Fuel electrode for electrochemical cell, method of manufacturing fuel electrode for electrochemical cell, and electrochemical cell

A fuel electrode with electronically and ionically conductive oxide particles and a mixed conductive oxide composition addresses Ni-related degradation issues, achieving high performance and reduced Ni usage in SOFC and SOEC cells.

JP2024132567AInactive Publication Date: 2024-10-01KK TOYOTA CHUO KENKYUSHO
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023043390
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional fuel electrodes for SOFC and SOEC suffer from performance degradation due to the oxidation and reduction of metallic Ni, leading to electrode damage and reduced catalytic activity, and are economically costly.

Method used

A fuel electrode composed of electronically conductive oxide particles, ion conductive oxide particles, and a mixed conductive oxide with specific compositional formulas, supported on the surfaces of these particles, reducing the amount of Ni used while maintaining high power generation and water electrolysis performance.

Benefits of technology

The proposed fuel electrode achieves high power generation and water electrolysis performance, improving durability and reducing Ni usage, thereby enhancing the performance and cost-effectiveness of both SOFC and SOEC cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132567000001
    Figure 2024132567000001
  • Figure 2024132567000002
    Figure 2024132567000002
  • Figure 2024132567000003
    Figure 2024132567000003
Patent Text Reader

Abstract

To provide a fuel electrode for an electrochemical cell, which, while sufficiently reducing the usage of Ni, can exhibit a sufficiently high level of power generation performance when used as a fuel electrode for a SOFC and also can exhibit a sufficiently high level of water electrolysis performance when used as a fuel electrode for a SOEC, and which can be used for both SOFC and SOEC cells.SOLUTION: There is provided a fuel electrode for an electrochemical cell, which comprises electronically conductive oxide particles, ion conductive oxide particles, and a mixed conductive oxide represented by the following compositional formula (1): (Ce1-x-yGdxNiy)O2 (1) [In the formula, x represents a numerical value within the range of 0.02- 0.3, and y represents a numerical value within the range of 0.02- 0.3.].SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anode for an electrochemical cell, a method for producing an anode for an electrochemical cell, and an electrochemical cell. [Background technology]

[0002] In recent years, as the promotion of carbon neutrality is being called for, electrochemical cells have been attracting attention as a technology for generating electricity using hydrogen and a technology for generating hydrogen. As such electrochemical cells, solid oxide fuel cells (SOFCs) and solid oxide electrochemical cells (SOECs) are known, and since these can generate electricity or generate hydrogen with high efficiency, they are attracting particular attention as next-generation energy devices. As such electrochemical cells, there are known ones that use an oxide ion conductor (e.g., yttria-stabilized zirconia (YSZ) or the like) as a solid electrolyte, and have a configuration in which a fuel electrode containing a porous body is arranged on one side of the solid electrolyte, and an air electrode is arranged on the other side.

[0003] Conventionally, a mixture of an oxide ion conductor (e.g., YSZ, etc.) and metallic Ni has been mainly used as the fuel electrode used in such an electrochemical cell. Since metallic Ni has high electronic conductivity and also has high activity as an electrochemical catalyst, it is known that its use can provide high performance (high output performance in the case of SOFC). However, when considering the use of a fuel electrode made of such a mixture in an SOFC, metallic Ni is a component that is easily oxidized and reduced. For example, when the fuel surplus is reduced and the fuel utilization rate is high, when a fuel shortage occurs locally, the oxygen partial pressure increases, causing the metallic Ni to be oxidized and expand, and then, when the fuel shortage is resolved, the metallic Ni is reduced and contracts. In this way, when an actual SOFC is operated, the metallic Ni is alternately oxidized and reduced, causing the metallic Ni to expand and contract. If such expansion and contraction are repeated, the joint between the electrode components in the fuel electrode is damaged, and the performance of the SOFC is reduced. Thus, when the fuel electrode made of the mixture is used in an SOFC, there is a problem that the performance of the SOFC is reduced due to damage to the components caused by the use of metallic Ni. On the other hand, when the fuel electrode made of the mixture is used in an SOEC, the fuel electrode is exposed to an atmosphere with a high concentration of water vapor during use, and in that case, problems such as Ni(OH)2 being generated by the reaction between metallic Ni and water vapor, some of which scatter and cause the electrode material to dissipate, and problems such as Ni coagulation and enlargement due to water vapor causing damage to the joints of the electrode components, a reduction in the three-phase interface, and a decrease in catalytic activity occur, which causes problems such as a decrease in the performance of the SOEC. In addition, the use of metallic Ni has problems such as cell damage as described above, and since Ni itself is an economically expensive component, in recent years, there has been a demand to reduce the amount of Ni used.

[0004] In order to address the problems associated with metallic Ni as described above, a technology that uses an oxide of Ni instead of metallic Ni is proposed in, for example, JP 2012-33418 A (Patent Document 1). The technology proposes the use of a fuel electrode for an SOFC, which includes a NiAl2O3 composite oxide film formed on at least a part of the surface of a porous sintered body made of a first oxide material having electronic conductivity and made of a perovskite-type titanate oxide mainly composed of SrTiO3, and a second oxide material having ionic conductivity and made of ZrO2 stabilized with at least one kind selected from the group consisting of Y2O3, Sc2O3, and Yb2O3 (see Example 1, etc.).

[0005] Meanwhile, in recent years, the future use of solid oxide reversible type fuel cell (SORC) systems, which perform both power generation and hydrogen production in the same cell, has also been proposed, and it is expected that the fuel electrodes of both SOFC and SOEC cells will be made of the same material and have the same structure.

[0006] In light of this, in the field of electrochemical cells, there is a need for a new anode structure that can reduce the amount of Ni used while exhibiting excellent power generation characteristics when used as an anode for SOFCs and excellent water electrolysis performance when used as an anode for SOECs. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2012-33418 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and has an object to provide an electrochemical cell fuel electrode that can be used in both SOFC and SOEC cells, and that can exhibit a sufficiently high level of power generation performance when used as a fuel electrode for SOFCs and a sufficiently high level of water electrolysis performance when used as a fuel electrode for SOECs, while sufficiently reducing the amount of Ni used; a manufacturing method for an electrochemical cell fuel electrode that can efficiently manufacture such an electrochemical cell fuel electrode; and an electrochemical cell using the electrochemical cell fuel electrode. [Means for solving the problem]

[0009] As a result of intensive research conducted by the inventors in order to achieve the above-mentioned object, they have found that by making an electrochemical cell fuel electrode composed of electronically conductive oxide particles, ionically conductive oxide particles, and a mixed conductive oxide represented by the following composition formula (1), it is possible to sufficiently reduce the amount of Ni used while exhibiting a sufficiently high level of power generation performance when used as a fuel electrode for an SOFC, and to exhibit a sufficiently high level of water electrolysis performance when used as a fuel electrode for an SOEC, and thus the present invention has been completed.

[0010] That is, the present invention provides the following aspects.

[0011] [1] Electronically conductive oxide particles; Ion-conductive oxide particles; The following composition formula (1): (Ce 1-x-y Gd x Ni y )O2(1) [In the formula, x represents a number in the range of 0.02 to 0.3, and y represents a number in the range of 0.02 to 0.3.] A mixed conducting oxide represented by A fuel electrode for an electrochemical cell comprising:

[0012] [2] The fuel electrode for an electrochemical cell according to [1], wherein the mixed conductive oxide is supported on the surfaces of the electronically conductive oxide particles and the ionically conductive oxide particles.

