Corrosion detection program, corrosion detection method, information processing device and corrosion detection device
The four-electrode method allows for accurate detection of internal reinforcing bar corrosion in concrete by measuring polarization resistance, addressing the inaccuracy of conventional methods and enabling precise corrosion rate assessment.
Patent Information
- Application Number
- JP2023043454
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-17
AI Technical Summary
Conventional methods cannot accurately detect the polarization resistance of internal reinforcing bars from the surface of concrete structures, which is crucial for assessing corrosion as it progresses internally before visible cracks appear.
A corrosion detection method using a four-electrode arrangement with two first electrodes on the concrete surface and two second electrodes spaced apart, measuring potential differences with alternating current power to calculate polarization resistance, and converting to a two-electrode arrangement for accurate measurement.
Enables accurate detection of polarization resistance of internal reinforcing bars from the concrete surface, allowing for precise assessment of corrosion rates.
Smart Images

Figure 2024132611000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a corrosion detection program, a corrosion detection method, an information processing device, and a corrosion detection device. [Background technology]
[0002] In recent years, concrete structures that were constructed in large numbers during the period of rapid economic growth are becoming increasingly dilapidated. In concrete structures, reinforcing bars installed inside the concrete corrode due to aging. As corrosion progresses, the reinforcing bars expand, which may cause the covering concrete to lift or fall off. Corrosion of reinforcing bars progresses internally before it becomes evident on the surface of the concrete, such as cracks.
[0003] Therefore, a detection method is known in which the polarization resistance of the surface of the reinforcing bar inside the concrete is measured to detect the corrosion rate of the reinforcing bar. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] M. Stern AL Geary, “Electrochemical Polarization”, Journal of the Electrochemical Society, Vol. 104 No. 1 p. 56-63, 1957. [Non-Patent Document 2] Keddam M, Novoa XR, Vivier V, “The concept of floating electrode for contact-less electrochemical measurements: Application to reinforcing steel-bar corrosion in concrete”, Corrosion Science Vol.51, pp.1795-1801, 2009. [Non-Patent Document 3] Keddam M, Novoa XR, Puga B, Vivier V, “Impedance based method for non-contact determination of the corrosion rate in buried metallic structures”, European Journal of Environmental and Civil Engineering, Vol. 15, pp. 1097-1103, 2011. [Non-Patent Document 4] Toshinori Kanemitsu and Shinpei Ono, “Proposal of a completely non-destructive method for evaluating the corrosion rate of rebars inside concrete”, Journal of the Japan Society of Civil Engineers, Vol. 76, No. 4, pp. 315-331, 2020. Summary of the Invention [Problem to be solved by the invention]
[0005] However, conventional detection methods cannot accurately detect the polarization resistance of the reinforcing bars inside the concrete from the surface.
[0006] The present invention has been made in consideration of the above, and aims to provide a corrosion detection program, a corrosion detection method, an information processing device, and a corrosion detection device that can accurately measure the polarization resistance of reinforcing bars inside concrete from the surface thereof. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems and achieve the object, the corrosion detection program of the present invention arranges two first electrodes at a distance from each other on the surface of concrete with rebar installed inside, arranges two second electrodes inside or outside the two first electrodes at a distance from each other and in a straight line with respect to the two first electrodes, calculates the polarization resistance of a four-electrode arrangement from measurement data obtained by applying AC power to the two first electrodes at frequencies changed within a predetermined frequency range and measuring the potential difference between the two second electrodes, and causes a computer to execute a process of calculating the polarization resistance of a two-electrode arrangement from the calculated polarization resistance of the four-electrode arrangement based on a predetermined measurement area of the rebar surface and a predetermined conversion coefficient that converts the four-electrode arrangement into a two-electrode arrangement using two first electrodes. Effect of the Invention
[0008] The present invention has an effect of being able to accurately detect the polarization resistance of reinforcing bars inside concrete from the surface thereof. [Brief description of the drawings]
[0009] [Figure 1] Figure 1 is a schematic diagram of the corrosion reaction of rebar inside concrete. [Diagram 2] FIG. 2 is a conceptual diagram of the relationship between overpotential and external current density. [Diagram 3] FIG. 3 is a diagram showing a schematic configuration example of the AC impedance method. [Figure 4] FIG. 4 is a diagram illustrating the relationship between time delay and measured impedance value. [Diagram 5] FIG. 5 is a diagram showing the simplest equivalent circuit model of the electrode system. [Figure 6] FIG. 6 is a diagram showing a Nyquist line plot of the simplest equivalent circuit model of an electrode system. [Figure 7A] FIG. 7A is a diagram showing a Nyquist plot when measuring reinforced concrete. [Figure 7B] FIG. 7B is a diagram showing an equivalent circuit when measuring reinforced concrete. [Figure 8]FIG. 8 shows an outline of a measurement experiment in a previous study and the measurement results. [Figure 9] FIG. 9 is an application diagram (cross-sectional view) of the non-destructive polarization resistance method. [Figure 10] FIG. 10 shows an equivalent circuit (cross-sectional view) set up by the nondestructive polarization resistance method. [Figure 11A] FIG. 11A is a diagram (cross-sectional view) for explaining the electrical resistance Rs of concrete, one of the three types of resistance that can be measured non-destructively. [Figure 11B] FIG. 11B is a diagram (cross-sectional view) for explaining the low-frequency resistance RfL, one of the three types of resistance that can be measured non-destructively. [Figure 11C] FIG. 11C is a diagram (cross-sectional view) for explaining high-frequency resistance RfH, one of the three types of resistance that can be measured non-destructively. [Figure 12] FIG. 12 is a schematic diagram of a Nyquist plot of the nondestructive polarization resistance method. [Figure 13] FIG. 13 is a cross-sectional view showing an example of a test sample and a terminal arrangement in a four-terminal arrangement. [Figure 14] FIG. 14 is a cross-sectional view showing a test sample and a terminal arrangement in a two-terminal arrangement. [Figure 15] FIG. 15 is a diagram showing an example of an analytical model simulating nondestructive polarization resistance measurement. [Figure 16A] FIG. 16A is a diagram showing the measurement results (Nyquist plot) of a two-terminal arrangement. [Figure 16B] FIG. 16B is a diagram showing the measurement results (Nyquist plot) of a four-terminal arrangement. [Figure 17A] FIG. 17A is a diagram showing the measurement results (Nyquist plot) of a two-terminal arrangement in which the terminal area, which is a corrosion factor, is changed. [Figure 17B] FIG. 17B is a diagram showing the measurement results (Nyquist plot) of a two-terminal arrangement in which the terminal area of the soundness factor is changed. [Figure 18] FIG. 18 is a diagram showing the measurement results (Nyquist plot) of a four-terminal arrangement in which the contact area is changed. [Figure 19A] FIG. 19A is an equivalent circuit of the terminal-mortar interface in a two-terminal configuration. [Figure 19B] FIG. 19B is an equivalent circuit of the terminal-mortar interface in a four-terminal configuration. [Figure 20] FIG. 20 is a diagram showing measurement results (Nyquist plots) obtained by changing the terminal arrangement to a four-terminal arrangement. [Figure 21A] FIG. 21A is a diagram for explaining an analysis example of the current density on the surface of a reinforcing bar. [Figure 21B] FIG. 21B is a diagram for explaining the correspondence between positive and negative current density on the surface of a reinforcing bar and resistance in an equivalent circuit. [Figure 21C] FIG. 21C is a diagram explaining the target range when evaluating the Ani of the reinforcing bar surface. [Figure 22A] FIG. 22A is a diagram showing a method for setting an insulating surface. [Figure 22B] FIG. 22B is a diagram showing an analysis result of the current density on the surface of the reinforcing bar when an insulating surface is set. [Figure 23A] FIG. 23A is a diagram illustrating cut points. [Figure 23B] FIG. 23B is a diagram illustrating cut points. [Figure 23C] FIG. 23C is a diagram illustrating the current density distribution after cutting at the cut point. [Figure 24] FIG. 24 is a cross-sectional view showing an example of a test specimen and an electrode arrangement in a three-electrode method. [Figure 25A] FIG. 25A is a diagram showing the measurement results of impedance by a non-destructive polarization resistance method for a soundness factor. [Figure 25B] FIG. 25B is a diagram showing the measurement results of impedance for soundness factors by a non-destructive polarization resistance method. [Figure 25C] FIG. 25C is a diagram showing the results of impedance measurement by a nondestructive polarization resistance method for corrosion factors. [Figure 25D] FIG. 25D is a diagram showing the results of impedance measurement by a nondestructive polarization resistance method for corrosion factors. [Figure 26] FIG. 26 is a diagram showing the frequency-Real(Z) relationship for the factor that reinforcing bars are not buried. [Figure 27] FIG. 27 is a diagram showing an example of the calculation results of each index by the nondestructive polarization resistance method. [Figure 28A] FIG. 28A is a diagram showing the relationship between the polarization resistance of an internal rebar by analysis and the area measured by a non-destructive method. [Figure 28B] FIG. 28B is a diagram showing the relationship between the polarization resistance of the internal reinforcing bars and the terminal arrangement magnification ratio obtained by analysis. [Figure 29A] FIG. 29A is a diagram showing the results of impedance measurement by the three-electrode method for health factors. [Figure 29B] FIG. 29B is a diagram showing the measurement results of impedance by the three-electrode method for the health factors. [Figure 29C] FIG. 29C is a diagram showing the results of impedance measurement by a three-electrode method for corrosion factors. [Figure 29D] FIG. 29D is a diagram showing the results of impedance measurement by a three-electrode method for corrosion factors. [Diagram 30] Figure 30 is a graph comparing Rp measured by the three-electrode method and Rp-ni(2) measured by the non-destructive polarization resistance method. [Diagram 31] Figure 31 is a graph comparing the nondestructive polarization resistance Rp-ni(2) of corrosion factors and sound factors. [Diagram 32] FIG. 32 is a diagram showing the relationship between Rp-ni(2) and Rp obtained by analysis. [Diagram 33] FIG. 33 is a cross-sectional view of the test specimen and the equally spaced four terminal arrangement. [Diagram 34] FIG. 34 is a diagram comparing the calculation results of Rp-ni(2) obtained by measurements with equal spacing and measurements with outer spacing. [Diagram 35] Figure 35 compares Rp-ni(2), which includes measurement data from previous studies, with Rp. [Diagram 36] Figure 36 is a graph comparing Rp-ni(2) for corrosion factors and soundness factors using measurement data from previous studies. [Figure 37] Figure 37 compares Rp-ni(2) and Rp using measurement data from previous studies. [Figure 38] FIG. 38 is a diagram showing possible fluctuation factors in the nondestructive polarization resistance method. [Figure 39] FIG. 39 is a diagram showing the analytical conditions that serve as the basis for carrying out a parametric study of each factor. [Figure 40A] FIG. 40A is a diagram showing the effect of electrical resistivity ρ on the relationship of Ani to Rp. [Figure 40B] FIG. 40B is a diagram showing the effect of electrical resistivity ρ on the relationship of r2 / 4 to Rp. [Figure 40C] FIG. 40C is a diagram showing the effect of electrical resistivity ρ on the relationship of Rp-ni(2) with respect to Rp. [Figure 41A] FIG. 41A is a diagram showing the effect of the cover c on the relationship of Ani to Rp. [Figure 41B] FIG. 41B is a diagram showing the effect of the fog c on the relationship of r2 / 4 to Rp. [Figure 41C] FIG. 41C is a diagram showing the effect of the cover c on the relationship of Rp-ni(2) with respect to Rp. [Figure 42A] FIG. 42A is a diagram showing the effect of the rebar diameter φ on the relationship of Ani to Rp. [Figure 42B] FIG. 42B is a diagram showing the effect of rebar diameter φ on the relationship of r2 / 4 to Rp. [Figure 42C] FIG. 42C is a diagram showing the effect of the rebar diameter φ on the relationship of Rp-ni(2) with respect to Rp. [Figure 43A] FIG. 43A is a diagram showing the influence of the distance Dout between the two outer terminals on the relationship of Ani to Rp. [Figure 43B] FIG. 43B is a diagram showing the effect of the distance Dout between the two outer terminals on the relationship of r2 / 4 to Rp. [Figure 43C] FIG. 43C is a diagram showing the influence of the distance Dout between the two outer terminals on the relationship of Rp-ni(2) with respect to Rp. [Figure 44A] FIG. 44A is a diagram showing the relationship between the rebar diameter for each cover layer and Ani. [Figure 44B] FIG. 44B is a diagram showing the relationship between the cover and Ani for each rebar diameter. [Diagram 45] FIG. 45 is a diagram showing the relationship between the analysis value of Ani and the difference value ΔAni between the analysis and estimation. [Figure 46] FIG. 46 is a diagram showing the relationship between the distance between the two outer terminals and r2 / 4. [Figure 47] FIG. 47 is a schematic diagram (cross-sectional view) of a concrete specimen. [Figure 48] FIG. 48 is a diagram showing the mix design of concrete test specimens. [Figure 49A] FIG. 49A is a cross-sectional view showing an example of terminal arrangement when measuring a concrete test specimen. [Figure 49B] FIG. 49B is a cross-sectional view showing an example of terminal arrangement when measuring a concrete test specimen. [Figure 50A] FIG. 50A is a diagram showing a Nyquist plot for each interval between two outer terminals. [Figure 50B] FIG. 50B is a diagram showing the relationship between frequency and Real(Z) for each interval between two outer terminals. [Figure 51] FIG. 51 is a diagram showing the relationship between the distance between the two outer terminals and (Rs-RfH) obtained by measurement. [Figure 52] FIG. 52 is a diagram showing the relationship between the distance between the two outer terminals and (Rs-RfH) obtained by analysis. [Diagram 53] FIG. 53 is a diagram showing the non-destructive polarization resistance and corrosion assessment results for each test specimen. [Figure 54] FIG. 54 is a diagram illustrating an example of a schematic configuration of a corrosion detection device according to an embodiment. [Figure 55] FIG. 55 is a diagram showing an example of measurement positions on a concrete structure. [Figure 56] FIG. 56 is a flowchart illustrating an example of a procedure of the corrosion detection process according to the embodiment. [Figure 57] FIG. 57 is a diagram showing a computer that executes a corrosion detection program. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of a corrosion detection program, a corrosion detection method, an information processing device, and a corrosion detection device according to the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to these embodiments. The embodiments can be appropriately combined as long as the processing contents are not contradictory. EXAMPLES
[0011] First, in order to show the difference between the corrosion detection method of the present disclosure and a conventional corrosion detection method, the conventional corrosion detection method will be described.
[0012] [Chapter 1 Previous research] Below, the polarization resistance method will be explained as a previous study.
[0013] 1.1 Polarization resistance method 1.1.1 Measurement theory of polarization resistance method (1) Calculation method of corrosion rate In the polarization resistance method, first, a lead wire is connected to the rebar inside the concrete, and a counter electrode and a reference electrode are installed on the surface or inside the concrete. In the polarization resistance method, a small potential difference is applied between the rebar and the counter electrode to generate a current, and the potential difference, which is the potential change from the potential in a natural state where there is no external action on the rebar against the reference electrode (called the natural potential), is measured. Then, in the polarization resistance method, the polarization resistance of the rebar-concrete interface is calculated by dividing the measured potential difference by the generated current. It has already been clarified that the polarization resistance and the corrosion rate of the rebar surface are inversely proportional to each other (for example, Non-Patent Document 1), and it is possible to convert the polarization resistance into the corrosion rate.
[0014] First, the area around the reinforcing steel inside the concrete is considered to be in an environment where there is a sufficient supply of oxygen and an alkaline aqueous solution. In this environment, the corrosion reaction of the internal reinforcing steel can be expressed by the following anodic reaction in formula (C1) and cathodic reaction in formula (C2).
[0015] [ka]
[0016] Figure 1 is a schematic diagram showing the corrosion reaction of rebar inside concrete. Rebar inside concrete is shown in Figure 1. The anodic reaction of formula (C1) and the cathodic reaction of formula (C2) occur near the rebar inside the concrete. Other electrochemical reactions include oxidation-reduction reactions of divalent and trivalent iron ions, but because the production ratio of each ion is unclear, these are omitted here for simplicity.
[0017] By measuring the current exchanged in equations (C1) and (C2), the rate at which iron dissolves as ferrous ions, i.e., the corrosion rate, can be calculated.
[0018] However, because this electrochemical reaction occurs on the same rebar surface and electrons are exchanged inside the rebar, the current cannot be measured by simply connecting an ammeter. Therefore, the polarization resistance is evaluated by applying an electrical disturbance from outside the rebar and measuring the response. Specifically, a metallic counter electrode and reference electrode are placed on the surface or inside of the concrete, and a potential difference is applied between the rebar and the counter electrode to pass a current, and the response of the potential change from the natural potential between the reference electrode and the rebar is measured.
[0019] The charge transfer rate i (hereinafter referred to as the “external current density”) inside and outside the rebar on the surface of the rebar in concrete is based on the Butler-Volmer equation, expressed as the following equation (1):
[0020]
number
[0021] Where: i0 is the corrosion current density (A / cm 2 ). i a is the anode current density (A / cm 2 ). i cis the cathode current density (A / cm 2 ). η is the overpotential (V). α is the charge transfer coefficient for the cathodic reaction (the charge transfer coefficient for the anodic reaction is 1-α). R is the gas constant (8.314 J / mol K). n is the valence of electrons in the iron ionization reaction, and assuming only equation (C1), n = 2. F is the Faraday constant (96500 C / mol).
[0022] The external current density is the current density exchanged between the anodic and cathodic reactions at the natural potential. Figure 2 shows a conceptual diagram of the overpotential and external current density expressed by equation (1).
[0023] Let us consider the case where the overvoltage η is small. When the overvoltage η is small enough to be approximated by a first order Taylor expansion, the Butler-Volmer equation (1) can be transformed into the following equation (2).
[0024]
number
[0025] Here, the ratio of the overpotential η to the external current density i is the polarization resistance R p (Ωcm 2 ) and the constant part of equation (2) (=RT / nF) is defined as the K value, equation (2) can be transformed into the following equation (3).
[0026]
number
[0027] From this formula (3), if the K value is set in advance, the current density-overpotential relationship in the low overpotential region can be measured and the polarization resistance R p It can be seen that the corrosion current density i0 can be calculated by calculating the K value. In this example, the K value is set to 26 (mV). The corrosion rate of the reinforcing bar surface is calculated as CR (g / cm2 / year), the corrosion current density i0 (A / cm 2 ) can be calculated.
[0028]
number
[0029] Where: M is the atomic weight of iron (55.85). F is the Faraday constant. α is a constant that converts years to seconds (=3.1536×10 7 (second / year)).
[0030] Equation (4) is a formula for calculating the dissolution rate of iron from the electrons generated, based on the half-reaction (equation (C1)) in which iron releases electrons and becomes a divalent ion.
[0031] From the above, it can be seen that the polarization resistance method is a method that can quantitatively evaluate the corrosion rate by measuring the current density-overpotential relationship in the low overpotential region and calculating the polarization resistance.
[0032] There are two main points that make it difficult to quantitatively evaluate the corrosion rate using the polarization resistance method. The first is that in the polarization resistance method, the K value is considered to be a constant and is used to calculate the corrosion rate, but the value changes depending on the reactants that are rate-limiting in the electrochemical reaction, the environmental conditions, and the measurement conditions. The second is that it is unclear which range of the rebar surface being measured is being measured for polarization resistance. The polarization resistance R that can be converted into the corrosion rate p (Ωcm 2 ) is defined as the polarization resistance per unit area of the rebar surface, and is the apparent polarization resistance R, which is the ratio of the overpotential (V) to the applied current (A). ’ p (Ω) is the surface area of the rebar surface into which the measurement current flows, A (cm 2) As a result, formula (3) can also be expressed as the following formula (5).
[0033]
number
[0034] Where: R ’ p is the apparent polarization resistance (Ω). A is the area to be measured (cm 2 ).
[0035] Analytical and experimental studies have been conducted to calculate this, but a highly accurate and rational setting method has not yet been established. In this example, in Chapter 2, we will consider an experimental method for evaluating the measured area.
