Cellulose particles and dispersion of cellulose particles
Patent Information
- Application Number
- JP2024048400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-11-29
AI Technical Summary
Existing cellulose particles and dispersions have poor dispersibility in oil-based media and tend to settle easily, limiting their use in applications beyond aqueous mediums.
Cellulose particles are formed by agglomerating fine fibrous cellulose with specific fiber diameters and lengths, achieving a consolidated bulk density within a certain range, which enhances their dispersibility and stability in oil-based media.
The resulting cellulose particles exhibit excellent dispersibility and stability in oil-based liquids, reducing settling and maintaining a stable dispersion.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to cellulose particles and a cellulose particle dispersion. [Background technology]
[0002] Fine fibrous cellulose, obtained by micronizing cellulose fibers, the basic skeleton of plants, has been the subject of research into applications in various fields in recent years due to growing environmental awareness such as the move away from plastics. In addition to utilizing the functions of the material itself, it is expected to be used in applied fields such as plastic materials, cosmetics, clothing, and construction.
[0003] A technology that focuses on the dispersibility of fine fibrous cellulose is disclosed in Patent Document 1. Patent Document 1 provides a powdered nanofiber that can improve dispersibility in a matrix component such as a resin as a problem to be solved by the invention, and the solution is a powdered nanofiber blended with a dispersant, in which the dispersant is a P-OH group, a -COOH group, a -SO 3 The present invention discloses a technique in which at least one selected from the group consisting of H groups and / or their metal bases, and imidazoline groups is bonded to the aryl group.
[0004] Also, Patent Document 2, which discloses a related technique, aims to provide cellulose particles that are small in diameter, have an emphasis on softness and feel, and are capable of reducing irritation to the skin, and the means for solving the problem is cellulose particles that have an average particle size D50 of 1 μm to 50 μm, a bulk density of 0.30 g / mL or less, a specific volume of 3.0 mL / g or more, and a linseed oil absorption of 100 mL / 100 g or more. These cellulose particles are made by preparing a cellulose sponge from viscose made from dissolving natural pulp, the main component of which is cellulose, to which reinforcing fibers have been added, and then pulverizing the cellulose sponge.
[0005] Patent Document 3 discloses a technique relating to a powder for use in cosmetics, in which porous cellulose particles are resistant to disintegration while having increased sphericity. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-210596 A [Patent Document 2] JP 2019-206662 A [Patent Document 3] JP 2020-50840 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the technology disclosed in Patent Document 1 aims to improve the dispersibility of powdered nanofibers in a solid matrix component such as a resin, and does not disclose any knowledge regarding whether powdered nanofibers can be mixed well in a liquid when the matrix component is a liquid.
[0008] The technology of Patent Document 2 assumes the use of cellulose particles as an additive in makeup products, but does not disclose any information on the matrix component to be used, and therefore does not disclose any knowledge on dispersibility in liquids. In addition, when used as an additive in makeup products, the bulk density is also thought to affect dispersibility, but there is room for further study on this point.
[0009] Like Patent Document 2, Patent Document 3 proposes improving the feel and texture when cellulose particles are mixed into cosmetics, but it is not a powder that can improve the settling properties or dispersibility of the particles when dispersed.
[0010] Furthermore, in conventional techniques, fine fibrous cellulose is often used in a state dispersed in water, and therefore its applications have been limited solely to aqueous media.
[0011] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide cellulose particles and a cellulose particle dispersion that have good dispersibility in an oil-based medium and are less likely to settle. [Means for solving the problem]
[0012] The above problem is solved by the following aspects. The cellulose fiber is formed by agglomerating fine fibrous cellulose having an average fiber diameter of 1 to 1000 nm and an average fiber length of 0.01 to 1000 μm, and has a packed bulk density of 0.1 to 200 mg / cm 3 The present invention also provides a cellulose particle dispersion in which the cellulose particles are dispersed in an oil component.
[0013] The cellulose particles of the above embodiment are formed by agglomeration of fine fibrous cellulose having an average fiber diameter and average fiber length in the above range, and it is presumed that each fine fibrous cellulose having a relatively large aspect ratio is easily entangled with each other and difficult to disentangle. If the packed bulk density is in the above range, the cellulose particles are light in weight relative to their volume, and therefore are unlikely to settle under their own weight even when left in a dispersed state in an oil-based dispersion medium, resulting in excellent dispersion stability. Effect of the Invention
[0014] According to the present invention, cellulose particles and a cellulose particle dispersion liquid are obtained which are less susceptible to aggregation of particles, are lightweight, and have good dispersibility in oil-based liquids. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is an explanatory diagram of a spray-freezing granulation device. [Diagram 2] 1 is an SEM image of cellulose particles. [Diagram 3] 1 is an SEM image of cellulose particles. [Figure 4] 1 is an SEM image of cellulose particles. [Diagram 5] 1 is an SEM image of cellulose particles. [Figure 6] FIG. 2 is a cross-sectional view of FIG. [Figure 7] FIG. 1 shows the results of an emulsification test. [Figure 8] FIG. 1 shows the results of dispersibility test 1. [Figure 9] FIG. 1 shows the results of dispersibility test 2. [Figure 10] 1 is an SEM image of particles of Comparative Example 1. [Figure 11] FIG. 13 is a side view of a dryer according to another embodiment. [Figure 12] FIG. 12 is a view of the dryer in FIG. 11 as viewed in the Y direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] An embodiment of the present invention will be described below. Note that the embodiment is an example of the present invention. The scope of the present invention is not limited to the scope of the embodiment.
[0017] The cellulose particles according to the present invention are formed by agglomerating fine fibrous cellulose having an average fiber diameter of 1 to 1000 nm and an average fiber length of 0.01 to 1000 μm, and have a packed bulk density of 0.1 to 200 mg / cm. 3 Before describing the cellulose particles, the fine fibrous cellulose, which is the raw material of the cellulose particles, will be described.
[0018] (Fine fibrous cellulose) Fine fibrous cellulose can be obtained by defibrating (refining) raw material pulp, and can be produced by known processing methods such as chemical processing and mechanical processing.
[0019] As the raw material pulp for the fine fibrous cellulose, one or more of wood pulp made from broadleaf trees, coniferous trees, etc., non-wood pulp made from straw, bagasse, cotton, hemp, bast fiber, etc., waste paper pulp (DIP) made from brown waste paper, envelope paper, magazine paper, flyer paper, cardboard paper, white waste paper, imitation waste paper, reclaimed waste paper, recycled waste paper, and broke paper, etc., can be selected and used. The above various raw materials may be in the form of a pulverized material called cellulose-based powder, for example. In recent years, the demand for products containing organic components that are environmentally friendly has been increasing, so wood pulp made from broadleaf trees or coniferous trees derived from plants other than waste paper is particularly suitable.
[0020] As the wood pulp, one or more types may be selected and used from chemical pulps such as hardwood kraft pulp (LKP), softwood kraft pulp (NKP), sulfite pulp (SP), dissolving pulp (DP), etc., and mechanical pulp (TMP). In particular, chemical pulps such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP), which are wood pulps that increase the cellulose component, are preferred, and bleached pulp (BKP) is suitable.
[0021] As the mechanical pulp, for example, one or more types can be selected and used from stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), ground pulp (GP), thermo-mechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), refiner mechanical pulp (RMP), bleached thermo-mechanical pulp (BTMP), etc.
[0022] From the viewpoint of producing fine fibrous cellulose having a relatively small average fiber diameter, it is preferable to use kraft pulp, which is easy to defibrate and has high dispersibility. In particular, when applied to white products (lotions, gels, etc.), it is convenient that the fine fibrous cellulose itself is white, and from the viewpoint of improving the high whiteness, it is more preferable to use LBKP and NBKP.
[0023] The fine fibrous cellulose may be pretreated prior to defibration. For example, the pretreatment may involve mechanically pre-beating the raw pulp or chemically modifying the raw pulp. The method of pre-beating is not particularly limited, and any known method may be used.
