Polyolefin resin composition and molding
A biomass-derived polyolefin resin composition with ultra-high molecular weight polyethylene and a compatible polyolefin ensures reduced environmental impact and maintains mechanical properties, addressing moldability issues in existing compositions.
Patent Information
- Application Number
- JP2023043147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polyolefin resin compositions containing ultra-high molecular weight polyethylene lack moldability while maintaining excellent properties such as hardness, abrasion resistance, and impact resistance, and there is a need to reduce the environmental burden by using biomass-derived materials.
A polyolefin resin composition comprising ultra-high molecular weight polyethylene and a different polyolefin, both derived from biomass sources, with specific intrinsic viscosity ranges and ratios, ensuring excellent moldability and retention of properties.
The composition achieves reduced environmental impact by using biomass-derived materials and maintains excellent mechanical properties with improved moldability.
Smart Images

Figure 2024132403000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyolefin resin composition and a molded article containing the composition. [Background technology]
[0002] Compared with general-purpose resins such as ordinary polyethylene, ultra-high molecular weight polyethylene has weaker intermolecular cohesion, a symmetrical molecular structure, and a high degree of crystallinity, and therefore has excellent sliding properties, as well as excellent impact resistance, abrasion resistance, tensile strength, etc. Therefore, polyolefin resin compositions containing ultra-high molecular weight polyethylene have been studied for various applications, including sliding materials.
[0003] In recent years, there has been a demand to reduce emissions of carbon dioxide, one of the greenhouse gases, in order to reduce the environmental impact throughout the life cycle of resin materials, from their manufacture to their use and disposal. The fossil fuels that have traditionally been used as raw materials for resin materials are carbon sources that exist outside the Earth's environment and are fixed deep underground. When these are used as raw materials to produce resin products, carbon that was not present in the Earth's environment is released into the atmosphere as carbon dioxide during the process of its life cycle (for example, when it is burned during disposal), and this is considered to be one of the causes of the increase in carbon dioxide in the Earth's environment. On the other hand, resin products made from biomass (living organisms such as plants and animals) that grow by absorbing carbon sources (such as carbon dioxide) that circulate in the global environment and converting them into organic matter, even if they are burned and carbon dioxide is generated, unlike fossil fuels, they only circulate the carbon present in the global environment, so there is no change in the total amount of carbon in the global environment. For this reason, such biomass-derived resin materials are attracting attention as carbon-neutral materials.
[0004] For example, Patent Documents 1 and 2 describe the production of biomass-derived propylene and the production of a biomass-derived propylene-based polymer from a raw material containing the biomass-derived propylene. Patent Document 3 describes a polyethylene resin composition of a plant-derived linear low-density polyethylene and a non-plant-derived low-density polyethylene. Patent Document 4 describes a thermoplastic elastomer composition obtained by using a biomass-derived copolymer as at least a part of the raw material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2007 / 055361 [Patent Document 2] Patent No. 7004864 [Patent Document 3] Patent No. 5845936 [Patent Document 4] Patent No. 6621364 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the above patent documents do not disclose or suggest a biomass-derived polyolefin resin composition containing ultra-high molecular weight polyethylene. Moreover, a polyolefin resin composition containing ultra-high molecular weight polyethylene is required to have good moldability while maintaining the above-mentioned excellent properties. An object of the present invention is to provide a polyolefin resin composition containing ultra-high molecular weight polyethylene, which can reduce the environmental load on the global environment (mainly reducing greenhouse gases such as carbon dioxide) and has excellent moldability while retaining the excellent properties derived from ultra-high molecular weight polyethylene. [Means for solving the problem]
[0007] As a result of the inventor's research, it has been found that the above-mentioned problems can be solved by the following configuration example. In this specification, the numerical range "A to B" indicates A or more and B or less.
[0008] That is, the present invention includes, for example, the following items [1] to [8].
[0009] [1] Ultra-high molecular weight polyethylene (A) satisfying the following requirement (a-1); Contains a polyolefin (B) that satisfies the following requirement (b-1), A biomass-derived polyolefin resin composition that satisfies the following requirement (I): (I) The MFR measured in accordance with ASTM D1238E under a load of 10 kg at a temperature of 190° C. is 0.01 to 500 g / 10 min. (a-1) The intrinsic viscosity [η] measured in decalin solvent at 135°C is 8 to 50 dl / g; (b-1) The intrinsic viscosity [η] measured in decalin solvent at 135°C is 0.1 to 5 dl / g.
[0010] [2] The content of the ultra-high molecular weight polyethylene (A) is 5 to 40 parts by mass, The content of the polyolefin (B) is 60 to 95 parts by mass (wherein the total amount of the polyethylene (A) and the polyolefin (B) is 100 parts by mass). The polyolefin resin composition according to [1]. [3] The polyolefin resin composition according to [1] or [2], wherein at least one of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contains a structural unit derived from a biomass-derived monomer. [4] The polyolefin resin composition according to any one of [1] to [3], which has a biomass degree in accordance with ASTM D 6866 of 1% or more. [5] The polyolefin resin composition according to any one of [1] to [4], wherein at least one of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contains a structural unit derived from a biomass-derived monomer and a structural unit derived from a non-biomass-derived monomer. [6] The polyolefin resin composition according to any one of [1] to [5], wherein the polyolefin (B) is polyethylene.
