Method for producing laminated molded article, decorative film, and decorative film laminate
The method of using an antistatic agent in decorative films to control charged potential prevents foreign matter adhesion, ensuring a clean appearance during vacuum-pressure forming on concavo-convex molded products.
Patent Information
- Application Number
- JP2023043204
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Decorative films laminated onto concavo-convex molded products using vacuum-pressure forming often expose minute foreign matter shapes due to stretching and thinning, leading to poor appearance.
A method involving a decorative film with a stretchable film base material, where at least one layer is impregnated with an antistatic agent, and a release liner is peeled off before stretching, ensuring the charged potential on the laminated side remains 0.5 kV or less to prevent foreign matter adhesion.
Prevents foreign matter from adhering to the decorative film, maintaining a clean appearance even when stretched and thinned during molding processes.
Smart Images

Figure 2024132444000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a laminated molded product, a decorative film, and a decorative film laminate. [Background technology]
[0002] 2. Description of the Related Art Conventionally, as a method for decorating the surface of a three-dimensional shape, vacuum and pressure molding has been known, in which a decorative film is adhered along the surface of a molded article having projections and recesses, as disclosed in Patent Document 1, for example.
[0003] According to vacuum and pressure molding, the decorative film is laminated onto the surface of the uneven molded product while being stretched, for example, under vacuum, and conforms well to the surface, so that the surface of the uneven molded product can be beautifully decorated. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-214559 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the present inventors laminated a decorative film onto a concave-convex molded product by vacuum and pressure forming, minute foreign matter shapes sometimes appeared on the surface of the decorative film, resulting in poor appearance.
[0006] The present inventors then investigated the causes of this problem and found that when the release liner of the decorative film is peeled off before use, or when individual decorative films are separated from a laminate of multiple decorative films, peel-off static electricity occurs on the side of the decorative film that will be laminated to the uneven molded product, and as a result, foreign matter such as fine dust and dirt adheres to the side of the decorative film that will be laminated to the uneven molded product, and when vacuum and pressure molding is performed with such fine foreign matter still adhering to the decorative film, the stretching and thinning of the decorative film due to the vacuum and pressure molding triggers the fine foreign matter shapes to appear on the surface of the decorative film.
[0007] In fact, when the inventors of the present invention simply attached and laminated a decorative film to a molded product with a concave-convex shape without stretching it, no defective appearance occurred, but when the decorative film was stretched and thinned by vacuum and pressure molding, minute foreign object shapes emerged, resulting in defective appearance. Furthermore, the same phenomenon is not limited to vacuum and pressure molding, and can occur in other molding methods involving decoration using a decorative film, such as film insert molding, in-mold molding, and press molding.
[0008] The present invention has been made to solve the new problem discovered by the inventor, and aims to provide a manufacturing method for a laminated molded product, a decorative film, and a decorative film laminate that are less likely to have fine foreign matter adhere to the side of the decorative film that is laminated to the uneven molded product, and that can prevent the appearance from being impaired even if the decorative film is stretched and thinned during molding that involves decoration. [Means for solving the problem]
[0009] In order to achieve the above object, the method for producing a laminate molded product of the present invention has the following configuration.
[0010] 1. A method for laminating a decorative film having a stretchable film substrate onto the surface of a concave-convex molded product, in which at least one of the layers to be laminated to the film substrate on the side to be laminated to the concave-convex molded product is impregnated with an antistatic agent, and the release liner arranged as the peelable layer is peeled off from the decorative film, or the decorative films that are laminated to each other are peeled off, and the decorative film is stretched and laminated onto the surface of the concave-convex molded product, a manufacturing method for a laminated molded product.
[0011] 2. The method for producing a laminated molded product according to 1., further comprising impregnating the film substrate with an antistatic agent.
[0012] 3. A method for producing a laminated molded product described in 1. or 2., in which a process film is arranged on the side of the film substrate opposite to the side that is laminated to the uneven molded product, and the process film is peeled off before the decorative film is stretched.
[0013] 4. A method for producing a laminated molded product described in any one of 1. to 3., wherein immediately after the decorative film is peeled off from the release liner, or immediately after the laminated decorative films are peeled off from each other, the absolute value of the electrostatic potential of the decorative film on the side that is laminated to the uneven molded product is 0.5 kV or less.
[0014] 5. A decorative film having a stretchable film substrate and a layer superimposed on one side of the film substrate, the peelable layer including a release liner, and the layer including an antistatic agent.
[0015] 6. The decorative film according to 5., further comprising an antistatic agent in the film substrate.
[0016] 7. The decorative film according to 5. or 6., in which a peelable process film is disposed on the surface opposite to the one surface on which the release liner is disposed.
[0017] 8. The decorative film according to any one of 5. to 7., wherein when the release liner is peeled off, the absolute value of the electrostatic potential on the one surface side is 0.5 kV or less.
[0018] 9. A decorative film having a film substrate that can be stretched to fit the shape of the uneven molded product is laminated in multiple layers. The decorative film is At least one of the layers to be laminated on the side of the film substrate that is to be laminated on the uneven molded product contains an antistatic agent, The decorative film is in direct contact with the adjacent decorative film in the lamination direction, and is laminated so as to be peelable only between the decorative films that are in direct contact with each other, or A peelable process film is arranged on the surface opposite to the side laminated to the uneven molded product, and is laminated in direct peelable contact with the process film arranged on the adjacent decorative film in the lamination direction.