[0024] Examples of pretreatment of raw material pulp by chemical techniques include hydrolysis of polysaccharides with acids (e.g., sulfuric acid, etc.) (acid treatment), hydrolysis of polysaccharides with enzymes (enzyme treatment), swelling of polysaccharides with alkali (alkali treatment), oxidation of polysaccharides with an oxidizing agent (e.g., ozone, etc.) (oxidation treatment), reduction of polysaccharides with a reducing agent (reduction treatment), oxidation with a TEMPO catalyst (oxidation treatment), anionization (anion treatment) and cationization (cation treatment) by phosphate esterification, carbamate formation, etc.
[0025] Examples of the alkali used in the alkali treatment include organic alkali such as sodium hydroxide, lithium hydroxide, potassium hydroxide, aqueous ammonia solution, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. From the viewpoint of production costs, it is preferable to use sodium hydroxide.
[0026] By subjecting the fine fibrous cellulose to an enzyme treatment, an acid treatment, or an oxidation treatment, it is possible to lower the water retention of the fine fibrous cellulose, increase the crystallinity, and increase the homogeneity. If the water retention of the fine fibrous cellulose is low, it is preferable because it is easy to dehydrate and dry.
[0027] When raw pulp is treated with an enzyme, acid, or oxidation, the hemicellulose and amorphous regions of cellulose contained in the pulp are decomposed, and as a result, the energy required for the fine pulp refining process can be reduced and the uniformity and dispersibility of the cellulose fibers can be improved. The dispersibility of the cellulose fibers contributes to improving the uniformity of the molded body, for example. However, since the pretreatment reduces the aspect ratio of the fine fibrous cellulose, excessive pretreatment is preferably avoided.
[0028] Examples of fine fibrous cellulose that has been modified by anionization through the introduction of anionic functional groups include fine fibrous cellulose that has been esterified with phosphorus oxoacid, fine fibrous cellulose that has been carbamate-treated, and fine fibrous cellulose in which the hydroxyl groups of the pyranose rings have been directly oxidized to carboxyl groups.
[0029] Fine fibrous cellulose modified by the introduction of anionic functional groups has relatively high dispersibility, which is presumably because the anionic functional groups cause localized charge bias and easily form hydrogen bonds with water and organic solvents in the dispersion.
[0030] When cellulose fibers are subjected to esterification with phosphorus oxoacid, which is an example of anionization, the fiber raw material can be finely divided, and the fine fibrous cellulose produced has a large aspect ratio, excellent strength, high light transmittance and high viscosity. Esterification with phosphorus oxoacid can be performed by the method described in JP 2019-199671 A. For example, modified fine fibrous cellulose in which hydroxyl groups of cellulose fibers are modified to introduce phosphite ester groups can be mentioned.
[0031] The cellulose fibers can be defibrated by the following defibration devices and methods. The defibration can be performed by using one or more means selected from homogenizers such as high-pressure homogenizers and high-pressure homogenizers, grinders, grinders, and other mill-type friction machines, refiners such as conical refiners and disk refiners, and various bacteria. However, it is preferable to defibrate the cellulose fibers using a water flow, particularly a high-pressure water flow, and a device or method for finely pulverizing the fibers. This device or method provides very high dimensional uniformity and dispersion uniformity for the fine fibrous cellulose obtained. In contrast, for example, when a grinder that grinds between rotating grindstones is used, it is difficult to uniformly pulverize the cellulose fibers, and in some cases, there is a risk that some fiber lumps will remain undisintegrated.
[0032] Grinders used to defibrate cellulose fibers include, for example, the Masscolloider manufactured by Masuko Sangyo Co., Ltd. Devices that use high-pressure water flow to pulverize materials include, for example, Starburst (registered trademark) manufactured by Sugino Machine Co., Ltd. and Nanovater (registered trademark) manufactured by Yoshida Kikai Kogyo Co., Ltd. High-speed rotary homogenizers used to defibrate cellulose fibers include the Clearmix-11S manufactured by M Technique Co., Ltd.
[0033] The present inventors have found that when cellulose fibers are defibrated using both a method of grinding between rotating grinding wheels and a method of refining with a high-pressure water jet, and the resulting fibers are observed under a microscope, the fibers obtained using the method of refining with a high-pressure water jet have a more uniform fiber width.
[0034] Defibration using a high-pressure water stream is preferably performed by pressurizing a dispersion of cellulose fibers with a pressure booster to, for example, 30 MPa or more, preferably 100 MPa or more, more preferably 150 MPa or more, and particularly preferably 220 MPa or more (high pressure condition), spraying it from a nozzle with a pore diameter of 50 μm or more, and reducing the pressure so that the pressure difference is, for example, 30 MPa or more, preferably 80 MPa or more, and more preferably 90 MPa or more (reduced pressure condition). The pulp fibers are defibrated by the cleavage phenomenon caused by this pressure difference. If the pressure of the high-pressure condition is low or the pressure difference from the high-pressure condition to the reduced pressure condition is small, the defibration efficiency decreases, and repeated defibration (spraying from the nozzle) becomes necessary to achieve the desired fiber width.
[0035] As a device for defibrating with a high-pressure water flow, it is preferable to use a high-pressure homogenizer. A high-pressure homogenizer is a homogenizer capable of ejecting a slurry of cellulose fibers at a pressure of, for example, 10 MPa or more, preferably 100 MPa or more. When cellulose fibers are treated with a high-pressure homogenizer, the cellulose fibers are effectively defibrated due to the action of collisions between the cellulose fibers, pressure differences, microcavitation, etc. Therefore, the number of defibration treatments can be reduced, and the production efficiency of fine fibrous cellulose can be improved.
[0036] It is preferable to use a high-pressure homogenizer that causes the cellulose fiber slurry to collide in a straight line. Specifically, for example, a high-pressure homogenizer of the counter-collision type (MICROFLUIDIZER (registered trademark), wet jet mill) is used. In this device, two upstream flow paths are formed so that the pressurized cellulose fiber slurry collide in a counter-collision manner at the junction. The cellulose fiber slurry collides at the junction, and the collided cellulose fiber slurry flows out from the downstream flow path. The downstream flow path is provided perpendicular to the upstream flow path, and a T-shaped flow path is formed by the upstream flow path and the downstream flow path. When such a counter-collision type high-pressure homogenizer is used, the energy provided by the high-pressure homogenizer is converted to collision energy to the maximum extent, so that the cellulose fibers can be defibrated more efficiently.
[0037] The fine fibrous cellulose obtained by defibration can be dispersed in an aqueous medium to prepare a dispersion liquid prior to mixing with inorganic fine particles. The aqueous medium is particularly preferably entirely water (aqueous solution). However, the aqueous medium may be partially other liquids that are compatible with water. As the other liquids, for example, lower alcohols having 3 or less carbon atoms can be used.
[0038] In this specification, fine fibrous cellulose in which the hydroxyl groups of cellulose fibers have been substituted (modified) and phosphorus oxo acid ester groups have been introduced is referred to as modified fine fibrous cellulose (hereinafter also referred to as "modified CNF"), and may be distinguished from unmodified fine fibrous cellulose in which the hydroxyl groups of cellulose fibers have not been substituted (hereinafter also referred to as "unmodified CNF"). Therefore, fine fibrous cellulose is a concept that includes modified fine fibrous cellulose and unmodified fine fibrous cellulose.
[0039] The fine fibrous cellulose forming the cellulose particles of this embodiment may consist of only unmodified fine fibrous cellulose, may consist of only modified fine fibrous cellulose, or may contain both unmodified fine fibrous cellulose and unmodified fine fibrous cellulose.
[0040] When the cellulose particles are formed from modified fine fibrous cellulose, the dispersion liquid in which the cellulose particles are dispersed in a dispersion medium exhibits a transparent color. On the other hand, when the cellulose particles are formed from unmodified fine fibrous cellulose, the dispersion liquid in which the cellulose particles are dispersed in a dispersion medium exhibits a white color. By adjusting the ratio of modified fine fibrous cellulose and unmodified fine fibrous cellulose in the fine fibrous cellulose forming the cellulose particles, a dispersion liquid having an intermediate color between white and transparent can be produced. To produce this dispersion liquid, for example, when producing cellulose particles as the dispersoid of the dispersion liquid, it is preferable to use a mixture of modified fine fibrous cellulose and unmodified fine fibrous cellulose as the fine fibrous cellulose, which is the raw material of the cellulose particles.