[0011] [7] A molded article comprising the polyolefin resin composition according to any one of [1] to [6]. [8] The molded article according to [7], which is an injection molded article. Effect of the Invention
[0012] According to the present invention, there is provided a polyolefin resin composition containing ultra-high molecular weight polyethylene which can reduce the environmental load on the global environment (the increase in greenhouse gases such as carbon dioxide) and has excellent moldability and other properties while retaining the excellent properties of ultra-high molecular weight polyethylene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Polyolefin resin composition> The polyolefin resin composition of the present invention is a biomass-derived polyolefin resin composition comprising a specific ultra-high molecular weight polyethylene (A) and a polyolefin (B) different from the ultra-high molecular weight polyethylene (A) (typically a low-molecular weight to high-molecular weight polyethylene polyolefin different from the ultra-high molecular weight polyethylene (A)) (hereinafter also referred to as "polyolefin (B)"). Here, the biomass-derived polyolefin resin composition is a resin composition that contains polyolefin and also contains a biomass-derived polymer. The biomass-derived polymer is a polymer that contains a structural unit derived from at least one biomass-derived monomer. For example, the biomass polyolefin is a polymer that contains a structural unit derived from at least one biomass-derived olefin (olefin such as ethylene or α-olefin). Biomass-derived monomers are monomers derived from any renewable natural raw materials and their residues, including fungi, yeasts, algae, and bacteria, of plant or animal origin, and contain carbon as a component. 14 C isotope 1×10 -12 It is a monomer having a biomass carbon concentration (unit: pMC) of about 100 pMC measured in accordance with ASTM D6866. The biomass-derived monomer (monomer such as ethylene or α-olefin) can be obtained, for example, by a conventionally known method. The polyolefin resin composition according to the present invention contains a biomass-derived polymer, and therefore it is possible to reduce the environmental load (mainly by reducing greenhouse gas emissions). In addition, if the polymer production conditions such as the polymerization catalyst, polymerization process, and polymerization temperature are equivalent, and the composition of the raw material monomers is the same, a (co)polymer containing a biomass-derived monomer as the raw material monomer is: 14 C isotope 1×10 -12 ~1×10 -14 Except for the fact that they contain a certain proportion of fossil fuel-derived monomers, their molecular structure is considered to be equivalent to that of (co)polymers whose raw material monomers contain only fossil fuel-derived monomers, and the performance of these polymers is considered to be unchanged. The raw material monomer of the biomass-derived polymer may contain only biomass-derived monomers, or may be a mixture of biomass-derived monomers and fossil fuel-derived monomers. Also, the same type of monomer as the biomass-derived monomer contained in the raw material of the biomass-derived polymer may be composed of only biomass-derived monomers, or may be composed of a mixture of biomass-derived monomers and fossil fuel-derived monomers. In the polyolefin resin composition of the present invention, it is desirable to contain a biomass-derived polyolefin, and it is more desirable that at least one of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contains a structural unit derived from a biomass-derived monomer, and it is desirable that both the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contain a structural unit derived from a biomass-derived monomer. In another embodiment, it is desirable that at least one of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contains a structural unit derived from a biomass-derived monomer and a structural unit derived from a fossil fuel-derived monomer, and it is a more desirable embodiment that both the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contain a structural unit derived from a biomass-derived monomer and a structural unit derived from a fossil fuel-derived monomer. The biomass-derived monomer that can be contained in the ultra-high molecular weight polyethylene (A) and polyolefin (B) is preferably a biomass-derived olefin, more preferably a biomass-derived ethylene. The fossil fuel-derived monomer that can be contained in the ultra-high molecular weight polyethylene (A) and polyolefin (B) is preferably a fossil fuel-derived olefin, more preferably a fossil fuel-derived ethylene.
[0014] <Ultra-high molecular weight polyethylene (A)> The ultra-high molecular weight polyethylene (A) satisfies the following requirement (a-1).
[0015] [Requirement (a-1)] The ultra-high molecular weight polyethylene (A) has an intrinsic viscosity [η] measured in decalin solvent at 135° C. of 8 to 50 dl / g, preferably 8 to 45 dl / g, more preferably 10 to 45 dl / g, and further preferably 15 to 45 dl / g.
[0016] When the ultra-high molecular weight polyethylene (A) has an intrinsic viscosity [η] of 8 dl / g or more measured in decalin solvent at 135°C, the polyolefin resin composition of the present invention is provided with excellent properties derived from ultra-high molecular weight polyethylene. When the ultra-high molecular weight polyethylene (A) has an intrinsic viscosity [η] of 50 dl / g or less measured in decalin solvent at 135°C, the moldability of the polyolefin resin composition of the present invention is not impaired. That is, when the intrinsic viscosity [η] of the ultra-high molecular weight polyethylene (A) is in the above range, the polyolefin resin composition of the present invention is provided with excellent properties derived from ultra-high molecular weight polyethylene and tends to have excellent moldability.
