electrode sheet can be 2.0g / cm 3 ~2.8 g / cm 3 , optional 2.3g / cm 3 ~2.6 g / cm 3 .

[0601] In some embodiments, the positive electrode active material includes a lithium composite metal oxide active material, and further, the mass proportion of the lithium composite metal oxide active material in the positive electrode active material can be greater than or equal to 50%, but is not limited thereto. When the positive electrode slurry is coated, the coating surface density (based on the coating surface density on both sides) on a dry weight basis (excluding the solvent) can be (0.1 ~ 1.2) g / 1540.25 mm 2 , optional: (0.2~ 0.6) g / 1540.25 mm 2 The compaction density of the positive electrode sheet can be 3.0 g / cm 3 ~ 4.2 g / cm 3 , optional 3.3 g / cm 3 ~ 3.8 g / cm3 .

[0602] The following are some additional descriptions about the negative electrode.

[0603] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on at least one surface of the negative electrode current collector, and the negative electrode active layer includes a negative electrode active material. It can be understood that at least one negative electrode active layer includes a first negative electrode active layer and a second negative electrode active layer, and the second negative electrode active layer is located between the negative electrode current collector and the first negative electrode active layer. The first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material. The definitions of the first negative electrode active material and the second negative electrode active material can be found in the above text.

[0604] As a non-limiting example, the negative electrode sheet includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode collector.

[0605] Without limitation, the mass fraction of the first negative electrode active material in the first negative electrode active layer may be greater than or equal to 80%, further may be greater than or equal to 90%, and may also be any of the following percentages or a range selected from any two of the following percentages: 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, etc.

[0606] Without limitation, the mass fraction of the second negative electrode active material in the second negative electrode active layer can be greater than or equal to 80%, further can be greater than or equal to 90%, and can also be any of the following percentages or a range selected from any two of the following percentages: 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 98.1%, etc.

[0607] As a non-limiting example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode active layer is disposed on any one or both of the two surfaces facing each other of the negative electrode current collector.

[0608] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. In the negative electrode current collector, the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. In the negative electrode current collector, the composite current collector may be formed by forming a metal material on a polymer material substrate. In the negative electrode current collector, non-limiting examples of the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In a non-limiting manner, in the negative electrode current collector, the polymer material substrate may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0609] In some embodiments, the first negative electrode active layer and the second negative electrode active layer each independently optionally include a binder. In some embodiments, the first negative electrode active layer includes a first binder, and the second negative electrode active layer includes a second binder.

[0610] Without limitation, in the negative electrode sheet, the first binder and the second binder may each independently include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0611] Without limitation, the mass fraction of the first binder in the first negative electrode active layer may be 0% to 15%, further 0% to 10%, further 0 to 5%, further 1% to 5%, further optionally 1% to 3%.

[0612] Without limitation, the mass fraction of the second binder in the second negative electrode active layer may be 0% to 15%, further 0% to 10%, further 0 to 5%, further 1% to 5%, further optionally 1% to 3%.

[0613] In some embodiments, the first negative electrode active layer and the second negative electrode active layer each independently optionally include a conductive agent. In some embodiments, the first negative electrode active layer includes a first conductive agent, and the second negative electrode active layer includes a second conductive agent.

[0614] Without limitation, in the negative electrode sheet, the first conductive agent and the second conductive agent may each independently include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0615] In a non-limiting manner, the mass fraction of the first conductive agent in the first negative electrode active layer may be 0% to 10%, and may further be 0% to 5%.

[0616] Without limitation, the mass fraction of the second conductive agent in the second negative electrode active layer may be 0% to 10%, and may further be 0% to 5%.

[0617] In some embodiments, the first negative electrode active layer and the second negative electrode active layer may each independently optionally include other additives, such as a thickener (such as sodium carboxymethyl cellulose (CMC-Na)), etc. Without limitation, the mass fraction of other additives in the first negative electrode active layer or the second negative electrode active layer may independently be 0% to 15%, further optionally 0% to 10%, further optionally 0% to 5%, further optionally 0% to 3%, further optionally 0% to 2%.

[0618] In some embodiments, the preparation method of the lithium-supplemented negative electrode sheet can refer to the third aspect of the present application, and can also refer to the second aspect of the present application.

[0619] In some embodiments, the method for preparing a lithium-ion secondary battery can refer to the third aspect of the present application, and can also refer to the second aspect of the present application.

[0620] The electrolyte solution is exemplarily described below.

[0621] The electrolyte has the function of conducting ions between the positive electrode and the negative electrode. The appropriate electrolyte can be selected according to the needs.

[0622] The electrolyte solution includes an electrolyte salt and a solvent.

[0623] In some embodiments, the electrolyte is a non-aqueous electrolyte. The non-aqueous electrolyte may include an electrolyte salt and a solvent.

[0624] The concentration of the electrolyte salt in the electrolyte solution may generally be 0.5 mol / L to 5 mol / L, and may be optionally 0.8 mol / L to 1.2 mol / L.

[0625] In some embodiments, the electrolyte salt includes an electrolyte lithium salt. Without limitation, the electrolyte lithium salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorobisoxalatophosphate (LiDFOP), and lithium tetrafluorooxalatophosphate (LiTFOP).

[0626] In some embodiments, the solvent in the non-aqueous electrolyte may include ethylene carbonate (EC, ), propylene carbonate (PC, )、ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC, ), fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0627] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0628] In some embodiments, the additive in the electrolyte may include, but is not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), and the like.

[0629] The separator is exemplarily described below.

[0630] In some embodiments, the lithium-ion secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0631] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0632] In some embodiments, the thickness of the isolation film is 6 μm to 40 μm, and optionally 6 μm to 20 μm.

[0633] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0634] In some embodiments, the lithium-ion secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0635] In some embodiments, the outer packaging of the lithium ion secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium ion secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and further, non-limiting examples of plastic can include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0636] A lithium-ion secondary battery includes at least one battery cell. A lithium-ion secondary battery may include one or more battery cells.