[0036] 1.1.2 Measurement theory of AC impedance method Figure 3 shows an application diagram of the AC impedance method, which is one of the detailed methods of the polarization resistance method. First, a lead wire is connected to a part of the rebar inside the concrete, and a counter electrode and a reference electrode are installed on the surface of the concrete. Next, a current is passed by applying a potential difference over a wide range of frequencies between the rebar and the counter electrode, and the potential difference between the rebar and the reference electrode is measured. The impedance Z for each frequency is calculated by dividing the measured potential difference by the current. The impedance Z for each frequency is then plotted on a complex plane, and the polarization resistance R of the rebar surface is calculated from its shape. p (Ωcm 2 ) and the electrical resistance of concrete R s (Ω) is separated and calculated. Polarization resistance R p (Ωcm 2 ) to the corrosion rate CR (g / cm 2 The procedure for converting to 10000 yen / year has already been shown in equations (3) and (4).
[0037] Impedance Z is measured by changing the frequency using a potentiogalvanostat with a frequency response analyzer (FRA). Generally, when measuring reinforced concrete, a time delay occurs in the potential response to the applied current due to the effect of the capacitor components contained in the rebar-concrete interface. Figure 4 shows the relationship between the time delay and the measured impedance value.
[0038] When there is a time delay between the applied current and the response potential as shown in Figure 4(a), if the impedance Z is calculated as a complex number, the time delay information can be expressed on the complex plane as phase shift information. On the complex plane, the potential difference measured with the same phase as the applied current is expressed as the real part component Real(Z). Furthermore, the potential difference with a phase shift of 90 degrees to the current is expressed as the imaginary part component Imag(Z). In other words, as shown in Figure 4(b), Real(Z) is the resistance value in DC, and Imag(Z) is expressed as a component reflecting the phase shift. Impedance Z is then expressed by the following equation (6).
[0039]
number
[0040] Here, in order to explain the principle of the AC impedance method, we will assume a reaction on the electrode surface in a solution. The simplest equivalent circuit model of the electrode system is shown in Figure 5. At the interface between the rebar and the solution, positive and negative ions separate when a change in potential occurs, so a capacitor C dl and polarization resistance R p A parallel circuit is formed. There is a solution resistance R s is added in series. The impedance locus on the complex plane is given by equation (7).
[0041]
number
[0042] That is, on the complex plane, there is a radius R p / 2, center coordinate (R s +R p This representation method is also called a Cole-Cole plot, a Nyquist plot, or an impedance plot, but in this embodiment it is called a Nyquist plot.
[0043] In this way, the impedance is measured while changing the frequency of the applied current, the Nyquist plot is displayed on the complex plane, and the polarization resistance R is calculated by performing semicircular curve fitting. p and solution resistance R s The AC impedance method is a method for separating and calculating the above. Curve fitting is the process of fitting an equivalent circuit to a Nyquist plot to obtain quantitative values for each component.
[0044] Next, typical Nyquist plots and assumed equivalent circuits when applying the AC impedance method to reinforced concrete are shown in Figures 7A and 7B. Figure 7A shows the Nyquist plot when measuring reinforced concrete. Figure 7B shows the equivalent circuit when measuring reinforced concrete. In addition to the appearance of a parallel circuit of resistance and capacitance components due to the electrical properties of the rebar-concrete interface, the Warburg impedance Z w Due to this effect, a straight line with a 45 degree inclination may appear in the low frequency range in the Nyquist plot, but by fitting the curved part with a circular arc, the apparent polarization resistance R ’ p Regarding concrete, there are studies that suggest that the interface between the coarse aggregate and the cement paste, and the cement paste itself, have electrical capacitance. Even in such cases, the capacitance C of the rebar-concrete interface is dl is generally two orders of magnitude larger than the capacitance of the concrete itself, and the electrical properties of the two can be separated by frequency band. In the examples, in order to focus on rebar corrosion, concrete is simply treated as a resistive component. From the above, the polarization resistance R can be calculated by curve fitting the semicircle that appears on the low-frequency side in reinforced concrete.’ p It was shown that the corrosion rate can be calculated quantitatively.
[0045] 1.1.3 Corrosion rate evaluation using polarization resistance method A representative example of the use of polarization resistance method for corrosion assessment in previous research is the CEB (European Concrete Board) assessment criteria shown in Table 1, which is used to diagnose corrosion before corrosion cracks occur on the concrete surface.
[0046] [Table 1]
[0047] 1.2 Completely non-destructive electrochemical measurement method The three-electrode polarization resistance method has the problem that, when applied, it is necessary to connect some lead wires to the rebar as shown in Figure 3, which involves partial destruction of the existing structure by drilling holes, etc. To solve this problem, several attempts have been made to measure the corrosion rate from the concrete surface in a completely non-destructive manner. Hereinafter, in this embodiment, the three-electrode polarization resistance method is also referred to as the three-electrode method.
[0048] In previous studies, there have been many attempts to estimate the polarization resistance of internal rebars using the Wenner electrode arrangement, with four electrodes placed on the surface of the concrete. The Wenner electrode arrangement is an arrangement in which four terminals are placed at equal intervals on the surface, with the two outer terminals used to apply voltage and measure current, and the two inner terminals used to measure potential difference. This arrangement is often used to measure the electrical resistivity of concrete, and it is assumed that many of the studies follow this method.
[0049] For example, in Non-Patent Document 2 and Non-Patent Document 3, Keddam et al. carried out measurements of varying cover thicknesses of cement paste in which rebars were embedded, and a reproduction analysis of a non-destructive AC impedance method using a three-dimensional finite element method (FEM), and revealed that the larger the cover thickness, the smaller the semicircular shape of the Nyquist plot. Here, the measurement experiment outline and measurement results of Keddam et al. are shown in FIG. 8. FIG. 8 is a diagram showing the measurement experiment outline and measurement results of previous research. FIG. 8(a) shows the test specimen and terminal arrangement. FIG. 8(b) shows the measurement results. The impedance of the four terminals is calculated by applying a potential difference between WE and CE to measure the current, measuring the potential at RE1 and RE2, and taking the ratio of the measured potential difference to the measured current. As a result, it was shown that the smaller the cover thickness, the smaller the semicircular shape of the Nyquist plot. This tendency is also reproduced by analysis.
[0050] However, previous studies have been unable to accurately detect the polarization resistance of rebars inside the concrete from the surface. For example, in Figure 8(b), even when measuring the same rebar, if the cover changes, the semicircular shape of the Nyquist plot changes, and the polarization resistance also changes. Previous studies have been unable to accurately detect the polarization resistance, and therefore are unable to accurately detect the corrosion rate.
[0051] [Chapter 2 Fundamental study on completely non-destructive corrosion rate evaluation method] 2.1 Introduction In this chapter, we propose the Non-Invasive Polarization Resistance method (NIPR method) as a new completely non-destructive corrosion rate evaluation method, and present the measurement theory and its calculation method. Below, we explain the basic consideration that led to the proposed method (non-destructive polarization resistance method) of this disclosure.
[0052] 2.2 Measurement theory of the non-destructive polarization resistance method The application diagram of the non-destructive polarization resistance method of the present disclosure is shown in FIG. 1、 P 1、 P 2、C2 are placed directly above and parallel to the internal rebars on the concrete surface, and the two outer terminals C 1、 Apply a voltage to C2 and a wideband current to the inner terminal P 1、 This is a method to calculate impedance by measuring the potential difference at terminal C. 1、 P 1、 P 2、 C2 are electrodes. It is not a two-terminal method with two terminals arranged, but the inner two terminals P of the four terminals 1、 The reason for measuring the potential difference at P2, which will be explained in 2.3 below, is to reduce the effects of the contact resistance and polarization resistance at the interface between the terminal (stainless steel) and the concrete, and to enable evaluation of impedance changes due to corrosion. Also, the schematic diagram of the current in Figure 9 shows two paths: the current flowing only through the concrete and the current passing through the inside of the rebar, but it should be noted that the actual current is spatially distributed within the concrete and the rebar. In Figure 9, these two paths are drawn as the average of each current, and were set up to make it easier to interpret the measurement results.
[0053] An equivalent circuit for the non-destructive polarization resistance method corresponding to the two current paths shown in Figure 9 is proposed as Figure 10. This equivalent circuit is made up of the resistance R1 of the current flowing only through the concrete, the resistance R2 of the concrete part of the current flowing inside the rebar, and the resistance R of the rebar surface of the current flowing inside the rebar. ’ p-ni , the capacitance of the rebar surface C, and the resistance inside the rebar R steel Of these, the resistor R ’ p-ni Since it is expected that the polarization resistance of the rebar surface, which can be measured by the three-electrode method, is positively correlated with the corrosion rate, that is, it is expected that the polarization resistance is negatively correlated with the corrosion rate, this index will be focused on. ’ p-ni is also called the apparent nondestructive polarization resistance. The electrical resistivity inside the rebar is 8.9×10 -8 (Ωm) and has almost no effect on the interpretation of the measurement results. steel will no longer be taken into consideration.
[0054] Here, in the conventional three-electrode AC impedance method, the polarization resistance R per unit area of the rebar surface is p (kΩcm 2 ) is an index that can be converted into the corrosion rate. This index is the apparent polarization resistance R ’ p The measured area A (cm2) is the surface area of the rebar into which the measurement current flows (Ω). 2 The nondestructive polarization resistance method disclosed herein also uses the apparent nondestructive polarization resistance R ’ p-ni (Ω), and the surface area of the rebar into which the measurement current flows is defined as the measurement area A of the non-destructive method. ni (cm 2 ) and the converted index is the nondestructive polarization resistance per unit area R p-ni (kΩcm 2 Hereafter, the polarization resistance per unit area measured by the three-electrode method is simply defined as the polarization resistance R p The nondestructive polarization resistance per unit area is simply called the nondestructive polarization resistance R p-ni The measurement area A of the three-electrode method and the measurement area A of the non-destructive method are called ni can be obtained by current dispersion analysis using FEM. The specific method will be described later.
[0055] R1, R2, and R ’ p-ni These three resistance values can be calculated using three types of resistance that can be measured non-destructively from the concrete surface shown in Figures 11A-11C. The three types of resistance that can be measured are the resistance R of concrete without rebar, s (Ω), high-frequency resistance R when current flows into the rebar fH (Ω), the low-frequency resistance R when current flows through the rebar fL (Ω). These resistance values can be interpreted as the combined resistance of the equivalent circuit in Figure 10.
[0056] R obtained from measurements without rebar sThe only resistance component is R1. For high frequency measurements when there is a rebar, the capacitors C and R ’ p-ni In the parallel circuit, current flows to the capacitor C side, and the resistance R ’ p-ni Since no current flows through the 2R side, the parallel circuit is made up of R1 and 2R2. On the other hand, in low-frequency measurements when there is a rebar, the parallel circuit is made up of C and R ’ p-ni In the parallel circuit of ’ p-ni Since current flows through R1 and 2R2+2R ’ p-ni Therefore, the measurable resistance R s , R fH , R fL is expressed by the following equations (8-1), (8-2), and (8-3).
[0057] R s = R1 (8-1)
[0058]
number
[0059] Expanding the above three equations, we obtain the resistance components R1, R2, and R ’ p-ni can be calculated using the following equations (9-1), (9-2), and (9-3).
[0060] R1 = R s (9-1)
[0061]
number
[0062] Next, the apparent nondestructive polarization resistance R ’ p-ni The area to be measured by the non-destructive method, A, is determined by analysis. ni By multiplying by , the nondestructive polarization resistance R is obtained as shown in equation (10). p-nican be calculated.
[0063] R p-ni = A ni ·R ’ p-ni (10)
[0064] Furthermore, as will be shown in "2.3 Consideration of terminal layout method" later, the R p-ni Since the current terminal and potential difference measurement terminal are separate, the measurement results are underestimated compared to the ideal measurement results using a two-terminal arrangement with no effects of contact resistance and polarization resistance, and so it is necessary to convert to that value. In actual measurements using a two-terminal arrangement, contact resistance and polarization resistance have a large effect, making it difficult to calculate the results, but it is possible to calculate the conversion factor by using current dispersion analysis using FEM. Therefore, the conversion factor is defined as the terminal arrangement magnification r 2 / 4 , R with 4-terminal configuration p-ni R p-ni(4) , the nondestructive polarization resistance of an ideal two-terminal arrangement is R p-ni(2) If we define it as above, the conversion formula is expressed as formula (11). p-ni(2) is an index that is expected to correlate with the corrosion rate.
[0065] R p-ni(2) = r 2 / 4 ·R p-ni(4) (11)
[0066] In actual measurements, it is expected that the frequency dependence of the capacitor C will change depending on the cover and diameter of the rebar, the arrangement of the measurement terminals, and the corrosion state of the rebar. fH and low frequency resistance R fLIt becomes unclear which frequency is the appropriate value to use. Therefore, these resistances are calculated by measuring AC impedance using a wide range of frequencies. Figure 12 shows a schematic diagram of a Nyquist plot measured while changing the frequency. Due to the effect of the parallel circuit of the capacitor and resistor, the measured value appears as part of a semicircular plot on the complex plane in Figure 12. By performing curve fitting on a part of this semicircle, Real(Z), the intersection with the real axis on the high frequency side, is calculated as R fH , the low frequency side is R fL On the other hand, the resistance of concrete alone, R s Regarding , since it is already clear that there is almost no change in Real(Z) at frequencies of about 1-100 Hz, the value of Real(Z) at a frequency of 100 Hz is used.
[0067] Hereafter, based on measurement experiments and analysis of mortar test specimens, we will examine the terminal arrangement method in the proposed method, compare the proposed method with conventional methods, and propose a method to correct measurement values due to changes in terminal arrangement and utilize previous research data using this method.
[0068] 2.3 Consideration of terminal layout method 2.3.1 Mortar specimen shape, materials used and mix proportions A small mortar specimen was prepared to evaluate the applicability of the non-destructive polarization resistance method. The factors of the specimen used in 2.4 and 2.5 below are also shown here. The specimen and the terminal arrangement during measurement are shown in Figure 13. Figure 13 shows the specimen 70 and the 4-terminal C 1、 P 1、 P 2、An example of the arrangement of C2 is shown. FIG. 13(a) shows a cross-sectional view of the test specimen 70 in the short direction. FIG. 13(b) shows a cross-sectional view of the test specimen 70 in the long direction. The test specimen 70 had a size of 40 mm×40 mm×160 mm. The buried rebar 71 was made of round steel (SS400) with no black skin, 10 mm in diameter and 140 mm in length, and was covered with epoxy resin 72 for 20 mm each from both ends, so that the central 100 mm was set as the test section. In addition, in order to fix the position of the rebar from the concrete surface, as shown in FIG. 13, the test specimen 70 used a hexagonal nut 73 made of polyvinyl chloride as a spacer to ensure the cover. In the experiment, multiple test specimens 70 were created for each of the following: no rebar, sound rebar, and corroded rebar. The corroded rebar was created by placing the sound rebar in a corrosion acceleration device for 14 days. The corrosion acceleration device was set up so that a 3.0% NaCl aqueous solution was sprayed once a day for three minutes in an atmosphere with a temperature of 40°C and a relative humidity of 80%. To corrode the entire test section of the rebar, the exposed surface was turned upside down on the third day after installation. After corrosion acceleration, corrosion products, mainly red rust, had settled over almost the entire surface. In addition, a coaxial cable used for measuring the three-electrode method was connected to the end of the rebar before the mortar was poured.
[0069] Table 2 shows the mix ratio of the mortar test specimens. Table 3 also shows the factors that were changed in the mortar test specimens. The mix ratio of the test specimens was W / C = 55 (%), C:S = 1:3, and no admixtures such as AE water reducers were used. The factors were the presence or absence of buried rebars, their degree of corrosion, and chloride ion concentration. Depending on the factors, the chloride ion concentration was changed to 0, 3, or 10 (kg / m 3 The materials for the mortar specimens were tap water, research cement manufactured by the Cement Association, and mountain sand (produced in Kimitsu, Chiba Prefecture, with a surface dry density of 2.57 (g / cm3)). 3), water absorption rate 2.40(%), and sodium chloride was NaCl special grade reagent. The names of the specimens in Table 3 are written as (rebar name) (corrosion days) d-CL (chloride ion concentration)-(specimen number). The rebar names are N: no rebar, S: sound rebar, and Cor: corroded rebar. The specimen number is written when multiple specimens under similar conditions are tested. The fresh properties of the mortar at the time of casting are shown in Table 4. These values were calculated using a mortar flow tester conforming to JIS R 5201 and a mortar air meter conforming to JIS A 1171. The flow value was higher and the air volume was lower as the chloride ion content increased. After casting the mortar, the specimens were sealed and cured for two weeks in an atmosphere of 20(℃) and 70(% relative humidity) by wrapping them in polyethylene film.
[0070] [Table 2]
[0071] [Table 3]
[0072] [Table 4]
[0073] 2.3.2 Measurement experiment method When measuring the test specimen, first, four terminals were placed parallel to the longitudinal direction of the rebar on the surface of the mortar and concrete directly above the rebar. The terminals were made of 10mm x 40mm x 10mm stainless steel pieces (SUS404), and the 10mm x 40mm surface was set as the contact surface with the surface of the test specimen, and the terminal length in the longitudinal direction of the rebar was 10mm. The shape of the terminals was such that the larger the contact area, the smaller the contact resistance between the terminal and mortar, so the length perpendicular to the axis of the rebar was made large at 40mm. Stainless steel was used as the material for the terminals, as it is an inexpensive metal with a stable potential. Here, as shown in Figure 13, the two outer terminals C 1、 The interval between C2 and Dout (mm), 2 terminals inside P 1、 The interval between P2 is D in (mm), outer terminal C 1、 C2 and inner terminal P 1、 The interval between P2 is D cp The cover of the test specimen 70 is c=25 (mm). The spacing between the terminals is the minimum spacing between the terminals, not the center spacing between the terminals.
[0074] Next, the outer (inner) 2 terminals C 1、 Apply a sine wave AC voltage with an amplitude of ΔV=30 (mV) at C2 with a frequency of 0.1Hz-10,000Hz, scanning from high to low frequencies, and measure the current between the terminals. 1、 The potential difference was measured at P2, and the impedance was calculated as the ratio of the measured potential difference to the measured current. The reason for setting ΔV=30(mV) is that when measurements were taken at ΔV=10, 20(mV), the variance in the impedance measurements was large in the low frequency range below 10Hz, but when ΔV=30(mV), the variance was improved. The measurement time under these measurement conditions was about 4 minutes and 30 seconds. Terminal C to which the AC voltage is applied 1、 C2 is also called the current terminal, and the terminal P for measuring the potential difference 1、 P2 is also called the potential difference measuring terminal.
[0075] In addition, measurements were performed on the test piece 70 using a two-terminal arrangement. The two-terminal arrangement consisted of two terminals C 1、 The arrangement is such that a voltage is applied at C2, a potential difference is measured, and a current is measured. 1、 An example of the arrangement of C2 is shown. In the case of a two-terminal arrangement, the two-terminal C 1、 The terminal spacing of C2 is defined as D (mm).
[0076] The measurement device used was the MFIA 500kHz impedance analyzer from Zurich Instruments Ltd. This device can measure impedances from 1mΩ to 1TΩ with a basic accuracy of 0.05% from frequencies from 1mHz to 500kHz. A conductive hydrogel sheet was used to contact the terminals and the concrete surface. This is a three-dimensional polymer matrix with water, moisturizers, and electrolytes added, which reduces the contact resistance between the terminals and the surface of the test specimen and can maintain that state for a long time. A sponge soaked in calcium hydroxide solution is often used for electrical measurements of concrete, but when it dries, the contact resistance increases and the noise during measurement increases. On the other hand, the advantage of the hydrogel sheet is that if it is in contact with the concrete when wet, the contact resistance remains low even after it dries.
[0077] 2.3.3 Analysis method A current dispersion analysis was performed using a three-dimensional finite element method (FEM) to reproduce measurements made using the nondestructive polarization resistance method and to analytically examine changes in measurement values due to changes in conditions such as the target and terminal arrangement. Figure 15 shows an example of an analytical model simulating measurements on a mortar specimen. The analytical procedure begins with generating tetrahedral mesh elements that simulate the rebar, terminals, and mortar according to the shape and terminal arrangement in Figure 13. Then, of the four terminals placed on the mortar surface, two current terminals C 1、 Apply a steady-state DC current to the top of C2 and measure the potential difference between the two potential difference measurement terminals P 1、 The purpose of this experiment was to obtain the potential difference on the top surface of P2. The reason for using tetrahedrons as mesh elements is that the geometry of the rebar is curved, and tetrahedrons are mesh elements with less distortion than hexahedrons. The maximum length of one side of an element was 0.56 (cm), and the total number of elements was 105,615.
