Laminate type capacitor and method for manufacturing the same
The multilayer capacitor design with a metal layer, conductive resin, and plating layer enhances bending strength and maintains ESR, addressing the need for durable automotive capacitors.
Patent Information
- Application Number
- JP2024022938
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-16
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-01
AI Technical Summary
Automotive multilayer capacitors require enhanced bending strength characteristics while maintaining equivalent series resistance (ESR) characteristics to withstand deformation on mounted boards.
A multilayer capacitor design featuring a metal layer with controlled surface roughness and composition, a conductive resin layer, and a plating layer, which are free from glass and binder resin, and include specific conductive metals and low melting point metals to enhance bending strength without compromising ESR.
The design achieves improved bending strength characteristics while ensuring equivalent series resistance, making it suitable for automotive applications.
Smart Images

Figure 2024132900000001_ABST
Abstract
Description
[Technical field]
[0001] This description relates to stacked capacitors and methods for making same. [Background technology]
[0002] Multi-layer ceramic capacitors (MLCCs) are used in a variety of electronic devices because they can be made small and have high capacitance. Recently, with the growing interest in autonomous driving and electric vehicles, the number of power drive systems in automobiles is increasing, which has led to an increase in the demand for multi-layer ceramic capacitors for automobiles.
[0003] Automotive multilayer capacitors require high levels of electrical reliability and impact resistance, and in particular, multilayer capacitors with excellent durability against deformation of the substrate on which they are mounted, i.e., excellent bending strength characteristics, are required. Summary of the Invention [Problem to be solved by the invention]
[0004] An aspect of the present disclosure can provide a multilayer capacitor having enhanced bending strength characteristics while maintaining equivalent series resistance (ESR) characteristics. [Means for solving the problem]
[0005] A multilayer capacitor according to one aspect includes a capacitor body including a dielectric layer and an internal electrode, and an external electrode arranged on the outside of the capacitor body, the external electrode including a metal layer arranged on the outside of the capacitor body and made of a first conductive metal, and a conductive resin layer arranged on the outside of the metal layer and including a resin, a second conductive metal, a low-melting point metal having a melting point lower than that of the second conductive metal, and an alloy of the second conductive metal and the low-melting point metal.
[0006] The multilayer capacitor may have a first direction in which the dielectric layers and the internal electrodes are stacked, and a second direction and a third direction that are perpendicular to the first direction and perpendicular to each other.
[0007] The capacitor body can have first and second sides opposing each other in a first direction, third and fourth sides opposing each other in the second direction, and fifth and sixth sides opposing each other in the third direction.
[0008] The metal layer may have a surface roughness on an outer surface.
[0009] The metal layer may have an average surface roughness (Ra) of 0.2 to 1 in a cross section cut in the first direction and in the third direction perpendicular to the second direction at the center in the second direction.
[0010] The metal layer may be free of glass and binder resin.
[0011] In a cross section cut in the first and third directions perpendicular to the second direction at the center of the second direction, the metal layer may have an area ratio of glass contained in a unit area of the metal layer of 2% or less.
[0012] In a cross section cut in the first and third directions perpendicular to the second direction at the center of the second direction, the metal layer may have an area ratio of the binder resin contained per unit area of the metal layer of 1% or less.
[0013] The first conductive metal or the second conductive metal may include copper (Cu), nickel (Ni), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), tungsten (W), titanium (Ti), alloys thereof, or combinations thereof.
[0014] The low melting point metal may include tin (Sn), lead (Pb), bismuth (Bi), silver (Ag), copper (Cu), alloys thereof, or combinations thereof.
[0015] In a cross section cut in the first direction and the third direction perpendicular to the second direction at the center in the second direction, the conductive resin layer may have an area ratio of resin contained in a unit area of the conductive resin layer of 5% to 30%.
[0016] In a cross section cut in the first and third directions perpendicular to the second direction at the center of the second direction, the conductive resin layer may have an area ratio of the second conductive metal, the low melting point metal, and the alloy of the second conductive metal and the low melting point metal contained in a unit area of the conductive resin layer of 5% to 30%.
[0017] The external electrodes may further include a plating layer disposed on the outer side of the conductive resin layer.
[0018] The external electrode may have a connection portion disposed outside the third and fourth faces of the capacitor body, and a band portion disposed extending from the connection portion onto the first and second faces of the capacitor body.
[0019] The metal layer, the conductive resin layer, and the plating layer can be located on the connection portion and the band portion.
[0020] The metal layer may be located on the connection portion and the band portion, the conductive resin layer may be located on the band portion, and the plating layer may be located on the connection portion and the band portion.
[0021] A method for manufacturing a multilayer capacitor according to another aspect includes the steps of: forming a capacitor body including a dielectric layer and an internal electrode; and forming an external electrode on an outside of the capacitor body.
[0022] The step of forming the external electrode includes a step of forming a metal layer made of a first conductive metal, and a step of applying a paste for a conductive resin layer, which paste includes a second conductive metal powder, a low-melting point metal having a melting point lower than that of the second conductive metal, and a resin, to the outside of the metal layer and then curing the paste to form a conductive resin layer.
[0023] The step of forming the metal layer is carried out by using a sintering method, a sputtering method, or a plating method.
[0024] The step of forming the metal layer may include applying a paste for the metal layer, including a first conductive metal powder and a binder resin, to the outside of the capacitor body, and then heat-treating the paste at a temperature 400° C. or more higher than a curing temperature of the binder resin to remove the binder resin, and sintering the first conductive metal powder to form the metal layer.
[0025] The metal layer paste may not include a glass frit.
[0026] The metal layer paste may contain 30 to 60 parts by weight of binder resin per 100 parts by weight of the first conductive metal.
[0027] In the step of forming the metal layer, the heat treatment temperature may be 600°C to 900°C.
[0028] The conductive resin layer paste may contain 5 to 30 parts by weight of resin per 100 parts by weight of the second conductive metal.
[0029] The conductive resin layer paste may contain 5 to 30 parts by weight of a low melting point metal with respect to 100 parts by weight of the second conductive metal.
[0030] The conductive resin layer paste is applied so as to be located only on the band portion.
[0031] The step of forming the external electrodes may further include the step of forming a plating layer on the outside of the conductive resin layer using a plating method. Effect of the Invention
[0032] According to one aspect of the multilayer capacitor, it is possible to enhance bending strength characteristics while maintaining equivalent series resistance (ESR) characteristics. [Brief description of the drawings]
[0033] [Figure 1] 1 is a perspective view showing a multilayer capacitor according to one side; [Diagram 2] 2 is a cross-sectional view of the multilayer capacitor taken along line II' in FIG. [Diagram 3] 2 is an exploded perspective view showing a laminated structure of internal electrodes in the capacitor body of FIG. 1. [Figure 4] FIG. 3 is an enlarged cross-sectional view of a portion III in FIG. 2. [Diagram 5] 11 is a cross-sectional view of a modified example of a multilayer capacitor according to one aspect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Hereinafter, with reference to the attached drawings, the embodiments of the present invention will be described in detail so that those skilled in the art to which the present invention pertains can easily carry out the present invention. In the drawings, parts unnecessary for the explanation are omitted in order to clearly explain the present invention, and the same or similar components are given the same reference numerals throughout the specification. In addition, the attached drawings are merely for the purpose of making the embodiments disclosed in the present specification easily understandable, and the technical ideas disclosed in the specification are not limited by the attached drawings, and it should be understood that the drawings include all modifications, equivalents, or alternatives included in the idea and technical scope of the present invention.