[0017] The ultra-high molecular weight polyethylene (A) is a homopolymer of ethylene or a copolymer of ethylene and an α-olefin such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, or 3-methyl-1-pentene. The ultra-high molecular weight polyethylene (A) is preferably a homopolymer of ethylene or a copolymer of ethylene and the above-mentioned α-olefin, a copolymer composed mainly of ethylene, and more preferably a homopolymer of ethylene. Here, the term "main component" refers to the component having the highest content (mol%) among the structural units contained in the polymer.
[0018] <Polyolefin (B)> The polyolefin (B) is a polymer different from the ultra-high molecular weight polyethylene (A) and is typically a low-molecular-weight to high-molecular-weight polyolefin. The polyolefin (B) satisfies the following requirement (b-1).
[0019] [Requirement (b-1)] The polyolefin (B) has an intrinsic viscosity [η] measured in decalin solvent at 135° C. of 0.1 to 5 dl / g, preferably 0.5 to 2 dl / g, more preferably 0.7 to 1.5 dl / g, and even more preferably 0.8 to 1.3 dl / g.
[0020] When the intrinsic viscosity [η] of polyolefin (B) measured in decalin solvent at 135 ° C. is 0.1 dl / g or more, the excellent properties derived from ultra-high molecular weight polyethylene are sufficiently imparted to the polyolefin resin composition of the present invention. In addition, when the intrinsic viscosity [η] of polyolefin (B) measured in decalin solvent at 135 ° C. is 5 dl / g or less, the moldability of the polyolefin resin composition of the present invention is good. That is, when the intrinsic viscosity [η] of polyolefin (B) measured in decalin solvent at 135 ° C. is in the above range, the polyolefin resin composition of the present invention is imparted with excellent properties derived from ultra-high molecular weight polyethylene and tends to have excellent moldability.
[0021] The polyolefin (B) preferably has a density of 950 to 985 kg / m 3 and more preferably 960 to 980 kg / m 3 and more preferably 960 to 975 kg / m 3 and more preferably 965 to 975 kg / m 3 By incorporating such a polyolefin (B) in the polyolefin resin composition of the present invention, the excellent properties derived from the ultra-high molecular weight polyethylene are not impaired, and the moldability also tends to be excellent.
[0022] Examples of the polyolefin (B) include polyethylene, polypropylene, and poly-4-methyl-1-pentene. From the viewpoint of imparting excellent properties to the ultra-high molecular weight polyethylene (A), polyethylene (B1) is preferred. The polyethylene (B1) is a homopolymer of ethylene or a copolymer of ethylene and an α-olefin, preferably a homopolymer of ethylene. The α-olefin constituting the copolymer includes linear or branched α-olefins having 3 to 20 carbon atoms, specifically propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 3,4-dimethyl-1-pentene, 4-methyl-1-hexene, 3-ethyl-1-pentene, 3-ethyl-4-methyl-1-pentene, 3,4-dimethyl-1-hexene, 4-methyl-1-heptene, 3,4-dimethyl-1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, or 1-eicosene. Among these, propylene and 1-butene are preferably used in view of the relationship with the density range of polyethylene (B1).
[0023] In addition, the copolymer of ethylene and α-olefin preferably contains 90 mol% or more of structural units derived from ethylene, and more preferably contains 95 mol% or more of structural units derived from ethylene. In addition, the copolymer of ethylene and α-olefin preferably contains 10 mol% or less of structural units derived from α-olefin, and more preferably contains 5 mol% or less of structural units derived from α-olefin. When the polyethylene (B1) is a copolymer of ethylene and α-olefin, the greater the amount of structural units derived from ethylene, the more preferable.
[0024] <Other ingredients> The polyolefin resin composition according to the present invention may contain thermoplastic resins such as other polyolefin-based resins, and resin additives (for example, stabilizers such as heat stabilizers and weather stabilizers, crosslinking agents, crosslinking assistants, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, fillers, mineral oil-based softeners, petroleum resins, waxes, etc.) within the scope of the present invention. When the other components are contained, the total amount of the other components in the polyolefin resin composition of the present invention is usually 5 mass% or less, preferably 2 mass% or less, and more preferably 1 mass% or less. In other words, the ratio of the total mass of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) in the polyolefin resin composition of the present invention to the mass of the polyolefin resin composition is usually 95 mass% or more, preferably 98 mass% or more, and more preferably 99 mass% or more.