[0019] 10. The decorative film laminate according to claim 9, wherein the decorative film further contains an antistatic agent in the film substrate.
[0020] 11. The decorative film laminate according to claim 9 or 10, wherein the process film is disposed on the decorative film.
[0021] 12. A decorative film laminate described in any one of 9. to 11., wherein the decorative film has a resin layer laminated in a non-peelable manner via an adhesive layer as the layer to be laminated on the side to be laminated to the uneven molded product.
[0022] 13. A decorative film laminate described in any one of 9. to 12., in which the absolute value of the electrostatic potential generated on the side of the decorative film peeled off from the decorative film laminate that is laminated to the uneven molded product is 0.5 kV or less.
[0023] In one embodiment of the decorative film laminate of the present invention for achieving the above object, a plurality of decorative films having a film substrate that can be stretched to fit the shape of the uneven molded product are laminated. The decorative film contains an antistatic agent in at least one of the layers laminated on the side of the film substrate that is laminated on the uneven molded product, and is in direct contact with the decorative film adjacent in the lamination direction and is laminated peelably only between the decorative film that is in direct contact with the decorative film, or a peelable process film is disposed on the surface opposite to the side that is laminated on the uneven molded product, and is laminated peelably in direct contact with the process film disposed on the decorative film adjacent in the lamination direction. Effect of the Invention
[0024] In the invention having the above configuration, peeling static electricity is effectively suppressed by the antistatic agent on the side of the decorative film that is laminated to the uneven molded product, so that fine foreign matter is less likely to adhere to the side of the decorative film that is laminated to the uneven molded product, and even if the decorative film is stretched and thinned during molding involving decoration, the appearance can be prevented from being impaired. [Brief description of the drawings]
[0025] [Figure 1] FIG. 2 is a side view showing the decorative film of the first embodiment. [Diagram 2] FIG. 1 is a schematic diagram showing a vacuum and pressure forming device together with a decorative film according to a first embodiment. [Diagram 3] FIG. 2 is a schematic diagram showing the inside of the vacuum and pressure molding device before molding starts. [Figure 4] FIG. 2 is a schematic view showing the inside of the vacuum and pressure molding apparatus when molding has started. [Diagram 5] 1 is a schematic diagram showing lamination of a decorative film onto a concave-convex molded product by vacuum and pressure molding. FIG. [Figure 6] 1 is a side view showing a laminated molded product that has been shaped by cutting off excess decorative film. FIG. [Figure 7] FIG. 1 is a schematic diagram showing an example of molding failure. [Figure 8] FIG. 11 is a side view showing a decorative film according to a second embodiment. [Figure 9] FIG. 2 is a side view showing an example of a decorative film laminate. [Figure 10] FIG. 11 is a side view showing another example of a decorative film laminate. [Figure 11] FIG. 4 is a schematic diagram showing a decorative film according to a second embodiment and a molding device used for molding the film. [Figure 12] FIG. 11 is a schematic diagram showing the formation of a decorative film according to a second embodiment. [Figure 13] FIG. 11 is a side view showing a decorative film according to a second embodiment after excess portions have been cut off and shaped. [Figure 14] FIG. 11 is a schematic diagram showing an injection molding die in an open state on which a decorative film of a second embodiment is arranged after molding. [Figure 15] FIG. 11 is a schematic diagram showing an injection molding die in a closed state on which a decorative film of a second embodiment is arranged after molding. [Figure 16] FIG. 11 is a schematic diagram showing the injection of resin into an injection mold in which a decorative film of the second embodiment is arranged after molding. [Figure 17] FIG. 2 is a schematic diagram showing the removal of a laminate molded product from an injection mold. [Figure 18] FIG. 2 is a side view showing the decorative film of Example 1. [Figure 19] FIG. 11 is a side view showing a decorative film and a laminate thereof according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. Note that the dimensional proportions in the drawings are exaggerated for the convenience of explanation and differ from the actual proportions.
[0027] <<Decorative film 10 according to the first embodiment>> 1, the decorative film 10 of the first embodiment has, in the lamination direction, a film substrate 11 and an adhesive layer 12 in this order. In addition, a release liner 20 is releasably disposed on the adhesive layer 12.
[0028] <Film base material 11> The film substrate 11 can be stretched. The thickness of the film substrate 11 is not particularly limited, but is, for example, from 10 μm to 10,000 μm before stretching and from 1 μm to 1,000 μm after stretching.
[0029] Examples of resin materials having excellent stretchability that form the film substrate 11 include, but are not limited to, polyethylene, non-oriented polypropylene, acrylic resin, vinyl chloride resin, acrylic urethane resin, and polyurethane resin. Among them, the film substrate is more preferably a urethane resin or a urethane acrylic resin, and even more preferably an acrylic urethane resin. The film substrate 11 also has a decorative property for decorating the surface of the molded product.
