Siloxane dispersion cross-linked separator

JP2024107173A5Active Publication Date: 2024-11-22ASAHI KASEI BATTERY SEPARATOR CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024092285
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-17
Filing Date
2024-06-06
Publication Date
2024-11-22
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing battery separators for lithium-ion secondary batteries face challenges in ensuring safety, longevity, and uniformity of the solid electrolyte interface (SEI) layer formation, leading to uneven stress distribution, non-uniform deformation, and reduced cycle characteristics, especially in larger batteries with varying temperatures and electrode materials like silicon-containing and nickel oxide.

Method used

A separator for non-aqueous secondary batteries is designed with specific configurations, including silicon-containing molecules dispersed uniformly, controlled Voronoi areas, and silane-modified polyethylene, which promotes uniform SEI layer formation and cross-linking, enhancing ion flow and mechanical stability.

Benefits of technology

The solution achieves improved safety, cycle characteristics, and longevity by ensuring uniform ion flow, reducing thermal deformation, and maintaining mechanical integrity, particularly in large batteries with varying temperatures and electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a separator for a nonaqueous secondary battery that can achieve both safety and a long life for the nonaqueous secondary battery, and a method for manufacturing the same, or a nonaqueous secondary battery including the same.SOLUTION: A separator for a nonaqueous secondary battery includes a polyethylene microporous membrane, and has an air permeability change ratio (air permeability Sh after compression / air permeability Sj before compression) of 1.1 to 7.0 times when compressed by 30% of its thickness.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for a nonaqueous secondary battery, and a method for producing the same, or a nonaqueous secondary battery including the same. [Background technology]

[0002] Microporous membranes are widely used as separation or permselective separation membranes for various substances, separators, etc., and examples of their applications include microfiltration membranes, separators for fuel cells and capacitors, base materials for functional membranes in which functional materials are filled into the pores to exhibit new functions, battery separators, etc. Among these, polyolefin microporous membranes are preferably used as separators for lithium ion batteries, which are widely used in electric vehicles, notebook personal computers, mobile phones, digital cameras, etc.

[0003] To ensure the safety of batteries, battery separators are required to have both a shutdown function and an increased membrane rupture temperature.

[0004] Furthermore, in order to ensure the safety and cycle characteristics of batteries, battery separators are required to have improved mechanical strength, a shutdown function, and improved membrane rupture temperature, etc. From the viewpoint of imparting functionality to battery separators, the inclusion of modified polyolefins in microporous membranes, the crystal structure of the resin that constitutes the microporous membrane, and coating of resin or inorganic-containing slurry on the microporous membrane are being considered.

[0005] For example, it has been proposed to incorporate inorganic particles and a polyolefin resin into a microporous polyolefin film that can be used as a separator for lithium ion batteries (Patent Document 1).

[0006] Furthermore, from the viewpoint of improving safety by introducing a higher-order structure such as a silane crosslinked structure into a polyolefin microporous membrane, a battery separator in which a silane crosslinking reaction is initiated within the battery (Patent Document 2) and a polyolefin microporous membrane having a sea-island structure obtained by blending a silane-modified polyethylene with a medium molecular weight polyethylene (Patent Document 3) have been proposed.

[0007] Patent Document 2 also describes incorporating a silane-modified polyolefin or the like into a polyolefin microporous membrane, and disposing an inorganic porous layer containing inorganic particles and a resin binder on at least one side of the polyolefin microporous membrane.

[0008] For example, in the manufacturing process of a silane-crosslinkable polyolefin separator described in Patent Document 4, the carbon numbers of the repeating units derived from ethylene, the repeating units derived from olefins other than ethylene, and the branched chains of the repeating units derived from olefins other than ethylene of the silane-modified polyolefin are investigated.

[0009] For example, a polyolefin microporous film containing a silane-modified polyolefin or the like has been investigated for its polyethylene crystallinity, polyethylene crystallite size, and cross-sectional crystal orientation measured by X-ray diffraction (XRD) (Patent Document 5). In addition, the crystal long period measured by small-angle X-ray scattering (SAXS) for a polyolefin microporous film (Patent Document 6) and an oriented polypropylene film (Patent Document 7) has also been investigated.

[0010] Patent Document 8 examines the film thickness of a stretched polyethylene film and the area ratio R=I(110) / (I(110)+I(200)), which is expressed by the area I(110) of the diffraction peak of the (110) plane when irradiated with X-rays in the film thickness direction and the area I(200) of the diffraction peak of the (200) plane when irradiated with X-rays in the film thickness direction, and describes coating an aramid resin or the like on the stretched polyethylene film.

[0011] In addition, Non-Patent Document 1, for example, discusses a synthetic scheme for converting a tetracoordinated allylsilane into a pentacoordinated allylsilicate. Non-Patent Document 1 describes that a low-molecular-weight organic Si compound forms a high-order coordination complex in the presence of an alkali metal fluoride, and Si not only exhibits Lewis acid properties, but also has a high affinity with oxygen, so that the compound can take a structure in which an unshared electron pair of an oxygen compound is coordinated, and thus an electron addition reaction from the β-position of the high-order coordination complex is promoted due to thermodynamic stabilization caused by the influence of stereoregularity.

[0012] Non-Patent Document 2 describes that in a battery using a Si-containing negative electrode active material, as lithium ions are charged to and discharged from the Si-containing particles, the volume of the Si-containing negative electrode active material greatly expands or contracts. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] International Publication No. 2008 / 035674 [Patent Document 2] International Publication No. 2020 / 075866 [Patent Document 3] International Publication No. 2020 / 040389 [Patent Document 4] Korean Patent Publication No. 10-2020-0078407 [Patent Document 5] International Publication No. 2020 / 067161 [Patent Document 6] International Publication No. 2014 / 175252 [Patent Document 7] International Publication No. 2015 / 012324 [Patent Document 8] Patent No. 6012839 [Non-patent literature]

[0014] [Non-Patent Document 1] "Special Feature: Silicone Polymers, Organosilicon Chemistry" Journal of the Society of Rubber Science and Technology, Japan, Vol. 62, No. 12 (1989) [Non-Patent Document 2] "Volume Expansion during Lithiation of Amorphous Silicon Thin Film Electrodes Studied by In-Operando Neutron Reflectometry" J.Phys.Chem. C2014,118,9395-9399 [Non-Patent Document 3] "Near-Shore Aggregation Mechanism of Electrolyte Decomposition Products to Explain Solid Electrolyte Interphase Formation" J. Electrochem. Soc.C2015, 162, 2670-2678 [Non-Patent Document 4] "Coupled LiPF6 Decomposition and Carbonate Dehydrogenation Enhanced by Highly Covalent Metal Oxides in High-Energy Li-Ion Batteries" J. Phys. Chem. C2018, 122, 48, 27368-27382 Summary of the Invention [Problem to be solved by the invention]

[0015] In recent years, the output and energy density of lithium-ion secondary batteries for mobile devices or vehicles have been increasing, while there is a demand for smaller battery cells and stable cycle performance or improved productivity during long-term use. Furthermore, the required battery safety standards are stricter than those of conventional products, so there is room for improvement in the battery separators described in Patent Documents 1 to 4 in terms of achieving a long battery life while ensuring battery safety. There is room for improvement in the battery separators described in Patent Documents 2, 5 to 8 in terms of ensuring productivity, improving battery safety, extending battery life, and / or achieving a balance between them.

[0016] It is generally known that SFC (SEI film components) formed on the surface of the positive electrode material aggregate and accumulate on the surface of the negative electrode material, forming a solid electrolyte interface (SEI) layer that covers the surface of the negative electrode material (Non-Patent Document 3). The SEI layer prevents the decomposition of the electrolyte on the electrode surface to suppress battery deterioration, while also allowing lithium ions (Li + ) movement and increase the internal resistance. In addition, the generation of SFC depends on temperature, and the higher the temperature, the thicker the SEI layer is formed. For example, when a battery is enlarged to improve the energy density of the battery or to increase the output, the temperature of the center of the battery tends to be higher than that of the outside due to the difference in heat dissipation capacity between the center and the outside of the battery, and the generation of SFC is prominent near the center of the battery. If the dispersion of SFC is insufficient, a non-uniform SEI layer is formed, and the cycle test capacity retention rate decreases due to the Li ions being confined in the SEI layer. As a method for enlarging the size of a battery, for example, there is a method of increasing the diameter and length of the battery, and it is possible to use a 4680-type cylindrical battery instead of the 18650-type cylindrical battery that is currently widely used. In addition, in a battery that uses a positive electrode material containing nickel oxide, the energy density can be improved by increasing the nickel (Ni) content, but as described in Non-Patent Document 4, the oxidation potential is lowered and the generation of SFC is promoted, so if the diffusion of SFC is insufficient, a non-uniform SEI layer tends to be formed.

[0017] In addition, in lithium-ion secondary batteries, the volume of the electrodes changes and the temperature inside the battery rises during charging and discharging. The volume change of the electrodes generates a non-uniform stress distribution inside the battery. When the temperature inside the battery rises in a state where non-uniform stress distribution has occurred, the separator deforms non-uniformly due to a phenomenon in which resin to which stress is applied at high temperatures gradually deforms (thermal creep), and the separator's microporous structure is non-uniformly crushed. This causes the flow of lithium ions to be partially blocked during charging and discharging, resulting in a decrease in cycle characteristics. Furthermore, lithium ions move non-uniformly in and out of the negative electrode, causing lithium dendrites to grow, which in turn deteriorates the cycle characteristics and the crush test pass rate. In particular, in cylindrical and prismatic batteries, the tightening of the winding that occurs during the winding process and changes over time is likely to cause non-uniform stress distribution inside the battery, which is likely to deteriorate the cycle characteristics and the crush test pass rate.

[0018] As described above, the SEI layer suppresses the decomposition of the electrolyte and suppresses battery deterioration, but if it is formed excessively, it increases the internal resistance of the battery and accumulates Li ions in the electrolyte, which deteriorates the cycle characteristics. Therefore, it is preferable that an SEI layer of appropriate thickness is formed uniformly. The separator is deformed unevenly, and the microporous structure of the separator is crushed unevenly, which partially inhibits the flow of the decomposition products of the electrolyte. This causes the SEI layer to be formed unevenly and the cycle characteristics to deteriorate. In particular, by enlarging the battery, it is possible to increase the output and improve the energy density, but the stress difference generated in the battery also becomes larger, making it easier for the separator to deform unevenly. Furthermore, the larger the battery, the greater the temperature difference between the center side and the outer edge side of the battery due to the difference in heat dissipation capacity. This makes it easier for thermal deformation of the electrodes, thermal shrinkage of the separator, thermal creep, etc. to occur, which in turn makes the stress difference generated in the battery larger, and the above mechanism makes it easier for the cycle characteristics to deteriorate and the safety to decrease in the crushing test to occur. Examples of large batteries include 4680-type cylindrical batteries and large prismatic batteries.

[0019] In addition, although the energy density can be improved in batteries using silicon-containing negative electrode materials, the expansion rate of the negative electrode material during charging and discharging is large, which tends to cause non-uniform deformation of the separator, and the microporous structure of the separator tends to be non-uniformly crushed. In turn, the above mechanism causes deterioration of cycle characteristics and reduced safety in crushing tests. Furthermore, in batteries using positive electrode materials containing nickel oxide, while the energy density can be improved, decomposition of the electrolyte tends to progress on the electrode surface, and SFC is likely to be generated non-uniformly. If the SFC reaches the negative electrode surface without being sufficiently diffused, a non-uniform SEI layer is likely to be formed, and cycle characteristics are likely to deteriorate. Examples of positive electrode materials containing nickel oxide include NMC111, NMC611, and NMC811.

[0020] In view of the above problems, an object of the present invention is to provide a separator for a nonaqueous secondary battery that can achieve both safety and long life for the nonaqueous secondary battery, and a method for producing the same, or a nonaqueous secondary battery including the same. [Means for solving the problem]

[0021] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by using a separator for a nonaqueous secondary battery having the following configuration, a method for producing the same, or a nonaqueous secondary battery including the same, and have completed the present invention. One example of the aspects of the present invention is as follows. (1) A non-aqueous secondary battery separator comprising a silicon (Si)-containing molecule, The Voronoi area (mu) of the maximum frequency among the Voronoi polygons obtained by performing Voronoi division on a Si-containing image detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS) measurement of the nonaqueous secondary battery separator is 1.0 μm 2 ~17.5μm 2 and The spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by the TOF-SIMS measurement is 0.5 μm 2 ~8.5μm 2 A separator for a non-aqueous secondary battery, the separator being within the range of 100%. (2) The separator for a nonaqueous secondary battery according to item 1, wherein the ratio (σ / mu) of the spread (σ) of the Voronoi area frequency distribution to the Voronoi area (mu) of the maximum frequency is 0.06 to 0.70. (3) A non-aqueous secondary battery separator including a silicon (Si)-containing molecule, The Voronoi area (mu) of the maximum frequency among the Voronoi polygons obtained by performing Voronoi division on the Si-containing image detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS) measurement of the nonaqueous secondary battery separator is 6.0 μm 2 ~12.0μm 2 A separator for a non-aqueous secondary battery, the separator being within the range of 100%. (4) The spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by the TOF-SIMS measurement is 2.0 μm 2 ~4.0μm 2 4. The separator for a non-aqueous secondary battery according to item 3, wherein the non-aqueous secondary battery separator is within the range of (5) The separator for a nonaqueous secondary battery according to item 3 or 4, wherein the ratio (σ / mu) of the spread (σ) of the Voronoi area frequency distribution to the Voronoi area of ​​maximum frequency (mu) is 0.20 to 0.40. (6) The nonaqueous secondary battery separator according to any one of items 1 to 5, wherein the Si-containing molecules are dispersed in a state other than a sea-island structure. (7) The nonaqueous secondary battery separator is a polyethylene microporous membrane, and 7. The separator for a nonaqueous secondary battery according to any one of items 1 to 6, wherein the air permeability change ratio (air permeability Sh after compression / air permeability Sj before compression) when compressed by 30% of the thickness is 1.1 to 7.0 times. (8) A non-aqueous secondary battery separator including a polyethylene microporous membrane, A separator for a non-aqueous secondary battery, in which the rate of change in air permeability when compressed by 30% of its thickness (air permeability Sh after compression / air permeability Sj before compression) is 1.1 to 7.0 times. (9) The separator for a nonaqueous secondary battery according to item 8, comprising a silane-modified polyethylene and a polyolefin other than the silane-modified polyethylene. (10) A separator for a nonaqueous secondary battery comprising a silane-modified polyolefin, the separator for a nonaqueous secondary battery comprising a polyethylene having a crystal long period of 20 to 50 nm as measured by small-angle X-ray scattering, a degree of crystallinity of 60% to 80% as measured by wide-angle X-ray scattering, and a polyethylene crystallite size (110) of 10 to 50 nm as measured by wide-angle X-ray scattering. (11) The crystal long period of polyethylene detected by the small angle X-ray scattering measurement and the crystallinity detected by the wide angle X-ray scattering measurement are calculated using the following formula: Formula: Amorphous thickness [nm] = (Crystal long period [nm]) × (1-Crystallinity [%] / 100) 11. The separator for a nonaqueous secondary battery according to item 10, wherein the amorphous portion has a thickness calculated by the above formula (1) is 3 to 23 nm. (12) The separator for a nonaqueous secondary battery according to item 10 or 11, wherein the polyethylene has a cross-sectional crystal orientation degree of 0.70 to 0.99 as measured in MD and a cross-sectional crystal orientation degree of 0.70 to 0.99 as measured in TD by wide-angle X-ray scattering measurement. (13) The separator for a nonaqueous secondary battery according to any one of items 10 to 12, wherein a ratio (MD / TD) of a cross-sectional crystal orientation degree of the polyethylene measured in the MD direction to a cross-sectional crystal orientation degree of the polyethylene measured in the TD direction is 0.5 to 1.2. (14) The separator for a nonaqueous secondary battery according to any one of items 10 to 13, wherein a ratio (110) / (200) of a crystallite size (110) of the polyethylene to a crystallite size (200) of the polyethylene, as detected by wide-angle X-ray scattering measurement, is 0.9 to 2.0. (15) The separator for a nonaqueous secondary battery according to any one of items 10 to 14, wherein the silane-modified polyolefin is a silane-modified polyethylene. (16) The separator for a nonaqueous secondary battery according to any one of items 10 to 15, wherein in the functional group containing silicon (Si) of the silane-modified polyolefin, the number of methylenes (CH2) constituting the linking portion of the organic moiety to the main chain is 2 to 10. (17) The separator for a nonaqueous secondary battery according to any one of items 10 to 16, comprising: a polyolefin microporous membrane as a substrate; and an inorganic porous layer containing inorganic particles and a resin binder, laminated on at least one surface of the polyolefin microporous membrane. (18) The separator for a nonaqueous secondary battery according to item 17, wherein the content of the inorganic particles contained in the inorganic porous layer is 5% by mass to 99% by mass based on the total mass of the inorganic porous layer. (19) The nonaqueous secondary battery separator according to item 17 or 18, wherein the inorganic particles are at least one selected from the group consisting of alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, iron oxide, silicon nitride, titanium nitride, boron nitride, silicon carbide, aluminum oxide hydroxide, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, diatomaceous earth, silica sand, and glass fiber. (20) The separator for a nonaqueous secondary battery according to any one of items 10 to 16, comprising a polyolefin microporous membrane as a substrate and a thermoplastic polymer-containing layer formed on at least one surface of the polyolefin microporous membrane, wherein the thermoplastic polymer contained in the thermoplastic polymer-containing layer contains at least one of a polymerization unit of a (meth)acrylic acid ester and / or a (meth)acrylic acid, polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE). (21) The separator for a nonaqueous secondary battery according to any one of Items 10 to 16, comprising a polyolefin microporous membrane as a substrate and an active layer disposed on at least one surface of the polyolefin microporous membrane, the active layer containing at least one fluorine-containing polyvinyl compound selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE), and inorganic particles. (22) The separator for a nonaqueous secondary battery according to any one of items 10 to 16, comprising: a polyolefin microporous membrane as a substrate; and a heat-resistant resin layer containing a heat-resistant resin laminated on at least one surface of the polyolefin microporous membrane, wherein the heat-resistant resin contains at least one selected from the group consisting of wholly aromatic polyamide, polyimide, polyamideimide, polysulfone, polyketone, polyether, polyetherketone, polyetherimide, and cellulose. (23) The separator for a nonaqueous secondary battery according to item 22, wherein the heat-resistant resin layer contains 30% by mass to 90% by mass of an inorganic filler having an average particle size of 0.2 μm to 0.9 μm. (24) The separator for a nonaqueous secondary battery according to any one of items 10 to 23, further comprising a polyolefin other than the silane-modified polyolefin. (25) For a Si-containing image of the nonaqueous secondary battery separator detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS), the Voronoi area (mu) of the Voronoi polygon with the highest frequency obtained by Voronoi division is 6.00 μm 2 ~12.00μm 2 25. The separator for a nonaqueous secondary battery according to any one of items 10 to 24, wherein the range is: (26) The spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by the TOF-SIMS measurement is 2.00 μm 2 ~4.00μm 2 26. The separator for a non-aqueous secondary battery according to item 25, wherein the non-aqueous secondary battery separator is within the range of (27) The separator for a nonaqueous secondary battery according to item 25 or 26, wherein a ratio (σ / mu) of the spread (σ) of the Voronoi area frequency distribution to the Voronoi area (mu) of the maximum frequency is 0.20 to 0.40. (28) A nonaqueous secondary battery comprising: a positive electrode; a negative electrode; the separator for a nonaqueous secondary battery according to any one of items 1 to 27; and a nonaqueous electrolyte. (29) The positive electrode has the formula: Li-Ni x -Mn y -Co z 29. The nonaqueous secondary battery according to item 28, comprising a lithium (Li)-nickel (Ni)-manganese (Mn)-cobalt (Co) composite oxide represented by the formula: {wherein x represents a Ni proportion, y represents a Mn proportion, z represents a Co proportion, and x+y+z=1}, wherein the Ni proportion x in the formula is 5 to 9. (30) The nonaqueous secondary battery according to item 28 or 29, wherein the negative electrode contains a negative electrode active material, and a proportion of Si in the negative electrode active material is 5% by weight to 90% by weight. (31) The nonaqueous secondary battery according to any one of items 28 to 30, wherein the nonaqueous electrolyte solution contains a lithium salt at a concentration in the range of 1.2 mol / L to 10 mol / L. (32) The nonaqueous secondary battery according to any one of items 28 to 31, wherein the nonaqueous electrolyte solution contains ethyl methyl carbonate (EMC) and / or acetonitrile (AcN), and the total content of EMC and AcN in the nonaqueous electrolyte solution is within a range of 50% by mass to 90% by mass. (33) The process of: (1) a sheet forming step of extruding the silane-modified polyolefin, polyethylene and plasticizer into a sheet using an extruder, cooling and solidifying the extruded material, and processing the extruded material into a sheet-like molded product; (2) a stretching step of biaxially stretching the sheet-like molded product at an areal magnification of 20 to 250 times to form a stretched product; (3) a porous body forming step of extracting the plasticizer from the stretched material to form a porous body; (4) a heat treatment step of subjecting the porous body to a heat treatment, stretching and relaxing in the width direction to obtain a heat-treated porous body; (5A) a coating step of applying a coating liquid containing the inorganic particles, the resin binder, and a surfactant and having a pH of 6.7 or less or 7.5 or more to at least one surface of the heat-treated porous body, thereby forming the inorganic porous layer on at least one surface of the heat-treated porous body; (6) a drying step of drying and removing the solvent in the inorganic porous layer; and (7) an assembly step of housing the laminate or the wound body of the electrodes and the nonaqueous secondary battery separator, and the nonaqueous electrolyte solution in an exterior case; and wherein the silane-modified polyolefin forms a crosslinked structure in at least one of steps (5A), (6) and (7). (34) The process of: (1) a sheet forming step of extruding the silane-modified polyolefin, polyethylene and plasticizer into a sheet using an extruder, cooling and solidifying the extruded material, and processing the extruded material into a sheet-like molded product; (2) a stretching step of biaxially stretching the sheet-like molded product at an areal magnification of 20 to 250 times to form a stretched product; (3) a porous body forming step of extracting the plasticizer from the stretched material to form a porous body; (4) a heat treatment step of subjecting the porous body to a heat treatment, stretching and relaxing in the width direction to obtain a heat-treated porous body; (5B) a coating step of applying a coating liquid containing the thermoplastic polymer and a surfactant and having a pH of 6.7 or less or 7.5 or more to at least one surface of the heat-treated porous body, thereby forming the thermoplastic polymer-containing layer on at least one surface of the heat-treated porous body; (6) a drying step of drying and removing the solvent in the thermoplastic polymer-containing layer; and (7) an assembly step of housing the laminate or the wound body of the electrodes and the nonaqueous secondary battery separator, and the nonaqueous electrolyte solution in an exterior case; and wherein the silane-modified polyolefin forms a crosslinked structure in at least one of steps (5B), (6) and (7). (35) The process of: (1) a sheet forming step of extruding the silane-modified polyolefin, polyethylene and plasticizer into a sheet using an extruder, cooling and solidifying the extruded material, and processing the extruded material into a sheet-like molded product; (2) a stretching step of biaxially stretching the sheet-like molded product at an areal magnification of 20 to 250 times to form a stretched product; (3) a porous body forming step of extracting the plasticizer from the stretched material to form a porous body; (4) a heat treatment step of subjecting the porous body to a heat treatment, stretching and relaxing in the width direction to obtain a heat-treated porous body; (5C) a coating step of forming the active layer on at least one surface of the heat-treated porous body by applying a coating liquid containing the fluorine atom-containing polyvinyl compound, the inorganic particles, and an organic solvent onto at least one surface of the heat-treated porous body; (6) a drying step for drying and removing the solvent in the active layer; and (7) an assembly step of housing the laminate or the wound body of the electrodes and the nonaqueous secondary battery separator, and the nonaqueous electrolyte solution in an exterior case; and wherein the silane-modified polyolefin forms a crosslinked structure in at least one of steps (5C), (6) and (7). (36) Between the coating step (5C) and the drying step (6), the following steps are carried out: (5.5C) a water washing step of replacing the organic solvent in the active layer with an aqueous solvent; and wherein the silane-modified polyolefin forms a crosslinked structure in the step (5.5C). (37) The process of: (1) a sheet forming step of extruding the silane-modified polyolefin, polyethylene and plasticizer into a sheet using an extruder, cooling and solidifying the extruded material, and processing the extruded material into a sheet-like molded product; (2) a stretching step of biaxially stretching the sheet-like molded product at an areal magnification of 20 to 250 times to form a stretched product; (3) a porous body forming step of extracting the plasticizer from the stretched material to form a porous body; (4) a heat treatment step of subjecting the porous body to a heat treatment, stretching and relaxing in the width direction to obtain a heat-treated porous body; (5D) a coating step of applying a coating liquid containing the heat-resistant resin and an organic solvent onto at least one surface of the heat-treated porous body to form the heat-resistant resin layer on at least one surface of the heat-treated porous body; (6) a drying step of drying and removing the solvent in the heat-resistant resin layer; and (7) an assembly step of housing the laminate or the wound body of the electrodes and the nonaqueous secondary battery separator, and the nonaqueous electrolyte solution in an exterior case; and wherein the silane-modified polyolefin forms a crosslinked structure in at least one of steps (5D), (6), and (7). (38) Between the coating step (5D) and the drying step (6), the following steps are carried out: (5.5D) a water washing step of replacing the organic solvent in the heat-resistant resin layer with an aqueous solvent; and wherein the silane-modified polyolefin forms a crosslinked structure in the step (5.5D). Effect of the Invention

[0022] According to the present invention, it is possible to achieve both safety and long life for a nonaqueous secondary battery including a separator for a nonaqueous secondary battery. More specifically, it is possible to improve, for example, safety in a nail penetration test and a hotbox test, cycle characteristics including low-temperature cycle characteristics and high-temperature cycle characteristics, and productivity. [Brief description of the drawings]

[0023] [Figure 1] 4 is an image showing the results of TOF-SIMS analysis of the separator according to Example 1. [Diagram 2] 1 is an example of a filter three-dimensional image in image processing of a TOF-SIMS spectrum in Example 1. [Diagram 3]1 is an example of a two-dimensional filtered image in image processing of a TOF-SIMS spectrum in Example 1. [Figure 4] 1 is an example of a state in which image processing (1) and (2) are performed on the TOF-SIMS spectrum of Example 1. [Diagram 5] 1 shows an example of a state in which image processing (1) to (6) have been performed on the TOF-SIMS spectrum of Example 1. [Figure 6] 1 shows an example of a Voronoi region obtained by Voronoi division of a TOF-SIMS spectrum in Example 1. [Figure 7] 1 shows an example of a Voronoi area determined to be effective from the results of Example 1. [Figure 8] 1 is a histogram of Voronoi areas in the first embodiment. [Figure 9] 13 is a histogram after the Voronoi area in the first embodiment is converted into an actual area. [Figure 10] 13 is an example illustrating a fitting result of the Voronoi area in the first embodiment. [Figure 11] 1 is an image showing the results of TOF-SIMS analysis of the separator according to Comparative Example 1. [Figure 12] 1 is an example of a state in which image processing (1) and (2) are performed on the TOF-SIMS spectrum of Comparative Example 1. [Figure 13] 1 is an example of a state in which image processing (1) to (6) are performed on the TOF-SIMS spectrum of Comparative Example 1. [Figure 14] 1 illustrates an example of a Voronoi region obtained by Voronoi division of the TOF-SIMS spectrum of Comparative Example 1. [Figure 15] 13 shows an example of a Voronoi area determined to be effective from the results of Comparative Example 1. [Figure 16] 13 is a histogram of Voronoi areas in Comparative Example 1. [Figure 17] 13 is a histogram after the Voronoi area in Comparative Example 1 is converted into an actual area. [Figure 18] 13 is an example illustrating a fitting result of the Voronoi area in Comparative Example 1. [Figure 19] FIG. 2 is a schematic diagram illustrating a repeating periodic structure of crystalline portions and amorphous portions in a separator using a crystalline resin such as polyethylene, and a partially enlarged view thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, the form for carrying out the present invention (hereinafter, simply referred to as "embodiment") will be described in detail. The present invention is not limited to the following embodiment, and various modifications are possible within the scope of the gist of the present invention. In this specification, the numerical range described using "~" includes the numerical values ​​described before and after it. The abbreviation "MD" refers to the longitudinal direction of the battery wound body when continuously forming the separator, and is an abbreviation for Machine Direction. The abbreviation "TD" refers to the direction crossing the MD at an angle of 90° (hereinafter, also referred to as the width direction), and is an abbreviation for Transverse Direction. The various measurement methods and evaluation methods described below are performed according to the methods described in the examples, unless otherwise specified.