[0025] <Polyolefin resin composition> The polyolefin resin composition according to the present invention preferably satisfies the following requirement (I). [Requirement (I)] The polyolefin resin composition of the present invention has a melt flow rate (hereinafter also referred to as "MFR") of 0.01 to 500 g / 10 min, preferably 0.1 to 100 g / 10 min, and more preferably 1.0 to 50 g / 10 min, measured at 190°C under a load of 10 kg according to the measurement method of ASTM D1238E. When the MFR of the polyolefin resin composition of the present invention is within the above range, the composition has good moldability while maintaining the excellent properties derived from the ultra-high molecular weight polyethylene.
[0026] The content of the ultra-high molecular weight polyethylene (A) in the polyolefin resin composition of the present invention is preferably 5 to 40 parts by mass, more preferably 5 to 35 parts by mass, even more preferably 8 to 30 parts by mass, and particularly preferably 8 to 25 parts by mass (wherein the total amount of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) is 100 parts by mass). The content of polyolefin (B) in the polyolefin resin composition of the present invention is preferably 60 to 95 parts by mass, more preferably 65 to 95 parts by mass, even more preferably 70 to 92 parts by mass, and particularly preferably 75 to 92 parts by mass (wherein the total amount of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) is 100 parts by mass).
[0027] When the contents of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) in the polyolefin resin composition of the present invention are within the above ranges, the excellent properties derived from the ultra-high molecular weight polyethylene can be more easily maintained, and the moldability can be more improved.
[0028] The biomass degree of the polyolefin resin composition of the present invention is preferably 1% or more, more preferably 5% or more, and further preferably 20% or more, and the upper limit may be 100%. When the biomass degree of the polyolefin resin composition of the present invention is within the above range, the environmental load is further reduced, while the excellent properties derived from the ultra-high molecular weight polyethylene are maintained and excellent moldability tends to be achieved.
[0029] The above "biomass content" (carbon concentration derived from biomass) is based on the radiocarbon ( 14 C) Obtained by the measurement method 14 The carbon content of atmospheric carbon dioxide is 14 Since plants grow by absorbing carbon dioxide from the atmosphere, the carbon dioxide present in the atmosphere during growth is 14 in the same proportion as C 14 The plant biomass-derived components contain 1,000 to 1,000 carbon atoms, and this ratio is maintained even after the plant is immobilized. 14 in the same proportion as C 14 C. On the other hand, fossil fuels contain 14 It is also known that it contains very little C. Therefore, the carbon atoms contained in the resin composition are 14 By measuring the proportion of C, the proportion of carbon derived from biomass can be calculated, and it can be confirmed whether the resin composition contains a biomass-derived component or a non-biomass-derived component.
[0030] <Method of producing polyolefin resin composition> The method for producing the polyolefin resin composition according to the present invention is not particularly limited as long as it is a production method that can contain the ultra-high molecular weight polyethylene (A) and the polyolefin (B) in a predetermined ratio. Preferred methods include the following methods (M-1) to (M-3).
[0031] Method (M-1): A method in which the ultra-high molecular weight polyethylene (A) and the polyolefin (B) are each produced in advance in the presence of an olefin polymerization catalyst, and then these ultra-high molecular weight polyethylene (A) and polyolefin (B) are blended so as to satisfy the conditions that the polyolefin resin composition of the present invention should satisfy, such as the above-mentioned (x-1) and (x-2). Method (M-2): A method for producing a polyolefin by a multi-stage polymerization method including at least two steps, namely, a first step of producing ultra-high molecular weight polyethylene (A) in the presence of an olefin polymerization catalyst, and a second step of producing polyolefin (B). The second step is carried out in the presence of the ultra-high molecular weight polyethylene (A) produced in the first step. The polymerization conditions in the first and second steps are selected so as to satisfy the conditions that the ultra-high molecular weight polyethylene (A), polyolefin (B) and the polyolefin resin composition of the present invention should satisfy, or are desired to satisfy. Method (M-3): A method for producing a polyolefin by a multi-stage polymerization method including at least two steps, namely, a first step of producing a polyolefin (B) in the presence of an olefin polymerization catalyst, and a second step of producing an ultra-high molecular weight polyethylene (A). The second step is carried out in the presence of the polyolefin (B) produced in the first step. The polymerization conditions in the first and second steps are selected so as to satisfy the conditions that the ultra-high molecular weight polyethylene (A), polyolefin (B) and the polyolefin resin composition of the present invention should satisfy, or are desired to satisfy. Furthermore, when the ultra-high molecular weight polyethylene (A) and polyolefin (B) are ultra-high molecular weight polyethylene (A) and polyethylene (B1), they can be produced by polymerizing monomers containing ethylene in the presence of a known olefin polymerization catalyst described, for example, in WO2008 / 013144 and WO2010 / 074073 under polymerization conditions (temperature of 70°C to 85°C, polymerization time of 45 minutes to 300 minutes) such that the polyolefin resin composition of the present invention has desired physical properties.
