Cross-linked polyolefin molding and method for producing the same
By integrating a silane crosslinked polyolefin resin with cyclodextrin compounds, the crosslinking density is increased, addressing the need for enhanced durability in high-temperature applications.
Patent Information
- Application Number
- JP2023043419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-17
AI Technical Summary
Crosslinked polyolefin molded articles require a higher degree of crosslinking to enhance durability in high-temperature environments.
Incorporating a silane crosslinked polyolefin resin with a cyclodextrin compound, specifically cyclodextrin or cyclodextrin derivatives, to increase the crosslinking density, along with a controlled production process involving plasticization, molding, and crosslinking steps.
The method significantly enhances the degree of crosslinking, improving the long-term durability and mechanical strength of the polyolefin molded articles.
Smart Images

Figure 2024132585000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinked polyolefin molded article and a method for producing the same. [Background technology]
[0002] Crosslinked polyolefin molded articles are excellent in heat resistance, mechanical strength, flexibility, light weight, etc. For this reason, crosslinked polyolefin molded articles are used for crosslinked polyolefin pipes such as water supply / hot water supply piping and floor heating piping. Crosslinked polyolefin pipes are used in environments where they are exposed to high-temperature water for long periods of time, and therefore they are required to have the durability to withstand such long-term use. In general, in crosslinked polyolefin molded articles, the creep performance required for long-term use at high temperatures correlates with the degree of crosslinking, and therefore crosslinked polyolefin molded articles with an increased degree of crosslinking are in demand.
[0003] For example, a crosslinked polyolefin molded article has been proposed in which a polyethylene base resin with specific physical properties is mixed with specific amounts of a silane compound and a radical generator to form a silane-modified polyethylene composition, which is then molded into a ring shape and crosslinked by a silal condensation reaction (Patent Document 1).The invention described in Patent Document 1 aims to improve the pressure resistance of the crosslinked polyolefin molded article. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4066114 Summary of the Invention [Problem to be solved by the invention]
[0005] However, there is a demand for a crosslinked polyolefin molded article with a higher degree of crosslinking. Therefore, an object of the present invention is to provide a cross-linked polyolefin molded article having a higher degree of cross-linking. [Means for solving the problem]
[0006] The present invention has the following aspects. <1> Contains a silane-crosslinked polyolefin resin and a cyclodextrin compound, The cyclodextrin compound is at least one selected from cyclodextrin and a cyclodextrin inclusion compound, The cyclodextrin inclusion compound is a crosslinked polyolefin molded article comprising at least one member selected from the group consisting of cyclodextrin and cyclodextrin derivatives, and a polyolefin having a viscosity average molecular weight Mv of 300 to 30,000. <2> The silane-crosslinked polyolefin resin is a silane-crosslinked polyethylene resin. <1> The crosslinked polyolefin molded article according to claim 1. <3> The cyclodextrin compound includes the cyclodextrin inclusion compound, The polyolefin constituting the cyclodextrin inclusion compound is polyethylene. <1> or <2> The crosslinked polyolefin molded article according to claim 1. <4> Density: 0.900~0.950g / cm 3 That is, <1> ~ <3> 2. The crosslinked polyolefin molded article according to claim 1 .
[0007] <5> A step (A) of plasticizing a resin composition containing a raw material polyolefin resin and a cyclodextrin compound in the presence of a silane compound; (B) a step of molding the plasticized resin composition into a desired shape to obtain an uncrosslinked molded product; and (C) a step of crosslinking the raw material polyolefin resin of the uncrosslinked molded body to obtain a silane-crosslinked polyolefin resin and obtain a crosslinked polyolefin molded body, The cyclodextrin compound is at least one selected from cyclodextrin and a cyclodextrin inclusion compound, The cyclodextrin inclusion compound comprises at least one selected from cyclodextrin and cyclodextrin derivatives, and a polyolefin having a viscosity average molecular weight Mv of 300 to 30,000, in accordance with a method for producing a crosslinked polyolefin molded article. <6> The raw material polyolefin resin is a polyethylene resin. <5> A method for producing the crosslinked polyolefin molded article according to claim 1. <7> The cyclodextrin compound includes the cyclodextrin inclusion compound, The polyolefin constituting the cyclodextrin inclusion compound is polyethylene. <5> or <6> A method for producing the crosslinked polyolefin molded article according to claim 1. Effect of the Invention
[0008] According to the crosslinked polyolefin molded article of the present invention, the degree of crosslinking can be further increased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] (Crosslinked polyolefin molded body) The crosslinked polyolefin molded article produced by the production method of the present invention is a molded article containing a silane-crosslinked polyolefin resin, which is a silane-crosslinked product of a polyolefin resin, a silane compound, and a cyclodextrin compound. The silane-crosslinked polyolefin resin is a polyolefin resin into which a silane group has been introduced, which is crosslinked as a result of the silane group reacting with water.