[0025] <Separator for non-aqueous secondary batteries> A separator for a non-aqueous secondary battery (hereinafter, also simply referred to as "separator") is required to have insulation properties and ion permeability, and is generally formed from an insulating material having a porous structure, such as paper, a polyolefin nonwoven fabric, or a resin microporous membrane. In particular, as a separator substrate used in a non-aqueous secondary battery having a positive electrode and a negative electrode capable of absorbing and releasing lithium, and a non-aqueous electrolyte solution obtained by dissolving an electrolyte in a non-aqueous solvent, a polyolefin microporous membrane that has oxidation-reduction resistance and can construct a dense and uniform porous structure is excellent. Therefore, the separator for a non-aqueous secondary battery may include a polyolefin microporous membrane. If desired, the separator for a non-aqueous secondary battery may include, in addition to the polyolefin microporous membrane, a layer formed on one or both sides thereof, such as a thermoplastic polymer-containing layer, an active layer, an inorganic porous layer, or a heat-resistant resin layer.

[0026] <Embodiment 1: Silicon-containing structure and Voronoi tessellation of separator (1)> The separator according to the first embodiment contains silicon (Si)-containing molecules, and the maximum frequency Voronoi area (mu) of the Voronoi polygons obtained by performing Voronoi division on a Si-containing image detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS) measurement of the separator is 1.0 μm 2 ~17.5μm 2 and the spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by TOF-SIMS measurement is within 0.5 μm 2 ~8.5μm 2 is within the range.

[0027] In the separator according to the first embodiment, when a TOF-SIMS measurement is performed on a 100 μm square area, at least one structure containing silicon is detected, and preferably, the Si-containing molecules are detected to be dispersed in the separator in a state other than a sea-island structure. Note that a sea-island structure is a structure in which a solid substance is broadly composed of two types, and one type (likened to islands) is discontinuously mixed in one that appears relatively continuous (likened to a sea).

[0028] In the first embodiment, various values ​​obtained by Voronoi tessellation are measured when the separator is a polyolefin microporous membrane, and can be indicators of the level of variation of the Si-containing molecules on the separator surface. TOF-SIMS measurement of the separator can be performed as described in the Examples with reference to Figures 1 to 6 and Figures 11 to 14, and Voronoi tessellation of TOF-SIMS images can be performed as described in the Examples with reference to Figures 7 to 10 and Figures 15 to 18.

[0029] The Voronoi area (mu) of the Voronoi polygon with the highest frequency obtained by the above Voronoi division is 1.0 μm 2 ~17.5μm 2Within this range, the Si-containing molecules are highly likely to be dispersed in the separator without forming an island structure. For example, in the case where the non-aqueous secondary battery is a lithium ion secondary battery, if a separator in which the Si element is uniformly dispersed coexists with a lithium (Li) complex solvated with an electrolyte having an unshared electron pair such as an oxygen atom, the following phenomena (a) and (b) may extend the product life in a cycle characteristic test of the battery: (a) Li complexes have a high probability of existing around dispersed Si atoms because they show high affinity with Si atoms. For this phenomenon, the reaction in which non-donor electron pairs in the molecular structure of the electrolyte are coordinated to Si atoms is important. As described in Non-Patent Document 1, Si atoms have a large atomic radius, so they can be coordinated four or more times, and have the special property that structures using four-electron three-center bonds and d-orbitals can exist. In other words, a path through which Li ions can easily flow uniformly is formed over the entire surface of the separator. Therefore, for example, when a secondary battery including a positive electrode such as an NMC positive electrode including a lithium (Li)-nickel (Ni)-manganese (Mn)-cobalt (Co) composite oxide is uniformly charged and discharged, crystal destruction tends to be suppressed; and (i) In addition, for example, when the negative electrode is a Si-containing negative electrode, the Si element in the negative electrode can be uniformly charged and discharged, and the uniform expansion and convergence of the Si-containing negative electrode can suppress deformation inside the secondary battery.

[0030] Although not wishing to be bound by theory, the above phenomena (a) and (b) are believed to occur in a non-aqueous secondary battery according to the following scheme 1: [ka] In the formula, Sol represents a non-aqueous solvent in the electrolyte, and X -represents a counter anion of a lithium salt as an electrolyte, an example of a non-aqueous solvent includes ethylene carbonate (EC), an example of a constituent resin of the separator according to embodiment 1 includes silane-modified polyethylene, and R represents, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, etc., or a siloxane bond crosslinked with a nearby silanol. As shown in Fig. 1, a complex is formed uniformly on the separator, and the Li + It is thought that this is also caused by the flow of ions becoming more uniform.

[0031] In a non-aqueous secondary battery system containing lithium hexafluorophosphate (LiPF6) as an electrolyte, due to the Jahn-Teller effect of phosphorus atoms, LiF exists in the system as a certain concentration of dissociated F anions or as lithium fluoride (LiF), and therefore when LiF is added to Si, it exhibits a stronger Lewis acid effect than before addition, which makes the above phenomena (a) and (b) more pronounced, and ultimately allows good low-temperature cycle characteristics to be exhibited. This was discovered by the present invention and is shown in Scheme 2 below: [ka] {In the formula, Sol represents a non-aqueous solvent in the electrolytic solution, an example of the non-aqueous solvent is ethylene carbonate (EC), an example of the electrolyte is LiPF6, an example of the constituent resin of the separator according to embodiment 1 is silane-modified polyethylene, and R represents, for example, H, Me, Et, Bu, or the like, or a siloxane bond crosslinked with a nearby silanol.} As shown in Fig. 1, physically solvated Li +This is believed to be because there is a high probability of the formation of a coordination complex in which the Si atom of the Si-containing molecule in the separator is stably coordinated to the Si atom of the Si-containing molecule in the separator's constituent polymer. This concept is specific to the amorphous structure obtained by forming a film from a polymer composition using Resin A and Resin B or C described below, and is a different approach from the Lewis acid property of Si in the coordination complex of a low-molecular-weight allylsilane compound as described in Non-Patent Document 1.

[0032] Furthermore, Si-containing molecules often have crosslinking properties. For example, when the Si-containing molecules have silane crosslinking properties, the silane crosslinking properties of the dispersed Si-containing molecules can be ensured even in a non-aqueous secondary battery, and the stability of the siloxane bonds can be ensured, and the crosslinked structure of the separator can be maintained for a long period of time, thereby ensuring safety in safety tests such as nail penetration tests. It is known that when a lithium-ion battery is charged and discharged, if the uneven flow of lithium ions moves at a slower rate than the intercalation reaction to the electrode, the lithium ions accumulate in the electrical retention area and form dendrites. In particular, when the battery is operated at low temperatures, the viscosity of the electrolyte increases, making it difficult for ions in the system to move, which tends to form dendrites, and there is a concern that the safety of the battery after low-temperature cycles will be significantly reduced. Such a phenomenon is a major issue when used in seasons and regions with large temperature differences, such as mobile device power sources and battery-powered automobile batteries. In the first embodiment, the separator is designed in which the Si-containing atoms are dispersed not in a sea-island structure (not in a matrix structure), thereby improving the uniformity of the lithium ion flow and solving the problem.

[0033] From the viewpoint of further improving the safety of the separator and the nonaqueous secondary battery including the separator, it is preferable that the separator includes, for example, a silane-modified polyethylene as a Si-containing molecule, and it is more preferable that a silane crosslinking reaction of the silane-modified polyethylene proceeds when the separator comes into contact with the electrolyte.

[0034] From the viewpoint of achieving both long life and safety in the cycle characteristics of the nonaqueous secondary battery and / or achieving a balance between them, the Voronoi area (mu) of the Voronoi polygon with the maximum frequency obtained by performing the Voronoi division is set to 1.5 μm 2 ~17.0μm 2 Preferably, the thickness is within the range of 4.0 μm. 2 ~16.0μm 2 More preferably, the range is 6.0 μm. 2 ~13.0μm 2 From the same viewpoint, it is more preferable that the spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by the above TOF-SIMS measurement is within the range of 0.5 μm 2 ~8.5μm 2 It is within the range of 1.7 to 6.3, and preferably within the range of 1.8 μm 2 ~4.2μm 2 It is more preferable that the ratio is in the range of 1.

[0035] Voronoi tessellation refers to dividing a number of points (kernel points) placed at any position in a certain metric space into regions based on which kernel points other points in the same space are closer to. A diagram containing the regions obtained in this way is called a Voronoi diagram. Generally, in a Voronoi diagram, the boundaries of multiple regions become part of the bisectors of each kernel point, and each region forms a polygon (Voronoi polygon).

[0036] When Voronoi division is performed on the observation field of view, any unclosed area is excluded from the Voronoi division. An example of an unclosed area is an area obtained by performing Voronoi division on an object when the object exists on the boundary of the observation field of view and the entire object is not observed. Therefore, in an image obtained by photographing at least a part of the separator surface, it is preferable to check whether the entire object is observed for an object located on the edge of the image.

[0037] For a Si-containing image detected by TOF-SIMS measurement, it is preferable that the ratio (σ / mu) of the spread (σ) of the Voronoi area frequency distribution to the Voronoi area (mu) of maximum frequency satisfies the following relationship. 0.06≦σ / mu≦0.70 In the first embodiment, the ratio (σ / mu) in the Voronoi division can be regarded as an index showing whether the Si-containing molecules are uniformly dispersed on the separator surface. When the ratio (σ / mu) is within the range of 0.06 to 0.70, the Si-containing molecules are uniformly dispersed on the separator surface, and in a non-aqueous secondary battery, the ratio (σ / mu) sufficiently contributes to the coexistence of the Li complex derived from the electrolyte and the separator, the silane crosslinking reaction of the separator, etc., and can extend the cycle product life of the battery. Although not wishing to be bound by theory, the concentration at which the intermediate in which the Li complex is coordinated in the separator surface exists, or the life of the intermediate in an equilibrium state, etc. are important, and in the first embodiment, it was experimentally discovered that the ratio (σ / mu) in the limited Voronoi division can uniformly contribute to the intercalation reaction into the electrode. From the viewpoint of further extending the cycle product life of the battery, the ratio (σ / mu) is preferably within the range of 0.07 to 0.57, and more preferably within the range of 0.19 to 0.38.

[0038] The numerical values ​​obtained by Voronoi tessellation of the separator according to embodiment 1 can be adjusted within the ranges described above by controlling, for example, the structure of the Si-containing molecule, the molecular weight or molecular weight distribution of the separator constituent raw materials, the blending range of the separator constituent raw materials, etc.

[0039] <Embodiment 2: Silicon-containing structure and Voronoi tessellation of separator (2)> The separator according to the second embodiment contains silicon (Si)-containing molecules, and the maximum frequency Voronoi area (mu) of the Voronoi polygons obtained by performing Voronoi division on the Si-containing image detected by TOF-SIMS measurement of the separator is 6.0 μm 2 ~12.0μm 2 is within the range.

[0040] When the separator according to the second embodiment is subjected to a TOF-SIMS measurement in a 100 mm square area, at least one structure containing silicon is detected, and preferably, it is detected that the Si-containing molecules are dispersed in the separator in a state other than a sea-island structure.

[0041] In the second embodiment, various numerical values ​​obtained by Voronoi tessellation are measured when the separator is a polyolefin microporous membrane, and can be indicators showing the level of variation of the Si-containing molecules on the separator surface.

[0042] The Voronoi area (mu) of the most frequent Voronoi polygon is 6.0μm 2 ~12.0μm 2 Within this range, as in the first embodiment, the Si-containing molecules tend to be dispersed in the separator in a state other than a sea-island structure, and the safety of the non-aqueous secondary battery having the separator is ensured while the cycle characteristics are extended. + The uniformity of ion flow, Lewis acid effect, or crosslinking of Si-containing molecules ensures low-temperature cycle characteristics and safety in nail penetration tests. In addition, in the second embodiment, when the separator in which Si elements are uniformly dispersed coexists with oligomers (SFC: SEI film components) generated by a chemical reaction of the electrolyte on the surface of the positive electrode material, as shown in the following scheme 3, the unshared electron pair of oxygen in the molecular structure of SFC can be coordinated to the Si atom, and SFC shows affinity with the Si atom, improving the diffusivity of SFC. [ka] In the formula, Sol represents a non-aqueous solvent in the electrolyte, and X -represents the counter anion of the lithium salt as an electrolyte. As an example, the right side shows a case where the non-aqueous solvent is ethylene carbonate (EC), SFC is an oligomer produced by the reduction polymerization of two EC molecules, and the constituent resin of the separator contains silane-modified polyethylene. R represents, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, etc., or a siloxane bond crosslinked with a nearby silanol.}

[0043] In the second embodiment, the Voronoi area (mu) of the separator is 6.0 μm 2 ~12.0μm 2 If the voronoi area of ​​the separator is within this range, the Si-containing molecules are finely and uniformly dispersed in the separator, so that the SFC is uniformly dispersed throughout the separator as shown in Scheme 3, and an SEI layer having a uniform thickness sufficient to suppress the decomposition of the electrolyte is uniformly formed on the negative electrode, which is believed to improve the cycle test capacity retention rate. If the voronoi area of ​​the separator is too large (i.e., the distance between the Si-containing molecules is too large), the diffusibility of the SFC is insufficient, a non-uniform SEI layer is easily formed, and the cycle test capacity retention rate is deteriorated. On the other hand, even if the voronoi area is too small (i.e., the distance between the Si atoms is too small), the SFC coordinated to the Si atoms is concentrated in a narrow range, which inhibits the movement of the SFC due to steric hindrance, resulting in insufficient diffusibility of the SFC, and ultimately worsening the cycle test capacity retention rate.

[0044] From the viewpoint of further improving the safety of the separator and the nonaqueous secondary battery including the separator, the separator according to embodiment 2 preferably includes, for example, a silane-modified polyethylene as a Si-containing molecule, and more preferably, a silane crosslinking reaction of the silane-modified polyethylene proceeds when the separator comes into contact with the electrolyte.

[0045] From the viewpoint of uniformly dispersing the SFC throughout the separator and simultaneously achieving both the cycle characteristics and the safety of the nonaqueous secondary battery and / or achieving a balance between them, the Voronoi area (mu) of the maximum frequency among the Voronoi polygons obtained by performing the Voronoi division on the separator according to embodiment 2 is 6.5 μm 2 ~11.5μm 2 Preferably, the thickness is within the range of 7.0 μm. 2 ~11.0μm 2 More preferably, the thickness is in the range of 7.5 μm. 2 ~10.5μm 2 From the same viewpoint, it is more preferable that the spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by the above TOF-SIMS measurement is within the range of 2.0 μm 2 ~4.0μm 2 Preferably, the thickness is in the range of 2.2 μm. 2 ~3.8μm 2 More preferably, the range is 2.5 μm. 2 ~3.5μm 2 It is more preferable that the ratio is in the range of 1:1.

[0046] For a Si-containing image detected by TOF-SIMS measurement, it is preferable that the ratio (σ / mu) of the spread (σ) of the Voronoi area frequency distribution to the Voronoi area (mu) of maximum frequency satisfies the following relationship. 0.20≦σ / mu≦0.40 In the second embodiment, the ratio (σ / mu) in the Voronoi division can be regarded as an index showing whether the Si-containing molecules are uniformly dispersed on the separator surface. When the ratio (σ / mu) according to the second embodiment is within the range of 0.20 to 0.40, the Si-containing molecules are uniformly dispersed on the separator surface as in the first embodiment, and in a non-aqueous secondary battery, the Si-containing molecules sufficiently contribute to the coexistence of the Li complex derived from the electrolyte and the separator, the silane crosslinking reaction of the separator, and the like, thereby extending the cycle characteristics of the battery. In addition, in the second embodiment, the dispersibility of SFC is increased and the uniform formation of the SEI layer is promoted, thereby improving the cycle characteristics of the battery. From the viewpoint of further extending the cycle product life of the battery, the ratio (σ / mu) according to the second embodiment is more preferably within the range of 0.22 to 0.38, and even more preferably within the range of 0.25 to 0.35.

[0047] The numerical values ​​obtained by Voronoi tessellation of the separator according to embodiment 2 can be adjusted within the ranges described above by controlling, for example, the structure of the Si-containing molecule, the molecular weight or molecular weight distribution of the separator constituent raw materials, the blending range of the separator constituent raw materials, etc.

[0048] <Embodiment 3: Change in air permeability before and after compression of separator> The separator according to embodiment 3 includes a polyethylene microporous membrane, and has an air permeability change ratio (air permeability Sh after compression / air permeability Sj before compression) when compressed by 30% of its thickness within a range of 1.1 to 7.0 times.

[0049] In the third embodiment, when the air permeability change ratio (air permeability Sh / air permeability Sj) is within the range of 1.1 to 7.0 times, even if a nonaqueous secondary battery including a separator is compressed in the thickness direction of the separator, ion permeability can be maintained, and safety and low-temperature cycle characteristics in a nail penetration test of the battery tend to be ensured. This tendency is remarkable when the negative electrode of the battery is an easily expandable negative electrode such as a Si-containing negative electrode. From this viewpoint, the air permeability change ratio (air permeability Sh / air permeability Sj) is preferably 1.3 to 6.9 times.

[0050] The air permeability change ratio (air permeability Sh / air permeability Sj) is measured when the separator is a polyolefin microporous film, and the measurement can be performed by the method described in the Examples.

[0051] <Embodiment 4: Silane-modified polyolefin content and crystal structure> The separator according to embodiment 4 contains a silane-modified polyolefin, and has a polyethylene crystal long period of 20 to 50 nm as measured by small-angle X-ray scattering (SAXS), a crystallinity of 60% to 80% as measured by wide-angle X-ray scattering (WAXS), and a polyethylene crystallite size (110) of 10 to 50 nm as measured by wide-angle X-ray scattering (WAXS).

[0052] Generally, in separators made of crystalline resins such as polyethylene, there is a repeating periodic structure of crystalline and amorphous parts in the separator (Figure 19). c ) means the average length of one period of the repeating period of the crystalline and amorphous parts, and the crystalline part thickness (t c ) refers to the average thickness of the crystalline part in the repeating period of the crystalline part and the amorphous part, and the amorphous part thickness (t a ) refers to the average thickness of the amorphous part in the repeating period of the crystalline part and the amorphous part, crystallite size refers to the average size of each crystallite, crystallinity refers to the proportion of the crystalline part in the whole, and crystal orientation (a c) refers to the degree of orientation of the crystal part in a certain direction. For example, crystallite size (110) refers to the average size of each polyethylene crystallite in the (110) direction, crystallite size (200) refers to the average size of each polyethylene crystallite in the (200) direction, MD cross section crystal orientation refers to the degree to which the (110) plane of the polyethylene crystal is aligned parallel to the MD-TD plane in a cross section (MD cross section) of the separator cut along a plane perpendicular to the MD, and TD cross section crystal orientation refers to the degree to which the (110) plane of the polyethylene crystal is aligned parallel to the MD-TD plane in a cross section (TD cross section) of the separator cut along a plane perpendicular to the TD. The crystal structure of the separator can be measured using an X-ray structure evaluation device.

[0053] In embodiment 4, the SAXS and WAXS measurements are performed on the separator as the substrate. Therefore, when the separator is in the form of a multilayer film or a laminated film, the SAXS and WAXS measurements are performed after removing layers other than the polyolefin microporous film.

[0054] In the fourth embodiment, in a combination of specific X-ray structural analyses, SAXS and WAXS, when the crystal long period is within a range of 20 nm to 50 nm, the degree of crystallinity is within a range of 60% to 80%, and the crystallite size (110) of the polyethylene is within a range of 10 to 50 nm, the distance between the silane-modified units is optimized while improving the heat creep resistance of the separator, and the crosslinking reaction is promoted when the separator comes into contact with the coating liquid in the coating process. As a result, the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery can be improved without adding a process for crosslinking.

[0055] After the separator is applied, the battery goes through an assembly process, a finishing process (charging / discharging, degassing), and an inspection process, and the non-aqueous secondary battery is manufactured in as little as 1 to 5 days after coating. From the viewpoint of ensuring that the crosslinking reaction has progressed sufficiently by that time, the ease with which the crosslinking proceeds (the speed of the reaction) is important.

[0056] It is known that the crosslinking reaction rate depends on environmental factors such as the liquidity of the solvent and temperature, but the effects of structural factors such as the distance between functional groups and steric hindrance have not been fully studied. The present inventors have found conditions under which the crosslinking reaction of the separator is likely to proceed by combining specific X-ray structural analyses such as SAXS and WAXS and, if desired, specific functional group dispersion state analysis such as TOF-SIMS, and have further found optimal conditions for a separator for a non-aqueous secondary battery, taking into account heat creep resistance. Although not wishing to be bound by theory, according to the present invention, by designing to determine the crystal structure, the number of tie molecules in the amorphous layer is increased, improving heat creep resistance, and even if non-uniform stress occurs in the battery, non-uniform deformation of the separator is suppressed, and partial obstruction of the flow of Li ions and electrolyte decomposition products is suppressed, which is believed to improve the high-temperature cycle life.

[0057] In addition, in the present invention, by designing to determine the numerical values ​​related to the crystal structure and to determine the dispersion state of the silicon (Si)-containing functional group, the diffusivity of the Li ion complex is improved by interaction with the Si element in the silicon (Si)-containing functional group, and the local growth of Li dendrites is suppressed, which is believed to improve cycle characteristics. In addition, by designing to determine the numerical values ​​related to the crystal structure and to determine the dispersion state of the silicon (Si)-containing functional group, the silicon (Si)-containing functional groups approach each other, making it easier for the crosslinking reaction to proceed, and thus the crosslinking reaction can proceed in the coating process during the separator manufacturing process. In addition, by designing to determine the numerical values ​​related to the crystal structure and to determine the dispersion state of the silicon (Si)-containing functional group, the number of crosslinks increases, and the fluidity of the resin at high temperatures decreases, which is believed to improve safety in the crush test. In the coating process, by using a coating liquid with high polyolefin impregnation, the solvent that has penetrated between the molecular chains of the polyolefin promotes the thermal vibration of the silicon (Si)-containing functional groups, making it possible to further promote the crosslinking reaction, and by using a coating liquid containing polar molecules, the polar molecules and / or hydrogen ions and / or hydroxide ions in the coating liquid act as catalysts to further promote the crosslinking reaction between the silicon (Si)-containing functional groups. As a result, the fluidity of the separator at high temperatures can be reduced, and the high-temperature cycle life and crushing safety of the non-aqueous secondary battery can be improved.

[0058] From the viewpoint of improving the ease of crosslinking of the separator, the crush test pass rate of the battery, the cycle test capacity retention rate, and the high-temperature cycle life, and / or balancing them, in the SAXS and WAXS measurements of the separator, it is preferable to analyze the crystalline structure of the polyolefin, and it is more preferable to analyze the crystalline structure of the polyethylene. The silane-modified polyolefin according to embodiment 4 may be contained at any position of the separator, for example, in the case of a single-layer separator consisting of only a polyolefin microporous membrane, it may be present in the microporous membrane or on the surface of the microporous membrane, and in the case of a multi-layer separator including a layer formed on one or both sides of the microporous membrane, it may be present in the microporous membrane or on the surface of the microporous membrane, or in or on the surface of the formed layer, and from the same viewpoint as above, it is preferable that it is present in or on the surface of the polyolefin microporous membrane as the substrate. The WAXS measurement may be a transmission method or a reflection method (XRD). From the viewpoint of analyzing not only the separator surface but also the internal crystal structure, the WAXS measurement of the separator is preferably performed by a transmission method.

[0059] From the same viewpoint, the crystal long period detected by SAXS is preferably more than 20 nm and less than 49 nm, and more preferably 22 nm or more and 47 nm or less. From the same viewpoint, the crystallinity detected by WAXS is preferably more than 60% and less than 80%, and more preferably 62% or more and 78% or less. From the viewpoint of improving the crush test pass rate, cycle test capacity retention rate, and high temperature cycle life of the battery, and / or achieving a balance therebetween, the crystallite size (110 plane) of the polyethylene detected in the WAXS measurement of the separator containing the silane-modified polyolefin is preferably in the range of 10 nm to 50 nm, and more preferably in the range of 12 nm to 47 nm.