[0032] Among the methods (M-1) to (M-3), the methods (M-2) and (M-3) using a multi-stage polymerization method are more preferred, and the method (M-2) in which the ultra-high molecular weight polyethylene (A) is produced in the first step is even more preferred. When the multi-stage polymerization method is used, when the polyolefin (B) is polyethylene (B1), the ultra-high molecular weight polyethylene (A) and the polyethylene (B1) contained in the polyolefin resin composition of the present invention are compatible with each other and the dispersibility is improved, so that it is easy to achieve both abrasion resistance and moldability, which is preferable. In addition, when the polyolefin (B) is polyethylene (B1), the polyolefin resin composition of the present invention is produced by the method (M-2), and by carrying out the addition of a chain transfer agent that causes a chain transfer reaction, the increase in the polymerization temperature, etc. in the second step, the molecular weight of the polyethylene (polyethylene (B1)) obtained in the second step can be easily adjusted to be lower than the molecular weight of the polyethylene (ultra-high molecular weight polyethylene (A)) obtained in the first step, which is preferable in terms of excellent production efficiency.
[0033] In this case, the olefin such as ethylene used in the polymerization contains a constituent unit derived from the desired biomass-derived monomer, and as long as the desired biomass degree can be achieved, various olefins described in the sections on ultra-high molecular weight polyethylene (A) and polyolefin (B) can be used without limitation.
[0034] <Molded body> The polyolefin resin composition according to the present invention can be molded into a container, tray, sheet, rod, film, or a coating for various molded articles by a conventionally known method, specifically, for example, an injection molding method, a profile extrusion molding method, a pipe molding method, a tube molding method, a coating molding method for heterogeneous molded articles, an injection blow molding method, a direct blow molding method, a T-die sheet or film molding method, an inflation film molding method, a press molding method, or the like.
[0035] The molded article obtained by the above molding method can be widely used for conventionally known polyethylene applications, but since it has particularly excellent abrasion resistance, it can be used for applications requiring this, such as metal coatings for steel pipes, electric wires, automobile slide rails, etc., pressure-resistant rubber hoses, automobile door gaskets, clean room door gaskets, automobile glass run channels, various rubber reels such as automobile weather strips, various guide rails, elevator rail guides, various protective liner materials, and the like. EXAMPLES
[0036] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0037] [Intrinsic viscosity [η]] The intrinsic viscosity [η] of each of the various polymers and polyolefin resin compositions obtained in the examples was measured at 135° C. in decalin solvent.
[0038] [Melt flow rate (MFR)] The MFR of the polyolefin resin compositions obtained in the examples was measured under a load of 10 kg in accordance with ASTM D1238E at a temperature of 190°C.
[0039] [Preparation of test pieces (molded bodies)] The polyolefin resin compositions obtained in the examples were injection molded using an injection molding machine (J110-AD, manufactured by The Japan Steel Works, Ltd.) to produce dumbbell-shaped test pieces and test pieces measuring 30 cm in length, 30 cm in width, and 3 mm in thickness.
[0040] [Evaluation of tensile modulus (tensile test)] The tensile modulus of elasticity was measured using a dumbbell-shaped test piece in accordance with JIS K 7161-2 using a tensile tester (AG-100kNX, manufactured by Shimadzu Corporation). The test conditions were speed: 1 mm / min, chuck distance: 115 mm, gauge distance: 50 mm, and measurement environment temperature: 23°C.
[0041] [Evaluation of tensile breaking strength and tensile breaking elongation (tensile test)] The tensile strength and elongation at break of dumbbell-shaped test pieces were measured in accordance with JIS K 7161-2 using a tensile testing machine (AG-100kNX, Shimadzu Corporation). The test conditions were speed: 50 mm / min, chuck distance: 115 mm, gauge length: 50 mm, and measurement environment temperature: 23°C.
[0042] [Evaluation of flexural modulus and flexural strength (bending test)] Using dumbbell-shaped test pieces, the flexural modulus and flexural strength were measured using a bending tester (AG-1kNX, Shimadzu Corporation) in accordance with ISO-178. The test conditions were speed: 2 mm / min, span distance: 64 mm, and measurement environment temperature: 23°C.
[0043] [Evaluation of dynamic friction coefficient and specific wear rate (ring wear test)] Using a test piece measuring 30cm long x 30cm wide x 3mm thick, the dynamic friction coefficient and specific wear rate were measured using a Suzuki-type friction and wear tester in accordance with JIS K 7218 "Sliding wear test method for plastics." The test conditions were as follows: mating material: S45C, speed: 30m / min, sliding distance: 3km, load: 25kg, and measurement environment temperature: 23℃.
[0044] The ethylene used in the following Examples 1 to 4 was produced by a known method using naphtha as a raw material, which was a mixture of biomass naphtha (manufactured by Neste) and naphtha derived from petroleum.