[0035] Terms including ordinal numbers such as first, second, etc. may be used to describe various components, but the components are not limited by the terms. The terms are used only to distinguish one component from another.
[0036] When a component is said to be "coupled" or "connected" to another component, it should be understood that it may be directly coupled, connected, or opposite the other component, but that there may be other components in between. In contrast, when a component is said to be "directly coupled" or "directly connected" to another component, it should be understood that there are no other components in between.
[0037] It should be understood that, throughout the specification, the terms "comprise" or "have" are intended to specify the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof. Thus, when a part "comprises" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0038] FIG. 1 is a perspective view showing a multilayer capacitor from one side, FIG. 2 is a cross-sectional view of the multilayer capacitor taken along line II' in FIG. 1, and FIG. 3 is an exploded perspective view showing the laminated structure of internal electrodes in the capacitor body of FIG. 1.
[0039] To define the directions for clearly explaining this aspect, the L axis, W axis, and T axis shown in the drawing respectively indicate the longitudinal direction, width direction, and thickness direction of the capacitor body 110. Here, the thickness direction (T axis direction) may be a direction perpendicular to the wide surface (principal surface) of the sheet-shaped component, and may be used in the same concept as the lamination direction in which the dielectric layers 111 are laminated, for example. The longitudinal direction (L axis direction) is a direction extending parallel to the wide surface (principal surface) of the sheet-shaped component and approximately perpendicular to the thickness direction (T axis direction), and may be, for example, a direction in which the first external electrode 131 and the second external electrode 132 are located on both sides. The width direction (W axis direction) may be a direction extending parallel to the wide surface (principal surface) of the sheet-shaped component and approximately perpendicular to the thickness direction (T axis direction) and the longitudinal direction (L axis direction), and the length of the longitudinal direction (L axis direction) of the sheet-shaped component is longer than the length of the width direction (W axis direction).
[0040] Therefore, the first direction in which the dielectric layer 111 and the first internal electrode 121 and the second internal electrode 122 are stacked may be the thickness direction (T-axis direction), and the second and third directions which are perpendicular to the first direction and perpendicular to each other may be the longitudinal direction (L-axis direction) and the width direction (W-axis direction), or the width direction (W-axis direction) and the longitudinal direction (L-axis direction), respectively.
[0041] 1 to 3, the multilayer capacitor 100 includes a capacitor body 110, and a first external electrode 131 and a second external electrode 132 disposed on opposite ends of the capacitor body 110 in the longitudinal direction (L-axis direction).
[0042] For example, the capacitor body 110 may have a substantially hexahedral shape.
[0043] In the present disclosure, for convenience of explanation, the two surfaces of the capacitor body 110 that face each other in the thickness direction (T-axis direction) are defined as the first surface and the second surface, the two surfaces connected to the first surface and the second surface and facing each other in the longitudinal direction (L-axis direction) are defined as the third surface and the fourth surface, and the two surfaces connected to the first surface and the second surface and the third surface and the fourth surface and facing each other in the width direction (W-axis direction) are defined as the fifth surface and the sixth surface. As an example, the first surface of the lower surface may be the surface facing the mounting direction. In addition, the first surface to the sixth surface may be flat, but are not limited thereto. For example, the center part may be a convex curved surface, and the corners that are the boundaries between the surfaces may be rounded.
[0044] The shape and size of the capacitor body 110 and the number of laminated dielectric layers 111 are not limited to those shown in the drawings of this embodiment.
[0045] The capacitor body 110 is formed by stacking a plurality of dielectric layers 111 in the thickness direction (T-axis direction) and then firing the laminate, and includes a plurality of dielectric layers 111 and a plurality of first internal electrodes 121 and second internal electrodes 122 that are alternately arranged in the thickness direction (T-axis direction) with the dielectric layers 111 sandwiched between them. At this time, the first internal electrodes 121 and the second internal electrodes 122 may have polarities different from each other.
[0046] At this time, the boundaries between the adjacent dielectric layers 111 of the capacitor body 110 are integrated to such an extent that it is difficult to confirm the boundaries without using a scanning electron microscope (SEM).
[0047] The capacitor body 110 may also include an active area and cover areas 112, 113.
[0048] The active region is a portion that contributes to forming the capacitance of the multilayer capacitor 100. As an example, the active region may be a region where the first internal electrode 121 and the second internal electrode 122 that are stacked along the thickness direction (T-axis direction) overlap each other.
[0049] The cover regions 112 and 113 may be located on the first and second surfaces of the active region in the thickness direction (T-axis direction) as margins. Such cover regions 112 and 113 may be a single dielectric layer 111 or two or more dielectric layers 111 laminated on the upper and lower surfaces of the active region, respectively.
[0050] In addition, the capacitor body 110 may further include a side cover region. The side cover region may be located on the fifth and sixth sides of the active region in the width direction (W-axis direction) as a margin portion. Such a side cover region is formed by applying a conductive paste layer for forming an internal electrode to only a part of the surface of the dielectric green sheet when applying the conductive paste layer to the surface of the dielectric green sheet, laminating dielectric green sheets not applied with a conductive paste layer on both sides of the surface of the dielectric green sheet, and then firing the laminate.
[0051] The cover regions 112, 113 and the side cover regions serve to prevent the first internal electrode 121 and the second internal electrode 122 from being damaged by physical or chemical stress.
[0052] As an example, the dielectric layer 111 may include a ceramic material with a high dielectric constant, such as BaTiO 3 , CaTiO 3 , SrTiO 3 , or CaZrO 3 In addition, these components may further contain auxiliary components such as Mn compounds, Fe compounds, Cr compounds, Co compounds, and Ni compounds. For example, BaTiO 3 Ca, Zr, etc. are partially dissolved in the system dielectric ceramic (Ba 1-x Ca x )TiO 3 (0 <x<1)、Ba(Ti 1-y Ca y )O 3 (0 <y<1)、(Ba 1-x Cax )(Ti 1-y Zr y )O 3 (0 < x < 1, 0 < y < 1) or Ba(Ti 1-y Zr y )O 3 can include (0 < y < 1), etc.
[0053] In addition, ceramic additives, organic solvents, plasticizers, binders, dispersants, etc. are further added to the dielectric layer 111 together with ceramic powder. As the ceramic additive, for example, transition metal oxides or transition metal carbides, rare earth elements, magnesium (Mg) or aluminum (Al), etc. can be used.
[0054] As an example, the average thickness of the dielectric layer 111 may be 0.5 μm to 10 μm.