[0010] The shape of the crosslinked polyolefin molded article is appropriately determined depending on the application. When the crosslinked polyolefin molded article is used as a pipe for water supply or hot water supply, a pipe for floor heating, or the like, the shape of the crosslinked polyolefin molded article is a cylindrical or polygonal tubular shape. The size of the crosslinked polyolefin molded article is generally determined according to the application it is used in. When the crosslinked polyolefin molded article is a pipe, it preferably has an outer diameter of 6 to 200 mm, a thickness of 1 to 30 mm, and a length of 0.3 to 200 m.
[0011] The crosslinked polyolefin molded article may be a multi-layered molded article having at least one covering layer and one reinforcing layer on one side, both sides, or in the middle. The material of the coating layer is preferably a flexible thermoplastic resin. Examples of such thermoplastic resins include polyolefin, polyvinylidene fluoride, and polyamide. The thermoplastic resin may be a single type or a combination of two or more types. The thickness of the covering layer is preferably 0.01 to 5 mm, more preferably 0.05 to 0.2 mm. The material of the reinforcing layer is preferably a metal. Examples of the material of the reinforcing layer include aluminum and copper. The multi-layer molded article is produced, for example, by multi-layer extrusion molding.
[0012] <Resin> The resin constituting the crosslinked polyolefin molded article includes a silane-crosslinked polyolefin resin, such as a silane-crosslinked polyethylene resin, a silane-crosslinked polypropylene resin, or a mixture thereof.
[0013] The density of the crosslinked polyolefin molded body is not particularly limited, but is preferably 0.900 to 0.950 g / cm. 3 is preferable, and 0.920 to 0.950 g / cm 3 More preferably, 0.930 to 0.950 g / cm 3 is more preferable. When the density is equal to or higher than the lower limit, the strength of the crosslinked polyolefin molded article can be further increased. When the density is equal to or lower than the lower limit, the efficiency of the progress of the crosslinking reaction can be further increased. The density is a value measured by the underwater displacement method in accordance with JIS K 7112. In the multi-layer molded article, the density of the crosslinked polyolefin molded article does not include the coated portion.
[0014] The crosslinking degree of the crosslinked polyolefin resin is preferably 65 to 100%, more preferably 70 to 100%, further preferably 75 to 100%, and particularly preferably 80 to 100%. When the crosslinking degree is equal to or higher than the lower limit, the long-term durability of the crosslinked polyolefin molded article can be further improved. The degree of crosslinking is adjusted by combining the type of raw material polyolefin resin, the amount of the silane compound, the heating temperature in step (C), and the like, which will be described later. The degree of crosslinking is represented by the gel fraction.
[0015] <Cyclodextrin compounds> The cyclodextrin compound is at least one selected from cyclodextrin and a cyclodextrin inclusion compound. By including the cyclodextrin compound, the crosslinked polyolefin molded article can have a higher degree of crosslinking.
[0016] Examples of cyclodextrin include α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, etc. Among them, β-cyclodextrin is preferred as the cyclodextrin.
[0017] The cyclodextrin inclusion compound includes at least one selected from cyclodextrin and cyclodextrin derivatives, and a low-molecular-weight polyolefin. One embodiment of the cyclodextrin inclusion compound is a compound in which a low-molecular-weight polyolefin is included in cyclodextrin or a cyclodextrin derivative.
