Method for producing biaxially stretched polyvinyl alcohol film and biaxially stretched polyvinyl alcohol film

A biaxially stretched polyvinyl alcohol film, composed of specific polyvinyl alcohol ratios and treated to enhance barrier properties, addresses the need for strong, biodegradable, and recyclable materials, achieving improved gas barrier and environmental performance.

JP2024132798APending Publication Date: 2024-10-01MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023134282
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2023-08-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing polyvinyl alcohol films lack sufficient strength and gas barrier properties, and there is a need for environmentally friendly materials that are biodegradable and recyclable.

Method used

A biaxially stretched polyvinyl alcohol film is produced using a composition of polyvinyl alcohol A with a 1,2-diol structure and polyvinyl alcohol B, with specific mass ratios, followed by biaxial stretching and heat treatment, to enhance gas barrier properties and environmental friendliness.

Benefits of technology

The resulting film exhibits excellent gas barrier properties, biodegradability, and recyclability, with improved tensile strength and reduced oxygen permeability, making it suitable for food packaging and supporting a circular economy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132798000001
    Figure 2024132798000001
  • Figure 2024132798000002
    Figure 2024132798000002
  • Figure 2024132798000003
    Figure 2024132798000003
Patent Text Reader

Abstract

To provide a biaxially stretched polyvinyl alcohol film having gas barrier properties, which is excellent in environmental friendliness such as biodegradability and recycling.SOLUTION: There are provided: a method for producing a biaxially stretched film, which comprises a step 1 of obtaining a film by forming a film from a composition comprising a polyvinyl alcohol A having a 1,2-diol structure and a polyvinyl alcohol B other than the polyvinyl alcohol A in a mass ratio of 5:95 to 45:55 and a step 2 of biaxially stretching the obtained film; and a biaxially stretched film which comprises a polyvinyl alcohol A having a 1,2-diol structure and a polyvinyl alcohol B other than the polyvinyl alcohol A in a mass ratio of 5:95 to 45:55.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl chloride (PVC) film having excellent gas barrier properties and excellent environmental friendliness, such as biodegradability and recyclability. Regarding Nylalcoholic Film. [Background technology]

[0002] In recent years, in the context of the demand for a circular economy, From the perspective of the circular economy, material recycling is also an important issue. For the cycle and organic recycling, it is important to make materials monomaterial and give them biodegradability. It is the essence. For example, Patent Document 1 discloses a composition containing polyvinyl alcohol having a 1,2-diol structure. The composition, gas barrier packaging material using the laminated film, and recyclable film are described. It has been done. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-208347 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the method of Patent Document 1 was insufficient in terms of strength, gas barrier properties, etc. Polyvinyl alcohol with excellent gas barrier properties and environmental friendliness, biodegradability, and recyclability. The purpose of this invention is to provide a film that can be used in various applications. [Means for solving the problem]

[0005] The present invention has the following aspects. <1> Polyvinyl alcohol A having a 1,2-diol structure and the polyvinyl alcohol A composition comprising polyvinyl alcohol B other than polyvinyl alcohol A in a mass ratio of 5:95 to 45:55. A biaxial stretching method comprising the steps of: forming a film by forming a film of the above-mentioned compound; and stretching the film by biaxial stretching. A method for producing stretched film.

[0006] <2> The stretching ratio of the first axis is 2 to 4 times, and the stretching ratio of the second axis is 2.5 to 5 times. <1> A method for producing the biaxially stretched film according to claim 1. <3> After stretching, heat treatment is performed. <1> or <2> The method for producing the biaxially stretched film according to the present invention . <4> The polyvinyl alcohol A is a polyvinyl alcohol having a structural unit represented by the following general formula 1: vinyl alcohol, <1> ~ <3> Manufacture of the biaxially stretched film according to any one of the preceding claims. method.

[0007] [ka]

[0008] (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms group, X represents a single bond or a bond chain, R 4 , R 5 and R 6 are each independently hydrogen atoms It represents an alkyl group having 1 to 3 carbon atoms.