[0041] The cellulose particles are in the form of a white powder whether the raw material is modified or unmodified fine fibrous cellulose. Since modified fine fibrous cellulose has a smaller average fiber diameter than unmodified fine fibrous cellulose, when compared with cellulose particles of the same mass, the cellulose particles formed from modified fine fibrous cellulose tend to have a larger specific surface area than the cellulose particles formed from unmodified fine fibrous cellulose.
[0042] The raw material pulp is preferably defibrated so that the physical properties of the resulting fine fibrous cellulose have the desired values or evaluations as shown below.
[0043] <Average fiber diameter> The upper limit of the average fiber diameter (average fiber width; average diameter of a single fiber) of the fine fibrous cellulose is 1000 nm, preferably 500 nm or less, more preferably 100 nm or less, and particularly preferably 50 nm or less. If the average fiber diameter of the fine fibrous cellulose exceeds 1000 nm, the formed cellulose particles will have a relatively small specific surface area, i.e., a poorly porous shape. There is no particular lower limit for the average fiber diameter of the fine fibrous cellulose.
[0044] The average fiber diameter of the fine fibrous cellulose can be adjusted, for example, by the selection of raw pulp, pretreatment, defibration, etc.
[0045] The method for measuring the average fiber diameter of the fine fibrous cellulose is as follows. First, 100 ml of an aqueous dispersion of fine fibrous cellulose with a solid content concentration of 0.01 to 0.1% by mass is filtered through a Teflon (registered trademark) membrane filter, and the solvent is replaced once with 100 ml of ethanol and three times with 20 ml of t-butanol. Next, the sample is freeze-dried and osmium-coated to obtain a sample. This sample is observed using an electron microscope SEM image at a magnification of 3,000 to 30,000 times depending on the width of the fibers that constitute it. Specifically, two diagonal lines are drawn on the observed image, and three straight lines passing through the intersections of the diagonal lines are arbitrarily drawn. Furthermore, the widths of a total of 100 fibers that intersect with these three straight lines are visually measured. The median diameter of the measured values is then taken as the average fiber diameter.
[0046] <Average fiber length> The average fiber length of the fine fibrous cellulose (average length of a single fiber) is, for example, preferably 0.01 to 1000 μm, more preferably 0.03 to 500 μm. If the average fiber length exceeds 1000 μm, the fibers of the fine fibrous cellulose tend to be entangled when dried, and are difficult to disentangle when dispersed in an oil-based dispersion medium. In addition, it becomes easy to support other substances on the fine fibrous cellulose, resulting in cellulose particles with the functionality of the other substances. If the average fiber length is less than 0.01 μm, the cellulose particles are poorly entangled.
[0047] The average fiber length can be adjusted as desired by, for example, selecting the raw pulp, pre-treating, defibrating, and the like.
[0048] The average fiber length of the fine fibrous cellulose is measured in the same manner as in the case of the average fiber diameter, by visually measuring the length of each fiber. The median length of the measured values is taken as the average fiber length.
[0049] <Axle ratio> The axial ratio of the fine fibrous cellulose (average fiber length / average fiber width) is preferably 10 to 1,000,000, more preferably 30 to 500,000, and particularly preferably 50 to 100,000. When the axial ratio of the fine fibrous cellulose is less than 10, the cellulose component is almost in a particulate form, making it difficult to form cellulose particles. On the other hand, when the axial ratio exceeds 1,000,000, the degree of entanglement between the fibers becomes large, making it difficult to obtain cellulose particles with the desired average particle size.
[0050] <Crystallization degree> The crystallinity of the fine fibrous cellulose has a lower limit of 50 or more, more preferably 60 or more, and particularly preferably 70 or more, and an upper limit of 100 or less, more preferably 95 or less, and particularly preferably 90 or less. If the crystallinity is less than 50, the entanglement of the fibers will be weakened due to the influence of temperature changes during drying, etc., and the retention of other substances will be weakened, making it difficult to form cellulose particles of the desired particle size.
[0051] The crystallinity is a value measured by X-ray diffraction in accordance with JIS-K0131 (1996) "General Rules for X-ray Diffraction Analysis." Note that fine fibrous cellulose has an amorphous portion and a crystalline portion, and the crystallinity refers to the proportion of the crystalline portion in the entire fine fibrous cellulose.
[0052] <Pseudo particle size distribution> The peak value in the pseudo particle size distribution curve of the fine fibrous cellulose is preferably one peak. When there is one peak, the fine fibrous cellulose has high uniformity in fiber length and fiber diameter, and the fine fibrous cellulose easily becomes entangled with each other during the production of cellulose particles, so that the produced cellulose particles are difficult to be unraveled even when redispersed. In addition, the cellulose particles have a small variation in particle size. If the cellulose particles are in the form of inorganic fine particles supported, the cellulose particles are sufficiently dispersed in the cosmetic when the cellulose particles are blended as one component of the cosmetic.
[0053] The peak value of the fine fibrous cellulose is measured in accordance with ISO-13320 (2009). More specifically, a particle size distribution measuring device (Laser Diffraction / Scattering Particle Size Distribution Meter manufactured by Seishin Enterprise Co., Ltd.) is used to examine the volumetric particle size distribution of the aqueous dispersion of the fine fibrous cellulose. Then, the most frequent diameter of the fine fibrous cellulose is measured from this distribution. This most frequent diameter is taken as the peak value. It is preferable that the fine fibrous cellulose has a single peak in a pseudo particle size distribution curve measured by a laser diffraction method in an aqueous dispersion state. In this way, the fine fibrous cellulose having one peak is preferable because it has been sufficiently refined and can exhibit good physical properties as fine fibrous cellulose. The peak value of the pseudo particle size distribution of the particle size of the fine fibrous cellulose having the single peak is, for example, preferably 300 μm or less, more preferably 200 μm or less, and particularly preferably 100 μm or less. If the peak value exceeds 300 μm, there are many relatively large fibers, the particle size of the cellulose particles varies greatly, and the shape of the cellulose particles tends to be non-uniform.
[0054] The peak value in the particle size and the median diameter in the pseudo-particle size distribution of the fine fibrous cellulose can be adjusted, for example, by the selection of raw pulp, pretreatment, defibration, etc.
[0055] <Water retention> The water retention of the fine fibrous cellulose is not particularly limited, but for example, in the case of unmodified fine fibrous cellulose, it is 500% or less, more preferably 100 to 500%. If the water retention exceeds 500%, the fine fibrous cellulose itself has high water retention and poor dehydration, so even if it is produced through a drying process, the drying time becomes long and productivity is poor. The lower limit of the water retention of the fine fibrous cellulose is not particularly limited, but if it is 100% or more, the bonding force between the fine fibrous celluloses acts, making it easy to maintain the shape of the porous particles.
[0056] The water retention of the fine fibrous cellulose can be adjusted as desired by, for example, selecting the raw pulp, pre-treating it, defibrating it, and the like.
[0057] The water retention of the fine fibrous cellulose is a value measured in accordance with JAPAN TAPPI No. 26 (2000).
[0058] <Pulp viscosity> The pulp viscosity of the defibrated fine fibrous cellulose is 1 to 10 cps, more preferably 2 to 9 cps, and particularly preferably 3 to 8 cps. The pulp viscosity is the viscosity of the solution obtained by dissolving cellulose in a copper ethylenediamine solution, and a higher pulp viscosity indicates a higher degree of polymerization of cellulose, which also affects the strength of the fiber itself.
[0059] <Additives> Additives can be added to improve the dispersibility of the cellulose particles produced through the drying process in a solvent. The additives can be added to the fine fibrous cellulose before freezing, and may be mixed uniformly. As the additives, one or more selected from the group consisting of polyhydric alcohols, polysaccharides, and water-soluble polymers may be used. The compounding ratio of the additives (=additives:fine fibrous cellulose) is 1:99 to 50:50, preferably 50:50, based on the solid content. If the compounding ratio of the additives to the fine fibrous cellulose is high, the dried product (cellulose particles) becomes sticky, the lightness of the cellulose particles of the present invention is lost, and the handling properties are deteriorated. On the other hand, if the compounding ratio is too low, the dispersion effect in the target solvent may be deteriorated.
