Lid body of packaging container

A packaging container lid with a recycled polyester layer and laminated virgin polyester layers, biaxially stretched for high tear strength, addresses tear resistance and air permeability issues, enhancing durability and environmental sustainability.

JP2024132417APending Publication Date: 2024-10-01RISU PACK CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023043167
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lids for packaging containers made from recycled plastic materials face issues with tear resistance and air permeability, particularly when exposed to steam pressure changes during heating, and may catch on obstacles, leading to practical problems.

Method used

A packaging container lid formed from a resin sheet with a recycled polyester layer and a virgin polyester layer laminated on both sides, biaxially stretched to ensure a tear strength of 4.0N or more, and featuring a C-shaped or U-shaped opening valve for air permeability.

Benefits of technology

The lid maintains air permeability while being difficult to tear and reduces environmental impact by utilizing a high proportion of recycled polyester, ensuring durability and preventing tearing even when caught on obstacles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132417000001_ABST
    Figure 2024132417000001_ABST
Patent Text Reader

Abstract

To provide a lid body of a packaging container that has an open valve for gas or liquid to enter / exit and is formed by a resin sheet, so that it is less apt to be torn without problems practically while securing aeration at an open valve.SOLUTION: A lid body 15 of a packaging container 10 is formed by a resin sheet 20 and the resin sheet 20 comprises a recycled polyester layer 21 that contains recycled polyester consisting of used polyester and a virgin polyester layer 22 that laid over one or both sides of the recycled polyester layer 21 and does not contain recycled polyester. The resin sheet 20 is a sheet formed through biaxial drawing. In a top-face portion 16 of the lid body 15 obtained by thermo-foaming to the resin sheet 20, an open valve 18 is formed for gas or liquid to enter / exit. The top-face portion 16 of the lid body 15 has a tear strength of 4.0 N or greater.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lid for a packaging container. [Background technology]

[0002] For example, Patent Document 1 discloses a synthetic resin lid that is placed over a synthetic resin container body that contains food to close the opening of the container body. A tongue portion of a desired shape is formed by making a cut in the top surface of the lid. The tongue portion is formed by making a cut in the top surface while leaving a connecting portion that connects to the top surface of the lid.

[0003] For example, when a lid is placed on the container body containing food and the food is heated in a microwave oven or the like, steam is generated from the food and the pressure inside the container body rises, causing the tongue portion to bend upward to form an exhaust port. Through the exhaust port formed by the bending of the tongue portion, the steam inside the container body can be exhausted to the outside of the container body. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-50008 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, the reuse of used plastic products has been attracting attention against the backdrop of environmental issues. Therefore, the inventor of the present application is considering forming a synthetic resin lid as disclosed in Patent Document 1 from a resin sheet containing a recycled plastic layer obtained by reusing used plastic products. The inventor of the present application is considering making it difficult for the tongue portion (in other words, the opening valve) of a lid body formed from a resin sheet containing a recycled plastic layer to be torn off even if the tongue portion is caught on clothing or an obstacle.

[0006] The present invention has been made in consideration of these points, and its object is to provide a lid for a packaging container which has an opening valve through which gas or liquid can enter and exit and is formed from a resin sheet, which ensures breathability of the opening valve of the lid while being difficult to tear without causing any problems in practical use. [Means for solving the problem]

[0007] The lid for a packaging container according to the present invention is a lid for a packaging container formed from a resin sheet. The resin sheet has a recycled polyester layer containing recycled polyester made of used polyester, and a virgin polyester layer not containing the recycled polyester, laminated on one or both sides of the recycled polyester layer. The resin sheet is a sheet formed by biaxial stretching. An opening valve for allowing gas or liquid to enter and exit is formed on the top surface of the lid obtained by thermoforming the resin sheet. The tear strength of the top surface of the lid is 4.0 N or more.

[0008] The inventors of the present application have found that when a resin sheet is biaxially stretched, the tear strength decreases due to the orientation of molecular chains. On the other hand, there is a possibility that the recycled polyester may contain impurities such as labels and caps of PET bottles. For example, when a resin sheet having a recycled polyester layer containing recycled polyester containing impurities is stretched during thermoforming, the area around the impurities is stretched, but the impurities themselves are difficult to stretch. This is thought to cause small voids to occur between the impurities and their surroundings. There is a risk that the tear strength will decrease from these voids. Furthermore, it is thought that the resin sheet containing recycled polyester will become more noticeable when biaxially stretched, and the tear strength will decrease. However, according to the above-mentioned lid for packaging containers, by providing a virgin polyester layer not containing recycled polyester on one or both sides of the recycled polyester layer in the resin sheet, the tear strength can be made 4.0 N or more even when the resin sheet is biaxially stretched. Therefore, the lid for packaging containers can be made difficult to tear without practical problems while ensuring the breathability of the opening valve of the lid.

[0009] According to a preferred embodiment of the present invention, the opening valve has an opening formed in the top surface portion and a valve body capable of opening and closing the opening. The valve body is C-shaped or U-shaped.

[0010] According to the above aspect, by making the valve body of the opening valve C-shaped or U-shaped, it is possible to ensure breathability with a simple configuration, while making it difficult for the opening valve of the lid body to be torn even if the valve body gets caught.

[0011] According to another preferred embodiment of the present invention, the ratio of a thickness of the recycled polyester layer to a total thickness of the resin sheet is 60% or more and 98% or less.

[0012] According to the above embodiment, the proportion of the thickness of the recycled polyester layer to the total thickness of the resin sheet is set to 60% or more and 98% or less, thereby contributing to a reduction in the environmental load.

[0013] According to another preferred embodiment of the present invention, the recycled polyester layer contains 80% by mass or more of the recycled polyester.

[0014] According to the above embodiment, a large amount of recycled polyester can be used, which contributes to reducing the environmental load.

[0015] According to another preferred embodiment of the present invention, the lid has a relative crystallinity of 30% or more.