[0013] [3] The electronic conductive oxide particles have the following composition formula (2): La 1-z M z TiO3(2) [In the formula, M represents at least one element selected from the group consisting of Ca and Sr, and z represents a numerical value in the range of 0.4 to 0.8.] The fuel electrode for an electrochemical cell according to [1] or [2], which is made of a perovskite-type oxide represented by the following formula:

[0014] [4] The ion-conductive oxide particles have the following composition formula (3): Ce 1-n A n O2(3) [In the formula, A represents at least one element selected from the group consisting of Gd and Sm, and n represents a numerical value in the range of 0.05 to 0.3.] The fuel electrode for an electrochemical cell according to any one of [1] to [3], which is made of an oxide represented by the following formula:

[0015] [5] A step of obtaining a porous body composed of electronically conductive oxide particles and ionically conductive oxide particles; a step of impregnating the porous body with a solution containing Ce ions, Gd ions and Ni ions, and firing the resulting porous body to obtain the fuel electrode for electrochemical cells according to any one of the items [1] to [4]; A method for producing an anode for an electrochemical cell, comprising:

[0016] [6] An electrochemical cell comprising the fuel electrode for an electrochemical cell according to any one of [1] to [4], an air electrode, and a solid electrolyte layer. Effect of the Invention

[0017] According to the present invention, it is possible to provide an electrochemical cell fuel electrode that can exhibit a sufficiently high level of power generation performance when used as a fuel electrode for an SOFC, and can exhibit a sufficiently high level of water electrolysis performance when used as a fuel electrode for an SOEC, while sufficiently reducing the amount of Ni used, and that can be used in both SOFC and SOEC cells; a manufacturing method for an electrochemical cell fuel electrode that can efficiently manufacture such an electrochemical cell fuel electrode; and an electrochemical cell using the electrochemical cell fuel electrode. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a schematic cross-sectional view showing a cross section of the electrochemical cell produced in Example 1. [Diagram 2] 1 is a graph showing an XRD chart of a calcined powder formed from solution (A) obtained in Example 1 and an XRD chart of a calcined powder formed from solution (B) obtained in Example 2. [Diagram 3] 1 is a graph showing the relationship between cell voltage and generated current for the electrochemical cells obtained in Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 4] 1 is a graph showing the relationship between cell voltage and electrolysis current for the electrochemical cells obtained in Examples 1 and 2 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described in detail below based on preferred embodiments thereof.

[0020] [Fuel electrodes for electrochemical cells] The fuel electrode for an electrochemical cell of the present invention comprises: Electronically conductive oxide particles; Ion-conductive oxide particles; The following composition formula (1): (Ce 1-x-y Gd x Ni y )O2(1) [In the formula, x represents a number in the range of 0.02 to 0.3, and y represents a number in the range of 0.02 to 0.3.] A mixed conducting oxide represented by The present invention is characterized in that it comprises:

[0021] The electronically conductive oxide particles according to the present invention are not particularly limited, and any known oxide particles having electronic conductivity that are used in the field of SOFC and SOEC can be appropriately used. As such electronically conductive oxide particles, from the viewpoint of improving electronic conductivity, particles of ABO3 type perovskite oxide (Ti-containing perovskite oxide) containing Ti as an element constituting the B site are preferable. In this way, the ABO3 type perovskite oxide that can be suitably used for the electronically conductive oxide particles necessarily contains Ti as a constituent element of the B site. In this way, the ABO3 type perovskite oxide contains Ti, so that higher electronic conductivity can be expressed. In addition, the constituent element of such a B site may contain at least one element selected from the group consisting of Nb, Ta, Co, Cr, Mn, and Mo together with Ti. In addition, it is more preferable that the B site of such an ABO3 type perovskite oxide is composed of only Ti as a constituent element from the viewpoint of further improving electronic conductivity.

[0022] In addition, the element constituting the A site of the ABO3 type perovskite oxide (Ti-containing perovskite oxide) is preferably at least one element selected from the group consisting of La, Ca, Sr, Ba and Y (more preferably Ca, Sr and Ba, and even more preferably Ca and Sr). From the viewpoint of improving electronic conductivity and reduction resistance, the element constituting the A site of the ABO3 type perovskite oxide that can be suitably used for such electronically conductive oxide particles preferably contains a combination of La and at least one element selected from the group consisting of Ca and Sr.

[0023] In addition, as such electronically conductive oxide particles, the following composition formula (2): La 1-z M z TiO3(2) [In the formula, M represents at least one element selected from the group consisting of Ca and Sr, and z represents a numerical value in the range of 0.4 to 0.8.] It is more preferable that the perovskite oxide is represented by the following formula:

[0024] In the formula (2), M represents at least one element selected from the group consisting of Ca and Sr. As the element M, Sr is particularly preferable from the viewpoint of further improving electronic conductivity and reduction resistance. Thus, as the electronically conductive oxide particles, lanthanum strontium titanium composite oxide (LST) represented by the formula (2) where M is Sr can be suitably used.

[0025] Furthermore, z in the formula (2) is a value in the range of 0.4 to 0.8 (more preferably 0.5 to 0.7, and even more preferably 0.5 to 0.6). When the value of z is equal to or greater than the lower limit, a higher effect in terms of electronic conductivity tends to be obtained compared to when the value is below the lower limit, while when the value is equal to or less than the upper limit, a higher effect in terms of electronic conductivity tends to be obtained compared to when the value exceeds the upper limit.

[0026] The average particle size of the electron conductive oxide particles is not particularly limited, but is preferably 100 to 3000 nm (more preferably 300 to 1500 nm). If the average particle size is equal to or greater than the lower limit, a higher effect tends to be obtained in that more contact points with the ion conductive oxide particles and the mixed conductive oxide can be formed compared to when the average particle size is less than the lower limit, while if the average particle size is equal to or less than the upper limit, a higher effect tends to be obtained in that more contact points with the ion conductive oxide particles and the mixed conductive oxide can be formed compared to when the average particle size exceeds the upper limit. The average particle size of such electron conductive oxide particles can be measured by using a laser diffraction method.

[0027] Furthermore, the method for producing such electron conductive oxide particles is not particularly limited, and any known method can be appropriately used.

[0028] The ion-conductive oxide particles according to the present invention are not particularly limited, and any oxide particles having electronic conductivity that are known to be used in the field of SOFCs and SOECs can be appropriately used. Examples of such ion-conductive oxide particles include zirconia-based oxides such as yttria-stabilized zirconia (YSZ), scandia-stabilized zirconia (ScSZ), and calcia-stabilized zirconia (CSZ); ceria-based oxides such as gadolinia-doped ceria (GDC) and samaria (Sm2O3)-doped ceria (SDC); lanthanum gallate-based oxides (e.g., those having the formula: La 1-x Sr x Gd 1-y Mg y O3 (wherein x is a number in the range of 0.05 to 0.2, and y is a number in the range of 0.1 to 0.3); apatite-type lanthanum silicate-based oxide; or other known particles of ion-conductive oxides can be appropriately used.

[0029] Such ion-conductive oxide particles have the following composition formula (3): Ce 1-n A n O2(3) [In the formula, A represents at least one element selected from the group consisting of Gd and Sm, and n represents a numerical value in the range of 0.05 to 0.3.] It is preferable that the oxide is made of an oxide represented by the formula (ceria-based oxide).

[0030] In the formula (3), A represents at least one element selected from the group consisting of Gd and Sm. Gd is particularly preferable as the element A, because it can further improve the ionic conductivity and is also excellent in terms of cost. Thus, gadolinia-doped ceria (GDC), which is represented by the formula (3) and in which A is Gd, can be suitably used as the ion-conductive oxide particles.

[0031] Furthermore, n in formula (3) is a value in the range of 0.05 to 0.3 (more preferably 0.1 to 0.2). When the value of n is equal to or greater than the lower limit, a higher effect in terms of improving ionic conductivity tends to be obtained compared to when the value is below the lower limit, while when the value is equal to or less than the upper limit, a higher effect in terms of improving ionic conductivity tends to be obtained compared to when the value exceeds the upper limit.

[0032] The average particle size of the ion-conductive oxide particles is not particularly limited, but is preferably 100 to 3000 nm (more preferably 100 to 1000 nm). If the average particle size is equal to or greater than the lower limit, a higher effect tends to be obtained in that more contact points with the electronic conductive oxide particles and the mixed conductive oxide can be formed compared to when the average particle size is less than the lower limit, while if the average particle size is equal to or less than the upper limit, a higher effect tends to be obtained in that more contact points with the electronic conductive oxide particles and the mixed conductive oxide can be formed compared to when the average particle size exceeds the upper limit. The average particle size of such ion-conductive oxide particles can be measured by using a laser diffraction method.

