P-type impurity diffusion composition or n-type impurity diffusion composition, and manufacturing method of solar cell using the same
The impurity diffusion composition with Group 13/15 elements, (meth)acrylic acid polymer surfactant, and optional polysiloxane and polyvinyl alcohol, addresses the issue of residues in solar cells, enhancing carrier life and uniformity.
Patent Information
- Application Number
- JP2024006487
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-14
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-01
AI Technical Summary
Conventional impurity diffusion compositions used in solar cell production form residues composed of carbon components due to bubble traces when applied by screen printing, leading to reduced carrier life of solar cells.
A p-type or n-type impurity diffusion composition containing a compound with Group 13 or Group 15 elements, a surfactant with a polymer of (meth)acrylic acid compound, and optionally including polysiloxane, hydroxyl group-containing polymers like polyvinyl alcohol, and a filler, to suppress bubble formation and residues.
The composition effectively reduces residues in the impurity diffusion layer, improving carrier life and uniformity of solar cells.
Smart Images

Figure 2024132877000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a p-type impurity diffusion composition or an n-type impurity diffusion composition, and a method for producing a solar cell using the same. [Background technology]
[0002] In the manufacture of solar cells, a method of forming an impurity diffusion layer by applying a composition (impurity diffusion composition) containing a p-type or n-type impurity diffusion component onto a substrate and diffusing the impurity by heat has been studied. As impurity diffusion compositions suitable for such a method, for example, a dopant diffusion coating liquid (see Patent Document 1, for example) characterized by containing a binder containing a (meth)acrylic resin and a polyvinyl alcohol resin, a dopant, and a solvent, an impurity diffusion composition containing a polysiloxane and an impurity diffusion component, the polysiloxane containing at least one of a carboxyl group and a dicarboxylic anhydride structure (see Patent Document 2, for example), a p-type impurity diffusion composition containing at least one resin selected from polyvinyl alcohol and polyethylene oxide, a solvent, and a compound containing a Group 13 element, the pH of the composition being 4 to 6.5, the solvent containing an organic solvent having a boiling point of 110°C or more and 210°C or less and water, and the amount of water being 10 to 50 mass% of the solvent (see Patent Document 3, for example), and the like have been proposed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-134558 A [Patent Document 2] International Publication No. 2018 / 21121 [Patent Document 3] International Publication No. 2020 / 116270 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to form the impurity diffusion layer uniformly, it is preferable to apply the impurity diffusion composition by a screen printing method. However, when a conventionally known impurity diffusion composition is applied by a screen printing method, bubbles trapped when passing through a mask mesh cause bubbles to become residues mainly composed of carbon components in the impurity diffusion layer, which causes a problem of reducing the carrier life of the solar cell.
[0005] The present invention has been made based on the above-mentioned circumstances, and aims to provide a p-type impurity diffusion composition or an n-type impurity diffusion composition that can suppress residues in an impurity diffusion layer and improve the carrier lifetime of a solar cell. [Means for solving the problem]
[0006] In order to solve the above problems, the present invention mainly has the following configuration. <1> A p-type impurity diffusion composition or an n-type impurity diffusion composition containing (A) a compound containing a Group 13 element or a Group 15 element, and (C) a surfactant, wherein the surfactant (C) contains a polymer of a (meth)acrylic acid compound. <2> (A) Compounds containing Group 13 elements or Group 15 elements include compounds containing Group 13 elements <1> The p-type impurity diffusion composition according to claim 1. <3> Further, (B) a hydroxyl group-containing polymer is included. <2> The p-type impurity diffusion composition according to claim 1. <4> (B) The hydroxyl-containing polymer includes polyvinyl alcohol. <3> The p-type impurity diffusion composition according to claim 1. <5> The degree of saponification of the polyvinyl alcohol is 20 mol % or more and 70 mol % or less. <4> The p-type impurity diffusion composition according to claim 1. <6> The polymer of the (meth)acrylic acid compound contains 50 mol % or more of a structural unit represented by the following general formula (1): <1> ~ <5> 2. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1 .
[0007] [ka]
[0008] (In the above general formula (1), A is an ether group or NR 3 R 1 R represents a monovalent organic group having 4 to 8 carbon atoms. 2 R represents a hydrogen atom or a methyl group. 3 represents hydrogen or a monovalent organic group having 1 to 3 carbon atoms. <7> R in the general formula (1) 1 is a monovalent aliphatic hydrocarbon group having 4 to 8 carbon atoms <6> The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1. <8> R in the general formula (1) 1 is an n-butyl group <7> The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1. <9> Further containing polysiloxane <1> ~ <8> 2. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1 . <10> Also contains 1,3-propanediol <1> ~ <9> 2. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1 . <11> Also contains fillers <1> ~ <10> 2. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1 . <12> A method for manufacturing a solar cell, comprising the step of forming an impurity diffusion layer having two or more different levels of impurity concentration, the step of forming the impurity diffusion layer having at least one level of impurity concentration comprising: <1> ~ <11> A step of applying the p-type impurity diffusion composition or the n-type impurity diffusion composition described in any one of the above onto a semiconductor substrate to partially form an impurity diffusion composition film (a); a step of heating the obtained impurity diffusion composition film (a) to diffuse the impurities into the semiconductor substrate to form an impurity diffusion layer (b); A method for manufacturing a solar cell comprising the steps of: <13> The above <1> ~ <11> The method for applying the p-type impurity diffusion composition or the n-type impurity diffusion composition according to any one of claims 1 to 5 to a semiconductor substrate is a screen printing method. <12> A method for producing a solar cell according to claim 1. <14> The method includes a step of diffusing impurities into a portion where the impurity diffusion composition film (a) is not formed, using the impurity diffusion composition film (a) as a mask. <12> or <13> A method for producing a solar cell according to claim 1. <15> The step of diffusing impurities into the portion where the impurity-diffusing composition film (a) is not formed is a step of heating in an atmosphere containing an impurity-diffusing component. <14> A method for producing a solar cell according to claim 1. Effect of the Invention
[0009] The p-type impurity diffusion composition or n-type impurity diffusion composition of the present invention can suppress residues in the impurity diffusion layer and improve the carrier life of the solar cell. [Brief description of the drawings]
[0010] [Figure 1] 1A to 1C are cross-sectional views showing steps in an example of a method for producing a solar cell of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, preferred embodiments of the p-type impurity diffusion composition or n-type impurity diffusion composition according to the present invention and the method for manufacturing a solar cell using the same will be described in detail with reference to the drawings as necessary. Note that the present invention is not limited to these embodiments.