[0009] <5> The degree of saponification of the polyvinyl alcohol B is 90 to 99.99 mol %. <4> 2. A method for producing a biaxially stretched film according to claim 1 , <6> The degree of polymerization of the polyvinyl alcohol B is 500 or more and 2600 or less. <1> ~ <5> 2. A method for producing a biaxially stretched film according to claim 1 , <7> Polyvinyl alcohol A having a 1,2-diol structure and the polyvinyl alcohol A biaxially stretched film containing polyvinyl alcohol B other than polyvinyl alcohol A in a mass ratio of 5:95 to 45:55. Stretched film.

[0010] <8> Oxygen permeability at 23℃ and 0% RH is 0.01cc / (m 2 ·day·atm )~1cc / (m 2 ·day·atm), <7> The biaxially stretched film according to claim 1. <9> The tensile strength in the MD and TD directions is 100MPa to 350MPa. <7> also teeth <8> The biaxially stretched film according to claim 1. <10> The polyvinyl alcohol A is a polyvinyl alcohol having a structural unit represented by the following formula 1: Vinyl alcohol, <7> ~ <9> 2. The biaxially stretched film according to claim 1 .

[0011] [ka]

[0012] (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms group, X represents a single bond or a bond chain, R 4 , R 5 and R 6 are each independently hydrogen atoms It represents an alkyl group having 1 to 3 carbon atoms.

[0013] <11> The degree of saponification of the polyvinyl alcohol B is 90 to 99.99 mol %. <10> 2. The biaxially stretched film according to claim 1 .

[0014] <12> The degree of polymerization of the polyvinyl alcohol B is 2400 or less. <7> <11> The biaxially stretched film according to any one of the above. <13> <7> ~ <12> A food packaging film comprising the biaxially stretched film according to any one of claims 1 to 5. Hmm. Effect of the Invention

[0015] According to the present invention, a gas barrier film having excellent environmental friendliness, such as biodegradability and recyclability, is provided. A polyvinyl alcohol film is obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] <Process 1> In the present invention, polyvinyl alcohol A having a 1,2-diol structure and the polyvinyl Contains polyvinyl alcohol B other than alcohol A in a mass ratio of 5:95 to 45:55 The composition is cast into a film. If the ratio of polyvinyl alcohol A is less than 5, the stretchability is insufficient and biaxial stretching is difficult. If the ratio is more than 45, the glass transition temperature of the film will be lowered and the elastic modulus will be reduced. Therefore, blocking between films and wrapping around rolls can occur during the film production process. Moreover, breakage occurs during stretching. The polyvinyl alcohol A is a polyvinyl alcohol containing a structural unit represented by the following formula 1: Alcohol is preferred.

[0017] [ka]

[0018] In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms group, X represents a single bond or a bond chain, R 4 , R 5 and R 6 are each independently hydrogen atoms It represents a carbon atom or an alkyl group having 1 to 3 carbon atoms.

[0019] In terms of thermal stability and stability under high temperature and acidic conditions, X is most preferably a single bond. The linking chain may be any linking chain as long as it does not impair the effects of the present invention. , alkylene, alkenylene, phenylene, naphthylene, etc. (these hydrocarbons In addition to -O-, -(C H2O) m -, -(OCH2) m -, -(CH2O) m CH2-, -CO-, -COCO -, -CO(CH2) m CO-, -CO(C6H4)CO-, -S-, -CS-, -SO -, -SO2-, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS- , -NRNR-, -HPO4-, -Si(OR)2-, -OSi(OR)2-, -OSi (OR)2O-, -Ti(OR)2-, -OTi(OR)2-, -OTi(OR)2O- , -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, etc. (R is independently is an arbitrary substituent, preferably a hydrogen atom or an alkyl group, and m is a natural number. ) can be mentioned.

[0020] Among these, alkylene groups having 6 or less carbon atoms, especially methyl groups, are preferred from the viewpoint of stability during production and use. The group -CH2OCH2- is preferred. In addition, R in the 1,2-diol structural unit represented by formula 1 1 ~R 3 and R 4 ~R 6 Gasu The most preferred is a structural unit represented by the following formula 2, in which X is a hydrogen atom and X is a single bond: More preferred is polyvinyl alcohol having the formula:

[0021] [ka]

[0022] The content of the 1,2-diol structural unit in the polyvinyl alcohol A is 1 to 1 It is preferably 5 mol %, more preferably 2 to 10 mol %, and even more preferably 3 to 9 mol %. If the content is too low, it is likely to break during the stretching process, and if it is too high, it may cause a strong bond with the metal. This adhesion tends to reduce flowability during melt molding and peelability from the roll. The polyvinyl alcohol A can be produced by a known method, and is not particularly limited. A copolymer of a vinyl ester monomer and a compound represented by the following general formula (2) is saponified. (ii) a method for producing a vinyl ester monomer and a compound represented by the following general formula (3): (iii) a method for saponifying and decarboxylating a polymer and a method for reacting a vinyl ester monomer with the following general monomers: A method of saponifying and deketalizing a copolymer with the compound represented by formula (4) is preferably used. I can.

