Polypropylene-based resin composition

A polypropylene resin composition stabilizes mechanical properties by blending recycled materials from bottle caps and other products with a crystal nucleating agent, addressing the variability in source materials.

JP2024127361APending Publication Date: 2024-09-20PRIME POLYMER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023036477
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-09-20

AI Technical Summary

Technical Problem

The challenge lies in maintaining consistent mechanical properties of recycled polypropylene resin compositions when derived from a wide range of products, as the physical properties vary widely, making it difficult to use them for specific applications.

Method used

A polypropylene resin composition is formulated by mixing recycled materials from bottle caps and other products, with specific ratios and inclusion of a crystal nucleating agent, ensuring stability and mechanical properties are maintained regardless of the source.

Benefits of technology

The composition achieves stable mechanical properties, such as tensile modulus and impact resistance, allowing it to be used for specific purposes despite varying sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024127361000001
    Figure 2024127361000001
Patent Text Reader

Abstract

To provide a polypropylene-based resin composition which is stable in mechanical properties (for example, tensile modulus and impact resistance) without influenced by the kind of a product derived from anything even when a recycled material recovered from not only a specific product but also a wide range of products is mixed, and can be used for a specific application.SOLUTION: A polypropylene-based resin composition comprises a recycled material (A) derived from a bottle cap and a recycled material (B) derived from a product other than the bottle cap.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polypropylene resin composition. [Background technology]

[0002] Polypropylene is easy to process and has excellent rigidity and heat resistance. It can be molded using a variety of molding methods, including injection molding and extrusion molding, and is widely used in household goods such as home appliances and food containers, as well as automotive interior exterior components. From the viewpoint of resource conservation, attempts are being made to collect and reuse polypropylene products used in the market. One example of a polypropylene product that can be collected is a plastic beverage bottle cap. However, the amount of polypropylene used in plastic beverage bottle caps on the market is very small compared to polyethylene, and the amount of polypropylene that can be collected from plastic beverage bottle caps is small.

[0003] Patent Document 1 discloses a method for producing a recycled propylene-based resin with controlled fluidity from propylene-based resin recovered from the market for home appliances, automobiles, and the like.

[0004] Furthermore, Patent Document 2 discloses a plastic molded product that uses plastic materials (recycled materials) containing polyethylene, polypropylene, and the like, and has an excellent balance between flexibility and hardness. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-277366 A [Patent Document 2] JP 2022-114370 A Summary of the Invention [Problem to be solved by the invention]

[0006] Considering the amount of polypropylene that can be recovered, it is desirable to use polypropylene-based resins (recycled materials) recovered widely from not only bottle caps but also other products; however, in that case, there is a problem that the range of physical properties of the composition obtained varies widely depending on the product from which the recycled material is derived, making it difficult to use for specific purposes. The present invention aims to provide a polypropylene resin composition which has stable mechanical properties (e.g., tensile modulus and impact resistance) without being affected by the type of product from which it is derived, even when mixed with recycled materials recovered from a wide range of products, not limited to a specific product, and which can be used for specific applications. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by mixing recycled materials from bottle caps, and have completed the present invention. For example, the present invention includes the following aspects.

[0008] [1] A polypropylene resin composition comprising: (A) a recycled material derived from a bottle cap; and (B) a recycled material derived from a product other than the bottle cap.

[0009] [2] The polypropylene resin composition according to [1], wherein the content of the recycled material (A) is 5 to 50 mass%, and the content of the recycled material (B) is 50 to 95 mass%, when the total content of the recycled material (A) and the recycled material (B) is 100 mass%.

[0010] [3] The polypropylene resin composition according to [1] or [2], wherein the recycled material (A) contains 0.01 to 0.5 parts by mass of a crystal nucleating agent per 100 parts by mass of the recycled material (A).

[0011] [4] The polypropylene resin composition according to any one of [1] to [3], wherein the melt flow rate (MFR) of the recycled material (A) measured in accordance with JIS K 7210 at 230°C under a load of 2.16 kg is in the range of 1 to 100 g / 10 min.

