Polybutylene terephthalate and method for producing the same
By controlling terminal groups and impurity levels in the production of PBT, the yellowish tinge is minimized, resulting in a PBT with improved color tone and enhanced applicability in diverse industries.
Patent Information
- Application Number
- JP2024022212
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-02-16
- Publication Date
- 2024-10-01
AI Technical Summary
Existing methods for producing polybutylene terephthalate (PBT) struggle with achieving a desirable color tone, particularly a yellowish tinge, due to impurities such as 4-carboxybenzaldehyde and cyclic acetals, and the purification processes to address this are either ineffective or complex.
The production of PBT involves specific amounts of terminal benzaldehyde groups, terminal methylphenyl groups, butyric acid units, and succinic acid units, using hydrogenated terephthalic acid and 1,4-butanediol with controlled impurity levels, and a refined manufacturing process to achieve a preferable color tone.
The resulting PBT exhibits a less yellowish color tone, suitable for various applications, enhancing its commercial value and usability in electrical, electronic, automotive, and textile products.
Smart Images

Figure 2024132894000001 
Figure 2024132894000002 
Figure 2024132894000003
Abstract
Description
[Technical field]
[0001] The present invention relates to polybutylene terephthalate (hereinafter sometimes abbreviated as "PBT"), and more particularly to PBT having a favorable polymer color tone and a method for producing the same. [Background technology]
[0002] PBT, which uses terephthalic acid (hereinafter sometimes abbreviated as "TPA") as the main dicarboxylic acid component and 1,4-butanediol (hereinafter sometimes abbreviated as "BDO") as the main diol component, has excellent mechanical properties, heat resistance, moldability and recyclability, and has high mechanical strength and excellent chemical resistance, so it is widely used as a material for industrial molded products such as connectors, relays and switches for automobiles and electrical and electronic devices. It is also widely used in films, sheets, fibers (filaments), etc., and as a result, there is a demand for high-quality PBT and a manufacturing method for it.
[0003] PBT manufacturing methods can be broadly divided into ester exchange methods, which use dimethyl terephthalate (hereinafter sometimes abbreviated as "DMT") as the dicarboxylic acid component, and direct polymerization methods, which use terephthalic acid as the raw material. Of these, the transesterification method has the disadvantage that the boiling points of the by-products generated in the reaction, methanol (boiling point 65°C) and tetrahydrofuran (hereinafter sometimes abbreviated as "THF") (boiling point 66°C), are close to each other, making it difficult to separate them by distillation after recovery. On the other hand, the direct polymerization method is attracting attention because it does not generate methanol and has a better raw material consumption rate than the transesterification method. However, in recent years, there has been a demand for technology to improve the color tone, especially the yellowness (b value), of PBT produced by the direct polymerization method in order to use it as molded products for various purposes.
[0004] In order to solve this color tone problem, for example, a method has been proposed in which the polycondensation temperature during the production of PBT is specified (see Patent Document 1).
[0005] The terephthalic acid used in the direct polymerization method contains 4-carboxybenzaldehyde (hereinafter sometimes abbreviated as "4CBA"), which is a by-product in the terephthalic acid manufacturing process, and it is known that this affects the color tone of PBT derived from the direct polymerization method (see Patent Document 2). In Patent Document 2, the use of terephthalic acid with fewer impurities is considered in order to reduce the yellow color of the resin, but the purification process of terephthalic acid becomes complicated and the effect is limited.
[0006] On the other hand, it is also known that the color tone of PBT can be improved by, for example, reducing the content of cyclic acetals, which are impurities, in BDO (see Patent Document 3). However, the effect of improving the color tone was insufficient in either case. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 51-47096 [Patent Document 2] JP 2006-152252 A [Patent Document 3] JP 2015-83657 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide PBT which has a preferable color tone as a resin, specifically, which has little yellowness, and a method for producing the same. [Means for solving the problem]
[0009] As a result of intensive research conducted by the present inventors to solve the above problems, it was discovered that these problems can be effectively solved by using PBT containing specific copolymerization components in specific amounts, and this led to the completion of the present invention. The present invention was completed based on these findings, and the gist of the present invention is as follows.
[0010] [1] Polybutylene terephthalate having a terminal benzaldehyde group concentration of 0.005 to 0.15 equivalents / ton, a terminal methylphenyl group concentration of 0.08 to 1.5 equivalents / ton, and containing, as copolymerization components, 0.001 to 0.220 mol% of butyric acid units and 0.001 to 0.220 mol% of succinic acid units.
