Powder Coating Method

JP2023551377A5Inactive Publication Date: 2024-11-01PARTIX
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023527337
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-29
Filing Date
2021-10-29
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for coating particulate materials using plasma often result in precursor decomposition and lack durability, with inefficiencies in precursor utilization and waste generation.

Method used

A cold atmospheric pressure plasma jet is used to excite precursors indirectly, forming a plasma coating stream that coats particulate matter, ensuring better adhesion and reducing precursor decomposition by using inert gases and controlled plasma conditions.

Benefits of technology

The method provides durable coatings with improved adhesion and reduced precursor waste, allowing for precise control over coating thickness and uniformity on various materials, including temperature-sensitive and fragile substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a plasma coating method for coating particulate matter, comprising the steps of: a) providing a low-temperature atmospheric pressure plasma jet from a plasma gas outside a reaction chamber, b) obtaining a plasma coating stream containing excited precursors by injecting precursors into the plasma jet, and subsequently injecting the plasma coating stream containing excited precursors into the reaction chamber, and c) exposing particulate matter to the plasma coating stream containing excited precursors, thereby obtaining a particulate matter comprising at least a partial coating. The present invention also relates to a coating reactor apparatus and system.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Technical Field The present invention relates to the field of plasma coating of particulate matter, such as powders and granules, by means of low-temperature atmospheric pressure plasma, in which precursors are intercalated which form a coating layer on the individual particles of the particulate matter. [Background technology]

[0002] Background of the Invention Particulate materials are used in many applications. In some applications, particulate materials are used in chemical reactions and are particularly useful due to their large contact surface. In other applications, particulate materials are used in mechanical applications, such as grinding, or particulate materials need to increase or decrease adhesion to other materials. In these and other applications, it can be beneficial to provide at least a partial coating on individual particles of the particles to enhance their functionality.

[0003] Several techniques exist for treating powders and other particulate materials to provide them with functionalized properties.

[0004] U.S. Patent No. 5,489,449 discloses particles of inorganic or metallic material coated on their surfaces with ultrafine particles of inorganic or metallic material. The coated particles are produced by introducing the particles of the inorganic or metallic material to be coated into a stream carrying ultrafine particles of the inorganic or metallic material formed in the gas phase, and contacting the particles with the ultrafine particles in a fluidized state. The coated particles are used to produce sintered bodies. It is believed that high-temperature vacuum plasma is used to coat the particles.

[0005] WO 2005039753 discloses a method for functionalizing a powder substrate. The method includes passing a gas through a means for forming excited and / or unstable gaseous species, typically an atmospheric pressure plasma, and treating the gas so that upon leaving the means, the gas contains substantially charge-free excited and / or unstable gaseous species. The gas containing substantially charge-free excited and / or unstable gaseous species is then used to treat the powder substrate and functionalizing precursor in a region downstream of the means for forming the excited and / or unstable gas, where neither the powder substrate nor the functionalizing precursor has undergone steps (i) and (ii), and the functionalizing precursor is introduced simultaneously with or after the introduction of the powder substrate. Preferably, the method is carried out in a fluidized bed. The method is believed to include striking a plasma in the gas, allowing the plasma to recombine into excited and / or unstable but electrically neutral gaseous species, and then exposing the powder to the unstable / excited gaseous species. Such treatment activates the powder and allows the functionalizing precursor to bind to the powder. While this method appears to work, it appears that improvements could be made with regard to ensuring that any coating applied to the powder is durable and maintains functionality over a long lifespan, as well as ensuring that any waste of precursor material is reduced as much as possible.

[0006] Summary of the Invention The present invention provides a plasma coating method for coating particulate matter, comprising the steps of: a) providing a low-temperature atmospheric pressure plasma jet from a plasma gas; b) injecting a precursor into the plasma jet, thereby obtaining a plasma coating stream containing the excited precursor; c) exposing particulate matter to the plasma coating stream containing the excited precursor; thereby obtaining particulate matter comprising an at least partial coating.

[0007] Here, coating of the particulate matter is performed within the reaction chamber. Further, the plasma jet in step a may be provided outside the reaction chamber. Step b may also include injecting a plasma coating flow containing excited precursors into the reaction chamber. The injection of the plasma coating flow containing excited precursors may be performed through a nozzle body of a nozzle, which extends through the reaction chamber to introduce the plasma coating flow containing precursors from outside the reaction chamber into the reaction chamber to coat the particulate matter in the reaction chamber.

[0008] This method allows for the application of layers to materials in the form of particles. The use of plasma gas, which is plasmatized and provided in the form of a plasma jet, allows for good flow control within the process. Inserting the actual precursor used to form the coating into the plasma allows for indirect excitation of the precursor by interacting with the plasma jet, rather than direct excitation, e.g., by a discharge. This reduces the decomposition of the precursor into smaller compounds during the plasmatization process. Once inserted into the plasma jet, the precursor is excited, e.g., ionized, by collisions with species in the plasma, typically making the precursor more reactive. The particulate material is then exposed to the excited precursor, which is better able to adhere to the particle's surface. This can also activate the particle's surface, increasing adhesion, if the species in the plasma are not all de-excited. Depending on certain conditions, particularly the duration of the particle's exposure to the plasma coating flow, the coating thus formed can partially or completely cover the particle's surface.