[0012] [5] The polypropylene resin composition according to any one of [1] to [4], wherein the melt flow rate (MFR) of the recycled material (B) measured in accordance with JIS K 7210 at 230°C under a load of 2.16 kg is in the range of 1 to 100 g / 10 min.

[0013] [6] The polypropylene resin composition according to any one of [1] to [5], wherein the recycled material (A) is derived from a plastic beverage bottle cap. Effect of the Invention

[0014] According to the present invention, it is possible to provide a polypropylene resin composition which has stable mechanical properties (e.g., tensile modulus and impact resistance) without being affected by the type of product from which it is derived, even when recycled materials recovered from a wide range of products, not limited to a specific product, are mixed, and which can be used for specific applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In the present disclosure, the expressions "XX or more and YY or less" and "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. Furthermore, when numerical ranges are described in stages, the upper and lower limits of each numerical range can be combined in any manner.

[0016] The present invention will be described in detail below. The polypropylene resin composition of the present invention (hereinafter also simply referred to as "the composition of the present invention") contains specific recycled material (A) and recycled material (B) described below.

[0017] [Recycled material (A)] The composition of the present invention contains a recycled material (A) derived from a bottle cap. By mixing the recycled material (A), the mechanical properties of the composition of the present invention are stable and not affected by the type of the derived product, even when a recycled material (B) derived from a product other than a bottle cap, which will be described later, is mixed, and the composition can be used for a specific purpose.

[0018] In the recycled material (A), the melt flow rate (MFR) measured according to JIS K 7210 at 230°C under a load of 2.16 kg is preferably in the range of 1.0 to 100.0 g / 10 min. The lower limit of the MFR is more preferably 2.0 g / 10 min, further preferably 4.0 g / 10 min, and particularly preferably 6.0 g / 10 min. On the other hand, the upper limit of the MFR is more preferably 50.0 g / 10 min, further preferably 30.0 g / 10 min, and particularly preferably 20.0 g / 10 min.

[0019] When the MFR of the recycled material (A) is within the above range, the recycled material (A) itself has good mechanical strength, and the composition of the present invention has excellent mechanical properties.

[0020] The recycled material (A) preferably contains a crystal nucleating agent. The content of the crystal nucleating agent is preferably 0.01 to 0.5 parts by mass, more preferably 0.02 to 0.4 parts by mass, and even more preferably 0.03 to 0.3 parts by mass, relative to 100 parts by mass of the recycled material (A). When the amount of the crystal nucleating agent in the recycled material (A) is within the above range, the crystal nucleating agent acts on the crystals of the entire composition, so that the composition of the present invention has stable mechanical properties without being affected by the type of the derived product even when the recycled material (B) derived from a product other than a bottle cap is mixed.

[0021] As the crystal nucleating agent, any agent capable of acting as a nucleus when the polypropylene resin crystallizes can be used without any limitation.

[0022] The crystal nucleating agent used in the present invention means an additive that generates a nucleation site when the polypropylene resin crystallizes in the transition state from the molten state to the cooled solid structure of the polypropylene resin. The crystal nucleating agent may be used alone or in combination of two or more kinds.

[0023] The crystal nucleating agent preferably used in the present invention is not particularly limited, and examples thereof include sorbitol-based crystal nucleating agents, phosphorus-based crystal nucleating agents, metal carboxylate-based crystal nucleating agents, polymer-based crystal nucleating agents, inorganic compounds, etc. As the crystal nucleating agent, sorbitol-based crystal nucleating agents, phosphorus-based crystal nucleating agents, and polymer-based crystal nucleating agents are preferred.

[0024] Specific examples of sorbitol-based crystal nucleating agents include 1,2,3-trideoxy-4,6:5,7-bis-O-[(4-propylphenyl)methylene]-nonitol (commercially available products containing this compound include the trade name "Milad NX8000" series (manufactured by Milliken)), 1,3,2,4-dibenzylidene sorbitol, 1,3,2,4-di-(p-methylbenzylidene) sorbitol, and 1,3-p-chlorobenzylidene-2,4-p-methylbenzylidene sorbitol.