[0060] As the additive, polyhydric alcohols such as glycerin, propylene glycol, butylene glycol, pentanediol, dipropylene glycol, hexanediol, heptanediol, etc. can be used, but are not limited to these. Glycerin is particularly preferred from the viewpoint of thickening properties and dispersibility of composite particles.
[0061] Examples of polysaccharides that can be used include, but are not limited to, quince seed, veegum, xanthan gum, hyaluronate, etc. Hyaluronate is particularly preferred from the viewpoint of thickening properties and dispersibility of cellulose particles.
[0062] Examples of the water-soluble polymer include, but are not limited to, polyvinyl alcohol, polyvinylpyrrolidone, carboxyvinyl polymer, and polyethylene glycol. In particular, polyvinylpyrrolidone is preferred from the viewpoints of viscosity increasing property and dispersibility of cellulose particles.
[0063] <Inorganic fine particles> The cellulose particles may contain inorganic fine particles. The inorganic fine particles can impart various functions to the cellulose particles. For example, metal-based inorganic fine particles have the effect of diffusely reflecting incident light, so that the cellulose particles can be imparted with the effect of diffusely reflecting light by containing inorganic fine particles in the cellulose particles. For example, the cellulose particles containing inorganic fine particles can be used as one component of a cosmetic to provide a cosmetic with a sunlight transmission suppression effect. The cosmetic with a sunlight transmission suppression effect can be applied to the skin to provide a sunscreen effect.
[0064] The content of inorganic fine particles in the cellulose particles may be set at an upper limit of 50% by mass, preferably 45% by mass or less, and at a lower limit of 0% by mass, preferably 5% by mass or more. If the content exceeds 50% by mass, the ratio of inorganic fine particles to the fine fibrous cellulose is large, the specific gravity of the cellulose particles is large, and there is a risk of high redispersibility in the dispersion medium being impaired. On the other hand, if the content is 5% by mass or more, the effect of suppressing the transmission of sunlight is sufficiently exhibited.
[0065] The upper limit of the primary particle diameter of the inorganic fine particles is preferably 10 μm, more preferably 5 μm or less, and more preferably 1 μm or less. If the primary particle diameter of the inorganic fine particles exceeds 10 μm, the inorganic fine particles are difficult to support by the fine fibrous cellulose. In addition, the surface area of the cellulose particles is not sufficiently large. The inorganic fine particles are not particularly limited in terms of the lower limit, but are preferably 1 nm, more preferably 2 nm or more, and more preferably 3 nm or more. If the primary particle diameter of the inorganic fine particles is 1 nm or more, when the inorganic fine particles are mixed with a slurry of the fine fibrous cellulose, the inorganic fine particles are easily dispersed and cling to the fine fibrous cellulose.
[0066] The primary particle size of the inorganic fine particles can be measured by observation under an electron microscope, and the average value of the obtained particle sizes is taken as the measured value.
[0067] The inorganic fine particles can be used as they are, but it is preferable to subject them to hydrophilic treatment, since it makes them more compatible with the aqueous dispersion of fine fibrous cellulose. The surface treatment agent used for hydrophilic treatment has the effect of suppressing the surface activity of the inorganic fine particles, improving the dispersibility of the inorganic fine particles, and improving transparency and squeaking. The surface treatment agent for the inorganic fine particles is not particularly limited as long as it is a treatment agent that can be dispersed in the aqueous dispersion of fine fibrous cellulose, but it is preferable to use one that contains silicic anhydride or hydrated silicic acid.
[0068] The inorganic fine particles are not particularly limited and known inorganic fine particles can be used, for example, barium titanate, lead zirconate titanate, silicon carbide, silicon nitride, aluminum nitride, alumina, zirconia, zircon, titanium oxide, zinc oxide, iron oxide, cerium oxide, etc. Cellulose particles having these powders and fine fibrous cellulose are preferable because they have excellent redispersibility in liquid. From the viewpoint of suppressing the transmission of sunlight, for example, one or a combination of two or more selected from the group consisting of titanium oxide, zinc oxide, iron oxide, and cerium oxide can be used. In particular, when the inorganic fine particles are titanium oxide, rutile type is preferable because it improves the suppression of the transmission of sunlight in the cosmetic composition.
[0069] The shape of the inorganic fine particles that can be contained in the cellulose particles is not particularly limited, and can be, for example, spherical, rod-like, needle-like, spindle-like, plate-like, polygonal, or the like.
[0070] The inorganic fine particles may be attached to the surface of the fine fibrous cellulose in the cellulose particles, or may be encapsulated in the fine fibrous cellulose. When the inorganic fine particles are encapsulated in the fine fibrous cellulose, the cellulose particles can support the inorganic fine particles not only on the surface but also inside, and have excellent transmittance suppression against irradiation of sunlight from various angles. Here, encapsulation can refer to a state in which a part of the surface of the inorganic fine particles is covered with the fine fibrous cellulose, or a state in which the inorganic fine particles are covered with the fine fibrous cellulose and cannot be observed when the cellulose particles are observed from the outside.
[0071] The inorganic particles can be added to the fine fibrous cellulose before freezing and mixed until homogeneous.
[0072] (Cellulose particles) The cellulose particles of the present embodiment are formed by drying fine fibrous cellulose, but when viewed microscopically, some are formed by drying and agglomerating fine fibrous cellulose as a single unit (in other words, a single thread becomes entangled within the thread), while others are formed by agglomerating multiple fine fibrous celluloses during drying to form agglomerates. Since the cellulose, which is the structural unit of fine fibrous cellulose, has hydroxyl groups (OH groups) and hydrogen groups (H groups), cellulose particles containing fine fibrous cellulose also have hydroxyl groups and hydrogen groups. The hydroxyl groups and hydrogen groups are hydrogen-bonded with other hydroxyl groups and hydrogen groups, and the fine fibrous cellulose is hydrogen-bonded within the cellulose or with each other to aggregate and form cellulose particles. When cellulose particles are mixed with an aqueous medium, the hydrogen bonds are broken by hydrolysis or the like, and the cellulose aggregation is weakened, and the cellulose particles and the broken fine fibrous cellulose are dispersed in the aqueous medium. On the other hand, when cellulose particles are mixed with an oil-based medium instead of an aqueous medium, it is speculated that the following will occur. Since the oil-based medium is hydrophobic, a reaction in the direction of breaking apart the aggregation of the cellulose particles is unlikely to occur. Therefore, in order to disperse the cellulose particles in the oil-based medium and maintain this state, it is preferable that the bulk density is within a predetermined range. If the bulk density of the cellulose particles is within the predetermined range, the cellulose particles are less likely to be compacted by their own weight and are less likely to settle.
[0073] The cellulose particles according to the present embodiment preferably contain 50% by mass or more of fine fibrous cellulose, more preferably 60% by mass or more, and even more preferably 70% by mass or more, with the upper limit being 100% by mass. If the mass percentage of fine fibrous cellulose in the cellulose particles is less than 50% by mass, the desired bulk density and specific surface area of the cellulose particles of the present invention may not be obtained.
[0074] <Average particle size> The cellulose particles according to the present embodiment preferably have an average particle diameter in the range of 0.1 to 1000 μm, more preferably in the range of 0.1 to 700 μm, and even more preferably in the range of 0.1 to 500 μm. The effects of the present invention can be achieved even if the average particle diameter is less than the above range, but in terms of ease of handling, it is desirable that the average particle diameter is equal to or greater than the lower limit of the above range. On the other hand, if the average particle diameter exceeds the above range, when the cellulose particles are filled or dispersed in a dispersion medium, the voids formed between the particles become large, making it difficult to adjust the concentration to the desired level.
[0075] The standard deviation of the particle size of the cellulose particles is preferably from 1 to 400 μm, more preferably from 1 to 300 μm, and particularly preferably from 2 to 200 μm.
[0076] The cellulose particles of this embodiment are characterized by having various particle sizes. Specifically, the particle size of the cellulose particles (or cellulose particle group) is large, that is, the dispersion coefficient of the particle size is large. The cellulose particles are not excellent in sphericity, and each has irregularities, a porous shape, and different shapes. Therefore, it may be difficult to intentionally separate large and small particles using a sieve, for example.