[0030] There is no particular limitation on how to impart decorativeness to the film substrate 11, and for example, the film substrate 11 may contain a colorant. There is no particular limitation on the colorant, and conventionally known knowledge may be appropriately referred to, and examples of the colorant include organic pigments such as quinacridones, anthraquinones, perylenes, perinones, diketopyrrolopyrroles, isoindolinones, condensed azos, benzimidazolones, monoazos, insoluble azos, naphthols, flavanthrones, anthrapyrimidines, quinophthalones, pyranthrones, pyrazolones, thioindigos, anthanthrones, dioxazines, phthalocyanines, and indanthrones; metal complexes such as nickel dioxin yellow and copper azomethine yellow; metal oxides such as titanium oxide, iron oxide, and zinc oxide; metal salts such as barium sulfate and calcium carbonate; and pigments such as carbon black, aluminum materials, pearl pigments, and glass materials.
[0031] Furthermore, the film substrate 11 is not limited to a form in which decorativeness is imparted to the constituent material itself, but may be in other forms, such as a form in which a decorative layer is provided directly on the film substrate 11; a support substrate is provided on the film substrate and a decorative layer is formed on the surface of the support substrate, etc.
[0032] In the latter embodiment, a resin film is preferred as the supporting substrate. Here, as the resin film, for example, a film made of a resin such as polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyvinyl chloride, polystyrene, polyurethane, polycarbonate, polyamide, polyimide, polymethyl methacrylate, polybutene, polybutadiene, polymethylpentene, ethylene vinyl acetate copolymer, ethylene (meth)acrylic acid copolymer, ethylene (meth)acrylic acid ester copolymer, ABS resin, ionomer resin, foam film, or a laminate film thereof can be used. Among these, a film made of polyvinyl chloride is preferred from the viewpoint of excellent curved surface conformability. When the supporting substrate is made of a resin film, the supporting substrate may be opaque or transparent. In addition, a through hole may be formed in the supporting substrate as necessary.
[0033] The decorative layer formed on the surface of the supporting substrate is provided on the front side of the supporting substrate when the supporting substrate is opaque, but when the supporting substrate is transparent, it may be provided on either side (front side, back side) of the supporting substrate or on both sides.
[0034] The decorative layer is not particularly limited, and may be one color or may display a color-coded pattern of two or more colors. The pattern may be a predetermined pattern, a photograph, a letter, or a number. The method of forming the decorative layer is not particularly limited, and the decorative layer can be formed by, for example, printing, printing, coating of paint, transfer from a transfer sheet, deposition, sputtering, or other methods. The supporting substrate may have an undercoat layer such as an easy-adhesion coat or a gloss adjustment coat for forming the decorative layer, or a topcoat layer such as a hard coat, an anti-stain coat, or a coat for adjusting surface roughness and specular gloss. The decorative layer, undercoat layer, or topcoat layer may be formed on the entire surface of the supporting substrate, or may be formed partially.
[0035] <Adhesive layer 12> The adhesive layer 12 is a layer containing an adhesive. There are no particular limitations on the specific composition of the adhesive contained in the adhesive layer 12. In addition, when selecting an adhesive, it is advisable to take into consideration the material of the adherend, and either an adhesive or a pressure-sensitive adhesive may be used. In the present invention, the adhesive includes a pressure-sensitive adhesive (pressure-sensitive adhesive).
[0036] Examples of adhesives include acrylic adhesives, silicone adhesives, rubber adhesives, polyester adhesives, and hot melt adhesives, and these adhesives may be either solvent type or emulsion type.
[0037] Alternatively, a chemically reactive adhesive may be used. Here, the chemically reactive adhesive refers to an adhesive of a type in which the constituent components are polymerized and solidified by a chemical reaction, and specific examples thereof include a heat-curing adhesive that initiates a chemical reaction when heat is applied from the outside, and a light / electron beam curing adhesive that initiates a chemical reaction when irradiated with visible light, ultraviolet light, electron beams, etc. A specific example of a heat-curing adhesive is an epoxy adhesive, and a specific example of a light / electron beam curing adhesive is polyester acrylate.
[0038] The thickness of the adhesive layer 12 is not particularly limited, but is preferably 5 to 100 μm, and more preferably 15 to 50 μm. The thickness of the adhesive layer 12 is appropriately selected and set depending on the size of the irregularities on the surface of the molded article to be adhered.
[0039] The adhesive layer 12 may further contain other additives that are conventionally known. Examples of such additives include tackifiers, fillers, and antioxidants. Examples of tackifiers include natural resins such as rosin resins and polyterpene resins, petroleum resins such as C5, C9, and dicyclopentadiene resins, and synthetic resins such as coumarone-indene resins and xylene resins. Examples of fillers include zinc oxide, silica, and calcium carbonate. Titanium dioxide can also function as a filler.
[0040] <Release liner 20> The release liner 20 has a base layer 21 and an antistatic layer 22 in this order in the lamination direction. In this embodiment, the base layer 21 is provided on the adhesive layer 12 side, but conversely, the antistatic layer 22 and base layer 21 may be laminated in this order from the adhesive layer 12 side. A preferred embodiment is one in which the antistatic layer 22 and base layer 21 are laminated in this order from the adhesive layer 12 side. A layer of a release agent (not shown), such as silicone, may be formed on the surface of the release liner 20 on the adhesive layer 12 side to improve releasability.
