Existing EUV lithography processes face challenges with pattern collapse and non-uniform component distribution in chemically amplified resists, leading to inferior image performance and aspect ratio issues in metal oxide photoresists, particularly for features like holes or vias.
A novel plasma-based process for patterning metal oxide photoresists involves exposing the resist to EUV light, separating organic ligands, followed by a bake process and iterative plasma etching steps using hydrocarbon or fluorocarbon-based plasmas for deposition and hydrogen or halogen-based plasmas for etching, to create precise patterns.
This method improves pattern fidelity and reduces line edge roughness and critical dimension control, enabling effective patterning of complex features like holes and vias with enhanced precision and cleanliness compared to traditional wet processes.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] Incorporation by Reference This disclosure claims the benefit of U.S. Non-Provisional Patent Application No. 17 / 097,921, filed Nov. 13, 2020, the entire contents of which are incorporated herein by reference.
Background Art
[0002] This disclosure relates to the processing of substrates. Specifically, this disclosure provides novel systems and methods for patterning EUV (or shorter wavelength) photoresists.
[0003] To achieve reduced feature sizes, patterning using extreme ultraviolet (EUV) lithography has been introduced into processing systems. EUV lithography typically uses light having a wavelength of 6 - 16 nanometers (nm) or less. For example, EUV patterning technology has been introduced into production in the manufacture of advanced semiconductor devices at the sub-7 nm node. Although reduced feature sizes have been achieved, there are problems with pattern performance in EUV patterning.
[0004] To transfer a pattern onto one or more underlying layers formed on a substrate, chemically amplified resists (CARs) have been used in EUV lithography. Such resists have good sensitivity, but the resolution of CARs is more strongly affected by pattern collapse, which becomes increasingly important as the feature size approaches the nanometer scale. In addition, it is difficult to reduce the aspect ratio (film thickness / critical dimension) of CARs because of their high sensitivity to non-uniform distributions of components in the film. As a result, CARs tend to have poor image performance.
[0005] Metal oxide photoresists have been used in negative-type EUV lithography to transfer patterns onto one or more underlying layers formed on a substrate. Compared to CAR, metal oxide photoresists offer the advantage of very thin film thicknesses, minimizing the risk of pattern collapse. The conventional processes used to form metal oxide photoresists are a promising alternative to CAR, but they utilize a wet process for pattern development. For example, metal oxide photoresists can be developed using a wet organic developer in a negative-type photoresist process. While negative-type photoresists may be suitable for patterning line / space features and blocks, they have not been satisfactory for patterning other features such as holes or vias. [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] Therefore, there is a need for improved processes and methods for patterning metal oxide photoresists used in EUV (or shorter wavelength) lithography. [Means for solving the problem]
[0007] Improved process flows and methods for patterning photoresists with extreme ultraviolet (EUV) or shorter wavelength light are provided herein. More specifically, improved process flows and methods for patterning metal oxide photoresists are provided herein, which can be used in EUV (or shorter wavelength) photolithography to transfer a pattern onto one or more underlayers formed on a substrate. In the disclosed process flows and methods, a patterning layer comprising a metal oxide photoresist is formed on one or more underlayers provided on a substrate, and portions of the patterning layer that are not covered by a mask on the patterning layer are exposed with EUV light or shorter wavelength light. Exposure with EUV or shorter wavelength light separates organic ligands from the metal oxide structure (e.g., cage or chain) in the exposed portions of the metal oxide photoresist, while leaving the unexposed portions of the metal oxide photoresist unchanged. After exposure with EUV or a shorter wavelength, a bake process is performed to release organic ligands released from the exposed areas of the metal oxide photoresist, and the exposed areas are removed using a plasma process (e.g., etching) to develop the metal oxide photoresist pattern.
[0008] The plasma processes described herein can develop metal oxide photoresist patterns using a plurality of deposition and etching steps. In some embodiments, a hydrocarbon or fluorocarbon plasma may be used in the deposition step to selectively deposit a protective layer (or film) on the unexposed areas of the metal oxide photoresist. During the etching step, a hydrogen or halogen plasma may be used to selectively convert the surface of the exposed areas of the metal oxide photoresist to a volatile material (e.g., metal hydrides, halides, or chlorides), which can be removed, for example, by ion bombardment. The protective layer selectively deposited on the unexposed areas of the metal oxide photoresist protects the unexposed areas from erosion while the exposed areas of the metal oxide photoresist are selectively etched during the etching step. In some embodiments, the plasma development process described herein may be continued in an iterative manner, repeating the selective deposition and selective etching steps until the exposed areas of the metal oxide photoresist are completely removed.
[0009] According to one embodiment, a method for patterning a substrate is provided. In this embodiment, the method may include forming a patterning layer and one or more underlayers on a substrate, wherein the patterning layer comprises a metal oxide photoresist, and performing an extreme ultraviolet (EUV) or shorter wavelength lithography process, wherein portions of the patterning layer not covered by an overhead mask are exposed to EUV light or shorter wavelength light. In addition, the method may include performing a repeated dry process to remove portions of the patterning layer exposed to EUV light or shorter wavelength light and to develop the metal oxide photoresist pattern.
[0010] In some embodiments, the iterative dry process may include selectively depositing a protective layer on the unexposed portions of the patterning layer by exposing the substrate to a first plasma, selectively etching the exposed portions of the patterning layer by exposing the substrate to a second plasma, and repeating the selective deposition and selective etching until the exposed portions of the patterning layer are completely removed. The unexposed portions of the patterning layer are covered by the mask above and are not exposed to EUV light or shorter wavelength light. In contrast, the exposed portions of the patterning layer are not covered by the mask above and are exposed to EUV light or shorter wavelength light.