[0060] If the crystal long period is too large, the Gibbs-Thomson effect will raise the melting temperature of the crystals, and the shutdown temperature will rise. Also, if the crystal long period is too large, the number of tie molecules will decrease, which will reduce the heat creep resistance. This will result in a decrease in the crush test pass rate and a decrease in high-temperature cycle life. Also, in order to increase the crystal long period, it is necessary to increase the amount of deformation during the stretching process, which will deteriorate the heat shrinkability of the separator.

[0061] On the other hand, if the crystal long period is too small, the distance between the silane-modified units in the amorphous portion becomes too small, which reduces the impregnation of the solvent and / or reduces the crosslinking ability due to the generation of steric hindrance between the silane-modified groups, resulting in a reduction in the viscoelasticity during melting and a reduction in the meltdown temperature. This leads to a reduction in the pass rate of the crush test and a reduction in the high-temperature cycle life. In addition, in order to reduce the crystal long period, it is necessary to reduce the amount of stretching in the stretching process, which reduces the pore size and number of pores in the separator, thereby deteriorating the permeability. This leads to a reduction in the pass rate of the crush test, a reduction in the cycle test capacity retention rate, and a reduction in the high-temperature cycle life.

[0062] Similarly, if the crystallinity is too high, the melting temperature of the crystals increases due to the Gibbs-Thomson effect, the shutdown temperature of the separator increases, and the number of tie molecules decreases, resulting in a decrease in heat creep resistance. The distance between the silane-modified units between the opposing crystal faces decreases, which reduces the impregnation of the solvent and the crosslinking ability due to the steric interference of the branched chains, resulting in a decrease in the viscoelasticity when melted and the meltdown temperature. This leads to a decrease in the crush test pass rate and a decrease in the high-temperature cycle life.

[0063] On the other hand, if the crystallinity is too low, the heat shrinkage deteriorates due to limitations in separator film formation, and the number of tie molecules decreases, resulting in a decrease in heat creep resistance. In addition, the distance between silane-modified units between opposing crystal faces increases, reducing crosslinking, lowering viscoelasticity during melting and meltdown temperature. This ultimately leads to a decrease in the crush test pass rate and a decrease in high-temperature cycle life.

[0064] If the crystallite size is too large, the melting temperature of the crystals increases due to the Gibbs-Thomson effect, and the shutdown temperature also increases. Also, the number of tie molecules decreases, which reduces the thermal creep resistance. This in turn reduces the crush test pass rate and the high-temperature cycle life.

[0065] On the other hand, in order to reduce the crystallite size, it is necessary to perform stretching and heat treatment at low temperature and high tensile force after sheet formation, which tends to leave residual stress in the separator, leading to deterioration of the heat shrinkability of the separator, and ultimately causing a decrease in the crush test pass rate and a decrease in the high-temperature cycle life.

[0066] From the viewpoint of improving the ease of crosslinking in the separator, as well as the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery, and / or achieving a balance therebetween, it is preferable that the crystallite size (110) of the polyethylene in the separator as measured by XRD is 14.2 to 40.0 nm and / or the crystallinity as measured by XRD is 80 to 99%.

[0067] The ratio (110) / (200), of the crystallite size perpendicular to the (110) plane to the crystallite size perpendicular to the (200) plane, detected in a WAXS measurement of a separator containing a silane-modified polyolefin, is preferably 0.9 to 2.0, and more preferably 1.0 to 1.7, from the viewpoints of improving the crush test pass rate, cycle test capacity retention rate, high-temperature cycle life, etc. of the battery and / or achieving a balance therebetween.

[0068] From the same viewpoint as above, the amorphous thickness (amorphous length) of the separator containing the silane-modified polyolefin is calculated by the following formula from the crystal long period of polyethylene detected by small-angle X-ray scattering measurement and the crystallinity detected by wide-angle X-ray scattering measurement: Formula: Amorphous thickness [nm] = (Crystal long period [nm]) × (1-Crystallinity [%] / 100) It is calculated by the formula, and is preferably in the range of 3 nm to 23 nm, more preferably in the range of 5 nm to 15 nm, and even more preferably in the range of 8 nm to 13 nm. If the amorphous thickness (amorphous length) is too large, the entanglement of molecular chains in the amorphous part increases, so that the intercrystalline constraint becomes stronger, and the shutdown temperature increases. In addition, the distance between the silane-modified units between the opposing crystal faces increases, so that the crosslinking property decreases, and the viscoelasticity and meltdown temperature at the time of melting decrease. As a result, the crush test pass rate and the high-temperature cycle life decrease. On the other hand, if the amorphous length is too small, the entanglement of molecular chains decreases, and the heat creep resistance decreases. In addition, the distance between the silane-modified units between the opposing crystal faces decreases, so that the crosslinking property decreases due to the decrease in the impregnation property of the solvent and the steric hindrance of the branched chains, and the viscoelasticity and meltdown temperature at the time of melting decrease. As a result, the crush test pass rate and the high-temperature cycle life decrease.

[0069] From the same viewpoint as above, the crystal thickness of the separator containing the silane-modified polyolefin is preferably in the range of 15 nm to 36 nm, more preferably in the range of 17 nm to 34 nm. If the crystal thickness (crystal length) is too large, the melting temperature of the crystal increases due to the Gibbs-Thomson effect, and the shutdown temperature also increases. In addition, the number of tie molecules decreases, so the heat creep resistance decreases. As a result, the crush test pass rate and the high-temperature cycle life decrease. On the other hand, if the crystal length is to be reduced, it is necessary to perform stretching and heat treatment at low temperature and high tensile force after sheet formation, which makes it easy for residual stress to remain in the separator, and ultimately leads to deterioration of heat shrinkability. As a result, the crush test pass rate and the high-temperature cycle life decrease.

[0070] From the same viewpoint as above, in the WAXS measurement of the separator containing the silane-modified polyolefin, it is preferable that the cross-sectional crystal orientation degree of the polyethylene measured from the MD direction of the separator is in the range of 0.70 to 0.99, and the cross-sectional crystal orientation degree of the polyethylene measured from the TD direction is in the range of 0.70 to 0.99. If the cross-sectional crystal orientation degrees measured from the MD and TD are 0.70 or more, it is easy to ensure the separator strength, and on the other hand, if they are 0.99 or less, it is easy to form the separator into a film. From the viewpoint of the strength and film formability of the separator, it is more preferable that the cross-sectional crystal orientation degree of the polyethylene measured from the MD direction of the separator is in the range of 0.76 to 0.98, and / or the cross-sectional crystal orientation degree of the polyethylene measured from the TD direction of the separator is more preferably in the range of 0.74 to 0.93.

[0071] If the cross-sectional crystal orientation is too large, the deformation in the orientation direction during melting will be large, and the heat shrinkage will deteriorate. This will result in a decrease in the crush test pass rate and high-temperature cycle life. On the other hand, if the cross-sectional crystal orientation is too small, the crush test pass rate and high-temperature cycle life will decrease. It is generally known that when stress is applied to a resin material, the fewer tie molecules oriented in the stress direction, the lower the heat creep resistance. If the cross-sectional crystal orientation is too small, the separator will deform unevenly when uneven stress occurs in the battery, the flow of SFC will become uneven, and an uneven SEI layer will be formed, which will result in a decrease in the crush test pass rate and a decrease in the high-temperature cycle life.

[0072] From the viewpoint of improving the mechanical strength of the separator, the crush test pass rate of the battery, the cycle test capacity retention rate, and the high-temperature cycle life, and / or achieving a balance between them, it is preferable that the cross-sectional crystal orientation degree of the polyethylene in the MD direction of the separator measured by XRD is 0.85 to 0.99, and / or the cross-sectional crystal orientation degree of the polyethylene in the TD direction is 0.85 to 0.99.

[0073] From the same viewpoint as above, the ratio MD / TD of the cross-sectional crystal orientation degree of the polyethylene measured in the MD direction of the separator to the cross-sectional crystal orientation degree of the polyethylene measured in the TD direction is preferably in the range of 0.45 to 1.35 or 0.5 to 1.2, more preferably in the range of 0.50 to 1.20 or 0.60 to 1.25, and even more preferably in the range of 0.80 to 1.15. When the ratio MD / TD of the cross-sectional crystal orientation degree of the polyethylene measured in the MD direction of the separator to the cross-sectional crystal orientation degree of the polyethylene measured in the TD direction is within the above range, the mechanical strength of the separator increases, and creep deformation is less likely to occur due to complex stresses that occur non-uniformly in the battery, which in turn improves the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery.

[0074] The numerical values ​​detected by SAXS and / or WAXS measurement of the separator can be adjusted to within the ranges described above, for example, by quantifying or selecting the Si modification rate, C3 / C4 molecular structure, number average molecular weight (Mn), weight average molecular weight (Mw), dispersity (Mn / Mw) and the like of the silane-modified polyolefin for uniform arrangement of Si-containing molecular structures in the manufacturing process of the separator, and / or by quantifying or selecting the polyolefin resin other than the silane-modified polyolefin based on Mn, Mw, Mn / Mw and the like, and / or by quantifying the blending ratio of the silane-modified polyolefin and the polyolefin resin other than the silane-modified polyolefin.

[0075] The maximum frequency Voronoi area (mu) of the Voronoi polygons obtained by performing Voronoi division on the Si-containing image detected by TOF-SIMS measurement of a separator containing silane-modified polyolefin was 6.00 m 2 ~12.00μm 2 It is preferable that the maximum frequency Voronoi area (mu) is within 6.00 μm 2 ~12.00μm 2In this case, the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery are improved, and / or it becomes easier to balance them. More specifically, when the Voronoi area (mu) of the maximum frequency of the Voronoi polygons obtained by the Voronoi division is 6.00 μm 2 ~12.00μm 2 Within this range, the Si-containing molecules are highly likely to be dispersed in the separator without forming a sea-island structure. For example, in the case where the nonaqueous secondary battery is a lithium ion secondary battery, if the separator in which the Si element is uniformly dispersed coexists with a lithium (Li) complex solvated with an electrolyte having an unshared electron pair such as an oxygen atom, the phenomena of items (A) and (B) described in the first embodiment may extend the product life in a cycle characteristic test of the battery.

[0076] Furthermore, Si-containing molecules often have crosslinking properties. For example, when the Si-containing molecules have silane crosslinking properties, the silane crosslinking properties of the Si-containing molecules dispersed in the nonaqueous secondary battery can be ensured, and the stability of the siloxane bonds can be ensured. This is thought to enable the crosslinked structure of the separator to be maintained over a long period of time, thereby ensuring safety in safety tests such as crush tests.

[0077] In the separator according to the fourth embodiment, when a TOF-SIMS measurement is performed in a 100 μm square area, at least one structure containing silicon is detected, and preferably, it is detected that the Si-containing molecules are dispersed in the separator in a state other than a sea-island structure.

[0078] From the viewpoint of further improving the safety of the separator and the nonaqueous secondary battery including the separator, the separator according to embodiment 4 preferably includes, for example, a silane-modified polyethylene as a Si-containing molecule, and more preferably, a silane crosslinking reaction of the silane-modified polyethylene proceeds when the separator comes into contact with a coating solution or an electrolyte solution.

[0079] From the viewpoint of improving the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery, and / or achieving a balance between them, the Voronoi area (mu) of the Voronoi polygon with the maximum frequency obtained by performing the Voronoi division is 6.20 μm 2 ~11.80μm 2 It is more preferable that the ratio is in the range of 1.

[0080] The spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by the above TOF-SIMS measurement is 2.00 μm 2 ~4.00μm 2 It is preferable that the σ of the separator is within the range of 2.00 μm. 2 If it is more than 4.00 μm, it is easy to form a separator film. 2 If the separator has a σ of 2.30 μm or less, the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery can be improved. 2 ~3.60μm 2 It is more preferable that the ratio is in the range of 1.

[0081] For a Si-containing image detected by TOF-SIMS measurement, it is preferable that the ratio (σ / mu) of the spread (σ) of the Voronoi area frequency distribution to the Voronoi area (mu) of maximum frequency satisfies the following relationship. 0.20≦σ / mu≦0.40 The ratio (σ / mu) in the Voronoi division can be regarded as an index showing whether the Si-containing molecules are uniformly dispersed on the separator surface. When the ratio (σ / mu) is within the range of 0.20 to 0.40, the Si-containing molecules are uniformly dispersed on the separator surface, and in a non-aqueous secondary battery, the ratio (σ / mu) sufficiently contributes to the coexistence of the Li complex derived from the electrolyte and the separator, and the silane crosslinking reaction of the separator, and can achieve both the film-forming properties of the separator containing the silane-modified polyolefin and the cycle characteristics of the non-aqueous secondary battery. Although not wishing to be bound by theory, the concentration at which the intermediate in which the Li complex is coordinated in the separator surface exists, or the life of the intermediate in the equilibrium state, is important, and in the fourth embodiment, it was experimentally discovered that the ratio (σ / mu) within the above numerical range can uniformly contribute to the intercalation reaction in the electrode. From the viewpoint of further extending the cycle product life of the battery while ensuring the film-forming properties of the separator, the ratio (σ / mu) is more preferably 0.22 or more and 0.38 or less.

[0082] The numerical values ​​obtained by Voronoi tessellation of the separator according to embodiment 4 can be adjusted within the ranges described above by controlling, for example, the structure of the Si-containing molecule, the molecular weight or molecular weight distribution of the separator constituent raw materials, the blending range of the separator constituent raw materials, etc.

[0083] If desired, the separator according to embodiment 4 may have a multi-layer structure, and can be provided as a non-aqueous secondary battery comprising the separator.

[0084] <Embodiment 5: Silane-modified polyolefin-containing structure of separator, Voronoi division, change in air permeability before and after compression, and crystal structure> In the fifth embodiment, a separator for a non-aqueous secondary battery is provided in which the configurations according to the first to fourth embodiments are combined.

[0085] The separator for a non-aqueous secondary battery according to the fifth embodiment is a polyolefin microporous film containing a silane-modified polyolefin, and the maximum frequency Voronoi area (mu) of the Voronoi polygons obtained by performing Voronoi division on a Si-containing image detected by TOF-SIMS measurement of the separator is 1.0 μm 2 ~17.5μm 2 or 6.0 μm 2 ~12.0μm 2 The spread (σ) of the Voronoi area frequency distribution of the Si-containing image detected by TOF-SIMS measurement is within the range of 0.5 μm 2 ~8.5μm 2 the air permeability change ratio when the separator is compressed by 30% of its thickness (air permeability Sh after compression / air permeability Sj before compression) is in the range of 1.1 to 7.0 times; the crystal long period of the polyethylene detected by SAXS measurement is 20 to 50 nm; the crystallinity detected by WAXS measurement is 60% to 80%; and / or the crystallite size (110) of the polyethylene detected by WAXS measurement is 10 to 50 nm.

[0086] The components of the separators according to the first to fifth embodiments will be described below.

[0087] <Polyolefin> The polyolefin is not particularly limited, and examples thereof include homopolymers of ethylene or propylene, and copolymers formed from at least two monomers selected from the group consisting of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, norbornene, and modified polyolefins. Among these, from the viewpoint of being able to perform heat setting (sometimes abbreviated as "HS") at higher temperatures without blocking pores, high density polyethylene, low density polyethylene, ultra-high molecular weight polyethylene (UHMWPE), or modified polyolefins are preferred, and high density polyethylene, UHMWPE, or modified polyolefins are more preferred. In general, it is known that the weight average molecular weight of UHMWPE is 1,000,000 or more. The polyolefins may be used alone or in combination of two or more kinds.

[0088] From the viewpoint of imparting to the separator the properties obtained by the Voronoi tessellation described above, the properties obtained by SAXS and / or WAXS, etc., it is preferable to use a modified polyolefin as the polyolefin, and it is more preferable to use a silane-modified polyethylene (hereinafter referred to as resin A).

[0089] From the viewpoint of achieving both a long life and safety in the cycle characteristics of a nonaqueous secondary battery and balancing them, as well as optimizing the various values ​​explained above for the uniform arrangement of Si-containing molecular structures, SAXS and / or WAXS measurement, and Voronoi tessellation, and improving the ease of crosslinking of the separator, as well as the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery, and / or balancing them, it is preferable to use at least one polyolefin other than silane-modified polyethylene in addition to resin A, and it is more preferable to use UHMWPE having a viscosity average molecular weight (Mv) of 1,800,000 or more (hereinafter referred to as resin B) as the polyolefin other than silane-modified polyethylene, and it is even more preferable to use not only resin B but also polyethylene having an Mv of less than 1,800,000 (hereinafter referred to as resin C).

[0090] (Separator silicon-containing structure and Voronoi tessellation) In the silicon (Si)-containing functional group of the silane-modified polyolefin in the separator, the number of methylenes (CH2) constituting the linking portion to the main chain is preferably 2 to 10. The number of methylenes (CH2) constituting the linking portion to the main chain refers to the number of (CH2) linking the main chain of the silane-modified polyolefin to a Si atom, and is, for example, the value of n in the following formula (I). [ka] In the formula, R includes methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, etc., and n is the number of methylene (CH2) constituting the linkage to the main chain described above. For example, with respect to the Si-containing functional group of the silane-modified polyolefin, when the number of CH2 constituting the linking portion is within the range of 2 to 10 with respect to the polyolefin main chain containing polyethylene or the like as the main component, it becomes easy to construct a higher-order structure that easily undergoes a silane crosslinking reaction. From the viewpoint of ensuring the ease of crosslinking of the separator, improving the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the battery, and / or achieving a balance therebetween, it is more preferable that the number of CH2 is within the range of 2 to 6.

[0091] <Resin A: Silane-modified polyethylene> A separator containing silane-modified polyethylene (resin A) is preferred because the silane crosslinking reaction of the silane-modified polyethylene proceeds when the separator comes into contact with a coating solution or an electrolyte. Examples of silane-modified polyethylene include silane-grafted polyethylene. It is considered that the functional group contained in the polyolefin constituting the separator is not incorporated into the crystalline portion of the polyolefin, but is crosslinked in the amorphous portion. Therefore, when the separator according to the first to fifth embodiments comes into contact with an electrolyte, it forms a crosslinked structure using chemical substances in the electrolyte, thereby suppressing an increase in internal stress or deformation of the produced battery, and improving safety in nail penetration tests and the like.

[0092] In addition, the separator according to the first to fifth embodiments is a coating liquid having H + It is possible to react with ions or -OH groups to promote a crosslinking reaction, thereby suppressing an increase in internal stress or deformation of the produced battery, and improving safety in crush tests and the like. Without wishing to be bound by theory, it is thought that when the water-based coating liquid is acidic, the activation energy of the reaction system is reduced, making it easier for the crosslinking reaction of the separator to proceed. When the water-based coating liquid is basic, OH - In the case of a non-aqueous coating liquid, the organic solvent in the coating liquid penetrates into the amorphous polyethylene part of the separator, promoting molecular motion and thus promoting the silane crosslinking reaction.

[0093] In the separator, by constructing a silane crosslinked structure (gelled structure) by silane-modified polyethylene, high-temperature membrane rupture resistance is exhibited, and safety in crush tests and the like can be improved. This is presumably because the polyethylenes dispersed in the mixed resin and / or the polyethylene and the polyolefin other than polyethylene are suitably linked by the silane crosslinked structure. That is, the morphology of the separator as a whole, including the polyolefin microporous membrane, changes, and the tensile elongation is also improved, which is expected to reduce the possibility of the separator breaking when the battery is deformed by an external force.

[0094] Silane-modified polyolefins have a structure in which the main chain is a polyolefin and an alkoxysilyl group is grafted to the main chain. Silane-modified polyolefins can be obtained, for example, by grafting an alkoxysilyl group to the main chain of a polyolefin. Examples of silane-unmodified polyolefins include polyethylene, polypropylene, and copolymers of ethylene and propylene. Examples of silane-modified polyethylenes include graft copolymers obtained by grafting unsaturated silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltriacetoxysilane to polyethylene such as high-density polyethylene, low-density polyethylene, and linear low-density polyethylene, or ethylene-ethylenically unsaturated silane compound copolymers.

[0095] It is presumed that the alkoxysilyl group of the silane-modified polyethylene is converted to a silanol group through a hydrolysis reaction with water, and then undergoes a crosslinking reaction to form a siloxane bond (see the hydrolysis reaction, condensation reaction, and dehydration condensation reaction shown in the following formula; the rate of change from the T0 structure to the T1 structure, T2 structure, or T3 structure is arbitrary, and the following formula describes the case where the number n of methylenes (CH2) constituting the linking portion to the main chain described in the above formula (I) is 2, but n may be 3 to 10). The alkoxide substituted on the alkoxysilyl group is not particularly limited, and examples thereof include methoxide, ethoxide, and butoxide. For example, in the following formula, R is methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, and tert-butyl. [ka]

[0096] In the silane-modified polyethylene, the main chain and the grafts are connected by a covalent bond. The structure forming such a covalent bond is not particularly limited, but examples thereof include alkyl, ether, glycol, and ester.

[0097] From the viewpoints of not only the uniform arrangement of Si-containing molecular structures and the lifespan of the equilibrium state intermediate Li complex coordination but also of optimizing the various values ​​explained above for the SAXS and / or WAXS measurement and Voronoi tessellation, and improving the ease of proceeding of crosslinking of the separator, as well as the pass rate of a crush test, the capacity retention rate in a cycle test, and the high-temperature cycle life of the battery, and / or of balancing them, it is preferable that, at a stage before the crosslinking reaction of Resin A, Resin A contains 0.03 to 1.0 mol % of silanol units (i.e., the silanol unit modification rate is 0.03 to 1.0 mol %), and this silanol unit modification rate is more preferably 0.05 to 0.35 mol %, further preferably 0.07 to 0.32 mol %, particularly preferably 0.08 to 0.30 mol %, and most preferably 0.12 to 0.28 mol %. In the first to fifth embodiments, the silane-modified units are present only in the amorphous portion of the separator, and a molecular structure that facilitates the construction of a crosslinking reaction was designed by focusing on the distance between the silane-modified units and the thermal vibration motion at -10°C to 80°C. In the above formula, the T0, T1, T2, and T3 structures can all construct a coordination intermediate with the Li complex, but since the Li complex is considered to randomly coordinate, decoordination, and recoordination between Si atoms in the amorphous portion, the effect was maximized by adjusting the amount of silanol unit modification of the resin A.

[0098] From the same viewpoint as above, resin A is preferably modified with 0.01 to 2.0 mol % of propylene-modified (C3) units, 0.01 to 2.0 mol % of butene (C4) units, or a total of 0.01 to 2.0 mol % of C3 units and C4 units.

[0099] From the same viewpoint as above, the C3 unit modification rate of resin A is more preferably 0.01 to 1.2 mol%, further preferably 0.01 to 0.75 mol%, particularly preferably 0.02 to 0.60 mol%, and most preferably 0.05 to 0.30 mol%.

[0100] From the viewpoint of the FUSE function of the separator as well as the cycle characteristics and safety of the nonaqueous secondary battery, the C4 unit modification rate of the resin A is more preferably 0.01 to 1.0 mol%, further preferably 0.30 to 0.70 mol%, and particularly preferably 0.48 to 0.65 mol% before the crosslinking reaction of the resin A. On the other hand, in the heat setting (HS) step in the formation of the separator, the C4 unit modification rate of the resin A is preferably 0.43 mol% or less, more preferably 0.40 mol% or less, and further preferably 0.1 mol% or less.

[0101] From the viewpoints of not only the cycle characteristics and safety of the nonaqueous secondary battery, but also from the viewpoints of optimizing the various values ​​described above for the SAXS and / or WAXS measurement and Voronoi tessellation of the separator, and improving the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the nonaqueous secondary battery, and / or achieving a balance therebetween, the total modification rate of the C3 units and the C4 units of Resin A is more preferably 1.5 mol % or less, even more preferably 1.0 mol % or less, particularly preferably 0.6 mol % or less, and most preferably 0.3 mol % or less.

[0102] From the viewpoint of cycle characteristics and safety of a nonaqueous secondary battery, the number average molecular weight (Mn) of resin A is preferably from 10,000 to 20,000, more preferably 16,000 or less, and even more preferably 15,000 or less.

[0103] From the same viewpoint as above, the weight average molecular weight (Mw) of resin A is preferably 45,000 to 200,000, more preferably 140,000 or less, further preferably 129,000 or less, particularly preferably 100,000 or less, and most preferably 72,000 or less.

[0104] From the same viewpoint as above, Mw / Mn of Resin A is preferably from 3.0 to 12, more preferably from 4.0 to 9.0, and further preferably from 4.1 to 8.0.

[0105] From the same viewpoint as above, the crystallinity of resin A is preferably from 40 to 70%, more preferably from 50 to 68%, and further preferably from 60 to 65%.

[0106] From the same viewpoint as above, the crystallite size (110) of resin A is preferably from 15 to 30 nm, more preferably from 17 to 28 nm, and even more preferably from 20 to 25 nm.

[0107] From the same viewpoint as above, the crystal long period of resin A is preferably from 15 to 30 nm, more preferably from 17 to 27 nm, and further preferably from 20 to 25 nm.

[0108] Resin A is not limited, but its viscosity average molecular weight (Mv) may be, for example, 20,000 to 150,000, and its density may be, for example, 0.90 to 0.97 g / cm 3 The melt mass flow rate (MFR) at 190° C. may be, for example, 0.1 to 15 g / min.

[0109] The polyethylene constituting the silane-modified polyethylene may be composed of one type of ethylene alone, or may be composed of two or more types of ethylene. Two or more types of silane-modified polyethylene composed of different ethylenes may be used in combination.

[0110] <Resin B: UHMWPE with Mv of 1,800,000 or more> Resin B is UHMWPE having an Mv of 1,800,000 or more, and is preferably used in combination with Resin A, and may be used in combination with Resin C if desired.

[0111] The Mn of Resin B is preferably 200,000 to 1,400,000, more preferably 210,000 to 1,200,000, and even more preferably 250,000 to 1,000,000, not only from the viewpoint of the cycle characteristics and safety of the nonaqueous secondary battery, but also from the viewpoint of optimizing the various values ​​explained above regarding the SAXS and / or WAXS measurement and Voronoi tessellation of the separator, and improving the crush test pass rate, cycle test capacity retention rate, high temperature cycle life, and the like of the nonaqueous secondary battery, and / or achieving a balance therebetween.

[0112] From the same viewpoint as above, Mw of Resin B is preferably from 1,500,000 to 8,800,000, more preferably from 1,600,000 to 7,100,000, and even more preferably from 1,700,000 to 6,200,000.

[0113] From the same viewpoint as above, the ratio of Mw to Mn (Mw / Mn) of Resin B is preferably 3.0 to 12, more preferably 4.0 to 9.0, and further preferably 6.0 to 8.8.