[0011] [2] A method for producing polybutylene terephthalate by reacting a dicarboxylic acid component with a diol component, the method comprising using, as the dicarboxylic acid component, terephthalic acid having a 4-carboxybenzaldehyde content of 1 to 200 ppm and a p-toluic acid content of 20 to 300 ppm, and using, as the diol component, 1,4-butanediol containing 50 to 8,000 ppm in total of one or more compounds represented by the following formula (1), formula (2) or formula (3), and containing 5 to 1,000 ppm in total of one or two compounds represented by the following formula (4) or formula (5):
[0012] [ka]
[0013] [3] The method for producing polybutylene terephthalate according to [2], wherein the terephthalic acid is terephthalic acid that has been subjected to a hydrogenation purification process, and the 1,4-butanediol is 1,4-butanediol obtained by hydrogenating succinic acid. Effect of the Invention
[0014] The PBT of the present invention has a preferable resin color tone, specifically, little yellowness, and therefore the PBT of the present invention, a compound containing the PBT of the present invention, and a molded article obtained using the same have a good color tone and high commercial value, and can be preferably used for various applications, such as electric and electronic parts, automobile parts, films, sheets, filaments, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the present invention will be described in detail. However, the description of the constituent elements described below is a representative example of the embodiments of the present invention, and the present invention is not limited to these contents. In the present invention, the "main component" in the dicarboxylic acid component refers to a component contained in an amount of 50 mol% or more in the component. The same applies to the "main component" in the diol component. Also, unless otherwise specified, "ppm" refers to "mass ppm" except for the unit of chemical shift of NMR described later.
[0016] [PBT] <Definition of PBT> In the present invention, PBT refers to a polymer having a structure in which a terephthalic acid component and a 1,4-butanediol (BDO) component are ester-bonded, and 50 mol% or more of the dicarboxylic acid component consists of the terephthalic acid component, and 50 mol% or more of the diol component consists of BDO. The proportion of the terephthalic acid component in the total dicarboxylic acid component is preferably 70 mol% or more, more preferably 80 mol% or more, still more preferably 95 mol% or more, and the proportion of BDO in the total diol component is preferably 70 mol% or more, more preferably 80 mol% or more, still more preferably 95 mol% or more. When the terephthalic acid component or BDO is less than 50 mol%, the crystallization rate of PBT decreases, leading to deterioration of moldability.
[0017] <Dicarboxylic acid> In the present invention, the dicarboxylic acid other than terephthalic acid is not particularly limited, and examples thereof include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid, alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid, and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. These dicarboxylic acid components other than terephthalic acid may be used alone or in combination of two or more.
[0018] <Diol component> In the present invention, the diol component other than BDO is not particularly limited, and examples thereof include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,8-octanediol, and dibutylene glycol; alicyclic diols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,1-cyclohexanedimethylol, and 1,4-cyclohexanedimethylol; and aromatic diols such as xylylene glycol, 4,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone. As for these diol components other than BDO, one type may be used alone, or two or more types may be used in combination.
[0019] <Other monomers> In the present invention, one or more of the following may be used as copolymerization components: hydroxycarboxylic acids such as lactic acid, glycolic acid, m-hydroxybenzoic acid, p-hydroxybenzoic acid, 6-hydroxy-2-naphthalenecarboxylic acid, and p-β-hydroxyethoxybenzoic acid; monofunctional components such as stearyl alcohol, benzyl alcohol, stearic acid, benzoic acid, t-butylbenzoic acid, and benzoylbenzoic acid; and polyfunctional components having three or more functional groups such as tricarballylic acid, trimellitic acid, trimesic acid, pyromellitic acid, gallic acid, trimethylolethane, trimethylolpropane, glycerol, and pentaerythritol.
[0020] <Origin of terminal benzaldehyde group and terminal methylphenyl group> One of the characteristics of the PBT of the present invention is that it contains specific amounts of terminal benzaldehyde groups and terminal methylphenyl groups. The terminal benzaldehyde group of the PBT of the present invention is sometimes referred to as a terminal benzaldehyde group derived from 4-carboxybenzaldehyde (hereinafter sometimes abbreviated as "4CBA") in the PBT raw material, particularly in the raw material terephthalic acid, because of its production method, but is specified by the measurement method described below and is not limited to being derived from 4CBA. Similarly, the terminal methylphenyl group of the PBT of the present invention is sometimes referred to as a terminal methylphenyl group derived from p-toluic acid (hereinafter sometimes abbreviated as "p-TA") in the PBT raw material, particularly in the raw material terephthalic acid, because of its production method, but is specified by the measurement method described below and is not limited to being derived from p-toluic acid.
[0021] <Terminal benzaldehyde group concentration> The PBT of the present invention has a terminal benzaldehyde group concentration whose lower limit is usually 0.005 equivalents / ton, preferably 0.015 equivalents / ton, more preferably 0.025 equivalents / ton, and whose upper limit is usually 0.15 equivalents / ton, preferably 0.10 equivalents / ton, more preferably 0.05 equivalents / ton. If the terminal benzaldehyde group concentration is below the lower limit, not only will the raw material purification cost increase, but the color tone of the PBT will become more bluish, which is not preferable. On the other hand, if the terminal benzaldehyde group concentration is above the upper limit, not only will the color tone of the PBT become more yellowish, but the molecular weight of the PBT will decrease due to the effect of terminal blocking, and the required strength may not be obtained.