[0055] The first internal electrode 121 and the second internal electrode 122 are electrodes having different polarities from each other, and are alternately arranged so as to face each other along the thickness direction (T-axis direction) with the dielectric layer 111 interposed therebetween, and one end can be exposed through the third surface and the fourth surface of the capacitor body 110, respectively.
[0056] The first internal electrode 121 and the second internal electrode 122 can be electrically insulated from each other by the dielectric layer 111 disposed in the middle.
[0057] The ends of the first internal electrode 121 and the second internal electrode 122 that are alternately exposed through the third surface and the fourth surface of the capacitor body 110 are respectively connected to the first external electrode 131 and the second external electrode 132 and can be electrically connected.
[0058] The first internal electrode 121 and the second internal electrode 122 contain a conductive metal, and for example, metals such as nickel (Ni), copper (Cu), silver (Ag), lead (Pd), or gold (Au), and alloys thereof, for example, Ag - Pd alloy can be included.
[0059] The first internal electrode 121 and the second internal electrode 122 may also contain dielectric particles of the same composition as the ceramic material contained in the dielectric layer 111 .
[0060] The first internal electrode 121 and the second internal electrode 122 are formed using a conductive paste containing a conductive metal. The conductive paste can be printed by screen printing, gravure printing, or the like.
[0061] As an example, the average thickness of the first internal electrode 121 and the second internal electrode 122 may be 0.1 μm to 2 μm.
[0062] The first external electrode 131 and the second external electrode 132 are provided with voltages of different polarities and can be electrically connected to exposed portions of the first internal electrode 121 and the second internal electrode 122, respectively.
[0063] With the above configuration, when a predetermined voltage is applied to the first external electrode 131 and the second external electrode 132, charge is accumulated between the mutually opposing first internal electrode 121 and second internal electrode 122. At this time, the capacitance of the multilayer capacitor 100 is proportional to the overlap area of the first internal electrode 121 and the second internal electrode 122 that overlap each other along the thickness direction (T-axis direction) in the active region.
[0064] The first external electrode 131 and the second external electrode 132 may each include a first connection portion and a second connection portion arranged on the third and fourth surfaces of the capacitor body 110, respectively, and connected to the first internal electrode 121 and the second internal electrode 122, and a first band portion and a second band portion arranged at the corner where the third and fourth surfaces of the capacitor body 110 meet the first and second surfaces or the fifth and sixth surfaces.
[0065] The first and second band parts may extend from the first and second connection parts to parts of the first and second faces or the fifth and sixth faces of the capacitor body 110. The first and second band parts may serve to improve the bonding strength between the first and second external electrodes 131 and 132.
[0066] Fig. 4 is an enlarged cross-sectional view of region III in Fig. 2, and is a cross-sectional view showing an enlarged schematic view of the second external electrode 132. Fig. 4 shows only the second external electrode 132, but the first external electrode 131 also has similar features to those in Fig. 4. Hereinafter, the first external electrode 131 and the second external electrode 132 according to this aspect will be described in detail with reference to Fig. 4.
[0067] As an example, the first external electrode 131 and the second external electrode 132 may each include a metal layer 1311, 1321 in contact with the capacitor body 110, a conductive resin layer 1312, 1322 arranged to cover the metal layer 1311, 1321, and, optionally, a plating layer 1313, 1323 arranged to cover the conductive resin layer 1312, 1322.
[0068] The metal layers 1311 and 1321 are in direct contact with the capacitor body 110, and are disposed on the third and fourth surfaces of the capacitor body 110, respectively, and are connected to the first and second internal electrodes 121 and 122. The metal layers 1311 and 1321 may be located at the first and second connection portions and the first and second band portions. That is, the metal layers 1311 and 1321 may be located at the first, second, third, fourth, fifth, and sixth surfaces.
[0069] Metal layers 1311 and 1321 are made of a first conductive metal.
[0070] The metal layers 1311 and 1321 may include, as a first conductive metal, copper (Cu), nickel (Ni), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), tungsten (W), titanium (Ti), alloys thereof, or combinations thereof, for example, copper (Cu) may include a copper (Cu) alloy. When the first conductive metal includes copper, the metal other than copper is included in an amount of 5 molar parts or less per 100 molar parts of copper.
[0071] For example, the metal layers 1311 and 1321 may be substantially made of the first conductive metal and may not contain glass or binder resin. By making the metal layers 1311 and 1321 only of the first conductive metal, the equivalent series resistance characteristics can be improved compared to when the metal layers 1311 and 1321 further contain glass and binder resin.
[0072] Here, the glass may be, for example, one or more selected from the group consisting of silicon oxide, boron oxide, aluminum oxide, transition metal oxide, alkali metal oxide, and alkaline earth metal oxide. The transition metal may be selected from the group consisting of zinc (Zn), titanium (Ti), copper (Cu), vanadium (V), manganese (Mn), iron (Fe), and nickel (Ni), the alkali metal may be selected from the group consisting of lithium (Li), sodium (Na), and potassium (K), and the alkaline earth metal may be one or more selected from the group consisting of magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba).
[0073] The binder resin may be, for example, epoxy, ethyl cellulose, acrylic, or butyral.
[0074] As described below, metal layers 1311, 1321 made only of the first conductive metal without including glass and binder resin are manufactured by applying a metal layer paste containing a first conductive metal powder and a binder resin to the outside of capacitor body 110, and then performing a heat treatment at a temperature 400° C. or more higher than the curing temperature of the binder resin to remove the binder resin and sinter the first conductive metal powder. As a result, metal layers 1311, 1321 can have surface roughness on the outer surface. However, this aspect is not limited thereto, and metal layers 1311, 1321 made only of the first conductive metal can also be manufactured by a method such as sputtering or plating.
[0075] Hereinafter, the average surface roughness (Ra) of metal layers 1311, 1321, the average area of metal layers 1311, 1321 and conductive resin layers 1312, 1322, and the average area and type of each component can be analyzed by observing a cross section (cross sections in the L-axis direction and T-axis direction) cut perpendicular to the width direction (W-axis direction) at the center (1 / 2 point) of the width direction (W-axis direction) of multilayer capacitor 100 in the longitudinal direction and stacking direction, or a cross section (hereinafter referred to as "cross section") cut perpendicular to the longitudinal direction (L-axis direction) at the center (1 / 2 point) of the longitudinal direction (L-axis direction) in the width direction (W-axis direction) and stacking direction (T-axis direction) using a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM), for example.
[0076] A cross-sectional sample of the multilayer capacitor 100 can be prepared, for example, by mounting the multilayer capacitor 100 on an epoxy mold, polishing the multilayer capacitor 100 so that the cross-section is exposed, and coating it with a Pt coater for 10 seconds.
[0077] A scanning electron microscope (SEM), for example, a Verios G4 product from Thermofisher Scientific, may be used under measurement conditions of 10 kV and an analytical magnification of 3000x, and measurement can be performed so that the first external electrode 131 and the second external electrode 132 extend outwardly from the interface between the first external electrode 131 and the second external electrode 132 and the dielectric layer 111 by approximately 70 μm.