[0016] The higher the relative crystallinity, the higher the proportion of crystalline portions in the entire resin, and the better the heat resistance. Therefore, by making the relative crystallinity of the lid 30% or more, a lid with high heat resistance can be provided. Effect of the Invention

[0017] According to the present invention, it is possible to provide a lid for a packaging container which has an opening valve through which gas or liquid can flow in and out and which is formed from a resin sheet, and which ensures the breathability of the opening valve of the lid, while preventing the opening valve from being torn without causing any practical problems when an obstacle such as clothing gets caught on the opening valve, and which is less likely to cause debris to be mixed in as impurities. [Brief description of the drawings]

[0018] [Figure 1] 1 is a perspective view showing a packaging container having a lid body and a container body according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a part of the lid body and also a cross-sectional view of a resin sheet. [Diagram 3] FIG. 2 is a diagram of a resin sheet showing the MD and TD directions in which it is biaxially stretched. [Figure 4A] FIG. 4 is a plan view showing the shape of a valve body of the opening valve. [Figure 4B] 13 is a plan view showing the shape of a valve body of an opening valve according to a modified example. FIG. [Diagram 5] 4 is a flowchart showing a procedure for producing a resin sheet and a packaging container. [Figure 6] FIG. 1 is a schematic diagram showing an extrusion device used in extrusion molding. [Figure 7] FIG. 1 is a schematic diagram of a mold and plug used in thermoforming. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of a lid for a packaging container according to the present invention will be described with reference to the drawings. It should be noted that the embodiment described here is not intended to limit the present invention. In addition, the same reference numerals are used for members and parts that perform the same function, and duplicated descriptions are omitted or simplified as appropriate. In addition, the same reference numerals are used for members and parts that perform the same function, and duplicated descriptions are omitted or simplified as appropriate.

[0020] FIG. 1 is a perspective view showing a packaging container 10 including a lid body 15 and a container body 11 according to the present embodiment. The packaging container 10 is, for example, a container in which food is stored. The packaging container 10 is a container to be heated. Here, for example, the packaging container 10 is a container in which food is stored and placed in a microwave oven to be heated. However, the packaging container 10 is not limited to a container in which food is stored. As shown in FIG. 1, the packaging container 10 includes a container body 11 and a lid body 15. The packaging container 10, i.e., the container body 11 and the lid body 15, are formed of a resin sheet 20. The type, use, shape, etc. of the packaging container 10 are not particularly limited as long as it is formed of the resin sheet 20.

[0021] The resin sheet 20 is a sheet made of polyester, or a so-called polyester sheet. For example, the resin sheet 20 is made of polyethylene terephthalate (hereinafter also referred to as PET). However, the material forming the resin sheet 20 is not limited to PET, and may be, for example, polylactic acid (hereinafter also referred to as PLA). PLA is a type of biodegradable plastic made from agricultural products such as corn, potatoes, sugar cane, and beets.

[0022] Fig. 2 is a cross-sectional view of the resin sheet 20. As shown in Fig. 2, the resin sheet 20 is formed of a plurality of layers. The number of layers forming the resin sheet 20 is not particularly limited. In the following, a resin sheet 20 formed of three layers will be described.

[0023] In this embodiment, the resin sheet 20 includes a recycled polyester layer 21 and a virgin polyester layer 22 (here, two virgin polyester layers 22). The resin sheet 20 is a sheet in which the recycled polyester layer 21 and the virgin polyester layer 22 are laminated.

[0024] The recycled polyester layer 21 is a layer containing recycled polyester. The recycled polyester layer 21 is a layer formed by recycled polyester. Here, recycled polyester is made of used polyester. Used polyester is polyester obtained from used polyester products. Used polyester products are, for example, used polyester products collected from the market. Here, polyester products refer to, for example, PET bottles and PET trays. Recycled polyester is polyester obtained by collecting used polyester products, and is reused polyester. Also, recycled polyester is polyester obtained by collecting used polyester products based on a predetermined recycling method.

[0025] Here, examples of recycling methods for polyester products such as PET bottles include material recycling, chemical recycling, and mechanical recycling. Material recycling is to crush collected polyester products, wash them with alkali, and reuse them as fibers. Chemical recycling is to chemically decompose collected polyester products, return them to the raw material level, and resynthesize PET. Mechanical recycling is to reuse collected polyester products by performing alkaline washing more strictly than in the above-mentioned material recycling, or by vacuum drying at high temperatures to reliably remove dirt from the polyester products. Here, polyester reused by mechanical recycling is called mechanically recycled polyester. In this embodiment, the regenerated polyester is, for example, mechanically recycled polyester.

[0026] The recycled polyester layer 21 may contain polyester other than recycled polyester (e.g., PET). Here, examples of polyester other than recycled polyester contained in the recycled polyester layer 21 include virgin polyester, which will be described later. In this embodiment, the recycled polyester contained in the recycled polyester layer 21 is 80% by mass or more, preferably 85% by mass or more, and particularly preferably 90% by mass or more.

[0027] In addition, the recycled polyester layer 21 may contain waste during the manufacturing process, such as edge waste and skeleton waste, which occurs when producing the resin sheet 20 or the packaging container 10, as long as this does not significantly impair moldability.

[0028] The virgin polyester layer 22 is a layer that does not contain recycled polyester. The virgin polyester layer 22 is a layer that contains so-called virgin polyester. The virgin polyester layer 22 is formed of virgin polyester. Here, virgin polyester means polyester that does not contain recycled polyester, and is unused (in other words, not reused) polyester. Virgin polyester is a new material. The virgin polyester layer 22 is a layer formed of unused polyester. Virgin polyester is different from recycled polyester obtained from used polyester products collected from the market.

[0029] For example, virgin polyester includes polyester derived from biomass. An example of a biomass-derived polyester is PET derived from biomass. Biomass-derived polyester refers to polyester produced using raw materials derived from plants such as corn, potatoes, sugarcane, and beets. Biomass-derived PET refers to PET produced using the above-mentioned raw materials derived from plants, and is a crystalline polyester. Virgin polyester may include polyester derived from petroleum, for example. Petroleum-derived polyester (e.g., PET) refers to polyester made from petroleum.