[0041] The base material layer 21 is formed of a plastic film such as, for example, a polyester film such as polyethylene terephthalate, polybutylene terephthalate, or polyethylene naphthalate, or a polyolefin film such as polypropylene or polyethylene, but is not limited to these, and may be formed of a paper base material such as glassine paper, kraft paper, fine paper, or clay-coated paper.
[0042] The antistatic layer 22 is a layer containing an antistatic agent. Examples of the antistatic agent include cationic antistatic agents having cationic functional groups such as quaternary ammonium salts, pyridinium salts, and primary, secondary, and tertiary amino groups; anionic antistatic agents having anionic functional groups such as sulfonates, sulfates, phosphonates, and phosphates; amphoteric antistatic agents such as alkylbetaines and their derivatives, imidazolines and their derivatives, and alanines and their derivatives; nonionic antistatic agents such as aminoalcohols and their derivatives, glycerin and its derivatives, and polyethylene glycol and its derivatives; ionic conductive polymers obtained by polymerizing or copolymerizing monomers having the above-mentioned cationic, anionic, and amphoteric ion conductive groups; polypyrrole-based conductive polymers, polythiophene-based conductive polymers, polyaniline-based conductive polymers, and polyacetylene-based conductive polymers; and conductive polymers such as polypyrrole-based conductive polymers and polythiophene-based conductive polymers. These compounds may be used alone or in combination of two or more.
[0043] Considering the stretchability of the film, the antistatic layer 22 is preferably an antistatic coating layer. Such an antistatic coating layer can be formed by using a coating liquid in which an antistatic agent is dissolved or dispersed in a solvent. For example, a polypyrrole-based conductive polymer can be used as a water-dispersible conductive polymer obtained by emulsion polymerization of pyrrole (monomer). A coating liquid is prepared by adding a binder resin to the water-dispersible conductive polymer as necessary, and the coating liquid is applied, heated, and dried to form an antistatic layer.
[0044] The antistatic layer 22 may also contain a binder resin. Examples of the binder resin include polyester resins, acrylic resins, polyvinyl resins, urethane resins, melamine resins, and epoxy resins. A crosslinking agent may also be used in combination. Examples of the crosslinking agent include methylolated or alkylolated melamine compounds, urea compounds, glyoxal compounds, acrylamide compounds, epoxy compounds, and isocyanate compounds.
[0045] The antistatic layer 22 has a thickness of, for example, 0.01 μm to 5 μm, but is not particularly limited as long as it can exhibit an antistatic effect. Furthermore, the antistatic layer 22 may contain at least one kind of additive, such as a defoamer, a coatability improver, a thickener, an organic lubricant, organic particles, or inorganic particles, as necessary.
[0046] <<Manufacturing method of laminated molded product according to the first embodiment>> In the manufacturing method of the laminate molded product of the first embodiment, the decorative film 10 and the release liner 20 are peeled off, and then the decorative film 10 is laminated and adhered to the surface of the molded product to be decorated by vacuum and pressure forming.
[0047] 2, in this embodiment, the decorative film 10 is set in a molding device 100 for performing vacuum and pressure forming after the release liner 20 is peeled off, and is laminated and adhered to the surface of the uneven molded product 1 to be decorated. The material for forming the uneven molded product 1 is, for example, a resin such as polypropylene, acrylonitrile-butadiene-styrene copolymer resin (ABS resin), polycarbonate, acrylic resin, etc., but is not limited to these, and may also be a metal.
[0048] The molding apparatus 100 has a lower mold 101, an upper mold 102, a table 103, a heating means 104, a pressurizing means 105, and a vacuum means 110. The lower mold 101 and the upper mold 102 can move toward and away from each other. The table 103 is provided inside the lower mold 101, and can move up and down inside the lower mold 101. The heating means 104 is provided inside the upper mold 102. The pressurizing means 105 is provided below the heating means 104 inside the upper mold 102. The vacuum means 110 is, for example, a vacuum pump, and is connected to the insides of the lower mold 101 and the upper mold 102.
[0049] 3, the decorative film 10 set in the molding device 100 is sandwiched at its ends between a lower die 101 and an upper die 102 and held in a stretched state away from the uneven molded product 1. In this state, vacuum and pressure molding is performed, and the decorative film 10 is laminated and adhered to the surface of the uneven molded product 1.
[0050] The vacuum pressure molding performed by the molding apparatus 100 is a method in which a vacuum is created inside the molding apparatus 100, the decorative film 10 is softened, and pressure is applied to the space opposite the space between the decorative film 10 and the uneven molded product 1, thereby pressing the decorative film 10 against the uneven molded product 1 to mold it.
[0051] 4, in this embodiment, the vacuum means 110 draws a vacuum inside the molding device 100, and the table 103 moves upward to bring the decorative film 10 and the uneven molded product 1 close to each other, while the heating means 104 heats and softens the decorative film 10. In addition, the pressure means 105 introduces air or an inert gas (nitrogen gas, argon gas, helium gas, etc.) into the upper mold 102, and pressurizes the space inside the upper mold 102 to a higher pressure than the space inside the lower mold 101.