[0012] The p-type impurity diffusion composition or n-type impurity diffusion composition (hereinafter, sometimes collectively referred to as "impurity diffusion composition") of the present invention contains (A) a compound containing a Group 13 element or a Group 15 element, and (C) a surfactant. (A) The compound containing a Group 13 element or the compound containing a Group 15 element is a component for forming an impurity diffusion layer, and the compound containing a Group 13 element is used for the p-type impurity diffusion composition, and the compound containing a Group 15 element is used for the n-type impurity diffusion composition. (C) The surfactant has an effect of suppressing uneven application of the impurity diffusion composition, but many of them tend to foam easily. As described above, when the impurity diffusion composition is applied by the screen printing method, bubbles trapped when passing through the mesh of the mask cause bubble marks in the impurity diffusion layer to become residues mainly composed of carbon components, which reduces the carrier life of the solar cell. According to the study by the present inventors, it was found that the bubble marks in the impurity diffusion layer are caused by the generated bubbles being stabilized by the influence of (A) the compound containing a Group 13 element or a Group 15 element, making it difficult to escape from the impurity diffusion layer. Therefore, the present invention is characterized in that, from the viewpoint of suppressing bubble entrapment and promoting bubble removal, a polymer of a (meth)acrylic acid compound is selected as the (C) surfactant. By selecting a polymer of a (meth)acrylic acid compound, it is possible to suppress the above-mentioned stabilization of bubbles, suppress bubble entrapment during printing and promote bubble removal after printing, and suppress residues mainly composed of carbon components in the impurity diffusion layer, thereby improving the carrier life of the solar cell.
[0013] ((A) Compounds containing Group 13 or Group 15 elements) Examples of compounds containing a Group 13 element include boron compounds, aluminum compounds, and gallium compounds. Two or more of these may be included. Among these, boron compounds are preferred from the viewpoint of ease of carrier generation.
[0014] Examples of boron compounds include boric acid, diboron trioxide, methylboronic acid, phenylboronic acid, trimethyl borate, triethyl borate, tripropyl borate, tributyl borate, trioctyl borate, triphenyl borate, etc. Two or more of these may be included. Among these, boric acid and diboron trioxide are preferred from the viewpoint of doping properties.
[0015] Examples of compounds containing a Group 15 element include phosphorus compounds, arsenic compounds, and antimony compounds. Two or more of these may be included. Among these, phosphorus compounds are preferred from the viewpoint of ease of carrier generation.
[0016] Examples of phosphorus compounds include phosphorus pentoxide, phosphoric acid, polyphosphoric acid, methyl phosphate, dimethyl phosphate, trimethyl phosphate, ethyl phosphate, diethyl phosphate, triethyl phosphate, propyl phosphate, dipropyl phosphate, tripropyl phosphate, butyl phosphate, dibutyl phosphate, tributyl phosphate, phenyl phosphate, diphenyl phosphate, and triphenyl phosphate, and phosphorus esters such as methyl phosphite, dimethyl phosphite, trimethyl phosphite, ethyl phosphite, diethyl phosphite, triethyl phosphite, propyl phosphite, dipropyl phosphite, tripropyl phosphite, butyl phosphite, dibutyl phosphite, tributyl phosphite, phenyl phosphite, diphenyl phosphite, and triphenyl phosphite. Two or more of these may be included. Among these, phosphoric acid, diphosphorus pentoxide, and polyphosphoric acid are preferred from the viewpoint of doping properties.
[0017] From the viewpoint of further improving the carrier lifetime, it is preferable that the (A) compound containing an element of Group 13 or Group 15 contains a compound containing an element of Group 13. In this case, the impurity diffusion composition becomes a p-type impurity diffusion composition.
[0018] The content of the compound (A) containing a Group 13 element or a Group 15 element in the impurity-diffusing composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, from the viewpoint of reducing the resistance value of the semiconductor substrate. On the other hand, the content of the compound (A) containing a Group 13 element or a Group 15 element in the impurity-diffusing composition is preferably 20% by mass or less, more preferably 10% by mass or less, from the viewpoint of further improving the carrier life of the solar cell. The content of the compound (A) containing a Group 13 element is further preferably 5% by mass or less.
[0019] ((B) Hydroxyl group-containing polymer) When the impurity diffusion composition of the present invention is a p-type impurity diffusion composition containing (A) a compound containing a Group 13 element, it is preferable that the composition further contains (B) a hydroxyl group-containing polymer. (B) The hydroxyl group-containing polymer forms a complex with (A) the compound containing a Group 13 element to stabilize the compound, thereby forming a uniform impurity diffusion layer, and in the manufacturing method of a solar cell described later, has the effect of suppressing precipitation of (A) the compound containing a Group 13 element during the formation of a p-type impurity diffusion composition film, thereby further suppressing residues in the impurity diffusion layer.
[0020] Examples of the (B) hydroxyl group-containing polymer include polyvinyl alcohol, polyvinyl alcohol resins such as modified polyvinyl alcohol, vinyl alcohol derivatives such as polyvinyl acetal and polyvinyl butyral, polyalkylene oxides such as polyethylene oxide and polypropylene oxide, hydroxyethyl cellulose, polyhydroxymethyl acrylate, polyhydroxyethyl acrylate, polyhydroxypropyl acrylate, and other polyhydroxyacrylic acrylates. Two or more of these may be included. Among these, polyvinyl alcohol is preferred from the viewpoints of the formation of a complex with the (A) compound containing a Group 13 element, particularly preferably a boron compound, the stability of the formed complex, and the storage stability of the p-type impurity diffusion composition.
[0021] The saponification degree of polyvinyl alcohol is preferably 20 mol% or more and 70 mol% or less. By making the saponification degree 20 mol% or more, the stability of the complex with the compound containing the group 13 element (A) can be improved, the resistance value can be further reduced, and the uniformity of the resistance value can be improved. In addition, the carrier life of the solar cell can be further improved. From the viewpoint of improving the storage stability of the p-type impurity diffusion composition, it is more preferable that it is 30 mol% or more. On the other hand, by making the saponification degree 70 mol% or less, the solubility in an organic solvent can be increased, and the stability of the complex with the compound containing the group 13 element (A) can be improved. In addition, the blurring of the pattern during screen printing can be suppressed, and the continuous printability and the uniformity of the printed film thickness can be improved. In addition, the storage stability of the p-type impurity diffusion composition can be improved.
[0022] Here, the degree of saponification of polyvinyl alcohol can be measured by the back titration method described in JIS K 6726 (1994). When two or more types of polyvinyl alcohol are contained, the degree of saponification means the overall degree of saponification of the two or more types of polyvinyl alcohol.
[0023] The average degree of polymerization of polyvinyl alcohol is preferably 150 or more from the viewpoint of further improving the stability of the complex with the (A) compound containing a Group 13 element, and is preferably 1,000 or less from the viewpoint of improving the solubility.
[0024] Here, the average degree of polymerization of polyvinyl alcohol can be measured in accordance with JIS K 6726 (1994). When two or more types of polyvinyl alcohol are contained, the average degree of polymerization means the average degree of polymerization of the two or more types of polyvinyl alcohol as a whole.
[0025] The content of the hydroxyl group-containing polymer (B) in the p-type impurity diffusion composition is preferably 1% by mass or more, more preferably 5% by mass or more, from the viewpoint of further improving the stability of the complex with the compound containing an element of Group 13 (A). On the other hand, the content of the hydroxyl group-containing polymer (B) in the p-type impurity diffusion composition is preferably 20% by mass or less, more preferably 15% by mass or less, from the viewpoint of further suppressing residues in the impurity diffusion layer.