[0114] From the same viewpoint as above, the Mv of Resin B is preferably more than 1,800,000 and not more than 10,000,000, more preferably from 1,850,000 to 8,500,000, further preferably from 1,950,000 to 7,800,000, and particularly preferably from 2,000,000 to 6,500,000.

[0115] <Resin C: Polyethylene with Mv less than 1,800,000> Resin C is a polyethylene having an Mv of less than 1,800,000, and is preferably used in combination with Resin A, and can be used in combination with Resin B if desired.

[0116] Mn of Resin C is preferably 20,000 to 250,000, more preferably 30,000 to 200,000, even more preferably 32,000 to 150,000, and particularly preferably 40,000 to 110,000, not only from the viewpoint of the cycle characteristics and safety of the nonaqueous secondary battery, but also from the viewpoint of optimizing the various values ​​explained above regarding the SAXS and / or WAXS measurement and Voronoi tessellation of the separator, and improving the crush test pass rate, cycle test capacity retention rate, high-temperature cycle life, and the like of the nonaqueous secondary battery, and / or achieving a balance therebetween.

[0117] From the same viewpoint as above, Mw of Resin C is preferably 230,000 to 1,500,000, more preferably 280,000 to 1,300,000, further preferably 320,000 to 1,200,000, and particularly preferably 400,000 to 1,000,000.

[0118] From the same viewpoint as above, the ratio of Mw to Mn (Mw / Mn) of Resin C is preferably 3.0 to 12, more preferably 4.0 to 9.0, and further preferably 6.0 to 8.8.

[0119] From the same viewpoint as above, the Mv of resin C is preferably 250,000 or more and less than 1,800,000, more preferably 300,000 or more and 1,600,000 or less, still more preferably 320,000 or more and 1,100,000 or less, and particularly preferably 450,000 to 800,000.

[0120] <Optional ingredients> Optional components that can be contained in the separator include components different from any of Resins A to C, such as at least one of a polymer different from any of Resins A to C or an additive described below. The optional components are not limited to a single type. The separator may contain multiple types of polymers different from any of Resins A to C, may contain multiple types of additives, or may contain both the polymer and the additive. Examples of optional polymer components include, for example, polypropylene (PP), polystyrene (PS), polyacrylate, polymethacrylate, polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), polyester, polycarbonate (PC), polysulfone (PSU), polyethersulfone (PES), polyphenylene oxide (PPO), polyarylene ether polymers, polyphenylene sulfide (PPS), polyphenylene sulfide sulfone, polyparaphenylene (PPP), polyarylene polymers, polyarylene ketone, polyether ketone (PEK), poly Examples of the additive include a homopolymer or copolymer containing at least one of arylene phosphine oxide, polyether phosphine oxide, polybenzoxazole (PBO), polybenzothiazole (PBT), polybenzimidazole (PBI), polyamide (PA), polyimide (PI), polyetherimide (PEI), and polyimide sulfone (PIS), and examples of the additive include antioxidants such as phenolic compounds, phosphorus compounds, and sulfur compounds; metal soaps such as calcium stearate and zinc stearate; ultraviolet absorbers; light stabilizers; antistatic agents; antifogging agents; coloring pigments, etc. When the separator contains multiple types of optional components, the total content of the multiple types of optional components may be 20 mass% or less.

[0121] The separator may contain not only the additives exemplified above but also known additives such as a plasticizer, but preferably does not contain an organometallic catalyst (dehydration condensation catalyst).

[0122] (Dehydration condensation catalyst) Alkoxysilyl groups undergo hydrolysis with water to form siloxane bonds. However, because the reaction rate is slow, in many cases, an organometallic catalyst can be used to promote the condensation reaction. The metal of the organometallic catalyst can be, for example, at least one selected from the group consisting of scandium, vanadium, copper, zinc, zirconium, palladium, gallium, tin, titanium, iron, nickel and lead. Organometallic catalysts include, in particular, di-butyltin dilaurate, di-butyltin diacetate, di-butyltin dioctoate, etc., and are known to be able to overwhelmingly accelerate the reaction rate by the reaction mechanism proposed by Wei et al. (FW van. de R. Wei, Macromol. Chem., 181, 2541, 1980.). In recent years, however, in order to avoid the environmental and human health hazards caused by organotins, it has become known that the Lewis function of copper or titanium chelate complexes can be utilized in combination with an organic base to accelerate the reaction of forming siloxane bonds between alkoxysilyl groups in the same manner as organotin complexes.

[0123] It is known that the organometallic catalyst (dehydration condensation catalyst) also functions as a catalyst for the siloxane bond formation reaction of the alkoxysilyl group-containing resin. In this specification, the resin containing silane-modified polyethylene to which the organometallic catalyst (or dehydration condensation catalyst) is added beforehand, prior to the sheet forming process (for example, at the stage of the kneading process performed as required), is referred to as the masterbatch resin.

[0124] It is preferable that the separator does not contain an organometallic catalyst (dehydration condensation catalyst) or a masterbatch resin containing the same.

[0125] <Separator characteristics> The following separator properties are for a polyolefin microporous flat membrane or monolayer membrane. When the microporous membrane is in the form of a laminate membrane, the following properties can be measured after removing layers other than the polyolefin microporous membrane from the laminate membrane.

[0126] The porosity of the separator is preferably 20% or more, more preferably 30% or more, and even more preferably 32% or more or 35% or more. By having a porosity of 20% or more, the separator tends to have improved puncture strength and followability to rapid movement of lithium ions. On the other hand, the porosity of the separator is preferably 90% or less, more preferably 80% or less, and even more preferably 50% or less. By having a porosity of 90% or less, the membrane strength tends to be improved, self-discharge tends to be suppressed, and / or the air permeability tends to be optimized. The porosity of the separator can be measured by the method described in the examples.

[0127] The air permeability of the separator, in a state not subjected to a compression test or before a compression test, is preferably 1 second or more, more preferably 30 seconds or more, even more preferably 50 seconds or more, even more preferably 55 seconds or more, particularly preferably 70 seconds or more, and most preferably 75 seconds or more. By having an air permeability of 1 second or more, the balance between the membrane thickness, the porosity, and the pore size tends to be improved, or the puncture strength tends to be improved. In addition, the air permeability of the separator is preferably 400 seconds or less, more preferably 300 seconds or less, and even more preferably 270 seconds or less. By having an air permeability of 400 seconds or less, ion permeability tends to be further improved. The air permeability of the separator can be measured by the method described in the examples.

[0128] The tensile strength of the separator is preferably 1000 kgf / cm in both MD and TD. 2 More preferably, it is 1050 kgf / cm 2 More preferably, it is 1100 kgf / cm 2 More than 1000kgf / cm 2 By being equal to or greater than this, breakage during lamination or winding with slits or electrodes tends to be more suppressed, and short circuits due to foreign matter or the like in the battery tends to be more suppressed. On the other hand, the tensile strength of the separator is preferably 5000 kgf / cm 2 More preferably, it is 4500 kgf / cm or less. 2More preferably, it is 4000 kgf / cm or less. 2 Tensile strength is 5000kgf / cm or less. 2 By keeping the temperature below 100° C., the separator will relax early during the heat test, weakening the contraction force, and as a result, safety tends to be improved.

[0129] The tensile modulus of the separator is preferably 120 N / cm or less, more preferably 100 N / cm or less, and even more preferably 90 N / cm or less in both MD and TD. A tensile modulus of 120 N / cm or less indicates that the separator is not extremely oriented as a separator for a non-aqueous secondary battery, and in a heating test or the like, when a blocking agent such as polyethylene melts and shrinks, the polyethylene etc. causes stress relaxation early, which suppresses the shrinkage of the separator in the battery and tends to easily prevent short circuits between electrodes (i.e., the safety of the separator during heating can be improved). A separator having such a low tensile modulus is easily achieved by including polyethylene having a weight average molecular weight of 500,000 or less in the polyolefin forming the polyolefin microporous membrane as the separator substrate. On the other hand, the lower limit of the tensile modulus of the separator is not particularly limited, but is preferably 10 N / cm or more, more preferably 30 N / cm or more, and even more preferably 50 N / cm or more. The tensile modulus can be appropriately adjusted by adjusting the degree of stretching and, if necessary, by relaxing the film after stretching.

[0130] The thickness of the separator is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 3.0 μm or more, 4.0 μm or more. By having a thickness of 1.0 μm or more, the membrane strength tends to be further improved. In addition, the thickness of the separator is preferably 24 μm or less, more preferably 22 μm or less, and even more preferably 20 μm or less, 18 μm or less. By having a thickness of 24 μm or less, the ion permeability tends to be further improved. The thickness of the separator can be measured by the method described in the examples.

[0131] In the polyethylene crystal structure in the separator, the polyethylene crystallinity measured by X-ray diffraction (XRD) is preferably 60 to 99%, the polyethylene (110) crystallite size is preferably 14.2 to 50.0 nm, the cross-sectional orientation is preferably 0.65 to 0.99, the lamellar thickness is preferably 15 to 40 nm, and the crystal long period is preferably 25 to 55 nm. The separator has an excellent crystal structure determined by such X-ray structure analysis due to its mechanical properties such as high compression elastic recovery rate and resistance to creep deformation due to external force.

[0132] From the viewpoints of ensuring ease of handling, safety in the Hot Box test, and stabilization of the thermal shrinkage rate, the puncture strength of the separator is preferably in the range of 200 gf to 600 gf, and more preferably in the range of 210 gf to 390 gf. From the same viewpoint, the puncture strength converted into the basis weight of the separator (puncture strength of the separator (gf) / basis weight of the separator (g / m 2 ) is 50 gf m 2 / g~100gf m 2 / g, and preferably in the range of 60 gf m 2 / g~90gf m 2 It is more preferable that the molecular weight is in the range of / g.

[0133] <Layer configuration> The separator may have either a single-layer structure or a multilayer structure, and preferably includes at least one polyolefin microporous film from the viewpoint of having oxidation-reduction resistance and a dense and uniform porous structure. The polyolefin microporous film may be a single-layer film consisting of a single polyolefin-containing microporous layer, a multilayer film consisting of multiple polyolefin-containing microporous layers, or a multilayer film consisting of a polyolefin-based resin layer and a layer containing other resins as the main component, such as a thermoplastic polymer-containing layer, an active layer, a heat-resistant resin layer, or an inorganic porous layer.

[0134] In the case of a bilayer membrane formed from two polyolefin-containing microporous layers, the polyolefin composition of the two layers can be different, and in the case of a multilayer membrane formed from three or more polyolefin-containing microporous layers, the polyolefin composition of the outermost and innermost layers can be different, for example, a three-layer membrane.

[0135] (Preferred multi-layer structure 1) A separator having a preferred multilayer structure 1 preferably comprises a polyolefin microporous membrane as a substrate, and an inorganic porous layer containing inorganic particles and a resin binder laminated on at least one side of the polyolefin microporous membrane. From the viewpoint of suppressing thermal shrinkage and improving the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the nonaqueous secondary battery, and / or achieving a balance therebetween, the content of the inorganic particles contained in the inorganic porous layer is preferably 5% by mass to 99% by mass, and more preferably 10% by mass or more and less than 99% by mass, based on the total mass of the inorganic porous layer.

[0136] (Other preferred multilayer structures 2 to 4) Separators having the following multilayer structures 2 to 4 are also preferred. Any combination of the multilayer structures 1 to 4 is also preferred.

[0137] The separator having the multilayer structure 2 comprises a polyolefin microporous membrane as a substrate and a thermoplastic polymer-containing layer formed on at least one side of the polyolefin microporous membrane. The thermoplastic polymer contained in the thermoplastic polymer-containing layer preferably contains a polymerized unit of (meth)acrylic acid ester and / or (meth)acrylic acid, or at least one fluorine atom-containing polyvinyl compound selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE). The provision of the thermoplastic polymer-containing layer improves the adhesive strength between the electrodes and the separator, improving handling during battery production.

[0138] The separator having the multilayer structure 3 comprises a polyolefin microporous membrane as a substrate and an active layer disposed on at least one side of the polyolefin microporous membrane. The active layer is preferably at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene (polymer PVDF-HFP), polyvinylidene fluoride-chlorotrifluoroethylene (polymer PVDF-CTFE), PVDF homopolymer, a mixture of PVDF and tetrafluoroethylene-ethylene copolymer (ETFE), or vinylidene fluoride-tetrafluoroethylene-ethylene terpolymer, and more preferably at least one selected from the group consisting of polymer PVDF-HFP and polymer PVDF-CTFE. By copolymerizing HFP or CTFE with vinylidene fluoride, the crystallinity of the fluorine-based resin can be controlled within an appropriate range, so that the flow of the active layer can be suppressed during the adhesion treatment with the electrode. Furthermore, since the adhesive strength is improved during the adhesion treatment with the electrode, when the separator is used as a secondary battery separator, the interface is less likely to slip, and the crush test pass rate is improved.

[0139] Examples of PVDF include the Kynar Flex® series from Arkema, e.g. LBG, LBG8200, etc.; Solef (registered trademark) series of SOLVAY Co., Ltd., for example , grades 1015, 6020 etc.

[0140] Specific examples of polymeric PVDF-HFP include the Solef (registered trademark) series from SOLVAY Co., Ltd. For example, grades 21216 and 21510 (both of which are soluble in acetone). Specific examples of molecular PVDF-CTFE include the Solef® series from SOLVAY, e.g. For example, grade 31508 (soluble in acetone).

[0141] The separator having the multilayer structure 4 includes a polyolefin microporous film as a substrate, and a heat-resistant resin layer containing a heat-resistant resin laminated on at least one side of the polyolefin microporous film. The heat-resistant resin preferably contains at least one selected from the group consisting of wholly aromatic polyamide (also called aramid), polyimide, polyamideimide, polysulfone, polyketone, polyether, polyetherketone, polyetherimide, and cellulose. Among them, wholly aromatic polyamide is preferred from the viewpoint of durability, and para-type aromatic polyamide and / or meta-type aromatic polyamide are more preferred. In addition, meta-type aromatic polyamide is preferred from the viewpoint of formability of the porous layer and oxidation-reduction resistance. Examples of meta-type polyamide include polymetaphenylene isophthalamide, etc. In addition, examples of para-type polyamide include copolyparaphenylene-3.4'oxydiphenylene-terephthalamide, polyparaphenylene terephthalamide, etc. The heat-resistant resin layer preferably contains 30% to 90% by mass of inorganic matter having an average particle size of 0.2 μm to 0.9 μm. By providing the heat-resistant resin layer, thermal deformation of the separator is suppressed even when a local short circuit occurs inside the battery, and the crush test pass rate is improved.

[0142] The inorganic particles relating to multilayer structure 1 and / or 3, and the inorganic filler relating to multilayer structure 4 may be inorganic materials described later in the manufacturing method for a separator for a nonaqueous secondary battery, and among them, it is preferable that the inorganic material is at least one selected from the group consisting of alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, iron oxide, silicon nitride, titanium nitride, boron nitride, silicon carbide, aluminum oxide hydroxide, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, diatomaceous earth, silica sand, and glass fiber.

[0143] <Method for producing a separator for a non-aqueous secondary battery> (Method of manufacturing polyolefin microporous membrane) As a method for producing a separator for a non-aqueous secondary battery, the following will be described for the case where the polyolefin microporous membrane is a single-layer membrane (flat membrane), but it is not intended to exclude forms other than the flat membrane. The method for producing the microporous membrane according to embodiments 1 to 5 includes the following steps: (1) Sheet forming process; (2) Stretching process; (3) a porous body forming step; and (4) Heat treatment process; The method for producing the microporous membrane according to embodiments 1 to 5 may optionally include a resin modification step or kneading step before the sheet forming step (1), and / or a winding and slitting step after the heat treatment step (3), but preferably does not include a crosslinked structure formation step or a contact step with a crosslinking-promoting catalyst from the viewpoint of maintaining the crosslinking property of the microporous membrane until it is housed in a battery.

[0144] The crosslinked structure forming step includes (1) a sub-step of condensing a plurality of functional groups contained in the microporous membrane, (2) a sub-step of reacting a functional group contained in the microporous membrane with a chemical substance inside the battery, or (3) a sub-step of reacting a functional group contained in the microporous membrane with another functional group. The crosslinking-promoting catalyst is any catalyst capable of promoting a crosslinking reaction, such as (I) a condensation reaction of a plurality of identical functional groups, (II) a reaction between a plurality of different functional groups, (III) a chain condensation reaction between a functional group and an electrolyte, or (IV) a chain condensation reaction between a functional group and an additive. The crosslinking-promoting catalyst may be, for example, an organometallic catalyst.

[0145] (Method of manufacturing multilayer film) Next, a method for producing a separator for a non-aqueous secondary battery will be described below with reference to the case of a multilayer film. The method for producing a multilayer film includes the following steps: (1) Sheet forming process; (2) Stretching process; (3) Porous body formation process; (4) Heat treatment process; (5) Coating process; (6) a drying step; and (7) Assembly process and may include a water-washing step (5.5) between steps (5) and (6).

[0146] In the method for producing a multilayer film, a polyolefin microporous film is formed by carrying out steps (1) to (4) in the same manner as in the method for producing a monolayer film, and a coating step (5) is carried out in which a coating liquid is applied to at least one surface of the obtained polyolefin microporous film or the heat-treated porous body obtained by the heat treatment step (4), a drying step (6) is carried out in which the coating liquid is dried and removed, and an assembly step (7) is carried out in which a laminate of electrodes and separators or a roll thereof and a nonaqueous electrolyte are housed in an exterior body. Between steps (5) and (6), a water washing step (5.5) may be included in which a solvent component in the coating liquid is replaced with another solvent component. In addition, the method for producing a multilayer film is characterized in that a crosslinked structure of the silane-modified polyolefin contained in the multilayer film is formed in at least one of the coating step (5), the water washing step (5.5), the drying step (6), and the assembly step (7), and preferably, a crosslinked structure of the silane-modified polyolefin is formed in the coating step (5) and the assembly step (7).

[0147] Each step included in the method for producing a single layer film and a multilayer film will be described below.

[0148] In the kneading step, for example, a polyolefin, and optionally other resins, and a plasticizer or inorganic material can be kneaded using a kneader. From the viewpoint of suppressing the generation of resin aggregates in the production process and maintaining the crosslinking property of the microporous membrane until it is housed in a battery, it is preferable not to add a masterbatch resin containing a crosslinking-promoting catalyst to the kneaded mixture.

[0149] The polyolefin subjected to the kneading step or the sheet forming step (1) is not limited to an olefin homopolymer, but may be a polyolefin copolymerized with a monomer having a functional group, or a functional group-modified polyolefin. The functional group is a functional group capable of participating in the formation of a crosslinked structure, and may be, for example, the alkoxysilyl group described above. By preparing a silane-modified polyethylene (resin A) as a raw material, the resin modification step can be omitted.

[0150] On the other hand, if the polyolefin raw material does not have functional groups capable of participating in the formation of a crosslinked structure or the molar fraction of such functional groups is less than a predetermined ratio, the polyolefin raw material can be subjected to a resin modification process to incorporate functional groups into the resin backbone or increase the molar fraction of functional groups to obtain functional group-modified polyolefins. The resin modification process can be carried out by known methods. For example, the polyolefin raw material can be contacted with a reaction reagent by liquid spraying, gas spraying, dry mixing, immersion, coating, etc., so that crosslinkable functional groups can be introduced into the polyolefin backbone.

[0151] From the viewpoint of imparting to the separator the properties obtained by the Voronoi tessellation or the rate of change in air permeability before and after compression described above, as well as from the viewpoint of optimizing the crystal structure of the Si-containing molecule and the various values ​​described above for the SAXS and / or WAXS measurements and the Voronoi tessellation, it is preferable to prepare silane-modified polyethylene (resin A) as the polyolefin raw material, and it is more preferable to prepare not only resin A but also resin B and / or resin C described above.

[0152] From the viewpoint of uniform arrangement of Si-containing molecular structure and equilibrium life of coordination intermediate of Li complex; uniform extrusion and kneading; crystal structure of Si-containing molecule, and optimization of various values ​​described above for SAXS and / or WAXS measurement and Voronoi division, as described above, it is possible to carry out molecular design or blending in which resin A and resins B and C are specified. As described above, Si-containing molecules are present only in the amorphous part of polyolefin resin, and the equilibrium life of coordination intermediate of Li complex can be controlled by incorporating siloxane unit, C3, C4 unit of resin A into the overall design. On the other hand, by blending resin A with resins B and C, an appropriate amorphous entanglement structure can be constructed, and reaction selectivity by molecular orbital angle design as described in Non-Patent Document 1 can be developed to control thermal vibration of molecules, that is, from the viewpoint of thermodynamics, it is possible to control the equilibrium life of coordination intermediate of Li complex.

[0153] The content of resin A in the polyolefin raw material subjected to the sheet forming step (1) is preferably 3 to 70 mass%, more preferably 5 to 60 mass%, and even more preferably 10 to 50 mass%, based on the total mass of the solid content of the polyolefin raw material, not only from the viewpoint of imparting to the separator the properties obtained by the Voronoi tessellation described above, but also from the viewpoint of optimizing the crystal structure of the Si-containing molecule and the various values ​​described above for the SAXS and / or WAXS measurement and the Voronoi tessellation as described above.

[0154] From the same viewpoint as above, the content of resin B in the polyolefin raw material is preferably 3 to 70 mass %, more preferably 5 to 60 mass %, and even more preferably 5 to 40 mass %, based on the total mass of the solid content of the polyolefin raw material.

[0155] From the same viewpoint as above, the content of resin C in the polyolefin raw material is preferably 1 to 90 mass %, more preferably 5 to 60 mass %, and even more preferably 5 to 50 mass %, based on the total mass of the solid content of the polyolefin raw material.

[0156] From the same viewpoint as above, the mass ratio (A / B) of resin A to resin B used in the sheet molding step (1) is preferably 0.07 to 12.00, more preferably 0.10 to 11.00, and further preferably 0.50 to 10.00.

[0157] From the same viewpoint as above, the mass ratio (A / C) of resin A to resin C used in the sheet molding step (1) is preferably 0.07 to 12.00, more preferably 0.10 to 11.00, and further preferably 0.20 to 10.00.

[0158] From the same viewpoint as above, the mass ratio (B / C) of resin B to resin C used in the sheet molding step (1) is preferably 0.06 to 7.00, more preferably 0.10 to 7.00, and further preferably 0.12 to 6.90.

[0159] From the same viewpoint as above, the molecular weights Mn, Mw, Mv, or Mw / Mn of the resins A to C subjected to the sheet forming step (1) are preferably the same as those explained above for the separator components.

[0160] By appropriately controlling the molecular weight, molecular weight distribution, compounding ratio, and the like of the raw material subjected to the sheet forming step (1) as described above, the characteristics related to Voronoi tessellation of the separator according to the first to fifth embodiments can be easily achieved.

[0161] From the viewpoint of improving safety by suppressing thermal runaway upon battery destruction while maintaining low-temperature cycle properties and resistance to membrane rupture at high temperatures, it is preferable that in the sheet molding step, resin A is not a masterbatch resin that contains a catalyst that promotes the crosslinking reaction of alkoxysilyl groups before the sheet molding step.

[0162] The plasticizer used in the sheet forming step (1) is not particularly limited, but may be, for example, an organic compound capable of forming a homogeneous solution with polyolefin at a temperature below the boiling point. More specifically, decalin, xylene, dioctyl phthalate, dibutyl phthalate, stearyl alcohol, oleyl alcohol, decyl alcohol, nonyl alcohol, diphenyl ether, n-decane, n-dodecane, paraffin oil, etc. are included. Among these, paraffin oil and dioctyl phthalate are preferred. The plasticizer may be used alone or in combination of two or more. The ratio of the plasticizer is not particularly limited, but from the viewpoint of the porosity of the obtained microporous film, the polyolefin and the silane-modified polyolefin are preferably 20% by mass or more based on the total mass as necessary, and from the viewpoint of the viscosity during melt kneading, it is preferably 90% by mass or less.

[0163] The sheet forming step (1) is a step of extruding the obtained kneaded product or a mixture of polyolefin and plasticizer with an extruder, cooling and solidifying it, and forming and processing it into a sheet to obtain a sheet. The method of forming the sheet is not particularly limited, but for example, a method of solidifying the melted product extruded by melt kneading and compression cooling or deformation cooling can be mentioned. The cooling method can be a method of directly contacting the melt with a cooling medium such as cold air or cooling water, a method of contacting the melt with a roll or press cooled with a refrigerant, etc., and the method of contacting the melt with a roll or press cooled with a refrigerant is preferred in terms of excellent film thickness controllability.

[0164] The stretching step (2) is a step of extracting a plasticizer or an inorganic material from the obtained sheet as necessary, and further stretching the sheet in at least one axial direction. Examples of the sheet stretching method include MD uniaxial stretching by a roll stretching machine, TD uniaxial stretching by a tenter, sequential biaxial stretching by a combination of a roll stretching machine and a tenter or a tenter and a tenter, and simultaneous biaxial stretching by a simultaneous biaxial tenter or inflation molding. From the viewpoint of obtaining a more uniform film, simultaneous biaxial stretching is preferable. The total areal magnification is preferably 8 times or more, more preferably 15 times or more, and even more preferably 20 times or more or 30 times or more, from the viewpoint of the uniformity of the film thickness, the balance between the tensile elongation, the porosity, and the average pore size. By having a total areal magnification of 8 times or more, it tends to be easy to obtain a film with high strength and good thickness distribution. In addition, from the viewpoint of preventing breakage, this areal magnification may be 250 times or less.

[0165] The porous body forming step (3) is a step of extracting the plasticizer from the stretched product after the stretching step to make the stretched product porous. The method of extracting the plasticizer is not particularly limited, but examples thereof include a method of immersing the stretched product in an extraction solvent and a method of showering the stretched product with the extraction solvent. The extraction solvent is not particularly limited, but for example, it is preferably a poor solvent for polyolefin and a good solvent for plasticizers or inorganic materials, and has a boiling point lower than the melting point of polyolefin. Such an extraction solvent is not particularly limited, but examples thereof include hydrocarbons such as n-hexane or cyclohexane; halogenated hydrocarbons such as methylene chloride or 1,1,1-trichloroethane, and fluorocarbons; alcohols such as ethanol or isopropanol; ketones such as acetone or 2-butanone; and alkaline water. The extraction solvent may be used alone or in combination of two or more types.