[0011] The first and second plasmas can utilize a wide variety of precursor gases. In some embodiments, the first plasma may contain hydrocarbon or fluorocarbon-based precursor gases. In some embodiments, the second plasma may contain hydrogen or halogen-containing precursor gases and an inert gas.
[0012] Each time a selective etching process is performed, a hydrogen or halogen-containing precursor gas converts the exposed surface of the patterning layer into a volatile material, and ions from an inert gas collide with the substrate surface to remove the volatile material from the exposed areas. Each time a selective deposition process is performed, a new protective layer is deposited on the unexposed areas of the patterning layer.
[0013] Another embodiment provides a method for patterning a substrate. This embodiment may include forming a patterning layer and one or more underlayers on the substrate, wherein the patterning layer comprises a metal oxide photoresist, and exposing the portion of the patterning layer not covered by a mask above the patterning layer with extreme ultraviolet (EUV) light or light of a shorter wavelength. In addition, the method may include selectively depositing a protective layer on the unexposed portion of the patterning layer by exposing the substrate to a first plasma, selectively etching the exposed portion of the patterning layer by exposing the substrate to a second plasma, and repeating the selective deposition and selective etching steps until the exposed portion of the patterning layer is completely removed.
[0014] In some embodiments, the patterning layer may include a metal oxide material, which includes clusters of metal oxide structures having chemically bonded organic ligands. In such embodiments, exposure of the portion of the patterning layer not covered by the patterned mask layer with EUV light or shorter wavelength light separates the organic ligands from the metal oxide structures while leaving the unexposed portion of the patterning layer unchanged. The method may further include performing a bake process after exposure of the portion of the patterning layer not covered by the patterned mask layer with EUV light or shorter wavelength light, and before selective deposition of a protective layer on the unexposed portion of the patterning layer, to release the organic ligands from the exposed portion of the patterning layer.
[0015] As described above, the first and second plasmas can utilize a wide variety of precursor gases. In some embodiments, the first plasma may contain hydrocarbon or fluorocarbon precursor gases. For example, the first plasma may contain CH4, C4F8, C4F6, or CH3F. In some embodiments, the second plasma may contain hydrogen or halogen-containing precursor gases. For example, the second plasma may contain CH4, CF4, CHF3, or BCl3. In some embodiments, the second plasma may further contain an inert gas. For example, the second plasma may further contain argon (Ar). When the second plasma contains a hydrogen or halogen-containing precursor gas and an inert gas, the hydrogen or halogen-containing precursor gas converts the surface of the exposed portion of the patterning layer into a volatile material, and the inert gas ions collide with the surface of the exposed portion to remove the volatile material.
[0016] In some embodiments, the steps of selectively depositing a protective layer on the unexposed portions of the patterning layer and selectively etching the exposed portions of the patterning layer are performed simultaneously in a plasma processing chamber using the same plasma precursor gas that generates the first and second plasmas. In such embodiments, for example, the first and second plasmas may each contain a hydrocarbon precursor and an inert gas, respectively.
[0017] In other embodiments, the steps of selectively depositing a protective layer on the unexposed portion of the patterning layer and selectively etching the exposed portion of the patterning layer are separated within the plasma processing chamber, so that the first and second plasmas are generated using different plasma precursor gases. In such embodiments, for example, the first plasma may contain a hydrocarbon precursor, and the second plasma may contain a halocarbon precursor and an inert gas.
[0018] A more complete understanding of the present invention and its merits can be obtained by referring to the following description, which is to be interpreted in conjunction with the accompanying drawings, which show similar reference numerals and similar features. However, it should be noted that the accompanying drawings are for illustrative purposes only and are not to be considered limiting, and that the disclosed concept may also be permitted in other equally effective embodiments. [Brief explanation of the drawing]
[0019] [Figure 1A-1F] This shows an improved process flow for patterning substrates, more specifically, for patterning extreme ultraviolet (EUV) photoresist. [Figure 2] This is a flowchart illustrating one embodiment of a method for patterning a circuit board. [Figure 3] This is a flowchart illustrating another embodiment of a method for patterning a substrate. [Figure 4] This is a block diagram representing one embodiment of a plasma processing system that can be used to pattern a substrate using the techniques described herein. [Modes for carrying out the invention]
[0020] Improved process flows and methods for patterning extreme ultraviolet (EUV) (or shorter wavelength) photoresists are provided herein. More specifically, improved process flows and methods for patterning metal oxide photoresists are provided herein, which can be used in EUV or shorter wavelength photolithography to transfer patterns onto one or more underlayers formed on a substrate. The process flows and methods disclosed herein can be used with a wide variety of metal oxide materials, including but not limited to metal oxides containing tin (Sn), hafnium (Hf), and zirconium (Zr). Although metal oxide materials containing Sn, Hf, or Zr are disclosed herein as examples, the process flows and methods disclosed herein are extendable to other metal oxide materials and metal-containing photoresists. Exemplary embodiments utilizing EUV wavelength light are discussed as described herein. However, the techniques used herein are not limited to EUV wavelengths. Furthermore, the techniques may be particularly advantageous for EUV light or shorter wavelength light. Therefore, although some embodiments in this specification are described with respect to EUV wavelengths, the techniques provided may also be applicable to EUV light or light of shorter wavelengths.
[0021] In the disclosed process flow and method, a patterning layer containing a metal oxide photoresist is formed on one or more underlying layers provided on a substrate, and portions of the patterning layer not protected by a mask between the light source and the patterning layer are exposed with EUV light. EUV exposure separates organic ligands from the metal oxide structure (e.g., cage or chain) in the exposed portions of the metal oxide photoresist, while leaving the unexposed portions unchanged. After EUV exposure, a bake process is performed to release the organic ligands released from the exposed portions of the metal oxide photoresist, and the exposed portions are removed (e.g., etched) using a plasma process to develop the metal oxide photoresist pattern. Thus, dry plasma development of a metal oxide photoresist is provided.