[0018] The cyclodextrin derivative means a compound in which some hydrogen atoms of the hydroxyl group of cyclodextrin are replaced with other substituents. The type of the substituent is not particularly limited, and for example, a monovalent group that can be substituted with the hydrogen atom of the hydroxyl group of cyclodextrin can be widely applied, and specifically, a hydrocarbon group having 1 to 20 carbon atoms, a hydroxyalkyl group having 1 to 20 carbon atoms, an acyl group having 1 to 20 carbon atoms, etc. can be mentioned. Among them, as the substituent, a hydroxyalkyl group having 1 to 20 carbon atoms is preferable, a hydroxyalkyl group having 2 to 4 carbon atoms is more preferable, and a hydroxypropyl group is even more preferable. That is, as the cyclodextrin derivative, a hydroxyalkylated cyclodextrin is preferable, and a hydroxypropylated cyclodextrin is more preferable. As described later, the cyclodextrin derivative is preferably a β-cyclodextrin derivative since it has a membered ring that easily incorporates polyolefins.
[0019] The cyclodextrin derivative used in the cyclodextrin inclusion compound may be one type alone or a combination of two or more types. The cyclodextrin derivative used in the cyclodextrin inclusion compound may be two or more types in combination with cyclodextrin.
[0020] The viscosity average molecular weight Mv of the low molecular weight polyolefin constituting the cyclodextrin clathrate compound is 30,000 or less, preferably 10,000 or less, more preferably 4,000 or less. When Mv is equal to or less than the upper limit, the degree of crosslinking of the silane-crosslinked polyolefin resin can be further increased. The lower limit of the viscosity average molecular weight Mv of the low molecular weight polyolefin is substantially 300 or more.
[0021] The low molecular weight polyolefin preferably has a structure similar to that of the raw material polyolefin resin described below. For example, when the raw material polyolefin resin is polyethylene, it is desirable to use polyethylene as the low molecular weight polyolefin.
[0022] The molecular structure of the low molecular weight polyolefin may be partially substituted with a substituent. The type of the substituent is not particularly limited, and examples thereof include polyolefins grafted with maleic anhydride. The low molecular weight polyolefin is preferably a polyolefin without a substituent so that it can be easily incorporated into the member ring of the cyclodextrin derivative.
[0023] An example of a method for producing a cyclodextrin inclusion compound is described below. A mixed powder is obtained by mixing 2 to 10 parts by mass of cyclodextrin or a cyclodextrin derivative with 1 part by mass of low molecular weight polyolefin. The mixed powder is heated and pressed to obtain a cyclodextrin inclusion compound. The heating temperature of the hot press is, for example, 150 to 200° C. The heating time of the hot press is, for example, 0.5 to 3 hours. The formation of cyclodextrin inclusion compounds is 1 This can be confirmed by the appearance of a peak at a position different from that of cyclodextrin or a cyclodextrin derivative by H-NMR.
[0024] The content of the cyclodextrin compound is preferably 0.05 to 10 mass%, more preferably 0.05 to 5 mass%, and even more preferably 0.05 to 2 mass%, calculated as cyclodextrin, based on the total resin mass of the crosslinked polyolefin molded article. When the content of the cyclodextrin compound is equal to or more than the lower limit, the degree of crosslinking of the crosslinked polyolefin molded article can be further increased. When the content of the cyclodextrin compound is equal to or less than the upper limit, the physical properties of the crosslinked polyolefin molded article can be better maintained.
[0025] The silane compound will be described later in the process for producing a crosslinked polyolefin molded article.
[0026] (Method of manufacturing crosslinked polyolefin molded article) The method for producing a crosslinked polyolefin molded article of the present invention comprises the steps of: (A) plasticizing a resin composition in the presence of a silane compound; (B) molding the plasticized resin composition into an arbitrary shape to obtain an uncrosslinked molded article; and (C) crosslinking the raw material polyolefin resin of the uncrosslinked molded article to obtain a silane-crosslinked polyolefin resin, thereby obtaining a crosslinked polyolefin molded article.
[0027] <Process (A)> Step (A) is a step of plasticizing a resin composition. The resin composition contains a raw material polyolefin resin and a cyclodextrin compound. Through step (A), a PO-silane polymer is obtained in which a silane compound is graft-polymerized onto the polyolefin resin. Step (A) may be carried out in the presence of a radical generator, if necessary.
[0028] The plasticization is carried out by heating and kneading the resin composition. As a kneading method, for example, a method of melting and extruding the mixture in an extruder having a screw can be mentioned. The temperature during kneading is, for example, preferably from 120 to 220°C, and more preferably from 200 to 210°C.