[0166] The heat treatment step (4) is a step of extracting a plasticizer from the sheet as necessary after the stretching step, and further performing heat treatment to obtain a microporous membrane. The heat treatment method is not particularly limited, but examples include a heat setting method in which stretching and relaxation operations are performed using a tenter or roll stretching machine. The relaxation operation refers to a reduction operation performed at a predetermined temperature and relaxation rate in the machine direction (MD) and / or transverse direction (TD) of the membrane. The relaxation rate refers to the value obtained by dividing the MD dimension of the membrane after the relaxation operation by the MD dimension of the membrane before the operation, or the value obtained by dividing the TD dimension of the membrane after the relaxation operation by the TD dimension of the membrane before the operation, or the value obtained by multiplying the relaxation rate of MD and the relaxation rate of TD when both MD and TD are relaxed. It is preferable that the stretching and relaxation operation in the heat treatment step (4) is performed at least in TD.

[0167] In the coating step (5), a coating liquid is applied to at least one surface of the polyolefin microporous membrane obtained as described above, or to at least one surface of the heat-treated porous body obtained by the heat treatment step (4). A known coating method can be used for the coating step (5), and examples of the method include a method in which a coating liquid is applied to a substrate, a microporous membrane, or a heat-treated porous body, a method in which the raw material of the microporous membrane and the raw material of another layer are laminated and extruded by a coextrusion method, and a method in which both layers are produced separately and then bonded together.

[0168] More specifically, the coating step (5) may be any one or any combination of the following steps (5A) to (5D): (5A) a coating step of applying a coating liquid containing inorganic particles, a resin binder, and a surfactant and having a pH of 6.7 or less or 7.5 or more to at least one surface of the polyolefin microporous monolayer membrane or the heat-treated porous body to form an inorganic porous layer on at least one surface of the polyolefin microporous monolayer membrane or the heat-treated porous body; (5B) a coating step of applying a coating liquid containing a thermoplastic polymer and a surfactant and having a pH of 6.7 or less or 7.5 or more to at least one surface of the polyolefin microporous monolayer membrane or the heat-treated porous body to form a thermoplastic polymer-containing layer on at least one surface of the polyolefin microporous monolayer membrane or the heat-treated porous body; (5C) a coating step of forming an active layer on at least one surface of the polyolefin microporous monolayer film or the heat-treated porous body by applying a coating liquid containing a fluorine atom-containing polyvinyl compound, inorganic particles, and an organic solvent to at least one surface of the polyolefin microporous monolayer film or the heat-treated porous body; and (5D) A coating step of applying a coating liquid containing a heat-resistant resin and an organic solvent to at least one surface of a polyolefin microporous monolayer membrane or a heat-treated porous body to form a heat-resistant resin layer on at least one surface of the polyolefin microporous monolayer membrane or the heat-treated porous body.

[0169] By the coating step (5A), a multilayer film comprising a microporous polyolefin film and an inorganic porous layer according to the preferred multilayer structure 1 described above can be formed.

[0170] By the coating step (5B), a multilayer film comprising a microporous polyolefin film and a thermoplastic polymer-containing layer according to the preferred multilayer structure 2 described above can be formed.

[0171] By the coating step (5C), a multilayer film can be formed comprising a microporous polyolefin film and an active layer according to the preferred multilayer structure 3 described above.

[0172] By the coating step (5D), a multilayer film including a microporous polyolefin film and a heat-resistant resin layer according to the preferred multilayer structure 4 described above can be formed.

[0173] In the coating steps (5A) and (5B), if the pH of the aqueous or non-aqueous coating liquid is 6.7 or less, the active energy of the reaction system of the silane-modified polyolefin in contact with the coating liquid is reduced, making the silane crosslinking reaction more likely to occur. On the other hand, if the pH of the aqueous or non-aqueous coating liquid is 7.5 or more, the OH - The presence of the silane crosslinking reaction of the silane-modified polyolefin can be accelerated.

[0174] In the coating steps (5C) and (5D), the organic solvent contained in the nonaqueous coating liquid penetrates into the amorphous parts of the polyolefin microporous monolayer membrane or the heat-treated porous body, thereby promoting the silane crosslinking reaction of the silane-modified polyolefin.

[0175] The coating liquid for forming the thermoplastic polymer-containing layer contains a thermoplastic polymer, and the thermoplastic polymer preferably contains at least one selected from the group consisting of polymerized units of (meth)acrylic acid ester and / or (meth)acrylic acid, polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE).

[0176] The coating liquid for forming the active layer contains a fluorine atom-containing polyvinyl compound, and the fluorine atom-containing polyvinyl compound is preferably at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE).

[0177] If desired, the coating liquid may contain a resin binder, inorganic particles or inorganic filler, a dispersant, a surfactant, a solvent, etc. The coating liquid for forming the inorganic porous layer contains inorganic particles and a resin binder.

[0178] Examples of the resin binder include the following: Polyolefin resins such as polyethylene, polypropylene, and α-polyolefin; Fluorine-based polymers such as polyvinylidene fluoride and polytetrafluoroethylene, or copolymers containing these; Diene-based polymers containing conjugated dienes such as butadiene and isoprene as monomer units, copolymers containing these, or hydrogenated products thereof; An acrylic polymer containing a (meth)acrylate, (meth)acrylic acid, or the like as a monomer unit and having no polyalkylene glycol unit, an acrylic polymer containing a (meth)acrylate, (meth)acrylic acid, or the like as a monomer unit and having one or two polyalkylene glycol units, or a copolymer containing these, or a hydrogenated product thereof; Rubbers such as ethylene propylene rubber, polyvinyl alcohol, and polyvinyl acetate; Polyalkylene glycols having no polymerizable functional groups, such as polyethylene glycol and polypropylene glycol; Resins such as polyphenylene ether, polyphenylene sulfide, and polyester; A copolymer having, as a copolymerization unit, an ethylenically unsaturated monomer having 3 or more repeating alkylene glycol units; and Combinations of these; or the above-mentioned thermoplastic polymers can be employed. Among these, from the viewpoint of improving safety in a puncture test of a battery including the separator, it is preferable that the resin binder contains polymerized units of a (meth)acrylic acid ester and / or (meth)acrylic acid.

[0179] The resin binder described above can be produced by a known polymerization method using the corresponding monomer or comonomer, such as solution polymerization, emulsion polymerization, bulk polymerization, or the like.

[0180] For resin binders, it is preferred to form a particulate binder polymer by emulsion polymerization, thereby using the resulting polymer emulsion as the water-based latex.

[0181] The coating liquid for forming the inorganic porous layer, active layer or heat-resistant resin layer contains inorganic particles or inorganic fillers.The inorganic particles or inorganic fillers are not particularly limited, but include oxide ceramics such as alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, aluminum hydroxide, aluminum oxide hydroxide, potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fibers.These may be used alone or in combination.

[0182] Among these, from the viewpoint of improving the electrochemical stability and heat resistance of the separator, at least one selected from the group consisting of alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, iron oxide, silicon nitride, titanium nitride, boron nitride, silicon carbide, aluminum oxide hydroxide, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, diatomaceous earth, silica sand, and glass fiber is preferred, and aluminum oxide compounds such as alumina and aluminum oxide hydroxide; and aluminum silicate compounds having no ion exchange capacity such as kaolinite, dickite, nacrite, halloysite, and pyrophyllite are more preferred.

[0183] Alumina has many crystal forms, such as α-alumina, β-alumina, γ-alumina, and θ-alumina, and any of these can be suitably used. Among these, α-alumina is preferred because it is thermally and chemically stable.

[0184] As the aluminum oxide compound, aluminum oxide hydroxide (AlO(OH)) is particularly preferred. As the aluminum oxide hydroxide, boehmite is more preferred from the viewpoint of preventing internal short circuits caused by the generation of lithium dendrites. For example, by employing particles mainly composed of boehmite as the inorganic filler constituting the heat-resistant resin layer, a very lightweight porous layer can be realized while maintaining high permeability, and even in a thinner porous layer, the thermal shrinkage of the microporous film at high temperatures is suppressed, tending to exhibit excellent heat resistance. Synthetic boehmite, which can reduce ionic impurities that adversely affect the characteristics of electrochemical devices, is even more preferred.

[0185] The content of inorganic particles in the coating liquid for forming the inorganic porous layer is preferably 5% by mass to 99% by mass, and more preferably 10% by mass or more and less than 99% by mass, based on the mass of the total solid content of the coating liquid.

[0186] The inorganic filler contained in the coating liquid for forming the heat-resistant resin layer preferably has an average particle size of 0.2 μm to 0.9 μm, and / or the content of the inorganic filler in the coating liquid is preferably 30% by mass to 90% by mass based on the mass of the total solid content of the coating liquid.

[0187] Examples of the dispersant contained in the coating liquid include an aqueous solution of ammonium polycarboxylate, etc. Examples of the surfactant contained in the coating liquid include an emulsifier and a soap.

[0188] Examples of the solvent contained in the coating liquid include water (e.g., ion-exchanged water, pure water, etc.), aqueous solvents (e.g., a mixture of water and alcohol, etc.), organic solvents, etc. Examples of the organic solvent that may be used include alcohol, N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMA), ethanol, toluene, hot xylene, methylene chloride, hexane, etc.

[0189] Examples of methods for preparing a coating liquid containing inorganic particles or an inorganic filler include mechanical stirring methods using a ball mill, a bead mill, a planetary ball mill, a vibrating ball mill, a sand mill, a colloid mill, an attritor, a roll mill, high-speed impeller dispersion, a disperser, a homogenizer, a high-speed impact mill, ultrasonic dispersion, and a stirring blade.

[0190] Examples of methods for applying a coating liquid containing inorganic particles or an inorganic filler include a gravure coater method, a small diameter gravure coater method, a reverse roll coater method, a transfer roll coater method, a kiss coater method, a dip coater method, a knife coater method, an air doctor coater method, a blade coater method, a rod coater method, a squeeze coater method, a cast coater method, a die coater method, a screen printing method, and a spray coating method.

[0191] In the coating step (5D), after the formation of the coating film, a step of introducing the coating film into an atmosphere with a humidity of 50% or more or blowing steam onto the coated surface may be included. By providing humidity to the coated surface, the precipitation of the aramid resin can be promoted.

[0192] In the drying step (6), the solvent is removed from the coating film formed in the coating step (5). Methods for removing the solvent include a method of drying at a temperature below the melting point of the material constituting the microporous film, a method of drying under reduced pressure at a low temperature, a method of replacing the solvent contained in the coating liquid with another solvent and then drying, and the like. In addition, as long as it does not significantly affect the characteristics of the nonaqueous secondary battery, a part of the solvent may remain. Methods for replacing the solvent contained in the coating liquid with another solvent include a method of immersing the film in the other solvent described above; a method of spraying the other solvent described above onto the film, and the like.

[0193] In the water washing step (5.5), the solvent in the coating film formed in the coating step (5) may be replaced with another solvent. Examples of the solvent before the replacement include DMF, DMA, NMP, DMSO, etc., and examples of the solvent after the replacement include water, alcohol, etc.

[0194] The method for producing a separator may optionally include a winding / slitting step, in which the obtained microporous membrane is slit, if necessary, and wound around a predetermined core.

[0195] In the assembly step (7), the laminate of electrodes and separators or a wound body thereof and the nonaqueous electrolyte are housed in an exterior body. Step (7) can be performed in the same manner as in the manufacture of a nonaqueous secondary battery described below, and the electrodes, nonaqueous electrolyte, and exterior body used in step (7) may be those described for a nonaqueous secondary battery.

[0196] In the coating step (5) and / or the water-washing step (5.5) and / or the drying step (6) and / or the assembling step (7), preferably in the coating step (5), the water-washing step (5.5), the drying step (6) and the assembling step (7), the silane-modified polyolefin contained in the separator forms a crosslinked structure.

[0197] The separator obtained by the method including the various steps described above can be used in a nonaqueous secondary battery including a positive electrode and a negative electrode capable of absorbing and releasing lithium, and a nonaqueous electrolyte solution obtained by dissolving an electrolyte in a nonaqueous solvent, and can be preferably used in a lithium secondary battery or a lithium ion secondary battery.

[0198] <Non-aqueous secondary battery> A non-aqueous secondary battery is configured by housing a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution in any battery exterior body.

[0199] The positive electrode is connected to a positive electrode lead body within the nonaqueous secondary battery, and the negative electrode is connected to a negative electrode lead body within the nonaqueous secondary battery. One end of each of the positive electrode lead body and the negative electrode lead body is extended to the outside of the battery exterior body so that they can be connected to external devices, etc., and their ionomer portions are heat-fused to one side of the battery exterior body.

[0200] The positive electrode is composed of a positive electrode current collector and a positive electrode active material layer. The negative electrode is composed of a negative electrode current collector and a negative electrode active material layer. The positive electrode active material layer contains a positive electrode active material, and the negative electrode active material layer contains a negative electrode active material. The positive electrode and the negative electrode are arranged with the separator interposed between them such that the positive electrode active material layer and the negative electrode active material layer face each other.

[0201] As the positive electrode, a known battery positive electrode can be used, and from the viewpoint of the effect of the present invention, a positive electrode that is easily thermally decomposed or releases O2 can also be used. In addition, a composite positive electrode active material of lithium and another metal can be used, and a composite positive electrode of at least one metal selected from the group consisting of nickel, manganese, and cobalt and lithium, such as an LNO positive electrode, an NCA positive electrode, an LCO positive electrode, or a positive electrode containing a lithium (Li)-nickel (Ni)-manganese (Mn)-cobalt (Co) composite oxide as a positive electrode active material (NMC positive electrode), can also be used.

[0202] Among them, from the viewpoint of the action and effect of the present invention, an NMC positive electrode is preferable, and among NMC positive electrodes, one having a relatively high nickel content is more preferably used, and the molar ratio of the amount of nickel (Ni) to the total amount of nickel, manganese and cobalt in the positive electrode is more preferably 3 to 9, 5 to 9, 6 to 9, 5 to 8, or 6 to 8, and particularly preferably 5 to 9. Specifically, the formula: Li-Ni x -Mn y -Co z In a positive electrode containing a lithium (Li)-nickel (Ni)-manganese (Mn)-cobalt (Co) composite oxide represented by the formula: {wherein x represents the Ni proportion, y represents the Mn proportion, z represents the Co proportion, and x+y+z=1}, it is preferable that the Ni proportion x in the formula is 5 to 9.

[0203] The positive electrode current collector can be made of a metal foil such as an aluminum foil, a nickel foil, or a stainless steel foil.

[0204] Examples of the negative electrode active material constituting the negative electrode include carbon materials such as hard carbon, graphite, pyrolytic carbon, coke, glassy carbon, baked bodies of organic polymer compounds, microbeads, carbon fibers, activated carbon, carbon colloids, and carbon black, as well as metallic lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon (Si)-containing materials, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. The negative electrode active material may be used alone or in combination of two or more.

[0205] Among them, from the viewpoint of the action and effect of the present invention, a Si-containing material is preferable as the negative electrode active material, and examples thereof include silicon, Si alloys, Si oxides, etc. From the same viewpoint, the Si ratio in the negative electrode active material is preferably 5 to 90 mol %.

[0206] It is known that the lithium ion storage capacity of the Si-containing negative electrode active material is significantly improved compared to the carbon material negative electrode, and at the same time, as the lithium ions are charged and discharged to and from the Si-containing particles, the Si-containing negative electrode active material undergoes a large volume expansion and contraction as shown in Non-Patent Document 2. At that time, the battery internal volume is constant, and the separator is greatly compressed or deformed in the thickness direction by the Si-containing negative electrode active material. According to the present invention, it has been found that, by adjusting the type and composition of the resin raw material, optimizing the various values ​​described above for the SAXS and / or WAXS measurement of the separator and the Voronoi division, it is possible to maintain permeability even when the separator is compressed or deformed in the thickness direction in a non-aqueous secondary battery, and to have an excellent balance between strength and ion diffusivity, and to improve the crush test pass rate, cycle test capacity retention rate, and high-temperature cycle life of the non-aqueous secondary battery, and / or to achieve a good balance between them.

[0207] Furthermore, the separator discovered by the present invention, which has a structure in which Si atoms are dispersed in a state other than a sea-island structure, allows the intercalation reaction into the Si-containing negative electrode active material to proceed uniformly, as described above, which leads to uniform expansion and contraction of the Si-containing negative electrode active material inside the battery, and can suppress deviation of the wound structure inside the battery, thereby achieving improvement in battery cycle performance and improvement in battery safety.

[0208] The negative electrode current collector can be made of a metal foil such as a copper foil, a nickel foil, or a stainless steel foil.

[0209] <Nonaqueous electrolyte> In this specification, the non-aqueous electrolyte refers to an electrolyte solution containing an electrolyte in a non-aqueous solvent, and the amount of water is 1 mass% or less based on the total mass. The non-aqueous electrolyte solution is preferably as free of water as possible, but may contain a very small amount of water. The content of such water is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, based on the total amount of the non-aqueous electrolyte solution.

[0210] The electrolyte in the battery may contain water, and the water contained in the system after the battery is produced may be water contained in the electrolyte, or water carried in from components such as electrodes or separators. The electrolyte may contain a non-aqueous solvent. Examples of the solvent contained in the non-aqueous solvent include alcohols such as methanol and ethanol; aprotic solvents, etc. Among them, aprotic solvents are preferred as the non-aqueous solvent.

[0211] Examples of aprotic solvents include cyclic carbonates, fluoroethylene carbonates, lactones, organic compounds having sulfur atoms, chain fluorinated carbonates, cyclic ethers, mononitriles, alkoxy group-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, and compounds in which some or all of the H atoms of the above aprotic solvents have been substituted with halogen atoms.

[0212] Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, trans-2,3-butylene carbonate, cis-2,3-butylene carbonate, 1,2-pentylene carbonate, trans-2,3-pentylene carbonate, cis-2,3-pentylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinylethylene carbonate.

[0213] Examples of fluoroethylene carbonate include 4-fluoro-1,3-dioxolan-2-one, 4,4-difluoro-1,3-dioxolan-2-one, cis-4,5-difluoro-1,3-dioxolan-2-one, trans-4,5-difluoro-1,3-dioxolan-2-one, 4,4,5-trifluoro-1,3-dioxolan-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolan-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolan-2-one.

[0214] Examples of lactones include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone.

[0215] Examples of organic compounds having a sulfur atom include ethylene sulfite, propylene sulfite, butylene sulfite, pentene sulfite, sulfolane, 3-sulfolene, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propene 1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite.

[0216] Examples of the chain carbonate include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, and ethyl propyl carbonate.

[0217] Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane.

[0218] Examples of mononitriles include acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile.

[0219] Examples of alkoxy-substituted nitriles include methoxyacetonitrile and 3-methoxypropionitrile.

[0220] Examples of dinitriles include malononitrile, succinonitrile, methylsuccinonitrile, glutaronitrile, 2-methylglutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanonane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, 2,4-dimethylglutaronitrile, and ethylene glycol bis(propionitrile) ether.

[0221] Examples of cyclic nitriles include benzonitrile.

[0222] Examples of short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl hydroangelate, methyl caproate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl hydroangelate, ethyl caproate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl hydroangelate, propyl caproate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, isopropyl valerate, and isopropyl pivalate. , isopropyl hydroangelate, isopropyl caproate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl pivalate, butyl hydroangelate, butyl caproate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl pivalate, isobutyl hydroangelate, isobutyl caproate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl pivalate, tert-butyl hydroangelate, and tert-butyl caproate.

[0223] Examples of chain ethers include dimethoxyethane, diethyl ether, 1,3-dioxolane, diglyme, triglyme, and tetraglyme. The fluorinated ethers include, for example, those represented by the general formula Rf aa -OR bb (In the formula, Rf aa is an alkyl group containing a fluorine atom, and R bb is an organic group which may contain a fluorine atom). Examples of ketones include acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0224] Examples of the above-mentioned aprotic solvent compounds in which some or all of the H atoms have been substituted with halogen atoms include compounds in which the halogen atoms are fluorine.

[0225] Here, examples of fluorinated chain carbonates include methyl trifluoroethyl carbonate, trifluorodimethyl carbonate, trifluorodiethyl carbonate, trifluoroethylmethyl carbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, and methyl 2,2,3,3-tetrafluoropropyl carbonate. The above-mentioned fluorinated chain carbonates are represented by the following general formula: R cc -OC(O)OR dd {where, R cc and R dd is CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, and the formula CH2Rf ee (In the formula, Rf ee is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is substituted with at least one fluorine atom), and R cc and / or R dd contains at least one fluorine atom. It can be expressed as:

[0226] Examples of fluorinated short-chain fatty acid esters include fluorinated short-chain fatty acid esters such as 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, and 2,2,3,3-tetrafluoropropyl acetate. Fluorinated short-chain fatty acid esters are represented by the following general formula: R ff -C(O)OR gg {where, R ff is CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, CF3CF2H, CFH2, CF2H, CF2Rf hh , CFHRf hh, and CH2Rf ii and R gg is CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, and CH2Rf ii Rf is at least one selected from the group consisting of hh is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom may be substituted with at least one fluorine atom, and Rf ii is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is substituted with at least one fluorine atom, and R ff and / or R gg contains at least one fluorine atom, and R ff If is CF2H, R gg is not CH3}.

[0227] From the viewpoint of the effects of the present invention, the non-aqueous electrolyte preferably contains ethyl methyl carbonate (EMC) and / or acetonitrile (AcN) as a non-aqueous solvent, and / or the total content of EMC and AcN in the non-aqueous electrolyte is preferably within the range of 50% by mass to 90% by mass.

[0228] The electrolyte is preferably a lithium salt, and from the viewpoint of promoting the silane crosslinking reaction, a fluorine-containing lithium salt that generates hydrogen fluoride (HF) is more preferable. Examples of the fluorine-containing lithium salt include lithium hexafluorophosphate (LiPF6), lithium fluorosulfonate (LiFSO3), lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiN(SO2F)2), lithium borofluoride (LiBF4), and lithium bisoxalate borate (LiBC4O8). Without being bound by theory, for example, when the electrolyte contains LiPF6, LiPF6 reacts with a small amount of moisture contained in the power storage device (for example, moisture contained in components such as electrodes, separators, and electrolyte) to generate HF or a fluorine-containing organic substance derived from HF. It is believed that the HF or fluorine-containing organic substances derived from the HF dissolve in the electrolyte, and swell and diffuse into the amorphous portion of the polyolefin having crosslinkable silane groups, thereby catalyzing the silane crosslinking reaction.

[0229] From the viewpoint of the effect of the present invention, the non-aqueous electrolyte preferably has a relatively high concentration of lithium salt, more preferably contains lithium salt at a concentration in the range of 1.2 mol / L to 10 mol / L, further preferably contains lithium salt at a concentration of 1.5 mol / L or more, and particularly preferably contains lithium salt at a concentration of 3.0 mol / L or more. In particular, in a non-aqueous secondary battery system containing lithium hexafluorophosphate (LiPF6) as an electrolyte, due to the Jan-Teller effect of phosphorus atoms, it exists as a certain concentration of dissociated F anion or lithium fluoride (LiF) in the system. Generally, a phenomenon of a decrease in battery life such as electrode corrosion due to dissociated F anion is known, but LiF exhibits a stronger Lewis acid effect when added to Si than in the state before addition, which makes the above phenomena (a) and (b) more prominent, and thus also exhibits good low-temperature cycle characteristics. It is preferable to select a combination of the electrolyte and the electrolyte so that the concentration of the lithium salt does not exceed the saturated solubility concentration.

[0230] The non-aqueous electrolyte may contain, as a catalyzing agent for the silane crosslinking reaction, an inorganic acid or an organic acid, which reacts with a trace amount of moisture contained in the non-aqueous electrolyte to generate hydrogen ions (acid source), or an alkali source, which reacts with a trace amount of moisture contained in the non-aqueous electrolyte to generate hydroxide ions. Examples of the alkali source include alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkali metal phosphates, ammonia, and amine compounds. Among these, from the viewpoint of the safety and silane crosslinking of the power storage device, alkali metal hydroxides or alkaline earth metal hydroxides are preferred, alkali metal hydroxides are more preferred, and sodium hydroxide is even more preferred.

[0231] The battery exterior of the non-aqueous secondary battery may have a known structure, for example, a battery can or a laminate film exterior.

[0232] The shape of the nonaqueous secondary battery may be, for example, a square type, a rectangular cylinder type, a cylindrical type, an elliptical type, a button type, a coin type, a flat type, a laminate type, or the like.

[0233] The nonaqueous secondary battery can be produced in the same manner as known production methods, except that the above-mentioned nonaqueous electrolyte, positive electrode, negative electrode, separator, and battery exterior body are used. EXAMPLES

[0234] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The physical properties in the examples were measured by the following methods. For the substrate basis weight, substrate thickness, substrate porosity, substrate air permeability, substrate pin puncture strength, SAXS, WAXS, NMR, and TOF-SIMS, the coating layer was scraped off when there was a coating layer on the substrate, and then the measurements were performed. For the crush test pass rate, cycle test capacity retention rate, and cycle life test, the coating layer was not scraped off even when there was a coating layer on the substrate. The battery evaluation tests (crush test, cycle capacity retention rate, high temperature cycle life) were all performed 4 days after the coating liquid was applied to the separator.

[0235] <Method for detecting silane-modified polyolefin contained in separator> In the crosslinked state, the silane-modified polyolefin contained in the separator is insoluble or has insufficient solubility in organic solvents, so that it may be difficult to measure the content of the silane-modified polyolefin directly from the separator. In this case, as a pretreatment of the sample, methyl orthoformate, which does not cause side reactions, is used to decompose the siloxane bond into methoxysilanol, and then a solution NMR measurement is performed to detect the silane-modified polyolefin contained in the separator or to perform a GPC measurement. The pretreatment experiment can be performed with reference to Japanese Patent No. 3529854 and Japanese Patent No. 3529858. After the depolymerization reaction, thermal analysis such as TMA and DMA is also possible.

[0236] Specifically, the silane-modified polyolefin used as a raw material in the manufacture of separators 1 H or 13 The C NMR identification can be used to detect silane-modified polyolefins contained in separators. 1 H and 13 An example of a C NMR measurement technique is described below.