[0078] The constitutive law used in the analysis is the continuity equation shown in Equation (12). Note that the vectors in the following equations and text are → " is added.
[0079]
number
[0080] Where: σ is the electrical conductivity (1 / Ωm). V is the electrical potential (V). J e → is the externally generated current density (A / m 2 ). The operator ∇ is the vector differential operator.
[0081] The initial charge during the analysis is set to 0, and the mortar surface and terminal surface other than the current application surface of the terminal, the potential difference measurement surface, and the contact surface between the terminal and the mortar are insulated. The current density at the insulated points satisfies equation (13).
[0082] n → J → = 0 (13)
[0083] Where: n → is the normal vector of the mortar surface. J → is the current density (A / m 2 ).
[0084] Furthermore, on the current application surface of the two terminals through which the current flows in and out, the current flows in the same direction as the normal vector of the terminal surface, as shown in (14).
[0085] n → J → = n → J0 → (14)
[0086] Where: J0 → is the current density (A / m 2 ).
[0087] Figure 15 shows the current terminal C 1、 Connect C2 to the potential difference measurement terminal P 1、This is an example of a current terminal C placed outside P2. 1、 Connect C2 to the potential difference measurement terminal P 1、 It is also possible to perform an analysis in which the material is placed inside P2. In this analysis, the electrical resistivity as the electrical resistance per unit volume and the surface resistance per unit area can be set for each geometry. Therefore, the polarization resistance R of the three-electrode method at the reinforcing steel-concrete interface is p (kΩcm 2 ) is set on the surface of the rebar, and this is taken as the true value. The nondestructive polarization resistance R obtained by the four-terminal method or the two-terminal method is p-ni (kΩcm 2 ) is R p The relationship between the potential difference and the value of P 1、 If the average values of the measured potentials on the top surface of P2 are V1 and V2, respectively, the resistance value R obtained by analysis is a (Ω) is defined by the following equation (15).
[0088]
number
[0089] Where: V1 and V2 are potential difference measurement terminals P 1、 is the average potential (V) on the top surface of P2. I is the current value (A).
[0090] In this analysis, steady-state direct current was used, so the capacitive component of the reinforced concrete was not taken into account, and low- and high-frequency measurements were simulated by varying the resistance of the reinforcement-concrete interface.
[0091] The conditions were set by applying a current of +1.0 (μA) in the -Z direction to one of the current terminals (current terminal C1), and the other current terminal (current terminal C2) was grounded. This current value was set based on the value that actually flowed in measurements on the test specimen. When a low-frequency current is applied, the capacitor component is charged in the parallel circuit at the rebar-concrete interface, causing the current to flow through the resistance side, and the resistance of the interface is the polarization resistance R in the three-electrode method. p(kΩcm 2 ) The analytical value at that time is R a =R fL On the other hand, when high-frequency current is applied, the current flows to the capacitor component side at the rebar-concrete interface, so the interface resistance is reduced to the same level as the internal resistance of the rebar. Therefore, the interface resistance is set to 8.9 × 10 -15 (kΩcm 2 ) and the analytical value at that time is R a =R fH (Ω). The resistance of this interface is calculated by dividing the thickness of the reinforcing bar-concrete interface by 1.0×10 -6 (cm), and then add the electrical resistivity inside the rebar (8.9×10 -9 kΩcm) 4) This was calculated by multiplying
[0092] In addition, the input value of the electrical resistivity ρ (Ωm) of the mortar was obtained from the measurement results of the non-destructive polarization resistance method for the factors (N-CL0, N-CL3, N-CL10) where the rebar was not embedded, as shown in Table 3. As shown in Figure 26 below, in the case of only mortar, Real(Z) (Ω) hardly changes depending on the frequency, so Real(Z) at a frequency of 100 Hz was used as the electrical resistivity R of the mortar. s (Ω), the electrical resistivity ρ (Ωm) of the mortar can be calculated using the following equation (16).
[0093] ρ = G p ·R s (16)
[0094] Where: G p is the electrode arrangement coefficient (m). This is a coefficient that converts the resistance value (Ω) obtained by electrical measurement into volume resistivity (Ωm), and is determined by the terminal arrangement method, the shape of the object to be measured, the terminal spacing, etc. p The value of R was calculated by performing a current dispersion analysis with a model of the mortar and terminals without reinforcing bars and a value of ρ = 1-100 (Ωm). s In the analysis simulating the measurement in this chapter, G p =1.94×10-2 The electrical resistivity of the terminal was 8.9×10 -9 (kΩcm), and the contact resistance between the terminal and the mortar is 8.9×10 -15 (kΩcm 2 The shape, dimensions, rebar position, and terminal spacing of the analysis object were determined based on the measurement experiment.
[0095] Based on the above conditions and procedures, R fL (Ω), R fH (Ω) and R s From these resistance values, the resistances R1(Ω), R2(Ω) and apparent non-destructive polarization resistance R related to the electrical resistance of concrete can be calculated. ’ p-ni (Ω). In addition, each R p (kΩcm 2 ) for the set value of the measurement area A of the non-destructive method ni For the calculation of the normal current density (A / m 2 The analysis and interpretation methods are shown below in 2.3.5 along with the results.
[0096] 2.3.4 Comparison of measurement results between 4-terminal and 2-terminal configurations In the measurement theory of the nondestructive polarization resistance method in 2.2 above, a method using a four-terminal arrangement was shown, but the two-terminal arrangement, which applies voltage, measures potential difference, and measures current with one terminal, has a simpler electrode configuration and is therefore more reasonable if no measurement problems arise. Therefore, comparative measurements were carried out between the two-terminal arrangement and the four-terminal arrangement for mortar specimens with sound rebar and corroded rebar embedded in them. In addition, to understand the degree of influence of the resistance between the terminals and the mortar, measurements were carried out by changing the area of the two terminals in the two-terminal arrangement and the area of the potential difference measurement terminal placed on the inside in the four-terminal arrangement.
[0097] In the four-terminal arrangement, the two outer terminals are current terminals C in the same arrangement as in Figure 13. 1、 C2, and the two inner terminals are potential difference measurement terminals P 1、 P2 and D out = 110 (mm), Din = 70 (mm). The two-terminal arrangement was the same as in Figure 14, with D = 110 (mm). In measurements with different terminal areas, D out = 110 (mm), D in = 60 (mm), and for the two-terminal arrangement, D = 100 (mm). From Table 3, one specimen was selected for each of the two factors: sound (S-CL0) and corroded (Cor14d-CL0).
[0098] As a comparison measurement result between the two-terminal arrangement and the four-terminal arrangement, Nyquist plots for each corrosion factor of the rebar are shown in Figures 16A and 16B. Figure 16A is a diagram showing a Nyquist plot measured with the two-terminal arrangement. Figure 16B is a diagram showing a Nyquist plot measured with the four-terminal arrangement. Comparing Figures 16A and 16B, it can be seen that both Real(Z)(Ω) and Imag(Z)(Ω) are much larger with the two-terminal arrangement than with the four-terminal arrangement.
[0099] In addition, when comparing the corrosion factors and soundness factors, the two-terminal arrangement produced plots of almost the same shape, while the four-terminal arrangement produced plots of parts of semicircles in which the corrosion factors were smaller than the soundness factors. This indicates that the two-terminal arrangement did not produce polarization resistance changes due to the corrosion of the internal rebar, whereas the four-terminal arrangement did. The reason for this is that in the two-terminal arrangement, current application and potential difference measurement are performed using the same terminal, so a large current flows through the terminal, and the polarization resistance at the terminal-mortar interface has a large effect on the measurement results, whereas in the four-terminal arrangement, the terminals for current application and potential difference measurement are separate, so almost no current flows into the potential difference measurement terminal, and the polarization resistance at the terminal-mortar interface has almost no effect on the measurement results. In addition, since the terminals are made of sound stainless steel, the polarization resistance at the terminal-mortar interface is thought to be very large.
[0100] In addition, it was predicted that there would be an effect of contact resistance between the potential difference measurement terminals and the mortar interface in both the two-terminal and four-terminal arrangements. Here, contact resistance is defined as the resistance component of the impedance at the terminal-mortar interface that is not dependent on frequency. To verify this, measurements were taken under conditions in which the area of the potential difference measurement terminals was doubled for both corrosion and soundness factors. In the two-terminal arrangement, the area of the two terminals was doubled, and in the four-terminal arrangement, the area of the potential difference measurement terminal placed on the inside was doubled.
[0101] Figures 17A and 17B show the measurement results (Nyquist plots) of two-terminal arrangements for each corrosion factor. Figure 17A shows the measurement results of the corrosion factor. Figure 17B shows the measurement results of the soundness factor. The electrical resistance R of concrete s The high-frequency resistance R fH When the area of both the corrosion factor and sound factor is doubled, fH is the original area R fH It was found that the contact resistance is smaller than that of the contact area in the two-terminal configuration. On the other hand, the shape of the plot hardly changes. This shows that the contact resistance changes due to the change in contact area in the two-terminal configuration.
[0102] Next, Figure 18 shows the Nyquist plots measured by changing the area of the potential difference measurement terminals in a four-terminal arrangement. With the four-terminal arrangement, there is almost no change in the impedance value even when the area of the potential difference measurement terminals is changed. As a result, it was found that the four-terminal arrangement can reduce the effect of the contact resistance at the terminal-mortar interface.
[0103] The reason why the measured impedance value changes can be explained by the equivalent circuit of the terminal-mortar interface for each terminal arrangement in Figures 19A and 19B. Figure 19A is the equivalent circuit of the terminal-mortar interface for the two-terminal arrangement. Figure 19B is the equivalent circuit of the terminal-mortar interface for the four-terminal arrangement. The terminal-mortar interface is the point where the terminal and the mortar surface come into contact, and is connected to the equivalent circuit of the reinforcing steel mortar shown in Figure 10. From the measurement results in Figures 16A, 16B, 17A, and 17B, it is considered that a series circuit of [contact resistance] and [parallel circuit of polarization resistance and capacitor] is formed at the terminal-mortar interface. In the two-terminal arrangement, all the current passes through the circuit shown in Figure 19A and is affected by the resistance in the circuit, making it difficult to detect the change in impedance value due to the corrosion state of the internal reinforcing steel, which is what we want to find. On the other hand, in the four-terminal arrangement shown in Figure 19B, the potential difference measurement terminal P 1、 The current flowing into P2 is small, and the potential difference measurement terminal P 1、 It is believed that the influence of the polarization resistance component between P2 and the mortar is hardly reflected, and it becomes possible to detect changes in impedance values due to the corrosion state of the internal rebar.
[0104] From the above, it became clear that it is difficult to perform measurements using the nondestructive polarization resistance method with a two-terminal arrangement, and that a four-terminal arrangement is necessary.
[0105] 2.3.5 Interpretation of impedance changes due to changes in terminal arrangement In the proposed method of this disclosure, how to arrange the four terminals is an important issue. For the purpose of measuring the electrical resistivity of concrete without buried reinforcing bars, a Wenner arrangement is often used, in which the current terminals are on the outside and the potential difference measurement terminals are on the inside, arranged at equal intervals. Also, in previous studies on completely non-destructive impedance measurement, there are many examples of Wenner arrangement following this. However, in contrast to the case of targeting only concrete, which can be assumed to be electrically homogeneous, in the case of reinforced concrete, since it is a composite of concrete and reinforcing bars, whose electrical properties are significantly different, it is expected that the current flow will be different from that in homogeneous concrete. Therefore, an equal interval arrangement is not necessarily optimal, and it is necessary to reconsider the method of arranging the terminals.
[0106] Therefore, for the small mortar test specimen shown in Fig. 13, the outer two terminal distance D out Fix the current terminal C 1、 C2 and potential difference measurement terminal P 1、 P2 Spacing D cp The measurements were made by changing the current. 1、 Instead of using C2 as the terminal for measuring potential difference, the outside is used as the terminal for measuring potential difference P 1、 P2, inside current terminal C 1、 The measurement was performed by changing the arrangement to C2 and comparing the results before and after the change. In addition, a reproduction analysis of the measurement was performed using current dispersion analysis by FEM, and the measurement area A of the non-destructive method required for quantitative evaluation of the corrosion rate was also performed. ni (cm 2 We also considered the calculation method of
[0107] The factors considered for the terminal arrangement are shown in Table 5. The test specimen used was the small mortar test specimen with soundness factor (S-CL0) shown in Figure 13. The distance between the two outer terminals was D out = 110 (mm). D cp In addition to changing the distance between 10, 30, and 70 mm, the current terminal C 1、 C2 and potential difference measurement terminal P 1、 The positional relationship of P2 was changed. Furthermore, although actual measurement is difficult, an analysis was carried out simulating a two-terminal arrangement.
[0108] [Table 5]
[0109] As a result of the measurement, the Nyquist plot when the terminal arrangement is changed in the four-terminal arrangement is shown in Figure 20. 1、 C2 and potential difference measurement terminal P 1、 P2 Spacing D cp The larger the impedance semicircle, the smaller the size of the part of the impedance. On the other hand, the current terminal C 1、No change was observed in the shape or position of the impedance when C2 was inside or outside. The reason for these measurement results will be considered using current dispersion analysis.
[0110] Two intersection points with the real axis were calculated by curve fitting a part of the semicircle of the measurement results shown in Figure 20. The Real(Z)(Ω) of the intersection point with the smaller value is the high-frequency resistance R fH (Ω), the intersection point with the larger value, Real(Z)(Ω), is the low-frequency resistance R fL (Ω). R fL Calculated result of (Ω) and measured R fL The calculation results of (Ω) are shown in Table 6. As analysis conditions, the polarization resistance of the rebar surface was set to R p =100(kΩcm 2 ) and the electrical resistivity of the mortar is set to the electrical resistivity R of the mortar without the reinforcing bars embedded. s (Ω) was measured and converted using equation (16) to set ρ = 50 (Ωm). The analysis results show that the terminal arrangement is 1、 When P2 is on the outside, R fL The values of (Ω) matched. Also, D cp The larger R fL (Ω) decreased. These trends were the same as the measured results. fL It was found that the analysis results largely reproduced the measurement results.
[0111] [Table 6]
[0112] Next, we will use analysis to consider why the above trend occurs when changing the pin layout. If the following two hypotheses are true, the above trend will occur. (1)D cp and current terminal C 1、 C2 and potential difference measurement terminal P 1、 Regardless of the positional relationship of P2, the measurement area A of the non-destructive method ni (cm2 ) remains unchanged. (2)D cp When is large, it underestimates the impedance compared to when it is small.
[0113] Potential difference measurement terminal P in the case of 4-terminal arrangement 1、 P2 is not a terminal that applies current, and since the internal resistance of the measurement device is extremely large, it is thought that almost no current flows into it. Therefore, it is a current terminal C 1、 When the position of C2 is the same, the way the current flows in the mortar is almost the same for the four-terminal arrangement and the two-terminal arrangement.
[0114] Therefore, we used an analysis using a simple two-terminal configuration to determine the measurement area A ni (cm 2 As mentioned above, it is difficult to actually measure the two-terminal arrangement due to the contact resistance and polarization resistance at the terminal and mortar interface, but it is feasible to do so in the analysis because these can be set very small. ni The scope of the evaluation will be explained using Figures 21A to 21C. As an example of current dispersion analysis, the polarization resistance of the rebar surface is R p =100(kΩcm 2 ), the electrical resistivity of the mortar is ρ = 50 (Ωm), and the terminal spacing in the two-terminal method is D = 70 mm. The current density on the surface of the reinforcing bar is shown in Figure 21A. p =100(kΩcm 2 ) simulates a sound rebar, and ρ=50(Ωm) is the electrical resistance R obtained from a measurement experiment on mortar without embedded rebar. s (Ω) is an approximate value converted from the current density. In the analysis, a direct current is applied from one of two terminals (current terminal C1) placed on the mortar surface, and the other (current terminal C2) is grounded and allowed to flow out. The analysis results show the current density flowing in and out perpendicularly to the rebar surface, with the direction in which current flows from the concrete into the rebar being defined as positive, and the direction in which current flows out from the rebar to the concrete being defined as negative. The results are always 0 (A / m 2) and the value is positive on the current terminal C1 side and negative on the current terminal C2 side. Here, in the equivalent circuit of the nondestructive polarization resistance method shown in FIG. 21B, there are two R ’ p-ni However, in this analysis, R ’ p-ni It can be interpreted that one of them is a resistance component that evaluates the positive current range and the other is a resistance component that evaluates the negative current range. ni When evaluating, only the positive range of the test length is considered, as shown in FIG. 21C.
[0115] Here, the measurement area A of the non-destructive method ni In the evaluation of the current density on the rebar surface shown in Figure 21C, the polarization resistance R p Even though the current density is set to be uniform, the maximum value of the current density appears to be biased toward the outer end. This indicates that the current applied from current terminal C1 flows once in the opposite direction to current terminal C2, which is the grounding point, in the mortar, flows into the rebar, and then flows in the direction of current terminal C2, which is an unusual current path. The reason for this current distribution is thought to be that the current that flows from current terminal C1 through only the mortar, without passing through the inside of the rebar, and then flows into current terminal C2 has a large influence. In other words, A ni When evaluating the R2 and R ’ p-ni In this analysis, the current flowing through R1 is also evaluated, although it is necessary to only consider the current flowing through R2.
[0116] Therefore, as shown in the setting of the insulating surface and the analysis results of the current density on the rebar surface in Figures 22A and 22B, an insulating surface was set on the cross section perpendicular to the axis of the rebar at the center of the mortar in the longitudinal direction. This insulating surface insulates only the mortar area, and does not insulate the inside of the rebar. Therefore, the current that flows from current terminal C1 through only the mortar and reaches current terminal C2 is interrupted, and the current that flows from current terminal C2 through the mortar only is interrupted. 1、The evaluation is limited to the current that passes from the current terminal C1 through the inside of the rebar and reaches current terminal C2. As a result, as shown in Figure 22B, the current density reaches a maximum value on the surface of the rebar directly under the current terminal C1 where the current was applied, and decreases the further away from current terminal C1 it is. This indicates that the current flows into the rebar, which is a conductor, over the shortest distance from current terminal C1, and is an expected phenomenon. Therefore, it is believed that an analysis that sets an insulating surface can more accurately calculate the current density distribution on the surface of the rebar for the current flowing inside the rebar. However, this insulating surface is located within the measurement area A of the non-destructive method, ni This is set only during calculation and is the apparent non-destructive polarization resistance R ’ p-ni (Ω) and terminal arrangement magnification r described later 2 / 4 It should be noted that this is not used in the calculation of
[0117] Here, the measurement area A of the non-destructive method ni is the total surface area A of the target section of the reinforcing bar all Instead, the current density at a cut point on the rebar surface is set as a threshold, current densities below that are excluded (cutoff) and the area where the current density is above the threshold is calculated. This is because the analysis also calculates current densities that have almost no effect on the calculated resistance. If there is no cutoff, A ni is always the total surface area A of the target area of the rebar all 23A to 23C are diagrams for explaining the cut point and the current density distribution after cutting. As shown in Fig. 23A and Fig. 23B, the cut point is set at the center point in the height direction on the circumference of the rebar directly below the terminal, and the current density below the value at that point is cut off. Fig. 23C shows the current density distribution after cutting. This is based on the idea that almost no current flows into the surface of the rebar opposite the terminal. The area where the current density is equal to or greater than the value at the cut point is the measurement area A of the non-destructive method. ni and can be calculated by the following steps (1)-(3).
[0118] (1) Conduct a current dispersion analysis to determine the current density i (A / m 2 ) is calculated. (2) The area of each mesh part in contact with the rebar surface, Δs (m 2 ) is calculated based on the total surface area A of the target area of the reinforcing bar. all (positive value range only) and the number of meshes in the range n all Using the number of pieces, it can be calculated using the following formula (17).