[0052] 5, the decorative film 10 is stretched and thinned while being laminated along the shape of the uneven molded product 1. The heating conditions under which the decorative film 10 is softened to an extent that it can sufficiently follow the shape of the uneven molded product 1 are appropriately set depending on the materials of the film substrate 11, the adhesive layer 12, etc., and are not particularly limited, but are, for example, a heating temperature of 50 to 200° C. and a heating time of 0.1 to 10 minutes.
[0053] After the decorative film 10 is laminated onto the uneven molded product 1, the introduction of air or inert gas into the upper mold 102 is stopped, the upper mold 102 and the lower mold 101 are separated, and the uneven molded product 1 together with the decorative film 10 is removed.
[0054] Then, as shown in Figure 6, any excess portion of the decorative film 10 that extends beyond the uneven molded product 1 is cut off using an appropriate cutting means such as a thermocutter or a cutter, and a laminated molded product 2 is completed in which the decorative film 10 is adhered to the uneven molded product 1.
[0055] In this embodiment, the decorative film 10 is laminated and adhered to the surface of the uneven molded product 1 by vacuum and pressure forming, but is not limited thereto. The decorative film 10 may be laminated and adhered to the surface of the uneven molded product 1 by, for example, vacuum forming or pressure forming.
[0056] In vacuum and pressure forming, the heated and softened decorative film 10 is subjected to a reduction in pressure on the side of the uneven molded product 1 and pressure from the opposite side to the uneven molded product 1, but in vacuum forming, the same pressure is not applied, and the decorative film 10 is laminated and bonded to the surface of the uneven molded product 1 by reducing the pressure on the side of the uneven molded product 1. On the other hand, in pressure forming, the heated and softened decorative film 10 is not reduced in pressure on the side of the uneven molded product 1, and pressure is applied from the opposite side to the uneven molded product 1 to laminate and bond the decorative film 10 to the surface of the uneven molded product 1.
[0057] Next, the effects of this embodiment will be described.
[0058] In this embodiment, the release liner 20 is peeled off before the decorative film 10 is used. However, unlike this embodiment, if the release liner 20 does not contain an antistatic agent, peeling static electricity will occur on the side of the decorative film 10 that is laminated to the uneven molded product 1, and foreign matter such as fine dust and dirt will easily adhere to the side of the decorative film 10 that is laminated to the uneven molded product 1.
[0059] As shown in Fig. 7, even if the decorative film 10 is laminated on the uneven molded product 1 with fine foreign matter A attached thereto, if the decorative film 10 is thick, the shape of the foreign matter A is unlikely to stand out, but since the decorative film 10 is stretched and thinned by vacuum pressure molding, the shape of the foreign matter A is likely to stand out as shown in the figure. In particular, if the diameter of the foreign matter A is, for example, 20 μm or more, the shape of the foreign matter A is likely to stand out, and there is a risk of impairing the appearance.
[0060] On the other hand, in this embodiment, the release liner 20 contains an antistatic agent, which effectively suppresses peel static electricity on the side of the decorative film 10 that is laminated to the uneven molded product 1, making it difficult for fine foreign matter A to adhere to the side of the decorative film 10 that is laminated to the uneven molded product 1, and preventing damage to the appearance even if the decorative film 10 is stretched and thinned by vacuum and pressure molding.
[0061] As long as the adhesion of foreign matter A is suppressed, the absolute value of the electrostatic potential on the side of the decorative film 10 that is laminated to the uneven molded product 1 is not particularly limited, but may be, for example, 0.5 kV or less, 0.3 kV or less, or 0.1 kV or less.
[0062] For example, immediately after the decorative film 10 and the release liner 20 are peeled off from one side of the decorative film 10, if the absolute value of the electrostatic potential on that side (the side that will be laminated to the uneven molded product 1 (the adhesive layer 12 side)) is 0.5 kV or less, foreign matter A that is prone to protruding, for example having a shape that is 20 μm or larger, is less likely to adhere to the adhesive layer 12 side of the decorative film 10, and damage to the appearance can be more effectively prevented.
[0063] Next, the decorative film 10A and decorative film laminate 1000 of the second embodiment, and a method for producing the laminate molded product of the second embodiment will be described.
[0064] <<Decorative film 10A and decorative film laminate 1000 according to the second embodiment>> 8, the decorative film 10A of the second embodiment differs from the first embodiment in that a resin layer 30 is laminated instead of the release liner 20, and in that an antistatic layer 40 is provided between the film substrate 11 and the adhesive layer 12. The film substrate 11 and the adhesive layer 12 are the same as those of the first embodiment.
[0065] The resin layer 30 is adhered and fixed to one side of the film substrate 11 via the adhesive layer 12, and is non-removable, unlike the release liner 20 of the first embodiment. The material for forming the resin layer 30 is not particularly limited as long as it is a resin that can be adhered to the concave-convex molded article 1 by heating and melting, and specific examples of the material include resins such as ethylene-α-olefin copolymers, ethylene-vinyl acetate copolymers, and thermoplastic polyesters.