[0078] The average surface roughness (Ra) of the metal layers 1311 and 1321 can be measured by using a New View from Zygo Corporation, using a cross-sectional photograph obtained by cross-sectional observation using a SEM or STEM. The New View is one of the most representative interferometers, and is a scanning type device using white light. Just as non-destructive analysis such as XRD does not damage the sample, non-contact roughness measuring devices also measure the shape of the surface, but can measure the surface roughness without damaging the sample. The measurement principle is that a CCD camera is located at the top, and a white light source is located in the middle and irradiates the sample. Unlike short-wavelength lasers, the white light source has the characteristic that the wavelength is not fixed and there are many wavelengths, which causes polarization interference. The interferometer is driven vertically to collect the interference fringes. PZT is used for this. If the interference is further increased by the beam splitter, the parts that cause constructive interference will appear in white, and the parts that cause destructive interference will appear in black. If the interference fringes are focused while moving the stage on which the sample is placed, and the height information is detected, the surface roughness can be measured.
[0079] The average area and components of the first conductive metal of the metal layers 1311 and 1321, the resin of the conductive resin layers 1312 and 1322, the second conductive metal, the low melting point metal, and the alloy of the second conductive metal and the low melting point metal can be measured by analyzing a cross-sectional photograph obtained by cross-sectional observation using an SEM or STEM with an electron beam microanalyzer (EPMA). When performing component analysis using an electron beam microanalyzer (EPMA), an EDS (energy dispersive spectrometer) or a WDS (wavelength dispersive spectrometer) can be used as an X-ray spectrometer. Alternatively, when the cross-sections of the first external electrode 131 and the second external electrode 132 are observed using a backscattered electron image of an SEM or a HAADF image of an STEM, the first conductive metal, the second conductive metal, the low melting point metal, or the alloy of the second conductive metal and the low melting point metal having a metallic bond can be recognized as bright contrast parts, and non-metallic components such as resin or pores can be recognized as dark contrast parts. Therefore, the average area of the first conductive metal of metal layers 1311, 1321, the resin of conductive resin layers 1312, 1322, the second conductive metal, the low-melting point metal, or an alloy of the second conductive metal and the low-melting point metal can be calculated as the area ratio of the parts with different contrast to the area of the entire measurement field of view, for example by binarizing the cross-sectional photograph.
[0080] The average surface roughness (Ra) of the metal layers 1311, 1321 may be 0.2 to 1, for example, 0.3 to 0.4.
[0081] Metal layers 1311 and 1321 may be substantially free of glass. For example, in the cross section, the area ratio of glass contained in a unit area of metal layers 1311 and 1321 may be 2% or less, 1% or less, 0.1% or less, or 0% or more.
[0082] Furthermore, the metal layers 1311 and 1321 may be substantially free of binder resin. For example, in the cross section, the area ratio of the binder resin contained in the unit area to the unit area of the metal layers 1311 and 1321 may be 1% or less, 0.1% or less, or 0% or more.
[0083] Here, the area ratio of the glass or binder resin in the metal layers 1311, 1321 may be a percentage (%) of the area occupied by the glass or binder resin in a unit area of the metal layers 1311, 1321 with respect to the unit area of the metal layers 1311, 1321.
[0084] The area ratio of glass or binder resin in metal layers 1311, 1321 can be measured within a unit area of 1 μm to 100 μm wide and 1 μm to 100 μm long, for example 10 μm x 2 μm, located within metal layers 1311, 1321 in a cross-sectional photograph taken with SEM or STEM.
[0085] Here, when the metal layers 1311, 1321 are located at the first connection portion and the second connection portion, the unit area may be located at the center (1 / 2) point of the length in the thickness direction (T-axis direction) where the thickness (i.e., the length in the L-axis direction) of the first external electrode 131 and the second external electrode 132, including all of the metal layers 1311, 1321, the conductive resin layers 1312, 1322, and the plating layers 1313, 1323, is the thickest.
[0086] On the other hand, when the metal layers 1311, 1321 are located in the first band portion and the second band portion, the unit area may be such that the center (1 / 2) point of the length in the longitudinal direction (L-axis direction) is located at the point where the thickness (i.e., the length in the T-axis direction) of the first external electrode 131 and the second external electrode 132, including all of the metal layers 1311, 1321, the conductive resin layers 1312, 1322, and the plating layers 1313, 1323, is the thickest.
[0087] However, the entire unit area is arranged to be located within the metal layers 1311 and 1321 .
[0088] The conductive resin layers 1312 and 1322 are disposed on the outside of the metal layers 1311 and 1321 .
[0089] The conductive resin layers 1312 and 1322 are located on the third and fourth surfaces of the capacitor body 110, and can extend to the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110. That is, the conductive resin layers 1312 and 1322 can be located on the first and second connection portions and the first and second band portions.
[0090] The length of the region where the conductive resin layers 1312, 1322 are arranged extending onto the first and second faces or the fifth and sixth faces of the capacitor body 110 (i.e., the first band portion and the second band portion) is longer than the length of the region where the metal layers 1311, 1321 are arranged extending onto the first and second faces or the fifth and sixth faces of the capacitor body 110 (i.e., the first band portion and the second band portion). In other words, the conductive resin layers 1312, 1322 are formed on the metal layers 1311, 1321 so as to completely cover the metal layers 1311, 1321.
[0091] The conductive resin layers 1312, 1322 include a resin and a second conductive metal.
[0092] The resin contained in the conductive resin layers 1312, 1322 is not particularly limited as long as it has adhesive and shock absorbing properties and can be mixed with the conductive metal powder to form a paste, and may include, for example, phenolic resin, acrylic resin, silicone resin, epoxy resin, or polyimide resin.
[0093] The second conductive metal contained in the conductive resin layers 1312 and 1322 serves to electrically connect to the metal layers 1311 and 1321 or the plating layers 1313 and 1323 .
[0094] By way of example, the second conductive metal may include copper (Cu), nickel (Ni), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), tungsten (W), titanium (Ti), alloys thereof, or combinations thereof. The first conductive metal and the second conductive metal may be the same metal.
[0095] The second conductive metal contained in the conductive resin layers 1312 and 1322 may have a spherical, flake-like shape, or a combination thereof. That is, the second conductive metal may be made up of only flake-like shapes, only spherical shapes, or a mixture of flake-like and spherical shapes.
[0096] Here, the term "spherical" may include shapes that are not completely spherical, and may include shapes in which the ratio of the major axis to the minor axis (major axis / minor axis) is 1.45 or less. The term "flaky powder" refers to a powder having a flat and elongated shape, and is not particularly limited, and may include shapes in which the ratio of the major axis to the minor axis (major axis / minor axis) is 1.95 or more, for example.
[0097] On the other hand, if the metal layers 1311 and 1321 are made of only the first conductive metal and do not contain glass and binder resin, it is difficult to relieve stress caused by deformation of the mounted board, and bending cracks may occur. Therefore, the conductive resin layers 1312 and 1322 further contain a low melting point metal and an alloy of the second conductive metal and the low melting point metal in addition to the resin and the second conductive metal, thereby ensuring the equivalent series resistance (ESR) characteristics by the metal layers 1311 and 1321 while complementing the bending strength characteristics reduced by the metal layers 1311 and 1321.