[0077] The average particle size, median size, cumulative 10% size, and cumulative 90% size of cellulose particles were measured using a measuring device conforming to ISO-13320 (2009), specifically, a laser diffraction / scattering type particle size distribution measuring device (particle size distribution) "LA-960V2", using a dry method without removing moisture adhering to the cellulose particles.
[0078] <Specific surface area> The specific surface area of the cellulose particles is preferably 20 m 2 / g or more, more preferably 30m 2 / g or more, more preferably 40m 2 / g or more, and the upper limit of the specific surface area is not particularly limited, but is 5000 m 2 / g. The specific surface area is 20m2 If the specific surface area is less than 5000 m / g, when inorganic fine particles are supported on cellulose particles, the amount of inorganic fine particles that can be supported is small, and the inorganic fine particles may not exhibit their full potential. 2 A particle size exceeding this limit is preferable in terms of reducing the particle weight and redispersibility, but is very difficult to produce.
[0079] The specific surface area was measured by the BET method. Specifically, the measurement was performed using a Quantachrome Instruments NOVA4200e measuring instrument, using the nitrogen gas adsorption method. The test method used was JIS Z8830:2013.
[0080] <Moisture percentage> The moisture content of the cellulose particles is preferably 50% or less, more preferably 40%, and even more preferably 30% or less. Cellulose particles with a moisture content of more than 30% contain a large amount of water, and even if mixed and dispersed in an oil-based dispersion medium, the dispersed state may not be maintained.
[0081] <Bulk density> The cellulose particles according to this embodiment preferably have a packed bulk density of 0.1 to 200 mg / cm 3 More preferably, the packed bulk density is 0.1 to 150 mg / cm 3 More preferably, the packed bulk density is 0.1 to 100 mg / cm 3 The range of the compacted bulk density is 200 mg / cm 3 Cellulose particles with a packed bulk density of more than 0.1 mg / cm are aggregates in which the fibers are tightly entangled, and are poorly dispersible. Even if dispersed in a dispersion medium, the particles may gradually begin to settle due to their own weight, and therefore cannot be said to have excellent dispersibility. 3 Cellulose particles smaller than this size tend to disintegrate in powder form in the air and are difficult to handle.
[0082] On the other hand, the loose bulk density, packed bulk density, and compressibility of the cellulose particles according to this embodiment satisfy the following relationship [Mathematical formula 1]. [Number 1] (Degree of compression (%)) = ((Packed bulk density) - (Loose bulk density)) / (Packed bulk density) x 100
[0083] The packed bulk density and loose bulk density are items used to calculate the Carr fluidity index, and were measured in accordance with the ASTM D6393-99 Compressibility Measurement Method. The measurements were performed using a multi-function powder property measuring instrument, Multitester MT-02 (manufactured by Seishin Enterprise Co., Ltd.).
[0084] <Compression level> The degree of compression of the cellulose particles is preferably 50% or less, more preferably 40% or less, and even more preferably 30%. Since the cellulose particles of this embodiment are relatively light, the voids are eliminated during the compression process for measuring the packed bulk density after measuring the loose bulk density (i.e., the cellulose particles are densely packed together in the container due to the voids formed between the cellulose particles being eliminated), and the change in density of the cellulose particles themselves is small, and the collapse of the particle shape is unlikely to occur. In addition, since the cellulose particles are not spherical with excellent sphericity, but are uneven granules (difficult to express), and are porous granules, when filled in a container, many voids of various shapes and sizes are generated. If the degree of compression exceeds 50%, in addition to filling the voids between the particles, the collapse of the cellulose particles is suggested, and the lightness of the particles may be lost. Note that, in the case of cellulose particles produced by hot drying, the fibers are firmly agglomerated to form solid particles, so the voids between the particles are only filled, and the collapse of the particles itself is small. The voids formed between cellulose particles can be conceptually understood as voids formed between atoms packed in a unit lattice. On the other hand, the lower limit of the compression degree of cellulose particles is not particularly limited (i.e., 0%), but considering that the above-mentioned voids may occur slightly, it may be, for example, 1% or more.
[0085] (Manufacturing) The cellulose particles can be produced by freeze-drying the cellulose nanofiber raw material, drying under reduced pressure, heat drying, spray drying, or the spray-type freezing and vacuum drying method of the present embodiment, but the spray-type freezing and vacuum drying method is particularly preferred because it allows the production of porous cellulose particles. If the cellulose particles are porous, it is possible to support another substance in the numerous pores formed in the cellulose particles, or to utilize the large surface area. This allows the cellulose particles to be endowed with properties not found in cellulose.
[0086] The cellulose particles according to the present invention can be produced by a freeze-drying process. For example, a spray-type freeze granulation apparatus 1 shown in Fig. 1 is preferable because it can produce particles with a relatively small specific gravity. The spray-type freeze granulation apparatus 1 comprises a freeze granulation tank 8, a spray mechanism unit 7 that sprays raw material M onto the upper part of the freeze granulation tank 8, and a drying unit 6 that is provided below the freeze granulation tank 8 and dries the frozen cellulose particles. The raw material M sprayed into the freeze granulation tank 8 is instantly frozen in the freeze granulation tank 8 to become a frozen body P. The frozen body P falls naturally into the drying unit 6 and is stored therein. The drying unit 6 is separably connected to the freeze granulation tank 8, and is separated from the freeze granulation tank 8 when the frozen body P is stored therein, and is sealed so that the frozen body P can be dried to obtain cellulose particles.
[0087] Examples of the raw material M include a slurry or dispersion of fine fibrous cellulose. The fine fibrous cellulose used in the raw material M may be fine fibrous cellulose consisting of one group, or may be a combination of fine fibrous cellulose consisting of two groups. When a combination of fine fibrous cellulose consisting of two groups is used, it may be a combination of fine fibrous cellulose group C1 having an average particle diameter R of 11 to 1000 nm and fine fibrous cellulose group C2 having an average particle diameter R of 1 to 10 nm, in a mixing ratio of 1:99 to 99:1.
[0088] The spray mechanism 7 has a raw material flow path to which the raw material M is supplied, a compressed gas flow path to which the compressed gas A is supplied, and a nozzle 5 (also called a two-fluid nozzle) that sprays a mixed fluid of the supplied raw material M and compressed gas A into the freeze granulation tank 8. Examples of the type of the nozzle 5 include a three-fluid type, a four-fluid type, a pressurized type, an ultrasonic type, and a centrifugal spray type.
[0089] The raw material flow path has a base end connected to a raw material tank that stores raw material M, and a pump provided in the raw material flow path causes raw material M to flow from the raw material tank to nozzle 5. The compressed gas flow path has a base end connected to a compressed gas supply device such as a compressor or a cylinder, and when the compressed gas supply device is started, compressed gas flows into nozzle 5. Examples of compressed gas include air, nitrogen, and rare gases.
[0090] In addition to the fine fibrous cellulose, the raw material M may contain additives and inorganic fine particles, and may also contain a plasticizer, such as a phthalate ester or a citrate ester.
[0091] The freezing granulation tank 8 is composed of three tanks, specifically, three cylinders of different diameters arranged concentrically with the same axis in the vertical direction. These three cylinders are, in order from the inside, an inner tank wall 2, a middle tank wall 3, and an outer tank wall 4. The inner tank surrounded by the inner tank wall 2 is a freezing tank 12 for freezing the raw material M, the bottomed middle layer surrounded by the inner tank wall 2 and the middle tank wall 3 is a cooling medium filled tank 13 filled with a cooling medium, and the bottomed outer tank surrounded by the outer tank wall 4 and the middle tank wall 3 is a vacuum insulation tank 14 for keeping the temperature inside the tank constant. The freezing tank 12 is preferably configured so that the lower end of the inner tank wall 2 is detachably connected to a flange portion 4a formed at the upper end of the drying section 6.
[0092] The freezing tank 12 freezes the raw material M sprayed from a nozzle 5 provided near the top surface to form a frozen body P. The temperature of the freezing tank 12 is preferably kept at -10°C to -200°C by the cooling medium supplied from a cooling medium filling tank 13.