[0637] The present application has no particular limitation on the shape of the battery cell, which may be cylindrical, square or any other shape. Figure 5 The battery cell 5 is a square structure as an example.

[0638] In some embodiments, reference Figure 6 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to actual needs.

[0639] The lithium-ion secondary battery may be a battery device 4 or a battery pack 1 .

[0640] The battery device includes at least one battery cell. The number of battery cells contained in the battery device can be one or more, and those skilled in the art can select a suitable number according to the application and capacity of the battery device.

[0641] Figure 7 4 is an example of a battery device. Figure 7 In the battery device 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery device 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.

[0642] Optionally, the battery device 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.

[0643] In some embodiments, the battery devices described above may also be assembled into a battery pack. The number of battery devices contained in the battery pack may be one or more. Those skilled in the art may select a suitable number according to the application and capacity of the battery pack.

[0644] Figure 8 and Fig. 9 1 is a battery pack 1 as an example. Figure 8 and Fig. 9 The battery pack 1 may include a battery box and a plurality of battery devices 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery devices 4. The plurality of battery devices 4 can be arranged in the battery box in any manner.

[0645] In a second aspect of the present application, a component for preparing a lithium-ion secondary battery is provided, which includes an electrode assembly and an electrolyte, wherein the electrode assembly includes a positive electrode sheet, a lithium-supplemented negative electrode sheet and a separator, and a separator is provided between the positive electrode sheet and the lithium-supplemented negative electrode sheet;

[0646] The lithium supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active initial layer, a first negative electrode active initial layer and a lithium supplemented layer sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active initial layer comprises a first negative electrode active material, and the second negative electrode active initial layer comprises a second negative electrode active material;

[0647] The lithium-supplemented negative electrode sheet meets one or both of the following characteristics (t1) and (t2):

[0648] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0649] (t2) The first negative electrode active material and the second negative electrode active material independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; the lithium-supplemented negative electrode sheet meets one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 Wherein, as defined above, the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is recorded as f15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 .

[0650] In the present application, unless otherwise specified, "components for preparing lithium-ion secondary batteries" at least include assembled electrode components and electrolytes. The component may be in a state before the electrolyte is injected, in which case the electrode components and the electrolyte are placed separately. The component may also be in a state before the electrolyte is injected but not fully infiltrated. In the component for preparing lithium-ion secondary batteries, the negative electrode lithium replenishing material in the lithium replenishing layer has not been consumed or has only been partially consumed.

[0651] As mentioned above, when the lithium-supplemented negative electrode sheet has any one of the above characteristics (t1) and (t2), it is beneficial to give the first negative electrode active layer a higher lithium insertion rate. Such a lithium-supplemented negative electrode sheet can be provided in a component for preparing a lithium-ion secondary battery. The lithium-supplemented negative electrode sheet is provided with a lithium-supplemented layer on the surface of the negative electrode active material layer. By providing a first negative electrode active layer and a second negative electrode active layer on the negative electrode active material layer, and making the first negative electrode active layer close to the lithium-supplemented layer have a higher lithium insertion rate, when the negative electrode is subjected to lithium-supplementing treatment, it is beneficial to efficiently embed active lithium ions into the first negative electrode active layer. In the process of assembling components for preparing lithium-ion secondary batteries using the lithium-supplemented negative electrode sheet, in the process after injecting the electrolyte, it is beneficial to make the active lithium provided by the lithium-supplementing layer embed into the first negative electrode active layer faster and more, which is beneficial to inhibit the deactivation of the active lithium before embedding into the negative electrode active material, and can reduce the loss of active lithium during lithium replenishment, which is beneficial to significantly improve the lithium replenishment efficiency, and obtain components with negative electrode sheets treated with efficient lithium replenishment. The prepared lithium-ion secondary battery can persistently replenish active lithium and continuously replenish capacity during the charge and discharge cycle, and can also reduce the enrichment of lithium ions on the surface of the negative electrode active material and reduce the generation of lithium precipitation, so that the lithium-ion secondary battery can have a significantly improved cycle life.

[0652] In the present application, the lithium replenishing layer in the lithium replenishing negative electrode sheet includes negative electrode lithium replenishing material.

[0653] Without limitation, the lithium supplement layer may include one or more of single lithium and lithium alloys, such as lithium-tin alloy.

[0654] In some embodiments, the lithium replenishing layer includes single-substance lithium. In this case, the negative electrode lithium replenishing material includes single-substance lithium.

[0655] By selecting a lithium replenishing layer including single-element lithium (a non-limiting example such as a lithium film), the preparation process is more controllable and the lithium replenishing efficiency is high.

[0656] In some embodiments, the thickness of the lithium supplement layer on one side of the negative electrode current collector is less than the sum of the thicknesses of the first negative electrode active initial layer and the second negative electrode active initial layer.

[0657] In some embodiments, the thickness of the lithium supplement layer on a single side of the negative electrode current collector is less than or equal to 8.5 μm, and may be 0.5 μm to 8.5 μm, and may be 1 μm to 8.5 μm.

[0658] In some embodiments, the thickness of the lithium supplement layer on a single side of the negative electrode current collector is less than or equal to 4.8 μm, and may be 1 μm to 4.8 μm, and may be further 2 μm to 4.8 μm.

[0659] Without limitation, the thickness of the lithium supplement layer on a single side of the negative electrode current collector can also be any of the following values ​​or a range consisting of any two of the following values: 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.8μm, 5μm, 6μm, 7μm, 8μm, 8.5μm, etc.

[0660] In the present application, unless otherwise specified, “the thickness of the lithium supplement layer” refers to the thickness on one side of the negative electrode current collector, which may also be recorded as “the thickness on one side of the lithium supplement layer”.