[0023] The polyvinyl alcohol B is a polyvinyl alcohol having no 1,2-diol structure. It's a call. Since most of the vinyl polymer side chains are occupied by hydroxyl groups, there are high hydrogen bonds between the molecular chains. Because of the effect of bonding, the interaction between molecular chains is large, and the mobility of the molecules is suppressed or filtered. The reduction in the free volume in the film reduces the permeability of gases including oxygen, providing high barrier properties. In addition, PVA is biodegradable and can be decomposed by PVA-decomposing bacteria present in soil. Disassembly is possible.

[0024] The saponification degree of the polyvinyl alcohol B is preferably 90 to 99.99 mol %, and more preferably 95 to 99.99 mol %. It is more preferably 99.99 mol %, and even more preferably 98 to 99.9 mol %. The degree of saponification of the polyvinyl alcohol B is preferably 95 mol % or more from the viewpoint of gas barrier properties. It is preferable that the content is 98 mol % or more. From the viewpoint of moldability, it is preferable that the content is 99.99 mol % or less. The degree of saponification is preferably 99.9 mol % or less, and more preferably 99.9 mol % or less. It can be measured in accordance with.

[0025] The average polymerization degree of the polyvinyl alcohol B is preferably 500 or more and 2600 or less. More preferably, the average polymerization degree is 1000 or more and 2000 or less. If the average polymerization degree is too high, the melt viscosity becomes low. If the viscosity is too low, the film tends to become brittle. The average degree of polymerization is measured in accordance with JIS K 6726. This can be done.

[0026] The polyvinyl alcohol is not particularly limited and can be produced by a known method. A vinyl ester polymer obtained by polymerizing a vinyl ester compound and then saponifying the vinyl ester polymer. That is why. Examples of the vinyl ester compounds include vinyl formate, vinyl acetate, and vinyl trifluoroacetate. Vinyl, Vinyl Propionate, Vinyl Butyrate, Vinyl Caprate, Vinyl Laurate, Versa Vinyl tetate, vinyl palmitate, vinyl stearate, etc. are used alone or in combination. However, vinyl acetate is preferred for practical purposes.

[0027] The composition of the present invention is a composition comprising the polyvinyl alcohol A and the polyvinyl alcohol other than the polyvinyl alcohol B. The composition may contain other components such as polymers, additives, etc. The amount is preferably 5% by mass or less. Other ingredients include heat stabilizers, antioxidants, antistatic agents, colorants, UV absorbers, and lubricants. agents, plasticizers, light stabilizers, surfactants, antibacterial agents, drying agents, antiblocking agents, flame retardants, Crosslinking agents, hardeners, foaming agents, crystal nucleating agents, anti-fogging agents, biodegradable additives, silane coupling agents, Examples of the additive include known additives such as oxygen absorbents, etc. Two or more of these may be used.

[0028] The composition can be formed into a film by a known method. For example, Examples of the method include a method of extruding the mixture using a kneading die and a solvent casting method. In the extrusion film formation, the extrusion temperature is about 100°C in view of the viscosity of the composition, and the unmelted material is kneaded. It is preferable that the water content is 45% by weight or more in order to prevent generation of defects. In order to provide strength, it is preferable that the content be 55% by weight or less.

[0029] The L / D of the twin screw extruder is preferably 25 or more to mix without unmelted material, and 40 or more is preferable. In order to prevent excessive evaporation of water, it is more preferable that the molecular weight is 100 or less, and more preferably 80 or less. is more preferred. In the solvent casting method, the solution concentration is preferably 2% by mass or more to prevent drying of only the surface. It is preferable that the content is 4 mass % or more, and more preferable that the content is 4 mass % or more. The content is preferably 10% by mass or less, and more preferably 7% by mass or less.