[0119]
number
[0120] (3) Calculate the current density at the cut point, and extract only the meshes where the current density is equal to or greater than the cut point. Then, the number of meshes that satisfy this condition, n cut Calculate the area A (pieces) to be measured using the non-destructive method. ni is calculated using equation (18).
[0121] A ni = n cut Δs (18)
[0122] However, the above method uses the area per mesh, Δs (m 2 ) is almost constant throughout the entire target section. Therefore, when there are complex meshes such as joints of multiple rebars or corners of bent rebars, it is necessary to devise a method to calculate the mesh size for each. Here, the accuracy of the analysis decreases when Δs is large, but the total surface area of the target range is A all =15.7 cm 2 ), the number of meshes on the rebar surface is 1,926, so the average mesh area is Δs = 0.0081 (cm 2 ) and it is considered that the division is sufficiently fine.
[0123] And, the cut policy set in Table 7 and the A calculated by the above method niand nondestructive polarization resistance R p-ni In Table 7, the apparent nondestructive polarization resistance R obtained by the analysis using the two-terminal method based on equation (10) is shown. ’ p-ni A ni By multiplying R p-ni As a result, R p-ni =103.3(kΩcm 2 ) and the polarization resistance of the rebar surface R p =100(kΩcm 2 ) was almost equal to the value shown in Fig. 23A-C.
[0124] [Table 7]
[0125] Next, A calculated by the terminal position ni (cm 2 The change in the terminal spacing D (mm) is shown in Table 8. The terminal positions were set at terminal spacing D = 10, 30, 70, and 110 (mm). When D = 10 (mm), the terminal was close to the insulating surface at the center of the test piece, and when D = 110 (mm), the terminal was close to the end of the test piece. ni Although the value is slightly smaller, the four calculated A ni The mean value was 5.2, the standard deviation was 0.21, and the coefficient of variation was 4.0%, indicating that there was little change.
[0126] [Table 8]
[0127] The above is the analysis result for a two-terminal arrangement, but based on this, we will consider how to calculate the measurement area for a four-terminal arrangement. Referring to the manual of the impedance analyzer used for the measurement, 1、 Apply a potential difference to C2 to measure the current value, and then connect the potential difference measurement terminal P 1、Measure the potential difference at P2. The impedance is calculated by dividing the measured potential difference by the measured current. 1、 P2 only measures the potential difference, and since the internal resistance of the measuring device is extremely large, almost no current flows in, so it is thought to have almost no effect on the current flow. Furthermore, from Table 8, current terminal C 1、 Even if the position of C2 changes, the measurement area A of the non-destructive method ni It is clear that there is almost no change in the current terminal C 1、 C2 is the potential difference measurement terminal P 1、 In the case of a positional relationship such as being inside or outside P2, A ni It is considered that there was almost no change in the measured impedance.
[0128] Next, terminal spacing D cp The reason why the impedance changes with the change in the distance (mm) is considered by FEM analysis. 1、 C2 is on the outside and D is on the inside out = 110 (mm), and the potential difference measurement terminal P 1、 P2 to D cp = 10, 30, 70 (mm). We also performed an analysis of a two-terminal arrangement with a terminal spacing of D = 110 (mm). Here, the current terminal C 1、 The potential difference across current terminal C2 is 1.0 (V). 1、 Apply current to C2 and measure the potential difference at terminal P 1、 The potential difference of P2 was measured. The insulating surface was A ni This is not set here because it is used only during evaluation. Table 9 shows the analysis results for each terminal arrangement. Current terminal C 1、 Since the position of C2 is fixed, the potential difference and current at that terminal are naturally the same. However, the potential difference measurement terminal P 1、 The potential difference measured at P2 is the potential difference between the current terminal C 1、 The potential difference between C2 and D cp The larger the (mm), the smaller the D cpIt is considered that the larger the resistance R, the greater the effect of the potential change caused by the concrete between the potential difference measurement terminal P1 and the current terminal C1, and between the potential difference measurement terminal P2 and the current terminal C2, resulting in an underestimation of the potential difference. fL (Ω) was underestimated. Similarly, the high-frequency resistance R fL (Ω), electrical resistance of concrete R s (Ω) and the apparent nondestructive polarization resistance R calculated based on these ’ p-ni (Ω) is also expected to be underestimated.
[0129] [Table 9]
[0130] Table 10 shows the analysis results of the corrosion rate index for each terminal arrangement. fL ,R fH ,R s is calculated analytically, and R ’ p-ni The non-destructive polarization resistance R p-ni D out = 110 (mm) when A ni =5.29(cm 2 ), so we used equation (10) to calculate it. From the results, R p-ni is the polarization resistance of the internal rebar R p =100(kΩcm 2 ) was almost the same as the 4-terminal arrangement, while cp Depending on the value of R p Therefore, it is necessary to use a more accurate R p-ni In order to calculate the R p-ni R when the calculated result is measured with a two-terminal configuration p-ni Therefore, it is necessary to convert the calculation result of R p-ni(4) R with two terminal configuration for p-ni(2) The ratio is the terminal arrangement magnification r 2 / 4With this definition, the calculation formula for the nondestructive polarization resistance in a four-terminal arrangement is expressed by the following formula (11).
[0131] R p-ni(2) = r 2 / 4 ·R p-ni(4) (11)
[0132] Table 10 shows 2 / 4 However, because it is thought that this will vary depending on various measurement conditions, it will be examined in detail in the parametric study section in Chapter 3, which will be described later. In this chapter, however, the values in this table will be used. Therefore, the semicircular shape obtained from the impedance in Figure 20 is affected by the resistance of the mortar between the current terminal and the potential difference measurement terminal, and the D cp It became clear that, as the resistance increases, the resistance becomes smaller, and as a result, the calculated resistance values are underestimated.
[0133] [Table 10]
[0134] 2.3.6 Considerations for optimal terminal layout method As a summary of the results of the study on terminal layout methods, the advantages and challenges of the two-terminal and four-terminal layouts are summarized.
[0135] The advantage of the two-terminal arrangement is that the nondestructive polarization resistance when there is no resistance between the terminal and the concrete is equal to the polarization resistance of the internal rebar. The challenge with the two-terminal arrangement is that corrosion evaluation is difficult due to the resistance between the terminal and the concrete.
[0136] The advantage of the four-terminal arrangement is that the resistance between the terminals and the concrete is not included in the measurement results. The problem with the four-terminal arrangement is that it underestimates the nondestructive polarization resistance compared to the two-terminal arrangement. Also, the larger the distance between the current terminal and the potential difference measurement terminal, the greater the underestimation.
[0137] Nondestructive polarization resistance R, which does not take into account the resistance between the terminals and concrete in a two-terminal configuration, as an index of corrosion rate p-ni(2)However, in the two-terminal configuration, corrosion evaluation is difficult due to the resistance between the terminal and the concrete. Therefore, the non-destructive polarization resistance R of the four-terminal configuration is calculated from measurements using a four-terminal configuration in which the resistance between the terminal and the concrete is not included in the measurement results. p-ni(4) The method is to calculate R p-ni(4) is the analytical R p-ni(2) Therefore, R p-ni(4) The terminal arrangement magnification r 2 / 4 The corrosion rate index R is corrected by multiplying p-ni(2) Here, in the four-terminal arrangement, the distance D between the current terminal and the potential difference measurement terminal is cp The smaller the D, the smaller the underestimation, and the larger the impedance (higher the sensitivity) can be calculated. cp = 10 mm) is considered to be the most accurate measurement. As will be described later in 2.5, a comparison of the measurement results of equal intervals in previous studies with the measurement results of the outer arrangement in this chapter shows that the outer arrangement is more accurate. Furthermore, 1、 C2 is the potential difference measurement terminal P 1、 The same impedance is measured on either the inside or outside of P2, but the current terminal C is arranged so that the possibility of measurement increases when the covering is large compared to the spacing between the current terminals. 1、 For these reasons, in the non-destructive polarization resistance method, the current terminal C 1、 It became clear that the optimal terminal arrangement was to place the four terminals on the outside, with C2 on the outside.
[0138] 2.4 Quantitative evaluation of corrosion using the non-destructive polarization resistance method 2.4.1 Measurement and analysis method using non-destructive polarization resistance method Based on the above discussion in 2.3, current terminal C 1、 Measurements were performed on all test specimens with the factors shown in Table 3 using a four-terminal arrangement with C2 on the outside. The terminal spacing was D out = 110 (mm), D in = 70 (mm), D cp= 10 (mm), according to 2.3.2 above. Furthermore, a reproduction analysis of the measurement of the proposed method using current dispersion analysis was carried out according to 2.3.3 above, and the measurement area A ni (cm 2 ) was calculated in accordance with 2.3.5 above. From this result, the nondestructive polarization resistance R p-ni (kΩcm 2 ) and calculate the polarization resistance R of the conventional method (three-electrode method) calculated by 2.4.2 below. p (kΩcm 2 ), as well as R p-ni The reproducibility of the measurement results was evaluated through analysis of the above.
[0139] 2.4.2 Conventional method (three-electrode method) To verify the accuracy of the nondestructive polarization resistance method, AC impedance measurements were performed using the three-electrode method, which is a slightly destructive method. The measurement dimensions for mortar are shown in FIG. 24. FIG. 24 is a cross-sectional view showing an example of a test specimen and electrode arrangement in the three-electrode method. Test specimen 70 was created by attaching a lead wire 74 extending to the outside to a reinforcing bar 71 so that the two were electrically connected. In the measurement using the three-electrode method, reinforcing bar 71 was used as the working electrode via lead wire 74. Note that when test specimen 70 is not used, such as when measuring with a four-terminal arrangement, lead wire 74 is insulated.
[0140] A stainless steel plate (SUS404) measuring 40 mm x 140 mm x 2 mm was used for the counter electrode 212. A lead reference electrode (PRE, manufactured by Nippon Corrosion Industry Co., Ltd.) was used for the reference electrode 214. The counter electrode 212 was installed so that its center was directly above the center position of the internal rebar 71 and its long side was parallel to the longitudinal direction of the rebar. The impedance was measured with an applied potential difference of ΔV = 30 mV and a frequency of 0.01 Hz to 10,000 Hz. The reason for setting ΔV = 30 mV is the same as in the case of the non-destructive polarization resistance method. The test specimen was measured immediately after the sealing curing was removed. Therefore, the moisture content was uniform near the surface and inside, and it is considered that the distortion of the current line distribution due to the moisture content is small.
[0141] In the three-electrode method, the apparent polarization resistance R is measured. ’ p(Ω) and the electrical resistivity of concrete R s (Ω) is calculated. R ’ p The measured area A (cm2) depends on the measurement conditions such as the rebar arrangement (cover, rebar diameter, number of bars) 2 ) are considered to be different, so the polarization resistance R p (kΩcm 2 ) must be converted to R p can be calculated using the following equation (19).
[0142] R p = A R ’ p (19)
[0143] Regarding the measured area A, if the rebar is sound, the measurement current is widely dispersed, so it is set to the total surface area of the rebar surface, and if the rebar is corroded, the measurement current is concentrated at the corroded area, so if it is set to the area of the corroded area, the corrosion rate can be evaluated with high accuracy. In the case of test specimen 70 in this chapter, corrosion has occurred over the entire rebar surface, even in the corrosion test specimen. Therefore, the corroded area is the total surface area of the rebar. Therefore, the measured area A is the total surface area of the test section of the rebar, A = 31.4 (cm 2 However, it should be noted that the above may not hold true if the rebar being measured is long compared to the counter electrode.
[0144] 2.4.3 Comparison of measurement results between the non-destructive polarization resistance method and the three-electrode method An example of the Nyquist plot and frequency-Real(Z) relationship obtained for a mortar specimen by the non-destructive polarization resistance method is shown in Figures 25A to 25D. Figure 25A is a Nyquist plot of the soundness factor. Figure 25B is the frequency-Real(Z) relationship of the soundness factor. Figure 25C is a Nyquist plot of the corrosion factor. Figure 25D is the frequency-Real(Z) relationship of the corrosion factor. Figure 25A and Figure 25C show plots showing a part of a semicircle for both the soundness factor and the corrosion factor, in accordance with the theory shown in 2.2 above. Therefore, curve fitting was performed on the plot of the part of the semicircle seen on the low-frequency side to obtain the low-frequency resistance R fL(Ω) and high-frequency resistance R fH (Ω) was calculated. R fH is calculated as the value of Real(Z) at the point where the semicircle plot intersects with the real axis, and the frequency at that time was about 100Hz. Measurements were performed up to a frequency of 10,000Hz, but for this test specimen, R fH It was found that a frequency of 100 Hz or less is sufficient for calculating
[0145] In addition, in measurements of specimens without embedded rebars, almost no change in Real(Z) was observed in the low frequency range, as shown in Figure 26. This shows that the change in Real(Z) accompanying a change in frequency below 100(Hz) is due to the change in Real(Z) at the rebar-mortar interface. Therefore, we calculated the value of Real(Z)(Ω) at 100 Hz for specimens without embedded rebars as a function of the electrical resistance R of the mortar. s (Ω). These three resistance values R fL , R fH , R s From this, the apparent nondestructive polarization resistance R ’ p-ni The results of calculating the resistance R1 (Ω) and R2 (Ω) are shown in Figure 27. ’ p-ni It can be seen that, regardless of the chloride ion concentration in the mortar, the value is clearly smaller than that of the sound factor, and changes depending on the corrosion state. From this, it is believed that quantitative information on the corrosion state of reinforcing bars in concrete can be obtained by evaluating the impedance focusing on the frequency range from 0.1 Hz to 100 Hz. Also, the resistance R2 (Ω) of the corrosion factor showed a smaller value compared to the sound factor. In the sound state, R ’ p-ni It is believed that the large R makes it difficult for current to flow into the rebar, and the current is dispersed inside the mortar, making the current path larger. ’ p-ni This is thought to be because the diameter is small, making it easier for current to flow into the rebar directly below the terminal, shortening the current path.
[0146] Next, R ’ p-ni (Ω) is the non-destructive polarization resistance R p-ni (kΩcm 2 ) to convert the measurement area A of the non-destructive method ni Based on the analysis method described in 2.3.5 above, the polarization resistance of the rebar surface is calculated as R p =1,5,10,25,50,75,100(kΩcm 2 ) and calculated. p-ni (kΩcm 2 ) is the nondestructive polarization resistance R of the two-terminal arrangement that does not consider the contact resistance between the terminal and the mortar. p-ni(2) To convert to , we use the analysis of the two-terminal configuration and D cp By comparing the analysis of the four-terminal arrangement with the terminal arrangement magnification r 2 / 4 The polarization resistance of the internal rebar R p and the measurement area A of the non-destructive method ni The relationship between R and R is shown in Figure 28A. p and terminal layout magnification r 2 / 4 The relationship between is shown in Figure 28B. ni is R p ≧10(kΩcm 2 ) is constant (A ni =5.8(cm 2 )) and R p <10(kΩcm 2 ) tended to decrease slightly. However, the largest decrease was observed in R p =1.0(kΩcm 2 ) even in the case of A ni =5.4(cm 2 ) This change was R p This is thought to be due to the concentration of current on the surface of the reinforcing bar as the R decreases, but it was found that the change was small enough that it could be considered constant. p and terminal layout magnification r 2 / 4 The relationship is R p ≧10(kΩcm 2 ) is constant (r 2 / 4 = 2.5), and R p <10(kΩcm 2 ) slightly increased in R p =1.0(kΩcm2 ) in the case of r 2 / 4 = 2.6. Therefore, r 2 / 4 Under these measurement conditions, R p It became clear that there was no need to consider changes in
[0147] Next, the polarization resistance R in the three-electrode method to be compared p (kΩcm 2 ) is obtained. Figures 29A to 29D show the Nyquist plots and frequency-Real(Z) relationships calculated by the AC impedance method of the three-electrode method. Figure 29A is a Nyquist plot of the soundness factor in the three-electrode method. Figure 29B is the frequency-Real(Z) relationship of the soundness factor in the three-electrode method. Figure 29C is a Nyquist plot of the corrosion factor in the three-electrode method. Figure 29D is the frequency-Real(Z) relationship of the corrosion factor in the three-electrode method. As with the measurement results using the non-destructive polarization resistance method, it was revealed that the value of Real(Z) increases in the low frequency range, and the increasing tendency is greater for sound rebars than for test specimens with embedded corroded rebars. This also shows that the frequency dependence of Real(Z) in the low frequency range of the non-destructive polarization resistance method is due to the change in Real(Z) of the rebar-concrete interface.
[0148] Non-destructive polarization resistance R of the test specimen using the non-destructive polarization resistance method p-ni(2) (kΩcm 2 ) and the polarization resistance R measured by the three-electrode method p (kΩcm 2 The results of comparing the non-destructive polarization resistance R p-ni(2) is the measured value R of the test specimen by the non-destructive polarization resistance method. ’ p-ni , and the measurement area A of the non-destructive method obtained by analysis ni and terminal layout magnification r 2 / 4 The polarization resistance R p is the measured value R by the three-electrode method ’ p and the measurement area A = 31.4 (cm 2) was used to calculate the corrosion factor. Figure 30 shows only the measurement results of the corrosion factors. Figure 30 also shows the linear regression line, regression equation, and coefficient of determination R 2 This shows that.
[0149] The reason why only the corrosion factor was used here is as follows. p (kΩcm 2 ) is extremely large, i.e., for sound factors, the Nyquist plot (Fig. 29A) obtained by measuring AC impedance using the three-electrode method is not semicircular but linear, making it difficult to calculate the polarization resistance. Therefore, in the comparison in Fig. 30, only data that can be calculated using the three-electrode method, i.e., corrosion factors, were used.
[0150] As shown in Figure 30, the non-destructive polarization resistance R p-ni(2) and polarization resistance R p are positively linearly correlated, R 2 = 0.92, which shows a high correlation. In addition, the slope of the approximation line is nearly 1, and it was found that the two indices are nearly equal in value. This shows that when the same test specimen is measured using both methods, nearly equal values are calculated, and it can be said that by defining an index per unit area, it is possible to extract only information related to the corrosion state of the internal rebar. At the same time, this relationship is also consistent with the non-destructive method's measurement area A ni It has been experimentally shown that the analysis method and cutoff method described above in 2.3.5 are appropriate for calculating the polarization resistance R by the three-electrode method. If the cutoff value is set to a lower value, p While there is almost no change in the non-destructive polarization resistance R p-ni(2) A ni Since the slope of the approximation line in Figure 30 increases with increasing R p-ni(2) A ni As the value of the cutoff frequency decreases, the slope of the approximation line in Figure 30 decreases. Therefore, it can be said that the cutoff policy this time, which has a slope of approximately 1, was appropriate.
[0151] Next, a bar graph comparing the nondestructive polarization resistance of the corrosion factors and the sound factors is shown in Figure 31. The values in the bar graph indicate the average value of each factor. The error bars in the bar graph indicate the standard deviation.
[0152] The health factor is R p-ni(2) The value of R was large, and there was a clear difference compared to the corrosion factors. p-ni(2) By calculating R p It was found that it is possible to estimate the R and to determine the presence or absence of corrosion and to calculate the corrosion rate. In this measurement, the lower limit frequency was 100 (mHz), but if longer measurements are allowed and the impedance measurement accuracy can be maintained, the lower limit frequency can be lowered to p-ni However, it should be noted that measurements at low frequencies generally have lower accuracy (larger variability) than measurements at high frequencies.