[0025] Specific examples of phosphorus-based crystal nucleating agents include sodium bis-(4-t-butylphenyl) phosphate, potassium bis-(4-t-butylphenyl) phosphate, sodium 2,2'-ethylidene bis(4,6-di-t-butylphenyl) phosphate, sodium 2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate, and bis(2,4,8,10-tetra-t-butyl-6-hydroxy-12H-dibenzo[d,g][1,3,2]dioxaphosphocin-6-oxide) sodium salt (trade name "ADK STAB (registered trademark)"). Examples of such a compound include a compound having bis(2,4,8,10-tetra-t-butyl-6-hydroxy-12H-dibenzo[d,g][1,3,2]dioxaphosphocin-6-oxide) aluminum hydroxide salt as the main component (trade name "ADK STAB NA-21", manufactured by ADEKA Corporation), and a compound containing lithium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate and 12-hydroxystearic acid and containing lithium as an essential component (trade name "ADK STAB NA-71", manufactured by ADEKA Corporation).

[0026] Specific examples of metal carboxylate crystal nucleating agents include aluminum pt-butylbenzoate, aluminum hydroxy-di(pt-butylbenzoate) (product name "AL-PTBBA", manufactured by Japan Chemtech), aluminum adipate, and sodium benzoate.

[0027] As the polymer-based crystal nucleating agent, branched α-olefin polymers are preferably used. Examples of branched α-olefin polymers include homopolymers of 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, and 3-ethyl-1-hexene, or copolymers thereof, and further copolymers thereof with other α-olefins. In particular, 3-methyl-1-butene polymers are preferred from the viewpoint of low-temperature impact resistance, good rigidity properties, and economic efficiency.

[0028] As the recycled material (A), propylene molded products recovered from bottle caps and their crushed products, molded parts (scrap materials) and molded balls generated in the propylene molding process and their crushed products can be used. As the recycled material (A), a single type or a mixture of multiple polypropylene resin components with different fluidity, density, and propylene content can be used, and it is particularly preferable to use a single type or a resin consisting of a mixture of multiple components with different fluidity and density, etc., in order not to impair mechanical properties. It is preferable to select and use one or a blend of two or more of these polypropylene resins that satisfy the above MFR.

[0029] Various known polypropylene-based resins can be used as the recycled material (A). The polypropylene-based resin may be homopolypropylene, or may be a copolymer of propylene and other olefins or a monomer component copolymerizable with propylene, such as a random copolymer or a block copolymer. Examples of other olefins include α-olefins such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, and 4-methyl-1-pentene, vinyl compounds such as vinylcyclopentene, vinylcyclohexane, and vinylnorbornane, vinyl esters such as vinyl acetate, and unsaturated organic acids such as maleic anhydride or derivatives thereof.

[0030] The polypropylene-based resin may contain a biomass-derived monomer. The same type of monomer constituting the polypropylene-based resin may be only a biomass-derived monomer, may be only a fossil fuel-derived monomer, or may contain both a biomass-derived monomer and a fossil fuel-derived monomer.

[0031] Biomass-derived monomers are monomers derived from any renewable natural raw materials, including fungi, yeasts, algae, and bacteria, and their residues, whether plant- or animal-derived, and contain carbon as the raw material.14 C isotope 10 -12 The biomass carbon concentration (pMC) measured in accordance with ASTM D 6866 is about 100 (pMC). The biomass-derived monomer is obtained by a conventionally known method.

[0032] It is preferable that the polypropylene-based resin contains a biomass-derived monomer from the viewpoint of reducing the environmental load (mainly reducing greenhouse gases). If the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, even if the raw olefin is a propylene-based polymer containing a biomass-derived olefin, 14 C isotope 10 -12 Other than the proportion of propylene in the polymer, the molecular structure is the same as that of propylene polymers made from fossil fuel-derived monomers, and therefore the performance is said to be the same.

[0033] The polypropylene resin may contain a chemically recycled monomer. The same type of monomer constituting the polypropylene resin may be only a chemically recycled monomer, or may contain a chemically recycled monomer and a fossil fuel-derived monomer and / or a biomass-derived monomer. The chemically recycled monomer is obtained by a conventionally known method.