[0022] <Terminal methylphenyl group concentration> The PBT of the present invention has a terminal methylphenyl group concentration whose lower limit is usually 0.08 equivalents / ton, preferably 0.1 equivalents / ton, and more preferably 0.25 equivalents / ton. The upper limit is usually 1.5 equivalents / ton, preferably 1.0 equivalents / ton, and more preferably 0.5 equivalents / ton. If the terminal methylphenyl group concentration is below the lower limit, not only will the raw material refining cost increase, but the color tone of the PBT will become more yellowish, which is not preferable. On the other hand, if the terminal methylphenyl group concentration exceeds the upper limit, not only will the color tone of the PBT become more blue, but the molecular weight of the PBT will decrease due to the effect of terminal blocking, and the required strength may not be obtained.
[0023] <Butyric acid unit and succinic acid unit> One of the characteristics of the PBT of the present invention is that it is a PBT containing specific amounts of butyric acid units and succinic acid units. The butyric acid unit of the PBT of the present invention may be referred to as being derived from a compound represented by the following formula (1), formula (2) or formula (3) in the PBT raw material, particularly in the raw material BDO, due to its production method, but is identified by the measurement method described below and is not limited to being derived only from the compound represented by the following formula (1), formula (2) or formula (3) contained in the raw material. Similarly, the succinic acid unit of the PBT of the present invention may be referred to as being derived from a compound represented by the following formula (4) or formula (5) in the PBT raw material, particularly in the raw material BDO, due to its production method, but is identified by the measurement method described below and is not limited to being derived only from the compound represented by the following formula (4) or formula (5) contained in the raw material. Here, the term "unit" refers to a structural unit that is incorporated into PBT as a result of the reaction of the monomer in the reaction step of producing PBT.
[0024] [ka]
[0025] Hereinafter, the compound represented by formula (1) may be referred to as "compound (1)", the compound represented by formula (2) may be referred to as "compound (2)", and the compound represented by formula (3) may be referred to as "compound (3)". Similarly, a compound represented by formula (4) may be referred to as "compound (4)," and a compound represented by formula (5) may be referred to as "compound (5)."
[0026] <Butyric acid unit amount> The PBT of the present invention has a butyric acid unit content of usually 0.001 mol%, preferably 0.007 mol%, more preferably 0.018 mol%, and usually 0.220 mol%, preferably 0.110 mol%, more preferably 0.044 mol% as the lower limit, and the upper limit is usually 0.110 mol%, more preferably 0.044 mol%. If the butyric acid unit content is below the lower limit, not only will the raw material purification cost increase, but the color tone of the PBT will become more yellowish, which is not preferable. On the other hand, if the butyric acid unit content is above the upper limit, the elastic modulus of the resin will decrease, and it may become unsuitable for compound use.
[0027] <Succinic acid unit amount> The PBT of the present invention has a lower limit of succinic acid unit content of usually 0.001 mol%, preferably 0.007 mol%, more preferably 0.018 mol%, and an upper limit of usually 0.220 mol%, preferably 0.110 mol%, more preferably 0.044 mol%. If the succinic acid unit content is below the lower limit, not only will the raw material purification cost increase, but the color tone of the PBT will become more yellowish, which is undesirable. On the other hand, if the succinic acid unit content is above the upper limit, the elastic modulus of the PBT will decrease, and it may become unsuitable for compound use.
[0028] <Terminal carboxyl group concentration> The terminal carboxyl group concentration of the PBT of the present invention is usually 0.1 to 50 equivalents / ton, preferably 1 to 40 equivalents / ton, more preferably 5 to 30 equivalents / ton, further preferably 7 to 25 equivalents / ton, and particularly preferably 10 to 19 equivalents / ton. If the terminal carboxyl group concentration is too high, the hydrolysis resistance may deteriorate. In order to make this value less than 0.1 equivalents / ton, for example, an extremely small production scale must be adopted, which is not realistic.
[0029] [Manufacturing method of PBT] The PBT of the present invention is not particularly limited in terms of the production method, except that it is essential that the PBT contains specific components in specific amounts, and the production method may be either continuous or batchwise. The PBT of the present invention can be produced by a conventional method, for example, through a process in which a dicarboxylic acid component mainly composed of terephthalic acid and a diol component mainly composed of PBT are mixed under stirring in a predetermined ratio to form a raw material slurry, then the raw material slurry is heated under normal or reduced pressure to cause an esterification reaction to form a PBT low polymer (oligomer), and then the resulting oligomer is gradually reduced in pressure and heated to cause a melt polycondensation reaction to obtain PBT.