[0661] Without limitation, the thickness of the lithium replenishment layer can be measured and analyzed based on the cross-sectional SEM image of the lithium replenishment negative electrode sheet, or can be measured using a laser thickness gauge. The method for obtaining the cross-sectional SEM image of the lithium replenishment negative electrode sheet can refer to the cross-sectional SEM image of the negative electrode sheet.

[0662] In the present application, unless otherwise specified, the “cross section of the lithium-supplemented negative electrode sheet” refers to the cross section of the lithium-supplemented negative electrode sheet.

[0663] The thickness of the lithium replenishment layer can be adjusted according to the amount of lithium replenishment required for the negative electrode. In addition, by controlling the thickness of the single side of the lithium replenishment layer within the aforementioned range, it is helpful to control the thickness of the lithium replenishment residual layer within a more appropriate range.

[0664] In the production process, water that is difficult to completely remove usually remains in the negative electrode plate, and the water may react with the lithium replenishing material in the lithium replenishing layer to generate heat. The thicker the lithium replenishing layer, the higher the heat generation. Without being limited to any theory, by controlling the thickness of the lithium replenishing layer within the aforementioned range, it is helpful to better control the heat generation caused by the reaction of water and lithium, thereby helping to improve production safety.

[0665] In some embodiments, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is less than or equal to 98%, optionally less than or equal to 70%, calculated on a single side of the negative electrode current collector. In some embodiments, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is greater than 0 and less than or equal to 90%, calculated on a single side of the negative electrode current collector. In some of these embodiments, in the negative electrode sheet, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is greater than 0 and less than or equal to 70%, calculated on a single side of the negative electrode current collector. Without limitation, in the negative electrode sheet, based on the single side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer can also be any of the following percentages, or selected from any two of the following percentages: 0.1%, 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, 98%, etc. Without limitation, based on the single side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer can be selected from any suitable range as follows: greater than 0 and less than or equal to 50%, 30% to 98%, 30% to 70%, 30% to 50%, 50% to 98%, 50% to 70%, etc.

[0666] By controlling the coverage area percentage of the lithium-replenishing layer in the lithium-replenishing negative electrode sheet relative to the first negative electrode active initial layer within the aforementioned range, it is beneficial to control the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer in the lithium-ion secondary battery within a more appropriate range, which is beneficial to better achieve good electrolyte infiltration performance and charge transfer performance, and is beneficial for the battery to have good battery dynamics.

[0667] The shape of the area covered by the lithium replenishing layer on the first negative electrode active layer is not particularly limited, and can be any suitable shape such as a strip shape, a grid shape, but is not limited thereto. A shape that is easier to operate in terms of process can be selected. By adjusting the shape of the area covered by the lithium replenishing layer on the first negative electrode active layer, the percentage of the coverage area of ​​the lithium replenishing residual layer relative to the first negative electrode active layer can be adjusted.

[0668] Without limitation, the shape and size of the lithium replenishing layer (such as stripe spacing, grid spacing, etc.) can be measured using a ruler or a CCD (inductively coupled device).

[0669] Figure 1 It is a schematic diagram of the structure of the lithium-supplemented negative electrode sheet in one embodiment of the present application, corresponding to the side view. Figure 2 yes Figure 1 Schematic diagram of the structure of the lithium-supplemented negative electrode sheet, corresponding to the top view. Figure 1The lithium supplemented negative electrode sheet 12 in the illustrated embodiment includes a negative electrode current collector 102 and a second negative electrode active initial layer 104 , a first negative electrode active initial layer 106 and a lithium supplemented layer 108 sequentially disposed on one side of the negative electrode current collector 102 . Figure 1 In the embodiment, the second negative electrode active initial layer 104, the first negative electrode active initial layer 106 and the lithium supplement layer 108 are sequentially stacked along the thickness direction Z of the negative electrode plate, and the lithium supplement layer covers the first negative electrode active initial layer in a strip shape.

[0670] In the present application, unless otherwise specified, the X direction corresponds to the width direction of the pole piece (which may be consistent with the height direction of the wound battery cell), the Y direction corresponds to the length direction of the pole piece, and the Z direction corresponds to the thickness direction of the pole piece.

[0671] Taking the electrode assembly assembled in a winding manner as an example, the Y direction may correspond to the winding direction of the electrode sheet, and the X direction may correspond to the extending direction of the electrode ear, that is, the X direction may correspond to the height direction of the electrode assembly or the bare cell.

[0672] Figure 3 This is a schematic diagram of the structure of a lithium-supplemented negative electrode sheet in another embodiment of the present application, corresponding to a top view, Figure 3 In the embodiment, the lithium supplement layer covers the first negative electrode active initial layer in a strip-like shape.

[0673] Figure 4 This is a schematic diagram of the structure of a lithium-supplemented negative electrode sheet in another embodiment of the present application, corresponding to a top view, Figure 4 In the embodiment, the shape of the covering area of ​​the lithium supplement layer on the first negative electrode active initial layer is a grid shape.

[0674] In some embodiments, the preparation method of the lithium-supplemented negative electrode sheet can refer to the third aspect of the present application.

[0675] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any suitable numerical value or range in the context):

[0676] The compaction density of the lithium-supplemented negative electrode sheet is 1.3g / cm 3 ~1.8g / cm 3 , optional 1.4g / cm 3 ~1.6g / cm 3 ;

[0677] The surface density of the lithium-supplemented negative electrode is 10 mg / cm 2 ~26mg / cm 2 , optional 15 mg / cm 2 ~20mg / cm 2 .

[0678] In some embodiments, the compaction density of the lithium-supplemented negative electrode sheet can be 1.3 g / cm 3 ~1.8g / cm 3 , optional 1.4g / cm 3 ~1.6g / cm 3 Without limitation, the compaction density of the lithium-supplemented negative electrode sheet can also be any of the following values ​​or a range consisting of any two of the following values: 1.30 g / cm 3 , 1.35 g / cm 3 , 1.40 g / cm 3 , 1.45 g / cm 3 , 1.50 g / cm 3 , 1.55 g / cm 3 , 1.60 g / cm 3 , 1.65 g / cm 3 , 1.70 g / cm 3 , 1.75 g / cm 3 , 1.8 g / cm 3 , 1.80 g / cm 3 wait.