[0009] The present invention also provides a coating reactor apparatus for coating particulate matter, comprising: a reactor chamber for exposing particulate matter in the reactor chamber to a plasma coating stream; a plasma jet device, a plasma jet outlet for generating a plasma jet; A nozzle, a set of nozzle inlets for injecting plasma and / or precursors, said nozzle inlets being located outside the reaction chamber; at least one nozzle outlet for emitting a precursor-containing plasma, the nozzle outlet being disposed within the reaction chamber; a nozzle comprising: a nozzle body extending from a nozzle inlet to a nozzle outlet for directing a precursor-containing plasma coating flow from outside the reaction chamber into the reaction chamber; wherein the at least one nozzle inlet is in fluid communication with the plasma jet outlet; a precursor source in fluid communication with at least one nozzle inlet; The present invention relates to a coating reactor apparatus comprising:

[0010] The coating reactor apparatus of the present invention is particularly preferred for carrying out the method of the present invention. This apparatus comprises a plasma jet device, a nozzle, and a reactor chamber. The nozzle extends from the plasma jet outlet of the plasma jet device, located outside the reaction chamber, into the reaction chamber, allowing the plasma to be injected into the particulate matter within the reaction chamber. The precursor can be added to the plasma jet at the nozzle inlet, near the nozzle outlet, or anywhere in between. The nozzle includes a nozzle body that allows mixing of the precursor and / or plasma afterglow in the plasma jet before the precursor-containing plasma coating stream is injected into the reaction chamber with the particulate matter.

[0011] The present invention further relates to a system comprising a plurality of coating reactor apparatuses according to the present invention, wherein the reactor chambers of the plurality of reactor apparatuses are connected in series so that particulate matter can be coated sequentially in each of the plurality of reactor apparatuses, and a system comprising a plurality of coating reactor apparatuses according to the present invention configured in parallel and configured to simultaneously coat particulate matter.

[0012] Drawing Overview 1A, 1B, 1C and 2 show an apparatus according to the invention. [Brief explanation of the drawings]

[0013] [Figure 1A] 1 shows an overview of three embodiments of the device according to the invention. [Figure 1B] 1 shows an overview of three embodiments of the device according to the invention. [Figure 1C] 1 shows an overview of three embodiments of the device according to the invention. [Figure 2] 1A in the area where the plasma jet device (7), the nozzle (12) and the reactor chamber (2) are connected. [Figure 3] 1 illustrates a system and method according to the present invention. [Figure 4] 1 illustrates an alternative apparatus and method according to the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0014] The drawings are intended to illustrate the invention. Detailed Description of the Invention The invention is further explained below with reference to the drawings, in which: Within the context of this document, the following terms have the following meanings:

[0015] The term "coating" refers to a layer on the surface of a substrate that has different properties from the substrate, for example, a different structure, a different chemical composition, a different density, etc.

[0016] The term "plasma" refers to a state of matter in which at least a portion of the matter is ionized to include ions or ionized molecules and free electrons.

[0017] The term "plasma coating" refers to a coating applied onto a substrate using plasma.

[0018] The term "plasma jet" refers to the plasma stream emitted from a plasma device.

[0019] The term "plasma afterglow" refers to a region in the flow coming from the plasma jet that contains excited species such as ions, free electrons, and excited compounds and extends from the exit of the plasma device to a location in the flow where substantially all particles in the flow are stable.

[0020] The term "particulate matter" refers to matter that is in the form of particles, which may be macroscopic or microscopic particles.

[0021] The term "particulate" refers to particulate matter in which the particles are macroscopic in size, typically having a size of at least 100 microns.

[0022] The term "partial coating" refers to a coating that covers a portion of the surface of a substrate, but not the complete surface. The portions may be a set of connected portions or disconnected portions. In the present context of coatings of particulate matter, "partial coating" refers to coatings of individual particles that are partial.

[0023] The term "fluidized" refers to a fluid-like state that particulate matter can be brought into, typically by dispersing the particulate matter in a flowing fluid.

[0024] The term "precursor" refers to a molecular or atomic compound that participates in a reaction, thereby changing its structure, for example, by chemical bonding, dissociation, or a change in electronic configuration. As used herein, the term precursor refers to a compound that forms a coating layer on a substrate.

[0025] The term "reaction chamber" refers to a defined portion of the system of the present invention in which particulate matter can be coated, which essentially deals with the containment of particulate matter during, for example, the coating of particulate matter.

[0026] The present invention relates to a plasma coating method for coating particulate matter as described above and in the claims and as further described below.

[0027] The precursor-containing plasma can penetrate deeply into the batch of particulate material. However, it has been found that treating the particulate material while it is in a fluidized state results in a particularly good, uniform coating. Thus, in one embodiment, particulate material (3) is exposed to the plasma in a fluidized state, as shown in Figures 1A-1C, which can generate a particle stream (4) due to the fluidized state. Without wishing to be bound by theory, it is believed that the fluidized state allows for better mixing of the particles with the precursor-containing plasma and better coating results. Preferably, this method is carried out using a fluidized-bed reactor. Fluidized particulate material allows for better coating of individual particles in the batch. Furthermore, it also allows for more uniform coating of individual particles. Fluidized-bed reactors are particularly preferred because they can be adapted to allow for the injection of a plasma coating stream instead of or in addition to a gas stream to fluidize the particulate material.

[0028] In one embodiment, the particulates are fluidized by a fluidizing stream. Alternatively or additionally, the particulates are fluidized by a plasma coating stream.

[0029] In one embodiment, the particulate matter is indirectly exposed to the plasma. Indirect exposure of the particulate matter to the plasma means that the particulate matter does not enter the plasma generation region, i.e., the region where the plasma is excited (20), such as the region between the electrodes (21 a, 21 b) when an electric discharge is used to ignite the plasma. Indirect exposure ensures that the plasma jet device (7) is not contaminated by the particulate matter.

[0030] In one embodiment, the at least partial coating is a complete coating. A complete coating covers substantially the entire surface of each particle. In many applications, complete coating of the particles in the microparticles is preferred. The completeness of the coating of the particles in the microparticles can depend on many parameters, such as the flow rates of the plasma gas and precursor and the intensity of the plasma, as well as the treatment time. The optimal parameters also depend heavily on the nature and size of the microparticles. A person skilled in the art can ensure complete coating by trial and error, for example, by increasing the exposure time or increasing the precursor gas flow if testing indicates incomplete coating.

[0031] The present invention can be used to process particles of various sizes. In one embodiment, the particulate material comprises a size of at least 100 microns. Alternatively or additionally, the particulate material comprises a size of up to 100 microns. Preferably, the particulate material consists essentially of particles having a size that allows the particles to be fluidized.