[0022] The plasma process described herein can develop a metal oxide photoresist pattern using multiple deposition and etching steps. In some embodiments, a hydrocarbon or fluorocarbon-based plasma may be used in the deposition step to selectively deposit a protective layer (or film) on the unexposed portions of the metal oxide photoresist. During the etching step, a hydrogen or halogen-based plasma can be used to selectively convert the surface of the exposed portions of the metal oxide photoresist into volatile materials (e.g., metal hydrides, halides, or chlorides), which can be removed, for example, by ion bombardment. The protective layer selectively deposited on the unexposed portions of the metal oxide photoresist protects the unexposed portions from erosion while the exposed portions of the metal oxide photoresist are being selectively etched during the etching step. In some embodiments, the plasma development process described herein may be continued in an iterative fashion by repeating the selective deposition step and the selective etching step until the exposed portions of the metal oxide photoresist are completely removed.
[0023] In response thereto, a novel plasma development process for metal oxide photoresists is disclosed herein for evolved EUV patterning. The plasma development process enables selective deposition and selective etching at the molecular / atomic level with precise plasma process control. In addition to other plasma process parameters, the plasma precursor is selected to selectively convert the surface of the EUV activation region (i.e., the exposed portion of the metal oxide photoresist) to a more volatile material (e.g., metal hydride, halogen or chloride) in the selective etching step and to selectively deposit a protective layer on the non-activation region (i.e., the unexposed portion of the metal oxide photoresist) in the selective deposition step. In some embodiments, the plasma treatment steps disclosed herein may be performed simultaneously in a plasma process chamber using the same plasma precursor for both the deposition and etching steps. In other embodiments, the plasma treatment steps may be separated in the plasma process chamber such that the deposition and etching steps can be performed using different plasma precursors.
[0024] Figures 1A - 1F illustrate one embodiment of an improved process flow for patterning an EUV metal oxide photoresist according to the technology disclosed herein. It will be understood that the embodiments shown in Figures 1A - 1F are merely exemplary and that the technology described herein may be applied to other process flows.
[0025] As shown in Figure 1A, substrate 100 includes a patterning layer 108 formed on top of one or more underlying layers such as, for example, hard mask layer 106, sacrificial carbon layer 104, and base substrate 102. Base substrate 102 can be any substrate on which the use of patterned features is desired. For example, base substrate 102 can be a semiconductor substrate having one or more semiconductor processing layers formed thereon. In one embodiment, base substrate 102 can be a substrate that has been subjected to a plurality of semiconductor processing steps that result in a wide variety of structures and layers, all of which are known in substrate processing technology.
[0026] The hard mask layer 106 and the sacrificial carbon layer 104 may be formed from any of the wide variety of materials known in the art. In one embodiment, the hard mask layer 106 may be a spin-on-glass (SOG) layer, and the sacrificial carbon layer 104 may be a spin-on-carbon (SOC) layer. However, it should be understood that the underlying layers described and illustrated are merely examples, and more underlying layers, fewer underlying layers, or other underlying layers may be used.
[0027] The patterning layer 108 shown in Figure 1A can be formed from any of the wide variety of materials commonly used in EUV lithography. For example, the patterning layer 108 may be a metal oxide photoresist. In some embodiments, the patterning layer 108 may contain a metal oxide material containing tin (Sn), hafnium (Hf), or zirconium (Zr). Other metal oxide materials can also be used to realize the patterning layer 108. In some embodiments, a metal-containing non-oxide photoresist material can be used to realize the patterning layer 108. The patterning layer 108 can generally be formed using any of the wide variety of deposition processes. In some embodiments, for example, a spin-coating process can be used to form the patterning layer 108. However, the techniques described herein are not limited to methods for forming the patterning layer 108.
[0028] In the exemplary embodiment shown in Figure 1A, the patterning layer 108 may include a metal oxide material, which includes clusters of metal oxide structures (MOs) having chemically bonded organic ligands (L). As will be described in more detail below, the process flow shown in Figures 1B-1C involves exposing a portion of the patterning layer 108 with extreme ultraviolet (EUV) light to separate or release the organic ligands (L) from the metal oxide structures (MOs), and then performing a bake process to release the ligands released from the EUV-exposed portion of the patterning layer 108. Once the organic ligands are released, the EUV-exposed portion of the patterning layer 108 is removed using a repeating dry process, as shown in Figures 1D-1F, to develop the metal oxide photoresist pattern.
[0029] In Figure 1A, the patterning layer 108 is formed, and in Figure 1B, a mask 110 is placed above the patterning layer 108, and an EUV lithography process is performed. During the EUV lithography process shown in Figure 1B, the exposed portion 114 of the patterning layer 108 (i.e., the portion of the patterning layer 108 not protected by the mask 110) is exposed by an EUV light source 112. As shown in Figure 1B, EUV exposure separates the organic ligand (L) from the metal oxide structure (MO) only within the exposed portion 114 of the patterning layer 108, while leaving the unexposed portion 116 of the patterning layer 108 unchanged.
[0030] In Figure 1B, after the EUV lithography process is performed, a post-exposure bake (PEB) process is carried out, and as shown in Figure 1C, the released ligands are released from the exposed areas 114 of the patterning layer 108, leaving only the dense metal oxide structure (MO) in the exposed areas 114. After the PEB process, a dry process (e.g., a plasma development process) is used to remove the exposed areas 114 of the patterning layer 108 and develop the metal oxide photoresist pattern.