[0034] It is preferable that the polypropylene resin contains a monomer derived from chemical recycling from the viewpoint of reducing the environmental load (mainly reducing waste). A monomer derived from chemical recycling is a monomer obtained by depolymerizing or pyrolyzing a polymer such as waste plastic back into a monomer unit such as ethylene, as well as a monomer produced using such a monomer as a raw material. Therefore, even if the raw material olefin is a propylene polymer containing a monomer derived from chemical recycling, the molecular structure is equivalent to a propylene polymer made of a monomer derived from a fossil fuel, provided that the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are equivalent. Therefore, the performance is said to be the same.

[0035] As the recycled material (A), recycled materials containing resins other than polypropylene-based resins and rubber components can be used within a range that does not impair the characteristics of the present invention, and it is preferable to use materials in which the polypropylene-based resin component is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and even more preferably 80% by mass or more.

[0036] Examples of rubber components other than polypropylene-based resin in the recycled material (A) include thermoplastic elastomers, rubber-like elastomers, etc. Examples of thermoplastic elastomers include olefin-based elastomers, styrene-based elastomers, polyester-based elastomers, polyamide-based elastomers, etc. For example, examples of polyolefin-based elastomers include amorphous or low-crystalline polyolefin-α-olefin copolymers, mixtures of polyolefin resins and olefin-based rubbers, mixtures of polyolefin resins and partially crosslinked products of olefin-based rubbers, mixtures of polyolefin resins and fully crosslinked products of olefin-based rubbers, etc. Examples of styrene-based elastomers include butadiene-styrene copolymers (including all of random copolymers, block copolymers, graft copolymers, etc.) and their hydrogenated products, styrene-butadiene-styrene copolymers, hydrogenated styrene-butadiene copolymers, etc. Examples of the polyester-based elastomers include elastomers made of polyester-polyether copolymers, polyester-polyester copolymers, and the like. Examples of the polyamide-based elastomers include thermoplastic elastomers made of polyamide-polyester copolymers, polyamide-polyether copolymers, and the like.

[0037] Examples of rubber-like elastomers include diene rubbers such as natural rubber, butadiene rubber, synthetic isoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, ethylene-propylene-diene terpolymer, chloroprene, halobutyl rubber, butyl rubber, nitrile-chloroprene rubber, nitrile-isoprene rubber, acrylate-butadiene rubber, vinylpyridine-butadiene rubber, vinylpyridine-styrene-butadiene rubber, styrene-chloroprene rubber, styrene-isoprene rubber, carboxylated styrene-butadiene rubber, carboxylated acrylonitrile-butadiene rubber, styrene-butadiene block copolymer, styrene-isoprene block copolymer, carboxylated styrene-butadiene block copolymer, and carboxylated styrene-isoprene block copolymer; chlorinated polyethylene, chlorosulfonated polyethylene, and ethylene Preferred are rubber components such as polyolefin rubbers, such as ethylene-vinyl acetate copolymers, ethylene-propylene rubbers, ethylene-propylene-diene terpolymers, ethylene-butene rubbers, and ethylene-butene-diene terpolymers; rubbers having a polymethylene main chain, such as polychlorotrifluorinated ethylene, acrylic rubbers, ethylene-acrylic rubbers, fluororubbers, and hydrogenated NBR; rubbers having oxygen atoms in the main chain, such as epichlorohydrin polymers, ethylene oxide-epichlorohydrin-allyl glycidyl ether copolymers, and propylene oxide-allyl glycidyl ether copolymers; silicone rubbers, such as polyphenylmethylsiloxane, polydimethylsiloxane, polymethylethylsiloxane, and polymethylbutylsiloxane; rubbers having nitrogen atoms and oxygen atoms in addition to carbon atoms in the main chain, such as nitroso rubbers, polyester urethanes, and polyether urethanes; and mixtures thereof. Also usable are those in which these rubbers have been epoxy-modified, silane-modified, or maleated.