[0030] <Examples of specific ingredients> Hereinafter, for the sake of convenience, 4CBA will be taken as an example of the origin of the terminal benzaldehyde group, and p-toluic acid will be taken as an example of the origin of the terminal methylphenyl group, and their addition amounts will be expressed as the content relative to terephthalic acid. Similarly, the butyric acid derivative represented by the above formula (1), formula (2) or formula (3) will be taken as an example of the origin of the butyric acid unit, and succinic acid and succinic acid derivatives represented by the above formula (4) or formula (5) will be taken as an example of the origin of the succinic acid unit, and their addition amounts will be expressed as the content relative to BDO.
[0031] <Production Example of Terephthalic Acid> The production method of the raw material terephthalic acid used in the PBT of the present invention is not particularly limited. As the raw material terephthalic acid, terephthalic acid obtained by oxidizing p-xylene in the coexistence of a manganese or cobalt catalyst by a conventional method may be used, or so-called high-purity terephthalic acid obtained by hydrogenation purification of the impurities of the terephthalic acid may be used. However, it is preferable to use high-purity terephthalic acid because the amount of specific components can be adjusted.
[0032] <Production Example of BDO> The production method of the raw material BDO used in the PBT of the present invention is not particularly limited. Examples of the production method of BDO include the generally used Reppe method, allyl alcohol method, butadiene method, and method of hydrogenating succinic acid. Furthermore, these intermediates or BDO itself may be produced by a fermentation method. As the raw material BDO, it is preferable to use BDO obtained by a direct fermentation method or a method of hydrogenating succinic acid obtained by a fermentation method. More preferably, BDO obtained by a method of hydrogenating succinic acid obtained by a fermentation method is used. In addition, in any BDO production method, it is preferable to perform distillation purification and hydrogenation purification as necessary in each step.
[0033] <4-CBA Content in TPA> In the present invention, the 4CBA content in the raw material terephthalic acid usually has a lower limit of 1 ppm, preferably 6 ppm, and an upper limit of usually 1000 ppm, preferably 350 ppm, more preferably 200 ppm, and still more preferably 50 ppm. When the 4CBA content is below the above lower limit, not only does the raw material purification cost increase, but also the color tone of the obtained PBT becomes bluer, which is not preferable. On the other hand, when the 4CBA content exceeds the above upper limit, the yellowness of the obtained PBT deteriorates, which is not preferable.
[0034] <p-Toluic acid content in TPA> In the present invention, the p-toluic acid content in the raw material terephthalic acid usually has a lower limit of 20 ppm, preferably 80 ppm, more preferably 100 ppm, and an upper limit of usually 300 ppm, preferably 200 ppm, more preferably 150 ppm. When the p-toluic acid content is below the above lower limit, not only does the raw material purification cost increase, but also the color tone of the obtained PBT becomes yellower, which is not preferable. On the other hand, when the p-toluic acid content exceeds the above upper limit, the blueness of the obtained PBT may increase, or the molecular weight of PBT may decrease due to the end-capping effect, and the required strength may not be obtained.
[0035] <Content of the compound represented by formula (1), formula (2) or formula (3) in BDO> In order to introduce a butyric acid unit into PBT in the present invention, as an example, BDO containing one or more compounds represented by the following formula (1), formula (2) or formula (3) can be used.
[0036]
Chemical formula
[0037] In the present invention, the total content of one or more of the compounds represented by the above formula (1), formula (2) or formula (3) in the raw material BDO (hereinafter, may be referred to as "total content of compounds (1) to (3)") is usually 50 ppm as its lower limit value, preferably 500 ppm, more preferably 1500 ppm, and usually 8000 ppm as its upper limit value, preferably 5000 ppm, more preferably 2500 ppm. When the total content of compounds (1) to (3) is less than the above lower limit value, the color tone of the obtained PBT becomes more yellowish, which is not preferable. On the other hand, when the total content of compounds (1) to (3) exceeds the above upper limit value, the elastic modulus of the obtained PBT decreases, and it may become unsuitable for compound applications.
[0038] <Content of the compounds represented by formula (4) and formula (5) in BDO> In order to introduce a succinic acid unit into PBT in the present invention, as an example, BDO containing one or two of the compounds represented by the following formula (4) or formula (5) can be used.
[0039] [Chemical formula]
[0040] In the present invention, the total content of one or two of the compounds represented by formula (4) or formula (5) in the raw material BDO (hereinafter, may be referred to as "total content of compounds (4) to (5)") is usually 5 ppm as its lower limit value, preferably 50 ppm, more preferably 150 ppm, and usually 1000 ppm as its upper limit value, preferably 600 ppm, more preferably 300 ppm. When the total content of compounds (4) to (5) is less than the above lower limit value, the color tone of the obtained PBT becomes more yellowish, which is not preferable. On the other hand, when the total content of compounds (4) to (5) exceeds the above upper limit value, the elastic modulus of the obtained PBT decreases, and it may become unsuitable for compound applications.