[0030] In addition, the film obtained in step 1 contains water in an amount of 10% by weight or more in terms of the biaxial stretchability of the film. It is preferable that the content of the polyvinyl chloride is 40% by weight or less in view of barrier properties, strength and stretchability. is preferred. The amount of water contained in the film can be adjusted by the composition, preheating temperature, roll speed, thickness, etc. The water content of the film can be confirmed by dry weight method, infrared spectroscopy, etc. Cut.

[0031] <Process 2> The film obtained in the above step 1 is subjected to biaxial stretching. Biaxial stretching may be performed by a known method such as simultaneous biaxial stretching or sequential biaxial stretching. In view of orientation anisotropy, simultaneous biaxial stretching is preferred. When performing biaxial stretching by the sequential biaxial stretching method, the stretching ratio of the first axis is 2 to 4 times, and the stretching ratio of the second axis is 1 to 2 times. The elongation ratio is preferably 2.5 to 5 times.

[0032] In the present invention, polyvinyl alcohol A having a 1,2-diol structure and the polyvinyl The polyvinyl alcohol B is other than polyvinyl alcohol A, and the polyvinyl alcohol B is contained in a mass ratio of 5:95 to 45:55. By doing so, biaxial stretching becomes possible. In addition, by subjecting the obtained film to heat treatment after stretching, the physical properties can be maintained in a high humidity atmosphere. The heat treatment is preferably performed by heating the stretched film in an oven or by The temperature conditions are preferably 150° C. or higher and 200° C. or lower. If the temperature is lower than 150°C, the barrier properties and strength are likely to be insufficient, and if the temperature is higher than 200°C, This can cause thermal decomposition, making the material more susceptible to problems such as a decrease in strength and discoloration.

[0033] <Biaxially stretched film> The biaxially stretched film of the present invention is made of polyvinyl alcohol A having a 1,2-diol structure. and polyvinyl alcohol B other than the polyvinyl alcohol A, in a ratio of 5:95 to 45:55 Contains in mass proportions of: If the ratio of polyvinyl alcohol A is less than 5, the stretchability is insufficient and biaxial stretching is difficult. If the ratio is more than 45, the glass transition temperature of the film will be lowered and the elastic modulus will be reduced. Therefore, blocking between films and wrapping around rolls can occur during the film production process. Moreover, breakage occurs during stretching. The polyvinyl alcohol A is a polyvinyl alcohol containing a structural unit represented by the following formula 1: Alcohol is preferred.

[0034] [ka]

[0035] In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms group, X represents a single bond or a bond chain, R 4 , R 5 and R 6 are each independently hydrogen atoms It represents a carbon atom or an alkyl group having 1 to 3 carbon atoms.

[0036] In terms of thermal stability and stability under high temperature and acidic conditions, X is most preferably a single bond. The linking chain may be any linking chain as long as it does not impair the effects of the present invention. , alkylene, alkenylene, phenylene, naphthylene, etc. (these hydrocarbons In addition to -O-, -(C H2O) m -, -(OCH2) m -, -(CH2O) m CH2-, -CO-, -COCO -, -CO(CH2) m CO-, -CO(C6H4)CO-, -S-, -CS-, -SO -, -SO2-, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS- , -NRNR-, -HPO4-, -Si(OR)2-, -OSi(OR)2-, -OSi (OR)2O-, -Ti(OR)2-, -OTi(OR)2-, -OTi(OR)2O- , -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, etc. (R is independently is an arbitrary substituent, preferably a hydrogen atom or an alkyl group, and m is a natural number. ) can be mentioned.