[0032] In one embodiment, the particulate material is coated by sequentially performing steps a-c, whereby the particulate material is exposed multiple times to the plasma coating stream containing the excited precursor. The particulate material (29) is then preferably subsequently coated with different plasma coating streams (30a, 30b, 30c). This allows for higher throughput of the particulate material and also allows for better control of the coating process, since the plasma coating streams can be individually configured. Such a serial process is shown in Figures 3 and 4.

[0033] In one embodiment, the particulate material is coated by performing steps a-c in parallel, whereby the particulate material is distributed among portions exposed to separate plasma coating streams. Such a parallel setup allows for higher throughput.

[0034] In one embodiment, the particulate matter can be coated in a batch process, whereby a quantity of the particulate matter is inserted into the reactor chamber and exposed to the plasma coating stream for a batch processing period, after which the coated particulate matter is discharged from the reactor chamber. Alternatively, the particulate matter can be coated in a continuous process, whereby the particulate matter is provided to the reactor chamber at a first location (31) and the coated particulate matter is extracted from the reactor chamber at a second location different from the first location.

[0035] Two types of processes are shown in Figures 3 and 4. Figure 3 illustrates a serial process using multiple coating reactors. Here, particulate matter (29) can be provided to a first coating reactor (32a) (31), where it can be initially coated; the at least partially coated particulate matter can then be extracted and provided to a second coating reactor (32b) (31a), where it can be further coated; and the coated particulate matter can then be extracted again and provided to a third coating reactor (32c) (31b). The final product, i.e., the particulate matter including the coating layer, can be extracted from the reactor chamber of the third coating reactor (31c) for storage, transportation, or any further use. The process of Figure 3 can be operated continuously, i.e., by continuous provision and extraction of particulate material, or it can be operated in a batch process, where particulate material is provided to a coating reactor apparatus, then processed in said apparatus for a processing period, and then extracted and provided to the next coating reactor apparatus from which the previous batch of particulate material was first extracted.

[0036] Figure 4 shows a serial process using multiple plasma coating streams in the same reactor chamber. Here, the process is preferably continuous, and particulate matter is provided to the reactor chamber at an insertion rate (31) and extracted at an extraction rate (31d), which may typically be the same size as the insertion rate. By adjusting the insertion and extraction rates, the average exposure time of the particulate matter to the plasma coating streams can be controlled.

[0037] A "low temperature" or "cold" plasma is defined herein as a plasma whose temperature is low enough so as not to melt or damage the precursor and / or substrate exposed to said cold plasma. The temperature of the plasma may be preferably 150°C or less, more preferably 130°C or less, even more preferably 100°C or less, even more preferably 70°C or less, even more preferably 60°C or less, even more preferably 55°C or less, even more preferably 50°C or less, and even more preferably 45°C or less. The temperature of the plasma may preferably be as low as room temperature, i.e., the temperature surrounding the plasma. Depending on where the coating process is performed, room temperature may range from 10 to 40°C, preferably 15 to 30°C, for example 20 to 25°C. The temperature of the plasma is generally not lower than room temperature.

[0038] When depositing a temperature-sensitive coating, it may be important to maintain the plasma temperature constant at an optimum value. The optimum temperature can be selected depending on the type and / or pressure of the precursor or precursor mixture. Thus, in one embodiment, the plasma temperature is selected taking into account the type of precursor, precursor mixture, and / or plasma pressure.

[0039] The plasma of the present invention is an atmospheric pressure plasma having a pressure near ambient pressure. Such plasma is generated and discharged at a pressure between 400 and 1600 hPa, preferably between 450 and 1400 hPa, even more preferably between 500 and 1300 hPa, even more preferably between 600 and 1250 hPa, even more preferably between 700 and 1200 hPa, even more preferably between 800 and 1150 hPa, even more preferably between 900 and 1100 hPa, and most preferably near ambient pressure, which may typically be about 1013 hPa. The pressure of the plasma can play an important role in the quality of the deposited layer. Some plasma precursors are sensitive to plasma pressures that are too low and / or too high compared to atmospheric pressure, while other precursors provide better coatings at lower or higher plasma pressures. However, it should be noted that low-energy cold plasmas can typically be applied at low pressures, below 400 hPa down to vacuum, or at high pressures above 1600 hPa, and both types require a pressure vessel to maintain such low or high pressures. The use of plasmas with pressures in the currently preferred range near ambient pressure reduces the costs and difficulties associated with maintaining pressure differentials and pressure gradients.

[0040] In a preferred embodiment, the plasma is a dielectric barrier discharge plasma at atmospheric pressure. The functionality of the layer may depend on the plasma conditions, such as temperature and pressure, under which the layer is deposited. Thus, the temperature and / or atmospheric conditions may be selected taking into account the desired functionality of the coating layer.

[0041] In a preferred embodiment, the plasma gas (22) is ionized by the electrodes (21a, 21b), more preferably the plasma gas is ionized within 1 cm of the electrode surface. 2 Maximum 10 watts per cm, more preferably maximum 9 W / cm 2 , and even more preferably up to 8 W / cm 2 , and even more preferably up to 7.5 W / cm 2In many embodiments of the present invention, the power applied by the electrodes is a minimum of 1 W / cm 2 , preferably a minimum of 2 W / cm 2 , and more preferably a minimum of 2.5 W / cm 2 The power is most preferably 2.5 to 7.5 W / cm 2 It is between.