[0031] Figures 1D to 1F show an embodiment of a plasma development process that can be used to develop a metal oxide photoresist pattern according to the techniques described herein. As will be described in more detail below, the disclosed plasma development process may generally include a plurality of deposition and etching steps. In some embodiments, the plasma development process can begin by exposing a substrate 100 to a first plasma 118, as shown in Figure 1D, to selectively deposit a protective layer 120 on the unexposed portions 116 of the patterning layer 108. After the protective layer 120 is formed on the unexposed portions 116, the substrate 100 is exposed to a second plasma 122, as shown in Figure 1E, to selectively etch or remove the exposed portions 114 of the patterning layer 108. The protective layer 120 protects the unexposed portions 116 of the patterning layer 108 from erosion, while the exposed portions 114 of the patterning layer 108 are selectively etched and removed during the selective etching step. In some embodiments, the plasma development process shown in Figures 1D and 1E may be repeated multiple times, and / or continued until the exposed portion 114 of the patterning layer 108 is completely removed, as shown in Figure 1F.
[0032] In the selective deposition process shown in Figure 1D, various plasma chemicals can be used. In some embodiments, the first plasma 118 can selectively deposit a protective layer 120 on the unexposed portion 116 of the patterning layer 108 using hydrocarbon or fluorocarbon precursor gas chemicals. Examples of hydrocarbon and fluorocarbon chemicals that can be used in the first plasma 118 include, but are not limited to, CH4, C4F8, C4F6, or CH3F. Other hydrocarbon or fluorocarbon chemicals can also be used in the selective deposition process shown in Figure 1D.
[0033] In the selective etching process shown in Figure 1E, various plasma chemicals can be used. In some embodiments, the second plasma 122 can use a hydrogen or halogen-containing precursor gas chemical to convert the surface of the exposed portion 114 into a volatile material (e.g., a metal hydride, halide, or chloride), and an inert gas (e.g., argon) can be used to selectively etch or remove the volatilized surface via ion bombardment. Examples of hydrogen or halogen-containing precursor gas chemicals that can be used in the second plasma 122 include, but are not limited to, hydrocarbon chemicals (e.g., CH4), halocarbon chemicals (e.g., CF4, CHF3), and other halogen chemicals (e.g., BCl3), which are commonly used in plasma etching. In some embodiments, a combination of a hydrocarbon precursor gas and an inert gas can be used to generate the second plasma 122. In other embodiments, the second plasma 122 may include a combination of a halocarbon, hydrogen, and an inert gas.
[0034] The hydrogen (or halogen) component in the second plasma 122 facilitates etching by converting the surface of the metal oxide material in the exposed area 114 into volatile metal hydrides, halides, or chlorides, which are removed by ion bombardment in one embodiment. In some embodiments, the selective etching process shown in Figure 1E can be carried out as a single step by exposing the substrate 100 to a plasma containing a hydrogen (or halogen)-containing precursor gas and an inert gas (e.g., argon). In other embodiments, the selective etching process may be an iterative process in which the substrate 100 is exposed to a hydrogen (or halogen)-based plasma before being exposed to an argon plasma.
[0035] In this specification, an exemplary embodiment is described with reference to argon (Ar), but in the selective etching process shown in Figure 1D, other inert gas ions may also be used to impact the surface of the exposed portion 114. Exemplary inert gases include, but are not limited to, He, Ne, Kr, and other noble gases. Furthermore, other gases can be used in combination with argon and / or noble gases. For example, the plasma is not limited to having only argon gas or noble gases, so other gases can be added to the plasma. For example, other inert gases, or other gases that are not inert gases, may be added to the process.
[0036] In some embodiments, the selective deposition and selective etching processes shown in Figures 1D and 1E may be carried out simultaneously within a plasma processing chamber, or they may be separated into two plasma processing processes, for example, by one or more purging processes. In one embodiment, the selective deposition and etching processes may be carried out simultaneously within a plasma process chamber using the same plasma precursor (e.g., CH4) for both the deposition and etching processes. In other embodiments, the selective deposition and etching processes may be separated within a plasma process chamber so that different plasma precursors can be used for the deposition and etching processes. For example, the selective deposition and etching processes may be separated within a plasma process chamber, resulting in the use of a hydrocarbon precursor (e.g., CH4) in the deposition process, while hydrogen (H2), halocarbon chemicals (e.g., CF4 or CHF3), and halogenated chemicals (e.g., BCl3) are used in the etching process.
[0037] The selective deposition and etching steps shown in Figures 1D and 1E may be carried out as an iterative process, which is repeated over multiple cycles until the exposed portions 114 of the patterning layer 108 are completely removed, as shown in Figure 1F. Each time the etching step is performed, some or all of the protective layer 120 formed on the unexposed portions 116 may be removed along with the volatilized surface of the exposed portions 114. In one embodiment, a very thin protective layer may remain after each cycle. In each subsequent deposition step, a new protective layer 120 is formed on the top and sides of the unexposed portions 116, as shown in Figure 1F. To avoid etching the hard mask layer 106 beneath the patterning layer 108, the plasma chemicals used in the selective deposition and etching steps described herein may generally be selective to the hard mask layer 106.
[0038] Compared to conventional pattern development processes that use a wet process to develop negative metal oxide photoresists, the plasma development process shown in Figures 1D-1F uses an iterative dry process for pattern development of positive photoresists. Unlike negative photoresists, positive photoresists can be used for patterning holes, blocks, and lines / spaces in processes with narrow geometric shapes. By utilizing an iterative dry process for pattern development, the plasma development process described herein provides atomic layer control of the surface reaction, improving control of line edge roughness (LER) and critical dimension (CD) compared to conventional wet-process pattern development. The plasma development process described herein is also cleaner and more cost-effective than conventional wet-process pattern development.