[0029] <Raw material polyolefin resin> Examples of the raw material polyolefin resin include homopolymers of olefins such as ethylene and propylene, and copolymers of olefins and α-olefins. The α-olefin is not particularly limited, but examples thereof include α-olefins having 3 to 10 carbon atoms, preferably 3 to 6 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, and 1-octene. The α-olefins may be used alone or in combination of two or more kinds.
[0030] The method for producing the raw material polyolefin resin is not particularly limited, but examples include a method in which an olefin alone or an olefin and an α-olefin are polymerized in one step or in multiple steps by a known polymerization method using any polymerization catalyst to obtain an uncrosslinked polyolefin resin.
[0031] The raw material polyolefin resin may be used alone or in combination of two or more kinds.
[0032] The content of the raw material polyolefin resin relative to the total mass of the resin in the resin composition is preferably 90% by mass or more, more preferably 95% by mass or more, and may be 100% by mass.
[0033] The density of the raw material polyolefin resin is not particularly limited, but is preferably 0.920 to 0.955 g / cm 3 is preferable, and 0.930 to 0.950 g / cm 3 More preferably, 0.935 to 0.945 g / cm 3 is more preferred.
[0034] If the density of the raw material polyolefin resin is equal to or higher than the lower limit, the degree of crosslinking of the crosslinked polyolefin molded article is increased, whereas if the density of the raw material polyolefin resin is equal to or lower than the upper limit, the flexibility of the crosslinked polyolefin molded article is increased.
[0035] The density of the raw material polyolefin resin is a value measured by an underwater displacement method in accordance with JIS K 7112.
[0036] The melt flow rate (MFR) of the uncrosslinked raw polyolefin resin is not particularly limited, but is preferably 0.01 to 10 g / 10 min. If the MFR of the uncrosslinked raw polyolefin resin is equal to or higher than the lower limit, the molecular weight of the uncrosslinked raw polyolefin resin is reduced, improving the flowability and improving the moldability. If the MFR of the uncrosslinked raw polyolefin resin is equal to or lower than the upper limit, the long-term durability of the crosslinked polyolefin molded article is improved.
[0037] The MFR of the uncrosslinked raw material polyolefin resin is a value measured in accordance with JIS K 7210-1 under conditions of a temperature of 190° C. and a load of 2.16 kg.
[0038] <Radical generator> The radical generator functions as a so-called crosslinking agent. The radical generator may be, for example, organic peroxide or organic perester, specifically, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3,1,4-bis(tert-butylperoxyisopropyl)benzene, lauroyl peroxide, tert-butyl peracetate, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butyl perbenzoate, tert-butyl perphenyl acetate, tert-butyl perisobutyrate, tert-butyl per-sec-octoate, tert-butyl perpivalate, cumyl perpivalate, and tert-butyl perdiethyl acetate. Among these, benzoyl peroxide is preferred.
[0039] As the radical generator, in addition to the above, for example, an azo compound such as azobisisobutylnitrile or dimethylazoisobutyrate may be used.
[0040] The radical generator may be used alone or in combination of two or more kinds.
[0041] The amount of the radical generator added to the resin composition is preferably 0.01 to 0.3 parts by mass, more preferably 0.01 to 0.2 parts by mass, and even more preferably 0.01 to 0.15 parts by mass, based on 100 parts by mass of the resin composition. If the amount of the radical generator added is equal to or greater than the lower limit, the crosslinking reaction proceeds sufficiently. If the amount of the radical generator added is equal to or less than the upper limit, odor problems can be prevented.
[0042] <Silane compounds> The silane compound functions as a so-called crosslinking agent. The silane compound is a silane compound having an olefin-based unsaturated bond and a hydrolyzable organic group. As a silane compound having such characteristics and being preferred for use in the present invention, for example, there is vinyltrisalkoxysilane, among which vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltris(methoxyethoxy)silane are preferred. In addition, vinylmethyldiethoxysilane, vinylphenyldimethoxysilane, etc. may also be used. The silane compounds may be used alone or in combination of two or more kinds.
[0043] The content of the silane compound in the resin composition is preferably 0.1 to 3.0 parts by mass, more preferably 0.1 to 2.0 parts by mass, and even more preferably 0.1 to 1.5 parts by mass, based on 100 parts by mass of the raw material polyolefin resin. When the amount of the vinylsilane compound added is equal to or greater than the above lower limit, the crosslinking reaction proceeds sufficiently. If the amount of the vinylsilane compound added is equal to or less than the above upper limit, the odor of the pipe can be suppressed.