[0237] ( 1 H NMR measurement) The sample was dissolved in o-dichlorobenzene-d4 at 140°C, and the proton resonance frequency was 600 MHz.1 Obtain H-NMR spectra. 1 The H-NMR measurement conditions are as follows. Equipment: Bruker AVANCE NEO 600 Sample tube diameter: 5mmφ Solvent: o-dichlorobenzene-d4 Measurement temperature: 130℃ Pulse angle: 30° Pulse waiting time: 1sec Accumulation count: 1000 times or more Sample concentration: 1 wt / vol%

[0238] ( 13 C NMR measurement) The sample was dissolved in o-dichlorobenzene-d4 at 140°C. 13 Obtain a C-NMR spectrum. 13 The measurement conditions for C-NMR are as follows: Equipment: Bruker AVANCE NEO 600 Sample tube diameter: 5mmφ Solvent: o-dichlorobenzene-d4 Measurement temperature: 130℃ Pulse angle: 30° Pulse waiting time: 5sec Accumulation count: 10,000 times or more Sample concentration: 10 wt / vol%

[0239] 1 H and / or 13 By measuring C NMR, it is possible to confirm the amount of silane unit modification in the silane-modified polyolefin, the amount of alkyl group modification in the polyolefin, the C4 unit modification rate (mol%), and the number of methylene (CH2) in the silane graft linkage in the polyolefin raw material, and it is also possible to identify the content of silane-modified polyolefin in the separator. The amount of modified silanol units in resin A was quantified by the NMR chemical shift and integral value of the methylene next to the Si atom (-CH2-Si: 1 H, 0.69 ppm, t; 13C, 6.11 ppm, s) can be determined. Propylene modification (C3) can be quantified by the NMR chemical shift and integral value of the terminal methyl group (-CH3: 13 C, 19.42 ppm, s) can be determined. Butene modification (C4) can be quantified by the NMR chemical shift and integral value of the terminal methyl group (-CH3: 13 C, 10.63 ppm, s) is possible.

[0240] <Weight average molecular weight and number average molecular weight> A calibration curve was created by measuring standard polystyrene under the following conditions using a Waters ALC / GPC 150C (trademark). Chromatograms were also measured under the same conditions for each of the following polymers, and the weight-average molecular weight of each polymer was calculated based on the calibration curve by the following method. Column: Tosoh GMH6-HT (trademark) x 2 + GMH6-HTL (trademark) x 2 Mobile phase: o-dichlorobenzene Detector: Differential refractometer Flow rate: 1.0ml / min Column temperature: 140℃ Sample concentration: 0.1wt%

[0241] (Weight average molecular weight and number average molecular weight of polyethylene, polypropylene and silane-modified polyolefin) Each molecular weight component in the obtained calibration curve was multiplied by 0.43 (Q factor of polyethylene / Q factor of polystyrene = 17.7 / 41.3) or 0.64 (Q factor of polypropylene / Q factor of polystyrene = 26.4 / 41.3) to obtain a molecular weight distribution curve converted into polyethylene or polypropylene, and the weight average molecular weight and number average molecular weight were calculated. Note that the same Q factor as polyethylene was used for silane-modified polyethylene, and the same Q factor as polypropylene was used for silane-modified polypropylene. (Weight average molecular weight of resin composition) The weight average molecular weight was calculated using the Q factor value of the polyolefin with the largest mass fraction, and otherwise in the same manner as in the case of polyethylene.

[0242] <Viscosity average molecular weight (Mv)> The intrinsic viscosity [η] in decalin solvent at 135°C was determined based on ASTM-D4020. The Mv of polyethylene and silane-modified polyethylene was calculated using the following formula. [η]=6.77×10 -4 Mv 0.67 The Mv of polypropylene was calculated using the following formula. [η]=1.10×10 -4 Mv 0.80

[0243] <Melt mass flow rate (MFR) (g / 10min)> Using a melt mass flow rate measuring instrument (Melt Indexer F-F01) manufactured by Toyo Seiki, the weight of the resin extruded in 10 minutes at 190°C and a load of 2.16 kg was determined as the MFR value for polyethylene and silane-modified polyethylene. The MFR value for polypropylene and silane-modified polypropylene was measured at 230°C.

[0244] <Film thickness (μm)> The thickness of the microporous membrane was measured using a micro thickness gauge (KBM (trademark)) manufactured by Toyo Seiki Seisakusho Co., Ltd.) at room temperature of 23±2° C. and a relative humidity of 60%. Specifically, the thickness was measured at five points at approximately equal intervals across the entire width in the TD direction, and the average value was obtained. The coating thickness is calculated by observing the cross section or side surface at any magnification using a SEM.

[0245] <Porosity (%) and substrate porosity (%)> A 10 cm x 10 cm square sample was cut from the microporous membrane and its volume (cm 3 ) and mass (g), and then calculate the density (g / cm 3 ) and the porosity was calculated using the following formula: The density of the mixed composition was determined by calculating the density of each of the raw materials used and the mixing ratio. Porosity (%) = (volume-mass / density of mixed composition) / volume x 100

[0246] <Air permeability (sec / 100cm 3 ) and base material air permeability (sec / 100cm 3 )> In accordance with JIS P-8117 (2009), the air permeability of the sample was measured using the Oken air permeability and smoothness tester, EGO1-55-1MR (trademark), manufactured by Asahi Seiko Co., Ltd.

[0247] <Puncture strength (gf) and base material puncture strength (gf)> Using a handy deformation tester "KES-G5" (manufactured by Kato Tech Co., Ltd., trademark), the puncture strength of the microporous membrane was determined by conducting a puncture test under the conditions of a needle tip curvature radius of 0.5 mm and a puncture speed of 2 mm / sec.

[0248] <SAXS (transmission method) measurement and crystal long period (nm)> Small-angle X-ray scattering (SAXS) by the transmission method of the microporous membrane made of polyolefin as the separator base material was measured under the following conditions. (Measurement) Using a Nano-Viewer manufactured by Rigaku Corporation, small-angle X-ray scattering (SAXS) measurement by the transmission method was performed. CuKα rays were irradiated onto the separator base material as the sample (however, the X-ray incident direction was parallel to the film thickness direction of the sample), and scattering was detected by PILATUS 100K manufactured by DECTRIS. The measurement was carried out under the conditions of a distance of 841.5 mm between the sample and the detector, an output of 60 kV, and 45 mA. The optical system adopted a point focus, and the slit diameters were 1st slit: ψ = 0.4 mm, 2nd slit: ψ = 0.2 mm, and guard slit: = 0.8 mm. As a pretreatment for the measurement, in order to reduce scattering due to particle size, a slurry was prepared by mixing the sample and propylene glycol at a weight ratio of 1:1 and measured.

[0249] (Analysis: Crystal long period (nm)) Regarding the obtained peaks, the analysis of the crystal long period was carried out by the following method. For the X-ray scattering pattern obtained from the imaging plate, air cell scattering correction was performed, and a one-dimensional SAXS profile I(q) was obtained by circular averaging. Here, q is the absolute value of the scattering vector. To calculate the crystal long period d, the square of the absolute value of the scattering vector was multiplied by the SAXS profile to emphasize the scattering derived from the crystal long period. Subsequently, the product of the SAXS profile multiplied by the square of the absolute value of the scattering vector and the absolute value of the scattering vector were each logarithmically plotted with base 10, with the vertical and horizontal axes. The horizontal axis is log 10 q, and the vertical axis is log 10 (I(q)×q2). For the plotted data, tangents were drawn so as to touch one point each on the small-angle side and the wide-angle side from the peak position derived from the lamella, and an operation of subtracting the tangent from the data was performed. Subsequently, the horizontal axis position Xm at which the maximum value was taken between the two contact points was obtained. Finally, the crystal long period d was obtained by the following formula. qm = 10 Xm d = 2π / qm

[0250] <WAXS (reflection method) and MD, TD cross-section crystal orientation degree (%)> Wide-angle X-ray scattering (WAXS) by the reflection method of the polyolefin microporous membrane as the separator substrate was measured under the following conditions. (Measurement) Using the X-ray structure evaluation apparatus NANO-Viewer manufactured by Rigaku Corporation, wide-angle X-ray scattering measurement by the reflection method was performed. The sample was irradiated with CuKα rays, and the scattering was detected by an imaging plate. Wide-angle X-ray scattering measurement was performed under the conditions of a sample-detector distance of 95.2 mm, an output of 60 kV, and 45 mA. A point focus was adopted for the optical system, and the measurement was performed under the conditions of 1st slit: φ = 0.4 mm and 2nd slit: φ = 0.2 mm for the slit diameter. The sample was set so that the angle between the sample cross-section and the X-ray incident direction was 10.5°. Since the measurement cannot obtain accurate results when the thickness of the microporous membrane is thin, the measurement is performed after stacking to a film thickness that can obtain sufficient intensity as needed.

[0251] (Analysis: MD, TD cross-section crystal orientation degree (%)) Among the directions of the sample surface normal, the direction facing the upstream side is projected onto the detector surface, and the direction is defined as the azimuth angle φ = 0°. On the detector surface, it is defined clockwise from φ = -180° to φ = 180°. Subsequently, background correction of the detector and air cell scattering correction were performed on the X-ray scattering pattern obtained from the imaging plate. Then, the integrated intensity I(φ) in the range of 19.5° < 2θ < 21.3° where the (110) plane diffraction peak of polyethylene exists at each azimuth angle φ was plotted against the azimuth angle φ in the range of azimuth angle -45° < φ < 45°. When the molecular chains are oriented in the direction parallel to the film surface in the cross-section, I(φ) becomes a single peak centered at φ = 0°. This curve was fitted with the sum of a constant and a Gaussian function as shown in Equation 2, and the cross-sectional orientation degree f’ was calculated according to Equation 3 from the full width at half maximum of the Gaussian function in the fitting result. I(φ)=A + B×exp(-((φ - φ0) / w)2) Equation 2 Explanation of symbols in Equation 2 I(φ): Integrated intensity in the range of 19.5° < 2θ < 21.3° at a certain azimuth angle φ after background correction and air cell scattering correction φ: Azimuth angle (rad) f’ = 1 - FWHM / 180 Equation 3 Explanation of symbols in Equation 3 f: Cross-sectional orientation degree FWHM: Full width at half maximum of the Gaussian function obtained from the fitting result (°)

[0252] <WAXS (transmission method) measurement, crystallinity (%), crystallite size (110) (nm), crystallite size (200) (nm), and crystal orientation degree in the film thickness direction (%)> Wide-angle X-ray scattering (WAXS) by the transmission method of the polyolefin microporous membrane as a separator substrate was measured under the following conditions. (Measurement) Wide-angle X-ray scattering measurements were performed using the transmission method with a Rigaku X-ray structure evaluation device, NANO-Viewer. The sample was irradiated with CuKα radiation, and scattering was detected using an imaging plate. Wide-angle X-ray scattering measurements were performed under conditions of a sample-detector distance of 95.2 mm, output of 60 kV, and 45 mA. Point focus was used for the optical system, and measurements were performed under the following conditions for slit diameters: 1st slit: φ=0.4 mm, and 2nd slit: φ=0.2 mm. The sample was set so that the angle between the sample surface and the X-ray incidence direction was 10.5°. Since the measurement was not performed accurately if the microporous membrane was too thin, it was necessary to stack the membrane to a thickness that provided sufficient strength before performing the measurement.

[0253] (Analysis: Crystallite size (110) (nm) and Crystallite size (200) (nm) and Crystallinity %) The range of 2θ=9.7° to 2θ=29.0° of the X-ray scattering pattern obtained from the imaging plate was separated into three peaks: the orthorhombic (110) diffraction peak, the orthorhombic (200) diffraction peak, and the amorphous peak. The crystallite size was calculated from the full width at half maximum of the (110) diffraction peak according to Scherrer's formula (Formula 1). The (110) diffraction peak and the (200) diffraction peak were approximated by a Voigt function, and the amorphous peak was approximated by a Gaussian function. The peak position of the amorphous peak was fixed at 2θ=19.6° and the full width at half maximum was fixed at 6.3°, while the peak position and full width at half maximum of the crystalline peak were not fixed. The crystallite size was calculated from the full width at half maximum of the (110) diffraction peak calculated by peak separation according to Scherrer's formula (Formula 1). D(110 or 200) = Kλ / (βcosθ) Equation 1 Explanation of symbols in formula 1 D(110 or 200): Crystallite size (nm) K: 0.9 (constant) λ: wavelength of X-rays (nm) β:(β1 2 -β2 2 ) 0.5 β1: Full width at half maximum (rad) of the (hkl) peak calculated as a result of peak separation β2: Full width at half maximum of the incident beam divergence (rad) θ: Bragg angle

[0254] The crystallinity (X) was calculated according to the following formula. Crystallinity X={I(110)+I(200)} / {I(110)+I(200)+Iamr}×100 Iamr: Area of ​​amorphous peak

[0255] In addition, the crystallite size ratio (110) / (200) is calculated by the following formula using the crystallite size calculated by formula 1. Crystallite size ratio (110) / (200)=(crystallite size (110) [nm]) / (crystallite size (200) [nm])

[0256] <Amorphous thickness (nm) and crystalline thickness (nm)> Using the SAXS crystal long period and WAXS crystallinity measured by the above methods, the amorphous thickness (nm) and crystalline thickness (nm) were calculated according to the following formula. Amorphous thickness [nm] = (crystal long period [nm]) × (1-crystallinity [%] / 100)

[0257] <Substrate separator TOF-SIMS analysis and image processing> (I) TOF-SIMS analysis of separator The separators obtained in the examples and comparative examples were subjected to TOF-SIMS analysis. A nano-TOF manufactured by ULVAC-PHI, Inc. was used as the TOF-SIMS mass spectrometer. The analysis conditions were as follows. (Image measurement conditions) Primary ion: Bismuth (Bi) Acceleration voltage: 30 kV Ion current: Approx. 0.5nA (as DC) Analysis area: 100μm x 100μm Analysis time: 90 minutes Detected ion: positive ion (m / z=28) Neutralization: Electron gun + Ar monomer ion Vacuum degree: approx. 5.0×10 -5 Pa (Oxygen is introduced to increase the detection intensity of Si) (Measurement conditions in the depth direction) 《Analysis conditions》 Primary ion: Bismuth (Bi) Acceleration voltage: 30 kV Ion current: Approx. 1.2nA (as DC) Analysis area: 100μm x 100μm Analysis time: 5 frames / cycle Detected ion: positive ion (m / z=28) Neutralization: Electron gun + Ar monomer ion Vacuum degree: approx. 5.0×10 -5 Pa (Oxygen is introduced to increase the detection intensity of Si) <Sputtering conditions> Sputter ion: GCIB (Ar 2500 + ) Acceleration voltage: 20 kV Ion current: approx. 5nA Sputtering area: 400μm×400μm Sputtering time: 30 seconds / cycle Neutralization: Electron gun + Ar monomer ion

[0258] Under the above conditions, spectrum detection of Si ions (corresponding to positive ions with m / z=28) was performed. As an example, the TOF-SIMS analysis result of the separator of Example 1 is shown in Fig. 1, and the TOF-SIMS analysis result of the separator of Comparative Example 1 is shown in Fig. 11. The vertical and horizontal axes in Fig. 1 are in pixels, and the vertical and horizontal axes in Fig. 11 are in pixels.

[0259] (II) Image Processing The TOF-SIMS spectrum image data obtained as described above was subjected to image processing according to the following procedure. (1) Create a filter that matches the beam shape (diameter 2 μm, pixel resolution 0.39 μm). A 3D image of the filter is shown in Figure 2, and a 2D image is shown in Figure 3. The filter value h1 is shown in Table 1 below. Note that the units of the vertical and horizontal axes in Figure 2 are pixels, and the units of each axis in Figure 3 are pixels.

[0260] [Table 1]

[0261] (How filter values ​​are calculated) The calculation was performed using the fspecial function in the Image Processing Toolbox of the numerical calculation software MATLAB (registered trademark) manufactured by Mathworks. fspecia(``gaussian'',

[1313] ,1.69865)

[0262] (2) Apply the created filter to the two-dimensional data. (3) Calculate the mean and standard deviation of the two-dimensional data after applying the filter. (4) The data is binarized using the mean value + standard deviation x 3 as the threshold value. (However, in the case of a normal distribution, 99.74% of the values ​​fall within the range of the mean + standard deviation × 3, so the intention was to extract numerically unusual parts.)

[0263] (5) Dilation and contraction of 7 pixels are performed to connect adjacent extracted regions. (6) Remove small areas (less than 50 pixels). (7) Calculate the parameters for each remaining region Extraction area (pixels), simple center of gravity position (x0, y0) Maximum value in the region, average value in the region, weighted center of gravity position (xm, ym)

[0264] (8) Calculate the distance between each weighted center of gravity position The calculation was performed using the WeightedCentroid option of the regionprops function in the Image Processing Toolbox of the numerical calculation software MATLAB manufactured by Mathworks. regionprops(cc,I,'WeightedCentroid') Here, cc is a variable indicating the extracted region, and I is a variable storing the two-dimensional data after the filter is applied.

[0265] As an example, the TOF-SIMS analysis results of a separator after image processing in the above steps (1) and (2) are shown in Fig. 4 (Example 1) and Fig. 12 (Comparative Example 1), and the results after image processing in the above steps (1) to (6) are shown in Fig. 5 (Example 1) and Fig. 13 (Comparative Example 1). Note that the units of the vertical and horizontal axes in Fig. 4 are pixels, the units of the vertical and horizontal axes in Fig. 12 are pixels, the units of the vertical and horizontal axes in Fig. 5 are pixels, and the units of the vertical and horizontal axes in Fig. 13 are pixels.

[0266] (III) Voronoi tessellation The Voronoi division was performed based on the weighted center of gravity position (xm, ym) calculated earlier, the Voronoi region was obtained, and its area was calculated. The calculation was performed using Mathworks' numerical calculation software MATLAB.

[0267] The Voronoi region diagram shown in Fig. 6 (Example 1) or Fig. 14 (Comparative Example 1) can be obtained by the following calculation procedure. Note that the units of the vertical and horizontal axes in Fig. 6 are pixels, and the units of the vertical and horizontal axes in Fig. 14 are pixels. VXB and VYB are temporary variables used in the calculation. [VXB,VYB] = voronoi(xm,ym); plot(VXB,VYB,'-b',xm,ym,'.r'); The calculation of the region and its area by Voronoi division was performed according to the following procedure. First, the following calculation procedure is performed. DTB=delaunayTriangulation([xm,ym]); [VB,rB] = voronoiDaigram(DTB); DTB is a temporary variable used during the calculation, and delaunayTriangulation(xm,ym) is a function that creates the Delaunay triangulation that is the element of that temporary variable. VB is a matrix variable that stores a list of positions indicating the positions of the endpoints of the triangles that make up the Voronoi tessellation, and rB is a list of columns that indicate which endpoints in VB are used for each Voronoi region that is divided by the Voronoi tessellation. Next, the following calculation is performed on each Voronoi region indicated by each column of rB in the order of the columns. The calculation is performed on the columns of the list indicated in rB in order from 1 to the end. The calculation for the kth column of the list is performed as follows.

[0268] (1) If the endpoints of VB indicated by the k-th list rB{k} of rB include points that correspond to the outside of the image region, then that region is excluded from the calculation as an unclosed region. This is because the region adjacent to the edge of the image includes a boundary that is the edge of the image, which is not a Voronoi tessellation that indicates an island structure, and therefore this region is considered to have no area that indicates the original characteristics of an island structure. Here, the list indicated by k that does not have any points to be excluded is determined to represent a valid Voronoi region.

[0269] (2) For the Voronoi region k that was determined to be valid by the previous judgment, its area A is calculated as follows: rBK = rB{k}; XPB = VB(rBK,1); YPB = VB(rBK,2); A(i) = polyarea(XPB,YPB); i is a number sequentially assigned to areas that are determined to be valid, starting from 1 and incrementing by 1 each time an entry is made in the above calculation. rBK, XPB, and YPB are temporary variables used in the calculation.

[0270] For these calculations (1) and (2), k is increased in order from 1. When the calculations are completed until the end of the list of rB, only the area of ​​the area that is determined to be valid as a Voronoi region is assigned to A.

[0271] As a result of this calculation, the Voronoi areas that are determined to be valid and have their areas calculated are shown in, for example, Fig. 7 (Example 1) and Fig. 15 (Comparative Example 1). Note that the units of the vertical and horizontal axes in Fig. 7 are pixels, and the units of the vertical and horizontal axes in Fig. 15 are pixels.

[0272] As an example of the calculation results of the area, the histograms of the separator are shown in FIG. 8 (Example 1) and FIG. 16 (Comparative Example 1).

[0273] The Voronoi area is calculated based on an image, so it is expressed in pixels, but it can be converted to an actual area based on the imaging conditions when the image was obtained. If the length of one side of a pixel obtained from the conditions set during imaging is lp (μm), then the area equivalent to one pixel is lp 2 (μm 2 ) The actual area can be obtained by multiplying the area of ​​the Voronoi region expressed in pixels by the area of ​​one pixel. For example, if an area of ​​100 μm square is imaged using 256 × 256 pixels, the length of one side of a pixel is 0.39 μm, and the area of ​​one pixel is 0.153 μm. 2 For example, a Voronoi region calculated to have an area of ​​100 pixels actually has an area of ​​153 μm 2 In this way, the area obtained from the image in pixel units can be easily converted to an actual area. Examples of histograms after conversion are shown in FIG. 9 (Example 1) and FIG. 17 (Comparative Example 1). Also, if the length of one side of a pixel is lp (μm), the area equivalent to one pixel is lp 2 (μm 2 ) the actual area of ​​the Voronoi region may be converted to obtain the converted histogram in the same manner as above.

[0274] Next, we will explain how to calculate the parameters that represent the characteristics of the distribution of the areas of Voronoi regions from this histogram. This calculation was performed by fitting the area distribution to the following probability distribution function.

number

[0275] Here, x is the input data. There are three fitting parameters: a shape parameter k, a position parameter μ indicating the maximum value, and a scale parameter σ indicating the dispersion. The calculation was performed using the GeneralizedExtremeValueDistribution option of the fitdist function in the Statistics and Machine Learning Toolbox of the numerical calculation software MATLAB manufactured by Mathworks, Inc. The calculation is performed as follows, using the area A calculated above as x. pd=fitdist(A,'GeneralizedExtremeValueDistribution'); The output pd holds the previously mentioned values ​​of k, μ, and σ as a structure containing the fitting results, and the individual data can be accessed as pd.k, pd.mu, and pd.sigma, respectively. Examples illustrating the fitting results are shown in FIG. 10 (Example 1) and FIG. 18 (Comparative Example 1). In this example, of the distribution parameters obtained by this fitting, the peak position and σ indicating the variation were used. σ / mu can also be calculated using the obtained mu and σ.

[0276] <Compression resistance test> Two separators were cut to 10cm x 10cm, stacked, and the air permeability Sj was measured. Furthermore, the thickness was measured at 9 arbitrary points within an area of ​​8cm x 8cm based on the intersection of the diagonal lines in a top view, and the average value was calculated. Then, the laminate was covered with two PET films (10cm x 10cm) from above and below to form a laminate. Furthermore, the laminate was sandwiched between two rubber sheets (10cm x 10cm) with a thickness of 5mm from above and below, and pressure was applied while heating using a mini test press (product number: MP-WCH) manufactured by TOYOSEIKI. The PET film and the rubber sheet were used so that pressure was applied uniformly over the entire surface, and the uniformity was confirmed with a pressure sensor. The temperature of the upper and lower heaters of the press was 90°C, and the samples were held for 3 minutes so that 8Mpa was uniformly applied to the 10cm x 10cm sample. After the heating and compression operation, the air permeability Sh of the two stacked separators was measured. Furthermore, the thickness of two stacked separators was measured at 9 arbitrary points within an area of ​​8 cm x 8 cm, based on the intersection of the diagonal lines when viewed from above, and the average value was calculated. According to the following formula, the change in thickness before and after compression was quantified as the thickness reduction rate (%), and the change in air permeability after compression and before compression was quantified as the air permeability change ratio. Thickness reduction rate (%) = ((thickness after compression (μm) - thickness before compression (μm)) / thickness before compression (μm)) × 100 Air permeability change ratio (%) = ((Air permeability after compression Sh (sec) - Air permeability before compression Sj (sec)) / Air permeability before compression Sj (sec)) x 100

[0277] <Contact angle of coating liquid (°)> Using a contact angle meter (CA-V) (model name) manufactured by Kyowa Interface Science Co., Ltd., 2 μl of each coating liquid was dropped onto the clean surface of the separator substrate, and the contact angle was measured after 40 seconds. The contact angle was measured three times in each direction, MD and TD, and the average value was used. This measurement method was also performed on both the front and back sides of the microporous membrane used as the separator substrate, and the larger value of either one was used.

[0278] <Checking the progress of crosslinking reaction during coating process> The TMA rupture temperature was measured before and after the coating solution was applied to a polyolefin microporous membrane as a separator substrate, and the progress of the crosslinking reaction during the coating process was confirmed by comparing the two temperatures. The progress of the crosslinking reaction was evaluated according to the following criteria for the TMA rupture temperature. (Coating of inorganic porous layer or thermoplastic polymer-containing layer) 〇(Good): 190℃ or higher △(Tolerance): 170℃~190℃ × (defective): 170℃ or less (Coating of active layer or heat-resistant resin layer) 〇(Good): 200℃ or more △(Tolerance): 180℃~200℃ × (defective): 180℃ or less

[0279] <Battery Evaluation I: Cycle Test, Hot Box Test, and Nail Penetration Test> Laminated cells or 4680-type cylindrical batteries were fabricated according to the following procedure. Cycle test (1), hot box test, and nail penetration test were performed using the laminated cells, and cycle test (2) was performed using the 4680-type cylindrical batteries. (Preparation of batteries for use in safety tests) a. Preparation of the positive electrode LiNi as the positive electrode active material 0.8 Mn 0.1 Co 0.1 O2, carbon black as a conductive assistant, and polyvinylidene fluoride solution as a binder were mixed in a solid content mass ratio of 91:5:4, and N-methyl-2-pyrrolidone was added as a dispersion solvent so that the solid content was 68 mass%, and further mixed to prepare a slurry solution. This slurry solution was applied to both sides of an aluminum foil with a thickness of 15 μm so that part of the aluminum foil was exposed, and then the solvent was dried and removed. Furthermore, the density of the positive electrode mixture part was 2.8 g / cm 3 The aluminum foil was then cut so as to include the exposed portion of the aluminum foil to obtain a positive electrode.

[0280] b. Preparation of the negative electrode Artificial graphite as the negative electrode active material, styrene butadiene rubber as the binder, and an aqueous carboxymethyl cellulose solution were mixed in a solid content mass ratio of 96.4:1.9:1.7, and water was added as a dispersion solvent so that the solid content was 50 mass%, and further mixed to prepare a slurry solution. This slurry solution was applied so that a part of the copper foil with a thickness of 10 μm was exposed, and then the solvent was dried and removed. Furthermore, the density of the negative electrode mixture part was 1.45 g / cm 3 The laminate was then cut so as to include the exposed copper foil portion, thereby obtaining a negative electrode.