[0033] The method for producing such ion-conductive oxide particles is not particularly limited, and any known method can be appropriately used.

[0034] The mixed conductive oxide according to the present invention has the following composition formula (1): (Ce 1-x-y Gd x Ni y )O2(1) [In the formula, x represents a number in the range of 0.02 to 0.3, and y represents a number in the range of 0.02 to 0.3.] The oxide (composite oxide) is represented by the formula (1). By using such an oxide represented by the formula (1) together with the electronically conductive oxide particles and the ionically conductive oxide particles, it is possible to impart the mixed conductive oxide with a transport function of electrons and ions (when the mixed conductive oxide is supported on the electronically conductive oxide particles and the ionically conductive oxide particles, it is possible to more efficiently impart the transport function of electrons and ions). This allows the high electrode function of the mixed conductive oxide to be utilized, and therefore a greater effect can be obtained in that the amount of Ni used (reduced Ni amount) can be reduced while the electrode function is fully exhibited.

[0035] In this formula (1), x is a value in the range of 0.02 to 0.3 (more preferably 0.05 to 0.3, even more preferably 0.05 to 0.2, and particularly preferably 0.1 to 0.2). When the value of x in this formula (1) is equal to or greater than the lower limit, a higher effect in terms of the reaction activity of the electrode reaction tends to be obtained compared to when the value is below the lower limit, and on the other hand, when the value is equal to or less than the upper limit, a higher effect in terms of the reaction activity of the electrode reaction tends to be obtained compared to when the value exceeds the upper limit.

[0036] In addition, y in the formula (1) represents a value in the range of 0.02 to 0.3 (more preferably 0.03 to 0.2, even more preferably 0.05 to 0.2, and particularly preferably 0.05 to 0.1). When the value of y in the formula (1) is equal to or greater than the lower limit, a higher effect in terms of the reaction activity of the electrode reaction tends to be obtained compared to when the value is below the lower limit, and on the other hand, when the value is equal to or less than the upper limit, a higher effect in terms of the reaction activity of the electrode reaction tends to be obtained compared to when the value exceeds the upper limit.

[0037] The method for producing such a mixed conductive oxide is not particularly limited, but it is preferable to use a solution containing Ce ions, Gd ions, and Ni ions, bring the solution into contact with (for example, impregnate, etc.) various substrates (for example, porous bodies, etc.), and sinter the solution under air to produce a mixed conductive oxide. Such a solution containing Ce ions, Gd ions, and Ni ions may be prepared by dissolving a Ce salt (nitrate, carbonate, hydroxide, etc.), a Gd salt (nitrate, carbonate, hydroxide, etc.), and a Ni salt (nitrate, carbonate, hydroxide, etc.) in a solvent in such a ratio that the composition formula after sintering is the formula shown in the above formula (1). The solvent used for producing such a solution is not particularly limited, and water, water containing citric acid, etc. can be used appropriately.

[0038] The electrochemical cell fuel electrode of the present invention may be any one that includes the electronically conductive oxide particles, the ionically conductive oxide particles, and the mixed conductive oxide, and the form thereof is not particularly limited, but from the viewpoint of enabling more efficient electrochemical reaction, it is preferable that the mixed conductive oxide is supported on the surfaces of the electronically conductive oxide particles and the ionically conductive oxide particles (supported on at least a part of the surfaces thereof), and here, it is more preferable that the electronically conductive oxide particles and the ionically conductive oxide particles are in the form of a porous body that is a sintered mixture of these particles. That is, in the electrochemical cell fuel electrode of the present invention, the mixed conductive oxide is preferably supported on the surfaces of the electronically conductive oxide particles and the ionically conductive oxide particles, and more preferably supported on the surface of the porous body (a sintered mixture of the electronically conductive oxide particles and the ionically conductive oxide particles). In this way, by supporting the mixed conductive oxide on the surfaces of the electronically conductive oxide particles and the ionically conductive oxide particles, it is possible to provide the fuel electrode with a sufficient number of highly active reaction sites even if the amount of Ni used is small, which tends to result in greater effectiveness in terms of efficient use of Ni (reduction in the amount of Ni used).

[0039] In the electrochemical cell fuel electrode of the present invention, when the mixed conductive oxide is supported on the surfaces of the electronically conductive oxide particles and the ionically conductive oxide particles, as described above, the electronically conductive oxide particles and the ionically conductive oxide particles preferably form a porous body that is a fired product of the mixed particles of the electronically conductive oxide particles and the ionically conductive oxide particles. The electronically conductive oxide particles and the ionically conductive oxide particles form the porous body, which makes it possible to efficiently diffuse fuel gases such as hydrogen and water vapor and generated gases, thereby enabling the fuel gas to be supplied more efficiently and sufficiently throughout the entire fuel cell, and thus tends to provide even higher effects in terms of power generation performance when used in an SOFC and electrolysis performance when used in an SOEC.

[0040] The form of the electrochemical cell fuel electrode of the present invention is not particularly limited and may be in various forms such as layered or cylindrical, but is preferably layered from the viewpoint of being more efficiently formed on the surface of the solid electrolyte (which may be in the form of a substrate, a membrane, or the like). When the electrochemical cell fuel electrode of the present invention is layered, the average thickness of the fuel electrode is preferably 1 to 100 μm (more preferably 5 to 50 μm). If the average thickness of the electrochemical cell fuel electrode is less than the lower limit, the connectivity between oxide particles in the electrode tends to decrease, resulting in a decrease in electrode performance, whereas if the average thickness exceeds the upper limit, the gas diffusion resistance tends to increase, resulting in a decrease in electrode performance.

[0041] In the electrochemical cell fuel electrode of the present invention, the content of the electronically conductive oxide particles is preferably 40 to 70 mass %, more preferably 40 to 60 mass %, based on the total mass of the fuel electrode. If the content of such electronically conductive oxide particles is less than the lower limit, the conduction in the electrode tends to decrease, leading to a decrease in electrode performance, whereas if the content exceeds the upper limit, the continuity of the ionically conductive oxide particles in the electrode tends to decrease, leading to a decrease in electrode performance.

[0042] Furthermore, in the electrochemical cell fuel electrode of the present invention, the content of the ion-conductive oxide particles is preferably 30 to 60 mass %, more preferably 40 to 60 mass %, based on the total amount of the fuel electrode. If the content of such ion-conductive oxide particles is less than the lower limit, the continuity of the ion-conductive oxide particles in the electrode tends to decrease, resulting in a decrease in electrode performance, whereas if the content exceeds the upper limit, the continuity of the electronically conductive oxide particles in the electrode tends to decrease, resulting in a decrease in electrode performance.

[0043] In the electrochemical cell fuel electrode of the present invention, the mass ratio of the electronically conductive oxide particles to the ionically conductive oxide particles ([electronically conductive oxide particles]:[ionically conductive oxide particles]) is preferably 2:1 to 1:2 (more preferably 1.5:1 to 1:1.5). In such a mass ratio, if the proportion of the electronically conductive oxide particles is less than the lower limit, the continuity of the electronically conductive oxide particles in the electrode tends to decrease, resulting in a decrease in electrode performance, whereas if it exceeds the upper limit, the continuity of the ionically conductive oxide particles in the electrode tends to decrease, resulting in a decrease in electrode performance.

[0044] In addition, the molar content of the mixed conductive oxide per gram of the total content of the electronically conductive oxide particles and the ionically conductive oxide particles in the electrochemical cell fuel electrode of the present invention is 5×10 -5 ~5×10 -3 mol / g (preferably 1×10 -4 ~5×10 -4 In other words, when the mixed conductive oxide is supported on the porous body, the amount (molar amount) of the mixed conductive oxide supported per 1 g of the mass of the porous body is preferably 5×10 -5 ~5×10 -3 mol / g (preferably 1×10 -4 ~5×10 -4 If the content (supported amount) of such a mixed conductive oxide is less than the lower limit, the electrode performance tends to decrease, whereas if it exceeds the upper limit, the gas diffusion resistance increases and the electrode performance tends to decrease.