[0044] <Cyclodextrin compound> The content of the cyclodextrin compound in the resin composition is preferably 0.05 to 10 mass %, more preferably 0.05 to 5 mass %, and even more preferably 0.05 to 2 mass %, calculated as cyclodextrin, relative to the total mass of the resin composition. When the content of the cyclodextrin compound is equal to or more than the lower limit, the degree of crosslinking of the silane-crosslinked polyolefin resin can be further increased. When the content of the cyclodextrin compound is equal to or less than the upper limit, the strength decrease of the molded article can be suppressed.
[0045] <Other optional ingredients> The resin composition may contain optional components such as a crystal nucleating agent, a process heat stabilizer, an ultraviolet absorber, an organic filler, an inorganic filler, a pigment, a dye, and a processing aid, as necessary. The resin composition may also contain a silanol condensation catalyst. By containing the silanol condensation catalyst in the resin composition, crosslinking of the polyolefin resin can be further promoted in the step (C) described later. The silanol condensation catalyst used in the present invention is not particularly limited as long as it is any compound generally used as a catalyst for promoting dehydration condensation between silanols, and examples thereof include compounds such as dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin diacetate, dibutyltin dioctoate, stannous acetate, cobalt naphthenate, lead naphthenate, ethylamine, dibutylamine, hexylamine, and pyridine; inorganic acids such as sulfuric acid and hydrochloric acid; and organic acids such as toluenesulfonic acid, acetic acid, stearic acid, and maleic acid. Among these, dibutyltin dilaurate and dioctyltin dilaurate are preferred. The silanol condensation catalyst may be used alone or in combination of two or more kinds.
[0046] <Process (B)> In step (B), the resin composition (plasticized product) plasticized in step (A) is molded into a desired shape, which is then cooled and solidified to obtain an uncrosslinked molded product. In the uncrosslinked molded product, the polyolefin resin is not crosslinked in whole or in part.
[0047] Examples of methods for molding the resin composition include extrusion molding. Examples of extrusion molding include a method in which a plasticized material is discharged from a die into an arbitrary shape, and then drawn off to form a plasticized material, and then the plasticized material is cooled to obtain an uncrosslinked molded product. Alternatively, a method in which a resin composition is injected into a mold having a core and a cavity, and then the uncrosslinked molded product is removed from the mold can be used.
[0048] The cooling rate for the uncrosslinked molded product immediately after molding is, for example, preferably 10 to 200°C / min, more preferably 50 to 200°C / min. When the cooling rate is equal to or higher than the lower limit, the spherulite radius of the silane-crosslinked polyolefin resin can be made smaller. When the cooling rate is equal to or lower than the upper limit, the load on the cooling and solidifying equipment can be reduced. The cooling rate can be adjusted by combining the cooling method, the temperature of the cooling water, and the like.
[0049] <Process (C)> Step (C) is a step of crosslinking a part or the whole of the polyolefin resin (PO-silane polymer) in the uncrosslinked molded article to form a silane-crosslinked polyolefin resin, thereby converting the uncrosslinked molded article into a crosslinked polyolefin molded article.
[0050] As a method for crosslinking the polyolefin resin of the uncrosslinked molded body, for example, a method of heating the uncrosslinked molded body (thermal crosslinking method) can be mentioned. A preferred example of the thermal crosslinking method is a method (water crosslinking) in which an uncrosslinked molded body is filled with water or steam and then subjected to a heat treatment to crosslink a part or all of the uncrosslinked polyolefin resin. Examples of the heating method include a method of heating the uncrosslinked molded body at a desired temperature in a heating furnace, a method of heating the uncrosslinked molded body by blowing steam at a desired temperature onto the uncrosslinked molded body, and a method of heating by infrared irradiation.
[0051] The heating temperature is preferably equal to or lower than the melting point of the uncrosslinked polyolefin resin contained in the uncrosslinked molded product. The heating temperature is, for example, preferably 40 to 120°C, more preferably 60 to 120°C, and even more preferably 80 to 120°C. If the heating temperature is equal to or higher than the lower limit, the crosslinking treatment of the uncrosslinked polyolefin resin can be carried out in a shorter time. If the heating temperature is equal to or lower than the upper limit, deformation or damage of the crosslinked polyolefin molded product can be suppressed.