[0026] From the viewpoint of improving the diffusion uniformity, the mass ratio ((B) / (A)) of the content of the hydroxyl group-containing polymer (B) to the content of the compound (A) containing a Group 13 element is preferably at least 1, and more preferably at least 3. On the other hand, from the viewpoint of improving the storage stability, the mass ratio ((B) / (A)) is preferably at most 20, and more preferably at most 15.
[0027] ((C) Surfactant) The impurity-diffusing composition of the present invention contains a surfactant (C), and the surfactant (C) contains a polymer of a (meth)acrylic acid compound. The composition may further contain another surfactant together with the polymer of (meth)acrylic acid.
[0028] The polymer of the (meth)acrylic acid compound preferably contains 50 mol % or more of the structural unit represented by the following general formula (1), which can further suppress bubble entrapment and residue in the impurity diffusion layer.
[0029] [ka]
[0030] In the above general formula (1), A is an ether group or NR 3 represents a group, R 3 represents hydrogen or a monovalent organic group having 1 to 3 carbon atoms. Among these, an ether group is preferred from the viewpoint of compatibility with other components in the impurity-diffusing composition. As the monovalent organic group, a monovalent aliphatic hydrocarbon group is preferred, and an alkyl group is more preferred. These may have a substituent, and examples of the substituent include a hydroxyl group.
[0031] In the above general formula (1), R 1 R represents a monovalent organic group having 4 to 8 carbon atoms. Examples of the monovalent organic group include a monovalent aliphatic hydrocarbon group and a monovalent aromatic hydrocarbon group. Among these, a monovalent aliphatic hydrocarbon group is preferred. 1By selecting a monovalent aliphatic hydrocarbon group as R, the impurity diffusion composition film can be smoothed and bubble inclusion and residue in the impurity diffusion layer can be further suppressed. These may have a substituent, and examples of the substituent include a hydroxyl group and an amino group. 1 is preferably a monovalent saturated aliphatic hydrocarbon group having 4 to 8 carbon atoms, more preferably an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an iso-butyl group, a sec-butyl group, or a tert-butyl group, and further preferably an n-butyl group.
[0032] R 2 represents hydrogen or a methyl group.
[0033] The content of the (meth)acrylic acid compound polymer in the impurity-diffusing composition of the present invention is preferably 0.0001% by mass or more, more preferably 0.1% by mass or more, from the viewpoint of further suppressing residues. On the other hand, the content of the (meth)acrylic acid compound polymer is preferably 10% by mass or less, more preferably 1% by mass or less, from the viewpoint of further suppressing residues in the impurity-diffusing layer.
[0034] (Polysiloxane) From the viewpoints of diffusion stability when the impurity-diffusing composition is applied to a semiconductor substrate and heated to diffuse impurities into the semiconductor substrate, and of reducing the intrusion of substances from the outside, such as in the heating environment (hereinafter sometimes referred to as "barrier properties"), it is preferable that the impurity-diffusing composition of the present invention further contains a polysiloxane.
[0035] The polysiloxane is preferably a polysiloxane obtained by condensation polymerization of organosilane, and more preferably a polysiloxane represented by the following general formula (2): Such a polysiloxane may be either a block copolymer or a random copolymer.
[0036] [ka]
[0037] In the above general formula (2), R4 represents an aryl group having 6 to 15 carbon atoms, and n R 4 may be the same or different.
[0038] R 5 represents a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyloxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms, and n R 5 may be the same or different. 6 and R 7 each independently represents a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyloxy group having 1 to 6 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms; m R 6 and R 7 may be the same or different, except that R 5 ~R 7 The hydroxyl group, alkoxy group having 1 to 6 carbon atoms, and acyloxy group having 1 to 6 carbon atoms in 5 ~R 7 may form a crosslinked structure by condensation with any one of a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, or an acyloxy group having 1 to 6 carbon atoms in the above.
[0039] X represents a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyloxy group having 1 to 6 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms; and Y represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an acyl group having 1 to 6 carbon atoms.
[0040] n and m represent the constituent ratio (%) of the component in each bracket in the general formula (2) and are in the range of 1 to 99, provided that n+m=100. n:m is preferably 95:5 to 25:75.
[0041] By setting n to 25 or more, that is, by including 25 mol % or more of units containing aryl groups having 6 to 15 carbon atoms in the polysiloxane in terms of silicon atoms, the crosslinking density between the polysiloxane skeletons is not too high, and cracks are suppressed even in a thick film. This makes it difficult for cracks to occur during the firing and thermal diffusion steps, improving the barrier properties and improving the stability of impurity diffusion. n is more preferably 35 or more, and even more preferably 40 or more.
[0042] On the other hand, when n is 95 or less, that is, when the unit containing an aryl group having 6 to 15 carbon atoms in the polysiloxane is 95 mol % or less in terms of Si atoms, the residue can be further suppressed.
[0043] When the constituent unit of the polysiloxane represented by the general formula (2) has a structure obtained by condensation polymerization of a tetrafunctional or trifunctional organosilane, R 5 ~R 7 The hydroxyl group, alkoxy group having 1 to 6 carbon atoms, and acyloxy group having 1 to 6 carbon atoms in 5 ~R 7 may form a crosslinked structure with any one of the hydroxyl group, the alkoxy group having 1 to 6 carbon atoms, and the acyloxy group having 1 to 6 carbon atoms in the above.
[0044] In order to form a film with higher barrier properties, R 5 and R 7 is preferably a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, or an acyloxy group having 1 to 6 carbon atoms, and R 6 is preferably an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 4 carbon atoms. In other words, it is preferable that all of the constituent units of the polysiloxane have a structure obtained by condensation polymerization of trifunctional organosilanes.
[0045] R in general formula (2) 4 and R 5The aryl group having 6 to 15 carbon atoms in the formula (I) may be either unsubstituted or substituted, and can be selected according to the properties of the composition. Examples of the aryl group having 6 to 15 carbon atoms include a phenyl group, a p-tolyl group, a m-tolyl group, an o-tolyl group, a p-hydroxyphenyl group, a p-styryl group, a p-methoxyphenyl group, and a naphthyl group. Among these, a phenyl group, a p-tolyl group, and a m-tolyl group are preferred.
[0046] R in general formula (2) 5 ~R 7 The alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, the acyloxy group having 1 to 6 carbon atoms, and the alkenyl group having 2 to 10 carbon atoms in the above may be either unsubstituted or substituted, and can be selected depending on the properties of the composition.
[0047] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an n-hexyl group, a trifluoromethyl group, and a 3,3,3-trifluoropropyl group. Examples of the alkyl group having 1 to 6 carbon atoms include those in which the hydrogen bonded to the carbon atom is replaced with an alkoxy group, an epoxy group, an amino group, an isocyanate group, a mercapto group, an acryloxy group, and the like, and examples thereof include a 3-methoxy-n-propyl group, a glycidyl group, a 3-glycidoxypropyl group, a 3-aminopropyl group, and a 3-mercaptopropyl group. Among these, from the viewpoint of further suppressing residues, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, and a t-butyl group having 4 or less carbon atoms are preferred.