[0038] As described above, the recycled material (A) is derived from bottle caps, and is particularly preferably derived from PET bottle caps for beverages. The PET bottle caps for beverages are manufactured by a general manufacturing method for PET bottle caps (compression molding or injection molding), and polypropylene or polyethylene is used.

[0039] The recycled material (A) derived from PET bottle caps for beverages can be made by crushing or pelletizing PET bottle caps collected after use using a known method. More specifically, the collected PET bottle caps are separated into polyethylene-based and polypropylene-based PET bottle caps using a spectroscopic method such as infrared spectroscopy (IR), and the separated polypropylene-based PET bottle caps are crushed and washed with water, and then melt-kneaded in an extruder to form pellets, thereby obtaining the recycled material (A). The method for separating the polyethylene-based and polypropylene-based PET bottle caps is not limited to the above-mentioned spectroscopy such as IR, and examples of the method include specific gravity sorting utilizing the difference in specific gravity between polyethylene and polypropylene.

[0040] [Recycled material (B)] The composition of the present invention contains recycled material (B) derived from products other than the bottle caps.

[0041] In the recycled material (B), the melt flow rate (MFR) measured according to JIS K 7210 at 230°C under a load of 2.16 kg is preferably in the range of 1.0 to 100.0 g / 10 min. The lower limit of the MFR is more preferably 2.0 g / 10 min, further preferably 4.0 g / 10 min, and particularly preferably 6.0 g / 10 min. On the other hand, the upper limit of the MFR is more preferably 50.0 g / 10 min, further preferably 30.0 g / 10 min, and particularly preferably 20.0 g / 10 min.

[0042] By making the MFR of the recycled material (B) within the above range and reducing the difference in MFR from the recycled material (A), the composition of the present invention has excellent mechanical properties.

[0043] The recycled material (B) is derived from a product other than the bottle cap. The product other than the bottle cap is not particularly limited, but may be propylene molded products collected from the market such as home appliances and automobiles, crushed products thereof, and molded parts (scrap materials) and molded balls and crushed products thereof generated in the propylene molding process.

[0044] The recycled material (B) may be a single type or a mixture of multiple polypropylene resin components with different fluidity, density, and propylene content, and is preferably a single type or a mixture of multiple resins with different fluidity, density, etc., in order to prevent the mechanical properties from being impaired. It is preferable to select and use one or a blend of two or more of these polypropylene resins that satisfy the above MFR.

[0045] As the recycled material (B), various known polypropylene-based resins can be used, and the same polypropylene-based resins as those exemplified in the above section [Recycled material (A)] can be used.

[0046] As the recycled material (B), a recycled material containing a resin other than polypropylene resin and a rubber component can be used within a range that does not impair the characteristics of the present invention, and it is preferable to use one in which the polypropylene resin component is preferably 50% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, and more preferably 80% by mass or more. As the rubber component, the same rubber components as those exemplified in the above [Recycled material (A)] column can be used.

[0047] The content ratio of the recycled materials (A) and (B) in the composition of the present invention is, when the total content of the recycled materials (A) and (B) is 100 mass%, The content of the recycled material (A) is preferably 5 to 50 mass%, more preferably 10 to 50 mass%, further preferably 20 to 50 mass%, particularly preferably 30 to 50 mass%, The content of the recycled material (B) is preferably 50 to 95 mass %, more preferably 50 to 90 mass %, further preferably 50 to 80 mass %, and particularly preferably 50 to 70 mass %.

[0048] By containing the recycled materials (A) and (B) in the above-mentioned ranges, the composition of the present invention has stable mechanical properties and can be used for specific applications, even when mixed with recycled material (B) recovered from a wide range of products, without being affected by the type of product from which it is derived.

[0049] [Other ingredients] The composition of the present invention may contain other additives, as necessary, such as a heat stabilizer, a weather stabilizer, a light stabilizer, an antiaging agent, an antioxidant, a fatty acid metal salt, a softener, a dispersant, a colorant, a pigment, an ultraviolet absorbing agent, etc., within the scope of not impairing the object of the present invention.