[0679] In some embodiments, the surface density of the lithium-supplemented negative electrode sheet is 10 mg / cm 2 ~26mg / cm 2 , optional 15 mg / cm 2 ~20mg / cm 2 Without limitation, the surface density of the lithium-supplemented negative electrode sheet can also be any of the following values ​​or a range consisting of any two of the following values: 10 mg / cm 2 , 12 mg / cm 2 , 15 mg / cm 2 , 16 mg / cm 2 , 18 mg / cm 2 , 20 mg / cm 2 , 22mg / cm 2 , 24 mg / cm 2 , 25 mg / cm 2 , 26 mg / cm 2 wait.

[0680] By adjusting the compaction density and / or surface density of the lithium-supplemented negative electrode sheet, the compaction density and / or surface density of the negative electrode sheet in the lithium-ion secondary battery can be adjusted accordingly. By controlling the compaction density and / or surface density of the lithium-supplemented negative electrode sheet within the aforementioned range, it is beneficial for the battery to have a higher energy density.

[0681] In the present application, unless otherwise specified, the compaction density of the lithium-supplemented negative electrode sheet refers to the ratio of the mass to volume of the negative electrode active material layer (excluding the lithium-supplemented layer) in the lithium-supplemented negative electrode sheet.

[0682] In the present application, unless otherwise specified, the surface density of the lithium-supplemented negative electrode sheet refers to the surface density calculated on the basis of the total amount on both sides, which is equal to the compaction density of the lithium-supplemented negative electrode sheet multiplied by the total thickness on both sides of the negative electrode active material layer.

[0683] Without limitation, the compaction density and the surface density of the lithium-supplemented negative electrode sheet based on the total amount on both sides can be obtained by the following method:

[0684] (1) Punch the lithium-supplemented negative electrode sheet into a piece with an area of ​​A (e.g. 1540.25mm 2 ) and measure the weight m and thickness L of the small disc;

[0685] (2) Take another lithium-supplemented negative electrode sheet, wipe off the film layer on the surface, and cut the remaining empty current collector foil into a piece with an area of ​​A (e.g. 1540.25mm 2 ) small disc, weigh the empty foil mass M0, thickness L0;

[0686] (3) The sum of the double-side density of the lithium-supplemented layer on the first negative electrode active layer in the lithium-supplemented negative electrode sheet of the tested embodiment is recorded as ρ A The total thickness of the lithium supplement layer on both sides is recorded as d D ;

[0687] (4) Calculation:

[0688] Compacted density PD of lithium-supplemented negative electrode A =(M-M0-ρ A ×d D ) / [A×(L-L0-d D )].

[0689] The surface density of the lithium-supplemented negative electrode sheet (based on the total amount on both sides) = (M-M0-ρ A ×d D ) / A.

[0690] In some embodiments, in a component for preparing a lithium ion secondary battery, the electrolyte includes an additive; without limitation, in a component for preparing a lithium ion secondary battery, the additive in the electrolyte may include one or more of vinyl carbonate (VC) and a sulfur-containing additive; without limitation, the sulfur-containing additive may include one or more of diethylene sulfate (DTD), diethylene sulfite (ES) and dipropylene sulfite (PS).

[0691] In some embodiments, in a component for preparing a lithium-ion secondary battery, the additive in the electrolyte includes vinylene carbonate (VC), fluoroethylene carbonate (FEC) and diethylene sulfate (DTD), and may further be a combination of vinylene carbonate (VC), fluoroethylene carbonate (FEC) and diethylene sulfate (DTD). Without limitation, in a component for preparing a lithium ion secondary battery, the mass fraction of vinylene carbonate (VC) in the electrolyte can be 0-3%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.01%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.16%, 0.18%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, etc.

[0692] Without limitation, in a component for preparing a lithium ion secondary battery, the mass fraction of fluoroethylene carbonate (FEC) in the electrolyte can be 0-6%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.01%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.16%, 0.18%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc.

[0693] Without limitation, in a component for preparing a lithium ion secondary battery, the mass fraction of vinyl sulfate (DTD) in the electrolyte can be 0-4%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.01%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.16%, 0.18%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, 3.5%, 4%, etc.

[0694] In a third aspect of the present application, a method for preparing a lithium ion secondary battery is provided, which can be used to prepare the lithium ion secondary battery of the first aspect of the present application.

[0695] In some embodiments, a method for preparing a lithium ion secondary battery is provided, comprising the following steps:

[0696] S100: Assembling a positive electrode sheet, a separator and a lithium-supplemented negative electrode sheet into an electrode assembly, so that a separator is provided between the positive electrode sheet and the lithium-supplemented negative electrode sheet; wherein the lithium-supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active initial layer, a first negative electrode active initial layer and a lithium-supplemented layer sequentially provided on at least one side of the negative electrode current collector; the first negative electrode active initial layer comprises a first negative electrode active material, and the second negative electrode active initial layer comprises a second negative electrode active material;

[0697] S200: placing the electrode assembly in the accommodating cavity of the shell, injecting electrolyte (the assembly for preparing a lithium-ion secondary battery can be obtained), allowing the electrolyte to infiltrate the positive electrode plate and the lithium-supplemented negative electrode plate, and forming them to prepare a lithium-ion secondary battery; wherein the lithium-supplemented negative electrode plate forms the negative electrode plate, the second negative electrode active initial layer forms the second negative electrode active layer, and the first negative electrode active initial layer forms the first negative electrode active layer.

[0698] The definition of lithium-supplemented negative electrode sheet can refer to the description in the second aspect of this application.

[0699] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide, and silicon-carbon composite; the lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (t1) and (t2):

[0700] (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material;

[0701] (t2) The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 Wherein, as defined above, the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is recorded as f15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 .