[0037] Among these, alkylene groups having 6 or less carbon atoms, especially methyl groups, are preferred from the viewpoint of stability during production and use. The group -CH2OCH2- is preferred. In addition, R in the 1,2-diol structural unit represented by formula 1 1 ~R 3 and R 4 ~R 6 Gasu The most preferred is a structural unit represented by the following formula 2, in which X is a hydrogen atom and X is a single bond: More preferred is polyvinyl alcohol having the formula:

[0038] [ka]

[0039] The content of the 1,2-diol structural unit in the polyvinyl alcohol A is 1 to 1 It is preferably 5 mol %, more preferably 2 to 10 mol %, and even more preferably 3 to 9 mol %. If the content is too low, it is likely to break during the stretching process, and if it is too high, it may cause a strong bond with the metal. This adhesion tends to reduce flowability during melt molding and peelability from the roll. The polyvinyl alcohol A can be produced by a known method, and is not particularly limited. A copolymer of a vinyl ester monomer and a compound represented by the following general formula (2) is saponified. (ii) a method for producing a vinyl ester monomer and a compound represented by the following general formula (3): (iii) a method for saponifying and decarboxylating a polymer and a method for reacting a vinyl ester monomer with the following general monomers: A method of saponifying and deketalizing a copolymer with the compound represented by formula (4) is preferably used. I can.

[0040] The polyvinyl alcohol B is a polyvinyl alcohol having no 1,2-diol structure. Since most of the vinyl polymer side chains are occupied by hydroxyl groups, Since the molecular chains are strongly hydrogen bonded to each other, the molecular chains have strong interactions with each other, suppressing the mobility of the molecules. Alternatively, the free volume in the film can be reduced, lowering the permeability of gases such as oxygen, It can exhibit high barrier properties. In addition, PVA is biodegradable and the PVA molecules present in soil It can be decomposed by lysis.

[0041] The saponification degree of the polyvinyl alcohol B is preferably 90 to 99.99 mol %, and more preferably 95 to 99.99 mol %. It is more preferably 99.99 mol %, and even more preferably 98 to 99.9 mol %. The degree of saponification of the polyvinyl alcohol B is preferably 95 mol % or more from the viewpoint of gas barrier properties. It is preferable that the content is 98 mol % or more. From the viewpoint of moldability, it is preferable that the content is 99.99 mol % or less. The degree of saponification is preferably 99.9 mol % or less, and more preferably 99.9 mol % or less. It can be measured in accordance with.

[0042] The average polymerization degree of the polyvinyl alcohol B is preferably 500 or more and 2600 or less. More preferably, it is 1,000 or more and 2,000 or less. If the average degree of polymerization is too high, the melt viscosity and solubility in water decrease, making extrusion difficult. If it is too low, the film tends to become brittle. It can be measured in accordance with K 6726.

[0043] The polyvinyl alcohol is not particularly limited and can be produced by a known method. A vinyl ester polymer obtained by polymerizing a vinyl ester compound and then saponifying the vinyl ester polymer. That is why. Examples of the vinyl ester compounds include vinyl formate, vinyl acetate, and vinyl trifluoroacetate. Vinyl, Vinyl Propionate, Vinyl Butyrate, Vinyl Caprate, Vinyl Laurate, Versa Vinyl tetate, vinyl palmitate, vinyl stearate, etc. are used alone or in combination. However, vinyl acetate is preferred for practical purposes.

[0044] The biaxially stretched film of the present invention is a film obtained by mixing the polyvinyl alcohol A and the polyvinyl alcohol B. The composition may contain other components such as polymers other than polymer B, additives, etc. The content of the component is preferably 5% by mass or less. Other ingredients include heat stabilizers, antioxidants, antistatic agents, colorants, UV absorbers, and lubricants. agents, plasticizers, light stabilizers, surfactants, antibacterial agents, drying agents, antiblocking agents, flame retardants, Crosslinking agents, hardeners, foaming agents, crystal nucleating agents, anti-fogging agents, biodegradable additives, silane coupling agents, Examples of the additive include known additives such as oxygen absorbents, etc. Two or more of these may be used.

[0045] In addition, the tensile strength in the MD direction of the biaxially stretched film of the present invention is 100 MPa or more, and 350 M The pressure is preferably 150 MPa or more and more preferably 300 MPa or less. Since it is necessary to have a strength capable of withstanding a high load, a value of 100 MPa or more is preferable, and a certain degree of elongation is required. Since a strain is necessary, the strain is preferably 350 MPa or less. The tensile strength in the TD direction is preferably 100 MPa or more and 350 MPa or less, and more preferably 150 MPa or less. It is more preferable that the strength is greater than or equal to a and less than or equal to 300 MPa. From a certain point of view, 100 MPa or more is preferable, and from a certain degree of elongation, 350 MPa is preferable. A or less is preferable.