[0041] [Specific example of the method for producing PBT] As described above, the method for producing the PBT of the present invention is not limited, but one example is a method in which the PBT is produced through the following esterification reaction step and polycondensation reaction step.
[0042] <Esterification reaction process> An example of the process of first esterifying the raw materials terephthalic acid and BDO to produce an oligomer is a method in which an esterification reaction is carried out using a single esterification reaction tank or a multistage reaction apparatus in which a plurality of esterification reaction tanks are connected in series, under normal or reduced pressure with or without the use of a catalyst until the esterification reaction rate (the proportion of carboxyl groups in the raw material dicarboxylic acid component that have reacted with the diol component and been esterified) usually reaches 90% or more, while removing water produced in the reaction and excess diol component from the system, to obtain an oligomer. Usually, the temperature of the esterification reaction is about 210 to 230° C., the pressure is about 10 to 133 kPa, and the residence time in the reaction tank, which corresponds to the reaction time, is about 1 to 4 hours.
[0043] <Polycondensation reaction process> An example of the polycondensation reaction step is a method in which a single melt polycondensation tank or a multistage reaction apparatus in which a plurality of melt polycondensation tanks are connected in series, for example, a first stage reactor of a complete mixing type equipped with an agitator, and second and third stages of horizontal plug-flow type reactors equipped with agitators, is used, in which the diol produced is distilled out of the system while being heated under reduced pressure in the presence of a catalyst.
[0044] Generally, the polycondensation reaction is carried out at a temperature of 210 to 280° C., preferably about 220 to 250° C., under reduced pressure of 27 kPa or less, preferably 13 kPa or less. A single or multiple reaction tank may be used, but in order to suppress coloration and deterioration and to suppress an increase in terminal groups such as vinyl groups, it is preferable to carry out the reaction in at least one reaction tank under high vacuum of generally 1.3 kPa or less, preferably 0.3 kPa or less.
[0045] The PBT obtained by the polycondensation reaction is usually drawn out in the form of a strand or sheet from an outlet provided at the bottom of the polycondensation reaction tank, and then cut with a cutter while or after water cooling into pellets, chips, or other granular bodies (e.g., lengths of about 3 to 10 mm). Alternatively, the molten resin is discharged from the polycondensation reaction tank through a pipe into cold water adjusted to a predetermined temperature, and cut with a cutter to form spheres (diameters of about 2 to 10 mm).
[0046] <Polycondensation catalyst> When the oligomer obtained by the esterification reaction between the diol component and the dicarboxylic acid component is polycondensed, a titanium compound and preferably a compound of a metal of Group 2A of the Periodic Table are usually used as a catalyst. These catalyst components may be used in the esterification reaction and then the polycondensation reaction may be carried out as is, or may not be used in the esterification reaction, or may be used only with the titanium catalyst and the remaining catalyst components added at the polycondensation stage. Furthermore, a part of the catalyst amount finally used may be used in the esterification reaction and then appropriately added as the polycondensation reaction proceeds. In any case, in the present invention, titanium and preferably a metal of Group 2A of the periodic table are inevitably contained in the PBT finally obtained, and the amount thereof will be described later.
[0047] (Example of titanium compound) Specific examples of titanium compounds used as catalysts include inorganic titanium compounds such as titanium oxide and titanium tetrachloride, titanium alcoholates such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate, etc. These may be used alone or in combination of two or more. Of these, tetraalkyl titanates are preferred, and among these, tetrabutyl titanate is preferred.
[0048] (titanium catalyst amount) The content of the titanium catalyst in the PBT of the present invention is preferably 5 to 100 ppm in terms of titanium atom mass ratio to the PBT. This amount is more preferably 10 ppm or more, even more preferably 20 ppm or more, and most preferably 25 ppm or more. This amount is more preferably 90 ppm or less, even more preferably 80 ppm or less, particularly preferably 60 ppm or less, particularly preferably 50 ppm or less, and most preferably 40 ppm or less. If the titanium content is too high, the color tone, hydrolysis resistance, and solution haze deteriorate, and fish eyes increase in the obtained molded product, whereas if the titanium content is too low, polymerization property deteriorates.
[0049] (Example of group 2A metal compounds) Specific examples of the metal compounds of Group 2A of the periodic table used as catalysts include various compounds of beryllium, magnesium, calcium, strontium, and barium, but from the viewpoints of ease of handling and availability, and catalytic effect, magnesium compounds and / or calcium compounds are preferred, and magnesium compounds with excellent catalytic effect are particularly preferred. Specific examples of magnesium compounds include magnesium acetate, magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium alkoxide, magnesium hydrogen phosphate, etc. Specific examples of calcium compounds include calcium acetate, calcium hydroxide, calcium carbonate, calcium oxide, calcium alkoxide, calcium hydrogen phosphate, etc. These metal compounds of Group 2A of the periodic table may be used alone or in combination of two or more. Of these, magnesium acetate is preferred.