[0045] In the electrochemical cell fuel electrode of the present invention, the content of the mixed conductive oxide is preferably 0.1 to 5 mass %, more preferably 1 to 3 mass %, based on the total mass of the fuel electrode. If the content of the mixed conductive oxide is less than the lower limit, the electrode performance tends to decrease, whereas if it exceeds the upper limit, the gas diffusion resistance increases and the electrode performance tends to decrease.

[0046] As an electrochemical cell using the electrochemical cell fuel electrode of the present invention, a known SOFC configuration or a known SOEC configuration can be appropriately used, except that the fuel electrode is made of the electrochemical cell fuel electrode of the present invention, and for example, a configuration including the electrochemical cell fuel electrode of the present invention, an air electrode, and a solid electrolyte layer may be used. As such an electrochemical cell (an electrochemical cell using the electrochemical cell fuel electrode of the present invention), the electrochemical cell of the present invention described below is preferable. In addition, the method for manufacturing the electrochemical cell fuel electrode of the present invention is not particularly limited, but it is preferable to adopt the manufacturing method of the electrochemical cell fuel electrode of the present invention described below.

[0047] [Method of manufacturing a fuel electrode for electrochemical cells] The method for producing an anode for an electrochemical cell of the present invention comprises the steps of: A step of obtaining a porous body composed of electronically conductive oxide particles and ionically conductive oxide particles (hereinafter, for convenience, sometimes simply referred to as the "first step"); a step of impregnating the porous body with a solution containing Ce ions, Gd ions and Ni ions, followed by firing the porous body to obtain the fuel electrode for electrochemical cells of the present invention (hereinafter, for convenience, sometimes simply referred to as the "second step"); Each step will be described below separately.

[0048] <First step> The first step is to obtain a porous body made of electronically conductive oxide particles and ionically conductive oxide particles.

[0049] The porous body made of such electron-conductive oxide particles and ion-conductive oxide particles is preferably a fired product of the mixed particles of the electron-conductive oxide particles and the ion-conductive oxide particles. From this viewpoint, the first step is preferably a step (A) of preparing a paste made of the mixed particles of the electron-conductive oxide particles and the ion-conductive oxide particles, applying the paste to a substrate (preferably a film or substrate made of a solid electrolyte) and firing the paste to form a porous body made of the electron-conductive oxide particles and the ion-conductive oxide particles on the substrate. Hereinafter, such a step (A) will be described.

[0050] The method for producing the paste made of such mixed particles is not particularly limited, and a method of producing the paste by mixing the electronically conductive oxide particles, the ionically conductive oxide particles, and a solvent (further mixing a binder, a pore former, etc., if necessary) may be adopted. Such a solvent is not particularly limited, and a known solvent may be appropriately used, for example, water, terpineol, butanol, ethanol, etc. may be used. In addition, when producing such a paste, other known components such as those used in producing a paste of metal particles may be contained. Examples of such other components include binders and pore formers. In addition, when a binder is used as the other component, the type is not particularly limited, and a known one (for example, ethyl cellulose, etc.) may be appropriately used. In addition, when a pore former is used as the other component in producing the paste, the type is not particularly limited, and a known one (for example, polyvinyl butyral, etc.) may be appropriately used. In addition, when producing such a paste, it is preferable to use the electronically conductive oxide particles and the ionically conductive oxide particles so that the mass ratio of the electronically conductive oxide particles and the ionically conductive oxide particles contained in the paste ([electronically conductive oxide particles]:[ionically conductive oxide particles]) is 2:1 to 1:2 (more preferably 1.5:1 to 1:1.5).

[0051] The method of applying the paste to the substrate is not particularly limited, and any known method capable of applying the paste can be appropriately used. For example, a method of applying the paste by screen printing may be adopted. In applying the paste, the thickness of the coating film is not particularly limited, and the type of paste and the amount of coating may be appropriately adjusted so that the thickness of the fuel electrode to be finally formed is the desired thickness. It is preferable to use such a substrate made of a solid electrolyte, since this makes it easier to form an electrochemical cell. However, when the fuel electrode for an electrochemical cell is peeled off and used after the fuel electrode for an electrochemical cell is formed in the second step (for example, when the peeled fuel electrode is separately attached to a solid electrolyte and used), a peelable sheet or the like may be used.

[0052] The conditions for firing the paste are not particularly limited, and the paste is preferably fired in an air atmosphere at a temperature of 800 to 1400°C (preferably 1200 to 1350°C) for 1 to 3 hours (preferably 1 to 2 hours). By such firing, a porous body (sintered body) consisting of electronically conductive oxide particles and ionically conductive oxide particles can be formed.

[0053] <Second process> The second step is a step of impregnating the porous body with a solution containing Ce ions, Gd ions and Ni ions, followed by firing, to obtain the fuel electrode for electrochemical cells of the present invention.

[0054] A preferred method for preparing such a solution containing Ce ions, Gd ions and Ni ions is to dissolve a Ce salt, a Gd salt and a Ni salt in a solvent in such a ratio that the composition formula of the oxide obtained after firing is the formula shown in the above formula (1).

[0055] Such Ce salts are not particularly limited, and include Ce salts such as nitrates, carbonates, chlorides, and hydroxides, among which Ce nitrates are particularly preferred due to their high water solubility. The Gd salts are not particularly limited, and include Gd salts such as nitrates, carbonates, chlorides, and hydroxides, among which Gd nitrates are particularly preferred from the viewpoint of cost. The Ni salts are not particularly limited, and include Ni salts such as nitrates, chlorides, and hydroxides, among which Ni nitrates are particularly preferred from the viewpoint of cost. The solvent used to prepare such a solution is not particularly limited, and water, citric acid-containing water, and the like can be used as appropriate.

[0056] In preparing the solution, since the value of x, which indicates the content ratio of Gd when the sum of the contents of Ce, Gd, and Ni in the compound (oxide) represented by the above formula (1) is converted to 1 mole, is 0.02 to 0.3, it is preferable to use a Gd salt so that the content of Gd ions in the solution when the total molar amount of metal ions in the solution (the total amount of Ce ions, Gd ions, and Ni ions) is converted to 1 mole is in the same numerical range as x (a range of 0.02 to 0.3, more preferably a range of 0.05 to 0.3, even more preferably a range of 0.05 to 0.2, and particularly preferably a range of 0.1 to 0.2). Similarly, with regard to the compound represented by the above formula (1), since the value of y, which indicates the Ni content when the sum of the contents of Ce, Gd, and Ni in the compound is converted to 1 mole, is 0.02 to 0.3, it is preferable to use a Ni salt so that the content of Ni ions in the solution, when the total molar amount of metal ions in the solution (the total amount of Ce ions, Gd ions, and Ni ions) is converted to 1 mole, is a molar amount in the same numerical range as y (a range of 0.02 to 0.3, more preferably a range of 0.03 to 0.2, even more preferably a range of 0.05 to 0.2, and particularly preferably a range of 0.05 to 0.1). The content (molar amount) of Ce ions when the total amount of metal ions in the solution (total amount of Ce, Gd, and Ni) is converted to 1 mole can be determined (designed) according to the amount x of Gd ions and the amount y of Ni ions in the solution, but it is preferable to use a Ce salt so that the content of Ce ions is 0.4 to 0.9 moles (more preferably 0.7 to 0.9 moles, and even more preferably 0.8 to 0.9 moles). If the content of Ce ions is less than the lower limit, by-products tend to be generated and the conductivity tends to decrease, while if it exceeds the upper limit, the conductivity tends to decrease.