[0046] The oxygen permeability of the biaxially stretched film of the present invention at 23°C and 0% RH is When used as a barrier film, such as a 2 ·day·atm) or less is preferred 0.5cc / (m 2 The oxygen permeability is preferably less than 100%. From the viewpoint of barrier, it is preferable that the barrier is as low as possible, but it is also necessary to provide sufficient biaxial stretchability of the film. To guarantee, 0.01cc / (m 2 ·day·atm) or more is preferable, and 0.1cc / (m 2 ·day·atm) or higher is preferable.

[0047] The biaxially stretched film of the present invention is made of polyvinyl alcohol A having a 1,2-diol structure. and polyvinyl alcohol B other than the polyvinyl alcohol A, in a ratio of 5:95 to 45:55 The composition containing the above in a mass ratio is formed into a film by a known method, and the film is then biaxially stretched. It can be obtained by: The film-forming method is, for example, a method of kneading with a twin-screw extruder and extruding the mixture using a die, a method of solvent casting, Examples include the Toray method. Biaxial stretching may be performed by a known method such as simultaneous biaxial stretching or sequential biaxial stretching. In view of orientation anisotropy, simultaneous biaxial stretching is preferred.

[0048] <Application> The biaxially stretched film of the present invention can be used as a food packaging film or various other packaging films. In order to reduce dross, films with high aroma retention and oxygen barrier properties are effective in suppressing flavor deterioration and It is effective in extending the expiration date of food. It is also a mono-material that exhibits high barrier properties and biodegradability. Therefore, it is expected that it will be applied to various packaging materials from the viewpoints of recycling and circular economy. It's promising. EXAMPLES

[0049] Next, the present invention will be described in more detail with reference to examples. The present invention was evaluated by the following methods. This was done by.

[0050] <Tensile strength, tensile elongation> The stretched film is cut into a size of 80 mm in length and 15 mm in width, and then measured according to JIS K7127 The test was performed using the Shimadzu Autograph AG-Xplus (manufactured by Shimadzu Corporation) in accordance with the The film was stretched uniaxially at a tensile speed of 100 mm / min and an ambient temperature of 23°C. The tensile strength and tensile elongation in the first and second stretching directions were measured, and the average of three measurements was calculated. did.

[0051] <Oxygen permeability> Based on JIS K7126-2:2006, Modern Control's OXY-TR Using an AN100 oxygen permeability measuring device, biaxial testing was performed under an atmosphere of 23°C and 0% RH. The oxygen permeability of the stretched film was measured.

[0052] Example 1 Degree of saponification: 99.7 mol%, degree of polymerization: 1200, 1,2-diol structure as 1,2-butanol Polyvinyl alcohol containing 6 mol% of phenyldiol (OKS-1009, Mitsubishi Chemical) (Polyvinyl alcohol A) and a saponification degree of 99.5 mol% and a polymerization degree of 1200 Completely saponified polyvinyl alcohol (GOHSENOL NM-11Q, manufactured by Mitsubishi Chemical Corporation) (Polyvinyl alcohol B) was mixed in a mass ratio of 10:90, and 50% by weight of water was added. The mixture is melted and kneaded in a twin-screw extruder under the following conditions while adding the ingredients, and then extruded into a film from a 250 mm wide single layer nozzle. The film thickness was approximately 200 μm.

[0053] Twin Screw Extruder ·Diameter (D): 15mm L / D:60 Screw speed: 200 rpm Mesh: 90 / 90mesh Extrusion temperature: 100℃ The obtained film was roll-stretched 3 times in the MD direction at 70°C, and then stretched in the TD direction at 80°C. The film was stretched 3 times in the tenter in the opposite direction. The obtained biaxially stretched film was heat-treated at 180° C. for 5 minutes. . The evaluation results of the obtained film are shown in Table 1.

[0054] Example 2 In Example 1, the film was stretched in the MD direction in the same manner as in Example 1, except that the stretch ratio in the MD direction was 2 times. The evaluation results of the obtained film are shown in Table 1.

[0055] Example 3 The same procedure as in Example 1 was carried out except that the mixing ratio of A and B was 20:80. A film was obtained. The evaluation results of the obtained film are shown in Table 1.