[0030] The virgin polyester layer 22 may contain other components besides polyester (e.g., PET) as necessary, as long as the transparency and functionality are not significantly impaired. Examples of such other components include additives used in known resin sheets (e.g., flame retardants, ultraviolet absorbers, fluorescent brighteners, antistatic agents, anti-fog agents, lubricants (e.g., lubricant MB (master batch)), antiblocking agents, flowability modifiers, plasticizers, dispersants, antibacterial agents, etc.).

[0031] In this embodiment, as shown in Fig. 2, the virgin polyester layers 22 are laminated on both sides of the recycled polyester layer 21. Here, the virgin polyester layers 22 are provided on both broad surfaces of the recycled polyester layer 21 (the upper and lower surfaces in Fig. 2). Here, the number of virgin polyester layers 22 is two. The recycled polyester layer 21 is sandwiched between the two virgin polyester layers 22.

[0032] Each recycled polyester layer 21 may be a single layer or a multilayer, and may be formed by laminating a plurality of layers (here, recycled polyester layers). Similarly, each virgin polyester layer 22 may be a single layer or a multilayer, and may be formed by laminating a plurality of layers (here, virgin polyester layers).

[0033] In this embodiment, the total thickness of the resin sheet 20 (in other words, the thickness of the container body 11 and the lid body 15) is 0.3 mm or less, and preferably 0.25 mm or less. Here, the thickness of the resin sheet 20 refers to the total thickness of the recycled polyester layer 21 and the virgin polyester layer 22 combined. In this embodiment, of the recycled polyester layer 21 and the virgin polyester layer 22 of the resin sheet 20, the recycled polyester layer 21 is thicker than the virgin polyester layer 22. For example, the ratio of the thickness of the recycled polyester layer 21 to the total thickness of the resin sheet 20 is 60% or more and 98% or less, preferably 70% or more and 95% or less, and particularly preferably 80% or more and 92% or less. For example, the ratio of the thickness of the recycled polyester layer 21 to the virgin polyester layer 22 is recycled polyester layer:virgin polyester layer=80:20 or 92:8. In this embodiment, the thicknesses of the two virgin polyester layers 22 are the same. However, the thicknesses of the two virgin polyester layers 22 may be different.

[0034] The resin sheet 20 is a sheet formed by biaxial stretching. FIG. 3 is a diagram of the resin sheet 20 showing the MD and TD directions in which the resin sheet 20 is biaxially stretched. Here, as shown in FIG. 3, the longitudinal direction and the transverse direction of the resin sheet 20 are defined as the MD and TD directions, respectively. The TD direction is perpendicular to the MD direction. The MD and TD directions are orthogonal to each other. Here, biaxial stretching refers to stretching the resin sheet 20 biaxially in the MD and TD directions to form a thin sheet. However, the direction in which the resin sheet 20 is biaxially stretched is not limited to the MD and TD directions.

[0035] The biaxial stretching of the resin sheet 20 may be simultaneous biaxial stretching or sequential biaxial stretching. Simultaneous biaxial stretching refers to stretching the resin sheet 20 in both the MD direction and the TD direction at the same time. Sequential biaxial stretching refers to stretching the resin sheet 20 in one of the MD direction and the TD direction and then stretching in the other direction. For example, in sequential biaxial stretching, the resin sheet 20 is stretched in the MD direction and then stretched in the TD direction, or is stretched in the TD direction and then stretched in the MD direction.

[0036] The resin sheet 20 according to this embodiment has been described above. In this embodiment, as shown in FIG. 1, the packaging container 10, i.e., the container body 11 and the lid body 15, are produced by molding the resin sheet 20. As described above, the packaging container 10 includes the container body 11 and the lid body 15. The container body 11 and the lid body 15 are formed from the resin sheet 20.

[0037] As shown in FIG. 1, the container body 11 has a bottom 12 and a side wall 13. The bottom 12 constitutes the bottom portion of the container body 11. The side wall 13 rises from the bottom 12. The side wall 13 extends upward from, for example, an end (for example, a peripheral end) of the bottom 12. The side wall 13 is disposed so as to surround the bottom 12 in a plan view. The side wall 13 may extend perpendicularly to the bottom 12, or may extend obliquely upward from the bottom 12. In other words, the side wall 13 may be inclined so as to face outward from the bottom 12 as it moves upward away from the bottom 12. The bottom 12 and the side wall 13 may have flat surfaces, or may be provided with convex or concave portions (not shown) to increase rigidity. Here, food or the like is contained in a space surrounded by the bottom 12 and the side wall 13.

[0038] In this embodiment, the bottom 12 is circular. However, the shape of the bottom 12 is not particularly limited, and the shape of the container body 11 is also not particularly limited. Here, the container body 11 has a container opening (not shown) surrounded by the upper edge of the side wall portion 13. The container opening opens upward.

[0039] 1, the lid body 15 can be attached to the container body 11. Here, the lid body 15 is attached to the container body 11 so as to be able to freely open and close the container opening of the container body 11. The lid body 15 closes the container opening by being attached to the upper end of the side wall portion 13 of the container body 11. In this embodiment, the lid body 15 includes a top surface portion 16 and a fitting portion 17.

[0040] Top surface portion 16 constitutes the top surface of lid body 15. Top surface portion 16 faces bottom portion 12 when lid body 15 is attached to container body 11. For example, when lid body 15 is attached to container body 11, top surface portion 16 is disposed so as to be parallel to bottom portion 12.