[0039] Figures 2 and 3 illustrate exemplary methods for patterning a substrate using the plasma development process described herein. The embodiments in Figures 2 and 3 are illustrative, and it will be understood that additional methods may utilize the techniques described herein. Furthermore, since the described processing steps are not intended to be exclusive, additional steps may be added to the methods shown in Figures 2 and 3. Moreover, the order of the steps is not limited to the order shown in the figures, as different orders may occur and / or various steps may be performed in combination or simultaneously. Furthermore, although the methods in Figures 2 and 3 are described with respect to EUV light, it will be understood that EUV light or shorter wavelength light may be advantageous.
[0040] Figure 2 shows one embodiment of Method 200 that can be used to pattern a substrate using the techniques disclosed herein. In some embodiments, Method 200 can begin by forming a patterning layer and one or more underlayers on a substrate, the patterning layer comprising a metal oxide photoresist (step 210). After the patterning layer is formed, Method 200 performs an extreme ultraviolet (EUV) lithography step, in which portions of the patterning layer not covered by the mask above are exposed to EUV light (step 220). In step 230, Method 200 performs a repeating dry process to remove portions of the patterning layer exposed to EUV light and develop the metal oxide photoresist pattern.
[0041] Figure 3 shows another embodiment of Method 300 that can be used to pattern a substrate using the techniques disclosed herein. In some embodiments, Method 300 can begin by forming a patterning layer and one or more underlayers on a substrate, the patterning layer comprising a metal oxide photoresist (step 310). After the patterning layer is formed, Method 300 exposes the portion of the patterning layer that is not covered by a mask above the patterning layer with extreme ultraviolet (EUV) light (step 320). In step 330, Method 300 selectively deposits a protective layer on the unexposed portion of the patterning layer by exposing the substrate to a first plasma. The unexposed portion of the patterning layer is covered by a mask and not exposed by the EUV light source. In step 340, Method 300 selectively etches the exposed portion of the patterning layer by exposing the substrate to a second plasma. In step 350, Method 300 repeats the selective deposition and selective etching until the exposed portion of the patterning layer is completely removed.
[0042] Figure 4 provides an illustrative embodiment of a plasma processing system 400 that may be used in relation to the disclosed technology and is provided for illustrative purposes only. The plasma processing system 400 shown in Figure 4 is a capacitively coupled plasma (CCP) processing system, but those skilled in the art will understand that the technology described herein may be implemented with inductively coupled plasma (ICP) processing systems, microwave plasma processing systems, radial line slot antenna (RLSA™) microwave plasma processing systems, electron cyclotron resonance (ECR) plasma processing systems, or other types of processing systems or combinations of systems. Accordingly, those skilled in the art will understand that the technology described herein may be used with any of the wide variety of plasma processing systems.
[0043] The plasma processing system 400 can be used for a wide variety of operations, including but not limited to etching, deposition, cleaning, plasma polymerization, plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), and atomic layer etching (ALE). The structure of the plasma processing system 400 is well known, and the specific structures described herein are for illustrative purposes only. It will be understood that different and / or additional plasma process systems can be realized while still utilizing the techniques described herein.
[0044] Looking at Figure 4 in more detail, the plasma processing system 400 may include a process chamber 405. As is well known in the art, the process chamber 405 may be a pressure control chamber. A substrate 410 (a semiconductor wafer in one example) may be held on a stage or chuck 415. As shown in the figure, an upper electrode 420 and a lower electrode 425 may be provided. The upper electrode 420 may be electrically coupled to a first radio frequency (RF) power supply 430 via a first matching network 455. The first RF power supply 430 has an upper frequency (f U The power supply voltage 435 can be supplied at ). The lower electrode 425 can be electrically coupled to the second RF power supply 440 via the second matching network 457. The second RF power supply 440 has a lower frequency (f L A bias voltage 445 can be supplied via ). Although not shown, it is well known to those skilled in the art that the voltage can also be applied to the chuck 415.
[0045] The components of the plasma processing system 400 are connected to and controlled by a control unit 470. The control unit 470 can then be connected to a corresponding memory storage unit and a user interface (all not shown). Various plasma processing operations can be performed via the user interface, and various plasma processing recipes and operations can be stored in the storage unit. Thus, a given substrate can be processed in the plasma processing chamber using various microfabrication techniques. It will be understood that the control unit 470 can be connected to various components of the plasma processing system 400 to receive inputs from the components and provide outputs to the components.
[0046] The control unit 470 can be implemented in a wide variety of ways. For example, the control unit 470 may be a computer. In another example, the control unit may include one or more programmable integrated circuits programmed to provide the functions described herein. For example, one or more processors (e.g., microprocessors, microcontrollers, central processing units, etc.), programmable logic devices (e.g., complex programmable logic devices (CPLDs), field programmable gate arrays (FPGAs), etc.), and / or other programmable integrated circuits can be programmed with software or other programming instructions to realize the functions of the proposed plasma process recipe. It should be further noted that the software or other programming instructions may be stored in one or more non-temporary computer-readable media (e.g., memory storage devices, flash memory, dynamic random access (DRAM) memory, reprogrammable storage devices, hard drives, floppy disks, DVDs, CD-ROMs, etc.), and that when the software or other programming instructions are executed by the programmable integrated circuit, they cause the programmable integrated circuit to perform the processes, functions, and / or capabilities described herein. Other variations may also be implemented.