[0098] As an example, the low melting point metal is a metal that has a lower melting point than the second conductive metal.
[0099] The low melting point metal can be any metal that has a lower melting point than the second conductive metal, and can include, for example, tin (Sn), lead (Pb), bismuth (Bi), silver (Ag), copper (Cu), alloys thereof, or combinations thereof.
[0100] The second conductive metal and the low melting point metal contained in the conductive resin layers 1312 and 1322 may be in the form of an alloy. For example, when the second conductive metal is copper (Cu) and the low melting point metal is tin (Sn), the alloy of the second conductive metal and the low melting point metal is, for example, Cu. 6 Sn 5 or Cu 3 When the second conductive metal is silver (Ag) and the low melting point metal is tin (Sn), the alloy of the second conductive metal and the low melting point metal is, for example, Ag. 3 It may be Sn.
[0101] For example, the area ratio of the resin contained in the conductive resin layers 1312 and 1322 to the unit area of the conductive resin layers 1312 and 1322 in the cross section may be 5% to 30%, for example, 5% to 20%, or 5% to 12%. If the area ratio of the resin contained in the conductive resin layers 1312 and 1322 is less than 5%, the bending strength characteristics may decrease, and if it exceeds 30%, the ESR characteristics may decrease.
[0102] In the cross section, the area ratio of the second conductive metal, low melting point metal, alloy of the second conductive metal and low melting point metal, or combination thereof contained in a unit area to a unit area of the conductive resin layers 1312, 1322 may be 5% to 30%, for example, 5% to 20%, or 8% to 15%. If the area ratio of the second conductive metal, low melting point metal, alloy of the second conductive metal and low melting point metal, or combination thereof contained in the conductive resin layers 1312, 1322 is less than 5%, the ESR characteristics may decrease, and if it exceeds 30%, the bending strength characteristics may decrease.
[0103] Here, the area ratio of the resin, the second conductive metal, etc. contained in the conductive resin layers 1312, 1322 may be the percentage (%) of the area occupied by the resin, the second conductive metal, etc. in a unit area of the conductive resin layers 1312, 1322 to a unit area of the conductive resin layers 1312, 1322.
[0104] In addition, the area ratio of the resin and the second conductive metal in the conductive resin layers 1312, 1322 can be measured within a unit area of 1 μm to 100 μm wide and 1 μm to 100 μm long, for example 10 μm x 2 μm, located within the conductive resin layers 1312, 1322 in a cross-sectional photograph such as SEM or STEM.
[0105] Here, when the conductive resin layers 1312, 1322 are located at the first connection portion and the second connection portion, the unit area may be located at the center (1 / 2) point of the length in the thickness direction (T-axis direction) where the thickness (i.e., the length in the L-axis direction) of the first external electrode 131 and the second external electrode 132, including all of the metal layers 1311, 1321, the conductive resin layers 1312, 1322, and the plating layers 1313, 1323, is the thickest.
[0106] On the other hand, when the conductive resin layers 1312, 1322 are located in the first band portion and the second band portion, the unit area may be such that the center (1 / 2) point of the length in the longitudinal direction (L-axis direction) is located at the point where the thickness (i.e., the length in the T-axis direction) of the first external electrode 131 and the second external electrode 132, including all of the metal layers 1311, 1321, the conductive resin layers 1312, 1322, and the plating layers 1313, 1323, is the thickest.
[0107] However, the entire unit area is arranged so as to be located within the conductive resin layers 1312 and 1322 .
[0108] FIG. 5 is a cross-sectional view of a modified example of the multilayer capacitor according to one aspect.
[0109] Since the multilayer capacitor 100 according to this modification is similar to the multilayer capacitor 100 described above, a duplicated description will be omitted and differences will be mainly described.
[0110] FIG. 2 shows that the conductive resin layers 1312, 1322 are located on the first, second, third, fourth, fifth, and sixth surfaces of the capacitor body 110, i.e., the connection portion and band portion, and are formed in a form that completely covers the metal layers 1311, 1321.
[0111] 5 shows that the conductive resin layers 1312 and 1322 are not located on the third and fourth faces of the capacitor body 110, but are located only on the first, second, fifth, and sixth faces. That is, the conductive resin layers 1312 and 1322 can be located only on the band portion, not on the connection portion.
[0112] When the conductive resin layers 1312, 1322 are located only in the band portion, the equivalent series resistance characteristics are ensured by the metal layers 1311, 1321, while the bending strength characteristics that are reduced by the metal layers 1311, 1321 can be further strengthened.
[0113] Optionally, the first external electrode 131 and the second external electrode 132 may further include plating layers 1313 and 1323 disposed on the outer sides of the conductive resin layers 1312 and 1322 .
[0114] The plating layers 1313, 1323 are located on the third and fourth surfaces of the capacitor body 110 and may extend to the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110. That is, the plating layers 1313, 1323 may be located on the first and second connection portions and the first and second band portions. The length of the plating layers 1313, 1323 in the region where they are arranged extending to the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110 (i.e., the first and second band portions) is longer than the length of the conductive resin layers 1312, 1322 in the region where they are arranged extending to the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110 (i.e., the first and second band portions). That is, the plating layers 1313 and 1323 are formed on the conductive resin layers 1312 and 1322 so as to completely cover the metal layers 1311 and 1321 and the conductive resin layers 1312 and 1322 .
[0115] The plating layers 1313 and 1323 may be a plating layer containing nickel (Ni), copper (Cu), tin (Sn), palladium (Pd), platinum (Pt), gold (Au), silver (Ag), tungsten (W), titanium (Ti), lead (Pb), or the like, or an alloy thereof. As an example, the plating layers 1313 and 1323 may be a nickel (Ni) plating layer or a tin (Sn) plating layer, or may be a form in which a nickel (Ni) plating layer and a tin (Sn) plating layer are sequentially laminated, or a form in which a tin (Sn) plating layer, a nickel (Ni) plating layer, and a tin (Sn) plating layer are sequentially laminated. The plating layers 1313 and 1323 may also include a plurality of nickel (Ni) plating layers and / or a plurality of tin (Sn) plating layers.
[0116] The plating layers 1313 and 1323 can improve the mountability of the multilayer capacitor 100 on a substrate, structural reliability, durability against the outside, heat resistance, and equivalent series resistance.
[0117] A method for manufacturing a multilayer capacitor according to another embodiment includes the steps of forming a capacitor body including a dielectric layer and an internal electrode, and forming an external electrode on the outside of the capacitor body.
[0118] First, the manufacturing process of the capacitor body will be described. In the manufacturing process of the capacitor body, a dielectric paste that will become a dielectric layer after firing and a conductive paste that will become an internal electrode after firing are prepared.
[0119] The dielectric paste is produced, for example, by the following method: Ceramic materials are mixed uniformly by wet mixing or other means, dried, and then heat-treated under specified conditions to obtain a plastic powder. An organic vehicle or an aqueous vehicle is added to the obtained plastic powder and kneaded to prepare the dielectric paste.