[0050] (Group 2A metal catalyst amount) The content of the metal catalyst of Group 2A of the periodic table in the PBT of the present invention is not particularly limited, but is preferably 3 to 150 ppm in terms of the mass ratio of the metal atom of Group 2A of the periodic table to the PBT. This amount is more preferably 5 ppm or more, and even more preferably 10 ppm or more. This amount is more preferably 50 ppm or less, even more preferably 40 ppm or less, particularly preferably 30 ppm or less, and most preferably 15 ppm or less. If the content of the metal of Group 2A of the periodic table is too high, the color tone, hydrolysis resistance, etc. are deteriorated, and if it is too low, the polymerizability is deteriorated. When an acetate of a metal of Group 2A of the Periodic Table is used, since the acetate source enters the reaction system, the amount of the metal of Group 2A of the Periodic Table in the PBT is preferably 15 ppm or less.
[0051] (M / Ti ratio) The molar ratio of titanium atoms to Group 2A metal atoms of the periodic table (metal of Group 2A of the periodic table / titanium) contained in the PBT of the present invention is usually 0.01 to 100, preferably 0.1 to 10, more preferably 0.3 to 3, and further preferably 0.3 to 1.5.
[0052] (Ti analysis method) The content of metals such as titanium atoms in PBT can be measured using methods such as atomic emission, atomic absorption, ICP emission, etc. after recovering the metals in the polymer by methods such as wet ashing.
[0053] (Other catalysts) In producing the PBT of the present invention, in addition to the above-mentioned titanium compound and the compound of a metal of Group 2A of the periodic table, reaction aids such as antimony compounds such as antimony trioxide, germanium compounds such as germanium dioxide and germanium tetroxide, manganese compounds, zinc compounds, zirconium compounds, cobalt compounds, phosphorus compounds such as orthophosphoric acid, phosphorous acid, hypophosphorous acid, polyphosphoric acid, esters or metal salts thereof, sodium hydroxide, sodium benzoate, etc. may be used.
[0054] [Intrinsic viscosity of PBT] When the PBT of the present invention is used for compounding or injection molding, the intrinsic viscosity of the PBT is preferably 0.6 to 1.3 dL / g. If the intrinsic viscosity is less than 0.6 dL / g, the mechanical strength of the molded product becomes insufficient, and if it exceeds 1.3 dL / g, the melt viscosity becomes high, the fluidity deteriorates, and the moldability tends to deteriorate. The intrinsic viscosity of the PBT of the present invention is more preferably 0.65 to 1.26 dL / g, and even more preferably 0.7 to 1.2 dL / g.
[0055] In addition, when the PBT pellet of the present invention is used for extrusion of a film, a sheet or a filament, the intrinsic viscosity of PBT is usually 1.00 to 1.60 dL / g, preferably 1.03 to 1.50 dL / g, more preferably 1.05 to 1.55 dL / g, particularly preferably 1.10 to 1.50 dL / g, and particularly preferably 1.15 to 1.35 dL / g. When the intrinsic viscosity is less than 1.00 dL / g, the extrusion moldability is deteriorated, which leads to drawdown of the resin and molding loss, and the mechanical strength of the extrusion molded product such as a film becomes insufficient, or the melt viscosity is lowered and the fluidity is too high, resulting in deterioration of the extrusion moldability. On the other hand, when the intrinsic viscosity exceeds 1.60 dL / g, the melt viscosity becomes high, the fluidity is deteriorated, and the extrusion moldability tends to be deteriorated.
[0056] [Compound] The PBT of the present invention can be made into a compound product by adding various additives or compounding materials as required during or after the PBT production stage. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples in any way as long as the gist of the present invention is not exceeded. The methods for measuring the physical properties and evaluation items used in the following examples are as follows.
[0058] (1) Intrinsic viscosity (IV) The viscosity was calculated using an Ubbelohde viscometer as follows: A mixed solvent of phenol / tetrachloroethane (mass ratio 1 / 1) was used, and the number of seconds it took for a polymer solution with a concentration of 1.0 g / dL and the solvent alone to fall at 30° C. was measured, and the viscosity was calculated using the following formula. IV=((1+4K H η sp ) 0.5 -1) / (2K H C) (However, η sp = η 0 -1, η is the time it takes for the polymer solution to fall, η 0 is the number of seconds the solvent falls, C is the polymer solution concentration (g / dL), and K H is Huggins' constant, which we used as 0.33.)