[0056] Comparative Example 1 The same procedure as in Example 1 was repeated except that only polyvinyl alcohol B was used. The film was then biaxially stretched. Breakage was likely to occur during the second stretching stage, and the film could not be obtained continuously. It was.

[0057] Comparative Example 2 Degree of saponification: 99.7 mol%, degree of polymerization: 1200, 1,2-diol structure as 1,2-butanol Polyvinyl alcohol containing 6 mol% of phenyldiol (OKS-1009, Mitsubishi Chemical) (Polyvinyl alcohol A) and a saponification degree of 99.5 mol% and a polymerization degree of 1200 Completely saponified polyvinyl alcohol (GOHSENOL NM-11Q, manufactured by Mitsubishi Chemical Corporation) (Polyvinyl alcohol B) was mixed in a mass ratio of 50:50 to prepare an aqueous solution.

[0058] The base film is made of polyethylene terephthalate film, and the silicone rubber is applied to the 10cm square. Separate the two, and pour 30 g of the prepared solution into a 10 cm square frame. The mixture was allowed to stand at room temperature for 4 days to allow the water to evaporate uniformly, thereby producing a film. Using a four-axis fixed stretching device, the free-standing film was left at 70°C for 30 seconds, and then The film was then subjected to sequential biaxial stretching at a speed of 10 mm / s, with the first axis stretching at 2 times the original length and the second axis stretching at 3 times the original length. The film broke during the first stretching stage, and no film was obtained.

[0059] [Table 1]

Claims

1. Polyvinyl alcohol A having a 1,2-diol structure and the polyvinyl alcohol A A composition containing polyvinyl alcohol B other than the above in a mass ratio of 5:95 to 45:55 is formed into a film. A biaxially stretched film comprising: a step 1 of obtaining a stretched film; and a step 2 of biaxially stretching the obtained film. How rum is manufactured.

2. The stretching ratio of the first axis is 2 to 4 times, and the stretching ratio of the second axis is 2.5 to 5 times. A method for producing the biaxially stretched film described above.

3. The method for producing a biaxially stretched film according to claim 1 or 2, further comprising the step of: subjecting the film to a heat treatment after the stretching.

4. The polyvinyl alcohol A contains a structural unit represented by the following general formula 1:

3. The method for producing a biaxially stretched film according to claim 1 or 2, wherein the alcohol is alcohol. 【Chemistry 1】 (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms group, X represents a single bond or a bond chain, R 4 , R 5 and R 6 are each independently hydrogen atoms It represents an alkyl group having 1 to 3 carbon atoms.

5. 2. The method according to claim 1, wherein the degree of saponification of the polyvinyl alcohol B is 90 to 99.99 mol %. A method for producing the biaxially stretched film according to claim 2.

6. 2. The method according to claim 1, wherein the degree of polymerization of the polyvinyl alcohol B is 500 or more and 2600 or less. A method for producing the biaxially stretched film according to claim 2.

7. Polyvinyl alcohol A having a 1,2-diol structure and the polyvinyl alcohol A A biaxially stretched film containing polyvinyl alcohol B other than the above in a mass ratio of 5:95 to 45:

55. Room.

8. Oxygen permeability at 23°C and 0% RH is 0.01 cc / (m 2 ・day・atm)~1 cc / (m 2 8. The biaxially stretched film according to claim 7, wherein the elongation constant is 1 / day·atm.

9. The tensile strength in the MD direction and the TD direction is 100 MPa to 350 MPa. The biaxially stretched film according to claim 8.

10. The polyvinyl alcohol A contains a structural unit represented by the following formula 1: The biaxially stretched film according to claim 7 or claim 8, which is an alcohol. 【Chemistry 2】 (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms group, X represents a single bond or a bond chain, R 4 , R 5 and R 6 are each independently hydrogen atoms It represents an alkyl group having 1 to 3 carbon atoms.

11. 8. The method according to claim 7, wherein the degree of saponification of the polyvinyl alcohol B is 90 to 99.99 mol %. The biaxially stretched film according to claim 8.

12. The polymerization degree of the polyvinyl alcohol B is 2400 or less. The biaxially stretched film described above.

13. A food packaging film comprising the biaxially stretched film according to claim 7 or 8.

Citation Information

Patent Citations

  • Polyvinyl alcohol resin composition and film