[0066] The antistatic layer 40 is a layer containing an antistatic agent, and is provided on the side of the film substrate 11 that is to be laminated to the uneven molded article 1. The antistatic layer 40 is provided integrally with the film substrate 11 and cannot be peeled off. The constituent material and thickness of the antistatic layer 40 are similar to those of the antistatic layer 22 in the first embodiment, for example.
[0067] As shown in Fig. 9, the decorative film laminate 1000 of this embodiment has a configuration in which decorative films 10A are laminated. The laminated decorative films 10A are directly laminated with each other without any film or the like therebetween. Since the film base material 11, the antistatic layer 40, the adhesive layer 12, and the resin layer 30 laminated in each decorative film 10A are inseparable from each other, in the decorative film laminate 1000, the decorative films 10A can be peeled off only between the decorative films 10A.
[0068] In the decorative film laminate 1000, the sheet-shaped decorative film 10A is laminated, but the present invention is not limited to this form. For example, as shown in the modified example in Fig. 10, a roll-shaped decorative film laminate 1000A in which a long decorative film 10A is wound is also included in the scope of the present invention.
[0069] <<Manufacturing method of laminated molded product according to the second embodiment>> In this embodiment, a laminated molded product is produced by film insert molding. In film insert molding, molding of the decorative film 10A and lamination of the decorative film 10A on the concave-convex molded product 1 are not performed simultaneously as in the first embodiment, but the decorative film 10A is molded first, and then the molded decorative film 10A is laminated integrally with the concave-convex molded product 1.
[0070] As shown in Fig. 11, the molding apparatus 100A used to mold the decorative film 10A has a lower mold 101A different from that of the first embodiment. As for other configurations, the molding apparatus 100A is substantially similar to the molding apparatus 100 of the first embodiment, and the same reference numerals as those of the first embodiment are used for the common configurations, and the duplicated explanations are omitted.
[0071] The lower mold 101A of this embodiment does not have the uneven molded product 1 as in the first embodiment, but has a convex portion 106A having the same shape as the uneven molded product 1. The lower mold 101A and the upper mold 102 sandwich and hold the decorative film 10A in a stretched state.
[0072] As shown in Figure 12, while the inside of the molding apparatus 100A is evacuated by the vacuum means 110, the decorative film 10A is softened by heating by the heating means 104 and pressurized by air or inert gas introduced from the upper mold 102 side, and is molded by being stretched and adhered closely to the convex portion 106A.
[0073] Without being limited to this type of vacuum pressure molding, the decorative film 10A may be adhered to the convex portion 106A by vacuum molding in which a vacuum is drawn from the lower die 101A side without applying pressure from the upper die 102 side, or by pressure molding in which pressure is drawn from the upper die 102 side without applying vacuum from the lower die 101A side.
[0074] After the decorative film 10A is formed, the lower die 101A and the upper die 102 are opened and relatively separated from each other, and the formed decorative film 10A is removed from the forming apparatus 100A.
[0075] As shown in FIG. 13, the decorative film 10A after molding is taken out, and excess portions not used for decoration are cut off using a suitable cutting means such as a thermo-cutter or a cutter, to adjust the shape.
[0076] 14, the decorative film 10A is set in an injection molding die 200. The injection molding die 200 has a first die 210 and a second die 220 that are relatively close to each other and spaced apart from each other.
[0077] The first die 210 is provided with a recess 211 having the same shape as the outer shape of the molded decorative film 10A. The second die 220 is provided with a protrusion 221 and a runner 222 into which resin is injected.
[0078] With the first die 210 and the second die 220 open, the decorative film 10A is placed in the recess 211, and after the decorative film 10A is set, the first die 210 and the second die 220 are closed in relatively close proximity.
[0079] 15, when the first mold 210 and the second mold 220 are closed, a cavity 201, which is a gap communicating with the runner 222, is formed between the decorative film 10A and the protrusion 221. After the cavity 201 is formed, injection molding is performed.
[0080] As shown in FIG. 16, in injection molding, heated and molten resin 202 is filled from a runner 222 into a cavity 201 beyond it, and then the resin 202 filled in the cavity 201 is cooled and hardened to form a concave-convex molded product 1.
[0081] The concave-convex molded product 1 is formed by injection molding, and is laminated integrally with the decorative film 10A so as not to be peeled off. It is preferable to form the resin layer 30 of the decorative film 10A, which is in contact with the concave-convex molded product 1, from the same resin as the concave-convex molded product 1, since this effectively increases the adhesive strength between the concave-convex molded product 1 and the decorative film 10A. The resin forming the concave-convex molded product 1 and the resin layer 30 is, for example, polypropylene, but is not limited thereto.
[0082] After injection molding, as shown in FIG. 17, the first mold 210 and the second mold 220 are separated from each other and opened, and the laminated molded product 2 in which the concave-convex molded product 1 and the decorative film 10A are laminated and integrated is removed.
[0083] Next, the effects of this embodiment will be described.
[0084] The decorative film 10A is used by peeling it off from the decorative film laminate 1000 (1000A), but because the antistatic layer 40 contains an antistatic agent, when the decorative film 10A is peeled off from the decorative film laminate 1000 (1000A), peel electrification is effectively suppressed on the side that is laminated to the uneven molded product 1, so that minute foreign matter is less likely to adhere to the side that is laminated to the uneven molded product 1. Therefore, even if the decorative film 10A is stretched and thinned during molding, it is possible to prevent poor appearance caused by minute foreign matter.