[0045] [Example 1] [Preparation of solid titanium catalyst component [C1]] 95.2 g of anhydrous magnesium chloride, 398.1 g of decane, and 306 g of 2-ethylhexyl alcohol were charged into a reaction vessel and heated at 140° C. for 6 hours. The solution in the reaction vessel was cooled to 50° C., and then 17.6 g of ethyl benzoate was added. The mixture was stirred and mixed at 130° C. for 1 hour to obtain a homogeneous solution. After cooling the homogeneous solution thus obtained to room temperature, the entire amount of the homogeneous solution (50 ml) was dropped into 200 ml of titanium tetrachloride held at 0 ° C. over 60 minutes while stirring to obtain a mixed solution. After the dropwise addition, the resulting mixed solution was held at 0 ° C. for 1 hour, and then the temperature of the mixed solution was raised to 20 ° C. over 1 hour, and then further raised to 80 ° C. over 30 minutes. When the temperature of the mixed solution reached 78 ° C., 2.35 g of ethyl benzoate was added to the mixed solution, and the reaction was carried out for 2 hours while maintaining the temperature at 80 ° C. After the reaction for 2 hours was completed, the solid portion was collected by hot filtration, and the solid portion was resuspended in 200 ml of titanium tetrachloride, and then heated again at 90 ° C. for 2 hours. After the second heating reaction was completed, the solid portion was collected again by hot filtration, washed with decane at 90 ° C. until no free titanium compounds were detected in the washings, and then thoroughly washed with hexane at room temperature. The solid titanium catalyst component prepared by the above procedure was stored as a decane slurry, and a portion of it was dried in order to examine the catalyst composition. The composition of the solid titanium catalyst component [C1] after drying was 3.1 mass% titanium, 18 mass% magnesium, 60 mass% chlorine, 15.4 mass% ethyl benzoate, and 1.5 mass% 2-ethylhexyl alcohol residue.
[0046] [Production of polyolefin resin composition] 500 ml of purified decane was charged at room temperature into a 1-liter polymerization vessel that had been thoroughly purged with nitrogen, and 0.5 mmol of triisobutylaluminum and a solid titanium catalyst component [C1] (0.01 mmol in terms of titanium atom) were added at a temperature of 48° C. Ethylene was then fed until the pressure inside the polymerization vessel reached 0.6 MPaG in gauge pressure, and the first stage of ethylene polymerization was carried out at a temperature of 53° C. When 21 liters of ethylene had been fed, the ethylene feed was stopped, and the temperature was rapidly cooled to 45° C., after which the pressure was released and the vessel was purged with nitrogen. By carrying out the first-stage ethylene polymerization under the above conditions, ultra-high molecular weight polyethylene (A-1) is obtained as the first-stage polyethylene. Next, hydrogen was fed into the polymerization vessel until the pressure in the polymerization vessel reached 0.40 MPaG in gauge pressure, and ethylene was further fed until the pressure in the polymerization vessel reached 0.60 MPaG in gauge pressure, and a second stage of ethylene polymerization was carried out at a temperature of 85° C. When 119 liters of ethylene had been fed, the ethylene feed was stopped, and the temperature was rapidly cooled to 40° C., after which depressurization and purging were carried out. By carrying out the second-stage ethylene polymerization under the above conditions, polyethylene (B1-1) (ultra-high molecular weight to low molecular weight polyethylene (B1-1)) corresponding to the polyolefin (B) as the second-stage polyethylene is obtained. The slurry containing the solid produced above was filtered and dried overnight under reduced pressure at a temperature of 80° C. The obtained polyolefin resin composition (1) weighed 177 g.
[0047] [Analysis of each component in polyolefin resin composition] · Content and intrinsic viscosity [η] of ultra-high molecular weight polyethylene (A-1) When only the first stage polymerization carried out when producing the polyolefin resin composition (1) was carried out separately under the same conditions as when producing the polyolefin resin composition (1), the yield of the obtained ethylene polymer was 26.6 g. Since the ultra-high molecular weight polyethylene (A-1) was produced by this polymerization, the content of the ultra-high molecular weight polyethylene (A-1) in the polyolefin resin composition (yield 177 g) was calculated to be 15.0 mass %. Furthermore, the intrinsic viscosity [η] of the ultra-high molecular weight polyethylene (A-1) contained in the polyolefin resin composition (1) was measured and found to be 30.0 dl / g.
[0048] Polyethylene (B1-1) content and intrinsic viscosity [η] The first stage polymerization of the polymerization carried out in producing the polyolefin resin composition (1) was omitted, and only the second stage polymerization was carried out separately under the same conditions as in producing the polyolefin resin composition (1), to produce polyethylene (B1-1'). The intrinsic viscosity [η] of the polyethylene (B1-1') was 1.0 dl / g. Next, the molecular weight distribution of the polyethylene (B1-1') was measured by gel permeation chromatography (GPC) and compared with the molecular weight distribution measurement result of the polyolefin resin composition (1) by GPC. The peak position and shape of the chromatogram were consistent with the low molecular weight component (polyethylene (B1-1)) contained in the polyolefin resin composition (1). Based on this result, the physical properties of the polyethylene (B1-1) were considered to be the same as those of the polyethylene (B1-1'). In other words, the intrinsic viscosity [η] of the polyethylene (B1-1) was set to 1.0 dl / g.