[0120] The obtained dielectric paste is formed into a sheet by a doctor blade method or the like to obtain a dielectric green sheet. The dielectric paste may also contain additives selected from various dispersants, plasticizers, dielectrics, subcomponent compounds, glass, and the like, as necessary.
[0121] The conductive paste for the internal electrodes is prepared by kneading a conductive powder made of a conductive metal or its alloy with a binder and a solvent. The conductive paste for the internal electrodes may contain a ceramic powder (e.g., barium titanate powder) as a co-material, as necessary. The co-material can suppress the sintering of the conductive powder during the firing process.
[0122] A conductive paste for internal electrodes is applied in a predetermined pattern to the surface of a dielectric green sheet by various printing methods such as screen printing or transfer methods. Then, the dielectric green sheets on which the internal electrode patterns are formed are laminated in multiple layers, and then pressed in the lamination direction to obtain a dielectric green sheet laminate. At this time, the dielectric green sheets and the internal electrode patterns can be laminated so that the dielectric green sheets are located on the upper and lower surfaces of the dielectric green sheet laminate in the lamination direction.
[0123] Optionally, the resulting dielectric green sheet laminate can be cut to a predetermined size by dicing or the like.
[0124] Furthermore, the dielectric green sheet laminate can be solidified and dried to remove plasticizers, etc., as necessary, and after solidification and drying, can be barrel polished using a horizontal centrifugal barrel machine, etc. In barrel polishing, the dielectric green sheet laminate is placed in a barrel container together with media and polishing liquid, and unnecessary parts such as burrs generated during cutting can be polished by applying rotational motion, vibration, etc. to the barrel container. Furthermore, after barrel polishing, the dielectric green sheet laminate can be washed with a cleaning liquid such as water and dried.
[0125] The dielectric green sheet laminate is subjected to a binder removal process and a firing process to obtain a capacitor body.
[0126] The conditions of the binder removal treatment can be appropriately adjusted depending on the composition of the main component of the dielectric layer and the composition of the main component of the internal electrode. For example, the temperature rise rate during the binder removal treatment may be 5°C / hour to 300°C / hour, the support temperature may be 180°C to 400°C, and the temperature maintenance time may be 0.5 hours to 24 hours. The binder removal atmosphere may be air or a reducing atmosphere.
[0127] The firing conditions can be appropriately adjusted depending on the composition of the main component of the dielectric layer and the composition of the main component of the internal electrode. For example, the firing temperature may be 1200°C to 1350°C, or 1220°C to 1300°C, and the firing time may be 0.5 hours to 8 hours, or 1 hour to 3 hours. The firing atmosphere may be a reducing atmosphere, for example, nitrogen gas (N 2 ) and hydrogen gas (H 2 If the internal electrodes contain nickel (Ni) or a nickel (Ni) alloy, the oxygen partial pressure in the firing atmosphere is 1.0×10 -14 MPa~1.0×10 -10 It may be MPa.
[0128] After the firing treatment, annealing can be performed as necessary. Annealing is a treatment for reoxidizing the dielectric layer, and can be performed when the firing treatment is performed in a reducing atmosphere. The conditions of the annealing treatment can also be appropriately adjusted according to the composition of the main component of the dielectric layer. For example, the temperature during annealing can be 950°C to 1150°C, the time can be 0 hours to 20 hours, and the temperature increase rate can be 50°C / hour to 500°C / hour. The annealing atmosphere can be humidified nitrogen gas (N 2 ) atmosphere, and the oxygen partial pressure is 1.0×10 -9 MPa~1.0×10 -5 It may be MPa.
[0129] In the binder removal treatment, firing treatment, or annealing treatment, for example, a wetter can be used to moisten the nitrogen gas or mixed gas, and in this case, the water temperature may be 5° C. to 75° C. The binder removal treatment, firing treatment, and annealing treatment may be performed consecutively or independently.
[0130] Optionally, the third and fourth faces of the obtained capacitor body can be subjected to a surface treatment such as sandblasting, laser irradiation, barrel polishing, etc. By performing such a surface treatment, the ends of the first and second internal electrodes are exposed on the outermost surfaces of the third and fourth faces, which improves the electrical connection between the first and second external electrodes and the first and second internal electrodes, making it easier to form an alloy part.
[0131] A metal layer paste may be applied to the outer surface of the obtained capacitor body and then sintered to form a metal layer, although the present invention is not limited thereto and the metal layer may be formed by a sputtering method, a plating method, or the like.
[0132] The paste for the metal layer may include a first conductive metal powder and a binder resin. At this time, the paste for the metal layer does not include a glass frit. The first conductive metal, the binder resin, and the glass are the same as those described above, so that the repeated description will be omitted.
[0133] In addition, the paste for the metal layer may selectively contain sub-components such as a solvent, a dispersant, a plasticizer, or an oxide powder. For example, the solvent may be an organic solvent such as terpineol, butyl carbitol, alcohol, methyl ethyl ketone, acetone, or toluene, or an aqueous solvent.
[0134] For example, the paste for the metal layer may contain 30 to 60 parts by weight, for example 40 to 50 parts by weight, of the binder resin with respect to 100 parts by weight of the first conductive metal. If the content of the binder resin in the paste for the metal layer is less than 30 parts by weight, the density of the metal decreases during sintering, and the electrical properties and moisture resistance reliability decrease, whereas if it exceeds 60 parts by weight, the binder may not be completely removed, in which case the ESR properties may decrease.
[0135] The metal layer paste can be applied to the outer surface of the capacitor body by a dipping method, various printing methods such as screen printing, an application method using a dispenser, a spraying method using a spray, etc. The metal layer paste is applied to at least the third and fourth surfaces of the capacitor body, and is selectively applied to a part of the first, second, fifth, or sixth surface on which the band portions of the first and second external electrodes are formed.
[0136] Thereafter, the capacitor body coated with the metal layer paste is dried and heat-treated at a temperature 400°C higher than the binder resin curing temperature to remove the binder resin and sinter the first conductive metal powder to form a metal layer. For example, the binder resin curing temperature may be 200°C to 240°C, and accordingly, the heat treatment temperature may be 600°C to 900°C or 630°C to 850°C, and the heat treatment time may be 70 minutes to 160 minutes, or 70 minutes to 120 minutes.
[0137] If the heat treatment temperature is less than 600° C., sintering is not complete and the density decreases. The upper limit of the heat treatment temperature is not limited as long as it does not affect the capacitor body, and may be, for example, 900° C. or less.
[0138] This makes it possible to produce a metal layer that is free of glass and binder resin, is made of only the first conductive metal, and has a surface roughness on its outer surface.
[0139] A conductive resin layer paste can be applied to the outer surface of the obtained metal layer and then cured to form a conductive resin layer.
[0140] The conductive resin layer paste may include a resin and a second conductive metal powder. The conductive resin layer paste may further include a low melting point metal having a melting point lower than that of the second conductive metal. The resin, the second conductive metal, and the low melting point metal are the same as those described above, so that repeated description will be omitted.