[0281] c. Preparation of non-aqueous electrolyte As shown in Tables 18 and 19, the electrolytic solution and electrolyte were mixed to prepare a non-aqueous electrolytic solution.

[0282] d-1. Battery assembly of laminated cells A long separator with a width of 55 mm was folded zigzag so that the active material surfaces of the positive and negative electrodes faced each other and were interposed between the positive and negative electrodes, to form a laminate consisting of 15 double-sided negative electrodes and 14 double-sided positive electrodes. At this time, the heat-resistant B layer of sample 1 was arranged to face the positive electrode. Aluminum lead pieces with sealant were welded to the exposed parts of the 14 positive aluminum foils of this laminate, and nickel lead pieces with sealant were welded to the exposed parts of the 15 negative copper foils, and then the laminate was inserted into an aluminum laminate exterior body, and the sides where the positive and negative lead pieces were exposed and the other two sides, a total of three sides, were laminated and sealed. Next, the nonaqueous electrolyte was injected into the exterior body, and then the opening was sealed to prepare a laminated type battery with 28 opposing electrodes. The resulting battery was left at room temperature for one day, and then charged at a constant current of 330 mA (0.3 C) in an atmosphere of 25°C up to a battery voltage of 4.2 V, and then charged at a constant voltage to maintain 4.2 V. This method was used for the first charging after the battery was fabricated, for a total of 8 hours. The battery was then discharged at a current value of 330 mA (0.3 C) down to a battery voltage of 3.0 V.

[0283] d-2. Cylindrical battery assembly Using the above positive electrode, negative electrode, and electrolyte, and using a long separator so that the active material surfaces of the positive electrode and negative electrode face each other and are interposed between the positive electrode and negative electrode, a cylindrical (4680 type) lithium secondary battery (battery dimensions: diameter 46 mm, height 80 mm) was prepared. When preparing the battery, the positive electrode and negative electrode were sealed with electrodes of the maximum length that could be placed inside the battery container. At this time, the coating layer of the separator was arranged to face the positive electrode. After leaving the obtained battery at room temperature for one day, it was charged at a constant current of 5A (0.3C) in an atmosphere of 25°C to a battery voltage of 4.2V, and then constant voltage charging was performed to maintain 4.2V after reaching that voltage, for a total of 8 hours, in this manner, the first charging after the battery preparation was performed. Next, the battery was discharged at a current value of 5A (0.3C) to a battery voltage of 3.0V.

[0284] (Cycle test (1): at 5°C and 50°C) The battery obtained in "d-1. Battery assembly of laminated cell" above was charged and discharged 1000 cycles in an atmosphere of 5°C and 50°C. The battery was charged for a total of 3 hours by charging at a constant current of 1A (1.0C) up to a battery voltage of 4.2V, and then constant voltage charging to maintain 4.2V after reaching that voltage. The battery was discharged at a current value of 1A (1.0C) down to a battery voltage of 3.0V. The capacity retention rate was calculated from the discharge capacity at the 1000th cycle and the discharge capacity at the 1st cycle. A high capacity retention rate was evaluated as having good cycle characteristics.

[0285] (Hot Box Test) The battery obtained by the above "d-1. Battery assembly of laminated cell" was subjected to 300 cycles of charge and discharge at 5°C, and then stored in a hot box set at a high temperature of 136°C for 1 hour, and the state of the battery was observed during and after storage.

[0286] When the microporous membrane contained in the battery as a separator undergoes thermal shrinkage during high-temperature storage, an internal short circuit may occur in the positive and negative electrodes of the battery, resulting in ignition or explosion. Batteries in which ignition or explosion was observed were evaluated as unacceptable. Batteries in which ignition or explosion was not observed were evaluated as acceptable.

[0287] This hot box test was carried out on 100 batteries using the same separator, and the pass rate (%) was calculated.

[0288] (Nail penetration test) A test was conducted to cause an internal short circuit by driving a 3mm diameter iron nail into the battery obtained by "d-1. Battery assembly of laminated cells" at a speed of 20mm / sec, penetrating the battery after charging it to 4.2V. This test can clarify the phenomenon at the time of an internal short circuit by measuring the time change behavior of the voltage drop of the battery due to an internal short circuit and the behavior of the rise in the battery surface temperature due to an internal short circuit. In addition, the battery may suddenly heat up due to an insufficient shutdown function of the separator or rupture at low temperatures during an internal short circuit, which may cause the electrolyte to ignite and the battery to smoke and / or explode.

[0289] The nail penetration test was performed on 100 batteries with the same separator, and the number of batteries that did not catch fire, emit smoke, or explode, X, was calculated as the pass rate (X / 100), which is shown in Tables 2 to 17.

[0290] (Cycle test (2)) The battery obtained in "d-2. Assembly of cylindrical battery" above was charged and discharged 500 cycles in an atmosphere of 40°C. The battery was charged for a total of 3 hours by charging at a constant current of 17.5A (1.0C) up to a battery voltage of 4.2V, and then constant voltage charging to maintain 4.2V after reaching that voltage. The battery was discharged at a current value of 17.5A (1.0C) down to a battery voltage of 3.0V. The capacity retention rate was calculated from the discharge capacity at the 1000th cycle and the discharge capacity at the 1st cycle. A high capacity retention rate was evaluated as having good cycle characteristics.

[0291] <Battery Evaluation II> (Battery construction) The battery evaluation was performed by preparing a non-aqueous secondary battery including the sample piece according to the following procedure: Crush test and cycle test Capacity retention rate and cycle life test were performed by preparing a 4680 type cylindrical battery and measuring 4 days after coating the separator.

[0292] a. Preparation of the positive electrode LiNi as the positive electrode active material 0.6 Mn 0.2 Co 0.2 O2, carbon black as a conductive assistant, and polyvinylidene fluoride solution as a binder were mixed in a solid content mass ratio of 91:5:4, and N-methyl-2-pyrrolidone was added as a dispersion solvent so that the solid content was 68 mass%, and further mixed to prepare a slurry solution. This slurry solution was applied to both sides of an aluminum foil with a thickness of 15 μm so that part of the aluminum foil was exposed, and then the solvent was dried and removed. Furthermore, the density of the positive electrode mixture part was 2.8 g / cm 3 The aluminum foil was then cut so as to include the exposed portion of the aluminum foil to obtain a positive electrode.

[0293] b. Preparation of the negative electrode Carbon-coated silicon powder, lithium-doped carbon-coated silicon oxide powder, and graphite powder as negative electrode active materials, and styrene butadiene rubber and carboxymethyl cellulose aqueous solution as binders were mixed in a solid content mass ratio of 3:27:66.4:1.9:1.7, and water was added as a dispersion solvent so that the solid content was 50 mass%, and further mixed to prepare a slurry solution. This slurry solution was applied to both sides of a 10 μm thick copper foil so that part of the copper foil was exposed, and then the solvent was dried and removed. Furthermore, the density of the negative electrode mixture part was 1.45 g / cm 3 The laminate was then cut so as to include the exposed copper foil portion, thereby obtaining a negative electrode.

[0294] c: Preparation of electrolyte A non-aqueous electrolyte solution was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 1.0 mol / L.

[0295] d. Battery assembly Using the above positive electrode, negative electrode, and electrolyte, and using a long separator so that the active material surfaces of the positive electrode and negative electrode face each other and are interposed between the positive electrode and negative electrode, a cylindrical (4680 type) lithium secondary battery (battery dimensions: diameter 46 mm, height 80 mm) was prepared. When preparing the battery, the positive electrode and negative electrode were sealed with electrodes of the maximum length that could be placed inside the battery container. At this time, the coating layer of the separator was arranged to face the positive electrode. After leaving the obtained battery at room temperature for one day, it was charged at a constant current of 1A (0.06C) in an atmosphere of 25°C to a battery voltage of 4.2V, and then constant voltage charging was performed to maintain 4.2V after reaching that voltage, for a total of 8 hours, in this manner, the first charging after the battery preparation was performed. Next, the battery was discharged at a current value of 1A (0.06C) to a battery voltage of 3.0V.

[0296] (Bar impact test (crushing test)) Using the battery obtained in "d. Battery Assembly" of Battery Evaluation II above, a SUS rod with a diameter of 15.8 mm was placed vertically along the length of the battery, and then a weight weighing 9.1 kg was allowed to fall freely from a height of 61 cm, causing it to collide with the battery, and the temperature rise and ignition status of the battery were checked for a specified number of cells. After the collision, cells that generated heat of 80°C or more were evaluated as failing the test, and the pass rate (%) was calculated based on the total number of cells.

[0297] (Cycle test capacity retention rate (%)) The battery obtained in "d. Battery assembly" of Battery Evaluation II above was charged and discharged 500 cycles in an atmosphere of 55°C. The battery was charged for a total of 3 hours by charging at a constant current of 8.7A (0.5C) up to a battery voltage of 4.2V, and then constant voltage charging to maintain 4.2V after reaching that voltage. The battery was discharged at a current value of 8.7A (0.5C) down to a battery voltage of 3.0V. The capacity retention rate was calculated from the discharge capacity at the 1000th cycle and the discharge capacity at the 1st cycle. A high capacity retention rate was evaluated as having good cycle characteristics.

[0298] (Cycle life test) The battery obtained in "d. Battery assembly" of Battery Evaluation II above was repeatedly charged and discharged in an atmosphere of 65°C until the capacity retention rate reached 50% or less. The battery was charged for a total of 3 hours by charging at a constant current of 8.7A (0.5C) up to a battery voltage of 4.2V, and then constant voltage charging to maintain 4.2V after reaching that voltage. The battery was discharged at a current value of 8.7A (0.5C) down to a battery voltage of 3.0V. The number of cycles at which the capacity retention rate reached 50% or less was recorded as the cycle life. A battery with a long cycle life was evaluated as having good cycle characteristics.

[0299] [Manufacturing method of silane-modified polyolefin] The raw polyolefin used for the silane-modified polyolefin may have a viscosity average molecular weight (Mv) of 10,000 to 1,000,000, a weight average molecular weight (Mw) of 30,000 to 920,000, and a number average molecular weight of 10,000 to 150,000, and may be a propylene or butene copolymerized α-olefin. While melt-kneading the raw polyethylene in an extruder, an organic peroxide (di-t-butyl peroxide) is added to generate radicals in the α-olefin polymer chain, and then trimethoxyalkoxide-substituted vinylsilane is injected to introduce alkoxysilyl groups into the α-olefin polymer by an addition reaction, forming a silane graft structure. At the same time, an appropriate amount of an antioxidant (pentaerythritol tetrakis [3-(3,5-di-t-butyl-4-hydroxyphenyl) propionate]) is added to adjust the radical concentration in the system, suppressing the chain reaction (gelation) in the α-olefin. The obtained silane-grafted polyolefin molten resin is cooled in water, pelletized, and then heated and dried at 80°C for 2 days to remove moisture or unreacted trimethoxyalkoxide-substituted vinylsilane. The residual concentration of unreacted trimethoxyalkoxide-substituted vinylsilane in the pellet is 3000 ppm or less. By using octenyltrialkoxysilane instead of trimethoxyalkoxide-substituted vinylsilane, a silane-modified polyolefin having 8 methylene (CH2) units constituting the linkage to the main chain can be produced, and by using dodecyltrialkoxysilane instead of trimethoxyalkoxide-substituted vinylsilane, a silane-modified polyolefin having 12 methylene (CH2) units constituting the linkage to the main chain can be produced.

[0300] [Production methods of polyolefins other than silane-modified polyolefins] Polyolefins used in the production method of polyolefins other than silane-modified polyolefins can be produced by the following method, although it is not preferred to be limited thereto. Hexane, ethylene, α-olefins such as 1-pentene or 1-butene, hydrogen, catalyst components such as Ziegler-Natta catalysts and metallocene catalysts, cocatalyst components such as triisobutylaluminum and diisobutylaluminum hydride, and antistatic agents are continuously fed into a vessel-type polymerization reactor equipped with a stirrer to obtain a polyethylene polymerization slurry. At this time, the polymerization temperature is kept constant by jacket cooling, and the polymerization slurry is continuously drawn into a flash drum with a constant temperature so that the level of the polymerization reactor is kept constant, and unreacted ethylene and hydrogen are separated. The solvent is then separated using a centrifuge, and the mixture is dried by nitrogen blowing to obtain polyethylene powder. To the obtained polyethylene powder, an aliphatic saturated alcohol such as methanol and calcium stearate are added, and the mixture is mixed uniformly in a Henschel mixer. Furthermore, a sieve with appropriate openings is used to remove the material that did not pass through the sieve, thereby obtaining polyolefins other than silane-modified polyolefins.

[0301] [Preparation of resin raw materials] (Preparation of resin raw material A1) 100 parts by mass of polyolefin having a viscosity average molecular weight of 150,000 was compounded with 1.4 parts by mass of vinyltrimethoxysilane, 0.025 parts by mass of di-t-butyl peroxide as an organic peroxide, and 0.15 parts by mass of calcium stearate, and mixed in a Henschel mixer. The mixture was then melt-kneaded at 220°C using a Japan Steel Works TEX-44 twin-screw extruder (screw diameter 44 mm, L / D=35) to granulate resin raw material A1.

[0302] (Preparation of resin raw material B1) Hexane 55L / h, Mg6(C4H9) as catalyst component 12A Ziegler-Natta catalyst containing Al(C2H5)3 and titanium tetrachloride (0.5 g / h) and a mixture of triisobutylaluminum and diisobutylaluminum hydride (9:1 mixture) (9 mmol / h) as cocatalyst components were fed into a vessel-type 300 L polymerization reactor kept at 53°C by jacket cooling, while ethylene was continuously fed so that the polymerization pressure was 0.3 MPa, and a polyethylene polymerization slurry was obtained. At this time, STATSAFE3000 was added as an antistatic agent so that the concentration relative to the polyethylene powder was 15 ppm. In addition, 1-butene was continuously added as an α-olefin so that the gas-phase ethylene concentration was 6.9 mol%. The polyethylene polymerization slurry was continuously drawn into a flash drum at a pressure of 0.05 MPa so that the level of the polymerization reactor was kept constant, and unreacted ethylene was separated. The solvent was then separated by centrifugation, and the mixture was dried under a nitrogen stream using a drum dryer with a jacket adjusted to 80°C and an oxygen concentration of 80 ppm, to obtain polyethylene powder. Methanol was added to the obtained polyethylene powder at a concentration of 150 ppb and calcium stearate (wet process) at a concentration of 1,000 ppm, and the mixture was passed through a sieve with 425 μm openings to remove any material that did not pass through the sieve, thereby obtaining a resin raw material B1.

[0303] (Preparation of resin raw material C2) Hexane 40L / h prepared at 3℃, Mg6(C4H9) as catalyst component 12A Ziegler-Natta catalyst containing Al(C2H5)3 and titanium tetrachloride (0.2 g / h) and a mixture of triisobutylaluminum and diisobutylaluminum hydride (9:1 mixture) (10 mmol / h) as cocatalyst components were fed into a vessel-type 300 L polymerization reactor kept at 80°C by jacket cooling, while ethylene was continuously fed so that the polymerization pressure was 0.5 MPa, and a polyethylene polymerization slurry was obtained. At this time, STATSAFE3000 was added as an antistatic agent so that the concentration relative to the polyethylene powder was 15 ppm. In addition, 1-butene was continuously added as an α-olefin so that the hydrogen concentration relative to the gas phase ethylene concentration was 5 mol%. Hydrogen was further fed so that the hydrogen concentration relative to the gas phase ethylene was 5.5 mol%. The polyethylene polymerization slurry was continuously drawn into a flash drum at a pressure of 0.05 MPa so that the level of the polymerization reactor was kept constant, and unreacted ethylene was separated. The solvent was then separated by centrifugation, and the mixture was dried under a nitrogen stream using a drum dryer with a jacket adjusted to 80°C and an oxygen concentration of 80 ppm to obtain polyethylene powder. Methanol was added to the obtained polyethylene powder at a concentration of 150 ppb and calcium stearate (wet method) at a concentration of 1,000 ppm, and the mixture was passed through a sieve with 425 μm openings to remove any material that did not pass through the sieve, obtaining resin raw material C2.

[0304] (Production of other resin raw materials) Resin materials A2 to A12 and resin materials D1 to D14 shown in Tables 20 to 25 were prepared in the same manner as the preparation of resin material A1, except that the molecular weight and copolymer concentration of the raw material polyolefin, the amount of trimethoxyalkoxide-substituted vinylsilane added, and the kneading conditions were changed. However, when preparing resin material D13, octenyl octenyl trialkoxysilane was used instead of trimethoxyalkoxide-substituted vinylsilane, and when preparing D14, dodecyl trialkoxysilane was used instead of trimethoxyalkoxide-substituted vinylsilane. Resin materials B2 to B6 and E1 to E5 shown in Tables 20 to 25 were prepared in the same manner as the preparation of resin material B1, except that the amount of raw material input, polymerization reactor temperature, and polymerization pressure were changed. Resin materials C1, C3 to C5, and F1 to F4 shown in Tables 20 to 25 were prepared in the same manner as the preparation of resin material C2, except that the amount of raw material input, polymerization reactor temperature, and polymerization pressure were changed.

[0305] [Example 1] Preparation and evaluation of separator (Preparation of polyolefin microporous membrane as a separator) To a mixed resin composition of 30 mass% of resin A1, 30 mass% of resin B1, and 40 mass% of resin C2, 1000 mass ppm of pentaerythrityl-tetrakis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] was added as an antioxidant, and the mixture was dry-blended using a tumbler blender to obtain a mixture. The resulting mixture was fed to a twin-screw extruder by a feeder under a nitrogen atmosphere. Liquid paraffin (dynamic viscosity at 37.78°C: 7.59×10 -5 m 2 / s) was pumped into the extruder cylinder by a plunger pump.

[0306] The mixture and liquid paraffin were melt-kneaded in the extruder, and the feeder and pump were adjusted so that the liquid paraffin content in the extruded polyolefin composition was 75% by mass (i.e., the polymer concentration was 25% by mass). The melt-kneading conditions were a set temperature of 230°C, a screw rotation speed of 100 rpm, and a discharge rate of 80 kg / h. Next, the molten mixture was extruded through a T-die onto a cooling roll whose surface temperature was controlled to 25° C., to obtain a gel sheet (sheet-shaped molded product) having a film thickness of 1250 μm.

[0307] Next, the sheet-shaped molded body was introduced into a simultaneous biaxial tenter stretching machine, and biaxial stretching was performed to obtain a stretched product. The set stretching conditions were MD magnification 7.0 times, TD magnification 6.4 times (i.e., 7 x 6.4 times), and biaxial stretching temperature 125 ° C. Next, the gel sheet after stretching was introduced into a dichloromethane tank and thoroughly immersed in dichloromethane to extract and remove liquid paraffin, and then the dichloromethane was dried and removed to obtain a porous body. Next, the porous body was introduced into a TD tenter to perform heat setting (HS), and HS was performed at a heat setting temperature of 133 ° C. and a stretching ratio of 1.8 times based on the sheet width at the TD tenter entrance, and then a relaxation operation was performed to TD 1.6 times based on the sheet width at the TD tenter entrance to obtain a microporous membrane. Then, the end of the obtained microporous membrane was cut and wound up as a mother roll with a width of 1,100 mm and a length of 5,000 m.

[0308] <Coating of inorganic coating layer> (Acrylic latex manufacturing method) The acrylic latex used as the resin binder is manufactured by the following method. 70.4 parts by mass of ion-exchanged water, 0.5 parts by mass of "Aqualon KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 0.5 parts by mass of "ADEKA REASOAP SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Corporation) as emulsifiers were added to a reaction vessel equipped with a stirrer, a reflux condenser, a dripping tank, and a thermometer. Next, the temperature inside the reaction vessel was raised to 80°C, and while maintaining the temperature at 80°C, 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate was added to obtain an initial mixture. The addition of the aqueous solution of ammonium persulfate was completed. Five minutes later, the emulsion was dripped from the dripping tank into the reaction vessel over 150 minutes. The above emulsion was prepared by mixing 70 parts by mass of butyl acrylate, 29 parts by mass of methyl methacrylate, 1 part by mass of methacrylic acid, 3 parts by mass of "Aqualon KH1025" (registered trademark, 25% aqueous solution manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) and 3 parts by mass of "Adeka Reasoap SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Corporation) as emulsifiers, 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate, and 52 parts by mass of ion-exchanged water using a homomixer for 5 minutes. After the emulsion was added, the temperature inside the reaction vessel was kept at 80°C for 90 minutes, and then cooled to room temperature. The resulting emulsion was adjusted to pH 8.0 with 25% aqueous ammonium hydroxide solution, and a small amount of water was added to obtain an acrylic latex with a solid content of 40%. The resulting acrylic latex had a number average particle size of 145 nm and a glass transition temperature of -23°C.

[0309] (Formation of inorganic porous layer) A dispersion was prepared by uniformly dispersing 95 parts by weight of aluminum hydroxide oxide (average particle size 1.4 μm) as inorganic particles and 0.4 parts by weight (solid content equivalent) of an aqueous solution of ammonium polycarboxylate (SN Dispersant 5468 manufactured by San Nopco, solid content concentration 40%) as an ionic dispersant in 100 parts by weight of water. The obtained dispersion was crushed with a bead mill (cell volume 200 cc, zirconia bead diameter 0.1 mm, filling amount 80%) to adjust the particle size distribution of the inorganic particles to D50 = 1.0 μm. A slurry containing inorganic particles was prepared by adding 4.6 parts by weight (solid content equivalent) of acrylic latex (solid content concentration 40%, average particle size 145 nm, glass transition temperature -23 ° C., constituent monomers: butyl acrylate, methyl methacrylate, methacrylic acid) as a resin binder to the dispersion with the adjusted particle size distribution. Next, the microporous membrane was continuously unwound from the microporous membrane mother roll, and one side of the microporous membrane was coated with an inorganic particle-containing slurry using a gravure reverse coater, followed by drying in a dryer at 60°C to remove water and winding up to obtain a separator mother roll. At the time of evaluation, the separator unwound from the mother roll was slit as necessary and used as an evaluation separator.

[0310] The thickness, air permeability, porosity, puncture strength, and air permeability change ratio before and after a compression test in which the resulting polyolefin microporous membrane was compressed by 30% of the thickness were measured, and the results are shown in Table 2. The separator for evaluation and the battery including the separator were subjected to various evaluations according to the above-mentioned evaluation methods, and the evaluation results are shown in Table 2.

[0311] [Examples 2 to 33, Comparative Examples 4 and 7] Preparation and evaluation of separators As shown in Tables 2 to 8, the molecular weight mixture composition, preparation conditions, composite composition conditions, etc. of the polyolefin microporous membrane were changed, and the same operations as in Example 1 were performed to obtain separators shown in Tables 2 to 8. The obtained separators and batteries including the same were subjected to various evaluations according to the above-mentioned evaluation methods, and the evaluation results are also shown in Tables 2 to 8.

[0312] The silane-modified PP described in Examples 28 and 30 was produced using polypropylene (E-100GV) manufactured by Prime Polymer Co., Ltd. in the same manner as described in the above [Method of producing silane-modified polyolefin] section. The PP used was polypropylene (E-100GV) manufactured by Prime Polymer Co., Ltd. The PP-PE used in Example 28 was a block polymer of olefin crystals, ethylene-butylene-olefin crystals (DYNARON6201B) manufactured by JSR Corporation.

[0313] [Comparative Example 1] Preparation and evaluation of separator The separator shown in Table 7 was obtained by the same operation as in Example 1, except that Resin B1 and Resin C2 were used in a ratio of 50:50 (mass ratio) and the preparation conditions of the polyolefin microporous membrane and the composite construction conditions were changed as shown in Table 7. The obtained separator and the battery including the same were subjected to various evaluations according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 7.

[0314] [Comparative Example 2] Preparation and evaluation of separator In the extruder, 24 kg / h of silane-unmodified polyethylene (VH035 manufactured by Daehan Oil & Chemical Industry Co., Ltd.) with a weight average molecular weight of 350,000 and a melting point of 136.2°C, 24 kg / h of resin raw material A1, and 24 kg / h of liquid paraffin (dynamic viscosity at 37.78°C of 7.59 × 10 -5 m 2The mixture was mixed at a flow rate of 112 kg / h (flow rate: 112 kg / h / s). The weight ratio of silane-unmodified polyethylene:silane-modified polyethylene:liquid paraffin was 15:15:70. Furthermore, 0.5 parts by mass of vinyltriethoxysilane as a carbon-carbon double bond group-containing alkoxysilane compound based on a total of 100 parts by mass of silane-unmodified polyethylene, silane-modified polyethylene, and liquid paraffin, 2 parts by mass of dibutyltin dilaurate as a crosslinking catalyst based on 100 parts by mass of the carbon-carbon double bond group-containing alkoxysilane compound, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP) as an initiator based on 100 parts by mass of the carbon-carbon double bond group-containing alkoxysilane compound were introduced into the extruder and mixed. Then, extrusion was performed at a temperature of 200°C to obtain a silane-modified polyethylene composition. The obtained silane-modified polyethylene composition was formed into a sheet using a T-die and a cooling casting roll, and biaxially stretched by MD stretching and then TD stretching using a tenter-type successive stretching machine. The MD stretch ratio was 5.5 times, and the TD stretch ratio was 5.0 times. The stretching temperatures were 105°C in MD and 125°C in TD. Liquid paraffin was extracted from the stretched sheet using methylene chloride, and the sheet was heat-set at 126°C with a stretch ratio of 1.3 to 1.1 times to prepare a porous membrane. This porous membrane was subjected to aqueous crosslinking for 48 hours under conditions of 85°C and 85% relative humidity to obtain a separator shown in Table 7. The obtained separator and the battery including the separator were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 7.