[0057] In addition, when preparing such a solution, the total amount (content) of the Ce salt, Gd salt and Ni salt contained in the solution is not particularly limited, but is preferably 0.2 to 1 mol / L (more preferably 0.3 to 0.7 mol / L, and even more preferably 0.4 to 0.6 mol / L). If the total amount of such Ce, Gd and Ni salts is less than the lower limit, it tends to be difficult to efficiently obtain a predetermined amount of the compound (oxide) represented by formula (1) (it takes time to produce a predetermined amount of the compound), while if it exceeds the upper limit, the composition of the obtained compound (oxide) tends to deviate from the desired composition, making it difficult to obtain a compound with a uniform composition.

[0058] In the second step, the solution is impregnated into the porous body. Thus, the method of impregnating the porous body with the solution is not particularly limited, and a known method can be appropriately adopted. As such a method, for example, a method of dripping the solution onto the porous body to impregnate it, a method of spraying the solution onto the porous body to impregnate it, a method of immersing the porous body in the solution for a certain period of time to impregnate it, etc. can be appropriately adopted.

[0059] When impregnated in this manner, the amount (molar amount) of the mixed conductive oxide supported per gram of the mass of the porous body in the resulting anode is 5×10 -5 ~5×10 -3 mol / g (preferably 1×10 -4 ~5×10 -4 It is preferable to use a solution so that the concentration is 100% (mol / g).

[0060] Furthermore, in the second step, the porous body is impregnated with the solution and then calcined. When carrying out such a calcination step, it is preferable to remove the solvent from the solution impregnated into the porous body before the calcination step (when the solvent is water, it is dried). Although there is no particular limitation on such a solvent removal step, it is preferable to carry out a step of leaving the solution at rest for 0.5 to 2 hours under a temperature condition of 80 to 200°C. Furthermore, although there is no particular limitation on the conditions for such calcination, it is preferable to calcinate, for example, in an air atmosphere at a temperature of 800 to 1200°C (preferably 900 to 1000°C) for 0.5 to 3 hours (preferably 1 to 2 hours). By such calcination, the mixed conductive oxide can be formed in a form supported on the porous body. Therefore, by carrying out the first and second steps, it is possible to manufacture a fuel electrode for an electrochemical cell, which is composed of the electronically conductive oxide particles, the ionically conductive oxide particles, and the mixed conductive oxide, and the fuel electrode can have a configuration in which the mixed conductive oxide is supported on a porous body composed of the electronically conductive oxide particles and the ionically conductive oxide particles.

[0061] [Electrochemical cell] The electrochemical cell of the present invention is characterized by comprising the electrochemical cell fuel electrode of the present invention, an air electrode, and a solid electrolyte layer.

[0062] The electrochemical cell fuel electrode used in such an electrochemical cell is the electrochemical cell fuel electrode of the present invention described above. Note that such an electrochemical cell fuel electrode is used as an anode electrode when the electrochemical cell is used as an SOFC, and is used as a cathode electrode when the electrochemical cell is used as an SOEC.

[0063] The air electrode used in such an electrochemical cell is not particularly limited, and any known air electrode used in the field of SOFC or SOEC (for example, a known electrode used as a cathode electrode of SOFC, a known electrode used as an anode electrode of SOEC, etc.) can be appropriately used. As such an air electrode, for example, La xSr 1-x CoO3-based oxide (lanthanum strontium cobalt complex oxide: LSC), La x Sr 1-x Co y Fe 1-y O3-based oxides (lanthanum strontium cobalt iron composite oxide: LSCF), Sm x Sr 1-x Examples of the material include transition metal perovskite oxides (wherein x and y in the above formula satisfy the conditions of 0≦x≦1 and 0≦y≦1, respectively) such as CoO3-based oxides (samarium strontium cobalt composite oxide: SSC). Such materials for the air electrode, such as transition metal perovskite oxides, may be used alone or in combination of two or more. The method for producing such transition metal perovskite oxides is not particularly limited, and known methods may be appropriately adopted.

[0064] In addition, such an air electrode is preferably in a layered form, and the lower limit of the average thickness is preferably 5 μm or more (more preferably 15 μm or more, and even more preferably 20 μm or more) from the viewpoint of improving current collection and increasing the reaction area. In addition, when the air electrode is in a layered form, the upper limit of the average thickness is preferably 100 μm or less (more preferably 80 μm or less, and even more preferably 60 μm or less) from the viewpoint of more sufficiently suppressing the occurrence of cracks due to the difference in the linear thermal expansion coefficient with other layers.

[0065] The solid electrolyte layer is not particularly limited, and may be a membrane, substrate, or the like made of a known solid electrolyte used in the field of SOFC or SOEC. From the viewpoint of excellent strength and thermal stability, such a solid electrolyte layer is preferably made of a zirconia-based oxide such as yttria-stabilized zirconia (YSZ) or scandia-stabilized zirconia (ScSZ), and among these, from the viewpoint of excellent oxygen ion conductivity, it is more preferable to use yttria-stabilized zirconia (YSZ).

[0066] In addition, such a solid electrolyte is preferably in the form of a substrate (plate, film, etc.), and its average thickness is preferably 3 to 20 μm, more preferably 4 to 15 μm, and particularly preferably 5 to 10 μm, from the viewpoint of reducing resistance. The method for producing such a solid electrolyte is not particularly limited, and a known method (for example, the method described in JP-A-2020-167052) can be appropriately adopted.

[0067] The electrochemical cell of the present invention may include the electrochemical cell fuel electrode of the present invention, an air electrode, and a solid electrolyte layer. Other configurations and structures (e.g., a structure regarding the arrangement of each layer, and a layer configuration such as whether or not other layers are included) are not particularly limited, and known configurations and structures used in the fields of SOFC and SOEC can be appropriately adopted. Such an electrochemical cell of the present invention preferably has a structure (arrangement structure) consisting of the solid electrolyte layer, the electrochemical cell fuel electrode of the present invention arranged on one side of the solid electrolyte layer, and an air electrode arranged on the other side of the solid electrolyte layer. In addition, such an electrochemical cell may include other known layers (e.g., a reaction prevention layer, etc.) used in the fields of SOFC and SOEC as necessary. In addition, when a reaction prevention layer is provided as another layer, for example, the structure may be such that a reaction prevention layer is further arranged between the solid electrolyte layer and the air electrode.

[0068] As such a reaction prevention layer, a material known in the field of SOFCs can be appropriately used, for example, a material made of ceria (CeO2); CeO2 doped with at least one element selected from Gd, Sm, Y, La, Nd, Yb, Ca, and Ho; can be appropriately used. The material of such a reaction prevention layer may be used alone or in combination of two or more. As such a reaction prevention layer, for example, a sheet (thin film) made of gadolinia-doped ceria (CeO2 doped with Gd2O3: GDC) can be suitably used. In addition, the average thickness of such a reaction prevention layer is preferably 1 to 20 μm, more preferably 2 to 10 μm, from the viewpoint of reducing the ohmic resistance when used in a SOFC and suppressing the diffusion of elements from the air electrode. As such a reaction prevention layer, a sheet manufactured by a known method can be appropriately used.

[0069] Examples of the method for producing such an electrochemical cell include a sheet lamination method and a printing method. Examples of the method for producing such an electrochemical cell include preparing a substrate made of the solid electrolyte, forming an air electrode on one side of the substrate (when a reaction prevention layer is provided, a reaction prevention layer is formed on one surface of the substrate, and then the air electrode is formed on the reaction prevention layer), and forming the fuel electrode for the electrochemical cell of the present invention on the other side (in this method, for example, the printing method described above may be used to produce the air electrode or the fuel electrode for the electrochemical cell). The substrate made of such a solid electrolyte may be appropriately produced by a method known in the field of electrochemical cells. The method for forming the air electrode is not particularly limited, and a known method may be appropriately used. For example, a method may be used in which a paste made of a material for the air electrode is prepared, and the paste is applied (preferably printed) on the surface of the substrate or the surface of the reaction prevention layer, and then the paste is fired. The method for producing the paste made of the material for the air electrode is not particularly limited, and a known method may be appropriately used (the paste may appropriately contain a known solvent such as water or a known binder, etc., as necessary). The firing conditions during production of the air electrode are not particularly limited, but it is preferable to fire the air electrode in an air atmosphere at a temperature of 900 to 1500° C. (preferably 950 to 1450° C.) for 1 to 10 hours (preferably 2 to 5 hours).