[0153] 2.4.4 Estimation of polarization resistance of internal rebars by non-destructive polarization resistance analysis A non-destructive polarization resistance analysis of the mortar specimen was carried out based on the analysis method described in 2.3.5 above, and it was verified whether the polarization resistance of the internal rebar could be estimated. The analysis conditions were set as follows: the specimen shape and terminal arrangement were as described in 2.4.1 above, and the electrical resistivity ρ (Ωm) of the mortar and the polarization resistance R of the rebar surface were calculated. p (kΩcm 2 ) as an input value, and the nondestructive polarization resistance R p-ni(2) (kΩcm 2 The electrical resistivity was set to ρ = 10, 30, 50, 100 (Ωm), and the polarization resistance was R p =1,5,10,25,50,75,100(kΩcm 2 The verification results are shown in Figure 32. The dotted line in Figure 32 is a linear approximation line of the analytical values of all factors. As a result, R p-ni(2) is R pIt was found that the slope of the approximation line is nearly 1 and increases linearly with an increase in ρ. On the other hand, it was found that there is no change at all depending on the value of electrical resistivity ρ. This means that the electrical resistance of the mortar and the resistance related to rebar corrosion can be calculated separately, just as the theory shows in the equivalent circuit in Figure 10. Based on this, it was possible to calculate the non-destructive polarization resistance R using FEM analysis. p-ni(2) By calculating the polarization resistance R of the internal rebar p It was found that it is possible to estimate
[0154] 2.5 Consideration of the applicability of the non-destructive polarization resistance method using the inventor's previous research results In a previous study (Non-Patent Document 4), the inventors of the present application conducted a measurement experiment on mortar specimens of the same shape as the experiment in this chapter, with equal intervals as shown in FIG. 33. The specimen factors in the previous study by the inventors are shown in Table 11. In addition to the factors of corrosion and soundness of polished round steel, and no rebar to obtain the electrical resistivity of mortar, polished round steel and deformed steel were set as the types of rebar. As a factor of the degree of corrosion, the period of promoting corrosion of rebar by salt spray in an environment of temperature 40°C and humidity 80% as shown in 2.3.1 above was changed to 0, 14, 28, and 84 days. Regardless of the period, in order to corrode the entire test section of the rebar, the exposed surface was turned upside down on the third day after installation. In order to change the electrical resistivity of mortar in response to these factors, sodium chloride was added when the mortar was poured, and chloride ion concentrations of 0, 3, and 10 (kg / m -3 The Cl content in Table 11 was - The concentration refers to the premixed chloride ion concentration.
[0155] [Table 11]
[0156] 2.5.1 Changes in measurement values due to changes in terminal layout The non-destructive polarization resistance method proposed in this chapter uses an outer arrangement, but all of the completely non-destructive methods proposed in the inventor's previous research have been proposed with four terminals arranged at equal intervals. As mentioned in 2.3, the non-destructive polarization resistance R calculated by measurement using a four-terminal arrangement p-ni(4) is the nondestructive polarization resistance R of a two-terminal configuration that does not consider the resistance between the terminals and the mortar. p-ni(2) However, the terminal arrangement magnification r 2 / 4 Therefore, to verify whether the results of the measurements with the equally spaced arrangement could be used in the same way as the measurements with the outer arrangement, measurements and analyses were carried out with different arrangement methods.
[0157] In the evenly spaced terminal arrangement, the distance D between the two outer terminals is as shown in Figure 33. out = 110 (mm), and the distance between the two inner terminals is D in D so that the four terminals are equally spaced in = 30 (mm). The test specimens used were those shown in 2.3.1 above, and measurements were performed on the same specimens on the same day as the measurements for the outer placement. The measurement conditions were the same as those shown in 2.3.2 above. The results are compared with the outer placement measurement results and the polarization resistance R obtained by the three-electrode method. p (kΩcm 2 ) was evaluated together. From the analysis results, the measurement area of the non-destructive method in the outer arrangement is A ni =5.8(cm 2 ), terminal arrangement magnification is r 2 / 4 = 2.5, and in the case of equal spacing, A ni =5.8(cm 2 ), r 2 / 4 The apparent nondestructive polarization resistance measured in each configuration was converted using these values to obtain the nondestructive polarization resistance R for the two-terminal configuration, which does not take into account the resistance between the terminals and the mortar. p-ni(2) The results of comparing the two are shown in Figure 34. In the figure, the straight line (x=y) where the two coincide is shown as a solid line, and the straight lines (y=2x) and (y=0.5x) where the measured values of the equally spaced positions are +100% and -50% of the measured values of the outer positions are shown as dotted lines.
[0158] As a result, it was found that almost all of the measurements of the equally spaced arrangements agreed with the measurements of the outer arrangements within the range of -50% to +100%. p-ni(2) Since the value of is about 5 to 10 times different between corrosion factors and sound factors, it is thought that the variation of about 0.5 to 2 times is not particularly problematic for the purpose of judging the presence or absence of corrosion and for the relative comparison of corrosion rates. Therefore, in the case of the equally spaced arrangement, the nondestructive polarization resistance R of the two-terminal arrangement, which does not consider the resistance between the terminal and the mortar, can be calculated in the same manner as in the outer arrangement. p-ni(2) It was found that by calculating this, it is possible to determine the presence or absence of corrosion and the rate of corrosion.
[0159] 2.5.2 Considerations by the inventors using measurement data from previous research The non-destructive polarization resistance R was calculated by combining the results of measurements using equally spaced placement in the inventor's previous research and the results of measurements using outer placement in this chapter, focusing only on corrosion factors. p-ni(2) and polarization resistance R p The results of the comparison are shown in Figure 35. The figure shows the approximate line and the coefficient of determination for the measurement data of the previous study by the inventor and the measurement data of the outer arrangement of this embodiment. The slope of the approximate line for the measurement data of this embodiment is 0.99, which is almost 1, but the slope of the approximate line for the corrected data of the previous study by the inventor is 0.77, which is almost 1. p Nondestructive polarization resistance R p-ni The reason why the error is smaller with the outer placement compared to the equal interval placement is thought to be because the part of the semicircle of the Nyquist plot measured with the outer placement is larger (higher sensitivity), allowing for more accurate curve fitting and higher calculation accuracy. For this reason, it was found that the outer placement is better when applying the proposed method.
[0160] Furthermore, Fig. 36 shows the results of a comparison of corrosion factors and soundness factors using measurement data from previous research by the inventors. The values in the bar graphs show the average value of each factor. Also, the error bars in the bar graphs show the standard deviation. Looking at the average values, the R p-niThe difference was about 10 times, indicating a clear difference. This result also shows that even if there is a variation of about 0.5 to 2 times, it can be used to determine the presence or absence of corrosion.
[0161] From the consideration using Figures 35 and 36 above, it was confirmed that the measurement data from the inventor's previous research could be fully utilized. Since the inventor's previous research involved experiments with various factors, a comparative study was conducted for each factor. Figure 37 shows the R p-ni(2) and R p The results of the comparison are shown below. Among the corrosion factors, differences were observed depending on the pre-corrosion period and the type of rebar. First, the data for the soundness factors shown in Figure 36 includes both deformed bars and round bars, so the deformed bars for the soundness factors were R-shaped like the round bars. p-ni(2) Based on this, the value of R was larger in CorD28d, which uses deformed bars, compared with Cor28d and Cor84d. p-ni(2) The value of was large. This is thought to be because CorD28d had a black surface and was less affected by salt spray corrosion. In addition, no difference in correlation was observed between deformed bars and polished round bars, and the effect of the type of bar was small. In other words, it was found that the method proposed in this chapter can be used to evaluate corrosion of deformed bars as well.
[0162] In this way, by utilizing the results of previous research by the inventors, it was confirmed that the non-destructive polarization resistance calculated by the proposed method changes depending on the corrosion state of the rebar, and that the corrosion rate of both deformed rebars and polished round steel can be quantitatively evaluated. In addition, although the measurement results of both the equally spaced and outboard arrangements can be used, the outboard arrangement has a higher R p-ni(2) It was revealed that the calculation accuracy was high.
[0163] The optimal terminal arrangement for the non-destructive polarization resistance method is current terminal C, as shown in 2.3.6 above. 1、In this section, we have used data from previous research to demonstrate that the accuracy of calculating the corrosion rate index is higher with an outer terminal arrangement than with an equal-spaced arrangement, and that this arrangement is optimal. In Chapter 3, we will consider how to improve the applicability of the nondestructive polarization resistance method, but based on the results of this chapter, we will mainly focus on the current terminal C 1、 An analysis will be performed for the outer four-terminal arrangement with C2 on the outside.
[0164] 2.6 Summary of this chapter In this chapter, we carried out a basic study of the nondestructive polarization resistance method, which is a completely nondestructive corrosion rate evaluation method, by optimizing the arrangement of the terminals during measurement, quantitatively evaluating the corrosion rate, and utilizing data from previous research. These studies were carried out by creating and measuring small mortar specimens with different corrosion conditions of the internal rebars, verifying the accuracy of polarization resistance measurements using the conventional three-electrode AC impedance method, and reproducing the measurements using current dispersion analysis using the finite element method (FEM). As a result, the following conclusions were obtained.
[0165] Nondestructive polarization resistance measurements using a two-terminal arrangement were compared with measurements using a four-terminal arrangement. As a result, with the two-terminal arrangement, the resistance (contact resistance and polarization resistance) between the stainless steel terminal and the mortar affected the measured values, and changes in impedance values due to the corrosion state of the internal rebar could not be detected. On the other hand, with the four-terminal arrangement, clear changes due to the corrosion state were observed, indicating that the four-terminal arrangement is necessary.
[0166] Based on the analysis using a two-terminal arrangement in which the resistance of the terminal and the mortar interface is set to be extremely small, the measurement area A ni As a result, the apparent non-destructive polarization resistance R ’ p-ni A ni The nondestructive polarization resistance R due to a two-terminal arrangement that does not take into account the resistance of the terminal and mortar interface is calculated by multiplying p-ni(2) (kΩcm 2 ) and the polarization resistance of the internal rebar R p (kΩcm 2 ) was found to be almost identical.
[0167] In a 4-terminal configuration, the distance D between the current terminal and the potential difference measurement terminal cp Measurements and analysis were carried out while changing the D cp The larger the R p-ni(2) Therefore, the terminal arrangement magnification r 2 / 4 and the converted nondestructive polarization resistance R p-ni(2) was proposed as an index of corrosion rate.
[0168] Nondestructive polarization resistance R obtained by measurement using a four-terminal configuration p-ni(2) and the polarization resistance R obtained by the three-electrode method p As a result of comparing the results, the two were almost identical for the specimens with corrosion factors. In addition, the R p-ni It was revealed that there was a clear difference between the two. This demonstrated that the proposed method is capable of distinguishing corrosion and quantitatively evaluating the corrosion rate.
[0169] The data from previous studies measured with equal spacing arrangement was compared with the data measured with the outer placement in this chapter. As a result, the appropriate terminal placement magnification r 2 / 4 By using the outer placement R p-ni(2) R with equal spacing p-ni(2) The results agreed with the variation of -50 to +100%. This shows that it is possible to utilize the existing data arranged at equal intervals.
[0170] Combining previous research data and the measurement results in this chapter, R p-ni(2) and R p As a result, the R p-ni(2) The change in the R is small depending on the type of rebar. p-ni(2) It was revealed that the calculation accuracy is high.
[0171] The terminal arrangement for the non-destructive polarization resistance method is current terminal C 1、 It became clear that the optimum arrangement was an outer arrangement of the four terminals with C2 on the outside.
[0172] Chapter 3: Study on improving the applicability of completely non-destructive corrosion rate evaluation methods 3.1 Introduction In Chapter 2, we performed AC impedance measurements using four terminals installed on the surface of a small mortar specimen with embedded rebar, and measured the nondestructive polarization resistance R p-ni (kΩcm 2 ), which is the polarization resistance R of the rebar-concrete interface. p (kΩcm 2 ) and it was shown that there is a high positive linear correlation with the measured value. In addition, it was shown that the measurement by the non-destructive polarization resistance method can be reproduced by current dispersion analysis using the finite element method (FEM). Based on this, it was clarified that the proposed measurement theory is highly valid.
[0173] However, the non-destructive polarization resistance R p-ni and polarization resistance R p Since the correlation was derived only from application to small mortar specimens, it is not clear how this relationship will change if the shape of the object to be measured or the measurement conditions change. Also, if the distance between the current terminals is small compared to the depth of the rebar from the measurement surface (referred to as the cover in this chapter), it is assumed that the measurement current will flow only through the concrete without passing through the inside of the rebar. Therefore, it is unclear under what measurement conditions the nondestructive polarization resistance R p-ni It is also unclear whether it is possible to calculate
[0174] Here, the factors of variation assumed in the nondestructive polarization resistance method of the present disclosure are shown in FIG. p-ni is the polarization resistance of the reinforcing steel inside the concrete, R p (kΩcm 2 ) in a four-terminal configuration, the two outer current terminals C 1、 C2 Spacing (Outer 2 Terminal Spacing D out), cover c, rebar diameter φ, number of rebars, electrical resistivity ρ of concrete, shape and dimensions of the target (height, depth, width of target), etc. From Chapter 2, in the four-terminal arrangement, the two potential difference measurement terminals P 1、 P2 is R for both equal spacing and outer placement. p-ni However, the outer placement has a higher sensitivity and can evaluate R more accurately. p-ni Therefore, it was found that the potential difference measurement terminal P 1、 P2 spacing (Inner 2 terminal spacing D in ) is the outer placement D in =D out Fix at -40(mm).
[0175] In this chapter, we examined the following three items with the aim of making the nondestructive polarization resistance method applicable to reinforced concrete of various shapes and dimensions, i.e., improving its applicability and expanding its range of application. (1) Parametric study using current dispersion analysis (2) Application to deep cover specimens (3) Application to beam specimens with multiple embedded rebars
[0176] (1) Non-destructive polarization resistance R due to changes in various measurement conditions p-ni The changes in corrosion resistance were quantitatively clarified by current dispersion analysis using FEM. In (2), assuming a deep-cover structure such as a coastal structure, a reinforced concrete specimen with a cover of 100 mm was fabricated and measured to demonstrate the conditions under which the proposed method can be used and a corrosion judgment procedure was proposed. In (3), uneven corrosion was generated in a beam-type reinforced concrete specimen with multiple buried rebars, and measurements were then taken while changing the position, verifying the applicability of the method to multiple rebars and proposing a method of using the method as a relative comparative evaluation method for unevenly corroded specimens. All three of the above items can be said to be studies assuming application to actual structures on site.
[0177] 3.2 Parametric study using current dispersion analysis 3.2.1 Setting analysis conditions Non-destructive polarization resistance R, an index of corrosion rate p-ni (kΩcm 2 ) is the polarization resistance of the internal rebar R p Understanding the influence of factors other than corrosion is useful for establishing criteria for determining the presence or absence of corrosion and for applying them in the field. Therefore, a parametric study was conducted by inputting multiple values for various factors.
[0178] The reference analysis conditions are shown in Figure 39. Since there are multiple variable factors, the polarization resistance R p (kΩcm 2 ) change (R p =1, 10, 50, 100 (kΩcm 2 In addition to the above, the following factors (1) to (4) were changed one by one to conduct the analysis. (1) Electrical resistivity of concrete ρ: 10, 50, 100 (Ωm) (2) Coverage c: 15, 30, 60, 90 (mm) (3) Steel bar diameter: 10, 16, 22, 25, 32 (mm) (4) Distance between two outer terminals D out :120,160,200,240(mm)
[0179] The analytical conditions were set assuming typical reinforced concrete structures in coastal areas, such as piers and caissons. Because the concrete surface is wet, the electrical resistivity ρ of the concrete was set to a small value, the cover thickness c was set to a large value, and the rebar diameter φ was set to a large value. The analysis was performed using current dispersion analysis using the finite element method (FEM). Details of the analysis method have already been given in 2.3.3 and 2.3.5 above. Potential difference measurement terminal P 1、 The size of P2 was set to 10mm x 40mm to match the specimen measurements in Chapter 2 above, and the terminal length in the longitudinal direction of the rebar was set to 10mm. Because the geometry of the rebar is curved, tetrahedral mesh elements were generated for both the rebar and the concrete. The maximum length of one side of the element was set to 2.1cm, and the total number of elements was 43,406. The terminal arrangement was such that the two outer terminals were current terminals C 1、 C2, and the inner potential difference measurement terminal P 1、P2 2 terminal spacing D in But, D in (mm)=D out The FEM analysis showed that the apparent non-destructive polarization resistance R ’ p-ni In addition to (Ω), the measurement area A of the non-destructive method ni (cm 2 ) and terminal arrangement magnification r 2 / 4 was calculated. 2 / 4 In order to calculate, an analysis was also performed using a two-terminal arrangement. The terminal spacing D for the two-terminal arrangement is 1 / 2 the D for the four-terminal arrangement. out Using these analytical results, the nondestructive polarization resistance R p-ni(2) was calculated.
[0180] 3.2.2 Analysis results Polarization resistance R of the rebar surface due to electrical resistivity ρ p The area A to be measured by the non-destructive method ni , terminal arrangement magnification r 2 / 4 and nondestructive polarization resistance R p-ni(2) The relationship between R and R is shown in Figures 40A-40C. p and A ni FIG. 40B shows the relationship between R p andr 2 / 4 FIG. 40C shows the relationship between R p and R p-ni(2) In addition, in Figure 40C, R based on the least squares method using all the data in the figure is p and R p-ni(2) As a result, even if the value of the electrical resistivity ρ changes, R p and A ni and R p andr 2 / 4 This is because the ratio of R1 to R2 in the equivalent circuit shown in Figure 10 of 2.2 above does not change with the electrical resistivity ρ, and does not affect the rate or path of current flow into the rebar. Also, looking at Figure 40A, the polarization resistance of the internal rebar is R p =1.0(kΩcm 2 ) and very small, A niwill decrease slightly, but R p ≧10(kΩcm 2 ), so as in 2.4.3 above, R p-ni(2) When calculating, A ni R p In addition, from Figure 40B, it is possible to consider r 2 / 4 R p It has been shown that there is no problem in considering it constant regardless of
[0181] Furthermore, if we look at Figure 40C, R p and R p-ni(2) It was found that there is a linear correlation, and the slope of the approximation line is 1.03, which is almost 1. This is because A ni , r 2 / 4 This shows that the calculation method of is appropriate. In addition, it was found that there is almost no change due to the electrical resistivity ρ. Therefore, R p-ni(2) From R p It was found that there is no need to take ρ into account when converting to
[0182] Next, the polarization resistance R of the rebar surface due to the cover thickness c p The area A to be measured by the non-destructive method ni , terminal arrangement magnification r 2 / 4 and nondestructive polarization resistance R p-ni(2) The relationship between R and R is shown in Figures 41A-41C. p and A ni FIG. 41B shows the relationship between R p andr 2 / 4 FIG. 41C shows the relationship between R p and R p-ni(2) In addition, in Figure 41C, R based on the least squares method using all the data in the figure is p and R p-ni(2) The results of FIG. 41A show that as the fog increases, A ni This is because the current flows while dispersing inside the concrete, but the larger the cover, the more the current reaches the surface of the rebar in a more spread out state. 2 / 4It was shown that R is constant regardless of the cover. p-ni(2) is R p The value is 1.0 to 1.1 times that of the original value, and it is believed that a difference of this magnitude can be considered to be roughly equal.
[0183] In addition, the polarization resistance R of the rebar surface due to the rebar diameter φ p The area A to be measured by the non-destructive method ni , terminal arrangement magnification r 2 / 4 and nondestructive polarization resistance R p-ni(2) The relationship between R and R is shown in Figures 42A-42C. p and A ni FIG. 42B shows the relationship between R p andr 2 / 4 FIG. 42C shows the relationship between R p and R p-ni(2) In addition, in Figure 42C, R based on the least squares method using all the data in the figure is p and R p-ni(2) The approximation line of the relationship between the rebar diameter and the load is shown in Figure 42A. ni Considering the cutoff conditions in Chapter 2 above, the larger the diameter of the rebar, the greater the potential drop, since the distance from the current terminal to the cutoff point becomes longer. As a result, the cut position in the axial direction of the rebar becomes farther away from the terminal, and the value of A ni The value of r is calculated to be large. 2 / 4 It was shown that R is constant regardless of the diameter of the rebar. p-ni is R p The value is 1.0 to 1.1 times that of the original value, and it is believed that a difference of this magnitude can be considered to be roughly equal.