[0052] The crosslinked polyolefin molded article is obtained by molding a part or the whole of the polyolefin resin being crosslinked in the presence of a cyclodextrin compound, thereby increasing the degree of crosslinking. EXAMPLES
[0053] Next, the present invention will be described in detail with reference to examples. (Raw materials used) <Raw polyolefin resin> Polyethylene resin (PE): Creolex K4750 (manufactured by Asahi Kasei Corporation), density 0.947 g / cm 3 , MFR5.0g / 10min.
[0054] <Cyclodextrin compounds> Cyclodextrin (CD): β-cyclodextrin, manufactured by CycloChem. Cyclodextrin inclusion compound (CD-HP / PE1): Prepared by Manufacturing Method 1 below.
[0055] <Low molecular weight polyolefin> Excelex 07500 (PE1) manufactured by Mitsui Chemicals, viscosity average molecular weight Mv = 700. The viscosity average molecular weight Mv is the molecular weight measured by the viscosity method. The viscosity method is a measurement method that utilizes the fact that the viscosity η of a polymer solution is a function of the average molecular weight as shown in formula (1). η = kMα (1) (In equation (1), k and α are constants specific to the polymer.)
[0056] <Production Method 1> Preparation of CD-HP / PE1 A mixed powder was prepared by mixing 3 parts by mass of a cyclodextrin derivative (hydroxypropylated β-cyclodextrin (CD-HP), manufactured by CycloChem) and 1 part by mass of a low molecular weight polyolefin (Excelex 07500 (PE1), manufactured by Mitsui Chemicals, Inc., viscosity average molecular weight Mv=700). The mixed powder was melted at 180°C for 1 hour using a hot press and then cooled using a cooling press to obtain a cyclodextrin inclusion compound (CD-HP / PE1).
[0057] Cyclodextrin inclusion compound (CD-HP / PE2): Prepared using Manufacturing Method 2 below.
[0058] <Production Method 2> Preparation of CD-HP / PE2 A cyclodextrin inclusion compound (CD-HP / PE2) was obtained in the same manner as in Production Example 1, except that EXCEREX 40800 (PE2, manufactured by Mitsui Chemicals, Inc., viscosity average molecular weight Mv=4000) was used instead of PE1.
[0059] <Comparison of cyclodextrin compounds> Cyclodextrin derivatives (CD-HP): Hydroxypropylated β-cyclodextrin. Cyclodextrin derivative (CD-M): Methylated β-cyclodextrin.
[0060] <Silane compounds> Vinyltrimethoxylane. <Radical generator> ·2,5-Dimethyl-2,5-di(peroxybenzoate)hexane.
[0061] Example 1 100 parts by mass of a resin composition containing 99% by mass of polyethylene resin (PE) and 1.0% by mass of cyclodextrin (CD) were fed to a Labo Plastomill, melted and kneaded with 2.6 parts by mass of vinyltrimethoxylane and 0.26 parts by mass of 2,5-dimethyl-2,5-di(peroxybenzoate)hexane to obtain a plasticized product (step (A)). The plasticized product was molded into a sheet, which was cooled and solidified to obtain an uncrosslinked molded product (step (B)). The obtained uncrosslinked molded body was immersed in 80°C hot water for 16 hours and subjected to heat treatment to obtain a crosslinked polyolefin molded body (step (C)). The crosslinking degree of the obtained crosslinked polyolefin molded body was measured, and the results are shown in Table 1.
[0062] Example 2 A crosslinked polyolefin molded article was obtained in the same manner as in Example 1, except that the polyethylene resin (PE) was changed from 99% by mass to 98.7% by mass, and the cyclodextrin inclusion compound (CD-HP / PE1) was changed from 1.0% by mass to 1.3% by mass, instead of 1.0% by mass. The crosslinked polyolefin molded article obtained was measured for the degree of crosslinking, and the results are shown in Table 1.
[0063] Example 3 A crosslinked polyolefin molded article was obtained in the same manner as in Example 1, except that the polyethylene resin (PE) was changed from 99% by mass to 98.7% by mass, and the cyclodextrin inclusion compound (CD-HP / PE2) was changed from 1.0% by mass to 1.3% by mass, instead of 1.0% by mass. The crosslinked polyolefin molded article obtained was measured for the degree of crosslinking, and the results are shown in Table 1.