[0042] In a preferred embodiment, the plasma gas (22) comprises at least 99% by volume of an inert gas. Using an inert gas as the plasma gas essentially ensures that no reactions occur between the plasma gas and the equipment and the molecules of the plasma gas itself, even as temperatures increase. Indeed, the lack of reaction also appears to allow the plasma temperature to be kept low, e.g., below 50°C, preferably near room temperature. The low temperature of the plasma allows for the processing of substrates made from a wide range of materials. Furthermore, this allows for better control over the coating formed and its adhesive properties. While not wishing to be bound by theory, the inventors believe that the absence of reactive gases in the plasma gas ensures that no or very little chemical reaction with the plasma gas occurs at the substrate surface, thus ensuring better control over adhesive properties. Furthermore, when the plasma gas is nitrogen (N2) or is primarily composed of N2, the low power applied to the plasma in embodiments of the present invention has been found to result in little or no nitrogen being incorporated into the resulting coating. This is in stark contrast to using, for example, O2, NH3 or CH4 as the plasma gas, all of which are considered reactive gases and which are all likely to leave more traces in the coating than the plasma gas, thereby resulting in a loss of control over the adhesion properties.

[0043] In a preferred embodiment, the precursor is added to the plasma gas afterglow. This allows the plasma gas to flow over and between a plasma induction system, e.g., a set of electrodes. Downstream of the plasma induction system, there is a plasma gas afterglow containing a large number of ionized plasma gas molecules that have not had time to deionize. The precursor is preferably introduced into the plasma gas afterglow. As a result, the precursor does not need to be introduced between the electrodes used to ionize the plasma gas, for example, and therefore the electrodes can be kept clean for a long period of time because the precursor cannot form a layer on the electrodes.

[0044] In a preferred embodiment, the plasma gas comprises at least 99% by volume of inert gas, i.e., 1% by volume (vol%) or less of the plasma gas is reactive gas. More preferably, at least 99.5% by volume, even more preferably at least 99.8% by volume, even more preferably at least 99.9% by volume, even more preferably at least 99.95% by volume, and even more preferably at least 99.99% by volume of the plasma gas is inert gas. This means that the plasma gas preferably comprises 1% by volume or less of O, more preferably at most 0.5% by volume, even more preferably at most 0.2% by volume, even more preferably at most 0.1% by volume, even more preferably at most 0.05% by volume, and even more preferably at most 0.01% by volume of O. In atmospheric plasma processes of the present invention, this can be achieved, for example, by using an overpressure relative to ambient pressure, e.g., the plasma gas is delivered at a pressure of at least 1013 mbar, preferably at least 1020 mbar, more preferably at least 1030 mbar, even more preferably at least 1040 mbar, and even more preferably at least 1050 mbar. Such a slight overpressure makes it possible to create oxygen-deficient or even oxygen-free regions in the plasma afterglow.

[0045] In one embodiment, the plasma gas comprises N2, preferably the plasma gas comprises at least 99% by volume of N2. Alternatively or additionally, the plasma gas comprises a noble gas, preferably He, Ne and / or Ar.

[0046] In a preferred embodiment, the particulate matter is exposed to the plasma in an oxygen-deficient region, whereby preferably the oxygen-deficient region contains up to 1% O2 by volume.

[0047] In one embodiment of the present invention, the plasma gas flow is from 1 to 1500 standard liters per minute ("slpm" or "slm"), more preferably from 50 to 1500 slpm. 1 "slpm" or 1 "slm" is a liter of gas at atmospheric pressure and room temperature. More preferably, the plasma gas flow is from 80 slpm to 1000 slpm.

[0048] In an embodiment of the present invention, the plasma coating has a thickness of between 5 and 600 nm, preferably between 5 and 500 nm, more preferably between 10 and 500 nm, even more preferably between 10 and 300 nm, even more preferably between 10 and 200 nm, even more preferably between 10 and 80 nm, such as 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, or any value therebetween, most preferably about 20 nm. The plasma coating thickness can be well controlled by controlling the exposure time of the particulates to the plasma coating stream (5).

[0049] The methods of the present invention are particularly useful for processing particulate matter that may be difficult to process, for example, due to their inert nature or extreme fragility (e.g., natural materials, or biodegradable / water-soluble materials). Preferably, the particulate material comprises any one or any combination of the following materials:

[0050] -polymer: PE, PP, PVC, PS, EPDM, polyolefin products, Engineering thermoplastics such as PET, PBT, PMMA, PC, PES, polyamide, aramid, acrylonitrile styrene acrylate (ASA), acrylonitrile butadiene styrene (ABS), Fluorinated polymers such as PTFE, PVDF, and fluorinated ethylene propylene (FEP), Biodegradable polymers such as PLA and PCL, Cross-linked polymers such as epoxyamines, polyurethanes, and silicones Carbon fiber Water-soluble polymers such as PEG, polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyacrylamide, divinyl ether-maleic anhydride (DIVEMA), polyoxazoline, polyphosphate, polyphosphazene, etc. -Natural materials such as rayon, viscose, polysaccharides, chitosan, collagen, proteins, xanthan gum, pectin, dextran, carrageenan, guar gum, hyaluronic acid (HA), leather, and cellulosic materials (paper). - Metals such as gold, silver, copper, iron, brass, lead, iron, tin, stainless steel, aluminum, zinc, titanium, including all possible alloys and oxides, - Inorganic materials such as glass, silicon wafers, metal oxides (e.g., Al2O3, ZnO), carbides (e.g., SiC, titanium carbide), and nitrides (e.g., Si3N4) In a preferred embodiment, the particulate material comprises fibers, preferably consisting essentially of fibers. The fibers preferably have a length of 1 mm to 100 mm, more preferably 5 mm to 90 mm, even more preferably 20 mm to 70 mm, and most preferably about 50 mm. Also, preferably, the fibers have a maximum diameter of at most 2000 μm, preferably at most 1500 μm, even more preferably at most 1000 μm, even more preferably at most 800 μm, for example, 700, 600, 500, 400, 300, 200, 100 μm, or any value therebetween. Preferably, the fibers comprise plastic fibers, polymer fibers, glass fibers, carbon fibers, or any combination thereof. Preferably, when polymer fibers are used as particulate material in the present invention, these polymer fibers comprise polyethylene, polyethylene terephthalate, or a combination thereof. Preferably, the fibers have a density of 1 to 100 grams per liter (g / l), preferably 2 to 80 g / l, more preferably 3 to 60 g / l, even more preferably 4 to 40 g / l, and most preferably about 10 g / l.

