Surface protective film
A polyolefin resin-based surface protection film with calcium carbonate particles addresses the issues of chlorine gas generation and burr/whisker formation, providing clean cutting without defects.
Patent Information
- Application Number
- JP2023043658
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Conventional surface protection films generate chlorine gas during disposal and produce burrs or whiskers during cutting, especially when applied to metal plates.
A surface protection film comprising a base layer made of polyolefin resin with calcium carbonate particles of specific size (1 μm to 8 μm) to prevent burr and whisker formation during cutting.
The film prevents chlorine gas generation and eliminates burrs or whiskers during cutting, ensuring clean cuts without surface defects.
Smart Images

Figure 2024132744000001 
Figure 2024132744000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface protection film for cutting processing. [Background technology]
[0002] Conventionally, surface protection films suitable for cutting processes have often been made of a soft polyvinyl chloride substrate with an adhesive layer provided on the back side. Surface protection films using the above-mentioned soft polyvinyl chloride substrate are still in wide use today due to their strength, which makes them relatively resistant to tearing during processing, and the versatility of the substrate. However, there has been a problem with waste disposal because they generate harmful hydrogen chloride when incinerated.
[0003] In contrast, a pressure-sensitive adhesive sheet that is environmentally friendly and has excellent cut processability that does not generate thread-like burrs on the cut surface is known, which comprises a base layer and an adhesive layer laminated on at least one surface thereof, and which has the following characteristics: (a) the longitudinal tensile modulus (MD-M) and transverse tensile modulus (TD-M) at 23°C are in the range of 50 to 2000 MPa, and the ratio of the longitudinal tensile modulus (MD-M) to the transverse tensile modulus (TD-M) {(MD-M) / (TD-M)} is in the range of 0.5 to 2, (b) the longitudinal tear strength (MD-T) and transverse tear strength (TD-T) at 23°C are in the range of 1 to 100 N / mm, and the ratio of the longitudinal tear strength (MD-T) to the transverse tear strength (TD-T) {(MD-T) / (TD-T)} is in the range of 0.5 to 2, and (c) the base layer contains an olefin-based polymer (see Patent Document 1).
[0004] In addition, a surface protection film which, when the adherend is cut while the surface protection film is attached thereto, causes no appearance defects such as stringiness or fuzzing, and causes very little contamination such as adhesive residue on the adherend surface after the film is peeled off, is provided, the surface protection film comprising a base layer mainly composed of an ethylene polymer (A1), 5 to 40 mass% of an amorphous α-olefin polymer (B1), and a density of 0.880 to 0.938 g / cm. 3A surface protection film is known which is characterized by having a co-extruded laminate film laminated with an adhesive layer mainly composed of a mixed resin of 60 to 95 mass % of linear low density polyethylene (B2) (see Patent Document 2).
[0005] Further, as a surface protection film having cut processability such that, when the adherend is cut while the surface protection film is attached thereto, the surface protection film is cut cleanly and does not cause poor appearance such as stringiness or fuzzing, the surface protection film has an adhesive layer (I) and a base layer (II), the adhesive layer (I) comprising a block copolymer (Ia) having a crystalline olefin block and a crystalline olefin block having a density of 0.880 to 0.938 g / cm 3 and a linear low-density polyethylene (Ib) as a main component, and the main component of the base layer (II) is an ethylene polymer (IIa), particularly a linear low-density polyethylene, a medium-density polyethylene, or a mixed resin of low-density polyethylene and high-density polyethylene (see Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-68420 A [Patent Document 2] JP 2009-166277 A [Patent Document 3] JP 2010-36448 A Summary of the Invention [Problem to be solved by the invention]
[0007] The surface protection films described in the prior art described above also had the problem that their processing characteristics were insufficient in terms of preventing the generation of burrs or whiskers when cutting, particularly when shearing, an adherend to which the surface protection film is attached, particularly a metal plate. An object of the present invention is to provide a surface protection film that does not generate chlorine even during cutting processing, and that adheres to an adherend during cutting processing without generating burrs or whiskers. [Means for solving the problem]
[0008] Means for Solving the Problems The inventors of the present invention have conducted intensive research to solve the above problems, and as a result have found that in a surface protection film consisting of a base layer and an adhesive layer, the base layer is a layer whose main component is a polyolefin resin containing a specific amount of calcium carbonate having a specific average particle size, thereby completing the present invention.