[0315] [Comparative Example 3] Preparation and evaluation of separator Modified polyolefin H3-1 (VH035H manufactured by Daehan Petrochemical Industries Co., Ltd.) containing an average of 7.7 alkylene groups with 3 carbon atoms as short chain branches (SCB) based on 1,000 carbon atoms was prepared. This modified polyolefin had a weight average molecular weight of 380,000 and a melting point of 129.1°C. In this case, the modified polyolefin was a polyolefin containing repeating units derived from ethylene and repeating units derived from α-olefin, and the repeating units derived from α-olefin were derived from 1-pentene. The modified polyolefin H3-1 prepared as the input polyolefin was 7.5 kg / h, silane-unmodified polyethylene (VH035 manufactured by Daehan Petrochemical Industries Co., Ltd.) with a weight average molecular weight of 300,000 and a melting point of 135°C was 7.5 kg / h, and liquid paraffin (dynamic viscosity at 37.78°C 7.59×10) was used as a plasticizer. -5 m 2The extruder was fed with 35 kg / h of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP) as an initiator, vinyltrimethoxysilane (VTMS) as a crosslinking agent containing a carbon-carbon double bond group as an alkoxysilane, and dibutyltin dilaurate (DBTDL) as a catalyst. The weight ratio of the modified polyolefin H3-1 to the silane-unmodified polyolefin was 50:50, and when the number of carbon atoms in the alkyl group of the repeating unit derived from α-olefin was 3, the number of carbon atoms in the main polyolefin chain of the polyolefin fed was 1,000. The weight ratio of the polyolefin fed to the plasticizer was 30:70. The content of the carbon-carbon double bond-containing alkoxyvinylsilane was 0.3 parts by weight based on 100 parts by weight of the total content of the input polyolefin and the plasticizer, the content of the initiator was 1.7 parts by weight based on 100 parts by weight of the carbon-carbon double bond-containing alkoxysilane, and the content of the crosslinking catalyst was 6.7 parts by weight based on 100 parts by weight of the carbon-carbon double bond-containing alkoxysilane. After that, the mixture was mixed in an extruder, and the resulting mixture was extruded at a temperature condition of 190°C to obtain a silane-modified polyolefin composition H3-2. The obtained silane-modified polyolefin composition H3-2 was formed into a sheet using a T-die and a cooling casting roll, and biaxially stretched using a tenter-type sequential stretching machine that performs MD stretching and then TD stretching. Both the MD stretching ratio and the TD stretching ratio were 7.0 times. The stretching temperatures were 103°C in MD and 118°C in TD. Considering the melting temperature of the modified polyolefin, the sheet was stretched at a temperature lower than that used for a typical polyolefin alone. Liquid paraffin was extracted from the stretched sheet using methylene chloride, and the sheet was heat-set at 124°C to produce a porous film. This porous film was subjected to aqueous crosslinking for 24 hours under conditions of 85°C and 85% relative humidity to obtain the separator shown in Table 7. The obtained separator and the battery containing the separator were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 7.

[0316] [Comparative Example 5] Preparation and evaluation of separator 18 parts by mass of high density polyethylene "SH800" (trademark, Asahi Kasei Chemicals Corporation) with a viscosity average molecular weight (Mv) of 270,000, 12 parts by mass of ultra-high molecular weight polyethylene "UH850" (trademark, Asahi Kasei Chemicals Corporation) with an Mv of 2 million, 20 parts by mass of silica "DM10C" (trademark, Tokuyama Corporation, hydrophobized with dimethyldichlorosilane) with an average primary particle size of 15 nm, 30 parts by mass of liquid paraffin "Sumoil P-350P" (trademark, Matsumura Oil Research Institute Corporation) as a plasticizer, and 0.3 parts by mass of pentaerythrityl-tetrakis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] as an antioxidant were premixed in a super mixer. The resulting mixture was fed to the feed port of a twin-screw co-rotating screw extruder by a feeder. In addition, liquid paraffin was side-fed into the twin-screw extruder cylinder so that the ratio of liquid paraffin to the total mixture (100 parts by mass) melt-kneaded and extruded was 50 parts by mass. The melt-kneading conditions in the extruder were a set temperature of 200°C, a screw rotation speed of 180 rpm, and a discharge rate of 12 kg / h. The melt-kneaded product was then extruded between a cooling roll whose surface temperature was controlled to 25°C through a gear pump, a conduit, and a T-die, each of which was set at a temperature of 220°C, to obtain a sheet-like polyolefin composition. Next, the sheet-like polyolefin composition was continuously introduced into a simultaneous biaxial tenter, and simultaneous biaxial stretching was performed 7 times in the longitudinal direction and 7 times in the transverse direction. At this time, the set temperature of the simultaneous biaxial tenter was 123°C. Next, the sheet-like polyolefin composition was introduced into a methylene chloride tank and thoroughly immersed in methylene chloride to extract and remove the liquid paraffin. After that, the methylene chloride was dried. The sheet-like polyolefin composition was then introduced into a transverse tenter, stretched 1.4 times in the transverse direction, and then relaxed to a final outlet of 1.2 times, followed by winding to obtain a separator as shown in Table 7. The set temperature of the transverse stretching section was 132° C., and the set temperature of the relaxation section was 137° C. The obtained separator and the battery including the same were subjected to various evaluations according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 8.

[0317] [Comparative Example 6] Preparation and evaluation of separator 25 parts by weight of high density polyethylene (HDPE) with a weight average molecular weight (Mw) of 380,000 and a molecular weight distribution (Mw / Mn) of 5, 0.5 parts by weight of resin raw material A1 with a kinetic viscosity at 40°C, and 70 parts by weight of paraffin oil were mixed and introduced into a twin-screw extruder (inner diameter 58 mm, L / D = 56, twin-screw extruder). This mixture was discharged from the twin-screw extruder into a T-die with a width of 300 mm under conditions of 200°C and a screw rotation speed of 40 rpm. The discharged material was then passed through a casting roll at a temperature of 40°C to produce a base sheet with a thickness of 800 μm. This base sheet was stretched six times in the longitudinal direction with a roll stretcher at 110°C, and then stretched seven times in the transverse direction with a tenter stretcher at 125°C to produce a stretched film. This stretched film was immersed in a dichloromethane leaching tank at 25°C for 1 minute to extract and remove the paraffin oil, and a porous membrane was produced. This porous film was dried at 50°C, and then heated to 125°C in a tenter-type stretching machine and heat-set at 1.25 times the width in the transverse direction (TD) compared to before stretching. This porous film was crosslinked for 72 hours in a thermo-hygrostat at a temperature of 85°C and a humidity of 85%, to obtain a separator shown in Table 8. The obtained separator and a battery including the same were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 8.

[0318] [Comparative Example 8] Preparation and evaluation of separator In the extruder, silane-unmodified polyethylene with a weight average molecular weight of 900,000 and a melting point of 135°C was fed at 22.4 kg / h, resin raw material A1 was fed at 22.4 kg / h, and liquid paraffin (dynamic viscosity at 37.78°C is 7.59 x 10 -5 m 2The mixture was mixed at a flow rate of 115.2 kg / h (flow rate: 1 / s). The weight ratio of silane-unmodified polyethylene:silane-modified polyethylene:liquid paraffin was 14:14:72. Furthermore, 0.5 parts by mass of vinyltriethoxysilane as a carbon-carbon double bond group-containing alkoxysilane compound based on a total of 100 parts by mass of silane-unmodified polyethylene, silane-modified polyethylene, and liquid paraffin, 2 parts by mass of dibutyltin dilaurate as a crosslinking catalyst based on 100 parts by mass of the carbon-carbon double bond group-containing alkoxysilane compound, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (DHBP) as an initiator based on 100 parts by mass of the carbon-carbon double bond group-containing alkoxysilane compound were introduced into the extruder and mixed. Then, extrusion was performed at a temperature of 200°C to obtain a silane-modified polyethylene composition. The obtained silane-modified polyethylene composition was formed into a sheet using a T-die and a cooling casting roll, and biaxially stretched by MD stretching and then TD stretching using a tenter-type successive stretching machine. The MD stretch ratio was 5.5 times, and the TD stretch ratio was 5.0 times. The stretching temperatures were 105°C in MD and 125°C in TD. Liquid paraffin was extracted from the stretched sheet using methylene chloride, and the sheet was heat-set at 126°C with a stretch ratio of 1.3 to 1.1 times to produce a porous membrane. This porous membrane was subjected to aqueous crosslinking for 48 hours under conditions of 85°C and 85% relative humidity to obtain a separator shown in Table 8. The obtained separator and the battery including the separator were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 8.

[0319] [Examples 1, 34 to 39, Comparative Examples 1, 4, 7, 9, and 10] As shown in Tables 2, 7, and 9 to 14, the separators obtained in Examples 1, 34 to 39 and Comparative Examples 1, 4, 7, 9, and 10 were arranged in order of the air permeability change ratio when compressed by 30% in the thickness direction, and the effects on the first battery configuration (Tables 9 and 10), the second battery configuration (Tables 11 and 12), and the third battery configuration (Tables 13 and 14) were tested, respectively.

[0320] [Relationship between the separator of Example 1 and various battery configurations: Examples 1A to 1Q] For the separator obtained in Example 1, evaluation was performed on batteries produced by changing the battery configuration as shown in Tables 15 to 17. The battery evaluation results are also shown in Tables 15 to 17, with sub-numbers of Examples 1A to 1Q given according to the battery configuration.

[0321] [Electrolyte blending conditions, electrolyte blending conditions, resin raw material composition] Table 18 shows the electrolyte blending conditions used in the production of the batteries and separators and in various evaluations, Table 19 shows the electrolyte blending conditions, and Tables 20 to 22 show the resin raw material compositions, respectively.

[0322] [Table 2]

[0323] [Table 3]

[0324] [Table 4]

[0325] [Table 5]

[0326] [Table 6]

[0327] [Table 7]

[0328] [Table 8]

[0329] [Table 9]

[0330]

Table 10

[0331]

Table 11

[0332]

Table 12

[0333]

Table 13

[0334]

Table 14

[0335]

Table 15

[0336]

Table 16

[0337]

Table 17

[0338]

Table 18

[0339]

Table 19

[0340] [Table 20]

[0341] [Table 21]

[0342] [Table 22]

[0343] <Evaluation of a separator having a multi-layer structure and a battery including the same>

[0344] [Table 23-1]

[0345] [Table 23-2]

[0346] [Table 24]

[0347] [Table 25]

[0348] (Acrylic latex manufacturing method) Acrylic latex used as a thermoplastic polymer or resin binder is produced by the following method. 70.4 parts by mass of ion-exchanged water, 0.5 parts by mass of "Aqualon KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 0.5 parts by mass of "ADEKA REASOAP SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Corporation) were added as emulsifiers to a reaction vessel equipped with a stirrer, a reflux condenser, a dripping tank, and a thermometer. Next, the temperature inside the reaction vessel was raised to 80°C, and while maintaining the temperature at 80°C, 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate was added to obtain an initial mixture. The addition of the aqueous ammonium persulfate solution was completed. Five minutes later, the emulsion was dripped from the dripping tank into the reaction vessel over 150 minutes. The above emulsion was prepared by mixing 70 parts by mass of butyl acrylate, 29 parts by mass of methyl methacrylate, 1 part by mass of methacrylic acid, 3 parts by mass of "Aqualon KH1025" (registered trademark, 25% aqueous solution manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) and 3 parts by mass of "Adeka Reasoap SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Corporation) as emulsifiers, 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate, and 52 parts by mass of ion-exchanged water using a homomixer for 5 minutes. After the emulsion was added, the temperature inside the reaction vessel was kept at 80°C for 90 minutes, and then cooled to room temperature. The resulting emulsion was adjusted to pH 8.0 with 25% aqueous ammonium hydroxide solution, and a small amount of water was added to obtain an acrylic latex with a solid content of 40%. The resulting acrylic latex had a number average particle size of 145 nm and a glass transition temperature of -23°C.

[0349] (Other resins) Commercially available PVDF latex and polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) were prepared. In addition, the above acrylic latex and PVDF latex were used to prepare an aqueous mixture of PVDF and acrylic (mixing ratio shown in the table below). Furthermore, an acrylic resin was formed by core-shell polymerization to prepare a PVDF / acrylic (core-shell polymerization) mixture.

[0350] <Confirmation that crosslinking occurs by coating an inorganic porous layer on a separator substrate> [Example 40-1: Preparation and evaluation of separator and confirmation of cross-linking during coating process] (Preparation of polyolefin microporous membrane as separator substrate) To a mixed resin composition of 30.0 mass% of resin D2 (number of silane graft linkages CH2: 2), 30.0 mass% of resin E3, and 40.0 mass% of resin F3, 1000 mass ppm of pentaerythrityl-tetrakis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] was added as an antioxidant to the whole, and the mixture was dry-blended using a tumbler blender to obtain a mixture. The obtained mixture was fed to a twin-screw extruder by a feeder under a nitrogen atmosphere. In addition, liquid paraffin (dynamic viscosity at 37.78°C: 7.59×10 -5 m 2 / s) was pumped into the extruder cylinder by a plunger pump.

[0351] The mixture and liquid paraffin were melt-kneaded in the extruder, and the feeder and pump were adjusted so that the liquid paraffin content in the extruded polyolefin composition was 75% by mass (i.e., the polymer concentration was 25% by mass). The melt-kneading conditions were a set temperature of 230°C, a screw rotation speed of 100 rpm, and a discharge rate of 80 kg / h. The melt-kneaded product was then extruded and cast onto a cooling roll whose surface temperature was controlled to 25°C through a T-die, to obtain a gel sheet (sheet-shaped molded product) with a thickness of 1250 μm.

[0352] Next, the sheet-shaped molded body was introduced into a simultaneous biaxial tenter stretching machine, and biaxial stretching was performed to obtain a stretched product. The set stretching conditions were MD magnification 7.0 times, TD magnification 6.4 times (i.e., 7 x 6.4 times), and biaxial stretching temperature 125 ° C. Next, the gel sheet after stretching was introduced into a dichloromethane tank and thoroughly immersed in dichloromethane to extract and remove liquid paraffin, and then the dichloromethane was dried and removed to obtain a porous body. Next, the porous body was introduced into a TD tenter to perform heat setting (HS), and HS was performed at a heat setting temperature of 133 ° C and a stretching ratio of 1.8 times, and then a relaxation operation was performed to TD 1.6 times based on the sheet width at the entrance of the TD tenter to obtain a microporous membrane. Then, the end of the obtained microporous membrane was cut and wound up as a mother roll with a width of 1,100 mm and a length of 5,000 m.

[0353] The obtained polyolefin microporous membrane was used as a separator substrate, and measurements and evaluations were carried out according to the above-mentioned methods. The evaluation results are shown in Table 26.

[0354] (Coating of inorganic porous layer and cross-linking confirmation) Next, boehmite was selected as the inorganic particles as shown in Table 26. Furthermore, inorganic particles and an aqueous solution of ammonium polycarboxylate (SN Dispersant 5468 manufactured by San Nopco, solid content concentration 40%) as an ionic dispersant were uniformly dispersed in 100 parts by weight of water at a predetermined ratio to prepare a dispersion. The obtained dispersion was crushed with a bead mill (cell volume 200cc, zirconia bead diameter 0.1mm, filling amount 80%) to adjust the particle size distribution of the inorganic particles to D50 = 1.0μm. The above acrylic latex (solid content concentration 40%, average particle size 145nm, glass transition temperature -23℃, constituent monomers: butyl acrylate, methyl methacrylate, methacrylic acid) was added as a resin binder to the dispersion with the adjusted particle size distribution so as to obtain the inorganic particle weight ratio shown in Table 26, thereby preparing an inorganic particle-containing slurry. According to the above-mentioned method, the pH of the inorganic particle-containing slurry and the contact angle of the coating liquid with respect to the clean surface of the separator substrate were also measured. A microporous membrane was continuously unwound from the microporous membrane mother roll, and one side of the microporous membrane was coated with an inorganic particle-containing slurry using a gravure reverse coater, then dried in a dryer at 60°C to remove water, and wound up to obtain a mother roll of a multilayer separator with a coating thickness as shown in Table 26. The progress of the crosslinking reaction in the coating process was confirmed by comparing the TMA rupture temperatures before and after coating. At the time of evaluation, the multilayer separator unwound from the mother roll was slit as necessary and used as an evaluation separator. The obtained separator for evaluation was subjected to various evaluations according to the above-mentioned evaluation methods, and the evaluation results are shown in Table 26.

[0355] (Testing of batteries containing multi-layer separators coated with inorganic porous layers) In Example 40-1, a separator substrate made of a polyolefin microporous membrane and a multi-layer separator coated with an inorganic porous layer were obtained. Furthermore, a non-aqueous secondary battery was produced using the multi-layer separator according to the battery production method described above, and the battery evaluation results are shown in Table 26.

[0356] [Examples 40-2 to 40-53, Comparative Examples 11-1 to 11-7] As shown in Table 26, except for changing the resin composition and molecular weight mixture composition of the polyolefin microporous membrane, preparation conditions, substrate characteristics, type and ratio of inorganic particles, composition and physical properties of the coating liquid, the same operation as in Example 40-1 was performed to obtain a separator substrate made of a polyolefin microporous membrane and a multi-layer separator coated with an inorganic porous layer. The obtained separator substrate and multi-layer separator were evaluated in various ways according to the above-mentioned evaluation method, and the evaluation results are also shown in Table 26. Furthermore, a non-aqueous secondary battery was obtained using the multi-layer separator coated with an inorganic porous layer. The obtained battery was evaluated in various ways according to the above-mentioned evaluation method, and the evaluation results are also shown in Table 26.

[0357] [Table 26-1]

[0358] [Table 26-2]

[0359] [Table 26-3]

[0360] [Table 26-4]

[0361] [Table 26-5]

[0362] [Table 26-6]

[0363] [Table 26-7]

[0364] <Confirmation that crosslinking occurs by coating a thermoplastic polymer-containing layer on a separator substrate> [Example 41-1] As shown in Table 27, separator substrates made of polyolefin microporous membranes were obtained by the same operations as in Example 40-1, except that the preparation conditions of the polyolefin microporous membranes were changed. Next, as shown in Table 27, the type of resin and the concentration of the organic solvent were adjusted to obtain a thermoplastic polymer-containing coating solution, and the pH of the coating solution and the contact angle of the coating solution with the clean separator substrate surface were also measured according to the method described above. Furthermore, the coating liquid was applied to the separator substrate using a gravure reverse coater in the same manner as in Example 40-1, to obtain a multi-layer separator having a coating thickness as shown in Table 27. The progress of the crosslinking reaction in the coating process was confirmed by comparing the TMA rupture temperature before and after coating. The obtained multi-layer separator was evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 27. Furthermore, a non-aqueous secondary battery was produced using the multi-layer separator according to the battery production method described above, and the battery was evaluated. The results of the battery evaluation are also shown in Table 27.

[0365] [Examples 41-2 to 41-49, Comparative Examples 12-1 to 12-7] As shown in Table 27, the resin composition and molecular weight mixture composition of the polyolefin microporous membrane, the preparation conditions, the substrate characteristics, the type of thermoplastic resin, the composition and physical properties of the coating liquid, etc. were changed, and the same operations as in Example 41-1 were performed to obtain a separator substrate made of a polyolefin microporous membrane and a multi-layer separator coated with a thermoplastic polymer-containing layer. The obtained separator substrate and multi-layer separator were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 27. Furthermore, a non-aqueous secondary battery was obtained by using a multi-layer separator coated with a thermoplastic polymer-containing layer. The obtained battery was evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 27.

[0366] [Table 27-1]

[0367] [Table 27-2]

[0368] [Table 27-3]

[0369] [Table 27-4]

[0370] [Table 27-5]

[0371] [Table 27-6]

[0372] <Confirmation that crosslinking occurs when the active layer is applied to the separator substrate> [Example 42-1] As shown in Table 28, separator substrates made of polyolefin microporous membranes were obtained by the same procedure as in Example 40-1, except that the preparation conditions of the polyolefin microporous membrane were changed. Next, commercially available PVDF-HFP was prepared as a fluororesin, as shown in Table 28. Furthermore, a coating liquid having an organic solvent concentration shown in Table 28 was prepared using 95 parts by weight of aluminum oxide hydroxide (average particle size 1.4 μm) as inorganic particles, PVDF-HFP, and N-methyl-2-pyrrolidone (NMP) as an organic solvent. Furthermore, the coating liquid was applied to the separator substrate using a gravure reverse coater in the same manner as in Example 40-1, followed by washing with water and drying to obtain a multi-layer separator having a coating thickness as shown in Table 28. The progress of the crosslinking reaction in the coating process was confirmed by comparing the TMA rupture temperature before and after coating. The obtained multi-layer separator was evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 28. Furthermore, a non-aqueous secondary battery was produced using the multi-layer separator according to the battery production method described above, and the battery was evaluated. The results of the battery evaluation are also shown in Table 28.

[0373] [Examples 42-2 to 42-43, Comparative Examples 13-1 to 13-7] As shown in Table 28, the resin composition and molecular weight mixture composition of the polyolefin microporous membrane, the preparation conditions, the substrate characteristics, the type of fluororesin, the composition and physical properties of the coating liquid, etc. were changed, and the same operations as in Example 42-1 were performed to obtain a separator substrate made of a polyolefin microporous membrane and a multilayer separator coated with an active layer. The obtained separator substrate and multilayer separator were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 28. Furthermore, a non-aqueous secondary battery was obtained by using a multi-layer separator coated with an active layer. The obtained battery was evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are shown in Table 28.

[0374] [Table 28-1]

[0375] [Table 28-2]

[0376] [Table 28-3]

[0377] [Table 28-4]

[0378] [Table 28-5]

[0379] [Table 28-6]

[0380] <Confirmation of crosslinking by coating a heat-resistant resin layer on a separator substrate> [Example 43-1] As shown in Table 29, separator substrates made of polyolefin microporous membranes were obtained by the same procedures as in Example 40-1, except that the preparation conditions of the polyolefin microporous membranes were changed. Next, as shown in Table 29, an inorganic filler having a predetermined inorganic particle size was prepared, and was blended into a coating liquid containing para-aromatic aramid or meta-aromatic aramid so as to obtain a predetermined inorganic particle weight ratio and organic solvent concentration.

[0381] (In the case of para-aromatic aramid) 150 parts by mass of paraphenylenediamine was added to 5000 parts by mass of N-methyl-2-pyrrolidone (NMP) / calcium chloride solution (calcium chloride concentration = 7.1% by mass), dissolved and stirred under N2 atmosphere, and then 273.94 parts by mass of terephthalic acid dichloride was added, stirred and reacted for 1 hour to obtain a polyparaphenylene terephthalamide polymerization solution. 1000 parts by mass of the polymerization solution, 3000 parts by mass of NMP, and a predetermined amount of alumina (Al2O3) particles (having a particle size shown in Table 29) were stirred and mixed, and dispersed with a homogenizer to obtain a coating solution. Using a drum-fixed bar coater, the coating solution was applied to one side of a polyolefin microporous film under conditions of a clearance of 20 μm to 30 μm and a coating film thickness shown in Table 29, and dried at a temperature of about 70 ° C. to obtain a multi-layer separator.

[0382] (In the case of meta-aromatic aramid) 100 parts by mass of meta-aromatic polyamide and a predetermined amount of boehmite (having a particle size shown in Table 29) were mixed, and the mixture was mixed with a mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (mass ratio = 1:1) so that the meta-aromatic polyamide concentration was 3 mass % to obtain a coating liquid. Using a Mayer bar coater, the coating liquid was applied to one side of a polyolefin microporous membrane under the conditions of a clearance of 20 μm to 30 μm and a coating thickness shown in Table 29 to obtain a coated separator. The coated separator was immersed in a coagulation liquid with a mass ratio of water:DMAc:TPG = 2:1:1 and a temperature of 35 ° C., followed by washing with water and drying to obtain a multi-layer separator.

[0383] For multi-layer separators coated with a heat-resistant resin layer containing para- or meta-aromatic aramid and inorganic filler, the progress of the cross-linking reaction during the coating process was confirmed by comparing the TMA rupture temperature before and after coating. The obtained multi-layer separators were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 29.

[0384] (Testing of batteries containing multi-layer separators coated with heat-resistant resin layers) In Example 43-1, a non-aqueous secondary battery was produced using the multi-layer separator according to the battery production method described above, and the battery was evaluated. The battery evaluation results are also shown in Table 29.

[0385] [Examples 43-2 to 43-50, Comparative Examples 14-1 to 14-7] As shown in Table 29, the resin composition and molecular weight mixture composition of the polyolefin microporous membrane, the preparation conditions, the substrate characteristics, the type, particle size and ratio of the inorganic filler, the type of aramid resin, the composition and physical properties of the coating liquid, etc. were changed, and the same operations as in Example 43-1 were performed to obtain a separator substrate made of a polyolefin microporous membrane and a multilayer separator coated with a heat-resistant resin layer. The obtained separator substrate and multilayer separator were evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 29. Furthermore, a non-aqueous secondary battery was obtained by using a multi-layer separator coated with a heat-resistant resin layer. The obtained battery was evaluated in various ways according to the above-mentioned evaluation methods, and the evaluation results are also shown in Table 29.

[0386] [Table 29-1]

[0387] [Table 29-2]

[0388] [Table 29-3]

[0389] [Table 29-4]

[0390] [Table 29-5]

[0391] [Table 29-6] [Explanation of symbols]

[0392] t c Crystal thickness t a Amorphous part thickness f c crystal long period a c crystal orientation degree

Claims

1. A non-aqueous secondary battery separator comprising a polyethylene microporous membrane, A silane-modified polyethylene and a polyolefin other than the silane-modified polyethylene, A separator for a non-aqueous secondary battery, in which the rate of change in air permeability (air permeability Sh after compression / air permeability Sj before compression) when compressed by 30% of its thickness is 1.1 to 7.0 times.

2. A non-aqueous secondary battery comprising: a positive electrode; a negative electrode; the separator for a non-aqueous secondary battery according to claim 1; and a non-aqueous electrolyte.

3. The positive electrode has the formula: Li-Ni x -Mn y -Co z 3. The nonaqueous secondary battery according to claim 2, comprising a lithium (Li)-nickel (Ni)-manganese (Mn)-cobalt (Co) composite oxide represented by the formula: {wherein x represents the Ni proportion, y represents the Mn proportion, z represents the Co proportion, and x+y+z=1}, wherein the Ni proportion x in the formula is 5 to 9.

4. 4. The nonaqueous secondary battery according to claim 2, wherein the negative electrode comprises a negative electrode active material, and a ratio of Si in the negative electrode active material is 5% by weight to 90% by weight.

5. 5. The nonaqueous secondary battery according to claim 2, wherein the nonaqueous electrolyte contains a lithium salt at a concentration in the range of 1.2 mol / L to 10 mol / L.

6. The non-aqueous electrolyte solution contains ethyl methyl carbonate (EMC) and / or acetonitrile (AcN), and the total content of EMC and AcN in the non-aqueous electrolyte solution is in the range of 50% by mass to 90% by mass. The non-aqueous secondary battery according to any one of claims 2 to 5.