[0702] As defined above, "lithium replenishing layer" refers to a structural layer containing lithium replenishing material. As a non-limiting example, the lithium replenishing layer can be a lithium sheet. The lithium replenishing material contained in the lithium replenishing layer disposed on the lithium replenishing negative electrode sheet can also be referred to as negative electrode lithium replenishing material.

[0703] In step S200, after being infiltrated and formed, the negative electrode lithium replenishing material in the lithium replenishing layer reacts with the electrolyte and is consumed, releasing active lithium, and the released active lithium is embedded in the negative electrode active initial layer to achieve lithium insertion, and the lithium replenishing negative electrode sheet is converted into a negative electrode sheet, and the second negative electrode active initial layer and the first negative electrode active initial layer are respectively converted into the second negative electrode active layer and the first negative electrode active layer. It can be understood that the second negative electrode active layer and the first negative electrode active layer each independently include pre-embedded lithium. The location of the consumed lithium replenishing layer usually produces residues generated as the lithium replenishment proceeds. Non-limiting examples of the residues include lithium that is inactivated because it is not able to be embedded in the negative electrode active material in time. In this way, a lithium replenishing residual layer including inactive lithium is formed at the location of the lithium replenishing layer; accordingly, the lithium replenishing residual layer formed at the location of the first lithium replenishing layer is called the first lithium replenishing residual layer, and the lithium replenishing residual layer formed at the location of the second lithium replenishing layer is called the second lithium replenishing residual layer.

[0704] In step S200, after infiltration and formation, the lithium ions released by the lithium supplement layer are embedded in the negative electrode active material, at least embedded in the first negative electrode active initial layer, so that the first negative electrode active initial layer is formed into a first negative electrode active layer pre-embedded with lithium. Similarly, the second negative electrode active initial layer is also formed into a second negative electrode active layer pre-embedded with lithium.

[0705] As mentioned above, when the lithium-supplemented negative electrode sheet has any one of the above characteristics (t1) and (t2), it is beneficial to give the first negative electrode active layer a higher lithium insertion rate. By contacting the electrode assembly including the above-mentioned lithium-supplemented negative electrode sheet with an electrolyte, infiltrating, and forming, a negative electrode sheet including a negative electrode lithium-supplemented treatment can be prepared, thereby making the negative electrode sheet include lithium pre-inserted by the negative electrode lithium-supplemented treatment. The negative electrode active material layer of the negative electrode plate is provided with a first negative electrode active layer located in an upper layer and a second negative electrode active layer located in a lower layer (the direction away from the surface of the negative electrode current collector is the upper layer, and the direction toward the surface of the negative electrode current collector is the lower layer). By giving the first negative electrode active layer located in the upper layer a higher lithium insertion rate, in the process of lithium replenishment using the above-mentioned method, based on the higher lithium insertion rate of the first negative electrode active layer, it is beneficial to make the active lithium provided by the negative electrode lithium replenishment material more efficiently embedded in the first negative electrode active layer, which is beneficial to inhibit the deactivation of the active lithium before being embedded in the negative electrode active material, and can reduce the loss of active lithium during lithium replenishment, thereby significantly improving the lithium replenishment efficiency. Therefore, the negative electrode plate treated with high-efficiency negative electrode lithium replenishment is introduced into the lithium ion secondary battery, which can replenish active lithium for a long time during the charge and discharge cycle and continuously replenish capacity; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reduce the enrichment of lithium ions on the surface of the negative electrode active material, which is beneficial to reduce the generation of lithium precipitation, thereby making the lithium ion secondary battery have a significantly improved cycle life.

[0706] Without limitation, in step S200, the infiltration temperature can be 20°C~60°C, or any of the following temperatures or a range consisting of any two of the following temperatures: 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, etc.

[0707] Without limitation, in step S200, the immersion time can be 10 h to 50 h, or any of the following durations or a range consisting of any two of the following durations: 10 h, 12 h, 15 h, 16 h, 18 h, 20 h, 24 h, 25 h, 26 h, 28 h, 30 h, 35 h, 36 h, 40 h, 42 h, 45 h, 48 h, 50 h, etc.

[0708] By controlling the wetting parameters within the aforementioned range, it is beneficial for the electrolyte to more fully infiltrate the negative electrode plate.

[0709] In step 200, the negative electrode lithium supplement material may generate gas while releasing active lithium. For example, when the negative electrode lithium supplement material is single substance lithium, the single substance lithium reacts with the electrolyte to form lithium ions, and the electrolyte decomposes to generate gas.

[0710] In some embodiments, the lithium-supplemented layer in the lithium-supplemented negative electrode sheet satisfies the following formula:

[0711] ...

Claims

1. A lithium ion secondary battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet; the negative electrode sheet comprises a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active layer comprises a first negative electrode active material, and the second negative electrode active layer comprises a second negative electrode active material; The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; The negative electrode plate satisfies one or both of the following characteristics (t1) and (t2): (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material; (t2) The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 The negative electrode sheet satisfies one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 ; The negative electrode plate is treated with negative electrode lithium supplementation.

2. The lithium ion secondary battery according to claim 1, characterized in that: The lithium insertion potential of the first negative electrode active material is 0.08 V ~ 0.5 V vs. Li / Li + .

3. The lithium ion secondary battery according to claim 1, characterized in that: The lithium insertion potential of the first negative electrode active material is 0.1 V to 0.5 V vs. Li / Li + .