[0049] [Granulation of polyolefin resin composition] The obtained polyolefin resin composition (1) was dry-blended with Irganox 1010 (manufactured by BASF), Irgafos 168 (manufactured by BASF), and calcium stearate (manufactured by NOF Corp.). The blending amount of each substance was 0.1% by mass for Irganox 1010, 0.2% by mass for Irgafos 168, and 0.12% by mass for calcium stearate, assuming the composition after dry blending to be 100% by mass. The composition after dry blending was melt-kneaded using a twin-screw extruder (manufactured by Technovel, φ=15 mm, L / D=30, cylinder temperature: 200° C.), and then granulated into pellets. The obtained pellets were used to measure the various physical properties of the polyolefin resin composition (1). The results are shown in Table 1.
[0050] [Example 2] The polymerization was carried out in the same manner as in Example 1, except that the amount of ethylene fed in the first polymerization step was changed from 21 liters to 25.2 liters, and the amount of ethylene fed in the second polymerization step was changed from 119 liters to 114.8 liters, to obtain a polyolefin resin composition (2) containing ultra-high molecular weight polyethylene (A-2) and polyethylene (B1-2). The composition was then analyzed and granulated, and each physical property was measured. The results are shown in Table 1.
[0051] [Example 3] The polymerization was carried out in the same manner as in Example 1, except that the amount of ethylene fed in the first polymerization step was changed from 21 liters to 30.8 liters, and the amount of ethylene fed in the second polymerization step was changed from 109.2 liters to 106.4 liters, to obtain a polyolefin resin composition (3) containing ultra-high molecular weight polyethylene (A-3) and polyethylene (B1-3). The composition was then analyzed and granulated, and each physical property was measured. The results are shown in Table 1.
[0052] [Example 4] Polymerization was carried out in the same manner as in Example 1, except that the amount of ethylene fed in the first polymerization step was changed from 21 liters to 33.6 liters, and the amount of ethylene fed in the second polymerization step was changed from 119 liters to 106.4 liters, to obtain a polyolefin resin composition (4) containing ultra-high molecular weight polyethylene (A-4) and polyethylene (B1-4). The composition was then analyzed and granulated, and each physical property was measured. The results are shown in Table 1.
[0053] [Example 5] [Granulation of polyolefin resin composition] A polyolefin resin composition (R) was obtained in the same manner as in Example 3, except that ethylene derived only from petroleum-derived naphtha was used instead of ethylene derived from naphtha containing biomass naphtha. 97.5% by mass of the polyolefin resin composition (R) and 2.5% by mass of polyethylene NOVON BN2 (manufactured by NOVON JAPAN, biomass content 95%) made from biomass-derived components (components containing biomass-derived monomers) were dry-blended, melt-kneaded using a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., φ=26 mm, L / D=64.6, cylinder temperature: 260°C), and then granulated to obtain a pellet-shaped polyolefin resin composition (5). Then, the physical properties were measured in the same manner as in Example 1. The results are shown in Table 1.
[0054] [Analysis of each component in polyolefin resin composition (5)] · Ultra-high molecular weight polyethylene content (A-5) and intrinsic viscosity [η] From the proportion (97.5% by mass) of the polyolefin resin composition (R) during dry blending, the content of the ultra-high molecular weight polyethylene (A-5) in the polyolefin resin composition (5) was calculated to be 21.5% by mass. The obtained pellets were used to measure the molecular weight distribution by gel permeation chromatography (GPC), and when compared with the results of the molecular weight distribution measurement by GPC for Example 3, the peak position and shape on the ultra-high molecular weight side of the chromatogram were consistent with those of the ultra-high molecular weight polyethylene (A-3) included in Example 3. Based on this result, the physical properties of the ultra-high molecular weight polyethylene (A-5) were considered to be the same as those of the ultra-high molecular weight polyethylene (A-3). In other words, the intrinsic viscosity [η] of the ultra-high molecular weight polyethylene (A-5) was determined to be 30 dl / g. Furthermore, the position and shape of the peak on the low molecular weight side of the chromatogram were consistent with those of the polyethylene (B1-3) included in Example 3. Based on this result, the physical properties of the polyethylene (B1-5a) (low to high molecular weight polyethylene (B1-5a)) were deemed to be the same as those of the polyethylene (B1-3). In other words, the intrinsic viscosity [η] of the polyethylene (B1-5a) was determined to be 1.0 dl / g. Next, the intrinsic viscosity [η] of polyethylene NOVON BN2 (manufactured by NOVON JAPAN, biomass content 95%) was measured and found to be 1.4 dl / g. From this result, polyethylene NOVON BN2 was designated as polyethylene (B1-5b) (low molecular weight to high molecular weight polyethylene (B1-5b)).