[0184] Furthermore, the distance between the two outer terminals D out The polarization resistance R of the reinforcing bar surface due to p The area A to be measured by the non-destructive method ni , terminal arrangement magnification r 2 / 4 and nondestructive polarization resistance R p-ni(2) The relationship between R and R is shown in Figures 43A-43C. pand A ni FIG. 43B shows the relationship between R p andr 2 / 4 FIG. 43C shows the relationship between R p and R p-ni In Figure 43C, the R p and R p-ni(2) The approximate line of the relationship between the out Even if A changes ni On the other hand, from Fig. 43B, D out The smaller r 2 / 4 has become larger. That is, D out The smaller the impedance, the more the four-terminal arrangement underestimates it compared to the two-terminal arrangement. This is because the four-terminal arrangement in this analysis has a constant distance of 10 mm between the current terminal and the potential difference measurement terminal, and D out It is presumed that the smaller the value, the greater the influence. In addition, the potential change applied from the current terminal C1 is measured at the potential difference measurement terminal P1, but D out One reason is that the smaller R is, the greater the influence of the current terminal C2. p-ni is R p The values are 1.0 to 1.2 times higher than the above, and it is believed that differences of this magnitude can be considered to be roughly equal.
[0185] To summarize the above analysis, the polarization resistance R p and nondestructive polarization resistance R p-ni(2) Regarding the relationship between R p For R p-ni(2) The non-destructive method was found to have a measurement area A of 1.0 to 1.2 times the original value, which is almost the same as the original value. ni changed with the change in the cover thickness c and the rebar diameter φ. In addition, the terminal arrangement magnification r 2 / 4 It was found that the smaller the distance between the two outer terminals, the larger the nondestructive polarization resistance R ’ p-ni (Ω) to A ni (cm 2 ) and r 2 / 4By multiplying by R, we obtain the nondestructive polarization resistance per unit area, R p-ni(2) (kΩcm 2 ) and the result is R p-ni(2) is the polarization resistance R of the rebar surface p (kΩcm 2 ) and no longer varies with other factors. In other words, A ni and r 2 / 4 The calculation method of R p-ni(2) This means that the value per unit area of the rebar surface can be evaluated. Based on this, a current dispersion analysis was carried out using FEM simulating the measurement object and measurement conditions, and the A ni and r 2 / 4 By calculating the apparent nondestructive polarization resistance R ’ p-ni (Ω) to non-destructively measure the polarization resistance R p-ni(2) (kΩcm 2 ) can be calculated. However, it is often difficult in terms of time and technology to perform analysis each time an actual structure or test specimen is measured. Therefore, based on the parametric study in this section, we have developed a method for calculating A ni and r 2 / 4 If a simple estimation formula for the apparent nondestructive polarization resistance R can be proposed, ’ p-ni (Ω) and simply insert it into these simple estimation formulas to obtain the non-destructive polarization resistance R p-ni(2) (kΩcm 2 ), which is believed to greatly improve on-site applicability. Therefore, a simplified estimation formula was developed in 3.2.3.
[0186] 3.2.3 Development of a simple estimation formula for measurement area and terminal arrangement magnification for non-destructive methods From the results of 3.2.2, the measurement area A of the non-destructive method ni and terminal arrangement magnification r 2 / 4 First, we construct a simple estimation formula for A ni With respect to the electrical resistivity ρ of concrete and the outer two-terminal distance D outThe effect of polarization resistance R is not taken into consideration because it was almost nonexistent. p Regarding R p ≧10(kΩcm 2 )A ni has little effect on R p =1.0(kΩcm 2 ) is small and difficult to obtain as prior information, so R p =100(kΩcm 2 ) and is not considered as a factor. On the other hand, A is set according to the cover thickness c and the rebar diameter φ. ni Since varies, we will develop an estimation formula that takes these two factors into account. Assuming application to actual structures, we set the cover to 15, 30, 60, and 90 mm, and the rebar diameter to 10, 16, 22, 25, and 32 mm, and the measurement area A ni In 3.2.2, A was calculated based on the rebar diameter when the cover is 30 mm. ni Calculation of A, factoring in cover when rebar diameter is 16 mm ni The calculation was based on the rebar diameter factor, but here the analysis was performed by changing the rebar diameter factor for each cover factor. However, factors that cannot be assumed in the design of an actual structure, such as rebar diameter φ=32mm and cover c=15,30mm, and φ=25mm and c=15mm, were excluded. The reason for this is that the Japan Society of Civil Engineers' Standard Specifications for Concrete [Design Edition] (pp.338-340) stipulates that the cover of the rebar should be designed to the larger value of either the rebar diameter or a cover that satisfies durability, taking into account construction errors.
[0187] As a result of the analysis, Fig. 44A shows the rebar diameter φ and A for each cover. ni The relationship between the cover thickness c and A for each rebar diameter is shown in Figure 44B. ni As a result, A ni It was found that A is correlated with the square of the rebar diameter φ, and that the cover thickness c and the slope are positively linearly correlated. ni The reason why A is correlated with the square of φ is that, as shown in Figures 23A-23C, the cut point is set at the center of the height direction of the side of the rebar directly below the terminal. niHowever, as the diameter of the rebar increases, the distance from the terminal to the cut point increases, and the potential on the surface of the rebar at the cut point becomes smaller than when the diameter of the rebar is small. As a result, the cut point is located at a point with a longer distance from the terminal in the axial direction of the rebar. In other words, the change in the diameter of the rebar reduces A ni Since there is a two-dimensional effect on A ni is thought to be correlated with the square of φ.
[0188] A ni As a consideration of the formulation, the following equations (20-1), (20-2), and (20-3) were set.
[0189] A ni = F φ +F c (20-1) F φ = α (φ-β) 2 +γ (20-2) F c = σ c + ε (20-3)
[0190] Where: A ni is the area to be measured by the non-destructive method (cm 2 ). F φ is a function of the rebar diameter. F c is a function of fog. φ is the diameter of the rebar (mm). c is the cover (mm). α, β, γ, σ, and ε are coefficients.
[0191] First, A ni Assuming that correlates only with the rebar diameter φ (F c = 0), and curve fitting was performed with a quadratic function of φ. As a result, (α, β, γ) = (0.0826, 9.38, 9.21) was obtained. Next, these values were substituted into equation (20-2) to obtain F φ Calculate A using equations (20-1) and (20-3). ni -F φ =Fc =σc+ε. And, (A ni -F φ A linear regression analysis based on the least squares method was performed on the relationship between A and cover c. ni from the rebar diameter function F φ The function of the cover c was formulated for the value assumed to be correlated only with the cover minus the value of the cover. As a result, (σ,ε) = (0.13, -7.04) was obtained. By substituting these results into equation (20-1), the measurement area A of the non-destructive method is ni A simple estimation formula for can be expressed as equation (21).
[0192] A ni = F φ +F c = (8.26×10) -2 ·(φ-9.38)+0.13·c+2.17 ···(21) (10≦φ≦32(mm)),(15≦c≦90(mm))
[0193] To verify the accuracy of the simplified estimation formula shown in (21), the difference between the analysis and estimation, ΔA ni (A ni Analytical value of - A using a simple estimation formula ni Calculate the estimated value of A ni The difference between the analysis and the estimation ΔA ni The relationship is shown in Figure 45.
[0194] From Figure 45, the difference between the analysis and estimation values ΔA ni A ni Regardless of the value, ±5(cm 2 ) and A ni <10(cm 2 ) and ΔA ni ±2(cm 2 ), and it was found that the estimation accuracy of the simplified estimation formula is high. Therefore, within the range presented in equation (21), A ni It was found that the error of the simplified estimation formula was within a range that could be used sufficiently.
[0195] Next, terminal arrangement magnification r 2 / 4 This index is evaluated by the distance between the two outer terminals D out The change was due to factors other than D out We construct an equation that takes only D as a factor. out andr 2 / 4 The relationship is shown below.
[0196] As a result, the relationship was nearly linear, so we formulated it by simple regression analysis based on the least squares method. In other words, the approximation line in the figure is the relationship equation, which is shown in equation (22).
[0197] r 2 / 4 = (8.9×10 -3 ) -2 D out +4.8 ···(22) (120≦D out ≦240(mm)
[0198] As a proposal for a simple method of measuring and calculating corrosion rates, ni and r 2 / 4 An example of a flow of calculating the corrosion rate by the non-destructive polarization resistance method using the estimation formula will be described.
[0199] First, the cover thickness c and diameter φ of the rebar at the measurement position are estimated using a non-destructive inspection method such as a rebar arrangement drawing or an electromagnetic radar method to detect the position of the rebar, and the outer two terminal distance D is calculated. out Set the D that corresponds to the fog. out The method for setting the apparent non-destructive polarization resistance R will be explained in 3.3.4 below. ’ p-ni Measure where R p =100(kΩcm 2 ) and use the simplified estimation formulas (21) and (22) or current dispersion analysis to determine the measurement area A of the nondestructive method. ni and terminal arrangement magnification r 2 / 4 Then, the nondestructive polarization resistance R is calculated based on equations (10) and (11). p-ni(2) , polarization resistance R p From the results of the parametric study in 5.2.2, Rp-ni(2) and R p were almost equal, so R p =R p-ni(2) Let this R p is converted to the corrosion rate CR using the above-mentioned formulas (3) and (4). By using this procedure, the corrosion rate CR can be calculated.
[0200] 3.3 Application to deep cover specimens 3.3.1 Reinforced concrete specimen In order to evaluate the applicability of the non-destructive polarization resistance method to deep-cover reinforced concrete, a reinforced concrete specimen was prepared and a measurement experiment was conducted. Figure 47 shows the outline of the specimen 70. The dimensions were (width) x (height) x (depth) = 200 (mm) x 200 (mm) x 600 (mm). The reinforcing bar 71 was a black-skinned deformed reinforcing bar (SD295A) with a nominal diameter of D16 (mm) and a length of 624 (mm). The reinforcing bar 71 was covered with epoxy resin 72 for 32 (mm) each from both ends, so that the central 560 (mm) was the test section. The factors of the specimen 70 are shown in Table 12. A particular problem with deep-cover structures is that seawater can penetrate through bending cracks caused by external factors such as earthquakes, causing early corrosion. Even if bending cracks are discovered and repaired early, seawater may seep in through the repaired area and cause corrosion due to the lack of adhesion of the repair agent or improper filling. Therefore, the presence or absence of bending cracks and the presence or absence of crack repairs were considered as factors.
[0201] [Table 12]
[0202] Next, the mix ratio of the concrete specimen is shown in Figure 48. The materials used were tap water, ordinary Portland cement from Ube Mitsubishi Cement Co., Ltd., and land sand from Namegata City, Ibaraki Prefecture (maximum dimension 5 (mm), surface dry density 2.56 (g / cm3). 3 The coarse aggregate was crushed stone from Kasama City, Ibaraki Prefecture (maximum dimension 13 (mm), surface dry density 2.71 (g / cm 3)) and Masterglanium SP8SV (manufactured by BASF Japan Ltd.) was used as the AE water reducer. The mix ratio was W / C = 55 (%). After pouring, the concrete was sealed and cured for 28 days in a cool, dark place at about 20 (℃). The compressive strength was calculated as the average value obtained from compressive strength tests based on JIS A 1108 for 70 test specimens, three cylindrical specimens with dimensions of φ100 (mm) x 200 (mm).
[0203] The specimen 70 was processed in the following order: bending crack introduction, crack repair, and waterproofing treatment. The cracks were introduced by placing a steel wedge of 200 mm or more in the center of the surface of the specimen 70 in the width direction (perpendicular to the rebar axis) of the specimen 70 with the exposed surface turned sideways, and compressive loading. The crack width of the exposed surface was measured with a crack scale during loading and unloading, and loading and unloading were repeated so that the maximum crack width at unloading was about 0.4 mm. As a result, the crack width of each specimen 70 was 0.35 to 0.45 mm. Furthermore, the cracks were repaired by a low-pressure injection method using Konishi's civil engineering and construction bond E206 depending on the cause. After the repair, it was visually confirmed that the repair agent was filled inside the cracks. After that, to limit saltwater intrusion in one direction, a heavy-duty anticorrosive paint called tar epoxy (Epotal BO Eco, Nippon Paint Co., Ltd.) was applied to the five surfaces other than the exposed surface.
[0204] After processing, the specimens were placed in a tidal environment simulator (hereafter referred to as a tidal tank) at the Central Research Institute of the Electric Power Industry (a general incorporated foundation) to accelerate corrosion. The environmental conditions were a temperature of 40°C, a relative humidity of 30-100% RH, and one cycle of immersion in a 3% NaCl aqueous solution for 0.5 hours and then in the air for 11.5 hours, with two cycles per day. Specimens 70 were placed with the exposed surface facing sideways, approximately 2 cm apart from each other to allow seawater to enter from the exposed surface.
[0205] 3.3.2 Measurement method The measurement procedure for specimen 70 is shown in Figures 49A and 49B. When making measurements, it was first confirmed that the tidal tank was drained, and then specimen 70 was rotated so that the exposed surface was facing up. Next, terminals were installed on the exposed surface, and measurements were performed using two types of terminal arrangements: measurement (1) shown in Figure 49A and measurement (2) shown in Figure 49B. A series of measurements was performed before the installation of the tidal tank (before corrosion was promoted) and two weeks after installation (two weeks after corrosion). The measurement terminals were stainless steel and measured 10 mm x 40 mm x 10 mm in size, and the 10 mm x 40 mm surface was brought into contact with the concrete, sandwiching a hydrogel sheet, so that the terminal length in the longitudinal direction of the rebar was 10 mm. Based on the knowledge gained in Chapter 2, the terminal arrangement was current terminal C 1、 C2 on the outside, potential difference measurement terminal P 1、 P2 is the inner terminal, and the distance between the two inner terminals is D. in =D out The measurement (1) shown in Figure 49A was set to -40 mm. fH (Ω) and low frequency resistance R fL (Ω). The distance between the two outer terminals is D out = 80, 120, 160, 200, 240 mm, and four terminals were placed on the surface of the concrete directly above and parallel to the internal rebar of the test piece 70 to measure the impedance. The applied voltage was 1.0 (V), and the frequency was 0.08 Hz to 1,000 Hz. Next, measurement (2) shown in Figure 49B was performed to measure the electrical resistance R of the concrete. s (Ω) is measured at a position on the concrete surface that is not directly above the rebar and is not cracked. out = 80 mm, D in The electrical resistance was measured at a frequency of 100 Hz with a diameter of 40 mm.
[0206] Here, each D out The electrical resistance of concrete at R s (D out )(Ω), then R s (80mm)(Ω) is calculated as the measured value. out Apparent nondestructive polarization resistance R ’ p-ni To calculate (Ω), R s (D out)(Ω) is required. s (80mm)(Ω) is first converted to electrical resistivity ρ(Ωm), and then out R in s (D out )(Ω). Using the following equation (23), R s (D out ) (Ω) can be converted to electrical resistivity ρ.
[0207] ρ = G p (D out )·R s (D out ) ···(twenty three)
[0208] Where: G p (D out ) is the distance between the two outer terminals D out is the electrode arrangement coefficient in
[0209] G p (D out ), R s (D out ) was calculated by performing a current dispersion analysis using FEM in advance, and the values shown in Table 13 below were calculated.
[0210] [Table 13]
[0211] This analysis was carried out by creating the geometry of the specimen 70 in Figure 47, which had no reinforcing bars embedded in concrete, and four terminals placed on the surface, and by using the analysis procedure shown in Chapter 2, 2.3.3, each D out Electrical resistance R of concrete at s (D out ) is calculated, and the electrode arrangement coefficient G is calculated using the electrical resistivity ρ (Ωm) set as the input value by equation (23). p (D out )
[0212] G obtained from this analysis p(D out ) to obtain the measurement result R s (80mm) to R s (D out ) was converted.
[0213] R s (D out ) = ρ / G p (D out ) = (R s (80mm) G p (80mm)) / G p (D out ) ···(twenty four)
[0214] The R calculated in this way s (D out ) and each D out R in fH (Ω) and R fL (Ω), the apparent nondestructive polarization resistance R is calculated using the above equation (9-3). ’ p-ni After the series of measurements were completed, the test piece 70 was returned to its original state, and the accelerated corrosion was continued.
[0215] 3.3.3 Impedance measurement results using the non-destructive polarization resistance method Figure 50A shows the Nyquist plot for each of the two outer terminal spacings measured for the NN factor after two weeks of accelerated corrosion. A crack-free test specimen 70 is placed in a tidal tank, and since it is not normally considered that chloride ions would penetrate to the rebar position (100 mm from the exposed surface) and cause corrosion in two weeks, it is treated as a sound factor. out For D = 120, 160, 200, and 240 mm, a shape resembling a part of a semicircle appeared at the position where Imag(Z) was negative on the complex plane. This indicates that a parallel circuit of resistors and capacitors exists at the interface between the rebar and the concrete, and it can be determined that a measurable amount of current flows into the rebar, resulting in an impedance that includes the effect of the polarization resistance of the rebar surface. On the other hand, for D out When the impedance was 80 mm, the impedance could not be considered to be semicircular.
[0216] Next, the frequency-Real(Z) relationship is shown in Figure 50B. The impedance including the current passing through the inside of the reinforcing bar (the current passing through R2 in the equivalent circuit shown in Figure 10) has the characteristic that Real(Z) increases as the frequency shifts from high to low. out Such features were observed only when D = 120 mm or more. out In the case of D = 80 mm, this characteristic was not observed, and it is considered that the current passing through the inside of the rebar could not be detected. out It was found that measurement was possible by setting the distance to ≧120mm.
[0217] 3.3.4 Proposal for setting the spacing between the two outer terminals according to the covering When performing the non-destructive polarization resistance method, it is necessary to determine the appropriate terminal arrangement based on various measurement conditions. However, with the knowledge obtained in 3.3.3 (c = 100 (mm)), the outer two terminal spacing D out ≧120(mm)) cannot be applied to other measurement targets. Also, in order to determine the terminal arrangement, the outer two terminal spacing D out Therefore, by using the measurement results for test piece 70 and current dispersion analysis by FEM, an appropriate D out Here, we propose a method for setting the above formula (9-3) as follows.
[0218]
number
[0219] however, R s (Ω) is the resistance of the concrete alone. R fH (Ω) is the high frequency resistance when current flows through the rebar. R fL (Ω) is the low frequency resistance when current flows through the rebar.
[0220] The interpretation of this equation (9-3) is R ’ p-ni Since is always a positive value, R fH <R fL <R s The prerequisite is that the following holds true. Here, R s and R fH If the difference between is small, R fL The range of values that can be taken by R becomes narrower. fL is calculated by fitting a semicircular curve to the Nyquist plot obtained by impedance measurement under the condition that some of the current flows into the rebar. s and R fH If the difference between R and R is small, even a small variation in measurement or fitting may affect the corrosion judgment. s and R fH The larger the difference, the greater the R fL It is believed that by widening the range of values that R can take, the effect of variation becomes less and the accuracy of corrosion judgment increases. s and R fH When the difference between these is small, the resistance R2 in the equivalent circuit of FIG. 10 becomes large, that is, when the amount of current flowing into the reinforcing bar is small due to a large covering depth or the like.
[0221] Therefore, the difference between the electrical resistance of concrete and the high-frequency resistance (R s -R fH ) was used as an index for optimizing the terminal layout. First, the (R s -R fH The experimental values of (R s -R fH ) is D out In the range of ≦160 mm, D out It increases with increasing D out At ≧160mm, it was almost constant. s -R fH ) is larger, the accuracy of corrosion judgment is improved. out It was found that a setting of 160mm or more is recommended.
[0222] Next, the analysis (R s -R fH The relationship between the distance between the two outer terminals and the cover thickness was reproduced. s -R fH ) is considered to vary, so a parametric study was conducted with cover thicknesses of 30, 60, and 100 mm. This analysis was conducted by creating the geometry of the reinforcing bar, concrete, and four terminals placed on the surface with the same dimensions as those of specimen 70 in Figure 47, and following the analysis procedure shown in 2.3.3. The electrical resistivity of concrete is D out = 80mm R s (80mm)(Ω) was converted by equation (23) to ρ=113(Ωm). out Electrical resistance R of concrete at s (D out ) and the distance between the two outer terminals D out The set values were 50, 80, 120, 160, and 200 mm.
[0223] The analysis results are shown in Figure 52. According to the experimental results, when the cover is 100 mm, D out ≧160mm was recommended, so D out = Resistance value at 160 mm (R s -R fH )=150(Ω) or more D out The calculation was also performed for the cases of c=30 and 60 mm. As a result, D out = 70mm or more, c = 60mm and D out = 120mm or more is recommended. Here, D out When / c was calculated for each fog, D out / c≧70 / 30=2.33 (c=30mm), 2.0 (c=60mm), 1.6 (c=100mm). Rounding up to the second decimal place gives D out The formula expressing the recommended value in terms of cover c is given by (25).