[0070] In addition, when forming a reaction prevention layer on the surface of the substrate, the manufacturing method is not particularly limited, and a sheet made of the material of the reaction prevention layer is prepared by a known method (for example, the method described in JP 2020-167052 A, etc.), and after laminating this on the substrate (after laminating by pressure bonding or the like by a known method as necessary), the antireflection layer laminated on the surface of the substrate may be formed by firing. In addition, the firing conditions in the production of the antireflection layer are not particularly limited, but for example, it is preferable to fire it in an air atmosphere at a temperature of 900 to 1500 ° C. (preferably, 950 to 1450 ° C.) for 1 to 10 hours (preferably, 2 to 5 hours). In addition, as a method for forming the electrochemical cell fuel electrode of the present invention on the other surface side of the substrate, it is preferable to adopt the method described in the manufacturing method of the electrochemical cell fuel electrode of the present invention described above. In this case, it is sufficient to finally manufacture the fuel electrode for electrochemical cells by carrying out both the first and second steps described above. For example, a method of continuously carrying out the first and second steps on one side of a substrate (solid electrolyte layer) may be adopted, or a method of carrying out both the first and second steps on one side of a substrate (solid electrolyte layer) may be adopted, in which the first step is carried out on one side of a substrate (solid electrolyte layer), and then another step, such as laminating an air electrode on the other side, is carried out at a different site, and then carrying out the second step. In this way, by forming each layer, an electrochemical cell having a structure (arrangement structure) consisting of the solid electrolyte layer, the fuel electrode for electrochemical cells of the present invention arranged on one side of the solid electrolyte layer, and the air electrode arranged on the other side of the solid electrolyte layer can be manufactured.

[0071] Such an electrochemical cell of the present invention is preferably used as a solid oxide fuel cell (SOFC) and / or a solid oxide electrolysis cell (SOEC). Note that such an electrochemical cell of the present invention can also be used in a solid oxide reversible type fuel cell (SORC) system in which power generation and hydrogen generation are performed in the same cell. EXAMPLES

[0072] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0073] Example 1 An electrochemical cell was produced by employing the "step of preparing a solution (A) for producing a mixed conductive oxide" and the "step of producing an electrochemical cell" described below. FIG. 1 shows a schematic cross-sectional view of the electrochemical cell produced in Example 1. The electrochemical cell 10 shown in FIG. 1 has a configuration including a solid electrolyte layer 11, a fuel electrode 12 arranged (laminated) on one side of the solid electrolyte layer 11, a reaction prevention layer 13 arranged on the other side of the solid electrolyte layer 11, and an air electrode 14 arranged on the reaction prevention layer 13.

[0074] <Preparation step of solution (A) for producing mixed conducting oxide> Using Ce(NO3)3·6H2O as the Ce salt, Gd(NO3)3·6H2O as the Gd salt, and Ni(NO3)2·6H2O as the Ni salt, dissolve the Ce salt, Gd salt, and Ni salt in ion-exchanged water in a specified ratio so that the content (total amount) of the Ce salt, Gd salt, and Ni salt becomes 0.5 mol / L. 0.85 Gd 0.1 Ni 0.05 A solution (A) was prepared to obtain O2. Note that when preparing such a solution (A), the composition of the oxide obtained after removing the solvent and firing was Ce. 0.85 Gd 0.1 Ni 0.05 To obtain O2, Ce salt, Gd salt, and Ni salt were used in such proportions that the molar amount of Ce ions was 0.85 mol, the molar amount of Gd ions was 0.1 mol, and the molar amount of Ni ions was 0.05 mol, when the total molar amount of Ce ions, Gd ions, and Ni ions in the solution was converted to 1 mol.

[0075] <About the manufacturing process of electrochemical cells> First, a commercially available YSZ substrate (manufactured by Nikkato Corporation; yttria-stabilized zirconia substrate using ZrO2 stabilized with 8 mol% Y2O3; disk-shaped with a diameter of 22 mm and a thickness of 0.5 mm) was prepared as a substrate for forming a solid electrolyte layer.

[0076] In addition, a disk-shaped sheet having a diameter of 22 mm and a thickness of 0.01 mm and made of gadolinia-doped ceria (abbreviation: GDC, CeO2 doped with 10 mol% Gd2O3, particles with an average particle diameter of 0.8 μm) was prepared as a sheet for forming a reaction prevention layer. The sheet for forming such a reaction prevention layer was manufactured by the following method. That is, first, a slurry consisting of a mixture of 25 g of the GDC powder, 2.75 g of polyvinyl butyral as a binder, and 16.5 g of a solvent (a mixed solvent of an alcohol-based solvent (manufactured by Imazu Pharmaceutical Co., Ltd., product name: Econol) and phthalic acid) was applied onto a resin sheet and dried for 2 hours. Thereafter, the obtained laminate was punched out with a punch having a diameter of 22 mm, and the resin sheet was peeled off to manufacture a disk-shaped sheet (sheet for forming a reaction prevention layer) made of GDC having a diameter of 22 mm.

[0077] The sheet (disc-shaped) for forming the reaction prevention layer was then attached to one surface of the substrate (disc-shaped) for forming the solid electrolyte layer, and pressed with a hot water isostatic press (temperature: 80°C, press pressure: 200 MPa, press time: 2 minutes), followed by sintering at 1350°C for 120 minutes to obtain a disc-shaped laminate (I) with a diameter of 22 mm, in which a reaction prevention layer made of GDC was laminated on one surface of a solid electrolyte layer made of YSZ. In the laminate (I) thus obtained, in which the reaction prevention layer / solid electrolyte layer were laminated in this order, the average thickness of the reaction prevention layer made of GDC was about 3 μm.

[0078] Next, La with an average particle size of 0.5 μm 0.4 Sr 0.6 The electronic conductive oxide particles consisted of TiO3 (abbreviation: LST, manufactured by Kcera) and Ce with an average particle size of 0.5 μm. 0.9 Gd 0.1A paste for forming a porous body was prepared by adding 18 g of mixed particles containing ion-conductive oxide particles made of O2 (abbreviation: GDC, manufactured by Kcera) in a mass ratio of 1:1 to 10 g of terpineol and kneading. Next, the paste was applied by screen printing to the center of the circular surface of the laminate (I) on the side where the reaction prevention layer 13 was not laminated (the surface of the solid electrolyte layer 11 (substrate) opposite to the surface on which the reaction prevention layer 13 was laminated) to form a circular coating film with a diameter of 8 mm, which was then fired at 1340°C for 2 hours to form a layer made of a circular porous body made of LST particles and GDC particles, thereby obtaining a laminate (II) having a structure in which the reaction prevention layer 13 made of GDC was laminated on one surface of the solid electrolyte layer 11 made of YSZ and a layer made of a circular porous body (average thickness: 40 μm, total amount: 0.015 g) made of LST particles and GDC particles was laminated on the other surface (note that in such a process (hereinafter sometimes referred to as the "porous body forming process"), the layer made of the porous body was formed so that the center of the circular surface of the layer of the porous body and the center of the solid electrolyte layer were at the same position).

[0079] Then, La 0.6 Sr 0.4 Co 0.2 Fe 0.8 A paste for forming an air electrode was obtained by adding 18 g of metal oxide particles made of O3 (abbreviation: LSCF, manufactured by Kcera) to 10 g of terpineol and kneading the mixture. The paste was then applied by screen printing to the center of the surface of the reaction prevention layer 13 of the laminate (II) to form a circular coating film with a diameter of 18 mm. The resulting film was then fired at 1000°C for 1 hour to form an air electrode 14 (average thickness: 50 μm) made of LSCF particles, thereby obtaining a laminate (III) laminated in the order of "air electrode / anti-reflection layer / solid electrolyte layer / porous layer" (note that in this process, the air layer was formed so that the center of the circular surface of the air layer was in the same position as the center of the solid electrolyte layer).