[0048] Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, and a t-butoxy group.
[0049] Examples of the acyloxy group having 1 to 6 carbon atoms include an acetoxy group, a propionyloxy group, an acryloyloxy group, and a benzoyloxy group.
[0050] Examples of the alkenyl group having 2 to 10 carbon atoms include a vinyl group, a 1-propenyl group, a 1-butenyl group, a 2-methyl-1-propenyl group, a 1,3-butadienyl group, a 3-methoxy-1-propenyl group, a 3-acryloxypropyl group, and a 3-methacryloxypropyl group. Among these, from the viewpoint of further suppressing residues, a vinyl group having 4 or less carbon atoms, a 1-propenyl group, a 1-butenyl group, a 2-methyl-1-propenyl group, a 1,3-butadienyl group, and a 3-methoxy-1-propenyl group are preferred.
[0051] R in general formula (2) 4 and R 5 Specific preferred examples of organosilanes that are raw materials for units having the formula include phenyltrimethoxysilane, phenyltriethoxysilane, p-hydroxyphenyltrimethoxysilane, p-tolyltrimethoxysilane, p-styryltrimethoxysilane, p-methoxyphenyltrimethoxysilane, 1-naphthyltrimethoxysilane, 2-naphthyltrimethoxysilane, 1-naphthyltriethoxysilane, and 2-naphthyltriethoxysilane. Among these, phenyltrimethoxysilane, p-tolyltrimethoxysilane, and p-methoxyphenyltrimethoxysilane are particularly preferred.
[0052] R in general formula (2) 6 and R 7Examples of organosilanes that can be used as raw materials for units having the above formula include tetrafunctional organosilanes such as tetramethoxysilane, tetraethoxysilane, and tetraacetoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltri-n-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, ethyltri-n-butoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-butyltrimethoxysilane, n-butyltriethoxysilane, and glyoxysilane. Examples of the organosilanes include trifunctional organosilanes such as lysidyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, trifluoromethyltrimethoxysilane, trifluoromethyltriethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-mercaptopropyltrimethoxysilane, and bifunctional organosilanes such as dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldiacetoxysilane, and di(n-butyl)dimethoxysilane. Two or more of these may be used. Among these organosilanes, trifunctional organosilanes are preferably used in terms of the denseness, crack resistance, residue, and curing speed of the film.
[0053] The polysiloxane represented by the general formula (2) is preferably R 4 R 5 Si(OR 8 )2 and organosilane represented by R 6 R 7 Si(OR 9 The organosilane represented by the formula R 8 and R 9 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an acyl group having 1 to 6 carbon atoms.
[0054] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an n-hexyl group, etc. Examples of the acyl group having 1 to 6 carbon atoms include an acetyl group, a propionyl group, a benzoyl group, etc.
[0055] The molar ratio of each unit of the polysiloxane represented by the general formula (2) can be adjusted by the type and amount of organosilane used during the hydrolysis and condensation reaction.
[0056] The content of polysiloxane in the impurity-diffusing composition of the present invention is preferably 1% by mass or more, more preferably 5% by mass or more, from the viewpoint of improving the barrier property and the diffusion stability of impurities, while the content of polysiloxane is preferably 25% by mass or less, more preferably 15% by mass or less, from the viewpoint of further suppressing residues.
[0057] The content of the polysiloxane represented by general formula (2) in the impurity-diffusing composition of the present invention is, from the viewpoint of improving the barrier properties and the impurity diffusion stability, preferably 60 mass % or more of the total polysiloxane, more preferably 80 mass % or more, and even more preferably 90 mass % or more.
[0058] The weight average molecular weight (Mw) of the polysiloxane is preferably 1,000 or more, more preferably 2,000 or more, from the viewpoint of suppressing shrinkage of the film during baking and obtaining a denser film, while Mw is preferably less than 50,000, more preferably less than 20,000, from the viewpoint of peelability.
[0059] Here, Mw of polysiloxane refers to the polystyrene equivalent molecular weight measured by gel permeation chromatography (GPC). When two or more types of polysiloxane are contained, Mw refers to the weight average molecular weight of the two or more types of polysiloxane as a whole.
[0060] (solvent) The impurity-diffusing composition of the present invention preferably further contains a solvent. The solvent is liquid at normal pressure and 23° C., and when the impurity-diffusing composition of the present invention contains the hydroxyl group-containing polymer (B), it is preferable that the solvent can dissolve the hydroxyl group-containing polymer (B).
[0061] When the impurity-diffusing composition of the present invention is applied by screen printing or spin-coat printing, the boiling point of the solvent is preferably 100° C. or higher from the viewpoint of improving printability. If the boiling point is 100° C. or higher, for example, when the impurity-diffusing composition is printed by screen printing, the impurity-diffusing composition can be prevented from drying and adhering on the printing plate. The boiling point of the solvent is more preferably 160° C. or higher, and even more preferably 180° C. or higher.
[0062] Examples of solvents with a boiling point of 100° C. or higher include ethyl lactate (boiling point 155° C.), diacetone alcohol (boiling point 169° C.), propylene glycol monomethyl ether acetate (boiling point 145° C.), propylene glycol monomethyl ether (boiling point 120° C.), 3-methoxy-3-methyl-1-butanol (boiling point 174° C.), γ-butyrolactone (boiling point 204° C.), N-methyl-2-pyrrolidone (boiling point 204° C.), N,N-dimethylimidazolidinone (boiling point 226° C.), terpineol (boiling point 219° C.), 1,3-propanediol (214° C.), etc. Two or more of these may be included.
[0063] Among these, it is more preferable to include 1,3-propanediol. By including 1,3-propanediol, the stability of the compound (A) containing a Group 13 element or a Group 15 element in the impurity diffusion composition can be further improved, the uniformity of the resistance value can be improved, and the pattern definition can be improved. In addition, thickening over time and the generation of gel-like foreign matter can be suppressed, the storage stability of the impurity diffusion composition can be improved, and the stability of the resistance value over time can be improved.
[0064] When two or more kinds of solvents are contained, it is preferable that the solvent having a boiling point of 100° C. or higher accounts for 20 mass % or more of the total amount of the solvent.
[0065] The content of the solvent in the impurity-diffusing composition of the present invention is preferably 10 to 90% by mass.
[0066] (Filler) The impurity-diffusing composition of the present invention preferably further contains a filler, which imparts thixotropy to the impurity-diffusing composition and improves the pattern definition when the impurity-diffusing composition is applied by screen printing or the like. Here, imparting thixotropy means increasing the ratio (η1 / η2) of the viscosity at low shear stress (η1) to the viscosity at high shear stress (η2). By increasing the thixotropy, the pattern precision of screen printing can be improved. This is for the following reasons. An impurity-diffusing composition with high thixotropy has low viscosity at high shear stress, so that clogging of the screen is unlikely to occur during screen printing, and has high viscosity at low shear stress, so that bleeding immediately after printing and thickening of the pattern line width are unlikely to occur.