[0051] In preferred embodiments, the particulate matter may comprise any suitable material, such as metals, metal oxides, silica and silicates, organic powder substrates including rice husk ash, carbon, polymers, dyes, fragrances, flavorings, pharmaceutical powder substrates such as penicillin and antibiotics, and biologically active compounds, such as proteins, including enzymes and other protein-based materials. The powder substrate may also contain biochemical compounds such as amino acids and / or their derivatives, grafted or covalently bonded biochemical compounds such as proteins, enzymes, and DNA, silicone resins, mineral fillers such as carbon black, clay, CaCO3, talc, silica, mica conductive fillers, TiO2 nanoparticles, metal oxides such as TiO2, ZrO2, Fe2O3Al2O3SiO2, BO3, Li2O, Na2O, PbO, ZnO, or CaO, Pb3O4, and CuO, as well as mixed oxides, graphite, phosphorus particles, pigments, semi-metallic oxides, mixed oxides, organometallic oxides, organometalloid oxides, organic mixed oxide resins and / or organic resins, sodium carbonate, potassium nitrate, silicon metal particles, silicone rubber crumb, organic rubber crumb such as EPDM, polypropylene, etc. Rice husk ash is a biogenic amorphous silica containing 93 to 97% crystalline silica, generally containing less than 5% amorphous carbon and less than 1% of various other silicas.

[0052] In one embodiment, the precursor is a polymerizable compound, which allows the coating to be a polymer coating. If the desired coating is a polymer coating, such a coating can be obtained by the present method, in which the precursor is a polymerizable compound, which allows the compound to be polymerized directly on the substrate, i.e., the particles. In one embodiment, the coating is a polymer coating.

[0053] In one embodiment, the coating is a graft coating. The precursors are preferably organic materials including carboxylates, methacrylates, acrylates, styrene, methacrylonitrile, alkenes and dienes, such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate and other alkyl methacrylates, and the corresponding acrylates, including organofunctional methacrylates and acrylates, including glycidyl methacrylate, trimethoxysilylpropyl methacrylate, allyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, dialkylaminoalkyl methacrylates and fluoroalkyl(meth)acrylates, methacrylic acid, acrylic acid, fumaric acid and esters, itaconic acid (and esters), maleic anhydride, styrene, α-methylstyrene, halogens, The polymerizable monomers may include fluorinated alkenes, for example, vinyl halides such as vinyl chloride and vinyl fluoride, and fluorinated alkenes, for example, perfluoroalkenes, acrylonitrile, methacrylonitrile, ethylene, propylene, allylamine, vinylidene halides, butadiene, acrylamides, for example, N-isopropylacrylamide, methacrylamide, epoxy compounds, for example, glycidoxypropyltrimethoxysilane, glycidol, styrene oxide, butadiene monoxide, ethylene glycol diglycidyl ether, glycidyl methacrylate, bisphenol A diglycidyl ether (and its oligomers), vinylcyclohexene oxide, conductive polymers, for example, pyrrole and thiophene and their derivatives, and phosphorus-containing compounds, for example, dimethylallylphosphonate. The organic precursor may also comprise an organic compound containing any one of the following groups: alkenyl, aryl, H, -OH, amino group, aldehyde group, halogenated alkyl group, alkyne group, amide group, carbamate group, urethane group, organic salt, carboxylic acid group and derivatives thereof, such as acid anhydride group, organic groups containing boron atoms, phosphorus and sulfur containing groups, such as mercapto and sulfide groups, and grafted or covalently bound biochemical groups, such as amino acids and / or derivatives thereof, grafted or covalently bound biochemical species, such as proteins, enzymes and DNA.

[0054] In a preferred embodiment, the excited precursor is ionized. In one embodiment of the above method, the precursor is injected into the plasma jet as a gas, liquid, or solid, preferably as a gas or as a liquid in the form of an aerosol, most preferably as a liquid in the form of an aerosol. Preferably, an aerosol is used and the temperature of the plasma is 150°C or less, more preferably 130°C or less, even more preferably 100°C or less, even more preferably 70°C or less, even more preferably 60°C or less, even more preferably 55°C or less, even more preferably 50°C or less, even more preferably 45°C or less. The temperature of the plasma may preferably be as low as room temperature, i.e., the temperature surrounding the plasma.

[0055] In one embodiment, the particulates are fluidized by a fluidizing flow. This allows the particulates to flow together with the particulate flow. Such fluidization is preferably achieved using a fluidized bed reactor. In a preferred embodiment, the plasma coating flow is directed essentially along the particulate flow when the particulates are exposed to the plasma coating flow. In an alternative embodiment, the plasma coating flow is directed essentially opposite to the particulate flow when the particulates are exposed to the plasma coating flow. In yet another embodiment, the plasma coating flow is directed essentially perpendicular to the particulate flow when the particulates are exposed to the plasma coating flow. In one embodiment, the plasma coating flow is directed in a direction between the direction of the particulate flow and a direction perpendicular to the particulate flow, or between a direction opposite to the particulate flow and a direction perpendicular to the particulate flow. Essentially, the direction in which the plasma coating flow is directed relative to the particulate flow is preferably selected to optimize the particulate particle coating process.

[0056] In one embodiment, the microparticles rotate during the step of exposing the particulate material to the plasma coating flow. This is particularly preferred when the particulate material is exposed to the plasma coating flow. Rotating the microparticles during the exposure step can result in a more uniform coating of the particles in the microparticles. Rotation of the microparticles can be achieved, for example, by rotating the bottom of the reaction chamber and / or by another rotating component within the reaction chamber. Furthermore, rotation of the particles can also allow the shape and / or size of the particles in the microparticles to be changed, for example, by grinding, agglomeration, spheronization, etc.

[0057] The particulates can be rotated without being fluidized. In this case, rotation can be achieved by rotating the bottom or any other receiver in which the particulate material is placed. However, in another embodiment, which may be more preferred, the particulates are rotated while in a fluidized state to obtain a uniform coating throughout the particulates. Rotation of the particulates in a fluidized state can be achieved by inducing a vortex, which can be achieved, for example, by a rotating bottom in the reaction chamber.