[0047] During operation, the plasma processing system 400 generates plasma 460 in the process chamber 405 using the upper and lower electrodes when power is applied to the system from the first RF power supply 430 and the second RF power supply 440. When power is applied, a high-frequency electric field is generated between the upper electrode 420 and the lower electrode 425. The processing gas sent to the process chamber 405 can then be dissociated and converted into plasma 460. The generated plasma 460 can be used to process a target substrate (e.g., substrate 410 or any material to be processed) in various types of processing, including but not limited to plasma deposition, etching, and / or ion bombardment / sputtering.
[0048] In some embodiments, the selective deposition and etching steps disclosed herein may be carried out simultaneously using the same plasma 460. For example, a hydrocarbon (e.g., CH4) plasma 460 can be used to selectively deposit a protective layer on the unexposed portions 116 and selectively etch the exposed portions 114 of the patterning layer 108. In other embodiments, the selective deposition and etching steps disclosed herein may use different plasmas 460 separated within the process chamber 405 by, for example, one or more purging steps.
[0049] As shown in Figure 4, the exemplary plasma processing system 400 described herein utilizes two RF power supplies. In the exemplary embodiment, the first RF power supply 430 supplies power at a relatively high frequency to convert the processing gas sent to the process chamber 405 into plasma and control the plasma density, while the second RF power supply 440 supplies bias power at a lower frequency to control the ion shock energy.
[0050] In one exemplary plasma processing system, a first RF power supply 430 may supply power to the upper electrode 420 with a power supply of approximately 0 to 1400 W in the high frequency (HF) range of approximately 3 MHz to 150 MHz (or above), and a second RF power supply 440 may supply bias power to the lower electrode 425 with a bias power of approximately 0 to 1400 W in the low frequency (LF) range of approximately 0.2 MHz to 60 MHz. Different operating ranges may be used depending on the type of plasma processing system and the type of processing performed (e.g., etching, deposition, sputtering, etc.).
[0051] In one exemplary embodiment, the first plasma 118 used in the deposition process shown in Figure 1D may be carried out under process conditions of 50W to 1000W power, 0W to 200W bias power, 10mT to 200mT pressure, 0°C to 150°C electrostatic chuck temperature, and 50 standard cubic centimeters (SCCM) of CH4 gas flow. Other gases, such as CH3F and CH2F2, may also be used in the gas flow.
[0052] In one exemplary embodiment, the second plasma 122 used in the etching process shown in Figure 1E may be carried out under process conditions of 50W to 1000W power supply, 0W to 200W bias power, 10mT to 200mT pressure, 10°C to 150°C electrostatic chuck temperature, and 20 to 100 standard cubic centimeters (SCCM) of CH4 gas flow. Other gases, such as Cl2, BCl3, and inert gases, may also be used in the gas flow. In some embodiments, the bias power may be adjusted or controlled to control the ion bombardment energy during the etching process. In some embodiments, a separate surface activation / ion bombardment process may be carried out under process conditions of 100W to 500W power supply, 0W to 200W bias power, 10mT to 200mT pressure, 10°C to 200°C electrostatic chuck temperature, and 800 standard cubic centimeters (SCCM) of Ar gas flow. Other gases, such as He, Ne, and Kr, may also be used in the gas flow.
[0053] It should be noted that the techniques described herein may be used in a wide range of plasma processing systems. While Figure 4 shows a specific plasma processing system 400, it will be understood that the techniques described herein may be used in other plasma processing systems. In one exemplary system, the RF power supply shown in Figure 4 may be interchangeable (for example, a higher frequency may be supplied to the lower electrode 425 and a lower frequency to the upper electrode 420). Furthermore, in Figure 4, a dual power supply system is shown simply as an exemplary system. It will be understood that the techniques described herein may be used in conjunction with other plasma processing systems in which a modulated RF power supply is supplied to one or more electrodes, a DC bias power supply is utilized, or other system components are utilized.
[0054] It should be noted that one or more of the material layers described herein can be formed using various deposition processes. For example, one or more layers can be deposited using chemical vapor deposition (CVD), plasma-enhanced CVD (PECVD), physical vapor deposition (PVD), atomic layer deposition (ALD), and / or other deposition processes. In exemplary plasma deposition processes, precursor gas mixtures, including but not limited to hydrocarbons and fluorocarbons, can be used in combination with one or more diluent gases (e.g., argon, nitrogen, etc.) under various pressure, power, flow, and temperature conditions.
[0055] It should be further noted that various etching processes can be used to etch one or more of the material layers shown and described herein. For example, one or more etching processes may be implemented using plasma etching processes, discharge etching processes, and / or other desired etching processes. The plasma etching processes described herein can be implemented using plasmas containing hydrogen, halocarbons and other halogen-containing chemicals, argon, and / or other gases. As described above, one or more operating parameters (e.g., bias power) of the plasma etching processes described herein may be adjusted to control the ion impact energy during the etching process.
[0056] Other operating variables for the process steps can also be adjusted to control the various deposition and / or etching processes described herein. These operating variables may include, for example, chamber temperature, chamber pressure, gas flow rate, gas type, and / or other operating variables for the processing steps. Modified forms can also be realized while still utilizing the techniques described herein.
[0057] Throughout this specification, any reference to “one embodiment” or “an embodiment” means that certain features, structures, materials, or properties described in relation to that embodiment are included in at least one embodiment of the present invention, but not that they are present in all embodiments. Therefore, the appearance of the phrase “in one embodiment” or “in an embodiment” in various places throughout this specification does not necessarily refer to the same embodiment of the present invention. Furthermore, certain features, structures, materials, or properties may be combined in any preferred form in one or more embodiments. In other embodiments, various additional layers and / or structures may be included, and / or the described features may be omitted.