[0067] Examples of the filler include fine particles of cellulose derivatives, sodium alginate, polysaccharides, bentonite, montmorillonite, silicon oxide, colloidal alumina, calcium carbonate, etc. Two or more of these may be included. Among these, fine particles of silicon oxide are preferred from the viewpoints of compatibility with other components in the impurity-diffusing composition and reduction of residues.
[0068] The content of the filler in the impurity-diffusing composition of the present invention is preferably 0.1% by mass or more, more preferably 1% by mass or more, from the viewpoint of imparting sufficient thixotropy to the impurity-diffusing composition, while the content of the filler in the impurity-diffusing composition is preferably 10% by mass or less, more preferably 5% by mass or less, from the viewpoint of improving diffusion uniformity.
[0069] The solid content concentration of the impurity-diffusing composition of the present invention is preferably 1% by mass or more and 90% by mass or less.
[0070] The impurity-diffusing composition of the present invention can be obtained, for example, by mixing and kneading (A) a compound containing a Group 13 or Group 15 element, (C) a surfactant, and if necessary (B) a hydroxyl-containing polymer, a solvent, a filler, and other components. A preferred mixing method is stirring and mixing, and examples of the stirring device include a mechanical stirrer and a planetary stirring and defoaming device. Examples of the kneading device include a planetary mixer, a three-roll mill, a ball mill, and a homogenizer. The time, temperature, and pressure of mixing and kneading can be appropriately set so as to obtain a uniform impurity-diffusing composition.
[0071] Furthermore, the impurity-diffusing composition after mixing and kneading may be filtered through a filter with an opening size of 0.01 μm to 100 μm to remove foreign matter. When the impurity-diffusing composition contains a filler, it is preferable to use a filter with a pore size larger than the particle size of the filler. Examples of the material for the filter include polypropylene (PP), polyethylene (PE), nylon (NY), and polytetrafluoroethylene (PTFE).
[0072] The impurity diffusing composition of the present invention can be used, for example, in photovoltaic elements such as solar cells, and semiconductor devices in which an impurity diffusion region is patterned on a semiconductor surface, such as transistor arrays, diode arrays, photodiode arrays, transducers, etc. Among these, it can be suitably used in solar cells.
[0073] <Solar cell manufacturing method> The method for producing a solar cell of the present invention is a method for producing a solar cell, comprising the steps of forming an impurity diffusion layer having two or more different levels of impurity concentration, The step of forming at least one level of impurity diffusion layer includes a step of applying the p-type impurity diffusion composition or the n-type impurity diffusion composition of the present invention to a semiconductor substrate to partially form an impurity diffusion composition film (a); a step of heating the obtained impurity diffusion composition film (a) to diffuse the impurities into the semiconductor substrate to form an impurity diffusion layer (b); The difference in impurity concentration here is 1×10 17 atoms / cm 3 This means that the difference in sheet resistance of the substrate surface in the portion where the impurity diffusion layer is formed is 10 Ω / □ or more. Hereinafter, this embodiment will be described in detail.
[0074] A cross-sectional view of one example of the steps of the method for producing a solar cell of the present invention is shown in Fig. 1. First, as shown in Fig. 1(i), the impurity diffusing composition of the present invention is partially applied onto a semiconductor substrate 1 to form a pattern 2 of an impurity diffusing composition film (a).
[0075] The semiconductor substrate may have an impurity concentration of, for example, 10 15 ~10 16 atoms / cm 3 Examples of crystalline silicon substrates include n-type single crystal silicon, polycrystalline silicon, crystalline silicon substrates mixed with other elements such as germanium and carbon, and semiconductor substrates other than silicon. Examples of crystalline silicon substrates include p-type single crystal silicon.
[0076] The thickness of the semiconductor substrate is preferably 50 to 300 μm, and the shape is preferably a roughly rectangular shape with an outer shape of 100 to 250 mm on each side. In addition, the surface is preferably etched with a hydrofluoric acid solution or an alkaline solution, etc., so that slice damage and natural oxide films can be removed. In this case, a countless uneven texture shape with a typical width of 40 to 100 μm and a depth of about 3 to 4 μm is formed on the surface of the semiconductor substrate.
[0077] Examples of the method for applying the impurity diffusing composition include spin coating, screen printing, inkjet printing, slit coating, spray coating, letterpress printing, intaglio printing, etc. Among these, screen printing is preferred from the viewpoint of pattern definition.
[0078] After the impurity-diffusing composition is partially applied, it is preferable to dry the semiconductor substrate 1 on which the impurity-diffusing composition is applied, so that the solvent contained in the impurity-diffusing composition can be removed. Examples of drying devices include a hot plate and an oven. The drying temperature is preferably 50 to 300° C., and the drying time is preferably 30 seconds to 30 minutes.
[0079] The thickness of the impurity-diffusing composition film (a) is preferably 100 nm or more from the viewpoint of improving the diffusibility of impurities, and is preferably 7 μm or less from the viewpoint of further suppressing the residue after etching.
[0080] 1(ii), the impurity diffusion composition film (a) is heated to diffuse the impurities into the semiconductor substrate 1 to form an impurity diffusion layer (b). Examples of a method for diffusing the impurities include thermal diffusion methods such as electric heating, infrared heating, laser heating, and microwave heating.
[0081] The heating temperature and heating time can be appropriately selected so as to obtain the desired diffusion characteristics such as impurity concentration and diffusion depth. For example, by heating at 800° C. or higher and 1200° C. or lower for 1 to 120 minutes, the surface impurity concentration is reduced to 10 19 ~10 21 atoms / cm 3 The impurity diffusion layer can be formed.
[0082] Thermal diffusion may be performed in the air, or the amount of oxygen in the atmosphere may be appropriately adjusted using an inert gas such as nitrogen or argon. From the viewpoint of shortening the thermal diffusion time, it is preferable to set the oxygen concentration in the atmosphere to 3% or less. Furthermore, if necessary, the impurity-diffused composition film (a) may be baked at a temperature in the range of 200°C to 850°C before diffusion to decompose and remove organic matter in the film.
[0083] Next, as shown in Fig. 1(iii), using the pattern 2 of the impurity diffusion composition film (a) as a mask, an impurity diffusion layer (c) having a different impurity concentration is formed in the pattern-unformed portion. In this process, a layer (d) containing silicon oxide, such as boron silicate glass when the impurity is p-type, or phosphorus silicate glass when the impurity is n-type, is formed by oxidation of the semiconductor substrate surface in the impurity diffusion composition film (a)-unformed portion.
[0084] Examples of the method for diffusing impurities into the portion where the impurity diffusion composition film (a) is not formed include a method of injecting ions containing an impurity diffusion component into the semiconductor substrate 1 with the pattern 2 of the impurity diffusion composition film (a) and then annealing the semiconductor substrate 1 with the pattern 2 of the impurity diffusion composition film (a) in an atmosphere containing the impurity diffusion component, a method of applying another impurity diffusion composition having a different impurity concentration to the portion where the impurity diffusion composition film (a) is not formed on the semiconductor substrate 1 with the pattern 2 of the impurity diffusion composition film (a), forming an impurity diffusion composition film, and then thermally diffusing the impurities in the same manner as in the formation of the impurity diffusion layer (b), etc. Among these, the step of heating in an atmosphere containing the impurity diffusion component is preferred.