[0085] As long as the adhesion of fine foreign matter is suppressed, the absolute value of the electrostatic potential on the side of the decorative film 10A that is laminated to the uneven molded product 1 is not particularly limited, but may be, for example, 0.5 kV or less, or 0.3 kV or less, or 0.1 kV or less, and the effect obtained thereby is the same as in the first embodiment.
[0086] In this embodiment, the decorative film 10A is provided with a resin layer 30, and the decorative film 10A adheres well to the resin 202 injected by injection molding, thereby increasing the adhesive strength between the concave-convex molded product 1 and the decorative film 10A.
[0087] Next, examples and comparative examples will be described.
[0088] <Example 1 and Comparative Example 1> 18, the decorative film 50 of Example 1 has a film substrate 51, an antistatic layer 52, an adhesive layer 53 (acrylic adhesive, thickness 30 μm), and a release liner 54, in this order in the lamination direction. The decorative film 50 of Example 1 also has a process film 55 on the side of the film substrate 51 opposite to the side to be laminated to the uneven molded product.
[0089] The film substrate 51 is made of acrylic urethane (thickness 170 μm). The release liner 54 is made of polyethylene terephthalate (PET) (thickness 50 μm), and the surface on the adhesive layer 53 side is silicone-treated.
[0090] The antistatic layer 52 is prepared by adding a butylated melamine resin (2 parts by mass, manufactured by DIC Corporation, product name "Super Beckamine (registered trademark) J820-60") as a binder resin to an emulsion containing a polypyrrole-based conductive polymer (100 parts by mass (solids)) obtained by emulsion polymerization of pyrrole (monomer), and thoroughly mixing the mixture to obtain a coating liquid for forming an antistatic layer. One side of the film substrate is then exposed to corona irradiation, the above-mentioned coating liquid for forming an antistatic layer is applied to the same side, and the coating liquid is dried by heating to form an antistatic layer having a thickness of 50 nm.
[0091] The processing film 55 is releasably disposed on the film substrate 51 on the side opposite to the release liner 54. The processing film 55 is made of polyethylene terephthalate (PET) and has a thickness of 100 μm.
[0092] The processing film 55 protects the film substrate 51, making it difficult for the film substrate 51 to be scratched and preventing the decorativeness from being damaged. The processing film 55 is peeled off before the decorative film 50 is laminated onto the concave-convex molded product.
[0093] For comparison with the decorative film 50 of Example 1, the present inventors prepared a decorative film of Comparative Example 1 in which the antistatic layer 52 was omitted from the decorative film 50. Example 1 and Comparative Example 1 are similar except for the presence or absence of the antistatic layer 52.
[0094] In Example 1, the inventor peeled off the release liner 54 from the decorative film 50, and then measured the electrostatic potential on the side that was to be laminated to the concave-convex molded product (the adhesive layer 53 side). The electrostatic potential was also measured in the same manner in Comparative Example 2. A static electricity meter FMX-003 manufactured by SIMCO JAPAN was used to measure the electrostatic potential. The measurement results are shown in Table 1 below.
[0095] [Table 1]
[0096] As shown in Table 1, the electrostatic potential in Example 1 was significantly reduced compared to Comparative Example 1, and it was confirmed that by providing the antistatic layer 52, peel-off static electricity can be effectively suppressed on the side of the decorative film 50 that is laminated to the uneven molded product when the release liner 54 is peeled off.
[0097] <Example 2 and Comparative Example 2> As shown in FIG. 19, in Example 2, the present inventors used a laminate 1000B including a decorative film 10B, and confirmed the effect of reducing peel electrification that occurs when the decorative film 10B is peeled off therefrom.
[0098] The decorative film 10B has a configuration according to the second embodiment, and includes, in the stacking direction, a film substrate 11, an antistatic layer 40, an adhesive layer 12, and a resin layer 30. In addition to these, the decorative film 10B further includes a process film 55B.
[0099] The processing film 55B is disposed on the opposite side of the film substrate 11 from the side (resin layer 30 side) to be laminated to the concave-convex molded product, so as to be peelable from the film substrate 11. The processing film 55B is made of polyethylene terephthalate (PET).
[0100] For comparison with Example 2, the present inventors prepared a decorative film of Comparative Example 2 in which the antistatic layer 40 was removed from the decorative film 10B, and also prepared a decorative film laminate by laminating the decorative film. Example 2 and Comparative Example 2 are similar except for the presence or absence of the antistatic layer 40.
[0101] In Example 1, the inventor peeled off one decorative film 10B located at the top end in the lamination direction of the decorative film laminate 1000B, and measured the electrostatic potential of the peeled off decorative film 10B on the side that was to be laminated to the uneven molded product (the resin layer 30 side). The electrostatic potential was also measured in the same manner in Comparative Example 2. The measurement results are shown in Table 2 below.