[0064] Comparative Example 1 Except for omitting cyclodextrin (CD), a crosslinked polyolefin molded article was obtained in the same manner as in Example 1. The crosslinking degree of the obtained crosslinked polyolefin molded article was measured. The results are shown in Table 1.
[0065] Comparative Example 2 A crosslinked polyolefin molded article was obtained in the same manner as in Example 1, except that 1.0 mass% of cyclodextrin (CD) was replaced with 1.0 mass% of a cyclodextrin derivative (CD-HP). The crosslinked degree of the obtained crosslinked polyolefin molded article was measured, and the results are shown in Table 1.
[0066] Comparative Example 3 Except for changing 1.0 mass % of cyclodextrin derivative (CD-M) to 1.0 mass % of cyclodextrin (CD), a crosslinked polyolefin molded article was obtained in the same manner as in Example 1. The crosslinking degree of the obtained crosslinked polyolefin molded article was measured, and the results are shown in Table 1.
[0067] (Evaluation method) <Crosslinking degree> To evaluate the degree of crosslinking, the gel fraction was measured by the following method. A higher gel fraction indicates a higher degree of crosslinking. Gel fraction measurement method: Immerse in xylene and heat to 140°C to dissolve the sol components, then divide the mass of the remaining gel by the mass before immersion in xylene to obtain the gel fraction.
[0068] [Table 1]
[0069] As shown in Table 1, in Examples 1 to 3 in which the present invention was applied, the degree of crosslinking was 41.2 to 48.3%. Comparative Example 1, lacking the cyclodextrin compound, had a crosslinking degree of 34.8%. The crosslinking degrees in Comparative Examples 2 and 3, in which a cyclodextrin derivative was used instead of a cyclodextrin compound, were 33.3 to 35.5%. From the above results, it was confirmed that the degree of crosslinking can be increased by applying the present invention.
Claims
1. The composition includes a silane-crosslinked polyolefin resin and a cyclodextrin compound, The cyclodextrin compound is at least one selected from cyclodextrin and a cyclodextrin inclusion compound, The cyclodextrin inclusion compound is a crosslinked polyolefin molded article comprising at least one member selected from the group consisting of cyclodextrin and cyclodextrin derivatives, and a polyolefin having a viscosity average molecular weight Mv of 300 to 30,000.
2. The crosslinked polyolefin molded article according to claim 1 , wherein the silane-crosslinked polyolefin resin is a silane-crosslinked polyethylene resin.
3. The cyclodextrin compound includes the cyclodextrin inclusion compound, 3. The crosslinked polyolefin molded article according to claim 1, wherein the polyolefin constituting the cyclodextrin inclusion compound is polyethylene.
4. Density is 0.900 to 0.950 g / cm 3 3. The crosslinked polyolefin molded article according to claim 1 or 2,
5. A step (A) of plasticizing a resin composition containing a raw material polyolefin resin and a cyclodextrin compound in the presence of a silane compound; (B) a step of molding the plasticized resin composition into a desired shape to obtain an uncrosslinked molded product; and (C) a step of crosslinking the raw material polyolefin resin of the uncrosslinked molded body to obtain a silane-crosslinked polyolefin to obtain a crosslinked polyolefin molded body, The cyclodextrin compound is at least one selected from cyclodextrin and a cyclodextrin inclusion compound, The cyclodextrin inclusion compound comprises at least one selected from the group consisting of cyclodextrin and cyclodextrin derivatives, and a polyolefin having a viscosity average molecular weight Mv of 300 to 30,000.
6. The method for producing a crosslinked polyolefin molded article according to claim 5, wherein the raw material polyolefin resin is a polyethylene resin.
7. The cyclodextrin compound includes the cyclodextrin inclusion compound, The method for producing a crosslinked polyolefin molded article according to claim 5 or 6, wherein the polyolefin constituting the cyclodextrin inclusion compound is polyethylene.
Citation Information
Patent Citations
Hydrosilylation
JP1993132489A
Food packaging film and packaged food
JP1999315213A
Grafted cyclodextrin
JP2004197084A
Elastomer composition, crosslinked elastomer composition, and method for producing crosslinked elastomer composition
JP2018154822A
Polyolefin resin composition, method for producing the same, molding
JP2018162429A