[0093] The cooling medium tank 13 is filled with a cooling medium for cooling the freezing tank 12. As the cooling medium, for example, liquid nitrogen, liquid argon, liquid helium, dry ice, etc. can be used.
[0094] The vacuum insulation tank 14 is surrounded by an inner tank wall 2 and an outer tank wall 4, with the upper end of the inner tank wall 2 and the upper end of the outer tank wall 4 closed, and the lower end of the inner tank wall 2 and the lower end of the outer tank wall 4 closed, so that no fluid flows into the vacuum insulation tank 14 from the outside, a vacuum state is maintained, and heat transfer between the cooling medium filled in the cooling medium filled tank 13 and the outside air is unlikely to occur.
[0095] The cooling medium tank 13 has a cooling medium supply pipe 15 extending from the outside into the cooling medium tank 13, and is configured so that the cooling medium N is supplied into the cooling medium tank 13, and has a cooling medium introduction pipe 16 that introduces the cooling medium gas vaporized from the cooling medium N in the cooling medium tank 13 into the freezing tank 12, and is configured so that the cooling medium gas is introduced into the freezing tank 12.
[0096] The frozen body P formed in the freeze granulation tank 8 is stored in the drying section 6 which is detachably provided to the freeze granulation tank 8. After a predetermined amount of frozen body P is stored in the drying section 6, the drying section 6 is separated from the freeze granulation tank 8 and sealed, and then freeze-drying is performed to obtain cellulose particles. The configuration of the dryer 100 according to this embodiment will be described below.
[0097] The dryer 100 has a drying section 6 and a vacuum mechanism. The drying section 6 can have a cylindrical wall with an axis in the vertical direction and a bottom continuous with the wall. The cylindrical wall can be provided with an openable and closable exhaust section (not shown), and the gas in the drying section 6 can be exhausted from the exhaust section as exhaust gas D. The upper edge of the cylindrical wall is a flange section 4a, which is detachably connected to the lower edge of the freeze granulation tank 8. After the frozen body P generated in the freeze granulation tank 8 falls into the drying section 6, the drying section 6 is removed from the freeze granulation tank 8, and the flange section 4a is covered with a top lid and sealed to freeze-dry the frozen body P.
[0098] The drying process of the frozen body P can be performed as follows. The drying section 6 is configured so that the base end of a gas pipe 21 for vacuum drawing can be connected, and the gas sucked into the gas pipe 21 is led to a cold trap 22 connected to the tip of the gas pipe 21, where a part of the gas is concentrated and separated as a concentrated liquid or concentrated solid, and the remaining gas is sucked by a vacuum pump 24 provided at the other end of a gas pipe 23 connected to the cold trap 22. When the vacuum pump 24 is started with the drying section 6 sealed, the air pressure inside the drying section 6 decreases, and the sublimable or vaporizable substance contained in the frozen body P (for example, water when the raw material M is a dispersion liquid consisting of water and fine fibrous cellulose) sublimes or vaporizes and is sucked into the vacuum pump 24, and the remainder becomes cellulose particles. In the process of drying, it is preferable to rock or vibrate the drying section 6 so that the frozen bodies P do not aggregate with each other and to dry each frozen body P evenly. The vibration or rocking of the drying section 6 may be performed manually, or a vibration mechanism or a rocking mechanism may be provided. When vibrating, for example, both ends of the diameter of the flange portion formed in a substantially circular shape (parts indicated by symbols 4a and 4a in FIG. 1) can be grasped and swung left and right, and when rocking, for example, the diameter can be used as the axis of rotation to rotate alternately clockwise and counterclockwise. The pivot angle to the right or left is not particularly limited, but a value of 30° to 100° is sufficient to rock the frozen body P in the drying section 6. In the drying process, rocking or vibration is not essential, and the frozen body P may be vacuum-dried while stationary. Although this cannot be said in general, rocking or vibration during drying may result in a relatively higher bulk density of the cellulose particles produced.
[0099] A dryer 200 according to another embodiment will be described with reference to Figs. 11 and 12. The difference from the dryer 100 in Fig. 1 described above is that a shaft core 30 for rocking the drying section 6 is provided. By providing a rocking mechanism on the shaft core 30, the drying section 6 can be rotated, for example, 100° clockwise or counterclockwise on the paper surface of Fig. 12 around the shaft core 30.
[0100] Cellulose particles 11, 12 produced by the above-mentioned production method are shown in Figs. 2 to 5. The cellulose particles 11 shown in Figs. 2 and 3 were produced by using a spray-type freeze granulation apparatus 1 using a 2% by mass aqueous dispersion of unmodified fine fibrous cellulose (ELLEX (registered trademark)-S) as a raw material. Numerous pores 11a were confirmed in the cellulose particles 11, and it was found that the cellulose particles 11 have a porous structure. The cellulose particles 11 shown in Figs. 4 and 5 were produced by using a spray-type freeze granulation apparatus 1 using a 2% by mass aqueous dispersion of modified fine fibrous cellulose (ELLEX (registered trademark)-Star) as a raw material. Numerous pores 12a were confirmed in the cellulose particles 12. The drying process was carried out by placing the particles in a vacuum dryer ("EYELA FDU-2110" manufactured by Tokyo Rikakikai Co., Ltd.) and vacuum drying while the particles were left stationary. An example of the freeze granulation tank 8 is "Freeze Granulation Chamber CS30" manufactured by Priss Co., Ltd., and an example of the dryer 200 is "TFD-10" manufactured by Priss Co., Ltd.
[0101] (Cellulose particle dispersion) The cellulose particles can be dispersed in an oil-based medium to prepare a cellulose particle dispersion. The oil-based medium is not particularly limited as long as it is an oil that has fluidity at 0 to 40°C, that is, a liquid oil (liquid, gel, solid solution, foam, cream, etc.). The oil can be one or a combination of two or more selected from, for example, hydrocarbons with a carbon number of C15 or more, fatty acids with a carbon number of C12 or more, alcohols with a carbon number of C6 or more, and dimethyl silicone. For example, natural animal and vegetable oils and fats such as jojoba oil, macadamia nut oil, avocado oil, evening primrose oil, mink oil, rapeseed oil, castor oil, sunflower oil, corn oil, cacao oil, palm oil, rice bran oil, olive oil, almond oil, sesame oil, safflower oil, soybean oil, camellia oil, persic oil, castor oil, mink oil, cottonseed oil, Japan wax, palm oil, palm kernel oil, egg yolk oil, lanolin, and squalene; hydrocarbons such as synthetic triglycerides, squalane, liquid paraffin, petrolatum, ceresin, microcrystalline wax, and isoparaffin; waxes such as carnauba wax, paraffin wax, whale wax, beeswax, candelilla wax, and lanolin; cetanol, stearyl alcohol, lauryl alcohol, cetostearyl alcohol, oleyl alcohol, behenyl alcohol, lanolin alcohol, and water. higher alcohols such as added lanolin alcohol, hexyldecanol, octyldodecanol, etc.; higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, isostearic acid, oleic acid, linoleic acid, oxystearic acid, undecylenic acid, lanolin fatty acid, hard lanolin fatty acid, soft lanolin fatty acid, etc.; cholesterol and its derivatives such as cholesteryl-octyldodecyl-behenyl; esters such as isopropyl myristic acid, isopropyl palmitic acid, isopropyl stearic acid, 2-ethylhexanoic acid glycerol, butyl stearic acid, etc.; polar oils such as diethylene glycol monopropyl ether, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxypropylene butyl ether, ethyl linoleate, etc.;Others include amino-modified silicone, epoxy-modified silicone, carboxyl-modified silicone, carbinol-modified silicone, methacryl-modified silicone, mercapto-modified silicone, phenol-modified silicone, one-end reactive silicone, heterogeneous functional group-modified silicone, polyether-modified silicone, methylstyryl-modified silicone, alkyl-modified silicone, higher fatty acid ester-modified silicone, hydrophilic special modified silicone, higher alkoxy-modified silicone, higher fatty acid-containing silicone, fluorine-modified silicone, etc., more specifically, silicone resin, methylphenylpolysiloxane, methylpolysiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexanesiloxane, methylcyclopolysiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, polyoxyethylene-methylpolysiloxane copolymer, polyoxypropylene-methylpolysiloxane copolymer, poly(oxyethylene-oxypropylene) One or a combination of two or more selected from silicones including various derivatives such as methyl polysiloxane copolymer, methyl hydrogen polysiloxane, tetrahydrotetramethylcyclotetrasiloxane, stearoxy methyl polysiloxane, sethoxy methyl polysiloxane, methyl polysiloxane emulsion, highly polymerized methyl polysiloxane, trimethylsiloxysilicate, crosslinked methyl polysiloxane, crosslinked methyl phenyl polysiloxane, and crosslinked methyl phenyl polysiloxane can be used. The concentration of cellulose particles contained in the cellulose particle dispersion can be 0.1 to 20 mass%, preferably 0.5 to 10 mass%. If the concentration of cellulose particles is less than 0.1 mass%, the amount of cellulose particles is small and the cellulose particles may not be distributed throughout the entire dispersion. If the concentration of cellulose particles exceeds 20 mass%, the viscosity of the dispersion becomes too high, and the use is extremely limited.;
[0102] Water and an emulsifier can be added to the cellulose particle dispersion. In this case, the oil and water are separated. The separated oil and water can be used, or the emulsion can be emulsified and used. When emulsifying, the emulsion can be dispersed and emulsified using a known dispersing machine (homogenizer, etc.). The emulsion is not strictly influenced by the properties of the emulsifier (surfactant). This is a feature of the emulsifier containing the cellulose particles of this embodiment, and the cellulose particle dispersion can be easily emulsified as long as the cellulose particles are contained, regardless of the emulsifier. In the case of emulsification, micelles are formed by the oil, water, and emulsifier, and the emulsion is maintained in an emulsified state without being separated into the oil and water by dispersing the micelles in the emulsion. Although the exact mechanism is unclear, it is speculated that the cellulose particles enter the micelles and are integrated, thereby suppressing the collapse of the shape of the micelles. In other words, it is speculated that the cellulose particles play a role like a reinforcing material for the micelles. The content of the emulsifier in the cellulose particle dispersion is 0.1 to 10% by mass, and preferably 0.2 to 8.0% by mass.