[0009] That is, the present invention relates to a surface protection film that is attached to an adherend during cutting processing, the surface protection film comprising a base layer and an adhesive layer laminated on one side of the base layer, the base layer being a resin layer mainly composed of a polyolefin resin, and containing 2 mass % or more of calcium carbonate, relative to the entire base layer, having a volume-based cumulative 50% particle diameter (D50) of 1 μm or more and less than 8 μm, as obtained by a laser diffraction scattering method. The polyolefin resin is preferably a low-density polyethylene. The volume-based cumulative 50% particle size (D50) of the calcium carbonate obtained by a laser diffraction scattering method is preferably in the range of 1 μm or more and less than 6 μm. The calcium carbonate is preferably surface-treated calcium carbonate, and the surface treatment is preferably a lipophilic treatment, and the lipophilic treatment is preferably a fatty acid treatment. The cutting process is preferably a shearing process. Furthermore, the adherend is preferably a metal plate. Effect of the Invention
[0010] By using the surface protection film of the present invention, no chlorine-based toxic gases are generated when an adherend to which the surface protection film of the present invention is affixed is heated and processed or when the surface protection film of the present invention is heat-treated, and there is an effect that no burrs or whiskers are generated on the surface protection film when an adherend to which the surface protection film of the present invention is affixed is cut and processed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The surface protection film of the present invention is a surface protection film comprising a base layer and an adhesive layer laminated on one side of the base layer, the base layer being a resin layer mainly composed of a polyolefin resin, containing 2 mass% or more of calcium carbonate with a volume-based cumulative 50% particle diameter (D50) of 1 μm or more and less than 8 μm, based on the entire base layer, as obtained by a laser diffraction scattering method, and being attached to an adherend when the adherend is cut.
[0012] The substrate layer constituting the surface protective film of the present invention is a resin layer mainly composed of a polyolefin resin. Here, in the present invention, the "main component" means preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more.
[0013] The polyolefin resin used in the present invention is not particularly limited as long as it is a homopolymer or copolymer of an olefin monomer such as ethylene, propylene, or butadiene, or a copolymer of the olefin monomer and an alkene derivative such as vinyl acetate. More specifically, low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, low-crystalline or amorphous ethylene-α-olefin copolymer, polypropylene, propylene-ethylene copolymer (random copolymer and / or block copolymer), propylene-α-olefin copolymer, ethylene-ethyl (meth)acrylate copolymer, ethylene-methyl (meth)acrylate copolymer, ethylene-n-butyl (meth)acrylate copolymer, ethylene-vinyl acetate copolymer, etc. These can be used alone or in combination of two or more.
[0014] The α-olefin is not particularly limited as long as it is copolymerizable with propylene or ethylene, and specific examples thereof include butene-1, hexene-1, 4-methylpentene-1, octene-1, pentene-1, and heptene-1.
[0015] The polyolefin resin is preferably low-density polyethylene. Specific examples of the low-density polyethylene include very low-density polyethylene resin (VLDPE), low-density polyethylene resin (LDPE), linear low-density polyethylene resin (LLDPE), etc. The density of the polyethylene is 0.880 g / cm 3 ~0.940g / cm 3 The range of 0.910 g / cm is preferable. 3 ~0.930g / cm 3 More preferably, the range is 0.915 g / cm 3 ~0.925g / cm 3 The range is more preferred.
[0016] The calcium carbonate used in the present invention is not particularly limited as long as it is a calcium carbonate represented by the composition formula CaCO3, which is a main component of shells, egg shells, limestone, chalk, etc. More specifically, it includes heavy calcium carbonate (natural calcium carbonate) obtained by crushing and classifying limestone, and light calcium carbonate (synthetic calcium carbonate) obtained by chemical reaction with the heavy calcium carbonate. In the present invention, both heavy calcium carbonate and light calcium carbonate can be used, but light calcium carbonate is preferably used in consideration of surface treatment. The calcium carbonate can be any of the crystal polymorphs such as calcite crystals (trigonal rhombohedral crystals), aragonite crystals (rectangular crystals), and vaterite crystals (hexagonal crystals), but among them, aragonite crystals are preferable.