[0141] In addition, the conductive resin layer paste may selectively include sub-components such as a binder, a solvent, a dispersant, a plasticizer, or an oxide powder. For example, the binder may be ethyl cellulose, acrylic, or butyral, and the solvent may be an organic solvent such as terpineol, butyl carbitol, alcohol, methyl ethyl ketone, acetone, or toluene, or an aqueous solvent.
[0142] For example, the conductive resin layer paste may contain 5 to 30 parts by weight, for example 5 to 13 parts by weight, of resin per 100 parts by weight of the second conductive metal. If the resin content in the conductive resin layer paste is less than 5 parts by weight, bending strength may decrease, and if it exceeds 30 parts by weight, ESR characteristics may decrease.
[0143] The conductive resin layer paste may contain 5 to 30 parts by weight, for example 10 to 15 parts by weight, of the low melting point metal relative to 100 parts by weight of the second conductive metal. If the content of the low melting point metal in the conductive resin layer paste is less than 5 parts by weight, the ESR characteristics may decrease, and if it exceeds 30 parts by weight, the bending strength characteristics may decrease.
[0144] As an example, the conductive resin layer can be formed by dipping the capacitor body 110 in a paste for the conductive resin layer and then curing it, or by printing the paste for the conductive resin layer on the surface of the capacitor body 110 using a screen printing method or a gravure printing method, or by applying the paste for the conductive resin layer to the surface of the capacitor body 110 and then curing it.
[0145] At this time, the conductive resin layer paste is applied so as to cover a part of the metal layer and expose the other part. For example, the conductive resin layer paste can be applied so as to be located only on the first band part and the second band part, not on the first connection part and the second connection part.
[0146] The method for applying the conductive resin layer paste so that it is located only on the first band portion and the second band portion is not particularly limited. For example, after forming a metal layer on the capacitor body, the conductive resin layer paste is applied onto the metal layer, and the conductive resin layer paste applied to the first connection portion and the second connection portion is removed using a porous nonwoven fabric or the like, so that the conductive resin layer paste is applied only to the band portions.
[0147] Next, a plating layer is formed on the outside of the metal layer and the conductive resin layer.
[0148] As an example, the fourth layer is formed by a plating method, and may be formed by sputtering or electrolytic deposition.
[0149] Specific examples of the present invention are presented below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and should not be construed as limiting the scope of the present invention.
[0150] [Manufacturing example: Manufacturing of stacked capacitors] (Example) Barium titanate (BaTiO 3A paste containing the powder is applied onto a carrier film and then dried to produce a plurality of dielectric green sheets.
[0151] A conductive paste containing nickel (Ni) is applied onto the dielectric green sheet by screen printing to form a conductive paste layer.
[0152] A plurality of dielectric green sheets are laminated so that the conductive paste layers at least partially overlap each other to produce a dielectric green sheet laminate.
[0153] The dielectric green sheet laminate is cut into individual chips, and then the chips are maintained at 230° C. in an air atmosphere for 60 hours to remove the binder, and then fired at 1200° C. to manufacture a capacitor body.
[0154] Next, a metal layer paste containing copper (Cu) as the first conductive metal and a binder resin (curing temperature: 230°C) is applied to the outer surface of the capacitor body by a dip method, dried, and then sintered at 630°C for 70 minutes to form a metal layer.
[0155] Next, a paste for a conductive resin layer containing epoxy resin, copper (Cu) as a second conductive metal, and tin (Sn) as a low melting point metal is applied to the outer surface of the capacitor body by a dipping method, dried, and then hardened to form a conductive resin layer.
[0156] Thereafter, nickel (Ni) and tin (Sn) plating is carried out to manufacture a multilayer capacitor.
[0157] (Comparative Example) Barium titanate (BaTiO 3 A paste containing the powder is applied onto a carrier film and then dried to produce a plurality of dielectric green sheets.
[0158] A conductive paste containing nickel (Ni) is applied onto the dielectric green sheet by screen printing to form a conductive paste layer.
[0159] A plurality of dielectric green sheets are laminated so that the conductive paste layers at least partially overlap each other to produce a dielectric green sheet laminate.
[0160] The dielectric green sheet laminate is cut into individual chips, and then the chips are maintained at 230° C. in an air atmosphere for 60 hours to remove the binder, and then fired at 1200° C. to manufacture a capacitor body.
[0161] Next, a metal layer paste containing glass frit and copper (Cu) as a conductive metal is applied to the outer surface of the capacitor body by a dipping method, dried, and then sintered to form a metal layer.
[0162] Next, a paste for a conductive resin layer, which contains epoxy resin and copper (Cu) powder as a conductive metal, is applied to the outer surface of the capacitor body by a dipping method, dried, and then hardened to form a conductive resin layer.
[0163] The capacitor body on which the conductive resin layer is formed is plated with nickel (Ni) and tin (Sn) to manufacture a multilayer capacitor.
[0164] [Experimental example: performance of multilayer capacitor] The surface roughness, bending strength, and equivalent series resistance (ESR) of the metal layer of the multilayer capacitors manufactured in the examples and comparative examples are measured.
[0165] 1) Method for measuring surface roughness of metal layer Five of the manufactured stacked capacitors are mounted on an epoxy mold, and the L-axis and T-axis faces (e.g., the fifth face) are polished to a depth of about 1 / 2 along the W-axis direction, and then coated with a Pt coater for 10 seconds to prepare a cross-sectional sample.
[0166] In the prepared cross-sectional sample, a position where the first electrode or the second electrode is entirely visible, approximately 70 μm from the interface between the first external electrode or the second external electrode and the dielectric layer in the plating layer direction, is measured using a UHR-SEM (Scanning Electron Microscope) at an accelerating voltage of 10 kV and an analytical magnification of 3000x, i.e., a magnification at which the interface between the metal layer and the conductive resin layer and the porous structure of the conductive resin layer are entirely visible.
[0167] The average surface roughness (Ra) of the metal layer is measured using a New View manufactured by Zygo Corporation on the cross-sectional photograph obtained.
[0168] 2) Bending strength measurement method Thirty stacked capacitors each according to the embodiment and the comparative example are prepared. The stacked capacitors are soldered onto a bending strength substrate (PCB) and then reflowed to be fixed to the substrate.
[0169] The bending strength measuring device may be, for example, Tira's TT28025S, Keithely 6485*4, or Keithely 6487*1.
[0170] The bending strength test was performed using a three-point bending method, with the substrate placed between two supports spaced 90mm apart with the stacked capacitor in the middle, and connected to a measuring device to measure the initial charge and leakage current during evaluation. After the connection was complete, the substrate was pressed and bent using bending strength measuring equipment, and at the same time, a current measurement was used to confirm whether the charge stored in the stacked capacitor leaked when pressed 3mm. The cross section of the stacked capacitor was then observed to determine the failure mode.