[0041] The fitting portion 17 is fitted to the container body 11 when the lid body 15 is attached to the container body 11. In this embodiment, the fitting portion 17 is capable of fitting to the upper end portion of the side wall portion 13 of the container body 11. The fitting portion 17 is provided at an end (e.g., a peripheral end) of the top surface portion 16 in a plan view. The fitting portion 17 is provided so as to surround the top surface portion 16 in a plan view. The fitting portion 17 is disposed at a position corresponding to the upper end portion of the side wall portion 13 in a state in which the lid body 15 is attached to the container body 11. The specific configuration of the fitting portion 17 is not particularly limited. The fitting portion 17 may be provided with a recess into which the upper end portion of the side wall portion 13 of the container body 11 is fitted, for example. The recess is provided so as to surround the top surface portion 16 in a plan view, and is configured to be recessed upward from the bottom surface of the fitting portion 17.

[0042] In this embodiment, an opening valve 18 is formed on the top surface 16 of the lid body 15. The opening valve 18 is a valve through which gas or liquid flows in and out. As described above, in this embodiment, the packaging container 10 is a container that is placed in a microwave oven or the like while containing food and heated. When heated in this manner, steam (e.g., water vapor) is generated by the food being heated. The opening valve 18 of the lid body 15 is in a closed state before being heated in the microwave oven, and when the food is heated in the microwave oven, the opening valve 18 opens when the steam generated by the food being heated is discharged to the outside of the lid body 15, and the steam passes through the opening valve 18. After the steam passes through, the opening valve 18 returns to its original closed state. Note that the number and position of the opening valves 18 formed on the top surface 16 are not particularly limited. In this embodiment, the number of opening valves 18 formed on the top surface 16 of the lid body 15 is two. Also, the opening valve 18 is formed in the center part of the top surface 16.

[0043] The configuration of the opening valve 18 is not particularly limited. Here, the opening valve 18 has an opening 19a formed in the top surface portion 16 and a valve body 19b capable of opening and closing the opening 19a. Gas and liquid pass through the opening 19a. The valve body 19b is connected to the top surface portion 16. In this embodiment, the opening valve 18 is formed by making a cut in the top surface portion 16. The cut portion of the top surface portion 16 becomes the opening 19a and also becomes the valve body 19b. Therefore, the valve body 19b has a shape that matches the opening 19a. The valve body 19b is formed by a known processing device such as a punching blade or a laser.

[0044] FIG. 4A is a plan view showing the shape of the valve body 19b of the opening valve 18. FIG. 4B is a plan view showing the shape of the valve body 19b of the opening valve 18 according to a modified example. In this embodiment, as shown in FIG. 4A, the shape of the valve body 19b of the opening valve 18 is U-shaped. At this time, the shape of the opening 19a is also U-shaped. The shape of the valve body 19b is not particularly limited. As shown in FIG. 4B, for example, the shape of the valve body 19b may be C-shaped. At this time, the shape of the opening 19a may also be C-shaped.

[0045] In this embodiment, as shown in FIG. 2, the packaging container 10 (in other words, the lid body 15) includes an inner layer 31, an outer layer 32, and an intermediate layer 33. In FIG. 2, the upper side shows the inside of the lid body 15, and the lower side shows the outside of the lid body 15. The top surface portion 16 (see FIG. 1) and the fitting portion 17 (see FIG. 1) of the lid body 15 are formed from the inner layer 31, the outer layer 32, and the intermediate layer 33. The inner layer 31 is the layer disposed on the innermost side among the multiple layers constituting the lid body 15. The inner layer 31 is the layer that constitutes the inner peripheral surface of the lid body 15. The inner layer 31 is the layer that comes into direct contact with the food when the food is contained in the packaging container 10. The outer layer 32 is the layer disposed on the outermost side among the multiple layers constituting the lid body 15, and is the layer that constitutes the outer peripheral surface of the lid body 15. The outer layer 32 is the layer that comes into direct contact with the user's hand, for example, when the user holds the packaging container 10 in his / her hand.

[0046] The intermediate layer 33 is a layer disposed between the inner layer 31 and the outer layer 32. As shown in Fig. 2, the intermediate layer 33 is sandwiched between the inner layer 31 and the outer layer 32. Therefore, the intermediate layer 33 can be a layer that is not directly touched by food or a user. Each of the inner layer 31, the outer layer 32, and the intermediate layer 33 may be a single layer, or may be a layer formed by laminating a plurality of layers.

[0047] In this embodiment, in the lid 15 of the packaging container 10, the inner layer 31 and the outer layer 32 are formed by the virgin polyester layer 22 of the resin sheet 20. The intermediate layer 33 is formed by the recycled polyester layer 21 of the resin sheet 20.

[0048] The container body 11 of the packaging container 10 is formed of an inner layer 31, an outer layer 32, and an intermediate layer 33, similar to the lid body 15. In other words, the container body 11 is formed of three layers in which the virgin polyester layers 22 are provided on both sides of the recycled polyester layer 21, and the recycled polyester layer 21 is sandwiched between the virgin polyester layers 22.

[0049] As described above, the opening valve 18 is formed on the top surface 16 of the lid body 15. Therefore, in order to make the valve body 19b of the opening valve 18 difficult to tear, in this embodiment, the tear strength of the top surface 16 of the lid body 15 (in other words, the resin sheet 20) is 4.0 N or more, preferably 4.5 N or more, and particularly preferably 5.0 N, for example, 5.2 N or more. Specifically, even if the opening valve 18 of the top surface 16 of the lid body 15 is formed in the stretching direction (for example, MD direction or TD direction) of the biaxially stretched resin sheet 20, since the tear strength of the top surface 16 is 4.0 N or more, the opening valve 18 can be made difficult to tear without any practical problems.

[0050] In this embodiment, the relative crystallinity of the cover 15 is 30% or more, preferably 50% or more, and particularly preferably 80% or more, for example 95% or more. Here, the relative crystallinity refers to the proportion of crystalline parts. When the relative crystallinity is high, the polymer chains become denser and the bonding force (intermolecular force) per unit area increases, thereby improving toughness, heat resistance, chemical resistance, and the like.