[0085] When heating in an atmosphere containing an impurity diffusing component, for example, boron bromide (BBr3) in the case of p-type, or phosphorus oxychloride (POCl3) in the case of n-type, is bubbled and N2 is introduced to create an atmosphere containing the impurity diffusing component, and the semiconductor substrate 1 with the pattern 2 of the impurity diffusion composition film (a) is heated at 800 to 1000°C to form the impurity diffusion layer (c). By setting the gas pressure and heating conditions, the impurity concentration of the impurity diffusion layer (c) can be set higher or lower than the impurity concentration of the impurity diffusion layer (b).
[0086] In addition, the impurity diffusion layer (b) and the impurity diffusion layer (c) may be formed simultaneously. After forming a pattern of the impurity diffusion composition film (a), the impurity diffusion layer (b) and the impurity diffusion layer (c) can be formed simultaneously by heating the pattern in an atmosphere containing an impurity diffusion component.
[0087] In addition, after forming a pattern of the impurity diffusion composition film (a), it may be placed in a heating furnace and first heated using only an inert gas to form an impurity diffusion layer (b), and then a gas containing an impurity diffusing component may be additionally introduced into the furnace and heated under conditions different from the heating conditions using only an inert gas to form an impurity diffusion layer (c) having an impurity concentration different from that of the impurity diffusion layer (b).
[0088] After forming the impurity diffusion layer with two or more different levels of impurity concentration, it is preferable to remove the pattern 2 of the impurity diffusion composition film (a) and the layer (d) containing silicon oxide formed on the surface as shown in Fig. 1 (iv). As a method for removing the pattern of the impurity diffusion composition film (a) and the layer (d) containing silicon oxide, for example, a known etching method can be mentioned.
[0089] The material used for etching is preferably one containing an etching component, water, or an organic solvent, for example, hydrogen fluoride, ammonium, phosphoric acid, sulfuric acid, or nitric acid.
[0090] The method for manufacturing a solar cell of the present invention may include a back surface formation step. Examples of the method for forming the back surface include the high impurity region formation method described in WO 2018 / 180227.
[0091] In the method for producing a solar cell of the present invention, after the etching step, or after the back surface formation step if any, a passivation film is preferably provided on the front and back surfaces of the semiconductor substrate, which can suppress surface recombination and suppress light reflection. For example, a method for forming a passivation film for a p-type diffusion layer includes the method for forming a passivation layer described in International Publication No. 2018 / 180227.
[0092] Next, if a passivation film is present, a metal paste is preferably printed by screen printing on the passivation film so that it is on the higher concentration impurity diffusion layer of the two levels of impurity diffusion layers, and then dried to form an electrode. The metal paste preferably contains metal particles and glass particles, and may further contain a resin binder and other additives. As the metal particles, particles of Ag, Al, etc. are preferably used.
[0093] Next, the electrode is preferably heat-treated (baked). When heat-treated (baked) for a few seconds to a few minutes at a temperature range of 600°C to 900°C, the anti-reflection film, which is an insulating film, melts on the light-receiving surface side due to the glass particles contained in the metal paste, and the silicon surface also partially melts, and the metal particles (e.g., silver particles) in the metal paste form contact parts with the semiconductor substrate and solidify. This provides electrical continuity between the formed light-receiving surface electrode and the semiconductor substrate. This is called fire-through.
[0094] The light-receiving surface electrode is generally composed of busbar electrodes and finger electrodes intersecting the busbar electrodes. Such light-receiving surface electrodes can be formed by screen printing of the above-mentioned metal paste, plating of the electrode material, vapor deposition of the electrode material by electron beam heating in a high vacuum, or other means. The busbar electrodes and finger electrodes can be formed by known methods.
[0095] The method for manufacturing a solar cell of the present invention is not limited to the above-described embodiment, and various modifications such as design changes may be made based on the knowledge of those skilled in the art, and such modified embodiments are also included in the scope of the present invention. EXAMPLES
[0096] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0097] (1) Evaluation of bubble inclusion in impurity-diffused composite film A semiconductor substrate (silicon wafer) made of n-type single crystal silicon with a side length of 156 mm was prepared, and both surfaces were subjected to alkali etching to remove slice damage and natural oxides. During this process, numerous irregularities (textures) with typical widths of 40 to 100 μm and depths of about 3 to 4 μm were formed on both sides of the semiconductor substrate, and these were used as coating substrates for impurity diffusion compositions 1 to 14.
[0098] A texture was formed on both sides of a semiconductor substrate in the same manner as above, except that p-type single crystal silicon having a side length of 156 mm was used instead of n-type single crystal silicon having a side length of 156 mm. This was used as a substrate for coating with impurity diffusion composition 15.
[0099] A screen printing machine (MT-14064: manufactured by Micro-Tech Co., Ltd.) was used, and a screen mask (manufactured by Nakanuma Art Screen Co., Ltd., SUS400 mesh, line diameter 23 μm) having openings of the same size as the coated substrate was used to screen print the impurity diffusion compositions 1 to 15 obtained in each Example and Comparative Example onto the entire surface of the coated substrate. The coating film surface was visually observed to check for the presence or absence of bubble bite. Then, each substrate was heated in air at 200° C. for 10 minutes to form an impurity diffusion composition film having a thickness of about 1.5 μm. The impurity diffusion composition film surface was visually observed to check for the presence or absence of bubble bite marks. A film in which bubble bite was confirmed in the coating film and the marks remained in the impurity diffusion composition film was rated C, a film in which bubble bite was confirmed in the coating film but the marks did not remain in the impurity diffusion composition film was rated B, and a film in which bubble bite was not confirmed in the coating film was rated A, with B or higher being considered as passing.
[0100] (2) Evaluation of residues in impurity diffusion layers Each substrate having the impurity diffusion composition formed thereon, which was prepared in the above (1) bubble trapping evaluation of the impurity diffusion composition film, was placed in an electric furnace (MT-10×8-A: manufactured by Koyo Thermo Systems Co., Ltd.) and heated in an atmosphere of nitrogen:oxygen = 99:1 (volume ratio) at 950°C for 60 minutes for impurity diffusion compositions 1 to 14 and at 900°C for 60 minutes for impurity diffusion composition 15 to thermally diffuse the impurities, thereby forming an impurity diffusion layer.
[0101] Each substrate after thermal diffusion was immersed in a 5% by weight aqueous solution of hydrofluoric acid at 23°C for 1 minute, and the presence or absence of adhesion (residue) was observed by visual observation of the surface while removing the impurity diffusion composition film. After immersion in the aqueous solution of hydrofluoric acid, the coated substrate was immersed in pure water for cleaning. After immersion in the aqueous solution of hydrofluoric acid for 1 minute, surface adhesions could be visually confirmed, but could be removed by rubbing with a rag after cleaning with pure water. Those whose surface adhesions could not be visually confirmed within 1 minute but more than 30 seconds after immersion in the aqueous solution of hydrofluoric acid were rated as C, those whose surface adhesions could not be visually confirmed within 1 minute after immersion in the aqueous solution of hydrofluoric acid were rated as B, and those whose surface adhesions could not be visually confirmed within 30 seconds after immersion in the aqueous solution of hydrofluoric acid were rated as A ... B or higher.