4. The lithium-ion secondary battery according to claim 1, characterized in that: The negative electrode plate meets one or more of the following characteristics: 50%≤f 10 ≤100%; 50%≤f 20 ≤100%; 0≤f 15 ≤50%; 0≤f 21 ≤50%; 0%≤f 19 ≤50%; 0%≤f 29 ≤50%。 5. The lithium ion secondary battery according to claim 4, characterized in that: The negative electrode plate meets one or more of the following characteristics: 80%≤f 10 ≤100%; 80%≤f 20 ≤100%; 0≤f 15 ≤30%; 1≤f 21 ≤30%; 1%≤f 19 ≤40%; 0%≤f 29 ≤40%。 6. The lithium ion secondary battery according to claim 4, characterized in that: The negative electrode plate meets one or more of the following characteristics: 90%≤f 10 ≤100%; 90%≤f 20 ≤100%; 0≤f 15 ≤20%; 10≤f 21 ≤30%; 5%≤f 19 ≤30%; 1%≤f 29 ≤30%。 7. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The first negative electrode active material includes one or more of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite.

8. The lithium ion secondary battery according to claim 7, characterized in that: The first negative electrode active material includes artificial graphite.

9. The lithium ion secondary battery according to claim 8, characterized in that: The proportion of artificial graphite in the total mass of the first negative electrode active material is denoted as f 11 , satisfying 50%≤f 11 ≤100%.

10. The lithium ion secondary battery according to claim 9, characterized in that: 70%≤f 11 ≤95%。 11. The lithium ion secondary battery according to claim 8, characterized in that: The proportion of artificial graphite in the total mass of the first negative electrode active material is 11 Higher than the proportion of artificial graphite in the total mass of the second negative electrode active material 22 , where f 11 >f 22 ≥0.

12. The lithium ion secondary battery according to claim 7, characterized in that: The first negative electrode active material includes artificial graphite and one or more of hard carbon, soft carbon, silicon oxide and silicon-carbon composite.

13. The lithium ion secondary battery according to claim 12, characterized in that: The proportion of the sum of the masses of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is denoted as f 12 , satisfying 0 <f 12 ≤50%.

14. The lithium ion secondary battery according to claim 13, characterized in that: 5%≤f 12 ≤30%。 15. The lithium ion secondary battery according to claim 7, characterized in that: The first negative electrode active material includes one or more of artificial graphite, silicon oxide and silicon-carbon composite, and the first negative electrode active material also includes one or more of hard carbon and soft carbon.

16. The lithium ion secondary battery according to claim 15, characterized in that: The first negative electrode active material includes artificial graphite.

17. The lithium ion secondary battery according to claim 15, characterized in that: The proportion of the sum of the mass of the hard carbon and the soft carbon in the total mass of the first negative electrode active material is denoted as f 13 , satisfying 0 <f 13 ≤50%.

18. The lithium ion secondary battery according to claim 17, characterized in that: 10%≤f 13 ≤30%。 19. The lithium ion secondary battery according to claim 7, characterized in that: The first negative electrode active material includes artificial graphite and further includes one or more of silicon oxide and silicon-carbon composite.

20. The lithium ion secondary battery according to claim 19, characterized in that: The first negative electrode active material satisfies one or more of the following characteristics: The proportion of the sum of the mass of silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is denoted as f 14 , satisfying 0 <f 14 ≤50%; The silicon-carbon composite comprises a porous carbon matrix and simple silicon located in the cavities of the porous carbon matrix.

21. The lithium ion secondary battery according to claim 20, characterized in that: 1%≤f 14 ≤30%。 22. The lithium ion secondary battery according to claim 20, characterized in that: 1%≤f 14 ≤15%。 23. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that: The first negative electrode active material comprises coated negative electrode active particles, wherein the coated negative electrode active particles comprise a first negative electrode active body and a coating layer located at least partially on a surface of the first negative electrode active body, wherein the coating layer comprises one or more of soft carbon and hard carbon.

24. The lithium ion secondary battery according to claim 23, characterized in that: The coated negative electrode active particles meet one or more of the following characteristics: The thickness of at least a portion of the coating layer is 1 nm to 10 nm; The average thickness of the coating layer is 1 nm to 10 nm; The sum of the mass fractions of the soft carbon and the hard carbon in the coating layer in the coated negative electrode active particles is 0.5% to 10%; The first negative electrode active body includes one or more of artificial graphite, silicon oxide and silicon-carbon composite; the proportion of the sum of the masses of artificial graphite, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active body is recorded as f 16 , satisfying 80%≤f 16 ≤100%.

25. The lithium ion secondary battery according to claim 24, characterized in that: The coated negative electrode active particles meet one or more of the following characteristics: The thickness of at least a portion of the coating layer is 1 nm to 5 nm; The average thickness of the coating layer is 1nm~5nm; The sum of the mass fractions of the soft carbon and the hard carbon in the coating layer in the coated negative electrode active particles is 1% to 4%; 90%≤f 16 ≤100%。 26. The lithium ion secondary battery according to claim 25, characterized in that: The first negative electrode active body includes artificial graphite; the proportion of artificial graphite in the total mass of the first negative electrode active body is denoted as f 17 , satisfying 80%≤f 17 ≤100%.

27. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The second negative electrode active material includes natural graphite.

28. The lithium ion secondary battery according to claim 27, characterized in that: The second negative electrode active material further includes artificial graphite.

29. The lithium ion secondary battery according to claim 28, characterized in that: The second negative electrode active layer satisfies one or more of the following characteristics: The proportion of natural graphite in the total mass of the second negative electrode active material is denoted as f 21 , satisfying 0 <f 21 ≤50%; The proportion of artificial graphite in the total mass of the second negative electrode active material is denoted as f 22 , satisfying 50%≤f 22 <100%.

30. The lithium ion secondary battery according to claim 29, characterized in that: The second negative electrode active layer satisfies one or more of the following characteristics: 10%≤f 21 ≤30%; 70%≤f 22 ≤90%。 31. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The first negative electrode active material and the second negative electrode active material each independently include carbon-coated negative electrode active particles; The carbon-coated negative electrode active particles include a second negative electrode active body and a carbon coating layer located on at least a portion of the surface of the second negative electrode active body, wherein the carbon coating layer includes one or more of amorphous carbon, soft carbon and hard carbon; The negative electrode plate meets one or more of the following characteristics: The graphitization degree of the carbon coating layer in the first negative electrode active material is higher than the graphitization degree of the carbon coating layer in the second negative electrode active material; The oxygen content of the carbon coating layer in the first negative electrode active material is lower than the oxygen content of the carbon coating layer in the second negative electrode active material.

32. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The first negative electrode active material includes secondary particles, and the second negative electrode active material includes single particles; The mass proportion or quantity proportion of the secondary particles in the first negative electrode active material is 60% to 100%; The mass ratio or number ratio of the single particle in the second negative electrode active material is 60% to 100%.

33. The lithium ion secondary battery according to claim 32, characterized in that: The first negative electrode active material includes graphite secondary particles, and the second negative electrode active material includes graphite single particles; The negative electrode plate meets one or two of the following characteristics: The mass proportion or quantity proportion of the graphite secondary particles in the first negative electrode active material is 60% to 100%; The mass ratio or quantity ratio of the single graphite particle in the second negative electrode active material is 60% to 100%.

34. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The negative electrode plate meets one or more of the following characteristics: The first negative electrode active material and the second negative electrode active material each independently include a carbon-based material, and the graphitization degree of the carbon-based material in the first negative electrode active material is lower than the graphitization degree of the carbon-based material in the second negative electrode active material; The sphericity of the first negative electrode active material is higher than the sphericity of the second negative electrode active material.

35. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The ratio of the thickness of the first negative electrode active layer to the sum of the thickness of the first negative electrode active layer and the second negative electrode active layer on one side of the negative electrode current collector is denoted as f H , satisfying 20%≤f H ≤70%.

36. The lithium ion secondary battery according to claim 35, characterized in that: 30%≤f H ≤50%。 37. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The constituent material of the first negative electrode active layer is recorded as the first negative electrode material, and the constituent material of the second negative electrode active layer is recorded as the second negative electrode material; The negative electrode plate meets one or two of the following characteristics: The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer; The powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

38. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The negative electrode plate meets one or two of the following characteristics: When the battery is fully discharged, the compaction density of the negative electrode plate is 1.08 g / cm 3 ~1.71g / cm 3 ; When the battery is fully discharged, the surface density of the negative electrode sheet is 10 mg / cm 2 ~26mg / cm 2 .

39. The lithium ion secondary battery according to claim 38, characterized in that: The negative electrode plate meets one or two of the following characteristics: When the battery is fully discharged, the compaction density of the negative electrode plate is 1.17 g / cm 3 ~1.52g / cm 3 ; When the battery is fully discharged, the surface density of the negative electrode is 15 mg / cm 2 ~20mg / cm 2 .

40. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that A lithium-replenishing residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer; the lithium-replenishing residual layer contains inactive lithium.

41. The lithium ion secondary battery according to claim 40, characterized in that: The negative electrode plate meets one or two of the following characteristics: The thickness of the lithium supplement residual layer is less than 0.1 μm on a single side of the negative electrode current collector; On one side of the negative electrode current collector, the lithium supplement residual layer accounts for less than or equal to 98% of the coverage area of ​​the first negative electrode active layer.

42. The lithium ion secondary battery according to claim 41, characterized in that: The negative electrode plate meets one or two of the following characteristics: The thickness of the lithium supplement residual layer is less than 0.08 μm on a single side of the negative electrode current collector; On one side of the negative electrode current collector, the lithium supplement residual layer accounts for 30% to 70% of the coverage area of ​​the first negative electrode active layer.

43. The lithium ion secondary battery according to claim 42, characterized in that: The negative electrode plate meets one or two of the following characteristics: The thickness of the lithium supplement residual layer is less than 0.05 μm on a single side of the negative electrode current collector; On one side of the negative electrode current collector, the lithium supplement residual layer accounts for 50% to 70% of the coverage area of ​​the first negative electrode active layer.

44. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that A plurality of micropores are arranged on a surface of the negative electrode current collector on one side close to the second negative electrode active layer.

45. The lithium ion secondary battery according to claim 44, characterized in that: The negative electrode current collector meets one or more of the following characteristics: The micropores penetrate the negative electrode current collector along the thickness direction of the negative electrode current collector; The pore size of the micropores is 5 μm to 500 μm.

46. ​​The lithium ion secondary battery according to claim 45, characterized in that: The pore size of the micropores is 30 μm to 200 μm.

47. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The NP ratio of the lithium ion secondary battery is 1.05-1.3, and the NP ratio of the lithium ion secondary battery is equal to the ratio of the negative electrode surface capacity to the positive electrode surface capacity.

48. The lithium ion secondary battery according to claim 47, characterized in that: The NP ratio of the lithium ion secondary battery is 1.1-1.

3.

49. The lithium ion secondary battery according to any one of claims 1 to 6, characterized in that The positive electrode plate includes a positive electrode active material, and the positive electrode active material includes one or more of a ternary positive electrode material, a modified form of a ternary positive electrode material, lithium iron phosphate, a modified form of lithium iron phosphate, lithium iron manganese phosphate, and a modified form of lithium iron manganese phosphate; the modified form includes one or more of a doping modification and a coating modification.

50. The lithium ion secondary battery according to claim 49, characterized in that: The positive electrode active material includes carbon-coated lithium iron phosphate, which includes a lithium iron phosphate body and a carbon coating layer located on at least a portion of the surface of the lithium iron phosphate body, and the carbon coating layer includes one or more of soft carbon, hard carbon and amorphous carbon.

51. A component for preparing a lithium ion secondary battery, characterized in that: It comprises an electrode assembly and an electrolyte, wherein the electrode assembly comprises a positive electrode sheet, a lithium-supplemented negative electrode sheet and a separator, and the separator is arranged between the positive electrode sheet and the lithium-supplemented negative electrode sheet; The lithium supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active initial layer, a first negative electrode active initial layer and a lithium supplemented layer sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active initial layer comprises a first negative electrode active material, and the second negative electrode active initial layer comprises a second negative electrode active material; The first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (t1) and (t2): (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material; (t2) The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 The lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 .