[0051] Next, a procedure for producing the resin sheet 20 and the packaging container 10 according to this embodiment will be described. FIG. 5 is a flow chart showing the procedure for producing the resin sheet 20 and the packaging container 10. In this embodiment, as shown in FIG. 5, pellets are prepared (step S101), and the pellets are extrusion molded (step S103), to produce the resin sheet 20. Then, the resin sheet 20 is biaxially stretched (step S105) and thermoformed (step S107) in this order, to produce the packaging container 10, i.e., the container body 11 and the lid body 15.

[0052] First, in step S101, pellets are prepared. In this embodiment, virgin pellets made of virgin polyester and recycled pellets made of recycled polyester are prepared as the pellets. The recycled pellets are made, for example, from used polyester resin molded products (in other words, used polyester products) collected from the market. Used polyester products are, for example, used PET containers such as used PET bottles and used PET trays. Here, the recycled pellets are made by crushing used polyester products collected from the market, removing foreign matter, washing, and drying.

[0053] Next, in step S103, the virgin pellets and the recycled pellets are extruded to produce the resin sheet 20. FIG. 6 is a schematic diagram of an extrusion device 50 used in the extrusion molding. In this embodiment, the extrusion device 50 shown in FIG. 6 is used in the extrusion molding. As shown in FIG. 6, the extrusion device 50 has a first hopper 51A, a first screw 52A, a second hopper 51B, a second screw 52B, a feed block 58, a joining die 53, a cooling roller 54, and a winder 55.

[0054] In this embodiment, the first hopper 51A and the first screw 52A are for virgin pellets (hereinafter referred to as for virgin). The second hopper 51B and the second screw 52B are for recycled pellets (hereinafter referred to as for recycled). The first hopper 51A is connected to the first screw 52A, and a first heater 57A is provided around the first screw 52A. The second hopper 51B is connected to the second screw 52B, and a second heater 57B is provided around the second screw 52B. In addition, the first screw 52A and the second screw 52B are connected to a feed block 58. The feed block 58 is connected to a joining die 53.

[0055] In the extrusion molding, the virgin pellets 40A are first put into the first hopper 51A. In the virgin use, the virgin pellets 40A put into the first hopper 51A are made to flow into the first screw 52A, and mixed by the rotation of the first screw 52A while being heated by the first heater 57A. The virgin pellets 40A mixed by the first screw 52A are made to flow toward the narrow feed block 58. Similarly, in the regeneration use, the regeneration pellets 40B are put into the second hopper 51B. The regeneration pellets 40B put into the second hopper 51B are made to flow into the second screw 52B, and mixed by the rotation of the second screw 52B while being heated by the second heater 57B. The regeneration pellets 40B mixed by the second screw 52B are made to flow toward the feed block 58.

[0056] In the feed block 58, the virgin pellets 40A and the recycled pellets 40B join together and are made to flow into the joining die 53. In the joining die 53, a layer of the virgin pellets 40A and a layer of the recycled pellets 40B are extruded (here, co-extruded) by the feed block 58 and discharged. Here, the layer of the virgin pellets 40A extruded from the joining die 53 by the feed block 58 becomes the virgin polyester layer 22 (see FIG. 2). The layer of the recycled pellets 40B extruded from the joining die 53 by the feed block 58 becomes the recycled polyester layer 21 (see FIG. 2).

[0057] In this embodiment, although detailed illustration is omitted, the virgin polyester layer 22, the recycled polyester layer 21, and the virgin polyester layer 22 are stacked in this order in a heated state to form a sheet, which is then discharged from the joining die 53. At this time, the virgin polyester layer 22 and the recycled polyester layer 21 are bonded to each other to form the resin sheet 20.

[0058] In this embodiment, as shown in Fig. 6, a cooling roller 54 and a winder 55 are arranged in this order downstream of the confluence die 53, i.e., at the destination of the resin sheet 20 discharged from the confluence die 53. The resin sheet 20 discharged from the confluence die 53 passes through the cooling roller 54. Here, since the resin sheet 20 discharged from the confluence die 53 is in a heated state, it is cooled by passing through the cooling roller 54. The resin sheet 20 passing through the cooling roller 54 is transported toward the winder 55 and wound into a roll by the winder 55. The resin sheet 20 is produced by the above procedure.

[0059] Next, in step S105 of Fig. 5, the resin sheet 20 produced in step S103 is biaxially stretched. The biaxial stretching at this time may be simultaneous biaxial stretching or sequential biaxial stretching as described above. Here, as shown in Fig. 3, the biaxial stretching is performed by stretching the resin sheet 20 in the MD direction and the TD direction. In this embodiment, the resin sheet 20 is thinned by biaxial stretching so that the total thickness of the resin sheet 20 is 0.3 mm or less, for example.

[0060] Next, in step S107 of FIG. 5, the biaxially stretched resin sheet 20 is thermoformed to produce the packaging container 10, i.e., the container body 11 and the lid body 15. Here, thermoforming can also be referred to as vacuum forming, pressure forming, or a combination of vacuum forming and pressure forming. FIG. 7 is a schematic diagram of a mold 60 and a plug 65 used in thermoforming. As shown in FIG. 7, a mold 60 and a plug 65 are used in thermoforming. A recess 61 is formed in the mold 60. A protrusion 66 is formed in the plug 65 to be inserted into the recess 61 of the mold 60. Here, during thermoforming, the mold 60 and the plug 65 are arranged in a spaced apart state so that the recess 61 and the protrusion 66 face each other. Thereafter, the heated resin sheet 20 is arranged between the mold 60 and the plug 65. At this time, the resin sheet 20 is arranged so that one of the two virgin polyester layers 22 of the resin sheet 20 is located on the plug 65 side, and the other of the two virgin polyester layers 22 is located on the mold 60 side.

[0061] 7, the mold 60 or the plug 65 is moved to insert the convex portion 66 of the plug 65 into the concave portion 61 of the mold 60. As a result, the resin sheet 20 is thermoformed between the concave portion 61 and the convex portion 66 along the shapes of the concave portion 61 and the convex portion 66, and the thermoformed resin sheet 20 is appropriately cut to produce the packaging container 10.