[0017] The calcium carbonate is preferably surface-treated calcium carbonate. Here, surface-treated calcium carbonate refers to calcium carbonate in which the surface of calcium carbonate is covered with a surface treatment agent, or calcium carbonate in which a surface treatment agent is attached to at least the surface of calcium carbonate. Specific examples of surface treatment agents for calcium carbonate include fatty acids and derivatives thereof, resin acids and derivatives thereof, silica, organic silicon compounds, condensed phosphoric acids, and condensed phosphates. Among these, metal salts of fatty acids are preferred, and fatty acid sodium salts or fatty acid potassium salts are particularly preferred. Specific examples of the fatty acids include saturated or unsaturated fatty acids having 6 to 24 carbon atoms, and preferably saturated or unsaturated fatty acids having 10 to 20 carbon atoms. Specific examples of the fatty acid include hexanoic acid (caproic acid), heptanoic acid (enanthic acid), octanoic acid (caprylic acid), nonanoic acid (pelargonic acid), decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), pentadecanoic acid (pentadecylic acid), hexadecanoic acid (palmitic acid), heptadecanoic acid (margaric acid), octadecanoic acid (stearic acid), icosanoic acid (arachidic acid), docosanoic acid (behenic acid), tetracosanoic acid, oleic acid, linoleic acid, linolenic acid, arachidonic acid, eicosapentaenoic acid, docosahexaenoic acid, myristoleic acid, palmitoleic acid, sapienic acid, eicosenoic acid, erucic acid, etc. These fatty acids and their metal salts can be used alone or in combination of two or more.
[0018] The surface-treated calcium carbonate can be produced, for example, by heating the fatty acid in an aqueous alkali metal solution such as an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution to obtain an aqueous fatty acid alkali metal salt solution, then adding the aqueous fatty acid alkali metal salt solution to a slurry of calcium carbonate and water and stirring the mixture, and further dehydrating the obtained calcium carbonate slurry by a method such as a filter press, and drying the slurry using a box dryer or the like.
[0019] The volume-based cumulative 50% particle size (D50) of the calcium carbonate including the surface-treated calcium carbonate obtained by a laser diffraction scattering method is 1 μm or more and less than 8 μm, more preferably 1 μm or more and less than 6 μm. When D50 is less than 1 μm or 8 μm or more, the trouser tear strength in the machine direction increases, the film stretches, and burrs or whiskers are generated in the surface protection film when an adherend to which the surface protection film is attached is cut.
[0020] The contents of the polyolefin-based resin and the calcium carbonate contained in the base layer are preferably in the range of 98 mass% or less of the polyolefin-based resin and 2 mass% or more of the calcium carbonate, more preferably in the range of 98 to 50 mass% of the polyolefin-based resin and 2 to 50 mass% of the calcium carbonate, still more preferably in the range of 98 to 60 mass% of the polyolefin-based resin and 2 to 40 mass% of the calcium carbonate, more preferably in the range of 98 to 70 mass% of the polyolefin-based resin and 2 to 30 mass% of the calcium carbonate, still more preferably in the range of 98 to 80 mass% of the polyolefin-based resin and 2 to 20 mass% of the calcium carbonate, and particularly preferably in the range of 98 to 90 mass% of the polyolefin-based resin and 2 to 10 mass% of the calcium carbonate.
[0021] The base layer may contain additives as necessary. Specific examples of the additives include antioxidants, ultraviolet absorbers, antiaging agents, light stabilizers, antistatic agents, surface lubricants, plasticizers, low molecular weight polymers, corrosion inhibitors, polymerization inhibitors, silane coupling agents, inorganic and organic fillers (e.g., calcium oxide, magnesium oxide, silica, zinc oxide, titanium oxide, etc.), metal powders, colorants, pigments, heat stabilizers, eye plug inhibitors, lubricants, and antiblocking agents.
[0022] The thickness of the base layer is not particularly limited, but is preferably in the range of 2 to 200 μm, more preferably in the range of 10 to 180 μm, more preferably in the range of 50 to 160 μm, more preferably in the range of 60 to 140 μm, and particularly preferably in the range of 80 to 130 μm.