[0102] [Table 2]
[0103] As shown in Table 2, the electrostatic potential in Example 2 was significantly reduced compared to Comparative Example 2, and it was confirmed that by providing the antistatic layer 40, when the decorative film 10B is peeled off from the decorative film laminate 1000B, peel-off electrostatic charge can be effectively suppressed on the side of the decorative film 10B that is laminated to the uneven molded product (the resin layer 30 side).
[0104] The present invention is not limited to the above-described embodiments and examples, and can be modified in various ways within the scope of the claims.
[0105] For example, the shape of the uneven molded product is not limited to a dome shape as in the above embodiment, and may be another three-dimensional shape. In addition, there is no particular limitation on the application for which the uneven molded product is used.
[0106] Furthermore, the antistatic agent may be contained in a layer that is overlaid on the side of the film substrate that is to be laminated to the uneven molded product. In addition to or without the antistatic layers 22, 40, and 52 disclosed in the above embodiments and examples, the antistatic agent may be contained in other layers, such as the adhesive layers 12, 53, the resin layer 30, and the release liner 54.
[0107] Furthermore, in the above-mentioned embodiments and examples, the film substrates 11 and 51 may also contain an antistatic agent, which is also within the scope of the present invention.
[0108] If the film substrate 11, 51 also contains an antistatic agent, static electricity is effectively suppressed on the front side opposite the side that is laminated to the uneven molded product, and dirt and dust in the air are less likely to adhere to the surface, so that the appearance of the article having the decorative film on its surface can be kept clean.
[0109] Furthermore, by incorporating an antistatic agent into the film substrates 11 and 51, static electricity can be effectively suppressed on the front side opposite the side that is laminated to the concave-convex molded product, and discharge to the human body can be effectively prevented. [Explanation of symbols]
[0110] 1 Concave and convex molded products, 2 Laminated moldings, 10, 10A, 10B, 50 decorative film, 11, 51 Film substrate, 12, 53 adhesive layer, 20, 54 Release liner, 21 base material layer, 22, 40, 52 Antistatic layer, 30 resin layer, 55, 55B process film, 100, 100A molding device, 101, 101A lower mold, 102 upper mold, 103 tables, 104 heating means, 105 Pressurizing means, 106A convex part, 110 vacuum means, 200 injection mold, 202 Resin, 210 First type, 211 recess, 220 Second type, 221 Convex part, 222 runners, 1000, 1000A, 1000B Decorative film laminate, A tiny foreign object.
Claims
1. A method for producing a laminated molded product, comprising laminating a decorative film having a stretchable film substrate on a surface of a concave-convex molded product, At least one of the layers to be laminated on the side of the film substrate that is to be laminated on the uneven molded product contains an antistatic agent; Peeling off the release liner disposed as the peelable layer from the decorative film, or peeling off the decorative films laminated together; The decorative film is stretched and laminated on the surface of the uneven molded product.
2. The method for producing a laminate molded product according to claim 1 , further comprising the step of: adding an antistatic agent to the film substrate.
3. The method for producing a laminated molded product according to claim 1 or claim 2, wherein a process film is arranged on the side of the film substrate opposite to the side to be laminated to the uneven molded product, and the process film is peeled off before the decorative film is stretched.
4. 3. The method for manufacturing a laminated molded product according to claim 1, wherein immediately after the decorative film is peeled off from the release liner, or immediately after the laminated decorative films are peeled off from each other, the absolute value of the electrostatic potential on the side of the decorative film that is laminated to the uneven molded product is 0.5 kV or less.
5. The present invention has a stretchable film substrate and a layer superposed on one side of the film substrate, and includes a release liner as the peelable layer, A decorative film comprising an antistatic agent in said layer.
6. The decorative film according to claim 5 , further comprising an antistatic agent in the film substrate.
7. 7. The decorative film according to claim 5, further comprising a peelable processing film disposed on the surface opposite to the one surface on which the release liner is disposed.
8. 7. The decorative film according to claim 5, wherein the absolute value of the electrostatic potential on said one surface side is 0.5 kV or less when said release liner is peeled off.
9. A decorative film having a film base material that can be stretched to fit the shape of the uneven molded product is laminated in multiple layers. The decorative film is At least one of the layers to be laminated on the side of the film substrate that is to be laminated on the uneven molded product contains an antistatic agent, The decorative film is in direct contact with the adjacent decorative film in the lamination direction, and is laminated so as to be peelable only between the decorative films that are in direct contact with each other, or A peelable process film is arranged on the surface opposite to the side laminated to the uneven molded product, and is laminated in direct peelable contact with the process film arranged on the adjacent decorative film in the lamination direction.
10. The decorative film laminate according to claim 9 , wherein the decorative film further comprises an antistatic agent in the film substrate.
11. 11. The decorative film laminate according to claim 9, wherein the process film is disposed on the decorative film.
12. 11. The decorative film laminate according to claim 9 or 10, wherein the decorative film has a resin layer laminated in an inseamless manner via an adhesive layer as the layer to be laminated on the side to be laminated on the uneven molded article.
13. 11. The decorative film laminate according to claim 9, wherein the absolute value of the electrostatic potential generated on the side of the decorative film peeled off from the decorative film laminate that is laminated on the uneven molded product is 0.5 kV or less.
Citation Information
Patent Citations
Film for molding and molding transfer foil using the same
JP2017214559A