[0050] [Physical properties of polypropylene resin composition] In the composition of the present invention, the melt flow rate (MFR) measured according to JIS K 7210 at 230°C under a load of 2.16 kg is preferably in the range of 1.0 to 100.0 g / 10 min. The lower limit of the MFR is more preferably 2.0 g / 10 min, further preferably 4.0 g / 10 min, and particularly preferably 6.0 g / 10 min. On the other hand, the upper limit of the MFR is more preferably 50.0 g / 10 min, further preferably 30.0 g / 10 min, and particularly preferably 20.0 g / 10 min.

[0051] When the MFR of the composition of the present invention is within the above range, the composition of the present invention is excellent in mechanical properties, particularly in tensile modulus and impact resistance.

[0052] [Method of producing polypropylene resin composition] The composition of the present invention can be obtained by mixing the above-mentioned recycled materials (A) and (B) and, if necessary, other components with a dry blend, a Henschel mixer, a Banbury mixer, or the like, or by mixing and then melt-kneading with a single-screw extruder, a twin-screw extruder, a high-speed twin-screw extruder, or the like.

[0053] [Molded body] The composition of the present invention has excellent moldability and can be used in various molding methods. Specific examples of molded products include injection molded products, foam molded products, injection foam molded products, extrusion molded products, hollow molded products, vacuum / pressure molded products, calendar molded products, stretched films, and inflation films, and injection molded products are particularly preferred. The molding conditions for producing molded products are not particularly limited, and known conditions can be used. EXAMPLES

[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0055] [material] The recycled materials used in the examples and comparative examples are shown below. <Recycled material (A)> (A1) Polypropylene derived from PET bottle caps for beverages (MFR: 9g / 10min) (A2) Polypropylene derived from PET bottle caps for beverages (MFR: 11g / 10min)

[0056] <Recycled material (B)> (B1) Polypropylene derived from home appliances (MFR: 20g / 10min) (B2) Polypropylene derived from home appliances (MFR: 4g / 10min)

[0057] [Measurement and evaluation methods] The physical properties of each recycled material and polypropylene resin composition used in the examples and comparative examples were measured and evaluated by the following methods.

[0058] (1) Melt flow rate (MFR) (g / 10 min) The melt flow rate (MFR) was measured in accordance with JIS K 7210 under conditions of 230° C. and a load of 2.16 kg (kgf).

[0059] (2) Tensile yield stress Multipurpose test pieces type A1 were prepared by injection molding based on JIS K 7152-1 using the pellets obtained in the examples and comparative examples, and measurements were performed according to the method of JIS K 7161.

[0060] (3) Nominal tensile strain at break Multipurpose test pieces type A1 were prepared by injection molding based on JIS K 7152-1 using the pellets obtained in the examples and comparative examples, and measurements were performed according to the method of JIS K 7161.

[0061] (4) Tensile modulus Multipurpose test pieces type A1 were prepared by injection molding based on JIS K 7152-1 using the pellets obtained in the examples and comparative examples, and measurements were performed according to the method of JIS K 7171.

[0062] (5) Charpy impact test The Charpy impact strength was measured in accordance with JIS K 7111-1 under conditions of 23°C and -20°C by preparing multipurpose test pieces type A1 by injection molding based on JIS K 7152-1 using the pellets obtained in the examples and comparative examples. The measurement was performed on notched test pieces.

[0063] (6) Deflection temperature under load The deflection temperature under load was measured by preparing a multipurpose test piece type A1 by injection molding based on JIS K 7152-1 using the pellets obtained in the examples and comparative examples, and following the method of JIS K 7191. That is, both ends of the test piece were supported in a heating bath, and a predetermined bending stress (a constant load of 0.45 MPa) was applied to the test piece by a central load rod below, while the temperature of the heating medium was increased at a rate of 2°C / min, and the temperature of the heating medium when the deflection of the test piece reached a predetermined amount was taken as the deflection temperature under load.