[0059] (2) Terminal benzaldehyde group concentration, terminal methylphenyl group concentration PBT was dissolved in a mixed solvent of deuterated chloroform / deuterated hexafluoroisopropanol / deuterated pyridine (volume ratio 21 / 9 / 1) containing a trace amount of tetramethylsilane, and the measurement was performed using an AVANCE NEO spectrometer (manufactured by Bruker). 1 H NMR spectrum was measured. The chemical shift reference was set to 0.00 ppm with respect to the signal of tetramethylsilane. In the obtained spectrum, the integral value of the signal of the proton of the phenyl group of the terephthalic acid unit (δ: 8.11 ppm) was used as the reference, and the equivalent weight of each functional group contained in 1 ton of PBT was calculated using the integral value of the signal of the proton assigned to each functional group in Table 1 shown below. In addition, "x" in each structural formula in Table 1 indicates the proton that was used as the reference when calculating the concentration.
[0060] (3) Butyric acid unit content, succinic acid unit content PBT was dissolved in a mixed solvent of deuterated chloroform / deuterated hexafluoroisopropanol / deuterated pyridine (volume ratio 21 / 9 / 1) containing a trace amount of tetramethylsilane, and the measurement was performed using an AVANCE NEO spectrometer (manufactured by Bruker). 1H NMR spectrum was measured. The chemical shift reference was set to 0.00 ppm with respect to the signal of tetramethylsilane. In the obtained spectrum, the integral value of the signal of the proton of the phenyl group of the terephthalic acid unit (δ: 8.11 ppm) was used as the reference, and the ratio R(-) of the number of moles of each unit / the number of moles of the terephthalic acid unit was calculated using the integral value of the signal of the proton assigned to each functional group in Table 1 shown later, and then the content of each unit was calculated by the following formula. Content of each unit = R×100
[0061] (4) Terminal carboxyl group concentration The content was determined by dissolving 0.5 g of PBT or oligomer in 25 mL of benzyl alcohol and titrating with a 0.01 mol / L solution of sodium hydroxide in benzyl alcohol.
[0062] (5) Color tone The evaluation was done using a Nippon Denshoku color difference meter "Z-300A" in the L, a, b color system. The lower the b value, the less yellowish it is, which is preferable. However, if the b value is lower than -2.2, the yellowishness is reduced, but the blueness increases, making the color tone undesirable.
[0063] (6) 4-carboxybenzaldehyde content and p-toluic acid content in terephthalic acid The sample was dissolved in a 2N ammonia solution, diluted to a given concentration with ultrapure water, and then measured by high performance liquid chromatography equipped with an ODS column.
[0064] (7) Content of the compound represented by formula (1), formula (2) or formula (3), and content of the compound represented by formula (4) or formula (5) in BDO The BDO to which the compound represented by the formula (1), (2) or (3) and the compound represented by the formula (4) or (5) were added was used as a sample, and the sample was dissolved in a deuterated chloroform solvent containing a trace amount of tetramethylsilane, and was measured using an AVANCE NEO spectrometer (manufactured by Bruker). 1H NMR spectrum was measured to determine the content (integral value) of the compound represented by formula (1), formula (2) or formula (3) and the compound represented by formula (4) or formula (5) relative to the content (integral value) of BDO. The chemical shift reference was set to 0.00 ppm for the tetramethylsilane signal. In the obtained spectrum, the integral value of the signal of the proton (δ: 1.49 ppm) bonded to the α-position carbon of the hydroxyl group of BDO was used as the reference, and the weight of each functional group contained in a unit weight of BDO was calculated using the integral value of the signal of the proton assigned to each functional group in Table 1 below. In addition, "x" in each structural formula in Table 1 indicates the proton that was used as the reference when calculating the concentration.
[0065] [Table 1]
[0066] [Raw material terephthalic acid] Terephthalic acid (TPA) used as a raw material for manufacturing PBT in the following examples and comparative examples was produced by oxidizing p-xylene in an acetic acid solvent in the presence of a catalyst containing cobalt and manganese, and then purifying it by hydrogenation, during which process a certain amount of 4-carboxybenzaldehyde and p-toluic acid may be contained. The contents of these substances vary depending on the production conditions, but in the following examples and comparative examples, these terephthalic acids were used alone or in blends to obtain the values in Table 1 below. The terephthalic acid used in the blends also includes terephthalic acid that has not been subjected to a hydrogenation reaction.
[0067] [Raw material 1,4-butanediol] In the following examples and comparative examples, 1,4-butanediol (BDO) used as a raw material for the production of PBT is one obtained by hydrogenating succinic acid obtained by fermentation and purifying it by distillation. In the production process, certain amounts of compounds (1), (2), (3), (4), and (5) may be contained. On the other hand, compounds (1), (2), (3), (4), and (5) were not detected in the BDO obtained by acetoxylating butadiene from naphtha and then hydrolyzing it. Thus, the contents of these compounds vary depending on the production method and production conditions, but in the following examples and comparative examples, both BDOs were blended to obtain the values in Table 2 shown below.