[0058] The present invention also relates to a coating reactor apparatus as described above and in the claims and as further described below.

[0059] A coating reactor apparatus (1) for coating particulate matter (3) includes a plasma jet device (7) having a plasma jet outlet (11) and a nozzle (12) for generating a plasma jet. The coating reactor apparatus also includes a precursor source (13) and a reactor chamber (2). The nozzle (12) includes a set of nozzle inlets (14) for injecting a plasma (15) and / or a precursor (16), i.e., the plasma (15) and / or the precursor (16) are injected into the nozzle (12) through the set of nozzle inlets. At least one nozzle inlet (14) is fluidly connected to the plasma jet outlet (11). The nozzle also includes at least one nozzle outlet (17) for discharging a precursor-containing plasma (5). The nozzle outlet (17) is positioned within the reactor chamber (2) so that the precursor-containing plasma, which is a plasma coating stream, is discharged from the nozzle into the reactor chamber. The nozzle comprises a nozzle body (18) extending from a nozzle inlet (14) to a nozzle outlet (17) for directing a precursor-containing plasma coating stream (5) into a reaction chamber. Preferably, the nozzle body comprises a cylindrical shape. Preferably, the nozzle comprises one nozzle inlet (14) in fluid communication with both the plasma jet outlet (11) and the precursor-providing source (13).

[0060] It should be noted that the nozzle inlet (14) is located outside the reaction chamber (2) and the nozzle outlet (17) is located inside the reaction chamber (2), which further confines the particulate matter to an essentially closed volume during coating.

[0061] A precursor source (13) is in fluid communication with at least one nozzle inlet (14) to allow insertion of a precursor (16) into the nozzle body (18). The reactor chamber is used to expose particulate matter in a reaction chamber to a plasma coating stream in a controlled environment.

[0062] Preferably, the reactor chamber (2) of the coating reactor apparatus is the reactor chamber (2) of a fluidized bed reactor (8), i.e., preferably, the coating reactor apparatus comprises a fluidized bed reactor (8), the reactor chamber of which is used as the reactor chamber of the apparatus of the present invention.

[0063] A fluidized bed reactor (FBR) (8) is a type of reactor apparatus that can be used to carry out a variety of multiphase chemical reactions. In this type of reactor, a fluid (gas or liquid) is passed through a solid particulate material at a velocity sufficient to suspend the solids and cause them to behave as if they were a fluid. The FBR comprises a reactor chamber (2) and preferably a porous plate (9), typically located at the bottom of the reactor chamber. This porous plate is commonly referred to as a "distributor." The distributor (9) prevents particulate particles from exiting the chamber but allows a fluid stream (10) to pass through to fluidize the particles.

[0064] In a preferred embodiment, the distributor comprises a hole, preferably a central hole, through which the nozzle body (18) passes such that the nozzle outlet is within the reactor chamber and one set of nozzle inlets is located outside the reactor chamber.

[0065] The inventors have already discussed a method in which the fine particles are fluidized by a fluidizing flow. Such fluidization is preferably achieved using a fluidized bed reactor. In some cases, the plasma coating flow is preferably guided along the fine particle flow. In the embodiments of FIGS. 1A and 2, the nozzle body (18) passes through a hole in the bottom of the reaction chamber. This allows the plasma coating flow (5) to be guided essentially along the fine particle flow when the fine particles are exposed to the plasma coating flow. In another embodiment, as shown in FIG. 1B, the nozzle body passes through a side wall or top wall of the reactor chamber. Preferably, this allows the nozzle outlet to be positioned so that the plasma coating flow (5) is guided essentially opposite to the fine particle flow when the fine particles are exposed to the plasma coating flow. In yet another embodiment, as shown in FIG. 1C, the nozzle body passes through a side wall of the reactor chamber, thereby preferably allowing the nozzle outlet to be positioned so that the plasma coating flow (5) is guided essentially perpendicular to the fine particle flow when the fine particles are exposed to the plasma coating flow. This can be achieved by positioning a nozzle body through the sidewall of the FBR and positioning the nozzle outlet so that the plasma coating flow is directed horizontally and tangentially to the sidewall and / or particulate flow, as shown in Figure 1C. In one embodiment, the location of the nozzle outlet and / or nozzle body is selected to optimize the particulate particle coating process. Additionally or alternatively, the orientation of the nozzle outlet and / or nozzle body is selected to optimize the particulate particle coating process.

[0066] In a preferred embodiment, the nozzles are positioned so that the plasma coating flow is directed tangentially to the sidewall, as shown in Figure 1C. This arrangement allows for a significant increase in throughput, speed, etc., compared to vertical positioning, i.e., when the nozzles are located at the top or bottom of the reaction chamber. This is because more nozzles can be placed in a tangential position compared to vertical positioning. This allows for uniform processing of particles in the microparticles by placing the nozzles at regular intervals around the sidewall.

[0067] Embodiments in which the nozzle and / or nozzle body are positioned such that the plasma coating flow is directed along or against the particulate flow may be preferred in cases where the plasma coating flow may seriously interfere with and / or alter the particulate flow, e.g., interference that may interfere with particulate fluidization or normal operation of the FBR.

[0068] In a preferred embodiment, the reactor chamber comprises a rotating bottom, for example to produce spherical particles to be coated. This embodiment is preferably combined with a nozzle and / or nozzle body that is oriented such that when the particles are exposed to the plasma coating flow, the plasma coating flow (5) is directed essentially perpendicular to the particle flow, preferably tangential to the side wall of the reaction chamber and / or horizontally to the particle flow.

[0069] In one embodiment, each of the nozzle bodies or sets of nozzle bodies passes through the bottom of the reactor chamber and is positioned such that the plasma coating flow is directed tangentially to the bottom of the reactor.