[0023] The pressure-sensitive adhesive layer used in the present invention contains a resin component as a main component, and is optionally composed of a tackifier, a softener, etc. By appropriately adjusting the type and amount of each of these components, the adhesive strength and tensile modulus of the pressure-sensitive adhesive layer can be adjusted.
[0024] Specific examples of the resin component include acrylic resins, styrene resins, silicone resins, polyolefin resins, EVA resins, rubber resins, polyvinyl ether resins, etc. In particular, at least one selected from the group consisting of polyolefin resins, EVA resins, acrylic resins, and rubber resins is preferred, and at least one selected from the group consisting of low-density polyethylene, linear low-density polyethylene, acrylic resins, and rubber resins is preferred. The resin component may be used alone or in combination of two or more.
[0025] Specific examples of the tackifier include known tackifiers such as rosin-based resins, terpene-based resins, aliphatic petroleum-based resins, alicyclic petroleum-based resins, aromatic resins, etc. The tackifiers may be used alone or in combination of two or more.
[0026] The amount of the tackifier is preferably in the range of 1 to 50 parts by mass, more preferably in the range of 1 to 30 parts by mass, and even more preferably in the range of 1 to 20 parts by mass, relative to 100 parts by mass of the resin component.
[0027] Specific examples of the softener include low molecular weight rubber-based materials, procell oil (paraffin-based oil), petroleum-based softeners, and epoxy-based compounds. The softeners may be used alone or in combination of two or more.
[0028] The blending amount of the softener is preferably 1 to 25 parts by mass, more preferably 5 to 25 parts by mass, and further preferably 5 to 15 parts by mass, based on 100 parts by mass of the resin component.
[0029] In addition to the above-mentioned components, the pressure-sensitive adhesive layer may contain additives such as an ultraviolet protection agent, an antioxidant, a filler, and a lubricant, if necessary.
[0030] When preparing the pressure-sensitive adhesive layer, the resin component can be blended with components other than the resin component (hereinafter also referred to as "other components") by mixing the resin component with the other components and extruding the mixture, or by extruding a master batch in which the other components have been kneaded into the resin component in advance.
[0031] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably in the range of 5 to 20 μm, more preferably in the range of 7 to 18 μm, and even more preferably in the range of 9 to 15 μm.
[0032] The method for producing the surface protection film of the present invention is not particularly limited. Specifically, the following methods include a method in which the components constituting the adhesive layer (hereinafter also referred to as "adhesive layer components") are supplied to an extruder for producing an adhesive layer, the components constituting the base layer (hereinafter also referred to as "base layer components") are supplied to an extruder for producing a base layer, and the materials are co-extruded from one die from two extruders to be integrally molded by a two-layer co-extrusion method, a method in which a base layer previously molded by a known inflation method, T-die method, calendar method, etc. is subjected to a surface treatment such as corona treatment, and then an adhesive material is applied and dried, a method in which an adhesive material is applied to a release sheet and dried, and then the adhesive material is pressure-bonded to a previously molded base layer, or a method in which an adhesive layer is melt-extruded and laminated to a previously molded base layer, etc.
[0033] The base layer component may be a mixture of the thermoplastic resin and the additive, or a master batch in which the additive is kneaded in advance into the thermoplastic resin may be supplied to the extruder. The pressure-sensitive adhesive layer component may be a mixture of the resin component and the other component, or a master batch in which the other component is kneaded in advance into the resin component may be supplied to the extruder.
[0034] The thickness of the surface protective film of the present invention is not particularly limited, but is preferably in the range of 60 to 220 μm, more preferably in the range of 70 to 180 μm, and even more preferably in the range of 80 to 140 μm.
[0035] The surface protection film may have a release layer on the surface opposite to the surface on which the pressure-sensitive adhesive layer is provided. The release layer may be made of any material having releasability, such as silicone resin, organic resin-modified silicone resin, fluororesin, aminoalkyd resin, melamine resin, acrylic resin, polyester resin, etc. In addition, a release aid may be added to the pressure-sensitive adhesive layer to improve the release property. Examples of the release aid include silicone-based release aids, paraffin-based release aids, polyethylene wax, and acrylic polymers.