[0062] In this embodiment, a mold 60 and a plug 65 for producing the container body 11, and a mold 60 and a plug 65 for producing the lid body 15 are prepared. When producing the container body 11, the recess 61 of the mold 60 and the protrusion 66 of the plug 65 have shapes corresponding to the shape of the container body 11. When producing the lid body 15, the recess 61 of the mold 60 and the protrusion 66 of the plug 65 have shapes corresponding to the shape of the lid body 15.

[0063] In the present embodiment, the packaging container 10 is used as a container for containing food, as described above, and is placed in a microwave oven or the like with the food contained therein and heated. When the food is heated in a microwave oven or the like, the moisture contained in the food evaporates and generates steam. When the food generates steam while contained in the packaging container 10, the pressure of the packaging container 10 increases, causing the packaging container 10 to expand. In order to prevent the packaging container 10 from expanding excessively, an opening valve 18 is formed on the lid 15 in the present embodiment, as shown in FIG. 1. The steam generated from the food passes through the opening valve 18 and is discharged to the outside of the packaging container 10, thereby preventing the packaging container 10 from expanding excessively.

[0064] In order to prevent foreign objects such as insects and dust from entering the packaging container 10, it is preferable that the opening valve 18 is opened by steam generated inside the packaging container 10 when the packaging container 10 is heated by a microwave oven or the like, and is closed at other times. In addition, the valve body 19b of the opening valve 18 may be torn by being caught on clothing or an obstacle. Therefore, by forming the valve body 19b into a U-shape or a C-shape, it is possible to make the valve body 19b less likely to be torn.

[0065] In addition, in order to make the valve body 19b of the opening valve 18 difficult to tear, it is preferable to increase the tear strength of the lid body 15 (in other words, the resin sheet 20). However, the resin sheet 20 forming the lid body 15 is a sheet in which a recycled polyester layer 21 and a virgin polyester layer 22 are laminated. Of these, the recycled polyester layer 21 may contain impurities because it contains recycled polyester that is collected, washed, crushed, etc. from used polyester products (e.g., PET bottles). When the recycled polyester layer 21 contains impurities and is stretched during thermoforming, the recycled polyester around the impurities is stretched, but the impurities themselves are not stretched. As a result, in the recycled polyester layer 21, voids (so-called voids) may be formed between the impurities and the recycled polyester around the impurities. If voids are formed in the recycled polyester layer 21, the voids may become starting points and cause the opening valve 18 of the lid body 15 to tear. Furthermore, it is believed that when the recycled polyester layer 21 containing impurities is biaxially stretched, the occurrence of the above-mentioned voids becomes significant, resulting in a decrease in tear strength.

[0066] However, in this embodiment, by laminating the virgin polyester layer 22 on the recycled polyester layer 21 in the resin sheet 20 forming the lid 15, even if a void is formed in the recycled polyester layer 21, the void is covered by the virgin polyester layer 22, making it difficult for tearing to occur starting from the void. As a result, even when the lid 15 is formed from the resin sheet 20 including the recycled polyester layer 21, a tear strength of 4.0 N or more can be ensured. Therefore, even when the lid 15 is formed from the resin sheet 20 including the recycled polyester layer 21, the opening valve 18 of the lid 15 can be made difficult to tear.

[0067] Next, an evaluation test was conducted to evaluate the tear strength of the lid 15 of the packaging container 10 according to this embodiment. Here, in order to conduct the evaluation test, the following packaging container lids of Samples 1 to 6 were prepared. In Samples 1 to 6, the thickness of the resin sheet was 0.25 mm. In addition, in Samples 1 to 6, the size of the packaging container was 244 mm in length, 171 mm in width, and 16 mm in height.

[0068] <Sample 1> Sample 1 is a lid for a packaging container formed from the resin sheet according to the present embodiment. In Sample 1, the intermediate layer is a recycled polyester layer, and the inner layer and the outer layer are virgin polyester layers. In Sample 1, the thickness ratio of the inner layer, intermediate layer, and outer layer in the lid for the packaging container (hereinafter referred to as layer ratio) is inner layer:intermediate layer:outer layer=4:92:4.

[0069] The recycled polyester layer in Sample 1 is composed of virgin polyester and recycled polyester, and contains 20 mass% virgin polyester and 80 mass% recycled polyester. The virgin polyester layer in Sample 1 is composed of virgin polyester and lubricant MB (master batch), and contains 94 mass% virgin polyester and 6 mass% lubricant MB.

[0070] In sample 1, mechanically recycled polyester made from PET bottles collected from the market was used as the recycled polyester. Bottle recycled PET "VF-31A" manufactured by Utsumi Recycle System Co., Ltd. was used as the mechanically recycled polyester. The intrinsic viscosity IV value of this recycled polyester (mechanically recycled polyester) was 0.74 dl / g. PET resin "YS-H01" manufactured by Hainan Yisheng Petrochemical Co., Ltd. in China was used as the virgin polyester in sample 1. The intrinsic viscosity IV value of this virgin polyester was 0.78 dl / g. In addition, "RE555" manufactured by Toyobo Co., Ltd. was used as the lubricant MB in sample 1. This lubricant MB contains polyester resin containing fine particles obtained by mixing 7000 ppm of spherical silica with an average particle size of 2.4 μm during polymerization into polyester resin with an intrinsic viscosity IV value of 0.62 dl / g.

[0071] In sample 1, the resin sheet and the lid of the packaging container were produced as follows. First, 94% by mass of virgin polyester and 6% by mass of lubricant MB were mixed to prepare a mixture for the virgin polyester layer. Next, 20% by mass of virgin polyester and 80% by mass of recycled polyester were mixed to prepare a mixture for the recycled polyester layer.

[0072] Then, extrusion molding was performed using a twin-screw extruder (here, extrusion device) of model "SBIN-42-S2-30-L" manufactured by Plastics Engineering Research Institute Co., Ltd. Here, the mixture for the virgin polyester layer and the mixture for the recycled polyester layer were supplied to the extrusion device, and melt kneaded and extruded at a temperature of 280°C to produce a resin sheet with a thickness of about 0.3 mm.