[0064] (7) Rockwell hardness The Rockwell hardness (R scale) was measured by preparing multipurpose test pieces type A1 by injection molding based on JIS K 7152-1 using the pellets obtained in the examples and comparative examples, and following the method of JIS K 7202 under the following conditions. <Measurement conditions> Test piece: 30mm (width) x 30mm (length) x 2mm (thickness) The test pieces were stacked in pairs for measurement.

[0065] (8) High-speed surface impact test Using an electric injection molding machine (Roboshot S-2000i-100B manufactured by FANUC) with a clamping force of 100 tons, under the conditions of a cylinder temperature of 200°C, a mold temperature of 40°C, a primary injection pressure of 100MPa, an injection speed of 37mm / sec, a dwell pressure of 35MPa, and a dwell time of 7.0 seconds, a sheet-shaped test piece with a long side of 130mm, a short side of 120mm, and a thickness of 2mm was produced using the pellets obtained in the examples and comparative examples. A striking core with a load cell having a tip diameter of 1 / 2 inch was collided with the test piece at a speed of 3m / sec in an atmosphere of 0°C. A stand with a tip diameter (receiving diameter) of 3 inches was used as a receiving stand on the back side of the test piece. The values ​​obtained were the total absorbed energy and the ductile energy from yield to destruction.

[0066] [Examples 1 to 3] The recycled materials (A1) and (B1) were dry-blended in the ratios shown in Table 1 using a tumbler mixer manufactured by Platec Co., Ltd., and then melt-kneaded under the following conditions using a twin-screw extruder (TEM35BS) manufactured by Toshiba Machine Co., Ltd. to obtain strands. Model: TEM35BS (35mm twin screw extruder) Screw speed: 300 rpm Screen mesh: #200 ·Resin temperature: 220℃ The resulting strand was cooled with water and then cut with a pelletizer to obtain pellets. The melt flow rate (MFR) of the obtained pellets was measured, and the results are shown in Table 1. In addition, the obtained pellets were used to measure various mechanical properties according to the methods described in the above column of [Measurement and evaluation methods], and the results are shown in Table 1.

[0067] [Examples 4 and 5] Pellets were obtained in the same manner as in Examples 1 to 3, except that the recycled materials (A2) and (B2) were used in the blending ratio shown in Table 1. The MFR and various mechanical properties were measured using the obtained pellets. The results are shown in Table 1.

[0068] [Comparative Examples 1 to 4] Each recycled material shown in Table 1 was used to obtain pellets by the method described in [Examples 1 to 3]. The obtained pellets were used to measure MFR and each mechanical property. The results are shown in Table 1.

[0069] [Table 1]

[0070] In Table 1 above, the content of the crystal nucleating agent is shown based on 100 parts by mass of recycled material.

Claims

1. A polypropylene-based resin composition comprising a recycled material (A) derived from a bottle cap and a recycled material (B) derived from a product other than the bottle cap.

2. 2. The polypropylene resin composition according to claim 1, wherein the content of the recycled material (A) is 5 to 50 mass%, and the content of the recycled material (B) is 50 to 95 mass%, when the total content of the recycled material (A) and the recycled material (B) is 100 mass%.

3. The polypropylene resin composition according to claim 1, wherein the recycled material (A) contains 0.01 to 0.5 parts by mass of a crystal nucleating agent per 100 parts by mass of the recycled material (A).

4. The polypropylene resin composition according to claim 1, wherein the recycled material (A) has a melt flow rate (MFR) measured in accordance with JIS K 7210 at 230° C. under a load of 2.16 kg in the range of 1 to 100 g / 10 min.

5. The polypropylene resin composition according to claim 1, wherein the recycled material (B) has a melt flow rate (MFR) measured in accordance with JIS K 7210 at 230° C. under a load of 2.16 kg in the range of 1 to 100 g / 10 min.

6. The polypropylene resin composition according to claim 1, wherein the recycled material (A) is derived from a plastic bottle cap for beverages.

Citation Information

Patent Citations

  • Method for producing recycled polypropylenic resin granular material, recycled polypropylenic resin, granular material and molded product thereof

    JP2007277366A

  • Plastic molded article utilizing plastic waste material and lid material for plastic container

    JP2022114370A