[0102] (3) Resistance value evaluation The substrate on which the impurity diffusion layer was formed, which was prepared in the above (2) Evaluation of impurity diffusion layer residue, was subjected to p / n judgment using a p / n judgment machine (K-706TS: manufactured by Kyowa Riken Co., Ltd.), and the surface resistance was measured using a four-point probe surface resistance measurement device (RT-70V: manufactured by Napson Co., Ltd.). This measurement was performed on a total of 13 data points at 20 mm intervals vertically and horizontally from the center of the square substrate. The average, maximum, and minimum values were calculated, and the average was taken as the sheet resistance value, and the value (%) of {(maximum value - minimum value) / average value} x 100 was taken as the variation. The sheet resistance value is an index of impurity diffusion, and a smaller value means a larger amount of impurity diffusion. The smaller the variation in the value indicating the uniformity of the resistance value, the better, and a value within 20% above or below the average was considered to be acceptable.
[0103] (4) Pattern definition (minimum pattern) evaluation The impurity diffusion compositions 1 to 15 obtained in each of the Examples and Comparative Examples were screen-printed on the coated substrate prepared in the above (1) bubble trapping evaluation of the impurity diffusion composition film using a screen printer (MT-14064: manufactured by Micro-Tec Co., Ltd.) using a screen mask (manufactured by Nakanuma Art Screen Co., Ltd., SUS400 mesh, line diameter 23 μm) in which one opening with a width of 70 μm and a length of 13.5 cm was formed on the center line of the substrate (parallel to the side of the substrate) and three openings on each side of the substrate at 1 cm intervals in parallel to sandwich the opening, for a total of seven openings, to form seven parallel stripe patterns. After that, the substrate was heated at 200° C. for 10 minutes in air to form a pattern with a thickness of about 1.5 μm.
[0104] The width of the pattern corresponding to the 70 μm wide screen mask opening was measured using a microscope (MX61L: manufactured by Olympus Corporation) to determine the minimum value. The pattern definition was evaluated from the amount of pattern spread relative to the 70 μm mask width.
[0105] (5) Carrier lifetime measurement The substrate on which the impurity diffusion layer was formed as described in (2) above for the evaluation of residues on the impurity diffusion layer was placed in a silicon wafer lifetime measuring device (WCT-120, manufactured by Siston), and the open circuit voltage (Voltage Open Circuit) V OC was measured. V OC The higher the value, the longer the carrier lifetime.
[0106] (6) Evaluation of stability over time Impurity-diffusing compositions 1 to 15 obtained in each of the examples and comparative examples were allowed to stand at 25°C for 14 days, after which the variation in resistance value was calculated in the same manner as in (3) Resistance Value Evaluation above, and a value within 20% above or below the average value was deemed to be acceptable.
[0107] (Synthesis Example 1) <(C) Synthesis of Surfactant A> A 500 ml flask was charged with 3 g of 2,2-azobis(isobutyronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.) and 50 g of propylene glycol monomethyl ether (manufactured by Showa Denko K.K.). Then, 76.9 g of butyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) was charged and stirred at room temperature for a while. The atmosphere in the flask was sufficiently replaced with nitrogen by bubbling, and then stirred at 70°C for 5 hours to obtain a resin solution. The obtained resin solution was dried at 85°C for 5 hours using a vacuum dryer (AVO-450NB: manufactured by AS ONE Corporation), and the resin solution was purified by distillation using a vacuum dryer (AVO-450NB: manufactured by AS ONE Corporation) to obtain a resin solution represented by the general formula (1) in which A is an ether group and R 1 is an n-butyl group, and R 2 Surfactant A, in which the hydrogen atom is contained, was obtained as a viscous liquid.
[0108] (Synthesis Example 2) <(C) Synthesis of Surfactant B> The same procedure as in Synthesis Example 1 was repeated except that 86.5 g of 4-hydroxybutyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of 76.9 g of butyl acrylate, and a compound represented by the formula (1) was prepared. 1 is a 4-hydroxybutyl group, and R 2 Surfactant B, in which the aryl group is hydrogen, was obtained.
[0109] (Synthesis Example 3) <(C) Synthesis of surfactant C> The same procedure as in Synthesis Example 1 was repeated except that 94.7 g of hexyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of 76.9 g of butyl acrylate, and a compound represented by the formula (1) was prepared. 1 is an n-hexyl group, and R 2 The surfactant C was obtained, in which the aryl group was hydrogen.
[0110] (Synthesis Example 4) <Synthesis of Polysiloxane> A 500mL three-neck flask was charged with 164.93g (1.21mol) of methyltrimethoxysilane, 204.07g (1.21mol) of phenyltrimethoxysilane, and 363.03g of GBL, and an aqueous phosphoric acid solution prepared by dissolving 1.215g of phosphoric acid in 130.76g of water was added over 30 minutes while stirring at 40°C. After the dropwise addition, the mixture was stirred at 40°C for 1 hour, then heated to 70°C and stirred for 30 minutes. The oil bath was then heated to 115°C. One hour after the start of the temperature increase, the internal temperature of the solution reached 100°C, and the mixture was heated and stirred for 1 hour (internal temperature: 100-110°C). The resulting solution was cooled in an ice bath to obtain a polysiloxane solution. The solids concentration of the polysiloxane solution was 39.8% by weight.
[0111] Example 1 3.0 g of boric acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), 10.0 g of polyvinyl alcohol having a saponification degree of 80 mol% (manufactured by Nippon Vinyl Acetate & Poval Co., Ltd., average polymerization degree 250) (hereinafter referred to as PVA(80)), 52.0 g of γ-butyrolactone (manufactured by Mitsubishi Chemical Corporation) (hereinafter referred to as GBL), 34.5 g of water, and 0.5 g of surfactant A obtained in Synthesis Example 1 were mixed and thoroughly stirred to obtain a homogeneous mixture, thereby obtaining a p-type impurity diffusion composition 1.
[0112] Example 2 Instead of surfactant A, A in the general formula (1) is an ether group, and R 1 and R 2 A p-type impurity diffusion composition 2 was obtained in the same manner as in Example 1, except that polymethyl methacrylate (manufactured by Sigma-Aldrich Co.) (hereinafter referred to as PMMA) in which both of the groups were methyl groups was used.
[0113] Example 3 A p-type impurity diffusion composition 3 was obtained in the same manner as in Example 1, except that the surfactant B obtained in Synthesis Example 2 was used instead of the surfactant A.
[0114] Example 4 A p-type impurity diffusion composition 4 was obtained in the same manner as in Example 1, except that the surfactant C obtained in Synthesis Example 3 was used instead of the surfactant A.
[0115] Comparative Example 1 A p-type impurity diffusion composition 5 was obtained in the same manner as in Example 1, except that a silicone surfactant ("BYK (registered trademark)" 333, manufactured by BYK-Chemie KK) was used instead of the surfactant A.