[0058] As used herein, the term “substrate” means and includes a base material or structure on which a material is formed. It will be understood that a substrate may include a single material, multiple layers of various materials, one or more layers having regions of various materials or various structures. These materials may include semiconductors, insulators, conductors, or combinations thereof. For example, a substrate may be a semiconductor substrate, a base semiconductor layer on a support structure, a metal electrode, or a semiconductor substrate on which one or more layers, structures, or regions are formed. A substrate may be a conventional silicon substrate or other bulk substrate including a layer of semiconducting material. As used herein, the term “bulk substrate” means and includes not only silicon wafers, but also silicon-on-insulator ("SOI") substrates such as silicon-on-sapphire ("SOS") substrates and silicon-on-glass ("SOG") substrates, an epitaxial layer of silicon on a base semiconductor substrate, and other semiconductor or optoelectronic materials, such as silicon germanium, germanium, gallium arsenide, gallium nitride, and indium phosphide. The circuit board may or may not be doped.
[0059] Systems and methods for processing substrates are described in various embodiments. The substrate may include any material portion or structure of a device, in particular a semiconductor or other electronic device, and may be a base substrate structure such as a semiconductor substrate, or a layer, such as a thin film, on or covering a base substrate structure. Therefore, the substrate is not intended to be limited to any particular base structure, underlay, or toplay, whether patterned or unpatterned, but rather to include any such layer or base structure, and any combination of layers and / or base structures.
[0060] As those skilled in the art will understand, various embodiments may be carried out without one or more of the specific details, or with other alternative and / or additional methods, materials, or components. In other examples, well-known structures, materials, or operations are not illustrated or described in detail so as not to obscure the various embodiments of the present invention. Similarly, a specific number, materials, and configurations are described for illustrative purposes in order to provide a full understanding of the present invention. Nevertheless, the present invention may be carried out without specific details. Furthermore, it should be understood that the various embodiments shown in the drawings are illustrative and not necessarily drawn to scale.
[0061] As this specification is considered, further modifications and alternative embodiments of the systems and methods described will be apparent to those skilled in the art. Therefore, it will be understood that the systems and methods described are not limited by these exemplary configurations. It should be understood that the forms of systems and methods illustrated and described herein should be interpreted as exemplary embodiments. Various modifications can be made to the implementation. Accordingly, although the invention is described herein with reference to specific embodiments, various modifications and changes can be implemented without departing from the spirit of the invention. Accordingly, this specification and the drawings should be considered illustrative rather than restrictive, and such modifications are intended to be within the scope of the invention. Furthermore, no benefit, advantage, or solution to a problem described herein with respect to a particular embodiment is intended to be interpreted as any or all of the important, necessary, or essential features or elements of the claims.
Claims
1. 1. A method of patterning a substrate, comprising the steps of: forming a patterning layer and one or more underlayers on the substrate, the patterning layer comprising a metal oxide photoresist; performing an extreme ultraviolet (EUV) or shorter wavelength lithography process, wherein portions of the patterning layer not covered by an overlying mask are exposed to EUV or shorter wavelength light; performing an iterative dry process to remove the portions of the patterning layer exposed to the EUV or shorter wavelength light and to develop a metal oxide photoresist pattern; The method comprising:
2. The repeated drying process includes: selectively depositing a protective layer on unexposed portions of the patterned layer by exposing the substrate to a first plasma, the unexposed portions of the patterned layer being covered by the overlying mask and not exposed to the EUV or shorter wavelength light; selectively etching exposed portions of the patterning layer by exposing the substrate to a second plasma, the exposed portions of the patterning layer not covered by the overlying mask and exposed to the EUV or shorter wavelength light; repeating the selectively depositing and selectively etching steps until the exposed portions of the patterning layer are completely removed; 2. The method of claim 1, comprising:
3. The method of claim 2 , wherein the first plasma comprises a hydrocarbon or fluorocarbon based precursor gas.
4. The method of claim 2 , wherein the second plasma comprises a hydrogen or halogen-containing precursor gas and an inert gas.
5. Each time the selective etching step is performed, the hydrogen or halogen-containing precursor gas converts the exposed surface portions of the patterned layer into a volatile material; The method of claim 4 , wherein ions of the inert gas bombard a surface of the substrate to remove the volatile material from the exposed portions.
6. The method of claim 5 , wherein each time the selectively depositing step is performed, a new protective layer is deposited on the unexposed portions of the patterned layer.
7. 1. A method of patterning a substrate, comprising the steps of: forming a patterning layer and one or more underlayers on the substrate, the patterning layer comprising a metal oxide photoresist; exposing portions of the patterning layer not covered by a mask on the patterning layer to extreme ultraviolet (EUV) light or shorter wavelength light; selectively depositing a protective layer on unexposed portions of the patterned layer by exposing the substrate to a first plasma, the unexposed portions of the patterned layer being covered by the mask and not exposed to the EUV or shorter wavelength light; selectively etching exposed portions of the patterned layer by exposing the substrate to a second plasma; The method comprising:
8. the patterning layer comprises a metal oxide material having clusters of metal oxide structures with chemically bonded organic ligands; 8. The method of claim 7, wherein exposing the portions of the patterning layer not covered by the mask to EUV light or shorter wavelength light dissociates the organic ligands from the metal oxide structures while the unexposed portions of the patterning layer remain unchanged.
9. Further, after the step of exposing the portions of the patterning layer not covered by the mask to EUV light or shorter wavelength light and before the step of selectively depositing a protective layer on the unexposed portions of the patterning layer, a baking process is performed, The method of claim 8 , wherein the organic ligand is released from the exposed portions of the patterned layer.