[0055] Polyethylene (B1-5) content and intrinsic viscosity [η] When the polyolefin resin composition (5) after granulation is taken as 100% by mass, the content of polyethylene (B1-5) was calculated to be 78.5% by mass from the content (21.5% by mass) of ultra-high molecular weight polyethylene (A-5). In addition, the content of polyethylene (B1-5a) derived from polyolefin resin composition (R) contained in polyolefin resin composition (5) was calculated to be 76.0% by mass, and the content of polyethylene (B1-5b) derived from polyethylene NOVON BN was calculated to be 2.5% by mass. From the contents and limiting viscosities of the polyethylene (B1-5a) derived from the polyolefin resin composition (R) and the low- to high-molecular-weight polyolefin (B1-5b) derived from NOVON BN2, the limiting viscosity [η] of the polyethylene (B1-5) (low- to high-molecular-weight polyethylene (B1-5)) in the polyolefin resin composition was calculated to be 1.0 dl / g.
[0056] [Example 6] The polyolefin resin composition (R) and polyethylene NOVON BN2 made from biomass-derived components were melt-kneaded and granulated in the same manner as in Example 5, except that the ratio of the polyolefin resin composition (R) and polyethylene NOVON BN2 made from biomass-derived components was changed from 97.5% by mass and 2.5% by mass to 95.0% by mass and 5.0% by mass, respectively, to obtain a pellet-shaped polyolefin resin composition (6). The physical properties of the polyolefin resin composition (6) were calculated and each physical property was measured. The results are shown in Table 1.
[0057] [Example 7] The polyolefin resin composition (R) and polyethylene NOVON BN2 made from biomass-derived components were melt-kneaded and granulated in the same manner as in Example 5, except that the ratio of the polyolefin resin composition (R) and polyethylene NOVON BN2 made from biomass-derived components was changed from 97.5% by mass and 2.5% by mass to 90.0% by mass and 10.0% by mass, respectively, to obtain a pellet-shaped polyolefin resin composition (7). The physical properties of the polyolefin resin composition (7) were calculated and each physical property was measured. The results are shown in Table 1.
[0058] [Example 8] The polyethylene resin composition (R) and polyethylene NOVON BN2 made from biomass-derived components were melt-kneaded and granulated in the same manner as in Example 5, except that the ratio of the polyethylene resin composition (R) and the polyethylene NOVON BN2 made from biomass-derived components was changed from 97.5% by mass and 2.5% by mass to 80.0% by mass and 20.0% by mass, respectively, to obtain a pellet-shaped polyolefin resin composition (8). The physical properties of the polyolefin resin composition (8) were calculated and each physical property was measured. The results are shown in Table 1.
[0059] [Example 9] The polyethylene resin composition (R) and polyethylene NOVON BN2 made from biomass-derived components were melt-kneaded and granulated in the same manner as in Example 5, except that the ratio of the polyethylene resin composition (R) and the polyethylene NOVON BN2 made from biomass-derived components was changed from 97.5% by mass and 2.5% by mass to 50.0% by mass and 50.0% by mass, respectively, to obtain a pellet-shaped polyolefin resin composition (9). The physical properties of the polyolefin resin composition (9) were calculated and each physical property was measured. The results are shown in Table 1.
[0060] [Table 1]
Claims
1. An ultra-high molecular weight polyethylene (A) that satisfies the following requirement (a-1); Contains a polyolefin (B) that satisfies the following requirement (b-1): A biomass-derived polyolefin resin composition that satisfies the following requirement (I): (I) The MFR measured in accordance with ASTM D1238E under a load of 10 kg at a temperature of 190° C. is 0.01 to 500 g / 10 min. (a-1) The intrinsic viscosity [η] measured in a decalin solvent at 135 ° C. is 8 to 50 dl / g; (b-1) The intrinsic viscosity [η] measured in a decalin solvent at 135° C. is 0.1 to 5 dl / g.
2. The content of the ultra-high molecular weight polyethylene (A) is 5 to 40 parts by mass, The content of the polyolefin (B) is 60 to 95 parts by mass (wherein the total amount of the polyethylene (A) and the polyolefin (B) is 100 parts by mass). The polyolefin resin composition according to claim 1.
3. The polyolefin resin composition according to claim 1, wherein at least one of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contains a structural unit derived from a biomass-derived monomer.
4. The polyolefin resin composition according to claim 1, having a biomass content of 1% or more according to ASTM D 6866.
5. The polyolefin resin composition according to claim 1, wherein at least one of the ultra-high molecular weight polyethylene (A) and the polyolefin (B) contains a structural unit derived from a biomass-derived monomer and a structural unit derived from a non-biomass-derived monomer.
6. The polyolefin resin composition according to claim 1, wherein the polyolefin (B) is polyethylene.
7. A molded article comprising the polyolefin resin composition according to any one of claims 1 to 6.
8. The molded article according to claim 7, which is an injection molded article.
Citation Information
Patent Citations
Polyethylene resin composition
JP2012025904A
Ultrahigh molecular weight polyethylene resin composition and method of producing the same
JP2016108475A
Resin composition for slide member and slide member
JP2021172705A
Resin composition containing biomass-derived raw material and applications thereof
JP2022123573A
Sliding composition and use thereof, and method for producing sliding composition