[0116] Comparative Example 2 A p-type impurity diffusion composition 6 was obtained in the same manner as in Example 1, except that a fluorine-based surfactant ("Megafac (registered trademark)" F444: manufactured by DIC Corporation) was used instead of the surfactant A.
[0117] Comparative Example 3 A p-type impurity diffusion composition 7 was obtained in the same manner as in Example 1, except that the surfactant A was not used.
[0118] Example 5 A p-type impurity diffusion composition 8 was obtained in the same manner as in Example 1, except that 25.0 g of polyvinyl alcohol having a saponification degree of 10 mol% (manufactured by Japan Vinyl Acetate & Poval Co., Ltd., average polymerization degree 250) (hereinafter referred to as PVA(10)) was used instead of 10.0 g of PVA(80), and 32.0 g of terpineol (manufactured by Tokyo Chemical Industry Co., Ltd.) (hereinafter referred to as TP) and 48.0 g of GBL were used instead of 52.0 g of GBL and 34.5 g of water.
[0119] Example 6 A p-type impurity diffusion composition 9 was obtained in the same manner as in Example 5, except that 13.5 g of polyvinyl alcohol having a saponification degree of 49 mol% (manufactured by Nippon Vinyl Acetate & Poval Co., Ltd., average polymerization degree 800) (hereinafter referred to as PVA (49)) was used instead of 25.0 g of PVA (10).
[0120] Example 7 A p-type impurity diffusion composition 10 was obtained in the same manner as in Example 1, except that 13.5 g of PVA(49) was used instead of 10.0 g of PVA(80), and 48.0 g of TP, 24.0 g of 1,3-propanediol (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) (hereinafter referred to as 1,3-PD), and 8.0 g of water were used instead of 52.0 g of GBL and 34.5 g of water.
[0121] Example 8 The p-type impurity diffusing composition 3 was mixed with 3.9 g of silica fine particles (Aerosil (registered trademark) 200, manufactured by Nippon Aerosil Co., Ltd.) and thoroughly stirred to obtain a homogeneous mixture, thereby obtaining a p-type impurity diffusing composition 11.
[0122] Example 9 A p-type impurity diffusion composition 12 was obtained in the same manner as in Example 8, except that the p-type impurity diffusion composition 4 was used instead of the p-type impurity diffusion composition 3.
[0123] Example 10 The p-type impurity diffusing composition 8 was mixed with 3.9 g of silica fine particles (Aerosil (registered trademark) VPNKC130, manufactured by Nippon Aerosil Co., Ltd.) and thoroughly stirred to obtain a homogeneous mixture, thereby obtaining a p-type impurity diffusing composition 13.
[0124] Example 11 A p-type impurity diffusion composition 14 was obtained in the same manner as in Example 10, except that the p-type impurity diffusion composition 10 was used instead of the p-type impurity diffusion composition 8.
[0125] Example 12 4.39 g of the polysiloxane solution having a solid content concentration of 39.8% by weight obtained in Synthesis Example 4, 1.47 g of phosphoric acid, 12.55 g of GBL, and 0.0925 g of surfactant A were mixed and thoroughly stirred to obtain a homogeneous mixture, thereby obtaining an n-type impurity-diffusing composition 15.
[0126] Evaluations (1) to (6) were carried out on the obtained impurity-diffusing compositions of Examples 1 to 12 and Comparative Examples 1 to 3. Table 1 shows these compositions, and Table 2 shows the evaluation results.
[0127] [Table 1]
[0128] [Table 2] [Explanation of symbols]
[0129] 1. Semiconductor substrate 2. Pattern of impurity diffusion composition film (a) 3 Gas containing impurity diffusion components (b), (c) Impurity diffusion layer (d) Layer containing silicon oxide
Claims
1. A p-type impurity diffusion composition or an n-type impurity diffusion composition containing (A) a compound containing a Group 13 element or a Group 15 element, and (C) a surfactant, wherein the surfactant (C) contains a polymer of a (meth)acrylic acid compound.
2. 2. The p-type impurity diffusion composition according to claim 1, wherein the compound (A) containing a Group 13 element or a Group 15 element includes a compound containing a Group 13 element.
3. The p-type impurity diffusion composition according to claim 2 , further comprising (B) a hydroxyl group-containing polymer.
4. 4. The p-type impurity diffusion composition according to claim 3, wherein the hydroxyl group-containing polymer (B) comprises polyvinyl alcohol.
5. 5. The p-type impurity diffusion composition according to claim 4, wherein the degree of saponification of the polyvinyl alcohol is from 20 mol % to 70 mol %.
6. 4. The p-type impurity diffusing composition or the n-type impurity diffusing composition according to claim 1, wherein the polymer of the (meth)acrylic acid compound contains 50 mol % or more of a structural unit represented by the following general formula (1): 【Chemistry 1】 (In the above general formula (1), A is an ether group or NR 3 R represents a group. 1 R represents a monovalent organic group having 4 to 8 carbon atoms. 2 represents hydrogen or a methyl group. 3 represents hydrogen or a monovalent organic group having 1 to 3 carbon atoms.
7. R in the general formula (1) 1 7. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 6, wherein is a monovalent aliphatic hydrocarbon group having 4 to 8 carbon atoms.
8. R in the general formula (1) 1 The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 7, wherein is an n-butyl group.
9. 4. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to claim 1, further comprising a polysiloxane.
10. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to any one of claims 1 to 3, further comprising 1,3-propanediol.
11. The p-type impurity diffusion composition or the n-type impurity diffusion composition according to any one of claims 1 to 3, further comprising a filler.
12. A method for manufacturing a solar cell, comprising the step of forming an impurity diffusion layer having two or more different levels of impurity concentration, the step of forming the impurity diffusion layer having at least one level of impurity concentration comprising: A step of applying the p-type impurity diffusion composition or the n-type impurity diffusion composition according to any one of claims 1 to 3 to a semiconductor substrate to partially form an impurity diffusion composition film (a); a step of heating the obtained impurity diffusion composition film (a) to diffuse the impurities into the semiconductor substrate to form an impurity diffusion layer (b); A method for manufacturing a solar cell comprising the steps of:
13. The method for producing a solar cell according to claim 12, wherein the method for applying the p-type impurity diffusion composition or the n-type impurity diffusion composition according to any one of claims 1 to 3 to a semiconductor substrate is a screen printing method.
14. The method for producing a solar cell according to claim 12, further comprising a step of diffusing impurities into a portion where the impurity-diffusing composition film (a) is not formed, using the impurity-diffusing composition film (a) as a mask.
15. The method for producing a solar cell according to claim 14, wherein the step of diffusing impurities into the portion where the impurity-diffusing composition film (a) is not formed is a step of heating in an atmosphere containing an impurity-diffusing component.
Citation Information
Patent Citations
Coating liquid for dopant diffusion, and method of manufacturing semiconductor prepared therefrom
JP2016134558A
Impurity diffusion composition and semiconductor element production method using impurity diffusion composition
WO2018021121A1
P-type impurity diffusion composition and production method thereof, manufacturing method of semiconductor element using said diffusion composition, and solar battery
WO2020116270A1