[0171] 3) How to measure equivalent series resistance (ESR) 200 stacked capacitors are prepared for each of the embodiment and comparative example. The stacked capacitors are soldered onto a PCB that can accommodate 400 capacitors, and then placed once in a reflow facility with a peak temperature of 290°C. The reflowed board is placed in an impedance analyzer and the ESR is measured in an environment with a temperature and frequency of 1MHz.
[0172] As an example of the ESR measuring device, an Impedance Analyzer manufactured by JK Tech can be used.
[0173] For the multilayer capacitors manufactured in the examples and comparative examples, the average surface roughness (Ra) of the outer surface of the metal layer, bending strength, and equivalent series resistance were measured. The results are shown in Table 1.
[0174] [Table 1] Referring to Table 1, it can be seen that the average surface roughness (Ra) of the outer surface of the metal layer of the stacked capacitor manufactured in the Example is 0.4, while the average surface roughness (Ra) of the outer surface of the metal layer of the stacked capacitor manufactured in the Comparative Example is 0.1.
[0175] Also, it can be confirmed that the multilayer capacitor manufactured in the embodiment had no defects and had good bending strength characteristics.
[0176] Furthermore, it can be seen that the multilayer capacitors manufactured in the examples have superior bending strength characteristics compared to the multilayer capacitors manufactured in the comparative examples, while still maintaining equivalent series resistance characteristics.
[0177] Although the preferred embodiment of the present invention has been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the claims, the description of the invention, and the accompanying drawings, and it is to be understood that these also fall within the scope of the present invention. [Explanation of symbols]
[0178] 100: Multilayer capacitor 110: Capacitor body 111: Dielectric layer 112, 113: Coverage area 121: 1st internal electrode 122:Second internal electrode 131: 1st external electrode 132:Second external electrode 1311, 1321: Metal layer 1312, 1322: Conductive resin layer 1313, 1323: plating layer
Claims
1. a capacitor body including a dielectric layer and an internal electrode; an external electrode disposed on an outer side of the capacitor body; The external electrode is a metal layer disposed outside the capacitor body and made of a first conductive metal; a conductive resin layer disposed outside the metal layer and including a resin, a second conductive metal, a low-melting-point metal having a melting point lower than that of the second conductive metal, and an alloy of the second conductive metal and the low-melting-point metal; Stacked capacitor.
2. the multilayer capacitor has a first direction in which the dielectric layers and the internal electrodes are laminated, and a second direction and a third direction perpendicular to the first direction and perpendicular to each other, 2. The multilayer capacitor according to claim 1, wherein the capacitor body has a first surface and a second surface opposed to each other in the first direction, a third surface and a fourth surface opposed to each other in the second direction, and a fifth surface and a sixth surface opposed to each other in the third direction.
3. The stacked capacitor of claim 2 , wherein the metal layer has a surface roughness on an outer surface.
4. In a cross section cut in the first direction and the third direction perpendicular to the second direction at the center in the second direction, 4. The multilayer capacitor according to claim 3, wherein the average surface roughness (Ra) of the metal layer is 0.2 to 1.
5. The multilayer capacitor according to claim 2 , wherein the metal layer is free of glass and binder resin.
6. In a cross section cut in the first direction and the third direction perpendicular to the second direction at the center in the second direction, 6. The multilayer capacitor according to claim 5, wherein the metal layer has an area ratio of the glass to a unit area of 2% or less and an area ratio of the binder resin to a unit area of the metal layer of 1% or less.
7. 7. The stacked capacitor according to claim 1, wherein the first conductive metal or the second conductive metal comprises copper (Cu), nickel (Ni), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), tungsten (W), titanium (Ti), an alloy thereof, or a combination thereof.
8. 7. The multilayer capacitor according to claim 1, wherein the low melting point metal comprises tin (Sn), lead (Pb), bismuth (Bi), silver (Ag), copper (Cu), an alloy thereof, or a combination thereof.
9. In a cross section cut in the first direction and the third direction perpendicular to the second direction at the center in the second direction, 3. The multilayer capacitor according to claim 2, wherein the conductive resin layer has an area ratio of the resin contained in a unit area of the conductive resin layer of 5% to 30%, and an area ratio of the second conductive metal, the low melting point metal, and an alloy of the second conductive metal and the low melting point metal of 5% to 30%.
10. The multilayer capacitor according to claim 2 , wherein the external electrodes further include a plating layer disposed on an outer side of the conductive resin layer.
11. 11. The multilayer capacitor of claim 10, wherein the external electrode has a connection portion arranged outside the third and fourth surfaces of the capacitor body, and a band portion extending from the connection portion onto the first and second surfaces of the capacitor body.
12. The multilayer capacitor according to claim 11 , wherein the metal layer, the conductive resin layer, and the plating layer are located in the connection portion and the band portion.
13. the metal layer is located on the connection portion and the band portion; the conductive resin layer is located on the band portion, The multilayer capacitor according to claim 11 , wherein the plating layer is located on the connection portion and the band portion.
14. forming a capacitor body including a dielectric layer and an internal electrode; forming an external electrode on an outer side of the capacitor body; The step of forming the external electrodes comprises: forming a metal layer comprising a first conductive metal; and applying a paste for a conductive resin layer, the paste including a powder of a second conductive metal, a low melting point metal having a melting point lower than that of the second conductive metal, and a resin, to an outside of the metal layer and then curing the paste to form a conductive resin layer.
15. The method of claim 14, wherein the forming of the metal layer is performed by using a sintering method, a sputtering method, or a plating method.
16. 16. The method of claim 15, wherein the forming of the metal layer comprises applying a paste for a metal layer, the paste including the powder of the first conductive metal and a binder resin, to the outside of the capacitor body, and then performing a heat treatment at a temperature 400° C. or more higher than a curing temperature of the binder resin to remove the binder resin, and sintering the powder of the first conductive metal to form the metal layer.
17. 17. The method for manufacturing a multilayer capacitor according to claim 16, wherein the metal layer paste contains 30 to 60 parts by weight of the binder resin with respect to 100 parts by weight of the first conductive metal.
18. 17. The method of claim 16, wherein in the forming of the metal layer, the heat treatment is performed at a temperature of 600 to 900.degree.
19. 15. The method for manufacturing a multilayer capacitor according to claim 14, wherein the conductive resin layer paste contains 5 parts by weight to 30 parts by weight of the resin and 5 parts by weight to 30 parts by weight of the low melting point metal relative to 100 parts by weight of the second conductive metal.
20. the multilayer capacitor has a first direction in which the dielectric layers and the internal electrodes are laminated, and a second direction and a third direction perpendicular to the first direction and perpendicular to each other, the capacitor body has a first surface and a second surface opposed to each other in the first direction, a third surface and a fourth surface opposed to each other in the second direction, and a fifth surface and a sixth surface opposed to each other in the third direction; the external electrode has a connection portion disposed on the outside of the third surface and the fourth surface of the capacitor body, and a band portion disposed extending from the connection portion onto the first surface and the second surface of the capacitor body, The method for manufacturing a multilayer capacitor according to claim 14 , wherein the conductive resin layer paste is applied so as to be located only on the band portion.