[0073] Next, the resin sheet having a thickness of 0.3 mm was biaxially stretched by stretching it 1.2 times in the MD direction and the TD direction in an environment where the stretching temperature was 80°C, and a biaxially stretched resin sheet was produced. The thickness of the biaxially stretched resin sheet was 0.25 mm. Then, the biaxially stretched resin sheet was subjected to a molding pressure of 3 kg / cm using a hot plate compressed air molding machine. 2The molding time was 4 seconds and the molding temperature was 90° C., and a lid for the packaging container of Sample 1 was produced.

[0074] <Sample 2> Sample 2 is a lid for a packaging container that was produced using the same configuration and production procedure as Sample 1, except that the resin sheet produced by extrusion molding did not include an inner layer or an outer layer, and instead was a single layer of recycled polyester, and was thermoformed to produce a lid for a packaging container. In Sample 2, the resin sheet is composed only of an intermediate layer, and the inner layer and the outer layer are omitted. In Sample 2, the thickness of the intermediate layer (in other words, the recycled polyester layer) included in the resin sheet is 0.25 mm.

[0075] <Sample 3> Sample 3 is a lid for a packaging container produced by the same configuration and production procedure as Sample 1, except that the lid for a packaging container was produced by thermoforming an unstretched resin sheet, without biaxially stretching the resin sheet produced by extrusion molding. That is, the resin sheet in Sample 3 has the same configuration as the resin sheet in Sample 1, but is not biaxially stretched. In Sample 3, the thickness of the resin sheet after extrusion molding is 0.25 mm.

[0076] <Sample 4> Sample 4 is a lid for a packaging container produced by the same configuration and production procedure as Sample 2, except that the lid for a packaging container was produced by thermoforming an unstretched resin sheet without biaxially stretching the resin sheet produced by extrusion molding. That is, the resin sheet in Sample 4 has the same configuration as the resin sheet in Sample 2, but is not biaxially stretched. In Sample 4, the thickness of the resin sheet after extrusion molding is 0.25 mm.

[0077] <Sample 5> Sample 5 is a lid for a packaging container that is produced by the same composition and production procedure as Sample 3, except that the composition of the intermediate layer of the lid for the packaging container is different. In Sample 5, the intermediate layer of the lid is not a recycled polyester layer, but a layer that does not contain recycled polyester. The intermediate layer in Sample 5 is formed of virgin polyester and contains 100% by mass of virgin polyester.

[0078] <Sample 6> Sample 6 is a lid for a packaging container that is produced by the same configuration and production procedure as Sample 4, except that the configuration of the resin sheet that forms the lid for the packaging container is different. In Sample 6, the lid is formed from a resin sheet that is composed only of an intermediate layer, with the inner and outer layers omitted. The resin sheet in Sample 6 is not composed of a recycled polyester layer, but of a layer that does not contain recycled polyester. The resin sheet (in other words, the intermediate layer) of Sample 6 is formed from virgin polyester and contains 100% by mass of virgin polyester.

[0079] The materials, blending, layer ratios, etc. of each layer in Samples 1 to 6 are shown in Table 1 below. Regarding biaxial stretching in Table 1, "◯" indicates a sample that was biaxially stretched, and "×" indicates a sample that was not biaxially stretched.

[0080] [Table 1]

[0081] Here, the intrinsic viscosity IV value (dl / g) of the lids of the packaging containers of Samples 1 to 6 was measured in accordance with JIS K7367-5. A mixed solvent of phenol / 1,1,2,2-tetrachloroethane (weight ratio 3 / 1) was used as the solvent. The intrinsic viscosity IV values ​​of the lids of the packaging containers of Samples 1 to 6 are shown in Table 1 above.

[0082] Next, a heat resistance test was conducted on the lids of the packaging containers of Samples 1 to 6. Here, a perfect oven "PHH102M" manufactured by Espec Corporation was used. The lids of the packaging containers of Samples 1 to 6 were placed in the oven and stored at a set temperature of 80°C for 1 minute. The lids of the packaging containers of Samples 1 to 6 were then removed from the oven and visually inspected for deformation. The results are shown in Table 1 above. In Table 1, samples in which deformation of the lids could be visually confirmed are indicated as "deformed," and samples in which no deformation of the lids could be visually confirmed are indicated as "no deformation."

[0083] Next, the relative crystallinity of the lids of the packaging containers of Samples 1 to 6 was measured in accordance with JIS K7122. Here, using a differential scanning calorimeter "DSC8230" manufactured by Rigaku Corporation, the crystallization heat value and melting endotherm value of Samples 1 to 6 were measured under the conditions of a sample weight of 5.0 mg and a heating rate of 10°C / min.

[0084] Here, the relative crystallinity is an index showing the degree (relative degree) of crystallization of the system to be measured, assuming that the maximum state of crystallization that the system to be measured (here, the resin system) can reach is 100% relative crystallinity. The relative crystallinity can be measured by a differential scanning calorimeter (DSC). Here, the relative crystallinity is calculated based on the crystallization heat of the resin system in the sample (the lid of the packaging container in Samples 1 to 6) measured by the differential scanning calorimeter under a temperature rise condition of 10°C / min and the melting endotherm of the resin system. Here, when the crystallization heat of the resin system is ΔHc and the melting endotherm of the resin system is ΔHm, the relative crystallinity xc can be calculated by the following formula (1). xc=100×(|ΔHm|-|ΔHc|) / |ΔHm| ···(1)

[0085] The relative crystallinity of Samples 1 to 6 calculated as above is shown in Table 1 above.