[0036] The surface protective film of the present invention is used by being attached to an adherend during cutting processing of the adherend. The adherend to which the surface protective film is attached is not particularly limited, and specific examples thereof include optical devices (liquid crystal displays, plasma display panels, inorganic EL displays, organic EL displays, cathode ray tube displays, surface electric field displays, electronic paper, etc.), optical films (polarizing plates, circularly polarizing plates, retardation plates, etc.), metal plates, painted metal plates, resin plates, glass plates, wood, etc. Among these, metal plates such as SUS plates and aluminum plates are preferred.
[0037] Specific examples of the cutting process include water jet cutting, which uses the force of cutting water or water mixed with an abrasive to cut the material, electric (plasma) cutting, which uses the heat of an arc (plasma) generated when electricity is discharged to melt and cut the material, and laser cutting, which uses the heat of laser light focused by a lens to melt and cut the material, among which mechanical cutting is preferred, and shearing is more preferred. The shearing process is not particularly limited as long as it is a method of cutting the material by shearing force using a press machine, a shear cutter, or the like, and specific examples include shearing (cutting) processing, punching processing, notching processing, and the like. EXAMPLES
[0038] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.
[0039] (Reference example 1) 80 parts by mass of low-density polyethylene (Novatec LD, LC620, manufactured by Japan Polyethylene Co., Ltd.) and 20 parts by mass of calcium carbonate (PO-320-B-10, manufactured by Shiraishi Calcium Co., Ltd., cumulative 50% particle size (D50): 1.20 μm on a volume basis obtained by a laser diffraction scattering method) were melt-mixed at 190°C to obtain a master batch in which calcium carbonate was dispersed. 12 parts by mass of the obtained master batch and 88 parts by mass of low-density polyethylene were extruded through a T-die at an extrusion temperature of 210°C to a film thickness of 90 μm to produce a film that becomes the base layer of the present invention (hereinafter referred to as "base layer film").
[0040] The obtained film for use as a base layer was evaluated by the following methods, and the results are shown in Table 1.
[0041] (Elongation at break) The breaking elongation was measured according to JIS K7127:1999. The above-mentioned base layer film with a size of 15 mm wide x 75 mm long was used for the measurement. The measurement directions of the sample were MD (the flow direction of the molten resin when the film was formed) and TD (the direction perpendicular to the flow direction of the molten resin when the film was formed). The distance between the chucks was 50 mm. The test speed was 300 mm / min.
[0042] (tear strength) The tear strength was measured according to the trouser method specified in JIS K7128-1:1998. The above-mentioned base layer film with a size of 50 mm wide x 150 mm long was used for the measurement. The measurement directions of the sample were MD and TD. The test speed was 200 mm / min. During the measurement, a case where at least a part of the sample was torn out of the specified cut direction was regarded as "fracture".
[0043] (Reference example 2) A film for a base layer was prepared in the same manner as in Reference Example 1, except that calcium carbonate (PO-220-B-10, manufactured by Shiraishi Calcium Co., Ltd., cumulative 50% particle size (D50): 2.10 μm on a volume basis obtained by a laser diffraction scattering method) was used, and was evaluated in the same manner. The results are shown in Table 1.
[0044] (Reference example 3) A film for a base layer was prepared in the same manner as in Reference Example 1, except that calcium carbonate (PO-150-B-10, manufactured by Shiraishi Calcium Co., Ltd., cumulative 50% particle size (D50): 3.90 μm on a volume basis obtained by a laser diffraction scattering method) was used, and was evaluated in the same manner. The results are shown in Table 1.
[0045] (Reference example 4) A film for a base layer was prepared in the same manner as in Example 1, except that calcium carbonate (PO-120-B-10, manufactured by Shiraishi Calcium Co., Ltd., cumulative 50% particle size (D50): 5.20 μm on a volume basis obtained by a laser diffraction scattering method) was used, and was evaluated in the same manner. The results are shown in Table 1.
[0046] (Comparative Reference Example 1) A film for a base layer was prepared in the same manner as in Reference Example 1, except that calcium carbonate (PO-100-B-10, manufactured by Shiraishi Calcium Co., Ltd., cumulative 50% particle size (D50): 8.00 μm on a volume basis obtained by a laser diffraction scattering method) was used, and was evaluated in the same manner. The results are shown in Table 1.