10. The method of claim 7 , wherein the first plasma comprises a hydrocarbon or fluorocarbon based precursor gas.
11. The first plasma is CH 4 , C 4 F 8 , C 4 F 6 , or C.H. 3 The method of claim 10 comprising F.
12. The method of claim 7 , wherein the second plasma comprises a hydrogen or halogen-containing precursor gas.
13. The second plasma is CH 4 , C.F. 4 , C.H.F. 3 , or BCl 3 The method of claim 12, comprising:
14. The method of claim 12 , wherein the second plasma further comprises an inert gas.
15. The method of claim 8 , wherein the second plasma further comprises argon (Ar).
16. 13. The method of claim 12, wherein the hydrogen or halogen containing precursor gas converts a surface of the exposed portions of the patterned layer into a volatile material, and inert gas ions bombard the surface of the exposed portions to remove the volatile material.
17. 8. The method of claim 7, wherein the steps of selectively depositing a protective layer on the unexposed portions of the patterning layer and selectively etching the exposed portions of the patterning layer are performed simultaneously in a plasma processing chamber using a same plasma precursor gas to generate the first plasma and the second plasma.
18. The method of claim 17 , wherein the first plasma and the second plasma each include a hydrocarbon precursor and an inert gas.
19. 8. The method of claim 7, wherein the steps of selectively depositing a protective layer on unexposed portions of the patterned layer and selectively etching exposed portions of the patterned layer are separated in a plasma processing chamber, and the first plasma and the second plasma are generated using different plasma precursor gases.
20. 20. The method of claim 19, wherein the first plasma comprises a hydrocarbon precursor and the second plasma comprises a halocarbon precursor and an inert gas.
21. The method of claim 7, further comprising repeating the selectively depositing and selectively etching steps until the exposed portion of the patterning layer is completely removed.
22. providing a patterning layer and one or more underlayers over a substrate, the patterning layer comprising a metal oxide photoresist; performing repeated dry processes to remove portions of the patterning layer defined by the lithographic process and develop a metal oxide photoresist pattern; The method comprising:
23. The repeated drying process includes: selectively depositing a protective layer on a first portion of the patterning layer by exposing the substrate to a first plasma; selectively etching a second portion of the patterning layer by exposing the substrate to a second plasma; repeating the selectively depositing and selectively etching steps until the second portion of the patterning layer is completely removed; and 23. The method of claim 22, comprising:
24. the first portion of the patterning layer being a non-exposed portion covered by an overlying mask during the lithography process; 24. The method of claim 23, wherein the second portion is an exposed portion of the patterning layer that is not covered by the overlying mask during the lithography step.
25. 25. The method of claim 24, wherein the first plasma comprises a hydrocarbon or fluorocarbon based precursor gas.
26. The first plasma is CH 4 , C 4 F 8 , C 4 F 6 , or C.H. 3 25. The method of claim 24, comprising F.
27. 25. The method of claim 24, wherein the second plasma comprises a hydrogen or halogen-containing precursor gas and an inert gas.
28. Each time the selective etching step is performed, the hydrogen or halogen-containing precursor gas converts the exposed surface portions of the patterned layer into a volatile material; 28. The method of claim 27, wherein ions of the inert gas bombard a surface of the substrate to remove the volatile material from the exposed portions.
29. The second plasma is CH 4 , C.F. 4 , C.H.F. 3 , or BCl 3 25. The method of claim 24, comprising:
30. 26. The method of claim 25, wherein each time the selectively depositing step is performed, a new protective layer is deposited on the unexposed portions of the patterned layer.
31. 23. The method of claim 22, wherein in the lithography process, the exposed portion is exposed to EUV or shorter wavelength light.
32. 25. The method of claim 24, wherein the steps of selectively depositing a protective layer on the unexposed portions of the patterned layer and selectively etching the exposed portions of the patterned layer are performed simultaneously in a plasma processing chamber using a same plasma precursor gas to generate the first plasma and the second plasma.
33. 25. The method of claim 24, wherein the steps of selectively depositing a protective layer on unexposed portions of the patterned layer and selectively etching exposed portions of the patterned layer are separated in a plasma processing chamber, and the first plasma and the second plasma are generated using different plasma precursor gases.
34. An apparatus for developing a resist, comprising: a process chamber having a substrate support; a process gas supply mechanism coupled to the process chamber; a plasma generating mechanism configured to generate plasma by utilizing one or more types of processing gas supplied by the processing gas supply mechanism; a control unit configured with instructions for processing a semiconductor substrate, the instructions including code for repeatedly performing a dry process to remove portions of a metal oxide patterning layer defined by a lithographic process and to develop a metal oxide photoresist pattern overlying one or more underlying layers on the substrate; An apparatus having the above configuration.
35. 35. The apparatus of claim 34, wherein the plasma generating mechanism is configured to generate a conductively coupled plasma (CCP), an inductively coupled plasma (ICP), a microwave plasma, a radial line slotted antenna microwave (RLSATM) plasma, an electron cyclotron resonance (ECR) plasma, or a combination thereof.
36. 35. The apparatus of claim 34, wherein the control unit is configured to control the repetitive dry process by controlling exposure of the substrate to a first plasma to selectively deposit a protective layer on a first portion of the patterning layer, and by controlling exposure of the substrate to a second plasma to selectively etch a second portion of the patterning layer, wherein the selective depositing and selective etching are repeated until the second portion of the patterning layer is completely removed.
37. exposing the portions of the patterning layer not covered by the patterned mask layer to EUV light or shorter wavelength light and prior to selectively depositing the protective layer on the unexposed portions of the patterning layer; 35. The apparatus of claim 34, wherein the method further comprises performing a bake process to release the organic ligands from the exposed portions of the patterned layer.