[0224] D out / c ≧ 2.4 (25)
[0225] When measuring on-site, refer to this formula and determine the distance D between the two outer terminals based on the cover c. out It is believed that appropriate measurements can be made by setting the value. However, it should be kept in mind that this recommended value depends on the current measurement sensitivity of the potentiostat being used, and is not always valid regardless of the device. Also, it is not possible to determine the D out The conclusion is that the larger the value, the more accurate the measurement, so we will show the disadvantages of using an excessively large value. In real structures, multiple rebars are embedded in the concrete, and D out When D is large, it is thought that the current will flow into rebars other than the rebar being measured, causing the measurement value to change. Therefore, it is necessary to set D to a level that is not affected by other rebars. out It is important to reduce
[0226] 3.3.5 Corrosion diagnosis for deep-covered specimens The grading proposed by the CEB (European Board of Concrete) as shown in Table 14 is often used to judge the presence or absence of corrosion and the tendency of the corrosion rate. Here, the polarization resistance R calculated by the conventional three-electrode method is p (kΩcm 2 The corrosion rate is classified into four stages according to the value of non-destructive polarization resistance R p-ni (kΩcm 2 ) is the polarization resistance R p The analytical results in 3.2.2 have already shown that the value is approximately equal to R p The value of R p-ni By comparing the results with the criteria set forth above, the tendency of the corrosion rate can be determined.
[0227] [Table 14]
[0228] Therefore, the non-destructive polarization resistance method was used to measure and calculate R p-ni The results of the corresponding CEB grading are shown in Figure 53. The measurement conditions are as follows: out The measurement was performed with the setting of R = 240 mm. The measurement results for each test piece 70 are shown in a bar graph. As an example of a criterion for determining whether corrosion is present or absent, if the boundary between the grades of low to medium corrosion rate and medium to high corrosion rate is set, R p =130(kΩcm 2 ) is the boundary, and if it is above that value, it is judged to be in a passive state in Table 14, that is, the rebar is sound, and if it is below that value, it is judged to be corroded. From Figure 53, before the corrosion promotion, R p-ni >130(kΩcm 2 After two weeks of accelerated corrosion, the NN factor, which had no cracks, and the CR factor, which had cracks repaired before the accelerated corrosion, were judged to be in good condition, while the CN factor, which had cracks, had a high value of R p-ni <130(kΩcm 2 ), and so it was determined that corrosion had occurred. From this, it was inferred that in the CN factor, saltwater had penetrated through cracks approximately 0.4 mm wide, causing the chloride ion concentration on the surface of the rebar to exceed the threshold for corrosion, causing corrosion of the rebar inside the concrete. On the other hand, in the case of the CR factor, where the cracks had been repaired, saltwater was prevented from penetrating through the cracks, and it is believed that no corrosion occurred. Therefore, it became clear that the nondestructive polarization resistance method is fully applicable to test specimen 70, which has a deep cover that is intended to be a coastal structure, and can at least be used to determine the presence or absence of corrosion.
[0229] Chapter 4 Corrosion detection device and corrosion detection method using the proposed method 4.1 Corrosion detection equipment Next, a configuration of a corrosion detection device that implements a corrosion detection method according to an embodiment will be described. Fig. 54 is a diagram showing an example of a schematic configuration of a corrosion detection device 10 according to an embodiment. Fig. 54 shows a concrete structure 1 that simulates a concrete structure. In the concrete structure 1, reinforcing bars 2 are provided so that their depths from the surface are the same inside.
[0230] The corrosion detection device 10 has two current terminals C 1、 C2 and two potential difference measurement terminals P 1、 P2. Current terminal C 1、 C2 and potential difference measurement terminal P 1、 P2 are electrodes. Current terminal C 1、 C2 and potential difference measurement terminal P 1、 P2 is placed on the surface of the concrete 1. Current terminal C 1、 C2 are placed on the surface of the concrete 1 at intervals. 1、 P2 is the current terminal C 1、 Current terminals C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C19, C20, C21, C22, C23, C24, C25, C26, C27, C28, C31, C32, C41, C52, C63, C74, 1、 Current terminal C at the same distance from C2 1、 In Figure 54, the potential difference measurement terminal P 1、 P 2を , current terminal C 1、 It is placed inside C2. Current terminal C 1、 C2, potential difference measurement terminal P 1、 Cords 12a-12d are individually connected to P2.
[0231] The corrosion detection device 10 includes a power supply unit 20, a measurement unit 21, and a control unit 22. The power supply unit 20 is connected to current terminals C1 and C2 via cords 12a and 12d. The measurement unit 21 is connected to a potential difference measurement terminal P 1、 It is connected to P2.
[0232] The power supply unit 20 is an AC power supply with a variable frequency. When detecting corrosion of the reinforcing bar 2, the power supply unit 20 applies AC power to the current terminals C1 and C2 via the cords 12a and 12d. For example, the power supply unit 20 applies AC power to the current terminals C1 and C2 while changing the frequency within a predetermined frequency range. The frequency range is, for example, 0.1 Hz to 1000 Hz. In the concrete 1, a current 13 flows through the inside of the concrete 1 and the reinforcing bar 2 between the current terminals C1 and C2 in response to the AC power applied from the current terminals C1 and C2.
[0233] The measuring unit 21 is a terminal P for measuring a potential difference when AC power is applied from the power supply unit 20. 1、 The measurement unit 21 measures the potential difference between P and P2. The measurement unit 21 outputs measurement data indicating the measured potential difference to the control unit 22.
[0234] The control unit 22 comprehensively controls the operation of the corrosion detection device 10. The control unit 22 is, for example, a computer, and has a controller 30, a user interface 31, and a storage unit 32.
[0235] The controller 30 includes a CPU (Central Processing Unit) and controls the power supply unit 20 .
[0236] The user interface 31 is composed of a keyboard for inputting commands for operating the corrosion detection device 10 and various pieces of information, a display for visualizing and displaying the corrosion detection results, and the like.
[0237] The storage unit 32 stores various programs executed by the controller 30. For example, the storage unit 32 stores a program for executing a corrosion detection process described below. Furthermore, the storage unit 32 stores various data used in the programs executed by the controller 30. For example, the storage unit 32 stores measurement data 33 output from the measurement unit 21. The various programs and data may be stored in a computer-readable computer recording medium (for example, a hard disk, an optical disk such as a DVD, a flexible disk, a semiconductor memory, etc.). Furthermore, the various programs and data may be stored in another device and read out online via, for example, a dedicated line for use.
[0238] When measuring the corrosion of reinforcing bar 2 in concrete 1, current terminal C 1、 C2 and potential difference measurement terminal P 1、 P2 is placed in a straight line at a position above the reinforcing bar 2 of the concrete 1. Then, AC power is applied from the power supply unit 20, and the measurement unit 21 measures the potential difference between the terminals P 1、 In an actual concrete structure, the arrangement of the reinforcing bars 2 is detected based on the design data showing the arrangement of the reinforcing bars 2, or by other means, and the current terminal C is placed at the top of the reinforcing bars 2. 1、 C2 and potential difference measurement terminal P 1、 Place P2. Potential difference measurement terminal P 1、 It is preferable that P2 is disposed at an interval of 2.4 times or more the covering thickness c of the reinforcing bar in the concrete 1. In this case, the measurement data 33 is obtained by measuring the current terminal C along the reinforcing bar 2. 1、 C2 and potential difference measurement terminal P 1、 The first measurement data is obtained by placing P2.
[0239] On the other hand, the resistance of concrete 1 R s When measuring, use current terminal C 1、 C2 and potential difference measurement terminal P 1、 P2 is placed at a position other than the buried position of rebar 2 or at the current terminal C 1、 The intervals between the current terminals C2 are set so that no current flows into the reinforcing bar 2. For example, 1、The interval between the reinforcing bars C2 is set to be less than 2.4 times the covering area c of the reinforcing bars 2 in the concrete 1. Then, AC power is applied from the power supply unit 20, and the potential difference measurement terminal P 1、 The potential difference between the current terminals C and P2 is measured. 1、 C2 and potential difference measurement terminal P 1、 P2 is placed at a position other than the buried position of rebar 2 or at the current terminal C 1、 The second measurement data includes data in which the spacing C2 is measured as a spacing at which no current flows into the inside of the reinforcing bar 2 (less than 2.4 times the cover c).
[0240] The controller 30 has an internal memory for storing programs and data, reads out programs stored in the storage unit 32, and executes the processing of the read out programs. The controller 30 functions as various processing units as the programs run. For example, the controller 30 has the functions of a calculation unit 30a and an output control unit 30b.
[0241] The calculation unit 30a calculates the polarization resistance from the measurement data 33 by the non-destructive polarization resistance method of the present disclosure described above.
[0242] Specifically, the calculation unit 30a calculates the apparent nondestructive polarization resistance R ’ p-ni Calculate the apparent nondestructive polarization resistance R ’ p-ni is the current terminal C 1、 C2, potential difference measurement terminal P 1、 P2 is the polarization resistance of the surface of the reinforcing bar 2 in a four-electrode arrangement. For example, the calculation unit 30a calculates the AC impedance for each frequency from the potential difference for each frequency indicated by the first measurement data included in the measurement data 33. The calculation unit 30a calculates the high-frequency resistance R fH and low frequency resistance R fLIn the Nyquist plot, it appears as a part of a semicircular plot as shown in FIG. 12. The calculation unit 30a performs curve fitting on a part of the semicircle, and calculates Real(Z) at the intersection with the real axis on the high frequency side as the high frequency resistance R fH , the intersection point Real(Z) with the real axis on the low frequency side is the low frequency resistance R fL The calculation unit 30a also calculates the electrical resistance R of the concrete from the second measurement data included in the measurement data 33. s For example, the calculation unit 30a calculates the value of Real(Z) at a frequency of 100 Hz as the electrical resistance R s The calculation unit 30a then calculates the calculated high-frequency resistance R fH , low frequency resistance R fL , the electrical resistance of concrete R s Non-destructive polarization resistance R ’ p-ni The calculation unit 30a calculates the high-frequency resistance R fH , low frequency resistance R fL , the electrical resistance of concrete R s From the above, the nondestructive polarization resistance R is calculated using equation (9-3). ’ p-ni The electrical resistance of concrete R s When measuring the same location multiple times or when measuring the same concrete 1 multiple times, it is acceptable to calculate it once and use it instead of calculating it every time. s If the value is determined by a prior survey or the like, the predetermined value may be set via the user interface 31 or the like. In this case, the electrical resistance R of the concrete s The calculation of is not necessary.
[0243] Then, the calculation unit 30a calculates the measurement area A ni and terminal arrangement magnification r 2 / 4 The apparent nondestructive polarization resistance R calculated based on ’ p-ni From the two-terminal non-destructive polarization resistance R p-ni(2) Calculate the non-destructive polarization resistance R p-ni(2)is the polarization resistance of a two-terminal arrangement that does not take into account the resistance between the terminals and the concrete. For example, the calculation unit 30a calculates the apparent non-destructive polarization resistance R ’ p-ni The area to be measured is A ni Multiplying by 4 terminals to obtain the non-destructive polarization resistance R p-ni(4) Then, the calculation unit 30a calculates the nondestructive polarization resistance R as shown in formula (11). p-ni(4) Terminal arrangement magnification r 2 / 4 Multiplying by R to obtain the nondestructive polarization resistance of the two-terminal configuration p-ni(2) Calculate.
[0244] Measured area A ni and terminal arrangement magnification r 2 / 4 A previously calculated value may be set via the user interface 31 or the like. ni and terminal arrangement magnification r 2 / 4 may be calculated by analysis using an analytical model that simulates the concrete 1 or by the above-mentioned simple estimation formula.
[0245] Measured area A ni As described above in 2.3.5, can be calculated from an analytical model simulating the concrete 1. For example, the calculation unit 30a constructs an analytical model simulating the concrete 1. The calculation unit 30a calculates the current terminal C 1、 For example, the calculation unit 30a sets an insulating surface at a portion other than the reinforcing bar 2 between the current terminals C 1、 The calculation unit 30a analyzes the current density on the reinforcing bar surface where the current due to the AC power flows into the reinforcing bar 2, using an analysis model in which the insulating surface is set. The calculation unit 30a then calculates the current density on the reinforcing bar surface by calculating the current density on the reinforcing bar surface at the current terminal C 1、 Current terminal C on the circumference of rebar 2 at the bottom of C2 1、 The area of the rebar surface that is equal to or greater than the current density at the center of the height of rebar 2 in the C2 direction is called the measured area A. ni For example, the calculation unit 30a performs cutoff using the cut points shown in FIGS. 23A to 23C to calculate the measurement area A ni Calculate.
[0246] In addition, the measurement area A ni can be calculated from equation (21) by inputting the reinforcing bar diameter φ of the reinforcing bar 2 and the cover thickness (cover c) of the reinforcing bar 2 from the user interface 31.
[0247] Terminal arrangement magnification r 2 / 4 As described above in 2.3.5 and 2.4.3, the calculation unit 30a can calculate the current from the analysis model simulating the concrete 1. For example, the calculation unit 30a calculates the current from the current terminal C 1、 The terminal arrangement magnification r is calculated by comparing the analysis of the two-terminal arrangement that does not consider the contact resistance between C2 and concrete 1 with the analysis of the four-terminal arrangement. 2 / 4 Calculate.
[0248] In addition, the terminal arrangement magnification r 2 / 4 is connected to the user interface 31 and to the current terminal C 1、 C2 Spacing (Outer 2 Terminal Spacing D out) By inputting the above, it can be calculated from equation (22).
[0249] The calculation unit 30a calculates a non-destructive polarization resistance R p-ni(2) For example, as shown in Figure 43C, the corrosion rate is calculated by the nondestructive polarization resistance R p-ni(2) is the polarization resistance R p Therefore, the calculation unit 30a calculates R p-ni(2) =R p Using equation (3), the nondestructive polarization resistance R p-ni(2) The calculation unit 30a calculates the corrosion rate CR from the corrosion current density i0 using equation (4).
[0250] The output control unit 30b performs various output controls. For example, the output control unit 30b displays information based on the corrosion rate calculated by the calculation unit 30a on the user interface 31. Also, for example, the output control unit 30b outputs data on the corrosion rate calculated by the calculation unit 30a to an external terminal device via a network (not shown).
[0251] 4.2 Corrosion detection process Corrosion detection for concrete structures can be roughly divided into three stages: prior examination, measurement using the corrosion detection device 10, and corrosion detection using the corrosion detection device 10.
[0252] In the preliminary study stage, the diameter and state of rebar in the concrete structure to be subjected to corrosion detection are identified based on design and construction documents. In addition, non-destructive testing methods such as electromagnetic radar and electromagnetic induction methods are used to estimate the position of rebar and cover in the concrete structure. In an actual concrete structure, there is a concern that rebar may be located in a position different from that described in the design and construction documents due to construction errors, so the position of rebar and cover are estimated using non-destructive testing methods. Measurement positions for the concrete structure are determined based on the results of the preliminary study.
[0253] In the measurement stage, the corrosion detection device 10 measures the determined measurement position of the concrete structure. In the measurement stage, the distance between the two outer terminals D is calculated based on the formula (25) according to the estimated cover value c obtained in the preliminary study stage. out (mm). For example, the potential difference measurement terminal P 1、 Based on formula (25), P2 is set to an interval of 2.4 times or more the covering thickness c of the rebar in concrete 1. In this case, if current flows into areas other than the rebar being measured, the area A ni (cm 2 ) and terminal arrangement magnification r 2 / 4 Therefore, it is necessary to measure D so that the current does not flow into other rebars, for example by making sure that the intersections of the lattice-shaped reinforcement are not included in the measurement range. out If multiple rebars are included in the measurement range, a current dispersion analysis simulating the reinforced concrete and terminal arrangement should be performed separately to determine the A ni (cm 2 ) and r 2 / 4 It is necessary to calculate
[0254] An example of measurement positions on a concrete structure is shown in Fig. 55. In Fig. 55, a concrete structure is shown, with embedded reinforcing bars 2 indicated by dotted lines.
[0255] In the measurement stage, measurement (a) is carried out by injecting current into the rebar 2. In measurement (a), the current terminal C 1、 C2 and potential difference measurement terminal P 1、 The four terminals of P2 are connected parallel to and directly above the axis of rebar 2, and 1、 C2 is placed on the outside and AC impedance is measured. 1、 P2 is placed at an interval that is 2.4 times or more the covering thickness c of the reinforcing bar in the concrete 1. Corrosion detecting device 10 stores the measurement data obtained by measurement (a) in measurement data 33 of memory unit 32 as first measurement data.
[0256] In the measurement stage, measurement (b) or measurement (c) is carried out without current flowing into rebar 2. In measurement (b), four terminals are placed at positions shifted from directly above rebar 2 at the same intervals as in measurement (a) to measure the AC impedance. In measurement (c), the terminals are placed directly above rebar 2, but the D is measured until almost no current flows into rebar 2. out D out In the method of reducing R, refer to the measurement in 3.3.2 and the method of converting the measurement results by the current dispersion analysis method. s D during measurement out The measurement results by R fL and R fH D during measurement out Convert to the value of R s In order to shorten the measurement time, the measurement may be performed at a constant frequency of about 1-100 (Hz) as an alternative to AC impedance measurement. The corrosion detection device 10 stores the measurement data obtained by measurement (b) or measurement (c) in measurement data 33 of the memory unit 32 as second measurement data.
[0257] In the corrosion detection stage, corrosion detection is performed by executing a corrosion detection process by the corrosion detecting device 10. Fig. 56 is a flowchart illustrating an example of a procedure of the corrosion detection process according to the embodiment.
[0258] The calculation unit 30a calculates the apparent non-destructive polarization resistance R of the four-electrode arrangement from the measurement data 33. ’ p-ni For example, the calculation unit 30a calculates the AC impedance for each frequency from the potential difference for each frequency indicated by the first measurement data included in the measurement data 33, and calculates the high-frequency resistance R from a Nyquist plot showing the AC impedance for each frequency on a complex plane. fH and low frequency resistance R fL The calculation unit 30a also calculates the electrical resistance R of the concrete from the second measurement data included in the measurement data 33. s For example, the calculation unit 30a calculates the value of Real(Z) at a frequency of 100 Hz as the electrical resistance R s The calculation unit 30a then calculates the calculated high-frequency resistance R fH , low frequency resistance R fL , electrical resistance of concrete R s Non-destructive polarization resistance R of four electrodes ’ p-ni The electrical resistance of concrete R s If the electrical resistance of the concrete is known in advance, R s may be set to a fixed value. In this case, measurements (b), (c) and the electrical resistance of the concrete R s There is no need to calculate
[0259] The calculation unit 30a calculates the measurement area A ni For example, the current terminal C 1、 C2 Spacing (Outer 2 Terminal Spacing D out) The calculation unit 30a calculates the input distance D between the two outer terminals by using the formula (22). out) From the measured area A ni The calculation unit 30a calculates the measurement area A by analyzing an analytical model simulating the concrete 1. ni Also, the measured area A ni If is known in advance, the area to be measured A niA fixed value may be set to , in which case step S11 is unnecessary.
[0260] The calculation unit 30a calculates the terminal arrangement magnification r 2 / 4 (Step S12). For example, the user inputs the reinforcing bar diameter φ of the reinforcing bar 2 and the cover thickness (cover c) of the reinforcing bar 2 from the user interface 31. The calculation unit 30a calculates the terminal arrangement magnification r from the input reinforcing bar diameter φ of the reinforcing bar 2 and the cover c of the reinforcing bar 2 using the formula (22). 2 / 4 The calculation unit 30a calculates the terminal arrangement magnification r by analyzing an analytical model simulating the concrete 1. 2 / 4 Also, the terminal arrangement magnification r 2 / 4 If is known in advance, the terminal layout magnification r 2 / 4 A fixed value may be set to , in which case step S12 is unnecessary.