52. The component for preparing a lithium ion secondary battery according to claim 51, characterized in that: The lithium supplement layer includes single substance lithium.

53. The component for preparing a lithium ion secondary battery according to claim 51, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: Measured on one side of the negative electrode current collector, the thickness of the lithium supplement layer is less than the sum of the thicknesses of the first negative electrode active initial layer and the second negative electrode active initial layer; Calculated on a single side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is less than or equal to 98%.

54. The component for preparing a lithium ion secondary battery according to claim 53, characterized in that: Based on a single side of the negative electrode current collector, the lithium supplement layer accounts for 50% to 98% of the coverage area of ​​the first negative electrode active initial layer.

55. The component for preparing a lithium ion secondary battery according to claim 53, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The thickness of the lithium supplement layer is less than or equal to 8.5 μm on a single side of the negative electrode current collector; Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is 30% to 70%.

56. The component for preparing a lithium ion secondary battery according to claim 53, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: Measured on one side of the negative electrode current collector, the thickness of the lithium supplement layer is 1 μm to 4.8 μm; Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active initial layer is 50-70%.

57. The component for preparing a lithium ion secondary battery according to any one of claims 51 to 56, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The compaction density of the lithium supplemented negative electrode sheet is 1.3 g / cm 3 ~ 1.8 g / cm 3 ; The surface density of the lithium supplemented negative electrode sheet is 10 mg / cm 2 ~ 26 mg / cm 2 .

58. The component for preparing a lithium ion secondary battery according to claim 57, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The compaction density of the lithium supplemented negative electrode sheet is 1.4 g / cm 3 ~1.6g / cm 3 ; The surface density of the lithium supplemented negative electrode sheet is 15 mg / cm 2 ~20 mg / cm 2 .

59. A method for preparing a lithium ion secondary battery, characterized in that: The steps include: Assembling a positive electrode sheet, a separator and a lithium-supplemented negative electrode sheet into an electrode assembly, so that the separator is arranged between the positive electrode sheet and the lithium-supplemented negative electrode sheet; wherein the lithium-supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active initial layer, a first negative electrode active initial layer and a lithium-supplemented layer sequentially arranged on at least one side of the negative electrode current collector; the first negative electrode active initial layer comprises a first negative electrode active material, and the second negative electrode active initial layer comprises a second negative electrode active material; Placing the electrode assembly in the housing cavity of the shell, injecting an electrolyte, allowing the electrolyte to infiltrate the positive electrode sheet and the lithium-supplemented negative electrode sheet, and forming them to prepare a lithium-ion secondary battery; wherein the lithium-supplemented negative electrode sheet forms a negative electrode sheet, the second negative electrode active initial layer forms a second negative electrode active layer, and the first negative electrode active initial layer forms a first negative electrode active layer; Wherein, the first negative electrode active material and the second negative electrode active material each independently include one or more of natural graphite, artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite; The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (t1) and (t2): (t1) the lithium insertion potential of the first negative electrode active material is higher than the lithium insertion potential of the second negative electrode active material; (t2) The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 10 The proportion of the sum of the mass of artificial graphite, hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 20 The proportion of natural graphite in the total mass of the first negative electrode active material is denoted as f 15 , the proportion of natural graphite in the total mass of the second negative electrode active material is recorded as f 21 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the first negative electrode active material is recorded as f 19 The sum of the mass of hard carbon, soft carbon, silicon oxide and silicon-carbon composite in the total mass of the second negative electrode active material is recorded as f 29 The lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics: (i) f 10 >f 20 ≥0, or, f 10 ≥f 20 And f 19 >f 29 ; and (ii) 0 ≤ f 15 <f 21 , or, 0≤f 15 ≤f 21 And f 19 >f 29 .

60. The method for preparing a lithium ion secondary battery according to claim 59, characterized in that: The lithium replenishment layer in the lithium replenishment negative electrode sheet satisfies the following formula: 1.05≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3; Among them, C N_A is the negative electrode surface capacity, C P_A is the preset surface capacity of the positive electrode, ρ A is the surface density of the lithium supplement layer on the first negative electrode active initial layer based on the total amount on both sides, C Li / g is the theoretical gram capacity of lithium.

61. The method for preparing a lithium ion secondary battery according to claim 59, characterized in that: After the step of injecting the electrolyte and before the step of allowing the electrolyte to infiltrate the positive electrode sheet and the lithium-supplemented negative electrode sheet, the component for preparing a lithium-ion secondary battery as described in any one of claims 52 to 58 is obtained.

62. The method for preparing a lithium ion secondary battery according to claim 61, characterized in that: The prepared lithium ion secondary battery is the lithium ion secondary battery described in any one of claims 2 to 50.

63. An electrical device, characterized in that: The invention comprises at least one of the lithium ion secondary battery described in any one of claims 1 to 50, the component for preparing a lithium ion secondary battery described in any one of claims 51 to 58, and a lithium ion secondary battery prepared by the method for preparing a lithium ion secondary battery described in any one of claims 59 to 61.

Citation Information

Patent Citations

  • Negative lithium supplementing pole piece and lithium ion battery

    CN112331928A

  • Negative pole piece, electrochemical device and electronic device

    CN113066961A

  • Negative plate capable of being quickly embedded with lithium and battery comprising negative plate

    CN115064658A

  • Negative plate, lithium ion battery and vehicle

    CN117577772A

  • Negative plate, lithium ion battery and vehicle

    CN117577773A

Cited By

  • Negative plate and secondary battery thereof

    CN119812199A

  • Negative pole piece, preparation method thereof and battery

    CN119812214A

  • Lithium secondary battery, negative pole piece for lithium secondary battery and electric device

    CN120015770A

  • A lithium secondary battery, a negative electrode sheet for a lithium secondary battery, and an electric device

    CN120015770B

  • Lithium-ion battery

    EP4832131A1