[0070] In a preferred embodiment, the nozzle is 3D printed. This allows the use of low-temperature plasma to enable the use of a printable nozzle. Preferably, a set of nozzle inlets, at least one nozzle outlet, and nozzle body are configured to optimize the plasma coating flow. 3D printing of the nozzle allows for easy modification of the nozzle to test other configurations, but also allows for easy replacement of the nozzle in the event of maintenance or repair.

[0071] In one embodiment, the reactor chamber includes a hollow body, a flow guider (23) including a flow inlet (24) and a flow outlet (25), whereby the nozzle outlet (17) is preferably disposed within the hollow body. The flow guider (23) serves to guide the fluidized particulate material into the plasma coating stream. The inventors have recognized that when the reactor chamber is relatively small, particles of the fluidized particulate material come into contact with the plasma coating stream. However, the inventors have also recognized that when the reactor chamber becomes larger, for example, to scale up the process, this can help guide the flow of the fluidized particulate material, particularly guiding the flow of the fluidized particulate material into contact with the plasma coating stream. Preferably, the flow guider is a hollow tube that is open at its longitudinal ends and can be disposed partially around the nozzle outlet and partially around the nozzle body.

[0072] In one embodiment, the coating reactor apparatus includes multiple plasma jet devices (27), each having a plasma jet outlet and a nozzle with a nozzle inlet and at least one nozzle outlet (28), with each nozzle outlet (28) of the multiple plasma jet devices positioned within the reaction chamber. Such a configuration allows for the generation of multiple separate plasma coating streams within the reactor chamber, thereby enabling better coating. The use of different plasma coating streams within the same reactor chamber allows for the sequential exposure of particulate matter to multiple plasma coating streams, thus enabling steps a through c of the method of the present invention to be performed sequentially. This type of apparatus is also preferred when particulate matter is to be coated in a continuous process.

[0073] The present invention also relates to a system comprising a plurality of coating reactor apparatuses, such a system being described above and in the claims and further explained below.

[0074] In one embodiment, the system includes multiple coating reactors, whereby the reactor chambers of the multiple reactors are connected in series to allow for sequential coating of particulate matter in each of the multiple reactors. Each reactor chamber has one or more chamber inlets and one or more chamber outlets, whereby the chamber outlet of a first reactor chamber is or can be fluidly connected to the chamber inlet of a second reactor chamber. Using different plasma coating streams in the multiple reactor chambers allows for sequential exposure of the particulate matter to multiple plasma coating streams, thereby enabling steps a-c of the method of the present invention to be performed sequentially. This type of system is also preferred when the particulate matter is coated in a continuous process, whereby coating particulate matter extracted from the outlet of a first reactor chamber is provided to a second reactor chamber via its inlet.

[0075] In one embodiment, the system comprises multiple coating reactors arranged in parallel, whereby the reactors are configured to simultaneously coat particulate material. This system thus allows steps a-c of the method of the present invention to be performed in parallel. This type of system is also preferred when particulate material is coated in a batch process, whereby at least one of the coating reactors can be unloaded from coated particulate material and / or loaded with uncoated or partially coated particulate material while another coating reactor is performing steps a-c of the method of the present invention.

[0076] Example Test beads were used in a method according to the invention using an apparatus according to the invention.

[0077] In the first two experiments, the test beads were sugar beads with an average diameter of approximately 1 mm. The amount of beads was selected to have optimal fluidization and was approximately 400 to 600 g. The plasma jet device was a PlasmaSpot® device manufactured by Molecular Plasma Group. A fluidized bed reactor was used to process the particles.

[0078] In the first experiment, sugar beads were treated using 6 g of 2-hydroxyethyl methacrylate (HEMA, CAS 868-77-9) and 1 wt. % rhodamine as a precursor. The plasma jet apparatus was operated at approximately 1 atmosphere pressure, a flow rate of 122 standard liters per minute (slm), and a plasma generating power of 450 W, using nitrogen gas as the plasma gas. The precursor flow was 1.6 slm, and the diluent flow was 10.0 slm. Subsequently, 600 grams of sugar beads with an average diameter of approximately 1 mm were treated twice for 600 seconds (total 1200 seconds). The effect of the treatment was clearly visible under a UV lamp. An additional 600-second treatment improved visual inspection of the coating even without a UV lamp. The treatment was very uniform. All treated beads were coated with a uniform color, i.e., a slight pink color due to the grafted rhodamine 6G, as could be visually inspected.

[0079] In the second experiment, sugar beads were treated using 1H,1H,2H,2H-perfluorodecyl acrylate (PFDA, CAS 27905-45-9) as a precursor. The plasma jet apparatus was operated at approximately 1 atmosphere pressure, a flow rate of 120 standard liters per minute (slm), and a plasma generating power of 450 W, using nitrogen gas as the plasma gas. The precursor flow was 1.6 slm, and the diluent flow was 10.0 slm. 460 grams of sugar beads with an average diameter of approximately 1 mm were treated for 600 seconds. The treated beads exhibited an electrostatic effect, and tests revealed that while untreated beads were highly wettable, the treated beads literally floated on the surface of a water film. The treated beads were analyzed using X-ray photoelectron spectroscopy (XPS), which quantitatively confirmed the grafting of fluorinated moieties.

[0080] In a third experiment, polyethylene powder with an average size of approximately 150 μm was treated using N-(3-trimethoxysilylpropyl)diethylenetriamine (TRIAP, CAS 35141-30-1) as the amine-functional precursor. The plasma jet apparatus was operated at approximately 1 atmosphere pressure, a flow rate of 80 standard liters per minute (slm), and a plasma generating power of 450 W, using nitrogen gas as the plasma gas. The precursor flow was 1.2 slm, and the diluent flow was 20 slm. The fluidized bed was maintained at a volume of 0.38 m. 3 The plasma-coated powders were operated with a nitrogen flow of 1 / min and a distributor plate with a 50 μm filter. The powders plasma-coated using the method according to the present invention exhibited grafting of TRIAP onto the powder that remained stable for at least 5 days. This was demonstrated using a dye test that allows for quantification of amino groups, as described below.