[0103] When the cellulose particle dispersion is emulsified to prepare an emulsion, the blending ratio of oil and water (oil:water) can be, for example, 99:1 to 1:99, preferably 95:5 to 5:95. If the cellulose particles are contained in the emulsion, the emulsion can be either a water-in-oil emulsion or an oil-in-water emulsion. In the case of a water-in-oil emulsion, the blending ratio of oil and water (oil:water) can be, for example, 99:1 to 51:49, preferably 95:5 to 51:49. On the other hand, in the case of an oil-in-water emulsion, the blending ratio of oil and water (oil:water) can be, for example, 1:99 to 49:51, preferably 5:95 to 49:51. However, the emulsion containing cellulose particles can be an intermediate emulsion between a water-in-oil emulsion and an oil-in-water emulsion, without strictly dividing the emulsion into a water-in-oil emulsion and an oil-in-water emulsion.
[0104] Examples of the emulsifier that can be used include nonionic surfactants, anionic surfactants, cationic surfactants, amphoteric surfactants, and phospholipids. In particular, it is preferable to use ester or ester-ether type nonionic surfactants. Examples of the emulsifier that can be used include glycerin fatty acid esters, polyglycerin, fatty acid esters, propylene glycol fatty acid esters, sorbitan fatty acid esters, and fatty acid esters of sorbitol, as well as alkylene glycol adducts thereof, polyalkylene glycol fatty acid esters, sucrose fatty acid esters, polysorbate 20, polysorbate 60, polysorbate 80, polyoxyalkylene alkyl ethers, and polyoxyethylene alkylphenyl ethers. EXAMPLES
[0105] (Preparation of Test Examples and Comparative Examples) <Test Example 1> Examples are shown below. Test Example 1 was produced as follows. A dispersion liquid in which unmodified fine fibrous cellulose ("ELLEX (registered trademark)-S" manufactured by Daio Paper Co., Ltd.) was dispersed in water to a concentration of 2% by mass was supplied to a spray-type freeze granulation device as a raw material to obtain cellulose particles, which were used as Test Example 1. The average fiber diameter of the fine fibrous cellulose was 50 nm. The raw material was sprayed into the spray-type freeze granulation device and frozen to obtain a frozen body as an intermediate, and this frozen body was vacuum-dried to obtain cellulose particles. The fine fibrous cellulose was frozen using Priss's "Freeze Granulation Chamber CS30", and after obtaining the frozen body, the frozen body was dried while being shaken using Priss's barrel freeze drying unit "TFD-10" until the frozen body was completely dried.
[0106] <Test Example 2> Test Example 2 was produced as follows. Using the same dispersion liquid as that used in Test Example 1 as a raw material, fine fibrous cellulose was supplied to a Priss "Freeze Granulation Chamber CS30" to obtain a frozen body as an intermediate, and this frozen body was vacuum dried to obtain cellulose particles, which was used as Test Example 2. In order to dry the frozen body while it was left stationary, the frozen body was placed in a vacuum dryer (Tokyo Rikakikai Co., Ltd. "EYELA FDU-2110") and vacuum dried while it was left stationary.
[0107] <Test Example 3> Test Example 3 was produced as follows. A mixture was obtained by mixing the same unmodified fine fibrous cellulose ("ELLEX (registered trademark)-S" manufactured by Daio Paper Co., Ltd.) as the fine fibrous cellulose used in Test Example 1 with a citric acid ester in a mixing ratio of 75%:25%. This mixture was dispersed in water to a concentration of 2% by mass, and the resulting dispersion was used as a raw material for freezing using a Priss Co., Ltd. "Freeze Granulation Chamber CS30". After obtaining a frozen body, the frozen body was dried while being shaken using a Priss Co., Ltd. barrel freeze drying unit "TFD-10" manufactured by Priss Co., Ltd. until the frozen body was completely dried. The cellulose particles obtained after drying were used as Test Example 3.
[0108] <Test Example 4> Test Example 4 was produced as follows. Fine fibrous cellulose in which hydroxyl groups have been modified to phosphite groups (product "ELLEX (registered trademark)-Star" manufactured by Daio Paper Co., Ltd.) was dispersed in water to a concentration of 0.5% by mass, and the dispersion was frozen using Priss's "Freeze Granulation Chamber CS30" to obtain a frozen body. The frozen body was then dried while being shaken using Priss's barrel freeze drying unit "TFD-10" until the frozen body was completely dried. The cellulose particles obtained after drying were used as Test Example 4. The average fiber diameter of the fine fibrous cellulose was 4 nm.
[0109] <Test Example 5> Test Example 5 was produced as follows: the same dispersion liquid as that used in Test Example 4 was supplied as a raw material to a "freeze granulation chamber CS30" manufactured by Priss to obtain a frozen body as an intermediate, and this frozen body was vacuum dried to obtain cellulose particles, which was used as Test Example 5. In order to dry the frozen body while it was left stationary, the frozen body was placed in a vacuum dryer ("EYELA FDU-2110" manufactured by Tokyo Rikakikai Co., Ltd.) and vacuum dried while it was left stationary.
[0110] <Comparative Example 1> In Comparative Example 1, unmodified fine fibrous cellulose (ELLEX (registered trademark)-S, a product manufactured by Daio Paper Co., Ltd.) and glycerin (glycerin, Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed in a mixing ratio of 71%:29% to obtain a mixture, which was then fed into a drum dryer and dried by heat to obtain a dried product, which was then pulverized to obtain cellulose particles with an average particle size of 53.1 μm, which was designated as Comparative Example 1. An SEM image of the particles of Comparative Example 1 is shown in FIG. 10. Compared to the cellulose particles of this embodiment, the particles of Comparative Example 1 have a solid interior, a small specific surface area, and a high density.
[0111] <Comparative Example 2> Comparative Example 2 is a cellulose granule produced by the same production method as Comparative Example 1, except that the cellulose granules had an average particle size of 238.8 μm.
[0112] The physical properties of the test examples and comparative examples were measured, including the degree of compression, loose bulk density, packed bulk density, specific surface area, moisture content, average particle size, median size, cumulative 10% size, and cumulative 90% size.