[0047] (Comparative Reference Example 2) A film for a base layer was produced in the same manner as in Reference Example 3, except that 91 parts by mass of low-density polyethylene and 9 parts by mass of calcium carbonate master batch were used, and was similarly evaluated. The results are shown in Table 1.
[0048] (Comparative Reference Example 3) Except for not using calcium carbonate, a film for a base layer was prepared in the same manner as in Reference Example 1, and was evaluated in the same manner. The results are shown in Table 1.
[0049] [Table 1] EXAMPLES
[0050] As the adhesive layer component, an acrylic adhesive layer composition obtained by mixing an acrylic adhesive and a curing agent was used, and the acrylic adhesive layer composition was applied to the base layer film prepared in Reference Example 1 so that the adhesive layer thickness after drying was 12 μm, and the film was dried at 60 ° C. for 3 minutes using an air bath to obtain a surface protection film with a base layer thickness of 90 μm, an adhesive layer thickness of 12 μm, and a film thickness of 100 μm. The obtained surface protection film was evaluated as follows. The results are shown in Table 2.
[0051] <Evaluation of punchability> The obtained surface protection film was attached to an aluminum plate having a thickness of 0.2 mm and left at room temperature for 24 hours. After that, a hole was punched out using a hole punch (50 mmφ), and the shape of the edge of the punched surface protection film was observed under an optical microscope to obtain an evaluation result. The evaluation results were judged according to the following criteria. ⊚: The shape of the punched edge of the protective film was smooth. ◯: Slight whiskers or the like were observed on the edge of the punched protective film. ×: The occurrence of whiskers or the like was observed on the edge of the punched protective film.
[0052] (Examples 2 to 4, Comparative Examples 1 to 3) Surface protection films of Examples 2 to 4 were produced and evaluated in the same manner as in Example 1, except that the resin compositions for base layer prepared in Reference Examples 2 to 4 were used. The results are shown in Table 2. Moreover, surface protection films of Comparative Examples 1 to 3 were prepared in the same manner as in Example 1, except that the resin compositions for base layer prepared in Reference Comparative Examples 1 to 3 were used, and similar evaluations were performed. The results are shown in Table 2.
[0053] [Table 2]
[0054] From the above, it was found that there is a correlation between the tear strength in the MD direction by the Trouser method and the punching evaluation of the film obtained from the resin composition for the base layer. [Industrial Applicability]
[0055] The surface protective film of the present invention is useful as a surface protective film for adherends such as metals for processing because it does not produce burrs, whiskers, etc. during cutting processing.
Claims
1. A surface protection film that is attached to an adherend during cutting processing, the surface protection film being made of a base layer and an adhesive layer laminated on one side of the base layer, the base layer being a resin layer mainly composed of a polyolefin resin, and containing 2 mass % or more of calcium carbonate, relative to the entire base layer, having a volume-based cumulative 50% particle diameter (D50) of 1 μm or more and less than 8 μm, as obtained by a laser diffraction scattering method.
2. 2. The surface protective film according to claim 1, wherein the polyolefin resin is a low-density polyethylene.
3. 3. The surface protection film according to claim 1, wherein the calcium carbonate has a volume-based cumulative 50% particle size (D50) measured by a laser diffraction scattering method of 1 μm or more and less than 6 μm.
4. 3. The surface protective film according to claim 1, wherein the calcium carbonate is a surface-treated calcium carbonate.
5. 5. The surface protective film according to claim 4, wherein the surface treatment is a lipophilic treatment.
6. 6. The surface protective film according to claim 5, wherein the lipophilic treatment is a fatty acid treatment.
7. 3. The surface protective film according to claim 1, wherein the cutting process is a shearing process.
8. 3. The surface protective film according to claim 1, wherein the adherend is a metal plate.
Citation Information
Patent Citations
Adhesive tape for securing semiconductor wafer
JP1995273173A
Flame retardant resin composition, and heat-resistant coated wire
JP2013053268A
Laminated sheet, manufacturing method of laminated sheet, and molded body
JP2020023055A
Pressure-sensitive adhesive sheet
JP2005068420A
Surface protective film
JP2009166277A