[0086] Furthermore, the tear strength was measured for the lids of the packaging containers of Samples 1 to 6. In accordance with JIS K7128-1 "Test method for tear strength of plastic films and sheets, Part 1: Trouser tear method," test pieces were cut out from the top surface of the lids of Samples 1 to 6 in the vertical or horizontal direction (direction corresponding to the MD or TD direction of biaxial stretching), and the tear strength was measured under the conditions of a distance between the grippers of the test piece of 75 mm and a test speed of 200 mm / min. The tear strengths of the lids of the packaging containers of Samples 1 to 6 measured as described above are shown in Table 1 above.

[0087] As shown in Table 1 above, in samples 3 to 6 that were not biaxially stretched, the relative crystallinity was less than 30%, and the lid of the packaging container was deformed in the heat resistance test. On the other hand, in samples 1 and 2 that were biaxially stretched with respect to the resin sheet, the relative crystallinity was 100%, and the lid of the packaging container was not deformed in the heat resistance test. Therefore, as in samples 1 and 2, by forming a lid of a packaging container using a biaxially stretched resin sheet, it is possible to manufacture a lid of a packaging container with high heat resistance. Also, as shown in Table 1 above, in sample 1, by forming a lid from a multi-layer resin sheet in which the inner and outer layers are virgin polyester layers and the middle layer is a recycled polyester layer, a tear strength of 4.0 N or more was obtained. On the other hand, in sample 2, by omitting the inner and outer layers and forming a lid from a single-layer resin sheet in which the middle layer is a recycled polyester layer, the tear strength was less than 4.0 N. From these results, it is believed that by making the resin sheet not only of recycled polyester layers but of multiple layers consisting of virgin polyester layers and recycled polyester layers laminated together, the tear strength can be increased, making it difficult for the opening valve of the lid to be torn.

[0088] As described above, in this embodiment, as shown in FIG. 1, the lid 15 of the packaging container 10 is a lid formed of a resin sheet 20. As shown in FIG. 2, the resin sheet 20 has a recycled polyester layer 21 containing recycled polyester made of used polyester, and a virgin polyester layer 22 that does not contain recycled polyester and is laminated on one or both sides of the recycled polyester layer 21. The resin sheet 20 is a sheet formed by biaxial stretching, as shown in FIG. 3. As shown in FIG. 1, an opening valve 18 through which gas or liquid enters and exits is formed on the top surface 16 of the lid 15 obtained by thermoforming to the resin sheet 20. The tear strength of the top surface 16 of the lid 15 is 4.0 N or more. In this embodiment, by providing a virgin polyester layer 22 that does not contain recycled polyester on one or both sides of the recycled polyester layer 21 in the resin sheet 20, the tear strength can be 4.0 N or more even when the resin sheet 20 is biaxially stretched. Therefore, the lid 15 of the packaging container 10 can be made difficult to tear without causing any practical problems while ensuring the breathability of the opening valve 18 of the lid 15.

[0089] In this embodiment, the relative crystallinity of the lid body 15 is 30% or more. Here, the higher the relative crystallinity, the more improved the heat resistance and the like. Therefore, by making the relative crystallinity of the lid body 15 30% or more, the heat resistance of the lid body 15 can be improved.

[0090] In this embodiment, as shown in Fig. 1, the opening valve 18 has an opening 19a formed in the top surface portion 16 and a valve body 19b capable of opening and closing the opening 19a. The valve body 19b is C-shaped (see Fig. 4B) or U-shaped (see Fig. 4A). By making the valve body 19b of the opening valve 18 C-shaped or U-shaped in this manner, it is possible to ensure ventilation with a simple configuration and make the opening valve 18 of the lid body 15 less likely to be torn even if the valve body 19b gets caught.

[0091] In this embodiment, the ratio of the thickness of the recycled polyester layer 21 to the total thickness of the resin sheet 20 is 60% or more and 98% or less, which can contribute to reducing the environmental load.

[0092] In this embodiment, the recycled polyester contained in the recycled polyester layer 21 is 80% by mass or more. This allows a large amount of recycled polyester to be used, which contributes to reducing the environmental impact.

[0093] In the above embodiment, as shown in FIG. 2, the virgin polyester layer 22 was laminated on both sides of the recycled polyester layer 21. In other words, the virgin polyester layer 22 was disposed on both sides of the wide surface of the recycled polyester layer 21, and the number of the virgin polyester layers 22 was two. However, the virgin polyester layer 22 may be laminated on one side of the recycled polyester layer 21. That is, the virgin polyester layer 22 may be disposed on only one of the wide surfaces of the recycled polyester layer 21, and the number of the virgin polyester layers 22 may be one. In this case, the outer layer 32 may be omitted in the lid 15 of the packaging container 10. [Explanation of symbols]

[0094] 10 Packaging containers 11 Container body 12 Bottom 15 Lid 16 Top section 18 Opening valve 19a aperture 19b Valve body 20 Resin sheet 21 Recycled polyester layer 22 virgin polyester layer

Claims

1. A lid for a packaging container formed from a resin sheet, The resin sheet is A recycled polyester layer containing recycled polyester made from used polyester; A virgin polyester layer that is laminated on one or both sides of the recycled polyester layer and does not contain the recycled polyester; and is a biaxially stretched sheet, an opening valve through which gas or liquid can enter and exit is formed on a top surface of the lid obtained by thermoforming the resin sheet; A lid for a packaging container, wherein the tear strength of the top surface of the lid is 4.0 N or more.

2. The opening valve is An opening formed in the top surface portion; a valve body capable of opening and closing the opening; having The lid for a packaging container according to claim 1 , wherein the valve body is C-shaped or U-shaped.

3. 2. The lid for a packaging container according to claim 1, wherein a ratio of a thickness of the recycled polyester layer to a total thickness of the resin sheet is 60% or more and 98% or less.

4. 2. The lid for a packaging container according to claim 1, wherein the recycled polyester contained in the recycled polyester layer is 80% by mass or more.

5. 5. A lid for a packaging container according to claim 1, wherein the lid has a relative crystallinity of 30% or more.

Citation Information

Patent Citations

  • Open valve for container for packaging, and punching die for forming open valve

    JP2008050008A