[0113] Compressibility is one of the items used to calculate Carr's fluidity index, and was measured in accordance with ASTM D6393-99 Compressibility Measurement Method. The measurement was performed using a multi-function powder property measuring instrument, Multitester MT-02 (manufactured by Seishin Enterprise Co., Ltd.). The specific surface area was measured using the BET multipoint method (N 2The measurements were performed in accordance with the gas adsorption method. The instruments used for the measurements were "3Flex" (manufactured by Micromeritics) and "Smart VacPrep (pretreatment device)" (manufactured by Micromeritics). The cellulose particles prepared in the test examples and comparative examples were degassed (dried under reduced pressure) at 60°C for 20 hours in the pretreatment device, and then dried under reduced pressure with N 2 The specific surface area was measured by a gas adsorption method. The equipment used to measure the average particle size, median size, cumulative 10% size, and cumulative 90% size was a "laser diffraction / scattering type particle size distribution measuring device (particle size distribution) LA-960V2 (dry measurement)" (manufactured by HORIBA).
[0114] The blending ratios of the raw materials for the test examples and comparative examples are shown in Table 1, and the physical properties are shown in Table 2.
[0115] [Table 1]
[0116] [Table 2]
[0117] (Emulsion test) The degree of emulsification of the produced cellulose particles was measured. Test examples and comparative examples were prepared at the blending ratios shown in Table 3.
[0118] [Table 3]
[0119] <Test Example 12> 0.3 parts by mass of emulsifier (Natural Cosmetics Research Institute product "Polysorbate 80") was added to 80 parts by mass of liquid paraffin, and the mixture was stirred at 3000 rpm for 30 seconds with a homogenizer (disperser, IKA "T-25", digital ULTRA-TURRAX (registered trademark)). 0.6 parts by mass of cellulose particles from Test Example 2 was then added, and the mixture was stirred at 5000 rpm for 30 seconds with the same homogenizer. 19.4 parts by mass of water was then added, and the mixture was stirred at 5000 rpm for 30 seconds with the same homogenizer to obtain Test Example 12.
[0120] <Comparative Example 12> 0.3 parts by mass of emulsifier was added to 80 parts by mass of liquid paraffin, and the mixture was stirred with a homogenizer at 3,000 rpm for 30 seconds. Then, 0.6 parts by mass of cellulose particles of Comparative Example 2 was added, and the mixture was stirred with the same homogenizer at 5,000 rpm for 30 seconds. Then, 19.4 parts by mass of water was added, and the mixture was stirred with the same homogenizer at 5,000 rpm for 30 seconds to obtain Comparative Example 12.
[0121] <Comparative Example 13> 0.3 parts of emulsifier was added to 80 parts by mass of liquid paraffin, and the mixture was stirred with a homogenizer at 3000 rpm for 30 seconds. Then, 20 parts by mass of a 3% aqueous dispersion (solid content 0.6 parts by mass) of unmodified fine fibrous cellulose (ELLEX (registered trademark)-S product manufactured by Daio Paper Co., Ltd.) was added, and the mixture was stirred with the same homogenizer at 5000 rpm for 30 seconds to obtain Comparative Example 13.
[0122] <Comparative Example 14> 0.3 parts by mass of emulsifier was added to 80 parts by mass of liquid paraffin and stirred with a homogenizer at 3000 rpm for 30 seconds, after which 20 parts by mass of water was added and stirred with the same homogenizer at 5000 rpm for 30 seconds to obtain Comparative Example 14.
[0123] The obtained Test Example and Comparative Example were transferred to a stoppered bottle, stirred, and then allowed to stand for 30 minutes, after which the state of the dispersion was observed. The results are shown in Figure 7. Test Example 12 and Comparative Example 13 maintained the emulsion state, and no interface was observed. Comparative Example 12 and Comparative Example 14 separated into liquid paraffin and water, and interface 10 was observed.
[0124] Both Test Example 12 and Comparative Example 12 are cellulose particles, but there are differences in bulk density and specific surface area, and these differences are presumed to be factors that affect emulsification.
[0125] (Dispersibility Test 1) In dispersibility test 1, the degree of dispersibility of the produced cellulose particles was measured. The test examples and comparative examples were prepared at the blending ratios shown in Table 4. The obtained test examples and comparative examples were dispersed in a homogenizer (IKA "T-25") at 8000 rpm for 1 minute to prepare a dispersion. After dispersion, the particles were transferred to a stoppered bottle and allowed to stand for 20 minutes, at which point the dispersed state was photographed, as shown in FIG. 8. In the figure, the reference numeral 20 denotes the interface of the cellulose particles.
[0126] [Table 4]
[0127] <Test Example 21> Test Example 21 was obtained by adding 2 parts by mass of the cellulose particles of Test Example 1 to 98 parts by mass of dimethyl silicone oil.
[0128] <Test Example 24> Test Example 24 was obtained by adding 2 parts by mass of the cellulose particles of Test Example 4 to 98 parts by mass of dimethyl silicone oil.
[0129] <Comparative Example 22> Comparative Example 22 was obtained by adding 2 parts by mass of the cellulose particles of Comparative Example 2 to 98 parts by mass of dimethyl silicone oil.
[0130] In Test Examples 21 and 24, the interface 20 was shallower than in Comparative Example 22, and good dispersibility was exhibited.
[0131] (Dispersibility Test 2) In dispersibility test 2, the degree of dispersibility of the produced cellulose particles was measured. The test examples and comparative examples were prepared at the blending ratios shown in Table 5. The obtained test examples and comparative examples were dispersed in a homogenizer (IKA "T-25") at 8000 rpm for 1 minute to prepare a dispersion. After dispersion, the particles were transferred to a stoppered bottle and allowed to stand for 20 minutes, at which point the dispersed state was photographed, as shown in FIG. 9. In the figure, the reference numeral 20 denotes the interface of the cellulose particles.
[0132] [Table 5]
[0133] <Test Example 31> Test Example 31 was obtained by adding 2 parts by mass of the cellulose particles of Test Example 1 to 98 parts by mass of liquid paraffin.
[0134] <Test Example 34> Test Example 34 was obtained by adding 2 parts by mass of the cellulose particles of Test Example 4 to 98 parts by mass of liquid paraffin.
[0135] <Comparative Example 32> Comparative Example 32 was obtained by adding 2 parts by mass of the cellulose particles of Comparative Example 2 to 98 parts by mass of liquid paraffin.
[0136] In Test Examples 31 and 34, no interface 20 was observed, whereas in Comparative Example 32, an interface 20 was observed, with Test Examples 31 and 34 exhibiting better dispersibility.
[0137] (others) Unless otherwise specified, the JIS, TAPPI and other tests and measurement methods shown in the above specification are performed at room temperature, particularly 25°C, and at atmospheric pressure, particularly 1 atm. [Industrial Applicability]
[0138] The cellulose particles and cellulose particle dispersion of the present invention can be provided as particles having improved dispersibility in oil-based liquids. [Explanation of symbols]
[0139] 11 Cellulose particles 11a Pore of cellulose particles 12 Cellulose particles 12a Pore of cellulose particles 10 Interface 20 Interface
Claims
1. A cellulose particle formed by agglomerating fine fibrous cellulose having an average fiber diameter of 1 to 1000 nm, The packed bulk density is 0.1 to 200 mg / cm 3 ; The fine fibrous cellulose is made from bleached hardwood kraft pulp (LBKP) or bleached softwood kraft pulp (NBKP) as a raw material pulp, The water retention of the fine fibrous cellulose is 100 to 500%. A cellulose particle characterized by:
2. A freeze-dried particle. The cellulose particles according to claim 1.
3. The fine fibrous cellulose is a modified fine fibrous cellulose in which a phosphite ester group is introduced into a hydroxy group of a cellulose fiber. The cellulose particles according to claim 1.
4. A cellulose particle dispersion in which the cellulose particles according to any one of claims 1 to 3 are dispersed in an oil component.
5. The cellulose particle dispersion according to claim 4, comprising 0.1 to 20% by mass of the cellulose particles according to any one of claims 1 to 3.