[0080] Next, 5 μL of the solution (A) for producing a mixed conductive oxide was dropped onto the layer of the porous body formed on one side of the laminate (III) (the side opposite to the side on which the air electrode was disposed) to impregnate the porous body constituting the layer with the solution (A). The solution was then heated at a temperature condition of 120° C. to remove the solvent of the solution (A) (drying step), and the porous body was impregnated with Ce by firing at 950° C. for 1 hour. 0.85 Gd 0.1 Ni 0.05 A mixed conductive oxide made of O2 was supported to form the fuel electrode 12, thereby obtaining an electrochemical cell 10 in which the air electrode 14 / anti-reflection layer 13 / solid electrolyte layer 11 / fuel electrode 12 were laminated in this order.

[0081] The fuel electrode 12 in the electrochemical cell 10 thus formed has a structure in which the mixed conductive oxide is supported on a porous body made of the electronically conductive oxide particles and the ionically conductive oxide particles. Furthermore, the Ni content (total amount) in the fuel electrode 12 is 7.3×10 -6 g (calculated value from the charge amount).

[0082] Example 2 An electrochemical cell 10 was formed in the same manner as in Example 1, except that a step of preparing a solution (B) for producing a mixed conductive oxide described below was carried out instead of a step of preparing a solution (A) for producing a mixed conductive oxide, and the solution (B) described below was used instead of the solution (A). The fuel electrode 12 in the electrochemical cell 10 thus formed was formed by dispersing Ce in a porous body made of the electron conductive oxide particles and the ion conductive oxide particles. 0.85 Gd 0.05 Ni 0.1 The resulting structure was a structure in which a mixed conductive oxide made of O2 was supported. The Ni content (total amount) in the anode 12 was 1.4 × 10 -5 g (calculated value from the charge amount).

[0083] <Preparation step of solution (B) for producing mixed conductive oxide> Using Ce(NO3)3·6H2O as the Ce salt, Gd(NO3)3·6H2O as the Gd salt, and Ni(NO3)2·6H2O as the Ni salt, dissolve the Ce salt, Gd salt, and Ni salt in ion-exchanged water in a specified ratio so that the content (total amount) of the Ce salt, Gd salt, and Ni salt becomes 0.5 mol / L. 0.85 Gd 0.05 Ni 0.1 A solution (B) was prepared to obtain O2. Note that when preparing such a solution (B), the composition of the oxide obtained after removing the solvent and firing was Ce. 0.85 Gd 0.05 Ni 0.1 To obtain O2, Ce salt, Gd salt, and Ni salt were used in such proportions that the molar amount of Ce ions was 0.85 mol, the molar amount of Gd ions was 0.05 mol, and the molar amount of Ni ions was 0.1 mol, when the total molar amount of Ce ions, Gd ions, and Ni ions in the solution was converted to 1 mol.

[0084] Comparative Example 1 The step of preparing the solution (A) for producing the mixed conductive oxide was not carried out, and the steps described in Example 1 up to the step of forming the laminate (III) were carried out, and the resulting laminate (III) was used as a comparative electrochemical cell. In this manner, an electrochemical cell having a structure in which the air electrode / anti-reflection layer / solid electrolyte layer / porous body layer (comparative fuel electrode (i))) were laminated in this order was formed in the same manner as in Example 1, except that the step of supporting the mixed conductive oxide on the porous body using the solution (A) was not carried out.

[0085] Comparative Example 2 An electrochemical cell having a structure in which the air electrode / antireflection layer / solid electrolyte layer / comparative fuel electrode (ii) were layered in this order was formed in the same manner as in Example 1, except that the step of forming a porous body was replaced by the step of forming a comparative fuel electrode (ii) described below, and the step of supporting a mixed conductive oxide on the porous body using the solution (A) was not performed.

[0086] <Step of forming fuel electrode (ii)> A paste for forming the fuel electrode was obtained by kneading 18 g of mixed particles containing Ni particles (manufactured by Kanto Chemical Co., Ltd.) with an average particle size of 1 μm and YSZ particles made of yttria-stabilized zirconia (abbreviated as YSZ, ZrO2 stabilized with 8 mol% Y2O3, manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.) with a mass ratio of 1:1, together with 10 g of terpineol. The paste was applied by screen printing to the center of the circular surface of the solid electrolyte layer 11 on the side where the reaction prevention layer 13 was not laminated, forming a circular coating film with a diameter of 8 mm, and then calcined at 1340 °C for 5 hours to form a fuel electrode (ii) made of a mixture of Ni particles and YSZ particles. The Ni content (total amount) in the fuel electrode (ii) was 5 × 10 -3 g (calculated value from the charge amount).

[0087] [Evaluation of the characteristics of electrochemical cells obtained in Examples 1 and 2 and Comparative Examples 1 and 2] <XRD Measurement of Calcined Powders of Solutions (A) and (B)> First, solutions (A) and (B) produced in Examples 1 and 2 were used to form calcined powders derived from each solution, and XRD measurements were performed on the resulting calcined powders. The calcined powders used in such measurements were formed by using solutions (A) and (B), respectively, heating the solutions at 500°C for 30 minutes to remove the solvent (water) from the solutions, and calcining the resulting solids at 950°C for 1 hour (thereby forming calcined powders derived from each solution). The XRD chart of the calcined powder formed from solution (A) obtained in Example 1 and the XRD chart of the calcined powder formed from solution (B) obtained in Example 2 are shown in FIG. 2.

[0088] As is clear from the results shown in Fig. 2, a pattern similar to that of CeO2 was confirmed in the XRD chart, and the peaks of Gd and Ni were not confirmed. From such an XRD chart, it was confirmed that Gd and Ni were dissolved in CeO2. And from the results of such XRD measurements, in Examples 1 and 2, during the production of the fuel electrode, a mixed-conducting oxide of the desired composition (according to the ratio of each metal contained in the solution) was formed according to the composition of the solution used, and it was found that they were supported on the porous body. (In Example 1, Ce 0.85 Gd 0.1 Ni 0.05 O2, and in Example 2, Ce 0.85 Gd 0.05 Ni 0.1 O2). Thus, in Examples 1 and 2, since Ni is dissolved in CeO2 and utilized, it is clear that the durability of the fuel electrode is higher compared to the prior art in which the metal Ni was directly used for the fuel electrode. For example, since Ni is dissolved in CeO2 and utilized as an oxide, it is considered that the oxidation and reduction of Ni based on the usage environment (gas atmosphere) of the fuel electrode can be sufficiently suppressed, and the expansion and contraction of Ni can be more highly suppressed. From such a perspective, it is speculated that the durability of the fuel electrode is improved.

[0089] From such measurement results, in Examples 1 and 2, since it is clear that the fuel electrode is composed of LST particles, GDC particles, and a mixed-conducting oxide (in Example 1, Ce 0.85 Gd 0.1 Ni 0.05 O2, and in Example 2, Ce 0.85 Gd 0.05 Ni 0.1 O2), it can be seen that the fuel electrode is entirely composed of oxides. And from the overall configuration of such a fuel electrode, it can be understood that the expansion and contraction of the fuel electrode are sufficiently suppressed, and it can be seen that the durability of the fuel electrode is sufficiently high.

[0090] <Measurement of Power Generation Performance when Used as an SOFC> The electrochemical cells obtained in Examples 1-2 and Comparative Examples 1-2 were used to evaluate the power generation performance when used as SOFC as follows. That is, the electrochemical cells were installed in an evaluation device (manufactured by BioLogic, product name "VSP", a device capable of evaluating the relationship between I (power generation current) and V (voltage)), and a mixed gas of N2 and O2 (O2: 20 volume %, N2: balance) was flowed to the air electrode side under the condition of temperature: 700 ° C., and a gas obtained by humidifying H2 (100 volume %) at 35 ° C. (water vapor content: 5.6 volume %) was flowed to the fuel electrode side, and the relationship between I (power generation current) and V (voltage) was measured by the evaluation device. The obtained results (a graph showing the relationship between cell voltage and current) are shown in FIG. 3.