[0068] [Manufacturing method of PBT] In the following examples and comparative examples, a two-tank production process using equipment consisting of an esterification reaction tank equipped with a screw stirrer and a rectification column, and a polycondensation reaction tank equipped with a double helical stirrer is described.
[0069] [Example 1] In an esterification reaction tank previously set at 150°C, a slurry was charged in which 75.44 parts by mass of terephthalic acid containing 4-carboxybenzaldehyde and p-toluic acid as shown in Table 2, and 122.77 parts by mass of BDO, which is the content of compounds (1), (2), (3), (4), and (5) as shown in Table 2, were mixed. Then, a 6% by mass BDO solution of tetrabutoxytitanium was charged in an amount that was 38 ppm as titanium atoms relative to the resulting PBT, and the temperature in the tank was raised from 150°C to 210°C over 90 minutes, and further maintained at 210°C for 60 minutes. During this time, the esterification reaction was carried out while removing by-product water in the distillation column. The esterification reaction was terminated when the distilled by-product water reached 41 parts by mass. The esterification reaction time in Table 2 was determined as the time from the start of raising the temperature in the tank to zero, until the distilled water reached 21 parts by mass.
[0070] Subsequently, the entire amount of the obtained oligomer was transferred to a polycondensation reaction tank previously set at 210 ° C. connected by piping from the bottom of the esterification reaction tank, and a 10% by mass BDO solution of magnesium acetate was charged in an amount equivalent to 12 ppm of magnesium atom relative to the obtained PBT. The temperature in the tank was raised from 210 ° C. to 240 ° C. over 45 minutes while stirring, and the pressure was gradually reduced from normal pressure to 0.5 Torr over 90 minutes. Thereafter, the pressure was maintained at 240 ° C. and 0.5 Torr, and when a predetermined torque was reached, the stirrer was stopped and the pressure was restored, and the resin was extracted in a strand shape from the bottom of the polycondensation reaction tank through a die head, cooled with a water flow slider, and then cut into PBT pellets (major axis about 3 mm, minor axis about 2 mm, length about 4 mm) with a rotary cutter. The polycondensation time listed in Table 2 represents the time from the time when the temperature in the tank was raised to the time when a predetermined torque was reached, with the time being set to zero. The obtained PBT was evaluated according to the above-mentioned items (1) to (5), and the results are shown in Table 2.
[0071] [Examples 2 to 4, Comparative Examples 1 to 6] PBT pellets were produced in the same manner as in Example 1, except that, as the raw material terephthalic acid, terephthalic acid having the 4-carboxybenzaldehyde and p-toluic acid contents shown in Table 2 was used, as the raw material BDO, BDO having the contents of compound (1), compound (2), compound (3), compound (4), and compound (5) shown in Table 2 was used, and the esterification reaction time and polycondensation reaction time were set as shown in Table 2. The obtained PBT was evaluated according to the above-mentioned items (1) to (5), and the results are shown in Table 2.
[0072] [Table 2]
[0073] As shown in Table 2, the PBT of Examples 1 to 4, which meets the requirements of the present invention, have a preferable color tone (b value). In contrast, the PBTs of Comparative Examples 1 to 6, which do not satisfy the requirements of the present invention, have unfavorable color tones (b value).
Claims
1. The terminal benzaldehyde group concentration is 0.005 to 0.15 equivalents / ton, and the terminal methylphenyl group concentration is 0.08 to 1.5 equivalents / ton; Polybutylene terephthalate containing, as copolymerization components, 0.001 to 0.220 mol % of butyric acid units and 0.001 to 0.220 mol % of succinic acid units.
2. A method for producing polybutylene terephthalate by reacting a dicarboxylic acid component with a diol component, the method comprising the steps of: using, as the dicarboxylic acid component, terephthalic acid having a 4-carboxybenzaldehyde content of 1 to 200 ppm and a p-toluic acid content of 20 to 300 ppm; and using, as the diol component, 1,4-butanediol containing 50 to 8,000 ppm in total of one or more compounds represented by the following formula (1), formula (2) or formula (3) and containing 5 to 1,000 ppm in total of one or two compounds represented by the following formula (4) or formula (5): 【Chemistry 1】
3. The method for producing polybutylene terephthalate according to claim 2, wherein the terephthalic acid is terephthalic acid that has been subjected to a hydrogenation purification process, and the 1,4-butanediol is 1,4-butanediol obtained by hydrogenating succinic acid.
Citation Information
Patent Citations
Horitetoramechirenterefutareetono seizoho
JP1976047096A
Polybutylene terephthalate and its production process
JP2006152252A
1,4-butanediol, method of producing polyester using the 1,4-butanediol and method of storing the 1,4-butanediol
JP2015083657A
Cited By
Polybutylene terephthalate and method for producing the same
JP2026150342A
Polybutylene terephthalate and its manufacturing method
JP2026181995A