[0261] The calculation unit 30a calculates the measurement area A ni and terminal arrangement magnification r 2 / 4 Based on this, the apparent non-destructive polarization resistance R calculated in step S10 ’ p-ni From the two-terminal non-destructive polarization resistance R p-ni(2) For example, the calculation unit 30a calculates the apparent nondestructive polarization resistance R by using the formulas (10) and (11). ’ p-ni Non-destructive polarization resistance R of two terminals p-ni(2) Calculate.
[0262] The calculation unit 30a calculates a non-destructive polarization resistance R p-ni(2) For example, the calculation unit 30a calculates the corrosion rate CR from R p-ni(2) =R p Using equations (3) and (4), the nondestructive polarization resistance R p-ni(2) The corrosion rate CR is calculated from the above.
[0263] The output control unit 30b outputs the calculation result (step S15), and ends the process. For example, the output control unit 30b causes the user interface 31 to display the calculated corrosion rate CR and the grading of the corrosion rate CR in the CEB.
[0264] In this way, the corrosion detection process according to the embodiment detects the polarization resistance R of the reinforcing bar 2 inside the concrete 1 from the surface of the concrete 1. p can be calculated with high accuracy. As a result, the corrosion detection process according to the embodiment can calculate the corrosion rate CR of the reinforcing bar 2 with high accuracy, and can quantitatively evaluate the corrosion rate CR of the reinforcing bar 2. Furthermore, the corrosion detection according to the embodiment can perform corrosion detection of a concrete structure in a non-destructive manner.
[0265] The information required for the corrosion detection process in the embodiment is the rebar diameter φ, the distance between the two outer terminals D out , cover thickness c, and reinforcing bar spacing and reinforcing bar intersections in a grid pattern. This necessary information can be obtained at the preliminary examination stage of the design and construction documents of the concrete structure. This can improve the on-site applicability of corrosion detection of concrete structures. In addition, when the simplified estimation formulas (21) and (22) disclosed in 3.2.3 are used, the corrosion detection in the embodiment can be performed with the current terminal C 1、 C2 Spacing (Outer 2 Terminal Spacing D out ), the reinforcing bar diameter φ of reinforcing bar 2, and the cover thickness of reinforcing bar 2 (cover c) can be input, allowing the corrosion rate evaluation results to be calculated instantly on-site without performing current dispersion analysis.
[0266] 4.3 Effects In this way, the corrosion detection device 10 according to the present embodiment is provided with a current terminal C at a distance from the surface of the concrete 1 having the reinforcing bar 2 (71) provided therein. 1、 Place C2 (the two first electrodes) and current terminal C 1、 Current terminals C are spaced apart on the inside or outside of C2. 1、 The same distance from C2 (distance D cp ) at current terminal C 1、 Potential difference measurement terminal P in a straight line with C2 1、 Place P2 (the two second electrodes) and current terminal C1、 Apply AC power to C2 at a frequency within a specified frequency range and measure the potential difference at terminal P 1、 The non-destructive polarization resistance R was calculated from the measurement data 33 that measured the potential difference of P2. ’ p-ni The corrosion detection device 10 calculates the polarization resistance (of the four-electrode arrangement) (step S10). 2 / 4 (Conversion factor) based on the calculated non-destructive polarization resistance R ’ p-ni From the above, the non-destructive polarization resistance R of the two-electrode arrangement p-ni(2) (polarization resistance of the two-electrode arrangement) is calculated (step S13). As a result, the corrosion detection device 10 calculates the polarization resistance of the reinforcing bar 2 from the surface of the concrete 1 to the inside (polarization resistance R p ) can be detected with high accuracy.
[0267] In addition, the corrosion detection device 10 calculates the non-destructive polarization resistance R ’ p-ni The measurement area Ani and terminal arrangement magnification r 2 / 4 Multiplying by , we get the nondestructive polarization resistance R of the two-electrode arrangement. p-ni(2) In this way, the corrosion detection device 10 calculates the non-destructive polarization resistance R ’ p-ni Non-destructive polarization resistance R of two electrodes p-ni(2) can be calculated.
[0268] In addition, the terminal arrangement magnification r 2 / 4 is the interval D cp The shorter the interval D, the smaller the value. cp The non-destructive polarization resistance R of the two-electrode arrangement corresponding to p-ni(2) can be calculated.
[0269] In addition, the corrosion detection device 10 constructs an analytical model simulating the concrete 1, and a current terminal C 1、 An insulating surface is set in the area other than rebar 2 between current terminals C2, and the current density on the surface of rebar 2 where the current due to AC power flows into rebar 2 is analyzed. The current density on the surface of rebar 2 is calculated by dividing the current density by the current terminal C 1、 Current terminal C on the circumference of rebar 2 at the bottom of C2 1、The area of the surface of the reinforcing bar 2 where the current density is equal to or greater than the current density at the center point of the height of the reinforcing bar 2 in the C2 direction is calculated as the measurement area Ani (step S11). The corrosion detection device 10 uses the calculated measurement area Ani to calculate the nondestructive polarization resistance R p-ni(2) (Step S13). This allows the corrosion detection device 10 to accurately calculate the measurement area Ani, and the non-destructive polarization resistance R p-ni(2) can be calculated with high accuracy.
[0270] The corrosion detection device 10 also uses equation (22) (first calculation equation) to calculate a measurement area Ani from the diameter of the reinforcing bar 2 in the concrete 1 and the cover thickness (cover c) of the reinforcing bar 2 (step S11). Using the calculated measurement area Ani, the corrosion detection device 10 calculates a nondestructive polarization resistance R p-ni(2) (Step S13). This allows the corrosion detection device 10 to easily and accurately calculate the measurement area Ani, and the nondestructive polarization resistance R p-ni(2) can be calculated with high accuracy.
[0271] In addition, the corrosion detection device 10 constructs an analytical model simulating the concrete 1 and detects the current terminal C 1、 Potential difference measurement terminal P for C2 1、 Terminal layout magnification r according to P2 layout 2 / 4 (Step S12). The corrosion detection device 10 calculates the calculated terminal arrangement magnification r 2 / 4 Using the non-destructive polarization resistance R of the two-electrode arrangement, p-ni(2) (Step S13). As a result, the corrosion detection device 10 calculates the terminal arrangement magnification r 2 / 4 can be calculated with high accuracy, and the non-destructive polarization resistance R p-ni(2) can be calculated with high accuracy.
[0272] In addition, the corrosion detection device 10 calculates the current terminal C 1、 Terminal arrangement magnification r from the spacing of C2 2 / 4 (Step S12). The corrosion detection device 10 calculates the calculated terminal arrangement magnification r 2 / 4Using the non-destructive polarization resistance R of the two-electrode arrangement, p-ni(2) (Step S13). As a result, the corrosion detection device 10 calculates the terminal arrangement magnification r 2 / 4 can be calculated easily and accurately, and the non-destructive polarization resistance R p-ni(2) can be calculated with high accuracy.
[0273] The corrosion detection device 10 also includes a non-destructive polarization resistor R p-ni(2) The corrosion rate CR is calculated from the above (step S14). This enables the corrosion detecting device 10 to accurately calculate the corrosion rate CR.
[0274] Also, measurement data 33 is for current terminal C 1、 The interval between C2 is set to 2.4 times or more the thickness (cover c) of the cover of the reinforcing bar 2 in the concrete 1, and the current terminal C is connected along the reinforcing bar 2. 1、 C2 and potential difference measurement terminal P 1、 The corrosion detection device 10 calculates the AC impedance for each frequency from the potential difference for each frequency indicated by the first measurement data, and calculates the high-frequency resistance R from a Nyquist plot showing the AC impedance for each frequency on a complex plane. fH and low frequency resistance R fL Calculate the high-frequency resistance R fH and low frequency resistance R fL and the electrical resistance R of a given concrete 1 s Non-destructive polarization resistance R ’ p-ni In this way, the corrosion detection device 10 calculates the non-destructive polarization resistance R of the corroded reinforcing bar 2 from the surface of the concrete 1 to the inside. ’ p-ni can be calculated with high accuracy.
[0275] Also, measurement data 33 is for current terminal C 1、 C2 and potential difference measurement terminal P 1、 P2 is placed at a position other than the buried position of rebar 2 or at the current terminal C 1、The corrosion detection device 10 further includes second measurement data obtained by measuring the interval C2 as an interval through which no current flows into the interior of the reinforcing bar 2. The interval through which no current flows is, for example, an interval that is less than 2.4 times the thickness (cover c) of the cover of the reinforcing bar 2 in the concrete 1. The corrosion detection device 10 determines the electrical resistance R s Calculate the high frequency resistance R fH and low frequency resistance R fL The calculated electrical resistance of concrete 1 is R s Non-destructive polarization resistance R ’ p-ni In this way, the corrosion detection device 10 calculates the non-destructive polarization resistance R of the corroded reinforcing bar 2 from the surface of the concrete 1 to the inside. ’ p-ni can be calculated with high accuracy.
[0276] In addition, current terminal C 1、 C2 are arranged at intervals of 2.4 times or more the cover c (cover thickness) of the reinforcing bar 2 in the concrete 1. In this way, the corrosion detection device 10 can measure the non-destructive polarization resistance R ’ p-ni can be calculated with high accuracy.
[0277] In addition, the potential difference measurement terminal P 1、 P2 is the current terminal C 1、 Inside C2, there are spaces D cp potential difference measurement terminal P 1、 P2 Spacing D in This allows the corrosion detection device 10 to calculate a large impedance, and the non-destructive polarization resistance R ’ p-ni can be calculated more accurately. EXAMPLES
[0278] Although the disclosed device has been described above by way of example, the disclosed technology may be embodied in various different forms other than the above-described example. Therefore, other embodiments included in the present invention will be described below.
[0279] For example, in the above embodiment, the corrosion detection device applies AC power to the concrete 1 to measure the potential difference, and calculates the non-destructive polarization resistance R from the measured measurement data 33. p-ni(2) In the above description, the corrosion detection device is described as calculating the corrosion rate CR and the non-destructive polarization resistance R from the measured data 33. p-ni(2) and a device for calculating the corrosion rate CR.
[0280] Moreover, each component of each device shown in the figure is a functional concept, and does not necessarily have to be physically configured as shown in the figure. In other words, the specific state of distribution and integration of each device is not limited to that shown in the figure, and all or a part of them can be functionally or physically distributed and integrated in any unit according to various loads, usage conditions, etc. For example, each processing unit of the calculation unit 30a and the output control unit 30b may be appropriately integrated. Furthermore, the processing of each processing unit may be appropriately separated into processing of multiple processing units. Furthermore, each processing function performed by each processing unit may be realized in whole or in any part by a CPU and a program analyzed and executed by the CPU, or may be realized as hardware by wired logic.
[0281] [Corrosion detection program] The various processes described in the above embodiments can also be realized by executing a prepared program on a computer system such as a personal computer or a workstation. Therefore, an example of a computer system that executes a program having the same functions as those in the above embodiments will be described below. Figure 57 is a diagram showing a computer that executes a corrosion detection program.
[0282] 57, a computer 300 includes a central processing unit (CPU) 310, a hard disk drive (HDD) 320, and a random access memory (RAM) 340. Each of these components 300 to 340 is connected via a bus 400.
[0283] A corrosion detection program 320a that performs the same functions as the calculation unit 30a and the output control unit 30b described above is stored in advance in the HDD 320. Note that the corrosion detection program 320a may be separated as appropriate.
[0284] In addition, the HDD 320 stores various types of information, for example, the HDD 320 stores various types of data used for detecting corrosion, such as the measurement data 33 described above.
[0285] The CPU 310 reads out and executes the corrosion detection program 320a from the HDD 320, thereby performing operations similar to those of the respective processing units in the embodiment. That is, the corrosion detection program 320a performs operations similar to those of the calculation unit 30a and the output control unit 30b.
[0286] It should be noted that the above-described corrosion detection program 320a does not necessarily need to be stored in the HDD 320 from the beginning.
[0287] For example, the program may be stored in a "portable physical medium" such as a flexible disk (FD), CD-ROM, DVD disk, magneto-optical disk, or IC card that is inserted into computer 300. Computer 300 may then read and execute the program from these.
[0288] Furthermore, the program may be stored in "another computer (or server)" connected to computer 300 via a public line, the Internet, a LAN, a WAN, etc. Then, computer 300 may read and execute the program from the other computer (or server). [Explanation of symbols]
[0289] 1. Concrete 2 Reinforcement bars 12a-12d code 10 Corrosion detection equipment 20 Power supply section 21 Measurement section 22 Control section 30 Controller 30a Calculation part 30b Output control section 31 User Interface 32 Storage section 33 Measurement data 70 Test specimen 71 Reinforcement Bar 72 Epoxy Resin 73 Hexagon Nut 74 Lead Wire 212 Opposite 214 Reference electrode 300 Computers 310 CPU 320 HDD 320a Corrosion Detection Program 400 Bus C 1、 C2 current terminal P 1、 P2 potential difference measurement terminal
Claims
1. two first electrodes are arranged at a distance from each other on a surface of concrete having reinforcing bars installed inside, two second electrodes are arranged at a distance from each other inside or outside the two first electrodes, respectively, in a straight line with respect to the two first electrodes at the same distance from the first electrodes, and AC power is applied to the two first electrodes at frequencies changed within a predetermined frequency range, and a potential difference between the two second electrodes is measured, and a polarization resistance of the four-electrode arrangement is calculated from the measurement data; Calculate the polarization resistance of the two-electrode arrangement from the polarization resistance of the four-electrode arrangement calculated based on a predetermined measurement area of the reinforcing bar surface and a predetermined conversion coefficient for converting the four-electrode arrangement into a two-electrode arrangement using two of the first electrodes. A corrosion detection program that causes a computer to execute a process.
2. The process of calculating the polarization resistance in the two-electrode arrangement includes multiplying the calculated polarization resistance in the four-electrode arrangement by the measurement area and the conversion coefficient to calculate the polarization resistance in the two-electrode arrangement. The corrosion detection program according to claim 1 .
3. The shorter the distance, the smaller the conversion factor. The corrosion detection program according to claim 1 .
4. constructing an analytical model simulating the concrete, setting an insulating surface in a portion of the analytical model other than the reinforcing bar between the two first electrodes, analyzing a current density on the surface of the reinforcing bar where a current caused by the AC power flows into the reinforcing bar, and causing a computer to execute a process of calculating, as the measured area, an area of the reinforcing bar surface where the current density on the surface of the reinforcing bar is equal to or greater than the current density at a point on the circumference of the reinforcing bar below the first electrodes where the height of the reinforcing bar relative to the direction of the first electrodes is the middle; The process of calculating the polarization resistance of the two-electrode arrangement uses the calculated measurement area to calculate the polarization resistance of the two-electrode arrangement. The corrosion detection program according to claim 1 .
5. Further, by using a first arithmetic formula for calculating the measured area from the diameter of the reinforcing bar and the thickness of the cover of the reinforcing bar, the computer executes a process of calculating the measured area from the diameter of the reinforcing bar and the thickness of the cover of the reinforcing bar in the concrete; The process of calculating the polarization resistance of the two-electrode arrangement uses the calculated measurement area to calculate the polarization resistance of the two-electrode arrangement. The corrosion detection program according to claim 1 .
6. and further causing the computer to execute a process of constructing an analytical model simulating the concrete and calculating the conversion factor according to an arrangement of the two second electrodes relative to the two first electrodes; The process of calculating the polarization resistance of the two-electrode arrangement uses the calculated conversion coefficient to calculate the polarization resistance of the two-electrode arrangement. The corrosion detection program according to claim 1 .
7. The method further includes causing the computer to execute a process of calculating the conversion factor from the distance between the two first electrodes in the concrete by using a second arithmetic expression for calculating the conversion factor from the distance between the two first electrodes; The process of calculating the polarization resistance of the two-electrode arrangement uses the calculated conversion coefficient to calculate the polarization resistance of the two-electrode arrangement. The corrosion detection program according to claim 1 .
8. The computer is further caused to execute a process of calculating a corrosion rate from the polarization resistance of the two-electrode arrangement. The corrosion detection program according to claim 1 .
9. The measurement data includes first measurement data measured by arranging the two first electrodes and the two second electrodes along the reinforcing bar with a distance between the two first electrodes that is 2.4 times or more the thickness of the cover of the reinforcing bar in the concrete, The process of calculating the polarization resistance of the four-electrode arrangement includes determining an AC impedance for each frequency from a potential difference for each frequency indicated by the first measurement data, calculating a high-frequency resistance and a low-frequency resistance from a Nyquist plot showing the AC impedance for each frequency on a complex plane, and calculating the polarization resistance of the four-electrode arrangement from the calculated high-frequency resistance and the low-frequency resistance and a predetermined electrical resistance of the concrete. The corrosion detection program according to claim 1 .
10. The measurement data further includes second measurement data obtained by measuring the two first electrodes and the two second electrodes at a position other than the buried position of the reinforcing bar or by measuring the distance between the two first electrodes as a distance at which no current flows into the reinforcing bar; The process of calculating the polarization resistance of the four-electrode arrangement includes calculating an electrical resistance of the concrete from the second measurement data, and calculating the polarization resistance of the four-electrode arrangement from the high-frequency resistance, the low-frequency resistance, and the calculated electrical resistance of the concrete. The corrosion detection program according to claim 9 .
11. two first electrodes are arranged at a distance from each other on a surface of concrete having reinforcing bars installed inside, two second electrodes are arranged at a distance from each other inside or outside the two first electrodes, respectively, in a straight line with respect to the two first electrodes at the same distance from the first electrodes, and AC power is applied to the two first electrodes at frequencies changed within a predetermined frequency range, and a potential difference between the two second electrodes is measured, and a polarization resistance of the four-electrode arrangement is calculated from the measurement data; Calculate the polarization resistance of the two-electrode arrangement from the polarization resistance of the four-electrode arrangement calculated based on a predetermined measurement area of the reinforcing bar surface and a predetermined conversion coefficient for converting the four-electrode arrangement into a two-electrode arrangement using two of the first electrodes. A corrosion detection method, characterized in that the processing is executed by a computer.
12. a storage unit that stores measurement data obtained by arranging two first electrodes at a distance from each other on a surface of concrete having reinforcing bars installed inside, arranging two second electrodes at a distance from each other inside or outside the two first electrodes and linearly connecting the two first electrodes to each other at the same distance from the first electrodes, and applying AC power to the two first electrodes at frequencies changed within a predetermined frequency range to measure a potential difference between the two second electrodes; A calculation unit that calculates a polarization resistance of a four-electrode arrangement from the measurement data stored in the memory unit, and calculates the polarization resistance of the two-electrode arrangement from the calculated polarization resistance of the four-electrode arrangement based on a predetermined measurement area of the reinforcing bar surface and a predetermined conversion coefficient that converts the four-electrode arrangement into a two-electrode arrangement using two of the first electrodes; 13. An information processing device comprising:
13. Two first electrodes are disposed at a distance from each other on a surface of the concrete having reinforcing bars therein; two second electrodes arranged on the inside or outside of the two first electrodes, spaced apart from each other and linearly aligned with the two first electrodes at the same distance from the first electrodes; a power supply unit that applies AC power to the two first electrodes by changing a frequency within a predetermined frequency range; a measurement unit that measures a potential difference between the two second electrodes when AC power is applied from the power supply unit; A calculation unit that calculates a polarization resistance of a four-electrode arrangement from the potential difference measured by the measurement unit, and calculates the polarization resistance of the two-electrode arrangement from the calculated polarization resistance of the four-electrode arrangement based on a predetermined measurement area of the reinforcing bar surface and a predetermined conversion coefficient that converts the four-electrode arrangement into a two-electrode arrangement using two of the first electrodes; A corrosion detection device comprising:
14. The two first electrodes are disposed at an interval of 2.4 times or more the thickness of the cover of the reinforcing bar in the concrete. The corrosion detection device of claim 13 .
15. The two second electrodes are disposed inside the two first electrodes such that a distance between each of the two second electrodes and the first electrodes closest to each other is narrower than a distance between the two second electrodes. The corrosion detection device of claim 13 .
Citation Information
Patent Citations
Corrosion detection device, corrosion detection method, and corrosion detection program
JP2020153782A
Non-destructive corrosion diagnosis system by the estimation of electrical resistivity in concrete structures
KR1020110010853A
Corrosion detection in structural tendons
US20150097589A1
Electrochemical measurement system and method for monitoring a concrete structure
US20220260548A1