[0091] As is clear from the results shown in Fig. 3, the mixed conductive oxide (Ce 0.85 Gd 0.1 Ni 0.05 O2 or Ce 0.85 Gd 0.05 Ni 0.1 It was found that when an electrochemical cell having an anode on which a mixed conductive oxide (O2) was supported was used (Examples 1 and 2), the generated current was sufficiently larger than when the anode was made of only the porous body (Comparative Example 1: a case in which solution (A) or (B) was not used and the porous body was not supported with a mixed conductive oxide).

[0092] In addition, the mixed conductive oxide (Ce 0.85 Gd 0.1 Ni 0.05 O2 or Ce 0.85 Gd 0.05 Ni 0.1When an electrochemical cell equipped with a fuel electrode supporting O2) (Examples 1 and 2) was used, a power generation current at a level comparable to that of an electrochemical cell equipped with a fuel electrode composed of a mixture of Ni particles and YSZ particles (Comparative Example 2) was confirmed. Considering the way Ni was utilized in the electrochemical cells obtained in Examples 1 to 2 and the electrochemical cell obtained in Comparative Example 2, it can be seen that when a mixed-conducting oxide was used as in Examples 1 to 2, it was possible to exhibit power generation performance comparable to that when metallic Ni was used while significantly reducing the amount of Ni used.

[0093] From such results, an electrochemical cell using the mixed-conducting oxide represented by the above formula (1) as the fuel electrode (for example, see Examples 1 to 2) exhibits a high level of power generation performance comparable to that of a conventional electrochemical cell using a mixture of Ni particles and YSZ particles as the fuel electrode (for example, see Comparative Example 2), and it was found that the amount of Ni used can be significantly reduced compared to a conventional electrochemical cell using a mixture of Ni particles and YSZ particles as the fuel electrode (thereby enabling cost reduction). As described above, since Ni is dissolved in CeO2 in the obtained mixed-conducting oxide, it is considered that the durability of the fuel electrode is higher than when metallic Ni is used as it is. According to the present invention, it can also be seen that it is possible to achieve both a reduction in the amount of Ni used for the fuel electrode and an improvement in the performance of the fuel electrode, and to make the durability of the fuel electrode even better.

[0094] <Measurement of electrolysis performance when used as an SOEC> The electrochemical cells obtained in Examples 1-2 and Comparative Examples 1-2 were used to evaluate the water electrolysis characteristics when used as an SOEC as follows. That is, the electrochemical cells were placed in an evaluation device (manufactured by BioLogic, product name "VSP", a device capable of evaluating the relationship between V (voltage) and I (electrolysis current)), and under the condition of temperature: 700°C, a mixed gas of N2 and O2 (O2: 20 volume %, N2: balance) was flowed to the air electrode side, and a mixed gas of H2O (water vapor) and H2 (H2O:H2 (volume ratio) = 1:1) was flowed to the fuel electrode side, and the relationship between V (voltage) and I (electrolysis current) was measured by the evaluation device. The obtained results (a graph showing the relationship between cell voltage and electrolysis current) are shown in FIG. 4.

[0095] The mixed conductive oxide (Ce 0.85 Gd 0.1 Ni 0.05 O2 or Ce 0.85 Gd 0.05 Ni 0.1 It was found that when an electrochemical cell having a fuel electrode on which a mixed conductive oxide (O2) was supported was used (Examples 1 and 2), the electrolysis current was sufficiently large compared to when the fuel electrode was made of only the porous body (Comparative Example 1: a case in which solution (A) or (B) was not used and the porous body was not supported with a mixed conductive oxide).

[0096] In addition, the mixed conductive oxide (Ce 0.85 Gd 0.1 Ni 0.05 O2 or Ce 0.85 Gd 0.05 Ni 0.1 When an electrochemical cell having a fuel electrode carrying a mixture of Ni particles and YSZ particles (Examples 1 and 2) was used, an electrolysis current was confirmed to be at a level equivalent to that of an electrochemical cell having a fuel electrode made of a mixture of Ni particles and YSZ particles (Comparative Example 2). Considering the way Ni was used in the electrochemical cells obtained in Examples 1 and 2 and the electrochemical cell obtained in Comparative Example 2, it can be seen that when a mixed conductive oxide is used as in Examples 1 and 2, electrolysis performance equivalent to that of the case of using metallic Ni can be exhibited while the amount of Ni used is significantly reduced.

[0097] From these results, it was found that an electrochemical cell using the mixed conductive oxide represented by the above formula (1) for the fuel electrode (see, for example, Examples 1-2) can achieve a high level of electrolysis performance equivalent to that of a conventional electrochemical cell using a mixture of Ni particles and YSZ particles for the fuel electrode (see, for example, Comparative Example 2), while significantly reducing the amount of Ni used (and thus reducing costs) compared to a conventional electrochemical cell using a mixture of Ni particles and YSZ particles for the fuel electrode. As described above, in the obtained mixed conductive oxide, Ni is dissolved in CeO2, so it is considered that the durability of the fuel electrode is higher than when metal Ni is used as is. It is also found that according to the present invention, it is possible to achieve both a reduction in the amount of Ni used for the fuel electrode and high performance of the fuel electrode, and to improve the durability of the fuel electrode. [Industrial Applicability]

[0098] As described above, according to the present invention, it is possible to provide an electrochemical cell anode that can exhibit a sufficiently high level of power generation performance when used as an anode for an SOFC and a sufficiently high level of water electrolysis performance when used as an anode for an SOEC while sufficiently reducing the amount of Ni used, and that can be used in both SOFC and SOEC cells; a method for producing an electrochemical cell anode that can efficiently produce the electrochemical cell anode; and an electrochemical cell using the electrochemical cell anode. Thus, the electrochemical cell anode of the present invention is particularly useful as, for example, an anode for an SOFC, an anode for an SOEC, an anode for an SORC, etc. [Explanation of symbols]

[0099] 10: electrochemical cell; 11: solid electrolyte layer (solid electrolyte substrate); 12: fuel electrode; 13: reaction prevention layer; 14: air electrode.

Claims

1. Electronically conductive oxide particles; Ion-conductive oxide particles; The following composition formula (1): (C) 1-x-y Gd x Ni y )O 2 (1) [In the formula, x represents a numerical value in the range of 0.02 to 0.3, and y represents a numerical value in the range of 0.02 to 0.3.] A mixed conducting oxide represented by 1. A fuel electrode for an electrochemical cell comprising:

2. 2. The fuel electrode for an electrochemical cell according to claim 1, wherein the mixed conducting oxide is supported on the surfaces of the electronically conducting oxide particles and the ionically conducting oxide particles.

3. The electronic conductive oxide particles have the following composition formula (2): The 1-z M z TO 3 (2) [In the formula, M represents at least one element selected from the group consisting of Ca and Sr, and z represents a numerical value in the range of 0.4 to 0.8.] 2. The fuel electrode for an electrochemical cell according to claim 1, characterized in that it is made of a perovskite type oxide represented by the formula:

4. The ion-conductive oxide particles have the following composition formula (3): Yes 1-n A n O 2 (3) [In the formula, A represents at least one element selected from the group consisting of Gd and Sm, and n represents a numerical value in the range of 0.05 to 0.3.] 2. The fuel electrode for an electrochemical cell according to claim 1, characterized in that it is made of an oxide represented by the formula:

5. obtaining a porous body comprising electronically conductive oxide particles and ionically conductive oxide particles; a step of impregnating the porous body with a solution containing Ce ions, Gd ions and Ni ions, and firing the porous body to obtain the fuel electrode for electrochemical cells according to any one of claims 1 to 4; 2. A method for producing an anode for an electrochemical cell, comprising:

6. 5. An electrochemical cell comprising the fuel electrode for an electrochemical cell according to claim 1, an air electrode, and a solid electrolyte layer.

Citation Information

Patent Citations

  • Solid oxide fuel cell and method for manufacturing the same

    JP2012033418A