[0081] -C Geismann, M Ulbricht, Macromol Chem and Phys2005, 206, 268, and -A Papra, HG Hicke, D Paul, J Appl Polym Sci 1999, 74, 1669 The staining test procedure is summarized as follows:

[0082] 1. Binding: The sample is shaken overnight in a solution of 500 μmol / L Acid Orange II (CAS 633-96-5) in water (pH 3, HCl) at room temperature.

[0083] 2. Washing: Wash / rinse the sample with water (pH 3). Repeat three times. 3. Elution solution: Immerse the sample in 10 mL of water (pH 12, NaOH). Shake for 15 minutes.

[0084] 4. Record the UV / Vis absorbance of the solution at 479 nm. 5. Establish a calibration curve for each dye in the solvent used for elution.

[0085] Three samples were tested using the stain test. -First untreated sample - A second sample treated with plasma without precursor. A third sample treated according to the method of the present invention using TRIAP as a precursor. The staining results were as follows:

[0086] #1: Untreated PE powder does not contain primary amines and therefore does not bind acid orange to the particles. The solution remains colored (i.e., due to the presence of acid orange in the solution) and the powder can be seen floating on top of the solution.

[0087] #2: The plasma-treated powder does not contain primary amines and therefore does not bind acid orange to the particles. The solution remains colored (i.e., due to the presence of acid orange in the solution). However, the particles behave more hydrophilic (remain dispersed longer in aqueous solution) due to the increased surface energy of the N2 plasma treatment.

[0088] #3: The plasma-coated powder (with TRIAP precursor) has a high surface content of primary amines, which bind all of the acid orange that was initially present in the solution. The particles remain visually orange, but the acid solution becomes completely clear.

Claims

1. 1. A plasma coating method for coating particulate matter in a reaction chamber, comprising: a) providing a low-temperature atmospheric pressure plasma jet from a plasma gas outside the reaction chamber; b) obtaining a plasma coating flow containing an excited precursor by injecting a precursor into the plasma jet, and subsequently injecting the plasma coating flow containing the excited precursor into the reaction chamber; c) exposing particulate matter in the reaction chamber to the plasma coating stream containing the excited precursor; Including, This results in a particulate matter having an at least partial coating thereon, in a plasma coating method.

2. 2. The plasma coating method of claim 1, wherein the particulate matter is exposed to the plasma in a fluidized state, preferably carried out using a fluidized bed reactor.

3. The plasma coating method of claim 1 or 2, wherein the particulate matter is indirectly exposed to the plasma.

4. 4. The plasma coating method according to claim 1, wherein the at least partial coating is a complete coating.

5. The plasma gas comprises an inert gas, preferably the plasma gas consists of at least 99% by volume of an inert gas, preferably the plasma gas is N 2 and preferably the plasma gas comprises at least 99% by volume N 2 5. A plasma coating method according to claim 1, wherein the plasma gas comprises a noble gas, preferably the plasma gas comprises He, Ne and / or Ar.

6. 6. A plasma coating method according to claim 1, wherein the particulate matter is rotated during step c.

7. The particulate matter is exposed to the plasma in an oxygen deficient region, preferably the oxygen deficient region has up to 1% by volume O 2 7. The plasma coating method according to claim 1, comprising:

8. The plasma coating method according to claim 1 , wherein the precursor is a polymerizable compound.

9. 9. A plasma coating method according to any one of claims 1 to 8, wherein the particulate matter is coated by performing steps a to c sequentially, whereby the particulate matter is exposed multiple times to a plasma coating flow containing the excited precursor.

10. 10. A plasma coating method according to any one of claims 1 to 9, wherein the particulate material is coated by carrying out steps a to c in parallel, whereby the particulate material is distributed in portions exposed to separate plasma coating streams.

11. 11. A plasma coating method according to any one of claims 1 to 10, wherein the precursor is injected into the plasma jet as an aerosol.

12. 12. The plasma coating method according to claim 1, wherein the particulate matter comprises fibers.

13. A coating reactor apparatus for coating particulate matter configured to carry out the method according to any one of claims 1 to 12, comprising: - a reactor chamber for exposing particulate matter in said reaction chamber to a plasma coating flow; - a plasma jet device, - a plasma jet outlet for generating a plasma jet; A nozzle, a set of nozzle inlets for injecting plasma and / or precursors, said nozzle inlets being located outside said reaction chamber; at least one nozzle outlet for emitting a precursor-containing plasma, said nozzle outlet being disposed within said reaction chamber; a nozzle comprising: a nozzle body extending from the nozzle inlet to the nozzle outlet for directing a precursor-containing plasma coating flow from outside the reaction chamber into the reaction chamber; wherein at least one nozzle inlet is in fluid communication with the plasma jet outlet; a precursor source in fluid communication with at least one nozzle inlet; A coating reactor apparatus comprising:

14. 14. The coating reactor apparatus of claim 13, wherein the coating reactor apparatus comprises a plurality of plasma jet devices, each comprising a plasma jet outlet and a nozzle comprising a nozzle inlet and at least one nozzle outlet, each nozzle outlet of the plurality of plasma jet devices being disposed within the reaction chamber.

15. 15. The coating reactor apparatus according to claim 13 or 14, comprising a fluidized bed reactor (FBR) (8) comprising the reactor chamber (2) and a distributor (9) arranged at the bottom of the reactor chamber, the distributor comprising holes, the nozzle body (18) passing through the holes such that the nozzle outlets are within the reactor chamber and the set of nozzle inlets are located outside the reactor chamber.

16. 16. A system comprising a plurality of coating reactor apparatuses as described in any of claims 13 or 15, wherein the reactor chambers of the plurality of reactor apparatuses are connected in series so as to enable continuous coating of particulate matter in each of the plurality of reactor apparatuses.

17. 16. A system comprising a plurality of coating reactor apparatus according to any of claims 13 to 15, arranged in parallel whereby the coating reactor apparatus are configured to coat particulate matter simultaneously.